Joint and substrate holding member

The joined body design with specific brazing materials addresses bonding issues by enhancing strength and crack resistance, ensuring robust bonding and durability through stress relaxation and material compatibility.

JP7576413B2Active Publication Date: 2024-10-31NITERRA CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020138526
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-19
Publication Date
2024-10-31
Estimated Expiration
2040-08-19

AI Technical Summary

Technical Problem

Existing bonding materials, such as Au-Ni brazing filler metal and brazing materials with active metals, suffer from poor wettability with ceramics, leading to gaps and weakened bonding strength, while materials with high Young's modulus become brittle and crack during thermal cycles, compromising the integrity of the bonded body.

Method used

A joined body configuration with a ceramic member, a metal terminal, and a stress relaxation part bonded via first and second brazing materials, where the first brazing material has a tensile strength of 100 MPa or more and a Young's modulus of 150 GPa or less, and the second brazing material has a Young's modulus of 90 GPa or more, to mitigate thermal stress and crack formation.

Benefits of technology

The configuration provides a bonded body with enhanced strength and resistance to cracking, ensuring reliable bonding and durability under thermal cycling conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576413000001
    Figure 0007576413000001
  • Figure 0007576413000002
    Figure 0007576413000002
  • Figure 0007576413000003
    Figure 0007576413000003
Patent Text Reader

Abstract

To provide a joint body that has higher strength and is not easily damaged by a crack of a joint layer, representing a plurality samples produced under the same condition.SOLUTION: The joint body comprises a ceramic member comprising a power receiving electrode including ceramic, a conductive metal terminal, and a stress relaxation section which is disposed between the ceramic member and the metal terminal, is jointed to the power receiving electrode via a first brazing material, and is jointed to the metal terminal via a second brazing material. The first brazing material has tensile strength of 100 MPa or higher and the second brazing material has Young's Modulus of 150 GPa or lower.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a bonded body and a substrate holding member. [Background technology]

[0002] A bonded body is known that is used in manufacturing semiconductors and has a conductive pad to which a power supply terminal for supplying power from the outside is connected to an electrode of an internally provided heater or the like (see, for example, Patent Document 1). A wafer support member as a bonded body described in Patent Document 1 has a power supply terminal coated with an Au-Ni based brazing material. Patent Document 2 describes a wafer mounting device that includes a bonded body. In Reference 2, an electrode and a power supply rod provided in the wafer mounting device are bonded via an Au-Ni brazing bonding layer. Patent Document 3 describes a structure in which a ceramic member and a metal bonding member are bonded by a bonding layer containing an active metal such as titanium. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-49217 A [Patent Document 2] JP 2017-183329 A [Patent Document 3] Japanese Patent Application Publication No. 11-12053 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the Au-Ni brazing material has poor wettability with ceramics. Therefore, as in Patent Documents 1 and 2, when an Au-Ni brazing material is used for the bonding layer, gaps may occur at the bonding portion with the surface conductive pad containing ceramics, and the bonding strength may be weakened. In addition, as described in Patent Document 3, when a brazing material with a high Young's modulus containing an active metal is used for the bonding layer, the bonding layer becomes brittle, so that cracks may occur in the bonding layer during use in a thermal cycle, and the cracks may extend and damage the bonded body. Therefore, a bonded body that is stronger and has less damage to the bonded body due to cracks in the bonding layer in multiple samples manufactured under the same conditions has been desired.

[0005] The present invention has been made to solve the above-mentioned problems, and has an object to provide a bonded body which has higher strength and is less susceptible to damage caused by cracks in the bonding layer. [Means for solving the problem]

[0006] The present invention has been made to solve the above-mentioned problems, and can be realized in the following form: A bonded body, comprising: a ceramic member having a power receiving electrode including ceramics, a metal terminal having electrical conductivity, and a stress relaxation part disposed between the ceramic member and the metal terminal, the stress relaxation part being bonded to the power receiving electrode via a first brazing material and being bonded to the metal terminal via a second brazing material, the first brazing material being mainly composed of nickel (Ni) and having a tensile strength of 100 MPa or more, the second brazing material being mainly composed of gold (Au) and having a Young's modulus of 100 MPa or more, Over 90GPa The present invention can also be realized in the following forms:

[0007] (1) According to one aspect of the present invention, there is provided a joined body comprising: a ceramic member having a power receiving electrode containing ceramics, a metal terminal having electrical conductivity, and a stress relaxation part disposed between the ceramic member and the metal terminal, the stress relaxation part being joined to the power receiving electrode via a first brazing material and being joined to the metal terminal via a second brazing material, the first brazing material having a tensile strength of 100 MPa or more, and the second brazing material having a Young's modulus of 150 GPa or less.

[0008] According to this configuration, the stress relaxation portion is inserted between the power receiving electrode and the metal terminal, so that the thermal stress caused by the difference in thermal expansion coefficient due to the difference in the material between the power receiving electrode and the metal terminal can be attenuated. In addition, since the power receiving electrode has a ceramic material, the first brazing material for bonding the power receiving electrode and the stress relaxation portion may cause a gap in the bonding portion between the power receiving electrode and the stress relaxation portion if the first brazing material has poor wettability with the ceramic member. If a gap occurs in the bonding portion, the ceramic member and the stress relaxation portion may not be bonded sufficiently, and sufficient bonding strength may not be obtained. In this regard, according to the bonded body of this configuration, the tensile strength of the first brazing material is 100 MPa or more, so that sufficient strength is obtained for bonding the power receiving electrode and the stress relaxation portion. In addition, if a brazing material with a high Young's modulus is used as the bonding material between the stress relaxation portion and the metal terminal, the difference in the thermal expansion coefficient between the stress relaxation portion and the metal terminal may cause cracks to occur in the bonding material between the stress relaxation portion and the metal terminal during a thermal cycle, which may damage the bonded body. In this regard, in the joint of the present configuration, since the Young's modulus of the second brazing filler metal is 150 GPa or less, the occurrence and extension of cracks in the joint material between the stress relaxation portion and the metal terminal during thermal cycles can be suppressed. In other words, this configuration provides a joint that has higher strength and is less susceptible to damage to the joint caused by cracks in the second brazing filler metal.

[0009] (2) In the joined body of the above aspect, the second brazing material may have a Young's modulus of 90 GPa or more. If the Young's modulus of the second brazing filler metal is too low, the second brazing filler metal is likely to deform and the tensile strength may decrease. In this regard, according to the joint of the present configuration, since the Young's modulus of the second brazing filler metal is 90 GPa or more, the joint can have a higher tensile strength.

[0010] (3) In the bonded body of the above aspect, the first brazing filler metal may be mainly composed of nickel (Ni). According to this configuration, the first brazing filler metal has higher strength because it is mainly composed of Ni, which makes it possible to provide a bonded body having higher tensile strength and to suppress the occurrence and propagation of cracks during brazing and thermal cycling.

[0011] (4) In the bonded body of the above aspect, the first brazing filler metal may contain phosphorus (P). According to this configuration, the liquid phase appearance temperature of the first brazing filler metal is lowered by containing P. Therefore, in manufacturing the bonded body, the power receiving electrode and the stress relaxation portion can be bonded at a lower temperature, making it easier to manufacture the bonded body.

[0012] (5) In the bonded body of the above aspect, the first brazing filler metal may contain chromium (Cr). According to this configuration, the first brazing filler metal contains Cr, which improves the strength and high-temperature oxidation resistance of the first brazing filler metal, thereby making it possible to prevent the metal terminal from coming off when the bonded body is left in the air for a long period of time.

[0013] (6) In the bonded body of the above aspect, the second brazing filler metal may be mainly composed of gold (Au). According to this configuration, since the second brazing filler metal contains Au, the Young's modulus of the second brazing filler metal is low and the second brazing filler metal has flexibility and therefore has crack resistance.

[0014] (7) In the bonded body of the above aspect, the second brazing filler metal may contain nickel (Ni). According to this configuration, since the second brazing filler metal contains Ni, the liquid phase appearance temperature is lower than that of a second brazing filler metal that does not contain Ni. In this way, the liquid phase appearance temperature of the second brazing filler metal is lowered, so that bonding with the first brazing filler metal and bonding with the second brazing filler metal can be performed simultaneously, and therefore the bonded body can be manufactured more easily.

[0015] The present invention can be realized in various forms, for example, in the form of a bonded body, a substrate holding device, a semiconductor manufacturing apparatus, a ceramic heater, parts including these, and methods for manufacturing these. [Brief description of the drawings]

[0016] [Figure 1] 1 is a schematic cross-sectional view of a substrate holding member including a bonded body according to an embodiment of the present invention. [Diagram 2] 10 is an explanatory diagram of the joining between the power receiving electrode and the second power feed rod. FIG. [Diagram 3] FIG. 2 is an explanatory diagram of the physical properties of examples 1 to 6 and comparative examples 1 to 5 of joined bodies in which the first brazing filler metal and the second brazing filler metal are different. [Figure 4] 1 is a flowchart of a method for producing a bonded body. [Diagram 5] 4 is a flowchart of a method for manufacturing a ceramic member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] <Embodiment> 1 is a schematic cross-sectional view of a substrate holding member 100 including a bonded body 10 according to an embodiment of the present invention. The substrate holding member 100 is a part of a semiconductor manufacturing apparatus that performs plasma etching, ion implantation, electron beam exposure, etc. The substrate holding member 100 holds, corrects flatness, transports, etc. a semiconductor wafer W (hereinafter, also simply referred to as "wafer W"), and is used as a heating device that heats the wafer W to a predetermined temperature.

[0018] 1, the substrate holding member 100 includes a bonded body 10 that holds a wafer W on a mounting surface 10F, and a hollow shaft 20 that is connected to the opposite side of the mounting surface 10F of the bonded body 10. The bonded body 10 includes a ceramic member 11 having a power receiving electrode (not shown in FIG. 1) containing ceramics, a resistance heating element 13 disposed in the ceramic member 11, and a conductive second power supply rod (metal terminal) 15 for supplying power to the power receiving electrode.

[0019] The ceramic member 11 is formed of ceramics such as alumina, aluminum nitride, YAG, silicon nitride, silicon carbide, magnesium oxide, zirconium oxide, yttria, spinel, mullite, calcium titanate, and barium titanate. The power receiving electrode is formed of W (tungsten) and ceramics. The resistance heating element 13 is supplied with power through a via conductor (not shown in FIG. 1), the power receiving electrode, and a second power supply rod 15, and functions as a heater electrode for heating the wafer W held by the bonded body 10. The resistance heating elements 13, which are shown divided in FIG. 1, are electrically connected in series. Note that the rectangular resistance heating element 13 shown in FIG. 1 is shown in a simplified form.

[0020] The second power supply rod 15 is disposed in the shaft 20, one end of which is connected to the resistance heating element 13, and the other end of which is connected to a heater power source (not shown). Although the details of the connection between the second power supply rod 15 and the resistance heating element 13 are not shown in Fig. 1, the details of the connection will be described with reference to Fig. 2 together with the shapes of the power receiving electrode and the via conductor.

[0021] FIG. 2 is an explanatory diagram of the joining of the power receiving electrode 12 and the second power supply rod 15. FIG. 2 is a schematic cross-sectional view in which the X1 portion of FIG. 1 is enlarged. As shown in FIG. 2, the joined body 10 includes the power receiving electrode 12, a via conductor 14 electrically connecting the power receiving electrode 12 and the resistance heating body 13, and a stress relaxation portion 16 disposed between the ceramic member 11 and the second power supply rod 15. The stress relaxation portion 16 electrically connects the ceramic member 11 and the second power supply rod 15. As shown in FIG. 2, the stress relaxation portion 16 is joined to the power receiving electrode 12 via a first brazing material 17 and is joined to the second power supply rod 15 via a second brazing material 18. Note that in FIG. 2, the resistance heating body 13 is omitted from illustration, and a part of the via conductor 14 on the side of the resistance heating body 13 is omitted from illustration.

[0022] The stress relaxation portion 16 of this embodiment is a tungsten-based sintered alloy containing W as a main component and at least one of Ni (nickel), iron, and copper as a binder phase. As shown in Fig. 2, a part of the stress relaxation portion 16 is inserted into a recess 11M formed in the ceramic member 11 so as to be recessed. The cross section of the recess 11M and the stress relaxation portion 16 with respect to the central axis OL is substantially circular. Since the cross section of the stress relaxation portion 16 is smaller than the cross section of the recess 11M, a gap is formed between the side surface 16S of the stress relaxation portion 16 and the recess 11M.

[0023] The power receiving electrode 12 is partially exposed in the recess 11M, and is joined to the stress relief portion 16 by a first brazing material 17. Meanwhile, the stress relief portion 16 is joined to the second power supply rod 15 by a second brazing material 18 on a surface opposite to the first brazing material 17 along the central axis OL. The second power supply rod 15 in this embodiment is made of flexible pure nickel.

[0024] The first brazing filler metal 17 of this embodiment is made of a material having a tensile strength of 100 MPa or more. The second brazing filler metal 18 of this embodiment is made of a material having a Young's modulus of 150 GPa or less. The first brazing filler metal 17 and the second brazing filler metal 18 have oxidation resistance.

[0025] FIG. 3 is an explanatory diagram of the physical properties of the joined body 10 in Examples 1 to 6 and Comparative Examples 1 to 5, in which the first brazing filler metal 17 and the second brazing filler metal 18 are different. FIG. 3 shows the materials and physical properties of the first brazing filler metal 17 and the second brazing filler metal 18 in Examples 1 to 6 and Comparative Examples 1 to 5, and the evaluation results of the strength test. Specifically, as the materials of the first brazing filler metal 17 and the second brazing filler metal 18, the alloy name standard (MBF-67 (Ni-based amorphous brazing filler metal), MBF-64 (Ni-based amorphous brazing filler metal), BNi-7 (JIS standard), BNi-9 (JIS standard), BAu-4 (JIS standard)) or other description (second brazing filler metal in Example 5 and Comparative Example) is shown. In addition to the materials of the first brazing filler metal 17 and the second brazing filler metal 18, FIG. 3 also shows the main components and contained elements of each material. MBF-67, MBF-64, BNi-7, and BNi-9 are all alloys containing Ni as the main component (50% or more). BAu-4 is an alloy containing Au (gold) as the main component. The second brazing filler metal 18 of Example 5 is a material in which 1 wt. % of Ti (titanium) as an active metal is added to BAu-4. The second brazing filler metal 18 of Comparative Example 3 is Au.

[0026] 3 also shows, as physical properties of the first brazing filler metal 17 and the second brazing filler metal 18, the liquid phase appearance temperature and tensile strength of the first brazing filler metal 17, and the liquid phase appearance temperature and Young's modulus of the second brazing filler metal 18. The liquid phase appearance temperature is the temperature at which a liquid phase begins to appear when the first brazing filler metal 17 or the second brazing filler metal is heated.

[0027] FIG. 3 also shows the evaluation results of strength tests for Examples 1 to 6 and Comparative Examples 1 to 5, including the presence or absence of cracks when the ceramic member 11 and the second power supply rod 15 are joined using the first brazing material 17 and the second brazing material 18, the presence or absence of cracks and their propagation during a thermal cycle test of the joined body 10, the results of a tensile strength test of the joined body 10, and the evaluation results of the oxidation resistance of the joined body 10 when it was left in the air.

[0028] Regarding the occurrence of cracks during brazing, among multiple samples manufactured under the same conditions, samples with no cracks were judged as "○", samples with a crack occurrence rate higher than 0% and less than 50% were judged as "△", and samples with a crack occurrence rate of 50% or more were judged as "X".

[0029] In the thermal cycle test for the joint 10, the temperature was raised and lowered from room temperature (25°C) to 700°C 300 times in a nitrogen atmosphere. The occurrence of cracks was checked every predetermined number of times (for example, 50 cycles), and the propagation of the cracks was judged based on whether or not the confirmed cracks had propagated. The evaluation of the occurrence of cracks during the thermal cycle test was the same as that during brazing. Regarding the evaluation of the propagation of cracks, samples in which the propagation of the confirmed cracks was less than 20% were evaluated as "○", and samples in which the propagation of the cracks was 20% or more were evaluated as "×". Note that, since the occurrence of cracks was not confirmed in the samples of Examples 1 to 5, the propagation of the cracks was indicated as "-".

[0030] In the evaluation of the tensile strength test, a tensile test was performed on the brazed samples along the central axis OL, which is the longitudinal direction of the second power supply rod 15. A sample in which the bond between the first brazing material 17 and the second brazing material 18 did not come apart even when a load of 20 kgf was applied was judged as "○", and a sample in which the bond came apart in even one of the multiple samples was judged as "×".

[0031] In the evaluation of the oxidation resistance test, among multiple samples that were left in the atmosphere at 550°C for 1,000 hours, the joined bodies 10 in which the second power feed rod 15 did not come off in any of the samples were judged as "○", the joined bodies 10 in which the second power feed rod 15 came off in some of the multiple samples were judged as "△", and the joined bodies 10 in which the second power feed rod 15 came off in all evaluated samples were judged as "×".

[0032] 3, the first brazing filler metal 17 used in each of the joined bodies 10 in Examples 1 to 6 has a tensile strength of 110 MPa or more, and the second brazing filler metal 18 has a Young's modulus of 150 GPa or less. On the other hand, each of the joined bodies in Comparative Examples 1 to 6 satisfies at least one of the conditions that the first brazing filler metal 17 has a tensile strength of less than 110 MPa and the second brazing filler metal 18 has a Young's modulus of more than 150 GPa.

[0033] As shown in FIG. 3, in the joined bodies 10 of Examples 1 to 5, no cracks were generated in any of the samples, and the results of the tensile strength test were also good. Furthermore, the results of the evaluation of the oxidation resistance of Examples 1 to 3 and Example 5 were also good. In Example 6, no cracks were generated during brazing, and although cracks were generated during the thermal cycle, the cracks did not propagate. Furthermore, the results of the tensile strength test of Example 6 were also good. Furthermore, the results of the evaluation of the oxidation resistance of Example 6 were also good.

[0034] Comparative Examples 1 to 5 satisfy at least one of the conditions that the tensile strength of the first brazing filler metal 17 is less than 100 MPa and the Young's modulus of the second brazing filler metal 18 is higher than 150 GPa. As a result, in the sample of Comparative Example 2, there is a sample in which a crack occurs during brazing. In addition, in the thermal cycle test, cracks occur in 50% or more of the samples of Comparative Examples 1, 2, and 4, and among them, in Comparative Examples 2 and 4, the cracks that occurred extend by 20% or more. In addition, in the tensile strength test, the first brazing filler metal 17 or the second brazing filler metal 18 is disengaged in the samples of Comparative Examples 2, 3, and 5. Furthermore, in the oxidation resistance test, the second power feed rod 15 is disengaged in 50% or more of the samples of Comparative Examples 1, 4, and 5.

[0035] Fig. 4 is a flowchart of a method for manufacturing the joined body 10. In the manufacturing flow of the joined body 10 shown in Fig. 4, first, the ceramic member 11 having the power receiving electrode 12 is manufactured (step S10). Next, the power receiving electrode 12 in the manufactured ceramic member 11 and the second power feed rod 15 are joined (step S20) to manufacture the joined body 10.

[0036] 5 is a flowchart of a method for manufacturing the ceramic member 11. As shown in FIG. 5, in the manufacturing flow of the ceramic member 11, first, a slurry for a green sheet that is the base of the ceramic member 11 is prepared (step S11). In this embodiment, a mixture of 100 parts by weight of aluminum nitride (AlN) powder and yttrium oxide (Y 2 O 3 An organic solvent (e.g., toluene) is added to a mixture of 0.5 parts by weight of (yttria) powder, 20 parts by weight of an acrylic binder, and an appropriate amount of a dispersant and plasticizer. The mixture is mixed in a ball mill for 20 hours to produce a slurry for the green sheet.

[0037] The slurry is cast onto a sheet by a casting device and dried to produce a green sheet (step S12). An electrode paste is printed into through holes provided in the produced green sheet to form via conductors 14 in the green sheet (step S13).

[0038] On the green sheet on which the via conductors 14 are formed, a power receiving electrode 12 having an electrode pattern such as a heater or a distributor is formed (step S14). The power receiving electrode 12 is formed by printing a metallization layer and printing vias after providing through holes. The paste used for printing the metallization layer is, for example, a paste made by mixing powder of W or Mo, aluminum nitride powder, an acrylic binder, and an organic solvent such as terpineol. The amount of aluminum nitride powder mixed into the paste is adjusted according to the amount of W and Mo.

[0039] A green sheet laminate (e.g., 8 mm thick) is produced by stacking a plurality of (e.g., 20) green sheets on which the power-receiving electrode 12 is formed (step S15). The green sheet laminate is produced by pressing a plurality of green sheets together and cutting the periphery as necessary. The green sheet laminate is cut at the periphery by machining to produce a disk-shaped compact.

[0040] The produced laminate of green bodies is degreased at a temperature in the range of 450° C. to 600° C., and then fired (step S16). In this way, the ceramic member 11 having the power-receiving electrode 12 is produced, and the manufacturing flow of the ceramic member 11 is completed.

[0041] 4, a first brazing filler metal 17 (e.g., MBF-67) is sandwiched between the power receiving electrode 12 and the stress relaxation portion 16 of the fabricated ceramic member 11, and a second brazing filler metal 18 (e.g., BAu-4) is sandwiched between the stress relaxation portion 16 and the second power feed rod 15, and then the resulting members are heated to be joined by brazing (step S20). Heating conditions include, for example, heating in a vacuum at 950°C to 1150°C for 10 minutes to 30 minutes.

[0042] Instead of sandwiching a brazing material between the power receiving electrode 12 and the stress relief portion 16 and between the stress relief portion 16 and the second power feed rod 15, a brazing material paste may be applied. The first brazing material 17 and the second brazing material 18 may not be brazed under the same heating conditions. For example, the first brazing material 17 may be brazed, and then the second brazing material 18 may be brazed under different heating conditions. In the brazing joint of Example 5 shown in FIG. 3, the stress relief portion 16 and the second power feed rod 15 are brazed in the first stage, and then the power receiving electrode 12 and the stress relief portion 16 are brazed in the second stage at a temperature lower than that in the first stage. In the brazing joint of Example 6, the power receiving electrode 12 and the stress relief portion 16 are brazed in the first stage, and then the stress relief portion 16 and the second power feed rod 15 are brazed in the second stage at a temperature lower than that in the first stage.

[0043] As described above, the joined body 10 of the present embodiment includes the stress relaxation portion 16 disposed between the ceramic member 11 and the second power feed rod 15. The stress relaxation portion 16 is joined to the power receiving electrode 12 of the ceramic member 11 via the first brazing material 17, and is joined to the second power feed rod 15 via the second brazing material 18. By fitting the stress relaxation portion 16 between the power receiving electrode 12 and the second power feed rod 15, it is possible to attenuate thermal stress caused by a difference in thermal expansion coefficient resulting from a difference in material between the power receiving electrode 12 with low thermal expansion and the second power feed rod 15 with high thermal expansion. In addition, the first brazing material 17 joining the surface electrode 12 and the stress relaxation portion 16 contains ceramics that coexist with the power receiving electrode 12. Therefore, if the first brazing material 17 has poor wettability with respect to the ceramic member 11, a gap may be generated at the joining portion between the power receiving electrode 12 and the stress relaxation portion 16. If a gap occurs at the joint, the ceramic member 11 and the stress relaxation portion 16 may not be sufficiently joined, and sufficient joint strength may not be obtained. In contrast, since the tensile strength of the first brazing filler metal 17 of this embodiment is 100 MPa or more, sufficient strength is obtained for the joint between the power receiving electrode 12 and the stress relaxation portion 16. In addition, if a brazing filler metal with a high Young's modulus is used for the joint between the stress relaxation portion 16 and the second power feed rod 15, as shown in Comparative Examples 1, 2, and 4 in FIG. 3, due to the difference in thermal expansion between the stress relaxation portion 16 and the second power feed rod 15, cracks may occur in the brazing filler metal during a heat cycle test, causing damage to the joint 10. In contrast, since the Young's modulus of the second brazing filler metal 18 of this embodiment is 150 GPa or less, the occurrence and extension of cracks in the brazing filler metal during a heat cycle test can be suppressed, as shown in Examples 1 to 6 in FIG. 3. That is, according to this embodiment, a joint 10 with higher strength and less damage due to cracks in the second brazing filler metal 18 can be provided.

[0044] Furthermore, if the Young's modulus of the second brazing filler metal 18 is too low, the second brazing filler metal 18 may be easily deformed and the tensile strength may decrease, as in Comparative Example 3 shown in Fig. 3. In contrast, the Young's modulus of the second brazing filler metal 18 of this embodiment is 110 MPa (>90 MPa) or more, as shown in Examples 1 to 6. Therefore, the joined body 10 of this embodiment can have a higher tensile strength.

[0045] In addition, the first brazing filler metal 17 in Examples 1 to 6 has higher strength because it contains Ni as a main component. As a result, the joined body 10 of the present embodiment has higher tensile strength and can suppress the occurrence and propagation of cracks in the joined body 10 during brazing and thermal cycle testing.

[0046] Furthermore, since the material (MBF-67, MBF-64, BNi-7) of the first brazing filler metal 17 in Examples 1 to 5 contains P (phosphorus), the liquid phase appearance temperature of the first brazing filler metal 17 decreases. Therefore, in manufacturing the joined body 10 in Examples 1 to 5, the power receiving electrode 12 and the stress relaxation portion 16 can be joined at a lower temperature, making it easier to manufacture the joined body 10.

[0047] Furthermore, since the materials (MBF-67, MBF-64, BNi-7, BNi-9) of the first brazing filler metal 17 in Examples 1 to 6 contain Cr (chromium), the strength and high-temperature oxidation resistance of the first brazing filler metal 17 are improved. Therefore, the joined body 10 of the present embodiment can suppress the second power feed rod 15 from coming off when left in the air for a long period of time.

[0048] Furthermore, the second brazing filler metal 18 in Examples 1 to 6 is mainly composed of Au, and therefore has a low Young's modulus and is flexible, resulting in the bonded body 10 of the present embodiment having crack resistance.

[0049] Furthermore, the second brazing filler metal 18 of Examples 1 to 4, which is mainly composed of Au, contains Ni, and therefore has a lower liquid phase appearance temperature than the second brazing filler metal of Comparative Example 3, which does not contain Ni. In this way, the lower liquid phase appearance temperature of the second brazing filler metal 18 makes it possible to perform bonding with the first brazing filler metal 17 and bonding with the second brazing filler metal 18, and therefore the bonded body 10 can be manufactured more easily.

[0050] <Modifications of this embodiment> The present invention is not limited to the above-described embodiment, and can be embodied in various forms without departing from the spirit and scope of the invention. For example, the following modifications are also possible.

[0051] Although an example of the bonded body 10 has been described in the above embodiment, the bonded body 10 includes the stress relaxation portion 16 disposed between the ceramic member 11 and the second power supply rod 15, and can be deformed in various ways within a range in which the tensile strength of the first brazing filler metal 17 is 100 MPa or more and the Young's modulus of the second brazing filler metal 18 is 150 GPa or less. For example, the shapes and materials of the ceramic member 11, the second power supply rod 15, the stress relaxation portion 16, the first brazing filler metal 17, and the second brazing filler metal 18 can be deformed. The mounting surface 10F of the bonded body 10 may be processed so as to easily hold the wafer W.

[0052] The parameters of Examples 1 to 6 shown in FIG. 3 are examples of the joined body 10. For example, the material of the first brazing filler metal 17 can be deformed in a range of tensile strength of 100 MPa or more. The material of the second brazing filler metal 18 can be deformed in a range of Young's modulus of 150 GPa or less. Among Examples 1 to 6, in Example 2 in which the tensile strength of the first brazing filler metal 17 is the smallest, the tensile strength is 110 MPa, but the tensile strength of the first brazing filler metal 17 of the modified example may be, for example, 100 MPa. Among Examples 1 to 6, in Example 5 in which the Young's modulus of the second brazing filler metal 18 is the largest, the Young's modulus is 130 MPa, but the Young's modulus of the second brazing filler metal 18 of the modified example may be, for example, 150 GPa. The Young's modulus of the second brazing filler metal 18 is more preferably 130 GPa or less. The Young's modulus of the second brazing filler metal 18 is more preferably 90 GPa or more.

[0053] The second power supply rod 15 may be made of an iron-nickel-cobalt alloy (Kovar: registered trademark) having low thermal expansion, or may be made of nickel-phosphorus-plated copper. When the second power supply rod 15 is made of nickel-phosphorus-plated copper, it has low resistance, is non-magnetic, has flexibility and oxidation resistance, and promotes wetting. Pure copper may also be used as the material for the second power supply rod 15.

[0054] At least one of the first brazing filler metal 17 and the second brazing filler metal 18 may extend around the side surface 16S of the stress relief portion 16 in addition to the cross section relative to the central axis OL, or may be joined to a part of the cross section. The joint portion formed by the first brazing filler metal 17 and the second brazing filler metal 18 may vary depending on the shape of the stress relief portion 16, etc. For example, the power receiving electrode 12 may be formed so that a part of it is exposed on the surface of the plate-shaped ceramic member 11 without being formed in the recess 11M. The cross sections of the stress relief portion 16 and the second power supply rod 15 do not have to be circular, and may be rectangular, or one may be rectangular and the other may be circular.

[0055] The substrate holding member 100 including the bonded body 10 can be modified in various ways as long as it includes the bonded body 10. For example, the substrate holding member 100 does not have to include the shaft 20.

[0056] Although the present aspect has been described above based on the embodiment and modified examples, the above-mentioned embodiment of the aspect is intended to facilitate understanding of the present aspect and does not limit the present aspect. The present aspect may be modified or improved without departing from the spirit and scope of the claims, and equivalents are included in the present aspect. Furthermore, if a technical feature is not described as essential in this specification, it may be deleted as appropriate. [Explanation of symbols]

[0057] 10...Zygote 10F…Placement surface 11...Ceramics components 11M…Concave 12...Receiving electrode 13...Resistance heating element 14…Via conductor 15...Second power supply rod (metal terminal) 16…Stress relief section 16S…Side of stress relief section 17…First brazing material 18…Second brazing material 20…Shaft 100...Substrate holding member OL…center axis W: Wafer

Claims

1. A conjugate comprising: a ceramic member having a power receiving electrode including ceramics; A metal terminal having electrical conductivity; a stress relaxation portion disposed between the ceramic member and the metal terminal, the stress relaxation portion being joined to the power receiving electrode via a first brazing material and joined to the metal terminal via a second brazing material; Equipped with The first brazing material is mainly composed of nickel (Ni) and has a tensile strength of 100 MPa or more; The second brazing material is characterized in that it is mainly composed of gold (Au) and has a Young's modulus of 90 GPa or more and 150 GPa or less.

2. The joint body according to claim 1 , The joint body, wherein the first brazing material contains phosphorus (P).

3. The joint body according to claim 2, A joint body, characterized in that the first brazing material contains chromium (Cr).

4. The joint body according to claim 1 , A joint body, characterized in that the second brazing material contains nickel (Ni).

5. A substrate holding member comprising the bonded body according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Structure of bonding ceramic and metal

    JP1986127675A

  • Adhesion between ceramics and metal

    JP1991037166A

  • Cr3c2 ceramic-metal joined body and its joining method

    JP1991088782A

  • Bonded structure of ceramic and its production

    JP1999012053A

  • Wafer holding member

    JP2000049217A