Silicon nitride sintered body, its manufacturing method, bonded body, and power module
A ceramic sintered body with controlled pore distribution and high bending strength addresses the reliability issues in power modules by improving heat cycle resistance and insulation, ensuring stable performance under temperature fluctuations.
Patent Information
- Application Number
- JP2024520596
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-11-25
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Existing ceramic sintered bodies used in power modules for high-power control applications face challenges in maintaining reliability due to insufficient heat cycle resistance and insulation reliability at high temperatures, primarily due to the presence of coarse and micropores that lead to crack formation and dielectric breakdown under temperature changes.
A ceramic sintered body with controlled pore distribution, specifically low average numbers and sizes of coarse and micropores, achieved through the use of finely pulverized sintering aid powder and uniform grain growth, resulting in high bending strength and improved thermal conductivity.
The ceramic sintered body exhibits excellent heat cycle resistance and insulation reliability at high temperatures, effectively suppressing crack formation and dielectric breakdown, thereby enhancing the overall reliability of power modules.
Smart Images

Figure 0007576209000009 
Figure 0007576209000010 
Figure 0007576209000011
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a ceramic sintered body, a manufacturing method thereof, a joined body, and a power module. [Background technology]
[0002] In recent years, power modules for controlling large electric power are used in industrial equipment such as motors and products such as electric vehicles. In such power modules, circuit boards and the like equipped with ceramic plates are used in order to efficiently diffuse heat generated from semiconductor elements and suppress leakage current (see, for example, Patent Document 1). The ceramic sintered body used in such ceramic plates is usually manufactured by forming a ceramic raw material powder into a predetermined shape to form a ceramic molded body, and then firing the ceramic molded body.
[0003] Known ceramic sintered bodies are composed of nitrides, carbides, borides, silicides, etc. When producing such ceramic sintered bodies, sintering aids are used to promote sintering. For example, Patent Document 2 proposes using Si powder, MgO powder, and Y2O3 powder when producing a silicon nitride sintered substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2019 / 022133 [Patent Document 2] International Publication No. 2017 / 170247 Summary of the Invention [Problem to be solved by the invention]
[0005] Electronic components such as power modules are becoming smaller and thinner while improving their performance. Accordingly, it is considered that the required level of reliability of various products used in electronic components will become higher and higher. The present disclosure provides a ceramic sintered body having excellent heat cycle resistance and excellent insulation reliability at high temperatures, a manufacturing method thereof, and a joined body. The present disclosure provides a power module having excellent reliability by including such a ceramic sintered body. [Means for solving the problem]
[0006] One aspect of the present disclosure provides the following ceramic sintered body.
[0007] [1] A ceramic sintered body containing ceramic particles, in which the average number of coarse pores having a size of 10 μm or more in a cross section is 1 / mm 2 The average number of micropores having a size of less than 400 / mm 2 and a flexural strength of 640 MPa or more.
[0008] The ceramic sintered body has a sufficiently small number of both coarse pores and micropores in the cross section, and has a high flexural strength. When such a ceramic sintered body is joined to a different material such as a metal plate, internal stress occurs when there is a temperature change, which causes dielectric breakdown. The ceramic sintered body has high flexural strength, and the number of coarse pores and micropores is sufficiently reduced. Therefore, when internal stress occurs due to a temperature change, the occurrence and progression of cracks can be sufficiently suppressed. Therefore, the ceramic sintered body has excellent heat cycle resistance and excellent insulation reliability at high temperatures.
[0009] The ceramic sintered body of the above [1] may be the following [2] or [3].
[0010] [2] The ceramic sintered body according to [1], wherein the maximum pore size in the cross section is 6 μm or less. [3] The ceramic sintered body according to [1] or [2], wherein the average size of the micropores is 1.0 μm or less and the standard deviation is 0.6 μm or less.
[0011] The ceramic sintered body of [2] above has a maximum pore size of 6 μm or less, which sufficiently suppresses the occurrence of cracks due to temperature changes, and therefore has even better insulation reliability. The ceramic sintered body of [3] above can have sufficiently high durability in a heat cycle environment.
[0012] One aspect of the present disclosure provides the following method for producing a ceramic sintered body.
[0013] [4] A step of pulverizing the sintering aid raw material with a pulverizer to obtain a sintering aid powder having a median diameter of 0.5 to 1.0 μm; preparing a mixed raw material containing a ceramic powder and the sintering aid powder; and firing the green body of the mixed raw material to obtain a ceramic sintered body having a flexural strength of 640 MPa or more.
[0014] The above manufacturing method includes a step of pulverizing the sintering aid raw material with a pulverizer to obtain a sintering aid powder having a median diameter of 0.5 to 1.0 μm. Such a sintering aid powder has a sufficiently small particle diameter and is sufficiently inhibited from agglomerating. By using a mixed raw material containing such a sintering aid, the grain growth of the ceramic powder proceeds uniformly and smoothly, and a ceramic sintered body having a sufficiently reduced number of pores and high flexural strength can be obtained. Such a ceramic sintered body can sufficiently inhibit the occurrence and progression of cracks when internal stress occurs with temperature change. Therefore, it has excellent heat cycle resistance and excellent insulation reliability at high temperatures.
[0015] The method for producing a ceramic sintered body according to the above item [4] may be the following item [5].
[0016] [5] In the cross section of the ceramic sintered body, the average number of coarse pores having a size of 10 μm or more is 1 / mm 2 The average number of micropores having a size of less than 400 / mm 2 Such a ceramic sintered body has even better insulation reliability.
[0017] One aspect of the present disclosure provides the following conjugate:
[0018] [6] A joined body comprising: the plate-shaped ceramic sintered body according to any one of the above [1] to [3]; a metal plate; and a brazing layer joining a main surface of the ceramic sintered body to a main surface of the metal plate.
[0019] The bonded body includes the ceramic sintered body. The ceramic sintered body can sufficiently suppress the occurrence and propagation of cracks when internal stress occurs due to temperature change. Therefore, the bonded body has excellent heat cycle resistance and excellent insulation reliability at high temperatures.
[0020] The conjugate of [6] above may be the following [7] or [8].
[0021] [7] The joined body according to [6], wherein the metal plate has a thickness of 0.8 mm or less. [8] The joined body according to [6] or [7], wherein the brazing material layer contains silver, copper, tin, and an active metal, and the active metal contains one or more selected from the group consisting of titanium, hafnium, zirconium, and niobium.
[0022] One aspect of the present disclosure provides the following power module.
[0023] [9] A joined body including the plate-shaped ceramic sintered body according to any one of the above [1] to [3], a metal plate, and a brazing material layer joining a main surface of the ceramic sintered body and a main surface of the metal plate; a semiconductor element electrically connected to the metal plate of the joint body.
[0024] The power module includes the ceramic sintered body as an insulator for a bonded body to which heat generated by a semiconductor element is transferred. The ceramic sintered body has excellent heat cycle resistance and excellent insulation reliability at high temperatures. Therefore, the power module has excellent reliability. Effect of the Invention
[0025] The present disclosure can provide a ceramic sintered body having excellent heat cycle resistance and excellent insulation reliability at high temperatures, a manufacturing method thereof, and a joined body. The present disclosure can provide a power module having excellent reliability by including such a ceramic sintered body. [Brief description of the drawings]
[0026] [Figure 1] FIG. 1 is an enlarged cross-sectional view that typically shows a portion of a cross section of a ceramic sintered body. [Diagram 2] FIG. 2 is a cross-sectional view of the bonded body taken along the thickness direction. [Diagram 3] FIG. 3 is a cross-sectional view of the power module. [Figure 4] FIG. 4 is a diagram showing an example of the volume-based particle size distribution of the sintering additive powder obtained by the laser diffraction / scattering method. [Diagram 5] FIG. 5 is a diagram showing an example of an image of grain growth as sintering progresses in an example of a manufacturing method. [Figure 6] FIG. 6 is a photograph (200x) showing an example of a cross section taken by a scanning electron microscope. [Figure 7] FIG. 7 is a photograph (1000x) showing an example of a cross section taken by a scanning electron microscope. [Figure 8] FIG. 8 is a diagram illustrating an example of an inspection device for inspecting for dielectric breakdown. [Figure 9] FIG. 9 is a diagram showing an image of grain growth as sintering progresses in a conventional manufacturing method. [Figure 10]FIG. 10 is a photograph (200x) taken by a scanning electron microscope of a cross section of a conventional molded body (ceramic green sheet) and an agglomerate of sintering additive powder contained in the cross section. [Figure 11] FIG. 11 is a scanning electron microscope photograph (200x) of the cross section of a conventional ceramic sintered body. [Figure 12] FIG. 12 is a diagram showing an example of the particle size distribution of a conventional sintering additive powder by a laser diffraction / scattering method. [Figure 13] FIG. 13 is a photograph (200x) showing an example of a conventional cross section taken by a scanning electron microscope. [Figure 14] FIG. 14 is a photograph (1000x) showing an example of a conventional cross section taken by a scanning electron microscope. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Hereinafter, the embodiments of the present disclosure will be described with reference to the drawings in some cases. However, the following embodiments are examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. The numerical range indicated by the symbol "~" includes the lower limit and the upper limit. That is, the numerical range indicated by "A~B" means A or more and B or less. The present disclosure also includes a numerical range that combines a numerical range having only an upper limit and a numerical range having only a lower limit. The present disclosure also includes a numerical range in which the upper limit or lower limit of each numerical range is replaced with the numerical value of any of the examples. When multiple materials are exemplified, one of them may be used alone, or multiple materials may be used in combination.
[0028] A ceramic sintered body according to an embodiment includes ceramic particles. The ceramic sintered body may include pores. The number and size of the pores included in the ceramic sintered body affect the heat cycle resistance and insulation reliability at high temperatures of the ceramic sintered body. The pores include coarse pores and micropores. The coarse pores and the micropores have different sizes, and the pore size is measured as follows.
[0029] Fig. 1 is a diagram showing an example of an image of a part of a cross section of a ceramic sintered body observed with a scanning electron microscope. As shown in Fig. 1, a cross section 10C of the ceramic sintered body includes ceramic particles and pores 20. In Fig. 1, the pores 20 are shown enlarged and schematic. Although the cross section 10C includes a large number of ceramic particles, the ceramic particles are not shown in Fig. 1 for the sake of convenience.
[0030] In the present disclosure, the size of the pore 20 is the length of the line segment L connecting two points selected so that the distance between them is the largest on the outer edge of the pore 20. Then, depending on the length of this line segment L, the pore is classified as a "coarse pore", a "micropore", or other pores. If the length of the line segment L of the pore 20 shown in FIG. 1 is 0.05 μm or more and less than 10 μm, it is classified as a "micropore". On the other hand, if the length of the line segment L measured in the same manner is 10 μm or more, it is classified as a "coarse pore". The length of the line segment L of other pores is less than 0.05 μm.
[0031] The bending strength of a ceramic sintered body varies greatly depending on the average number of coarse pores and the average number of micropores. The average number P1 of coarse pores in the ceramic sintered body of this embodiment is 1 pore / mm 2 The average number P1 of coarse pores is calculated by observing the cross section (magnification: 200 times) in five or more fields of view using a scanning electron microscope, and adding up the number of coarse pores contained in each field of view, using the following formula: Average number of coarse pores P1 = total number of coarse pores / number of fields / area per field
[0032] From the viewpoint of sufficiently increasing the heat cycle resistance and insulation reliability at high temperatures of the ceramic sintered body, the average number P1 of coarse pores is set to 0.8 pores / mm 2 may be less than 0.6 pieces / mm 2 may be less than 0.5 pieces / mm 2 may be less than 0.1 pieces / mm 2 The lower limit of the average number P1 of coarse pores may be less than 0 pores / mm 2The average number P1 of coarse pores can be adjusted, for example, by changing the particle size or degree of aggregation of the sintering aid powder.
[0033] The average number P2 of micropores in the ceramic sintered body of this embodiment is 400 pores / mm 2 The average number of micropores P2 is calculated by observing the cross section (magnification: 1000 times) in five or more fields of view using a scanning electron microscope, and adding up the number of micropores contained in each field of view, using the following formula. The size and number of micropores can be counted using image processing software such as ImageJ. Average number of micropores P2 = Total number of micropores / Number of fields / Area per field
[0034] From the viewpoint of sufficiently increasing the heat cycle resistance and insulation reliability at high temperatures of the ceramic sintered body, the average number of micropores P2 is set to 350 pores / mm 2 may be less than 320 pieces / mm 2 may be less than 290 pieces / mm 2 may be less than 210 pieces / mm 2 The average number of micropores P2 may be less than 10 / mm 2 More than 50 pieces / mm 2 More than 100 pieces / mm 2 The average number P2 of micropores can be adjusted, for example, by changing the particle size or degree of aggregation of the sintering aid powder.
[0035] The average number of coarse pores P1 is 0 / mm 2The maximum size of the pores contained in the cross section of the ceramic sintered body may be 6 μm or less, 5 μm or less, or 3 μm or less. This allows the flexural strength of the ceramic sintered body to be further increased. The maximum size of the pores contained in the cross section of the ceramic sintered body may be 0.5 μm or more, 1.0 μm or more, or 1.2 μm or more. The maximum pore size is determined from the measured value of the size of all pores detected when observing the cross section (magnification: 200 times) in five or more visual fields using a scanning electron microscope.
[0036] From the viewpoint of further improving the heat cycle resistance and the insulation reliability at high temperatures, the average size of the micropores contained in the cross section of the ceramic sintered body may be 1.0 μm or less, and the standard deviation of the size may be 0.6 μm or less. In some examples, the average size of the micropores contained in the cross section of the ceramic sintered body may be 0.7 μm or less, and the standard deviation of the size may be 0.5 μm or less. In other examples, the average size of the micropores contained in the cross section of the ceramic sintered body may be 0.6 μm or less, and the standard deviation of the size may be 0.47 μm or less. The average size of the micropores contained in the cross section of the ceramic sintered body may be 0.1 μm or more. The average size of the micropores is obtained in the same manner as when obtaining the average number P2 described above. That is, it is obtained as the arithmetic average of the sizes of the micropores contained in five or more visual fields. The standard deviation of the sizes of the micropores is also obtained as the standard deviation of the sizes of the micropores contained in five or more visual fields.
[0037] The cross section 10C may contain a sintering aid phase in addition to the pores 20 and ceramic particles. The average area ratio of the ceramic particles (ceramic phase) in the cross section 10C may be 70 to 90%, or may be 75 to 85%. The average area ratio of the sintering aid phase in the cross section 10C may be 10 to 25%, or may be 14 to 22%. A ceramic sintered body having a cross section 10C containing ceramic particles and a sintering aid phase in such an area ratio has sufficiently high thermal conductivity and flexural strength.
[0038] It is preferable that the number of ceramic grains having a major axis of 20 μm or more contained in the cross section of the ceramic sintered body is large. This allows both flexural strength and thermal conductivity to be achieved at a high level. The number of ceramic grains having a major axis length of 20 μm or more was measured using a scanning electron microscope, which was used to measure the number of grains by magnifying the image by 1000 times (field area: 0.02 mm2). 2 ) is used. The length of the major axis of the ceramic particle can be measured in the same manner as the size of the pores 20. That is, the length of the major axis of the ceramic particle is the length of the line segment (major axis) connecting two points selected so that the distance between them is the greatest on the outer edge of the ceramic particle.
[0039] The measurement is performed in five or more visual fields, and the average number is the average number of ceramic particles whose major axis length is 20 μm or more in each visual field. The average number of ceramic particles having a major axis of 20 μm or more may be 10 or more, 15 or more, or 17 or more. The average number of ceramic particles having a major axis of 20 μm or more may be 50 or less, 45 or less, or 40 or less. The standard deviation of the number of ceramic particles having a major axis of 20 μm or more may be less than 0.6 μm or less than 0.5 μm. The standard deviation of the number of ceramic particles having a major axis of 20 μm or more may be 0.1 μm or more, or 0.15 μm or more. Such a ceramic sintered body has a highly uniform microstructure. Therefore, it has excellent reliability.
[0040] The aspect ratio of a ceramic particle having a major axis (size) of 20 μm or more may be 3 or more, and may be 4 or more. The number of ceramic particles having such shapes and sizes can be increased by smooth grain growth during sintering. The aspect ratio is the ratio of the length of the major axis to the length of the minor axis. The minor axis is the line segment connecting two points selected to have the greatest spacing at the outer edge of the ceramic particle in a direction perpendicular to the major axis.
[0041] The ceramic particles constituting the ceramic sintered body may contain at least one selected from the group consisting of silicon nitride particles, aluminum nitride particles, and alumina particles.
[0042] Examples of the ceramic sintered body include a silicon nitride sintered body containing silicon nitride particles as a main component, an aluminum nitride sintered body containing aluminum nitride particles as a main component, and an alumina sintered body containing alumina particles as a main component. Also, a composite sintered body containing multiple types of ceramic particles may be used.
[0043] The flexural strength of the ceramic sintered body is 640 MPa or more. Such a ceramic sintered body has excellent reliability. The flexural strength of the ceramic sintered body may be 670 MPa or more, 690 MPa or more, or 720 MPa or more. This flexural strength is measured by the method described in the Examples. A ceramic sintered body having such a high flexural strength has high insulation. In addition to such flexural strength, the average number of coarse pores and micropores is sufficiently small, so that the ceramic sintered body has excellent heat cycle resistance and excellent insulation reliability at high temperatures. Such a ceramic sintered body can be suitably used, for example, as an insulating substrate for a power module. The upper limit of the flexural strength of the ceramic sintered body may be, for example, 950 MPa. Note that the use of the ceramic sintered body is not limited thereto.
[0044] The bonded body according to one embodiment includes a plate-shaped ceramic sintered body (ceramic plate), a metal plate, and a brazing material layer that bonds a main surface of the ceramic sintered body to a main surface of the metal plate. The ceramic plate may be the ceramic sintered body according to the above embodiment. This ceramic sintered body can sufficiently suppress the occurrence and progression of cracks when internal stress occurs due to temperature change. Therefore, the bonded body has excellent heat cycle resistance and excellent insulation reliability at high temperatures.
[0045] FIG. 2 is a cross-sectional view along the thickness direction showing an example of the bonded body of this embodiment. However, the description of this example is not limited to this example, and is also applicable to other examples of the bonded body. The bonded body 100 of FIG. 2 includes a ceramic plate 10, a metal plate 41 bonded to one main surface 10A of the ceramic plate 10 via a brazing material layer 51, and a metal plate 42 bonded to the other main surface 10B of the ceramic plate 10 via the brazing material layer 51. The metal plate 41 is patterned and functions as, for example, a circuit. In this specification, such a patterned one is also referred to as a metal plate. The metal plate 42 is not patterned and functions as, for example, a heat sink. The ceramic plate 10 is composed of the above-mentioned ceramic sintered body.
[0046] The metal plates 41, 42 may be, for example, copper plates. From the viewpoint of improving heat dissipation performance and electrical conductivity, the thickness of the metal plates 41, 42 may be 0.3 mm or more, or may be 0.4 mm or more. From the viewpoint of reducing internal stress generated in the ceramic plate 10 due to temperature change, the thickness of the metal plates 41, 42 may be 0.8 mm or less, or may be 0.7 mm or less. An example of the thickness range of the metal plates 41, 42 is 0.3 to 0.8 mm.
[0047] The thickness of the ceramic plate 10 may be 0.2 mm or more, or may be 0.3 mm or more, from the viewpoint of improving the insulation property, and may be 0.8 mm or less, or may be 0.6 mm or less, from the viewpoint of making the bonded body 100 thinner.
[0048] The brazing material layers 51, 52 are layers for joining the ceramic plate 10 and the metal plates 41, 42, and contain brazing material components. The brazing material layers may contain, for example, silver derived from the brazing material, or silver and copper. The brazing material layers 51, 52 may further contain one or more metals selected from the group consisting of tin and active metals derived from the brazing material. In the brazing material layers 51, 52, the two or more metals may be alloyed. The active metal may contain one or more metals selected from the group consisting of titanium, hafnium, zirconium, and niobium. The silver and copper contained in the brazing material layers 51, 52 may be contained as an alloy such as an Ag-Cu eutectic alloy. The content of silver in the brazing material layers 51, 52 may be 45 to 95 mass % or 50 to 95 mass % in terms of Ag. The total content of silver and copper in the brazing material layers 51, 52 may be 65 to 100 mass%, 70 to 99 mass%, or 90 to 98 mass%, calculated as Ag and Cu, respectively. The thickness and composition of the brazing material layers 51, 52 may be the same as or different from each other.
[0049] In a modified example of the bonded body, the metal plates bonded to both main surfaces of the ceramic plate may have the same shape. For example, the bonded body may be a body before a circuit pattern is formed. In another modified example, a plurality of metal plates may be bonded to one main surface of the ceramic plate. A metal plate may be bonded to only one main surface of the ceramic plate.
[0050] The power module according to one embodiment includes a bonded body (circuit board) and a semiconductor element electrically connected to the metal plate of the bonded body. The bonded body may be the above-mentioned bonded body 100 or a modified example thereof. The contents of the description regarding the ceramic sintered body, the bonded body, and the modified examples thereof are applied to the power module of this embodiment. Such a power module includes a bonded body having ceramic plates that are excellent in heat cycle resistance and also excellent in insulation reliability at high temperatures. Therefore, even when used in an environment where the temperature fluctuates greatly, high performance can be maintained. Thus, the power module has excellent reliability.
[0051] FIG. 3 is a cross-sectional view showing an example of a power module. The description of this example is not limited to this example, and is also applicable to other examples of power modules. The power module 200 of FIG. 3 includes a base plate 90 and a joint body 100 joined to one side of the base plate 90 via solder 82. A metal plate 42 (heat sink) on one side of the joint body 100 is joined to the base plate 90 via the solder 82.
[0052] A semiconductor element 80 is attached to a metal plate 41 (circuit pattern) on the other surface side of the bonded body 100 via solder 81. The semiconductor element 80 is connected to a predetermined location of the metal plate 41 by a metal wire 84 such as an aluminum wire. In this manner, the semiconductor element 80 and the metal plate 41 are electrically connected. To electrically connect the outside of the housing 86 to the metal plate 41, a metal plate 41a, which is one of the metal plates 41, is connected to an electrode 83 provided penetrating the housing 86 via solder 85.
[0053] A housing 86 is disposed on one of the main surfaces of the base plate 90, and is integrated with the main surface to accommodate the bonded body 100. A space formed by the one of the main surfaces of the base plate 90 and the housing 86 is filled with a resin 95. The resin 95 seals the bonded body 100 and the semiconductor element 80. The resin may be, for example, a thermosetting resin or a photocurable resin.
[0054] A cooling fin 92 serving as a heat dissipation member is joined to the other main surface of the base plate 90 via grease 94. Screws 93 are attached to the ends of the base plate 90 to fix the cooling fin 92 to the base plate 90. The base plate 90 and the cooling fin 92 may be made of aluminum. The base plate 90 and the cooling fin 92 function well as a heat dissipation section due to their high thermal conductivity.
[0055] The metal plate 41 and the metal plate 42 are electrically insulated by the ceramic plate 10 (plate-shaped ceramic sintered body). The metal plate 41 (41a) may form an electric circuit. The metal plate 41 and the metal plate 42 are respectively joined to the main surface 10A and the main surface 10B of the ceramic plate 10 by a brazing material layer (not shown) containing a brazing material component. The power module 200 has excellent reliability because it includes the joined body 100.
[0056] A method for producing a ceramic sintered body according to one embodiment includes a grinding step of grinding a sintering aid raw material with a grinder to obtain a sintering aid powder having a D50 (median diameter) of 0.5 to 1.0 μm, a mixing step of preparing a mixed raw material containing a ceramic powder and a sintering aid powder, and a firing step of firing a compact of the mixed raw material.
[0057] The sintering aid powder contains at least two selected from the group consisting of alkaline earth metal oxides, rare earth oxides, transition metal oxides different from the rare earth oxides, silica, and alumina. The sintering aid powder may contain at least three selected from the group.
[0058] The alkaline earth metal oxide has an alkaline earth metal and oxygen as constituent elements. The alkaline earth metal oxide may include at least one selected from the group consisting of magnesium oxide, calcium oxide, and strontium oxide. The rare earth oxide has a rare earth element and oxygen as constituent elements. The rare earth oxide may include at least one selected from the group consisting of yttrium oxide and cerium oxide, for example. The transition metal oxide different from the rare earth oxide has a transition metal different from the rare earth and oxygen as constituent elements. Such a transition metal oxide may include, for example, iron oxide.
[0059] An example of the sintering aid powder contains magnesium oxide, rare earth oxide, and silica. In this case, when the entire sintering aid powder is taken as 100 parts by mass, the content of the rare earth oxide may be 30 to 80 parts by mass, or may be 40 to 70 parts by mass. In this case, the content of the magnesium oxide may be 5 to 40 parts by mass, or may be 10 to 30 parts by mass. In this case, the content of the silica may be 5 to 40 parts by mass, or may be 10 to 30 parts by mass.
[0060] The D50 (median diameter) of the sintering aid powder in the pulverizing step may be adjusted, for example, by pulverizing the sintering aid raw material with a pulverizer. As the pulverizer, a bead mill type pulverizer may be used. The particle size distribution of the sintering aid powder may be adjusted by changing at least one condition selected from the group consisting of the diameter of the beads of the bead mill type pulverizer, the peripheral speed, and the pulverizing time. The diameter of the beads may be 0.1 to 0.3 mm. The peripheral speed of the rotor may be 8 to 12 m / sec. The pulverizing time may be 5 to 20 minutes. Examples of pulverizers other than the bead mill type pulverizer include a ball mill, a vibration mill, and a pot mill.
[0061] If the D50 of the sintering aid powder exceeds 1.0 μm, the number and size of the pores will increase, and the flexural strength will decrease. If the D50 of the sintering aid powder is less than 0.5 μm, the crushed particles tend to aggregate due to the relationship between the input energy applied to the sintering aid raw material from the crusher and the crushing ratio. This is thought to be due to the fact that the frequency of contact between the crushed particles increases as the crushing progresses, and that the potential energy becomes rich in attractive forces.
[0062] The D50 of the sintering aid powder is determined based on the volumetric particle size distribution measured by a particle size distribution measuring device using the laser diffraction / scattering method. By having the D50 of the sintering aid powder within the above range, the particles contained in the sintering aid powder are sufficiently small, and the particles can be prevented from agglomerating together. This makes it possible to prevent the generation of pores caused by the particles and agglomerates of the sintering aid powder when producing a ceramic sintered body. In addition, the grain growth of the ceramic particles can be promoted with high uniformity.
[0063] 4 and 12 are diagrams showing examples of volumetric particle size distribution of sintering aid powders by laser diffraction and scattering. The horizontal axis is particle size [μm] in logarithmic scale, and the vertical axis is frequency [volume %]. The particle size distribution in this disclosure is measured in accordance with the method described in JIS Z 8825:2013 "Particle size analysis - Laser diffraction and scattering method". For particle size distribution measurement, LS-13 320 (product name) manufactured by Beckman Coulter can be used. Measurement conditions are a particle refractive index of 2.2 and a solvent refractive index of 1.33.
[0064] The sintering aid powder may have only one peak in the particle size distribution (frequency %) as shown in FIG. 4. Such a sintering aid powder is more sufficiently suppressed from agglomerating than one having multiple peaks as shown in FIG. 12. Therefore, the size and number of pores in the ceramic sintered body can be sufficiently reduced. The peak in the particle size distribution may be sharp. For example, the D100 of the sintering aid powder may be less than 5.5 μm, or may be less than 5 μm. For example, the ratio of D100 to D50 may be 5 or less. An example of the lower limit of D100 is 2 μm. An example of the lower limit of the ratio of D100 to D50 is 2.
[0065] In the mixing step, the sintering aid powder obtained by pulverization, the ceramic powder, and additives, if necessary, are blended and mixed using, for example, a ball mill. In this way, a mixed raw material containing the sintering aid powder and the ceramic powder is prepared. Examples of additives include binders, plasticizers, dispersion media, and release agents. Examples of binders include methylcellulose-based binders having plasticity or surface activity, and acrylic ester-based binders having excellent thermal decomposition properties. Examples of plasticizers include glycerin. Examples of dispersion media include ion-exchanged water and ethanol.
[0066] As the ceramic powder, for example, silicon nitride powder, aluminum nitride powder, or aluminum oxide powder can be used. The D50 (median diameter) of the ceramic powder may be 0.1 to 6 μm, or may be 0.5 to 4 μm. This allows a sufficiently densified ceramic sintered body to be obtained. The D50 of the ceramic powder is determined in the same manner as the D50 of the sintering aid powder. The number of peaks in the particle size distribution (frequency %) of the ceramic powder may also be one.
[0067] The mass ratio of the sintering aid powder to the ceramic powder may be 0.03 to 0.12, or may be 0.05 to 0.1, which makes it easier to densify the ceramic sintered body and allows the bending strength to be sufficiently high.
[0068] The mixed raw material obtained in the mixing step is applied to a release film in a predetermined thickness by a doctor blade method, a calendar method, an extrusion method, or the like, dried, and molded to obtain a molded body. The molding pressure may be 3 to 30 MPa. The molded body may be produced by uniaxial pressing or by CIP. It may also be fired while being molded by hot pressing. For example, after producing a ceramic green sheet substrate by the above-mentioned method such as the doctor blade method, the ceramic green sheet substrate may be punched out using a mold equipped with a die and a punch to obtain a molded body.
[0069] The solid content of the ceramic green sheet substrate when punched with a die may be 65 to 85 mass %, or may be 75 to 85 mass %. The solid content may be adjusted by carrying out a drying process of drying the ceramic green sheet substrate before punching with a die.
[0070] Before firing the molded body in the firing step, the molded body may be degreased. The degreasing method is not particularly limited, and may be, for example, performed by heating the molded body in air or a non-oxidizing atmosphere such as nitrogen to 300 to 700° C. The heating time may be, for example, 1 to 10 hours.
[0071] The ceramic sintered body can be obtained by firing the molded body. The atmosphere, temperature, time, etc. during firing can be appropriately set depending on the type of ceramic sintered body. When a silicon nitride sintered body is produced as the ceramic sintered body, the firing may be performed in an inert gas atmosphere such as nitrogen gas or argon gas. The pressure during firing may be 0.7 to 1 MPa. The firing temperature may be 1800 to 2100°C, 1800 to 2000°C, or 1800 to 1900°C. The firing time at the firing temperature may be 3 to 20 hours, or 4 to 16 hours.
[0072] When an aluminum nitride sintered body is produced as the ceramic sintered body, the firing temperature may be, for example, 1760 to 1840°C. The holding time in the temperature range of 1760 to 1840°C may be, for example, 1 to 10 hours. The firing may be performed under atmospheric pressure. When producing a ceramic sintered body other than a silicon nitride sintered body and an aluminum nitride sintered body (for example, an aluminum oxide sintered body), the sintering conditions may be appropriately set so that the sintered body is sufficiently densified.
[0073] FIG. 5 is a diagram showing an image of grain growth as sintering progresses in an example of the manufacturing method of this embodiment. In this example, as shown in FIG. 5(a), fine sintering aid powder 32 is dispersed in ceramic particles 12 with high uniformity in the molded body. When such a molded body is fired, the liquefied sintering aid phase 32a diffuses to the grain boundaries by capillary action as shown in FIG. 5(b). When the sintering aid phase 32a diffuses, the shrinkage of the molded body (ceramic sintered body) progresses, and the pores 22 disappear as shown in FIG. 5(c). When heating is continued, the ceramic particles 12 melt into the sintering aid phase 32a, and columnar ceramic particles 14 are generated as shown in FIG. 5(d). In this way, as liquid phase sintering progresses, the pores 22 disappear sufficiently with the smooth grain growth of the ceramic particles, so that the pores contained in the ceramic sintered body can be sufficiently reduced. A part of the sintering aid phase 32a may remain in the ceramic sintered body.
[0074] FIG. 9 is a diagram showing an image of grain growth as sintering progresses in a conventional manufacturing method. In the conventional manufacturing method, as shown in (a) of FIG. 9, in the molded body, aggregates 132 of sintering aid powder are contained in ceramic particles 112. A cross-sectional photograph of such a conventional molded body is shown in FIG. 10. When such a molded body is fired, as shown in (b) of FIG. 9, the liquefied sintering aid phase 132a diffuses from the aggregates 132 to the grain boundaries by capillary action. As diffusion by capillary action progresses, pores 122 are generated in the aggregates 132 because of the large size of the aggregates 132. Since the pores 122 have a large size, they do not disappear even when the molded body shrinks, and the pores 122 remain in the ceramic sintered body as shown in (c) of FIG. In this way, the number of large pores contained in the ceramic sintered body increases. FIG. 11 shows a cross section 110C of a conventional ceramic sintered body obtained in this way. The cross section 110C includes pores 122 derived from the aggregates 132.
[0075] In contrast to the conventional manufacturing method, in the manufacturing method of this embodiment, the particles of the sintering aid powder are sufficiently fine, and the aggregation of the particles is suppressed. Therefore, it is possible to reduce the pores remaining as traces of the sintering aid powder. This reduces the number of pores generated during the sintering process and reduces the size of the pores. The number of pores in the ceramic sintered body obtained in this manner is sufficiently reduced, and the size of the pores is sufficiently reduced. In addition, this ceramic sintered body has a high flexural strength of 640 MPa or more. As described above, the flexural strength of the ceramic sintered body may be 670 MPa or more, 690 MPa or more, or 720 MPa or more. The average numbers P1 and P2 of the coarse pores and micropores contained in the ceramic sintered body are also as described above. Such a ceramic sintered body can sufficiently suppress the occurrence and progression of cracks when internal stress occurs with a change in temperature. Therefore, it has excellent heat cycle resistance and excellent insulation reliability at high temperatures.
[0076] 8 is a diagram showing a schematic diagram of an example of an inspection device that measures leakage current of a bonded body (circuit board) to inspect for dielectric breakdown. The inspection device 400 includes an AC power source 60 and a withstand voltage tester 50 connected to the AC power source 60. One terminal of the withstand voltage tester 50 is electrically connected to a conductive support part 72a that contacts a metal plate 41 bonded to a ceramic plate 10. The other terminal of the withstand voltage tester 50 is electrically connected to a conductive support part 72b that contacts a metal plate 42 via an electrode 70 arranged in a storage tank 77 that stores insulating oil 76.
[0077] The electrode 70 is disposed along the bottom surface and one side surface of the storage tank 77. As shown in Fig. 8, the electrode 70 has an L-shape when viewed in vertical cross section. The electrode 70 has two insulating supports 74 disposed adjacent to the conductive support 72b. The two insulating supports 74 each contact the metal plate 42 and support the assembly 100 in the insulating oil 76.
[0078] The electrode 70 and the conductive supporting parts 72a, 72b may be made of, for example, oxygen-free copper. The insulating oil 76 may be, for example, a fluorine-based inert liquid. The withstand voltage tester 50 may be a commercially available one. In such an inspection device 400, a voltage of, for example, about 10 to 15 kV is applied between the metal plates 41, 42 sandwiching the ceramic plate 10, and the withstand voltage tester 50 measures the presence or absence of leakage current. By heating the insulating oil 76, the insulating performance of the ceramic plate 10 in the joined body 100 at a high temperature of, for example, 100° C. or higher can be evaluated.
[0079] The inspection device is not limited to the configuration of FIG. 8, and any inspection device can be used without particular limitations as long as it is capable of measuring leakage current when a voltage is applied between metal plates 41 and 42 at a temperature of, for example, 100° C. or higher.
[0080] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments. The contents of the description of the embodiments of the ceramic sintered body are also applicable to the joined body, the power module, and the manufacturing method of the ceramic sintered body. The contents of the description of the embodiments of the manufacturing method of the ceramic sintered body are also applicable to the ceramic sintered body.
[0081] Any combination of the upper and lower limit values of the numerical ranges specifically described in each of the above embodiments is also included in the present disclosure. In addition, the upper and / or lower limit values of the numerical ranges are also included in the present disclosure in which the values of the examples described below are substituted. EXAMPLES
[0082] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the specific examples below.
[0083] [Preparation of sintering aid powder] (Comparative Examples 1 to 5, Examples 1 to 3) Commercially available yttrium oxide powder, magnesium oxide powder, and silica powder were prepared as raw materials for the sintering aid powder. These were mixed to obtain a mixed powder with a mass ratio of Y2O3:MgO:SiO2 = 5:2:2. The mixed powder was pulverized using a bead mill type pulverizer (manufactured by Ashizawa Finetech Co., Ltd., device name: Star Mill LMZ) to obtain a sintering aid powder. The pulverization conditions (bead diameter, rotor circumferential speed, and pulverization time) of the bead mill type pulverizer were changed as shown in Tables 1 and 2 to prepare multiple types of sintering aid powders with different pulverization conditions.
[0084] The volumetric particle size distribution of each sintering aid powder was measured using a particle size distribution measurement device (manufactured by Nikkiso Co., Ltd., device name: particle size distribution measurement device MT3000II) using a laser diffraction / scattering method. From the particle size distribution measurement results, D50 (median size) and D100 (maximum particle size) were calculated. The results are shown in Tables 1 and 2. Tables 1 and 2 also show the ratio of D100 to D50. The particle size distributions (frequency %) of Examples 1 to 3 all had only one peak, as shown in FIG. 4.
[0085] [Table 1]
[0086] [Table 2]
[0087] From the results of Comparative Examples 1 to 3 in Table 1, it was confirmed that the D50 and D100 of the sintering aid can be reduced by reducing the diameter of the beads. Also, from the results of Comparative Examples 3 and 4 and Example 1, it was confirmed that the D50 and / or D100 can be reduced by increasing the circumferential speed of the rotor. From the results of Examples 1 and 2, it was confirmed that the D50 and D100 can be reduced by extending the grinding time. On the other hand, from the results of Examples 2 and 3 and Comparative Example 5, it was confirmed that the D50 and D100 increase when the grinding time is extended too much. This is considered to be due to the aggregation of the ground powder.
[0088] [Preparation of silicon nitride plate] Example 4 Commercially available silicon nitride powder (D50: 0.7 μm), the sintering aid powder of Example 2, and an additive (solvent-based binder) were mixed in a bead mill to prepare a raw material slurry. The compounding ratio of the silicon nitride powder and the sintering aid powder was silicon nitride powder: sintering aid powder = 91:9. Next, the above-mentioned raw material slurry was applied to a release film by a doctor blade method to prepare a green sheet. The prepared ceramic green sheet was cut to a length x width = 250 mm x 180 mm, and 70 sheets were stacked to obtain a laminate. The above laminate was placed in an electric furnace equipped with a carbon heater and heated in air at 500 ° C for 20 hours to degrease it.
[0089] The degreased molded body was placed in a sintering furnace, the pressure in the furnace was reduced to 100 Pa or less, and the temperature was raised to 900°C. Nitrogen gas was then introduced into the sintering furnace, and the temperature was raised to 1500°C under a pressure of about 0.9 MPa and held for 4 hours. After that, the temperature was raised to 1830°C and held at 1830°C for 5 hours. In this way, a silicon nitride plate with a thickness of 3 mm was obtained.
[0090] Example 5 A silicon nitride sintered body was obtained in the same manner as in Example 4, except that the sintering aid powder of Example 1 was used instead of the sintering aid powder of Example 2.
[0091] Example 6 A silicon nitride sintered body was obtained in the same manner as in Example 4, except that the sintering aid powder of Example 3 was used instead of the sintering aid powder of Example 2.
[0092] Comparative Example 6 Commercially available yttrium oxide powder, magnesium oxide powder, and silica powder were mixed in the same mass ratio as in Example 1 to obtain a mixed powder. This mixed powder was mixed with the silicon nitride powder and additives used in Example 4 as a sintering aid powder without being pulverized in a bead mill type pulverizer. These were mixed using a ball mill to prepare a raw material slurry. A silicon nitride sintered body was obtained in the same manner as in Example 4, except that this raw material slurry was used. The particle size distribution of the mixed powder (sintering aid powder) before being put into the ball mill was measured using the particle size distribution measuring device used in Example 1. From the measurement results of this particle size distribution, D50 (median size) and D100 (maximum particle size) were obtained. As a result, D50 was 3.171 μm and D100 was 497.7 μm. In addition, the particle size distribution of the sintering aid powder used in Comparative Example 6 had two peaks as in FIG. 12. The presence of two peaks is due to the inclusion of particle aggregates in the sintering aid powder.
[0093] [Evaluation of sintered silicon nitride] <Density measurement> The density of the plate-shaped silicon nitride sintered body obtained in each Example and Comparative Example was measured. Specifically, five silicon nitride sintered bodies obtained in each Example and Comparative Example were randomly selected, and the density was measured by Archimedes' method. The results were as shown in Table 3. As shown in Table 3, the density of the silicon nitride sintered bodies in each Example and Comparative Example was equivalent. From this, it is considered difficult to estimate the average number of coarse pores and micropores based on the density.
[0094] [Table 3]
[0095] <Measurement of coarse pores> The silicon nitride sintered bodies obtained in each of the Examples and Comparative Examples were cut in the thickness direction, and each cut surface was polished. The cut surfaces were observed at a magnification of 200 times using a scanning electron microscope (SEM). In each cut surface as shown in Fig. 6 and Fig. 13, 24 fields of view (area per field of view: 0.74 mm2) were observed. 2) were observed to measure the size and total number of coarse pores. As described above, a coarse pore was defined as one in which the length of the line segment connecting two points selected so that the distance between them was the greatest on the outer edge of the pore was 10 μm or more. Based on these measurement results, the average number P1 of coarse pores was calculated. The results are shown in Table 4.
[0096] [Table 4]
[0097] <Measurement of Micropores> Each cut surface of the silicon nitride plate was observed at a magnification of 1000 times. The size and number of micropores in the SEM photographs shown in Figures 7 and 14 were measured using image processing software (ImageJ). As in the measurement of coarse pores, 24 fields of view (area per field: 0.02 mm) were measured on each cut surface. 2 ) to measure the size and total number of micropores. As described above, a micropore was defined as one in which the length of the line segment connecting two points selected so that the distance between them is the largest on the outer edge of one pore is 0.05 μm or more and less than 10 μm. Based on the measurement results, the average number P2 of micropores, and the maximum, average, minimum and standard deviation of the size of the micropores (the line segment) were calculated. The results are shown in Table 5.
[0098] <Measurement of silicon nitride particles> Cross sections of each Example and Comparative Example (area per field of view: 0.02 mm 2 Among the silicon nitride particles contained in the SEM photograph (1000x magnification) of the sample, the number of silicon nitride particles with a line segment (major axis) length of 20 μm or more, which connects two points selected so that the distance between the two points is the greatest on the outer edge, was counted. The results are shown in the "Number of Particles" column in Table 5.
[0099] [Table 5]
[0100] As shown in Table 5, the average size of the micropores was not significantly different between each Example and Comparative Example 6. On the other hand, the variation in the size of the micropores was smaller in each Example than in Comparative Example 6. It was also confirmed that the grain growth of the silicon nitride particles in each Example was more sufficiently advanced than in the Comparative Example. All of the silicon nitride particles having the line segment length of 20 μm or more contained in the silicon nitride plate of each Example had an aspect ratio of 4 or more. The "number of particles" in Table 5 is the measurement result in one visual field, but when the same measurement was performed in 10 visual fields, the number of silicon nitride particles having a major axis length of 20 μm or more in each visual field was 15 or more in each of Examples 4 to 6.
[0101] <Measurement of bending strength (before heat cycle test)> The three-point bending flexural strength of the silicon nitride plates of each Example and Comparative Example 6 was measured. The measurement was performed in accordance with JIS R 1601:2008 using a commercially available flexural strength meter (manufactured by Shimadzu Corporation, device name: AG-2000). For each Example and Comparative Example 6, 20 measurement samples were prepared and measurements were performed (N=20). The average, maximum, and minimum values of the measured values were as shown in Table 6.
[0102] [Table 6]
[0103] As shown in Table 6, the silicon nitride sintered bodies of the Examples had higher flexural strength than Comparative Example 6.
[0104] <Measurement of bending strength (after heat cycle test)> Ag powder (manufactured by Fukuda Metal Foil & Powder Industry Co., Ltd., product name: Ag-HWQ, average particle size D50: 2.5 μm, specific surface area 0.4 m 2 / g) 89.5 parts by mass, Cu powder (manufactured by Fukuda Metal Foil & Powder Co., Ltd., product name: Cu-HWQ, average particle size D50: 3.0 μm, specific surface area: 0.4 m 2A brazing filler metal was prepared containing 9.5 parts by mass of titanium hydride powder (manufactured by Toho Tech Co., Ltd., product name: TCH-100) and 3.5 parts by mass of titanium hydride powder (manufactured by Toho Tech Co., Ltd., product name: TCH-100) for a total of 100 parts by mass. This brazing filler metal was applied in an amount of 8 mg / cm 2 The coating was applied to both main surfaces of Examples 4, 5, and 6 and Comparative Example 6 by screen printing so as to obtain the following:
[0105] A copper plate for forming a circuit was placed on the brazing material layer on one main surface of a plate-shaped silicon nitride sintered body (silicon nitride plate), and a copper plate for forming a heat sink (both 0.8 mm thick, oxygen-free copper plate of C1020 with a purity of 99.60% by mass) was placed on the brazing material layer on the other main surface to obtain a laminate. -3 The bonded body was obtained by heating the copper plates for forming a circuit at 830°C for 30 minutes in a vacuum of 0.1 Pa or less. An etching resist was printed on the bonded copper plates for forming a circuit, and the copper plates for forming a circuit were etched with a ferric chloride solution to form a circuit pattern. Furthermore, the excess brazing material layer was removed with an ammonium fluoride / hydrogen peroxide solution. In this way, a circuit board was produced.
[0106] The fabricated circuit board was subjected to a heat cycle test in which 2500 cycles were repeated, with one cycle being -55°C for 15 minutes, 25°C for 15 minutes, 175°C for 15 minutes, and 25°C for 15 minutes. After the heat cycle test, the circuit pattern and the copper plate for forming the heat sink were removed by etching using a ferric chloride solution and an ammonium fluoride / hydrogen peroxide solution to obtain a silicon nitride plate. The three-point bending strength of the silicon nitride plate thus obtained was measured. The measurement method and the number of measurement samples were the same as those used in the measurement before the heat cycle test. The average, maximum, and minimum values of the measured values were as shown in Table 7.
[0107] [Table 7]
[0108] Even after the heat cycle test, the silicon nitride plates of Examples 4 to 6 had higher flexural strength than the silicon nitride plate of Comparative Example 6. Comparing the values in Tables 6 and 7, the degree of decrease in flexural strength due to the heat cycle test was smaller in Examples 4 to 6 than in Comparative Example 6. This shows that the silicon nitride plates of Examples 4 to 6 have excellent heat cycle resistance. The reason for this is thought to be that the number of coarse pores and micropores is smaller in Examples 4 to 6 than in Comparative Example 6, thereby suppressing the occurrence and progression of cracks due to internal stress caused by thermal expansion and thermal contraction.
[0109] <Evaluation of high temperature insulation> Circuit boards were produced using the silicon nitride sintered bodies of Examples 4 to 6 and Comparative Example 6 in the same procedure as that for measuring the bending strength. A voltage resistance test was performed on each circuit board in accordance with JIS C2110-1:2010 using an inspection device as shown in FIG. 8 (N=3). For this test, an AC20kV voltage resistance tester (model: 7473) manufactured by Keisoku Gijutsu Kenkyusho Co., Ltd. was used. Perfluorocarbon (manufactured by 3M Japan Ltd., product name: Fluorinert, model number: FC-3283) was used as the insulating oil. An inspection tool manufactured by Onishi Electronics Co., Ltd. was used as the storage tank 77, the electrode 70, the conductive support parts 72a, 72b, and the insulating support part 74. The electrode 70 was made of oxygen-free copper, and the conductive support parts 72a, 72b were made of carbon tool steel (SK material) plated with rhodium.
[0110] The insulating oil of the inspection device was heated to 120°C, and the circuit board was set in the insulating oil. The voltage was increased to 9 kV at a rate of 0.1 kV / sec and kept for 60 seconds. After that, the voltage was increased at a rate of 0.1 kV / sec. In this manner, the voltage was increased to 15 kV by repeatedly keeping the voltage at 1 kV for 60 seconds and increasing the voltage at 0.1 kV / sec. Before reaching 15 kV, if a current flowed that was equal to or greater than the threshold for the current interruption current flow, it was determined that an insulation breakdown had occurred. The threshold was set to 9.99 mA. The results were as shown in Table 8.
[0111] [Table 8]
[0112] In Example 4, no dielectric breakdown occurred even when the voltage reached 15 kV. This confirmed that the circuit board of Example 4 has the best insulation reliability at high temperatures. It was also confirmed that the circuit boards of Examples 5 and 6 have better insulation reliability at high temperatures than the circuit board of Comparative Example 6. [Industrial Applicability]
[0113] According to the present disclosure, there are provided a ceramic sintered body having excellent heat cycle resistance and excellent insulation reliability at high temperatures, a manufacturing method thereof, and a joined body. The present disclosure also provides a power module having excellent reliability by including such a ceramic sintered body. [Explanation of symbols]
[0114] 10A, 10B...main surface, 10C, 110C...cross section, 10...ceramic plate, 12, 14, 112...ceramic particles, 20, 22, 122...pores, 32...sintering aid powder, 32a, 132a...sintering aid phase, 41, 41a, 42...metal plate, 50...voltage resistance tester, 51, 52...brazing material layer, 60...AC power source, 70...electrodes, 72a, 72b...conductive support, 74...insulating support, 76...insulating oil, 77...reservoir, 80...semiconductor element, 81, 82, 85...solder, 83...electrodes, 84...metal wire, 86...casing, 90...base plate, 92...cooling fin, 93...screw, 94...grease, 95...resin, 100...joint, 132...aggregate, 200...power module, 400...inspection device.
Claims
1. A silicon nitride sintered body containing silicon nitride particles, In the cross section, the average number of coarse pores having a size of 10 μm or more is 1 / mm 2 The average number of micropores having a size of 0.05 μm or more and less than 10 μm is less than 320 pores / mm 2 is less than A silicon nitride sintered body having a flexural strength of 670 MPa or more.
2. 2. The silicon nitride sintered body according to claim 1, wherein the maximum pore size in the cross section is 6 μm or less.
3. 2. The silicon nitride sintered body according to claim 1, wherein the average size of the micropores is 1.0 μm or less and the standard deviation is 0.6 μm or less.
4. A process for pulverizing a sintering aid raw material containing yttrium oxide, magnesium oxide, and silica with a pulverizer to obtain a sintering aid powder having a median diameter of 0.5 to 1.0 μm and a maximum particle diameter of 3.9 μm or less; A step of preparing a mixed raw material containing silicon nitride powder and the sintering aid powder; and sintering the molded body of the mixed raw material in an inert gas atmosphere at a pressure of 0.7 to 1 MPa and a sintering temperature of 1800 to 2100°C to obtain a silicon nitride sintered body. In the cross section of the silicon nitride sintered body, the average number of coarse pores having a size of 10 μm or more is 1 / mm 2 and the average number of micropores having a size of 0.05 μm or more and less than 10 μm is 320 / mm 2 and the flexural strength of the silicon nitride sintered body is 670 MPa or more.
5. A joint comprising the plate-shaped silicon nitride sintered body according to any one of claims 1 to 3, a metal plate, and a brazing layer joining a main surface of the silicon nitride sintered body and a main surface of the metal plate.
6. The joined body according to claim 5 , wherein the metal plate has a thickness of 0.8 mm or less.
7. the braze layer includes silver, copper, tin, and an active metal; 6. The joined body according to claim 5, wherein the active metal comprises one or more metals selected from the group consisting of titanium, hafnium, zirconium, and niobium.
8. A joint body comprising the plate-shaped silicon nitride sintered body according to any one of claims 1 to 3, a metal plate, and a brazing material layer joining a main surface of the silicon nitride sintered body and a main surface of the metal plate; a semiconductor element electrically connected to the metal plate of the joint body.
Citation Information
Patent Citations
Silicon nitride ceramic substrate and silicon nitride ceramic circuit substrate using it and its manufacturing method
JP2002201075A
Silicon nitride substrate, method of producing the same and silicon nitride substrate having thin film obtained by using the substrate
JP2003192445A
Brazing material for ceramic substrates, and ceramic circuit board using the same
JP2004314161A
Silicon nitride sintered compact and its manufacturing method
JP2006036554A
Silicon nitride sintered compact and sliding member using the same
JP2008285349A