Light emitting device and method for manufacturing the same
The use of a single crystal silicon substrate with thermal oxide film and glass frit layer, along with controlled AuSn bonding, addresses the deterioration and misalignment issues in AlGaN LEDs, enhancing the reliability and efficiency of ultraviolet light emitting devices.
Patent Information
- Application Number
- JP2020145631
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Aluminum gallium nitride (AlGaN) LEDs used in ultraviolet light emitting devices are susceptible to deterioration due to oxygen or hydrogen from water or hydrocarbons, and existing hermetic sealing methods using AuSn eutectic bonding can lead to manufacturing defects such as misalignment during the second melting step.
A light emitting device with a substrate made of single crystal silicon, featuring a thermal oxide film and a glass frit layer, where the AuSn bonding is limited to the light emitting element, and the glass frit layer is bonded using a laser to prevent remelting, combined with a lattice-patterned through electrodes to enhance stability and hermetic sealing.
The solution effectively prevents manufacturing defects by maintaining the position of the light emitting element and ensuring high airtightness, reducing voids and cracks, while improving manufacturing efficiency and reducing costs.
Smart Images

Figure 0007576415000001 
Figure 0007576415000002 
Figure 0007576415000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a light emitting device and a method for manufacturing a light emitting device. [Background technology]
[0002] 2. Description of the Related Art In recent years, light emitting devices that use semiconductor light emitting elements such as ultraviolet light emitting diodes (LEDs) as light sources have become widespread as light emitting devices that irradiate ultraviolet light.
[0003] For example, Patent Document 1 discloses a light emitting device that emits ultraviolet light, in which an ultraviolet light emitting element made of aluminum gallium nitride (AlGaN) is placed on a mounting substrate and the ultraviolet light emitting element is hermetically sealed on the mounting substrate with a cap made of a spacer and a cover. In the light emitting device disclosed in Patent Document 1, the cap is formed by bonding a glass cover and a silicon spacer by anodic bonding, and the cap and the mounting substrate made of aluminum nitride (AlN) are eutectic bonded with a bonding layer made of gold-tin (AuSn), thereby hermetically sealing the ultraviolet light emitting element. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-127249 A Summary of the Invention [Problem to be solved by the invention]
[0005] Aluminum gallium nitride (AlGaN), which is generally used as a material for LEDs that emit ultraviolet light, particularly deep ultraviolet light of 280 nm or less, is prone to degradation such as high resistance due to oxygen or hydrogen derived from water or hydrocarbons. Therefore, in a light-emitting device using an LED element made of aluminum gallium nitride as a material, such as that described in Patent Document 1, it is important to hermetically seal the LED element with an inert gas or the like.
[0006] However, in the light emitting device disclosed in Patent Document 1, eutectic bonding is performed by melting AuSn twice, when the ultraviolet light emitting element is mounted on the mounting substrate and when the cap is mounted on the mounting substrate. As a result, when AuSn is melted for the second time when the cap is mounted for hermetic sealing, the AuSn that was eutecticized to bond the ultraviolet light emitting element when the element was mounted may remelt, resulting in manufacturing defects such as misalignment of the ultraviolet light emitting element.
[0007] The present invention has been made in consideration of the above-mentioned points, and has an object to provide a light emitting device capable of hermetically sealing an ultraviolet light emitting element and suppressing manufacturing defects, and a manufacturing method thereof. [Means for solving the problem]
[0008] The light emitting device of the present invention includes a substrate made of single crystal silicon having an upper surface on which a thermal oxide film is formed and a recess formed in the upper surface, a light emitting element placed on the bottom surface of the recess, and a light transmissive member made of glass having a glass frit layer on its lower surface and bonded to the upper surface of the substrate via the glass frit layer, and is characterized in that at the bonding portion between the substrate and the glass frit layer, the thermal oxide film and a reaction layer between the thermal oxide film and the glass frit layer are formed in that order from the surface of the substrate between the substrate and the glass frit layer.
[0009] Furthermore, a method for manufacturing a light emitting device according to the present invention includes the steps of: preparing a composite substrate having a first substrate made of single crystal silicon, an oxide film made of silicon oxide formed on the first substrate, and a second substrate made of single crystal silicon bonded to the first substrate via the oxide film, the composite substrate having a plurality of element mounting regions on an upper surface of the composite substrate defined by lattice-shaped parting lines; a hole forming step of forming a plurality of columnar holes extending from a lower surface of the composite substrate to the oxide film in one region of each of the plurality of element mounting regions in each of the plurality of element mounting regions; a recess forming step of forming each of a plurality of concave recesses on the upper surface of the composite substrate in each of the plurality of element mounting regions, the concave recesses extending from the upper surface of the composite substrate to the oxide film and having a region including the one region as a bottom surface thereof; and removing the oxide film exposed on the bottom surface of each of the plurality of recesses to form a plurality of holes and a plurality of recesses. a thermal oxide film forming process for forming a thermal oxide film having a thickness of 0.8 μm to 1.2 μm on the lower surface of the composite substrate, the upper surface of the composite substrate, and the inner surface of each of the plurality of holes; a through electrode forming process for forming a columnar through electrode by electrolytic plating so as to fill the inside of each of the plurality of holes; a die bonding process for mounting a light-emitting element on the bottom surface of each of the plurality of recesses; a light-transmitting member bonding process for placing a light-transmitting member made of glass having a frit glass layer on one surface facing the upper surface of the composite substrate on the upper surface of the composite substrate so as to cover each of the plurality of recesses, and scanning a laser from above along the periphery of each of the plurality of recesses on the frit glass layer to bond the light-transmitting member to the upper surface of the composite substrate; and a dicing process for cutting the composite substrate along the parting lines of the composite substrate to individual pieces.
[0010] Furthermore, a method for manufacturing a light emitting device according to the present invention includes the steps of: preparing a substrate made of single crystal silicon and having an element mounting region with a recess; a thermal oxide film forming step of forming a thermal oxide film on an upper surface of the substrate; a die bonding step of mounting a light emitting element in the recess; and a light transmissive member joining step of arranging a light transmissive member made of glass having a frit glass layer on the upper surface of the substrate so as to cover the recess with the frit glass layer side facing the upper surface of the substrate, melting the frit glass layer, and joining the light transmissive member to the upper surface of the substrate, wherein in the light transmissive member joining step, the thermal oxide film and the frit glass layer mutually diffuse, so that at the joint between the substrate and the frit glass layer, the thermal oxide film, an interdiffusion layer in which the thermal oxide film and the frit glass layer are mutually diffused, and the frit glass layer are stacked in this order from the upper surface of the substrate. [Brief description of the drawings]
[0011] [Figure 1] 1 is a top view of a light emitting device according to a first embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention. [Diagram 3] 2 is an enlarged view of an element mounting surface of the light emitting device according to the first embodiment of the present invention. [Figure 4] 3 is an enlarged cross-sectional view of a bonding region between a composite substrate and frit glass in the light-emitting device according to Example 1 of the present invention. FIG. [Diagram 5] 5 is a diagram showing a manufacturing flow of the light emitting device according to the first embodiment of the present invention. [Figure 6] 5 is a diagram showing a manufacturing flow of the light emitting device according to the first embodiment of the present invention. [Figure 7] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 8] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 9] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 10]1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 11] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 12] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 13] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 14] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 15] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 16] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 17] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 18] 1 is a cross-sectional view of a light emitting device according to a first embodiment of the present invention at one step during manufacturing. [Figure 19] FIG. 5 is a cross-sectional view of a light emitting device according to a second embodiment of the present invention. [Figure 20] 6 is a diagram showing a manufacturing flow of the light emitting device according to Example 2 of the present invention. [Figure 21] 10 is a cross-sectional view of a light emitting device according to a second embodiment of the present invention at one step during manufacturing. [Figure 22] 10 is a cross-sectional view of a light emitting device according to a second embodiment of the present invention at one step during manufacturing. [Figure 23] FIG. 11 is a cross-sectional view of a light emitting device according to Example 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following is a detailed description of an embodiment of the present invention. In the following description and the accompanying drawings, the same reference numerals are used for substantially the same or equivalent parts. In the following description, the expression "material 1 / material 2" refers to a laminated structure in which material 2 is laminated on material 1. EXAMPLES
[0013] Fig. 1 shows a top view of a light emitting device 100 according to Example 1. Fig. 2 shows a cross-sectional view of the light emitting device 100 taken along line AA in Fig. 1.
[0014] The light emitting device 100 comprises a composite substrate 10 having a cavity as a recess on its upper surface, a light emitting element 40 mounted on an element mounting surface 13 which is the bottom surface of the cavity of the composite substrate 10, and a light transmissive member 50 formed on the upper surface of the composite substrate 10 so as to cover the cavity of the composite substrate 10. Note that the light transmissive member 50 is omitted in Fig. 1 in order to clarify the structure and positional relationship of each element.
[0015] As shown in FIG. 2, the composite substrate 10 is, for example, an SOI (Silicon On Insulator) substrate having a first substrate 11 made of single crystal silicon (Si) having a (100) crystal plane as its main surface, a buried oxide film (BOX: Buried Oxide) 14 made of silicon oxide (SiO2) formed on the upper surface of the first substrate 11, and a second substrate 12 made of single crystal silicon (Si) having a (100) crystal plane as its main surface and bonded to the upper surface of the first substrate 11 via the buried oxide film 14.
[0016] The first substrate 11 is, for example, a substrate having a thickness of about 50 μm. The second substrate 12 is, for example, a substrate having a thickness of about 250 μm. The buried oxide film 14 has a thickness of, for example, about 1 μm, and bonds the first substrate 11 and the second substrate 12 to each other.
[0017] The opening 15 is formed on the upper surface of the composite substrate 10 so as to penetrate from the upper surface of the second substrate 12 to the upper surface of the first substrate 11. The opening 15 is formed so that the opening surface narrows from the upper surface to the lower surface of the second substrate 12 so that the inner surface of the opening 15 is the (111) crystal plane of the second substrate 12. Specifically, the inner surface of the opening 15 is formed at an angle of about 54.74° with respect to the upper surface of the first substrate 11. That is, the second substrate 12 functions as a side wall of the cavity of the composite substrate 10. In addition, the upper surface of the first substrate 11 exposed from the opening 15 of the second substrate 12 functions as the element mounting surface 13, which is the bottom surface of the cavity.
[0018] As described above, the composite substrate 10 of the light-emitting device 100 is formed by bonding together a first substrate 11 made of plate-shaped single crystal silicon and a second substrate 12 made of single crystal silicon having an opening 15 in the shape of a recess, and a buried oxide film 14 is formed on the surface of the first substrate 11 facing the second substrate 12.
[0019] The plurality of through holes 16 are formed in a columnar shape on the lower surface of the composite substrate 10, penetrating from the lower surface to the upper surface of the first substrate 11. The plurality of through holes 16 are also formed in a predetermined region within the region of the element mounting surface 13, which is the bottom surface of the cavity when viewed from above. The plurality of through holes 16 are also regularly arranged in the predetermined region.
[0020] The thermal oxide film 17 formed on the first substrate 11 is formed on the upper and lower surfaces of the first substrate 11 and on the inner surfaces of the plurality of through holes 16. Similarly to the thermal oxide film 17, the thermal oxide film 18 formed on the second substrate 12 is formed on the upper surface of the second substrate 12 and on the inner surfaces of the openings 15.
[0021] That is, the light emitting device 100 includes a composite substrate 10 made of single crystal silicon having an upper surface on which a thermal oxide film 18 is formed and on which a cavity recessed from the upper surface is formed. Also, a plurality of through holes 16 are formed in the composite substrate 10, which penetrate in a columnar shape from the bottom surface of the cavity to the rear surface of the composite substrate 10 and have inner surfaces covered with a thermal oxide film 17.
[0022] Each of the thermal oxide films 17 and 18 is an oxide film made of SiO2 formed by, for example, performing a thermal oxidation process on the first substrate 11 and the second substrate 12, which are single crystal Si. Each of the thermal oxide films 17 and 18 is formed to a film thickness of, for example, about 1 μm. Each of the thermal oxide films 17 and 18 is preferably formed to a film thickness of 0.8 μm or more and 1.2 μm or less. This is because, if the film thickness of the thermal oxide film 18 at the joint with the translucent member 50 is small, there is a possibility that cracks or the like will occur at the joint between the second substrate 12 and the translucent member 50, as described later. In addition, the film thickness of the thermal oxide film 17 on the inner side surface of the through hole 16 is also preferably configured to be 0.8 μm or more and 1.2 μm or less. Thermal oxide film 17 on the inner surface of through hole 16 needs to be about 0.3 μm thick to ensure insulation, but by configuring it to a thickness of 0.8 μm to 1.2 μm, it is possible to suppress cracks caused by stress in a certain direction due to the plane orientation of first substrate 11, which is single crystal Si. The surface of composite substrate 10 is insulated by thermal oxide films 17 and 18.
[0023] In this embodiment, the light emitting device 100 is in the form of a wafer level package (WLP) in which a plurality of light emitting devices 100 are manufactured in a batch in a continuous grid pattern on a wafer-shaped composite substrate 10. The plurality of light emitting devices 100 manufactured on the wafer are separated into individual pieces by dicing. That is, the outer surface of the light emitting device 100 is a diced cut surface. Therefore, the thermal oxide films 17 and 18 are not formed on the outer surfaces of the first substrate 11 and the second substrate 12. Note that a SiO2 film formed by natural oxidation is formed on the side of the outer end of the composite substrate 10, but the SiO2 film formed by natural oxidation is not shown in this description.
[0024] Further, a plurality of columnar through electrodes 30 are formed in each of the plurality of through holes 16 so as to fill the respective through holes 16. That is, the light emitting device 100 has a plurality of columnar through electrodes 30 filling the plurality of through holes 16.
[0025] The through electrodes 30 are formed, for example, from the lower surface of the composite substrate 10 in the following order: a Cu layer 31, a Ni layer 32, and a gold-tin alloy (hereinafter referred to as AuSn) layer 33 as a metal bonding layer.
[0026] The Cu layer 31 is filled in each of the through holes 16 to a thickness of, for example, about 49 μm from the lower surface of the composite substrate 10. The height of the upper surface of the Cu layer 31 does not reach the height of the upper surface of the element mounting surface 13. The Ni layer 32 is filled in each of the through holes 16 to a thickness of, for example, about 1 μm on the upper surface of the Cu layer 31. The AuSn layer 33 is formed on the upper surface of the Ni layer 32 to a thickness of about 5 μm so as to protrude from the upper surface of the element mounting surface 13. The AuSn layer 33 is formed to have an upper surface shape that follows the upper surface shape of the Ni layer 32. In this embodiment, as shown in FIG. 2, the Ni layer 32 is formed so that the upper surface of the Ni layer 32 and the upper surface of the element mounting surface 13 are at the same height. The AuSn layer 33 has a cross-sectional structure such that the AuSn layer 33 protrudes from the upper surface of the element mounting surface 13.
[0027] The AuSn layer 33 functions as a metal bonding layer that is bonded to a metal electrode formed on the bottom surface of the light emitting element 40 by being heated and melted. The Ni layer 32 functions as a barrier layer that suppresses diffusion and mixing of the Cu layer 31 and the AuSn layer 33 when the AuSn layer 33 is heated and melted. In this embodiment, the upper surface of the Ni layer 32 is at the same height as the upper surface of the element mounting surface 13, but the height position of the upper surface of the Ni layer 32 is not limited thereto. For example, the upper surface of the Ni layer 32 can be formed so as to be located inside the upper surface of the element mounting surface 13. By positioning the upper surface of the Ni layer 32 inside the upper surface of the element mounting surface 13, the bonding stability with the light emitting element can be improved compared to when the upper surface of the Ni layer 32 is located outside the upper surface of the element mounting surface 13. This is because, if the upper surface of the Ni layer 32 is located outside the upper surface of the element mounting surface 13, it may become difficult to ensure the stability of the bond with the light-emitting element, such as by controlling the film thickness of the AuSn layer 33 between the Ni layer 32 and the metal electrode formed on the bottom surface of the light-emitting element 40.
[0028] The AuSn layer 33 protruding from the upper surface of the element mounting surface 13 is regularly arranged, so that regular melting initiation points can be formed in the bonding with the metal electrode formed on the bottom surface of the light emitting element 40. Therefore, compared with a flat AuSn bonding layer without regular protrusions, it is possible to suppress the unintentional formation of voids at random positions, and it is possible to provide a light emitting device 100 with high bonding stability with the light emitting element 40.
[0029] Further, a first external electrode 21 and a second external electrode 22 are formed on the lower surface of the composite substrate 10, spaced apart from each other. Each of the first external electrode 21 and the second external electrode 22 is a metal layer, for example, laminated in the order of titanium (Ti) / copper (Cu) / nickel (Ni) / gold (Au) from the thermal oxide film 17 side of the composite substrate 10. Each of the first external electrode 21 and the second external electrode 22 is formed so as to cover each of the plurality of through electrodes 30 formed on the lower surface of the composite substrate 10. Each of the plurality of through electrodes 30 has a Cu layer 31 electrically contacted with the first external electrode 21 or the second external electrode 22 on the bottom surface. That is, the lower surface side of the light emitting device 100 becomes a mounting surface for a mounting substrate (not shown), and the first external electrode 21 and the second external electrode 22 function as mounting electrodes for the mounting substrate.
[0030] Each of the plurality of through electrodes 30 is formed so as to fill each of the plurality of through holes 16. Also, each of the first external electrode 21 and the second external electrode 22 is formed so as to cover each of the plurality of through electrodes 30 on the lower surface of the composite substrate 10. This makes the cavity of the composite substrate 10 airtight with respect to the lower surface side of the composite substrate 10 via the plurality of through holes 16.
[0031] The light emitting element 40 is placed on the upper surface of the element mounting surface 13. In other words, the light emitting device 100 includes the light emitting element 40 placed on the bottom surface of the cavity. The light emitting element 40 is, for example, a light emitting diode that emits deep ultraviolet light using an aluminum gallium nitride (AlGaN)-based semiconductor layer as a light emitting layer. Specifically, the light emitting element 40 is a light emitting element in which an n-type AlGaN semiconductor layer, an AlGaN active layer, and a p-type AlGaN semiconductor layer are laminated on an aluminum nitride (AlN) substrate, and deep ultraviolet light is emitted from the AlGaN active layer. In this embodiment, an AlN substrate, an n-type AlGaN semiconductor layer, an AlGaN active layer, and a p-type AlGaN semiconductor layer are formed from the upper surface side of the light emitting element 40. The light emitting element 40 is a flip-chip connected light emitting element in which an anode electrode 41 electrically connected to the n-type AlGaN semiconductor layer and a cathode electrode 42 electrically connected to the p-type AlGaN semiconductor layer are formed on the lower surface. The deep ultraviolet light emitted from the AlGaN active layer is transmitted through the AlN substrate and emitted from the upper surface of the light emitting element 40. That is, the upper surface of the light emitting element 40 functions as a light extraction surface, and the lower surface functions as a mounting surface for mounting onto the composite substrate 10.
[0032] The light emitting element 40 is bonded such that each of the anode electrode 41 and the cathode electrode 42 is placed on the upper surface of each of the plurality of through electrodes 30. Specifically, each of the anode electrode 41 and the cathode electrode 42 of the light emitting element 40 is bonded to the AuSn layer 33 of each of the through electrodes 30. In other words, the light emitting element 40 has a pair of element electrodes, the anode electrode 41 and the cathode electrode 42, on a surface facing the bottom surface of the cavity, and the anode electrode 41 and the cathode electrode 42 are bonded to the plurality of through electrodes 30 via the AuSn layer 33. As shown in FIG. 2, the light emitting element 40 has the anode electrode 41 electrically connected to the first external electrode 21 via the through electrode 30, and the cathode electrode 42 electrically connected to the second external electrode 22 via the through electrode 30.
[0033] The light-transmitting member 50 is disposed on the upper surface of the composite substrate 10 via a frit glass layer 60 so as to cover the cavity of the composite substrate 10. In other words, the light-emitting device 100 includes a light-transmitting member 50 made of glass having a frit glass layer 60 on its lower surface and bonded to the upper surface of the composite substrate 10 via the frit glass layer 60. The light-transmitting member 50 is, for example, a deep ultraviolet-transmitting glass whose main material is SiO2 and which transmits deep ultraviolet light emitted from the light-emitting element 40. The thermal expansion coefficient of the light-transmitting member 50 is 3×10 -6 / ℃ or more 5×10 -6 / ° C. or less. The light-transmitting member 50 has a thermal expansion coefficient (3.9×10 -6 / ° C. The light-transmitting member 50 is bonded to the upper surface of the composite substrate 10 via a glass frit layer 60.
[0034] The frit glass layer 60 is made of, for example, a paste containing powdered frit glass. The paste is applied in advance to the surface of the light-transmitting member 50 facing the upper surface of the second substrate 12 so as to surround the periphery of the cavity of the composite substrate 10. The light-transmitting member 50 to which the paste is applied is pre-fired at about 500° C. before being bonded to the composite substrate 10.
[0035] Similarly to the composite substrate 10, the light-transmitting member 50 and the frit glass layer 60 are formed in a continuous lattice pattern on the surface of the wafer-shaped light-transmitting member 50 facing the composite substrate 10. That is, during the manufacture of the light-emitting device 100, the light-transmitting member 50 is bonded via the frit glass layer 60 so as to collectively cover a plurality of cavities formed in a lattice pattern on the composite substrate 10. The light-transmitting member 50 is cut at the same time that the composite substrate 10 is divided into individual pieces.
[0036] The frit glass layer 60 is made of glass mainly made of SiO2. The frit glass layer 60 bonds the light-transmitting member 50 and the second substrate 12 by heating and melting the frit glass layer 60 surrounding the periphery of the cavity of the composite substrate 10. The frit glass layer 60 is melted by heating locally in a short time by a laser described later, thereby bonding the light-transmitting member 50 and the second substrate 12. As a result, the cavity of the composite substrate 10 has a storage space HS hermetically sealed by the light-transmitting member 50 and the frit glass layer 60.
[0037] The housing space HS is filled with a sealing gas that is not altered by ultraviolet light, such as nitrogen (N2) gas.
[0038] As configured above, by using a wafer-shaped composite substrate 10 as the composite substrate 10, the light emitting device 100 can be manufactured as a wafer level package (WLP) in which the light emitting device 100 is formed in a lattice pattern on a wafer. Conventionally, individual substrates made of AlN were used and it was necessary to hermetically seal the substrates one by one, which caused problems in terms of tact time and cost during manufacturing.
[0039] In this embodiment, the light emitting device 100 can be made by forming cavities in a lattice pattern on the wafer-like composite substrate 10, hermetically sealing the entire device with the light-transmitting member 50 having the frit glass layer 60, and then dicing the device into individual pieces. This makes it possible to improve the tact time and cost during manufacturing of the light emitting device 100.
[0040] Furthermore, conventionally, light emitting devices are hermetically sealed twice, once for bonding the light emitting element to the element mounting portion and once for bonding the light transmitting member to the AlN substrate, using AuSn eutectic bonding. During this process, the AuSn bonding the light emitting element may remelt during the second AuSn eutectic bonding when bonding the light transmitting member, which is the hermetic sealing step, resulting in manufacturing defects such as misalignment of the light emitting element.
[0041] In this embodiment, the light emitting device 100 is manufactured such that the only location where eutectic bonding is performed using AuSn is the bonding of the light emitting element 40, and the light transmissive member 50 is locally heated for a short period of time by the laser of the frit glass layer 60. This makes it possible to prevent remelting of the eutectic bonding layer using AuSn between the light emitting element 40 and each of the plurality of through electrodes 30 when bonding the light transmissive member 50 to the composite substrate 10. Therefore, the light emitting device 100 can prevent manufacturing defects such as misalignment of the placement of the light emitting element due to remelting of AuSn during manufacturing.
[0042] Fig. 3 is an enlarged view of the upper surface of the element mounting surface 13, showing the structure of the plurality of through electrodes 30 of the light emitting device 100 according to Example 1. In Fig. 3, the light emitting element 40, the anode electrode 41, and the cathode electrode 42 are shown by dashed lines in order to clarify the structure and positional relationship of the plurality of through electrodes 30.
[0043] 3, the plurality of through electrodes 30 are formed in a region where the anode electrode 41 or the cathode electrode 42 of the light emitting element 40 is placed. Each of the plurality of through electrodes 30 is formed in a cylindrical shape having a diameter of 30 μm, for example. That is, the light emitting element 40 has the plurality of through electrodes 30 bonded to the electrode surface of each of the anode electrode 41 or the cathode electrode 42.
[0044] For example, if an internal electrode having the same shape as the anode electrode 41 and the cathode electrode 42 of the light emitting element 40 is formed on the element mounting surface 13, the internal electrode and the anode electrode 41 or the cathode electrode 42 are AuSn bonded to each other on one surface. In this case, unpredictable or uncontrollable voids may occur in the AuSn bonding layer at the bonding surface between the internal electrode and the anode electrode 41 or the cathode electrode 42. These voids may affect reliability, such as cracking the bonding layer, when heat is generated during operation of the light emitting element after manufacture.
[0045] In this embodiment, the plurality of through electrodes 30 are formed to be spaced apart from each other. The AuSn layer 33 of the regularly arranged through electrodes 30 protrudes from the element mounting surface 13, so that the melting start points can be regularly arranged by contacting the anode electrode 41 or the cathode electrode 42 in the bonding process. The light emitting element 40 is bonded so as to rest on the upper surface of each of the plurality of through electrodes 30. This makes it possible to suppress the occurrence of unpredictable or uncontrollable voids as described above, and to reduce the influence of voids on reliability at the bonding portions between the light emitting element 40 and each of the plurality of through electrodes 30 after the light emitting device 100 is manufactured.
[0046] 3, the plurality of through electrodes 30 are arranged on the lattice points of an equilateral triangular lattice on the bottom surface of the cavity. Each of the plurality of through electrodes 30 is formed, for example, as a cylinder having a diameter of 30 μm, and is arranged such that the distance between the centers of adjacent through electrodes 30 is 60 μm. By arranging the plurality of through electrodes 30 in the above-mentioned arrangement, each of the plurality of through electrodes 30 is arranged such that the distance between one through electrode 30 and the other through electrodes 30 arranged around it is uniform.
[0047] For example, if a plurality of through electrodes 30 are formed in a matrix, one through electrode 30 is spaced at an equal distance from the other through electrodes 30 arranged above, below, left and right in top view. However, the distance between one through electrode 30 and the other through electrodes 30 arranged in a diagonal direction is different. This causes a bias in the stress applied within the upper surface of the element mounting surface 13 when the light emitting element 40 is bonded or when the light emitting element 40 is driven and generates heat, and this may cause minute cracks or the like in the first substrate 11, breaking the airtightness in the cavity.
[0048] In this embodiment, as described above, each of the plurality of through electrodes 30 is arranged on the lattice points of the equilateral triangular lattice. This makes it possible to suppress cracks in the first substrate 11 since stress applied to the upper surface of the element mounting surface 13 becomes uniform during bonding of the light emitting element 40 or heat generation during operation of the light emitting element 40.
[0049] Furthermore, by arranging each of the plurality of through electrodes 30 on the lattice points of the equilateral triangular lattice as in this embodiment, it is possible to form a greater number of through electrodes 30 than by arranging the plurality of through electrodes 30 in a matrix shape. This makes it possible to dissipate more heat generated during operation of the light emitting element 40 to the mounting board. According to the inventor's verification, by arranging each of the plurality of through electrodes 30 on the lattice points of the equilateral triangular lattice as in this embodiment, it is possible to arrange a plurality of through electrodes 30 in a quantity 1.2 times greater than by arranging the plurality of through electrodes 30 in a matrix shape.
[0050] FIG. 4 is an enlarged view of a bonding area CA between the frit glass layer 60 and the second substrate 12 shown in FIG.
[0051] As described above, the composite substrate 10 is bonded to the light-transmitting member 50 via the frit glass layer 60. In addition, the thermal oxide film 18 is formed on the upper surface of the second substrate 12. At this time, between the frit glass layer 60 and the second substrate 12, the frit glass layer 60, the mutual diffusion layer 70 as a reaction layer in which the thermal oxide film 18 and the frit glass layer 60 are mutually diffused, and the residual thermal oxide film 18A are formed in this order from above. In other words, in the light-emitting device 100, at the bonding portion between the composite substrate 10 and the frit glass layer 60, the residual thermal oxide film 18A and the mutual diffusion layer 70 between the thermal oxide film 18 and the frit glass layer 60 are formed in this order from the surface of the composite substrate 10.
[0052] The interdiffusion layer 70 is formed by interdiffusion between the SiO2 of the thermal oxide film 18 formed on the upper surface of the second substrate 12 and the SiO2 of the frit glass layer 60 by heating and melting the frit glass layer 60. That is, at the joint of the frit glass layer 60, the remaining thermal oxide film 18A, the interdiffusion layer 70, and the frit glass layer 60 are laminated in this order from the upper surface of the second substrate 12. The thermal oxide film 18 is formed in the thermal oxidation process so that the thickness (d1) of the thermal oxide film 18 is 0.8 μm or more and 1.2 μm or less.
[0053] Furthermore, the thickness of the thermal oxide film 18 is designed in consideration of the thickness of the interdiffusion layer 70 formed during bonding so that the remaining thermal oxide film 18A is formed. The formation of the remaining thermal oxide film 18A can suppress the occurrence of cracks near the lower end of the interdiffusion layer 70. By setting the thickness of the thermal oxide film 18 to be 0.8 μm or more and 1.2 μm or less, the formation of the remaining thermal oxide film 18A after heat treatment can be more reliably achieved.
[0054] The remaining thermal oxide film 18A preferably has a thickness (d2) of 0.5 times or more the thickness (d1) of the thermal oxide film 18. That is, the remaining thermal oxide film 18A preferably has a thickness (d2) of 0.4 μm or more and 0.6 μm or less. If the remaining thermal oxide film 18A has a thin thickness (d2) or if the remaining thermal oxide film 18A is not formed, a crack may occur near the lower end of the interdiffusion layer 70, and the airtight sealing of the accommodation space HS may be broken.
[0055] Specifically, the thermal oxide film 18 is formed as a SiO2 film by diffusing oxygen from the surface of the second substrate 12, which is single crystal Si, by thermal oxidation treatment. However, the thermal oxide film 18 is not formed uniformly as SiO2 from the upper surface of the thermal oxide film 18 to the upper surface of the second substrate 12. Specifically, the abundance ratio of SiO2 to Si gradually increases from the upper surface of the second substrate 12 upward, and the Si crystallinity is also lost. That is, the thermal oxide film 18 near the surface of the second substrate 12 has some Si crystallinity and is a mixture of Si and SiO2.
[0056] Moreover, the interdiffusion layer 70 between the thermal oxide film 18 and the frit glass layer 60 is made of SiO2 having an amorphous structure. That is, when the thickness (d2) of the remaining thermal oxide film 18A is thin, the upper end of the remaining thermal oxide film 18A may partially contain Si and its crystallinity.
[0057] If an SiO2 layer having an amorphous structure is bonded to an SiO2 layer containing Si and some of its crystallinity, the arrangement of atoms at the bonding interface changes suddenly. In this case, the bonding strength at the bonding interface is expected to be low. As a result, if stress is generated at the bonding interface due to heat generation during operation of the light emitting element 40, cracks may occur at the bonding interface and the airtight seal of the storage space HS may be broken. In contrast, if SiO2 layers having a sufficiently amorphous structure are bonded to each other, neither layer has crystallinity, so there is no sudden change in the atomic arrangement, and stress is less likely to occur when heat is generated.
[0058] Therefore, it is preferable that the remaining thermal oxide film 18A remains with a thickness of 0.4 μm to 0.6 μm, which is assumed to be a thickness sufficient to turn the SiO2 into an amorphous structure. This allows the composite substrate 10 and the light-transmitting member 50 to be bonded with high bonding strength via the glass frit layer 60.
[0059] That is, the remaining thermal oxide film 18A functions as a buffer layer that improves the bonding strength when bonding the second substrate 12 and the frit glass layer 60. The thickness (d2) of the remaining thermal oxide film 18A may be any thickness that is sufficient to turn the film into SiO2 with an amorphous structure.
[0060] As described above, at the joint between the frit glass layer 60 and the second substrate 12, the remaining thermal oxide film 18A, the mutual diffusion layer 70, and the frit glass layer 60 are formed in this order from the upper surface of the second substrate 12, thereby making it possible to maintain high airtightness of the accommodation space HS. According to verification by the inventors, in a helium (He) leak test specified in the Japanese Industrial Standard JIS-Z2331, the accommodation space HS of the light emitting device 100 was able to obtain airtightness equal to or greater than that of a conventional AlN substrate and a product in which an AlN substrate and a light-transmitting member are joined with AuSn.
[0061] Next, a manufacturing procedure for the light emitting device 100 according to the first embodiment of the present invention will be described with reference to FIGS.
[0062] FIG. 5 and FIG. 6 are diagrams showing a manufacturing flow of the light emitting device 100 according to the first embodiment of the present invention. Also, FIG. 7 to FIG. 17 are cross-sectional views of the light emitting device 100 in each step of the manufacturing procedure shown in FIG. 5 and FIG. 6. In FIG. 7 to FIG. 17, as in FIG. 2, the cross section along the line AA shown in FIG. 1 will be used for the description. In this embodiment, as described above, the light emitting device 100 is a WLP in which the light emitting devices 100 are formed in a lattice pattern on the wafer-like composite substrate 10. Therefore, the composite substrate 10 has a plurality of element mounting regions R1 defined by predetermined lattice-like division lines CL on the wafer-like composite substrate 10. That is, the processing of each step described below is performed continuously in a lattice pattern on the wafer-like composite substrate 10. In the description of the processing of each step below, the processing will basically be performed on one element mounting region R1.
[0063] First, as a step of preparing a composite substrate, as shown in FIG. 7, a composite substrate 10 is prepared in which a first substrate 11 made of single crystal Si is bonded to a second substrate 12 made of single crystal Si via a buried oxide film 14 made of SiO2 (step S101). In other words, the manufacturing method of the light emitting device 100 includes a step of preparing a composite substrate 10 having a first substrate 11 made of single crystal silicon, a buried oxide film 14 made of silicon oxide formed on the first substrate 11, and a second substrate 12 made of single crystal silicon bonded to the first substrate 11 via the buried oxide film 14, and having a plurality of element mounting regions R1 defined by lattice-shaped division lines CL on the upper surface. Note that SiO2 is formed by natural oxidation on the upper surface of the first substrate 11 and the lower surface of the second substrate 12, but the natural oxide film is not shown in this description.
[0064] Next, as shown in FIG. 8, in the hole forming step, etching is performed from the lower surface side of the composite substrate 10 to form a plurality of columnar holes 16A that will become a plurality of through holes 16 in the following step (step S102). Each of the plurality of holes 16A is formed using deep reactive ion etching (DREI) by the Bosch process. Also, etching of each of the plurality of holes 16A is performed from the lower surface of the first substrate 11 until it reaches the lower surface of the buried oxide film 14. At this time, the buried oxide film 14 functions as an etch stopper. Also, each of the plurality of holes 16A is formed in each of the regions corresponding to the anode electrode 41 and the cathode electrode 42 of the light emitting element 40 in the element mounting step described later. Although not shown, this step includes the steps of applying a photoresist to the lower surface of the composite substrate 10, exposing the photoresist to remove each region of the plurality of holes 16A, removing the photoresist in the corresponding region, etching the first substrate 11 in the photoresist opening portion, and removing the photoresist. In other words, the manufacturing method for the light-emitting device 100 includes a hole formation process for forming a plurality of columnar holes 16A extending from the lower surface of the composite substrate 10 to the buried oxide film 14 in each of the plurality of element mounting regions R1 in regions corresponding to the anode electrode 41 and the cathode electrode 42 of each of the light-emitting elements 40 in the plurality of element mounting regions R1.
[0065] Next, as shown in FIG. 9, a thermal oxide film 17B is formed on the lower surface of the composite substrate 10 and on the inner surface of each of the holes 16A, and a thermal oxide film 18B is formed on the upper surface of the composite substrate 10 (step S103). The thermal oxide films 17B and 18B formed in this step form an etch stopper for the side of the groove during etching in the next step. The thermal oxide films 17B and 18B are formed by wet oxidation in which the substrate is heated at 1100° C. for 7 hours or more in a water vapor atmosphere. The thermal oxide films 17B and 18B formed in this step are formed to a thickness of about 1 μm. As described above, the thermal oxide films 17B and 18B function as an etch stopper during etching in the next step. Therefore, the thickness of the thermal oxide films 17B and 18B formed in this step is not limited to this. Specifically, it is sufficient that the thermal oxide films 17B and 18B are formed to a thickness that functions as an etch stopper during etching in the next step.
[0066] Next, as a recess forming step, as shown in FIG. 10, etching is performed from the upper surface side of the composite substrate 10 to form a recess that will become a cavity of the composite substrate 10 (step S104). The recess is formed by wet etching using a tetramethylammonium hydroxide solution (TMAH). The recess is etched from the upper surface of the second substrate 12 until it reaches the upper surface of the buried oxide film 14. The recess is formed in each of the element mounting regions R1 with the region including the region in which each of the multiple holes 16A formed in step S102 is formed as the bottom surface. As in the explanation of step S102, this step includes, although not shown, the steps of applying photoresist to the upper surface of the second substrate 12, exposing the photoresist to remove the regions of the respective recesses, removing the photoresist from the regions, etching the thermal oxide film 18B and the second substrate 12 in the photoresist openings, and removing the photoresist. As a result, an opening 15 is formed in the upper surface of the second substrate 12 with the (111) crystal plane of single crystal Si exposed on the side surface. As in step S102, the buried oxide film 14 functions as an etch stopper when the recesses are formed. That is, the buried oxide film 14 is exposed at the bottom of the recesses. In other words, the manufacturing method of the light-emitting device 100 includes a recess forming step of forming, in each of the element mounting regions R1, a plurality of concave recesses on the upper surface of the composite substrate 10 so that the bottom surface of each of the recesses extends from the upper surface of the composite substrate 10 to the buried oxide film 14 and includes regions corresponding to the anode electrode 41 and the cathode electrode 42 of the light-emitting element 40.
[0067] Next, as an oxide film removing step, as shown in FIG. 11, the thermal oxide films 17B and 18B and the buried oxide film 14 exposed on the bottom surface of the recess are removed (step S105). These oxide films are removed using buffered hydrofluoric acid (BHF). As a result, the buried oxide film 14 exposed on the bottom surface of the recess is removed, and each of the multiple holes 16A formed in step S102 communicates with the bottom surface of the recess, forming multiple through holes 16. In other words, the manufacturing method of the light emitting device 100 includes an oxide film removing step of removing the buried oxide film 14 exposed on the bottom surface of each of the multiple recesses to communicate the multiple holes 16A with the bottom surface of each of the multiple recesses.
[0068] 12, thermal oxide films 17 and 18 are formed on the exposed Si surface of composite substrate 10 from which thermal oxide films 17B and 18B have been removed (step S106). Thermal oxide film 17 is formed on the lower surface of first substrate 11, the upper surface of first substrate 11 exposed at the bottom surface of the recess, and the inner surfaces of each of the multiple through holes 16. Thermal oxide film 18 is formed on the upper surface of second substrate 12 and the inner surfaces of the recess.
[0069] The thermal oxide films 17 and 18 are formed by wet oxidation in which the substrate is heated at 1100°C for 7 hours or more in a water vapor atmosphere, as in the method of step S103. The thermal oxide films 17 and 18 formed at this time are formed to a thickness of 0.8 μm or more and 1.2 μm or less, as described above. In addition, the thermal oxide film 18 is formed on the side surface of the opening 15, so that the space surrounded by the opening 15 functions as a cavity of the composite substrate 10. In other words, the manufacturing method of the light emitting device 100 includes a thermal oxide film forming step of heating the composite substrate 10 at 1100°C for 7 hours or more in a water vapor atmosphere to form the thermal oxide films 17 and 18 on the lower surface of the composite substrate 10, the upper surface of the composite substrate 10, and the inner surfaces of each of the plurality of through holes 16.
[0070] Next, as a through electrode forming process, as shown in FIG. 13, a plurality of through electrodes 30 consisting of a Cu layer 31, a Ni layer 32, and an AuSn layer 33 are formed inside each of the plurality of through holes 16 (step S108). The formation of the plurality of through electrodes 30 is performed by first forming a seed layer in which titanium (Ti) / Cu are laminated in this order on the lower surface of the composite substrate 10 and on a part of the inner surface of each of the plurality of through holes 16 from the lower surface side of the composite substrate 10 by sputtering film formation. In this description, the seed layer is not shown. Thereafter, the lower surface of the composite substrate 10 is masked, and the Cu layer 31, the Ni layer 32, and the AuSn layer 33 are formed in each of the plurality of through holes 16 by electrolytic plating in the order of Cu, Ni, and AuSn from the lower surface of the composite substrate 10.
[0071] As described above, in each of the plurality of through electrodes 30, the Cu layer 31 is filled in each of the plurality of through holes 16 with a thickness of about 49 μm from the lower surface of the first substrate 11, and the Ni layer 32 is filled in each of the plurality of through holes 16 with a thickness of about 1 μm on the upper surface of the Cu layer 31. In this embodiment, the upper surface of the Ni layer 32 is formed to be flush with the upper surface of the thermal oxide film 17 formed on the upper surface of the first substrate 11, and the AuSn layer 33 is formed to be flush with the upper surface of the thermal oxide film 17 with a thickness of about 5 μm so as to protrude from the upper surface of the thermal oxide film 17. In other words, the manufacturing method of the light emitting device 100 includes a through electrode forming step of forming the plurality of columnar through electrodes 30 by electrolytic plating so as to fill the interiors of each of the plurality of through holes 16. In this embodiment, the case where the Ni layer 32 is flush with the upper surface of the thermal oxide film 17 formed on the upper surface of the first substrate 11 has been described, but the height position of the Ni layer 32 is not limited thereto.
[0072] In steps S106 and S107, the thermal oxide film 17 and each of the plurality of through electrodes 30 are formed on the exposed surface of the upper surface of the first substrate 11, so that the exposed surface of the upper surface of the first substrate 11 functions as the element mounting surface 13. Thereafter, the mask on the lower surface of the first substrate 11 is removed to expose the Cu layer 31 of each of the plurality of through electrodes 30 on the lower surface of the first substrate 11.
[0073] Next, as shown in FIG. 14, the first external electrode 21 and the second external electrode 22 are formed on the lower surface of the composite substrate 10 (step S108). The first external electrode 21 and the second external electrode 22 are formed by laminating Ni / Au in this order on the lower surface of the composite substrate 10 by electrolytic plating after masking the lower surface of the composite substrate 10 except for the respective external electrodes with a resist. Each external electrode formed by electrolytic plating is formed on the lower surface of the seed layer (not shown) formed in step S108 and on the lower surface of the Cu layer 31 of the through electrode 30 exposed on the lower surface of the first substrate 11. At this time, the Ni layer of each external electrode is formed to a thickness of about 3 μm, and the Au layer is formed to a thickness of 0.2 μm so as to cover the lower surface of the Ni layer. The seed layer is composed of a sputtered film laminated in the order of Ti / Cu.
[0074] Thereafter, the resist on the lower surface of the first substrate 11 is removed, and further the seed layer remaining in the portions excluding the external electrodes is etched, thereby electrically insulating the first external electrode 21 and the second external electrode 22.
[0075] Next, as a die-bonding process, as shown in FIG. 15, the composite substrate 10 is set in a die-bonding device, and the light-emitting element 40 is placed on the element mounting surface 13 (step S109). The light-emitting element 40 is placed by aligning the through electrode 30 electrically connected to the first external electrode 21 and the anode electrode 41, and the through electrode 30 electrically connected to the second external electrode 22 and the cathode electrode 42, so that the light-emitting element 40 is placed. Thereafter, the composite substrate 10 on which the light-emitting element 40 is placed is heated at 340° C. for 30 seconds in a nitrogen (N2) atmosphere, and the AuSn layer 33 of the through electrode 30 is eutectic-bonded to the anode electrode 41 and the cathode electrode 42 of the light-emitting element 40, the lowermost layer of which is made of Au. In other words, the manufacturing method of the light-emitting device 100 includes a die-bonding process in which the light-emitting element 40 is placed on each of the element mounting surfaces 13, which are the bottom surfaces of each of the multiple cavities.
[0076] 16, the light-transmitting member 50, on whose surface facing the upper surface of the second substrate 12 a frit glass layer 60 has been formed in advance, is placed on the upper surface of the second substrate 12 so as to cover each of the cavities of the element mounting regions R1 (step S120). The light-transmitting member 50 has the raw material paste of the frit glass layer 60 printed in a lattice pattern, similar to the composite substrate 10. The light-transmitting member 50 on which the raw material paste of the frit glass layer 60 has been applied has been pre-fired in an oxygen (O2) atmosphere at a temperature of about 500° C. for one hour. The raw material paste of the frit glass layer 60 is applied at a position corresponding to the upper surface position of the second substrate 12 so as to surround the cavities and to a size that does not overlap the parting lines CL of the composite substrate 10. As described above, the light-transmitting member 50 is positioned so that the frit glass layer 60 corresponds to the upper surface position of the second substrate 12, surrounds the cavity, and is positioned so as not to overlap with the dividing line CL of the composite substrate 10.
[0077] Next, as shown in FIG. 17, the composite substrate 10 on which the light-transmitting member 50 is placed is irradiated with a laser LB from above, and the frit glass layer 60 is melted to bond the composite substrate 10 and the light-transmitting member 50 (step S121). The laser LB is, for example, a laser beam having a wavelength of near infrared light. The frit glass layer 60 is locally heated and melted at the laser irradiated portion in an N2 atmosphere, and bonded to the composite substrate 10. At this time, as described in FIG. 4, the melted frit glass layer 60 and the thermal oxide film 18 on the upper surface of the second substrate 12 are mutually diffused to form an interdiffusion layer 70. As a result, the inside of the cavity is filled with N2, which is an inert gas, and a storage space HS is formed in which the cavity is hermetically sealed. In addition, in bonding the light-transmitting member 50, the thickness of the thermal oxide film 18 and various conditions during bonding are set so that the remaining thermal oxide film 18A is also formed by the mutual diffusion between the thermal oxide film 18 and the frit glass layer 60. That is, the joint between the second substrate 12 and the glass frit layer 60 has a structure in which the remaining thermal oxide film 18A, the mutual diffusion layer 70, and the glass frit layer 60 are laminated in this order from the upper surface of the second substrate 12.
[0078] The laser LB scans the frit glass layer 60 surrounding the cavity along the periphery of the cavity. The scanning time of the laser LB is about 2 to 3 seconds per light emitting device 100. In this manner, the bonding portion of the frit glass layer 60 is locally heated in a short time by the laser LB to bond the frit glass layer 60, thereby making it possible to prevent the AuSn layer 33 of the through electrode 30 from being remelted due to overheating.
[0079] Moreover, the inside of the cavity is a space filled with N2 gas, and its thermal conductivity is very small compared to that of the composite substrate 10 mainly made of single crystal Si. That is, the N2 near the portion irradiated with the laser LB accumulates heat, so that the portion irradiated with the laser LB reaches the melting temperature of the frit glass layer 60. In addition, the heat of the element mounting surface 13 is dissipated to the lower surface of the composite substrate 10 due to the high thermal conductivity of single crystal Si, which makes it possible to further prevent overheating of the AuSn layer 33. According to the inventors' verification, the temperature of the element mounting surface 13 during the laser LB irradiation was 250°C or less.
[0080] The above steps S120 and S121 are processed as a light-transmitting member bonding step. In other words, the manufacturing method of the light-emitting device 100 includes a light-transmitting member bonding step of placing a light-transmitting member 50 made of glass having a frit glass layer 60 on one surface facing the upper surface of the composite substrate 10 so as to cover each of the multiple cavities, and bonding the light-transmitting member 50 to the upper surface of the composite substrate 10 by scanning the frit glass layer 60 from above along the periphery of each of the multiple cavities with a laser LB.
[0081] 18, the composite substrate 10 to which the light-transmitting member 50 is joined is set in a dicer device, and the composite substrate 10 and the light-transmitting member 50 are cut along the division lines CL to separate them (step S122). As a result, the light-emitting device 100 is diced into individual units, and a plurality of light-emitting devices 100 are manufactured. In other words, the manufacturing method for the light-emitting device 100 includes a dicing step of cutting the composite substrate 10 along the division lines CL of the composite substrate 10 to separate them.
[0082] According to this embodiment, the light emitting device 100 has a composite substrate 10 made of an SOI substrate in which a first substrate 11 made of single crystal Si and a second substrate 12 made of single crystal Si are bonded together via a buried oxide film 14. The light emitting device 100 also has a cavity, which is a recess extending from the upper surface of the second substrate 12 to the upper surface of the first substrate 11. The light emitting device 100 also has a plurality of through electrodes 30 formed so as to penetrate the first substrate 11 on the element mounting surface 13, which is the bottom surface of the cavity. The light emitting device 100 also has thermal oxide films 17 and 18 having a thickness in the range of 0.8 μm to 1.2 μm on the surface of the composite substrate 10. The light emitting device 100 also has a translucent member 50 bonded to the upper surface of the second substrate 12 via a frit glass layer 60 so as to cover the cavity. In addition, in the light emitting device 100, at the bonding portion between the second substrate 12 and the frit glass layer 60, a remaining thermal oxide film 18A and an interdiffusion layer 70 between the thermal oxide film 18 and the frit glass layer 60 are formed in this order from the surface of the second substrate 12. In addition, in the light emitting device 100, at the bonding portion between the second substrate 12 and the frit glass layer 60, the remaining thermal oxide film 18A remains at 0.5 times or more the size of the thermal oxide film 18.
[0083] The light emitting device 100 having the above-mentioned configuration enables the light-transmitting member 50 and the glass frit layer 60 to hermetically seal the cavity of the composite substrate 10 .
[0084] In addition, the interdiffusion layer 70 between the thermal oxide film 18 and the frit glass layer 60 is formed by irradiating the bonding portion with a laser LB to heat it locally and for a short time. This makes it possible to prevent remelting of the AuSn layer 33 bonding the light emitting element 40 and the through electrode 30 when the cavity of the composite substrate 10 is hermetically sealed by the laser LB irradiation.
[0085] That is, the light emitting device 100 can provide a light emitting device capable of hermetically sealing the light emitting element 40 and suppressing manufacturing defects, and a manufacturing method thereof.
[0086] Moreover, according to this embodiment, the light emitting device 100 has a plurality of through electrodes 30 spaced apart from one another on the element mounting surface 13. The light emitting element 40 is joined so as to support the upper surfaces of the plurality of through electrodes 30. Each of the plurality of through electrodes 30 is disposed in the region of the cavity bottom surface on a lattice point of an equilateral triangular lattice.
[0087] By having the above-mentioned configuration, the light-emitting device 100 can suppress the occurrence of voids at the bonding interface between each of the anode electrode 41 or the cathode electrode 42 of the light-emitting element 40 and the multiple through electrodes 30, thereby making it possible to reduce the impact of voids on reliability after manufacturing.
[0088] Furthermore, by having the above-mentioned configuration, the light emitting device 100 is arranged so that the distance between one through electrode 30 and the other through electrodes 30 arranged around it is uniform. This makes it possible to suppress cracks in the first substrate 11 since the stress acting on the upper surface of the element mounting surface 13 becomes uniform when the light emitting element 40 generates heat or the like.
[0089] Furthermore, by having the above-mentioned configuration, the light-emitting device 100 can form a greater number of through electrodes 30 than if the through electrodes 30 were arranged in a matrix, making it possible to dissipate more heat generated when the light-emitting element 40 is driven to the mounting substrate.
[0090] In this embodiment, the light emitting element 40 is bonded so as to rest on the upper surfaces of the plurality of through electrodes 30. However, the method of bonding the light emitting element 40 is not limited to this. Specifically, an internal electrode may be formed so as to cover the plurality of through electrodes 30, and the light emitting element 40 may be bonded onto the upper surface of the internal electrode. EXAMPLES
[0091] Fig. 19 shows a cross-sectional view of a light emitting device 100A according to Example 2. Similar to Fig. 2, the cross-sectional view shown in Fig. 19 shows a cross section at a position corresponding to the line AA in Fig. 1.
[0092] The light emitting device 100A has a basically similar configuration and similar appearance to the light emitting device 100 of Example 1. However, the light emitting device 100A differs from the light emitting device 100 in that the plurality of through electrodes 30A are made only of Cu, and a first internal electrode 80 and a second internal electrode 81 are formed on the upper surface of the element mounting surface 13 so as to cover the plurality of through electrodes 30A.
[0093] As described above, each of the plurality of through electrodes 30A is made of Cu, and is formed so as to fill the through hole 16 from the lower surface of the first substrate 11 to the upper surface of the element mounting surface 13.
[0094] Moreover, a first internal electrode 80 is formed on the upper surface of the element mounting surface 13 so as to cover each of the multiple through electrodes 30A connected to the first external electrode 21 and the thermal oxide film 17 formed on the first substrate 11. The first internal electrode 80 is composed of a composite metal layer 80A made of a Ti layer / Cu layer / Ni layer, and a bonding metal layer 80B made of AuSn formed on the upper surface of the composite metal layer 80A.
[0095] Moreover, a second internal electrode 81 is formed on the upper surface of the element mounting surface 13 so as to cover the multiple through electrodes 30A connected to the second external electrodes 22 and the thermal oxide film 17 formed on the first substrate 11. The second internal electrode 81 is composed of a composite metal layer 81A made of a Ti layer / Cu layer / Ni layer, and a bonding metal layer 81B made of AuSn formed on the upper surface of the composite metal layer 81A.
[0096] Moreover, the first internal electrode 80 is formed in the same shape as the anode electrode 41 of the light emitting element 40 when viewed from above. Moreover, the second internal electrode 81 is formed in the same shape as the cathode electrode 42 of the light emitting element 40 when viewed from above.
[0097] As described above, the first internal electrode 80 and the second internal electrode 81 are formed on the upper surface of the first substrate 11 so as to cover the respective through electrodes 30A. Also, the first external electrode 21 and the second external electrode 22 are formed on the lower surface of the first substrate 11 so as to cover the respective through electrodes 30A. This allows the light emitting device 100A to form a more airtight storage space HS.
[0098] As described above, the first internal electrode 80 and the second internal electrode 81 are formed to have the same top surface shapes as the anode electrode 41 and the cathode electrode 42 of the light emitting element 40, respectively. This enables self-alignment with respect to the respective positions of the internal electrodes of the light emitting element 40 in the light emitting device 100A when the bonding metal layers 80B and 81B of each internal electrode melt during bonding of the light emitting element 40.
[0099] Furthermore, since the structure and bonding method of the joints of the glass frit layer 60 are similar to those of the light emitting device 100 of the first embodiment, the same effect as that of the light emitting device 100 of the first embodiment can be obtained with respect to hermetic sealing of the joints of the glass frit layer 60.
[0100] Also in this embodiment, regular fine irregularities are formed on the upper surfaces of the bonding metal layers 80B and 81B made of AuSn due to the regularly arranged through electrodes 30A, so that in the bonding process, the regularly arranged protrusions can come into contact with the anode electrode 41 and the cathode electrode 42 to form melting starting points. Therefore, it is possible to suppress the occurrence of unpredictable or uncontrollable voids in the bonding portion with the light emitting element 40.
[0101] Fig. 20 is a diagram showing a manufacturing flow of the light emitting device 100A according to Example 2. Fig. 21 and Fig. 22 show cross-sectional views of the light emitting device 100A in each step of the manufacturing procedure shown in Fig. 20. In Fig. 21 and Fig. 22, similar to Fig. 19, the explanation will be given using a cross section at a position corresponding to the line AA shown in Fig. 1. In this example, similar to Example 1, the processing of each step described below is performed continuously in a lattice pattern on a wafer-shaped composite substrate 10.
[0102] Incidentally, the steps before the manufacturing flow shown in Fig. 20 are similar to those in the manufacturing flow shown in Fig. 5, and therefore the description thereof will be omitted. Also, steps S209 to S213 in the manufacturing flow shown in Fig. 20 are similar to steps S108 to S112 in the manufacturing flow shown in Fig. 6, and therefore the description thereof will be omitted.
[0103] As shown in FIG. 21, the process of step S106 shown in FIG. 5 is completed, and a plurality of through electrodes 30A are formed inside each of the plurality of through holes 16 of the composite substrate 10 on which the thermal oxide film 17 and the thermal oxide film 18 are formed (step S207). Each of the plurality of through electrodes 30A is made of Cu as described above. The formation of the plurality of through electrodes 30A is performed in the same manner as in step S107 described in FIG. 6, by forming a seed layer on the lower surface of the first substrate 11 and a part of the side surface of the through hole 16, and then forming the plurality of through electrodes 30A by electrolytic plating after masking the lower surface of the first substrate 11. However, unlike step S107, the formation is performed so that Cu is filled from the lower surface to the upper surface of the first substrate 11 by electrolytic plating. Thereafter, the mask on the lower surface of the first substrate 11 is removed to expose the plurality of through electrodes 30A on the lower surface of the first substrate 11.
[0104] Next, as shown in FIG. 22, the first internal electrode 80 and the second internal electrode 81 are formed on the upper surface of the first substrate 11 so as to cover each of the through electrodes 30A (step S208). The first internal electrode 80 and the second internal electrode 81 are formed by first forming a seed layer in which Ti / Cu are laminated in this order by sputtering film formation so as to cover the bottom surface of the cavity from the upper surface side of the first substrate 11. In addition, in this description, the seed layer is not shown. Next, after masking the portion of the upper surface of the composite substrate 10 except for each internal electrode with a resist, the Ni layers of the composite metal layers 80A and 81A and the AuSn layers of the bonding metal layers 80B and 81B are laminated on the upper surface of the first substrate 11 by electrolytic plating, respectively, to form the first internal electrode 80 and the second internal electrode 81.
[0105] The Ni layers of the composite metal layers 80A and 81A are formed to a thickness of about 1 μm. The bonding metal layers 80B and 81B are formed to a thickness of about 5 μm on the upper surfaces of the Ni layers of the composite metal layers 80A and 81A, respectively. Thereafter, the resist on the upper surface of the composite substrate 10 is removed, and the seed layer remaining in the portions other than the internal electrodes is etched. As a result, the first internal electrode 80 and the second internal electrode 81 are electrically insulated.
[0106] Thereafter, steps S209 and after (corresponding to steps S108 and after in FIG. 6) are carried out to manufacture the light emitting device 100A of the second embodiment.
[0107] In the first and second embodiments, a case has been described in which an SOI substrate in which a first substrate 11 and a second substrate 12 are bonded together with a buried oxide film 14 interposed therebetween is used as the composite substrate 10. However, the composite substrate 10 is not limited to an SOI substrate. Specifically, a Si wafer made of a single layer of single crystal Si may be used. EXAMPLES
[0108] Fig. 23 shows a cross-sectional view of a light emitting device 100B according to Example 3. The cross-sectional view shown in Fig. 19 shows a cross section at a position corresponding to the line AA in Fig. 1, similar to Fig. 2.
[0109] The light emitting device 100B has a basically similar configuration and almost the same appearance as the light emitting device 100 of Example 1. However, the light emitting device 100B differs from the light emitting device 100 in that the substrate 10A is made of a Si substrate 11A made of a single layer of single crystal Si, and a thermal oxide film 17C formed so as to cover the upper and lower surfaces of the Si substrate 11A and the inner side surfaces of each of the plurality of through holes 16.
[0110] In the light emitting device 100B, the structure of the through electrodes 30 formed inside each of the plurality of through holes 16 is the same as that of the light emitting device 100. In addition, the structure and bonding method of the bonding portion of the frit glass layer 60 at the bonding portion between the substrate 10A and the light-transmitting member 50 are the same as those of the light emitting device 100. Therefore, the same effect as that of the light emitting device 100 of the first embodiment can be obtained with respect to the airtight sealing of the accommodation space HS.
[0111] The manufacturing method of the light emitting device 100B of this embodiment 3 is the same as the manufacturing method of the light emitting device 100 of embodiment 1. In the processing of steps S102 and S104 of the manufacturing method shown in Fig. 5, since there is no buried oxide film 14 functioning as an etch stopper in this embodiment 3, the processing end point of the etching process in the steps is controlled by the amount of Si processing.
[0112] That is, the manufacturing method of the light emitting device 100B of Example 3 includes the steps of preparing a substrate 10A made of single crystal silicon and having an element mounting region with a recess, a thermal oxide film forming step of forming a thermal oxide film 17C on the upper surface of the substrate 10A, a die bonding step of mounting the light emitting element 40 in the recess, and a light-transmitting member bonding step of arranging a light-transmitting member 50 made of glass having a frit glass layer 60 on the upper surface of the substrate 10A so as to cover the recess with the frit glass layer 60 side facing each other, and melting the frit glass layer 60 to bond the light-transmitting member 50 to the upper surface of the substrate 10A. In the light-transmitting member bonding step, the thermal oxide film 17C and the frit glass layer 60 mutually diffuse, so that at the bonded portion between the substrate 10A and the frit glass layer 60, the thermal oxide film 17C, the interdiffusion layer 70 in which the thermal oxide film 17C and the frit glass layer 60 are mutually diffused, and the frit glass layer 60 are stacked in this order from the upper surface of the substrate 10A.
[0113] According to the third embodiment, by using the Si substrate 11A made of a single layer of single crystal Si as the substrate 10A, it is possible to reduce the manufacturing cost as compared with the case of preparing the SOI substrate of the first embodiment.
[0114] Each of the above-described embodiments is merely an example. For example, the above-described various embodiments can be combined. For example, the light emitting device 100B of the third embodiment may have a plurality of through electrodes 30A, a first internal electrode 80, and a second internal electrode 81 of the light emitting device 100A so that the light emitting device 100B can perform self-alignment when the light emitting element 40 is placed.
[0115] Furthermore, the various numerical values, dimensions, materials, and the like in each of the above-described embodiments are merely examples, and can be appropriately selected depending on the application and the light emitting device to be manufactured. [Explanation of symbols]
[0116] 100 Light emitting device 10 Substrate 11 First substrate 12 Second board 13 Element mounting surface 14 Buried oxide film 15 Opening 16 Through hole 17, 18 Thermal oxide film 21 First external electrode 22 Second external electrode 30 Through electrode 31 Cu layer 32 Ni layer 33 AuSn layer 40 Light emitting element 41 Anode electrode 42 Cathode electrode 50 Translucent material 60 frit glass layers 70 Interdiffusion Layer
Claims
1. a substrate made of single crystal silicon having an upper surface on which a thermal oxide film is formed and a recess formed in the upper surface; a light emitting element placed on a bottom surface of the recess; a light-transmitting member made of glass having a frit glass layer on a lower surface thereof and bonded to the upper surface of the substrate via the frit glass layer; the thermal oxide film and a reaction layer between the thermal oxide film and the glass frit layer are formed in this order from a surface of the substrate between the substrate and the glass frit layer at a bonding portion between the substrate and the glass frit layer, a thickness of the thermal oxide film at the junction portion being at least 0.5 times the thickness of the thermal oxide film other than the junction portion;
2. the substrate is provided with a plurality of through holes each extending in a columnar shape from the bottom surface of the recess to a rear surface of the substrate, the inner surface of the through hole being covered with the thermal oxide film; The light emitting device according to claim 1 , further comprising a plurality of columnar through electrodes filling the plurality of through holes.
3. The light emitting device according to claim 2 , wherein the plurality of through electrodes are arranged on lattice points of an equilateral triangular lattice on the bottom surface of the recess.
4. the light emitting element includes a pair of element electrodes on a surface facing the bottom surface of the recess, 4. The light emitting device according to claim 2, wherein each of the pair of element electrodes is joined to the plurality of through electrodes via a metal joining layer.
5. the substrate is formed by bonding together a first substrate made of plate-shaped single crystal silicon and a second substrate made of single crystal silicon having an opening in the shape of the recess, 5. The light emitting device according to claim 1, wherein a buried oxide film is formed on a surface of the first substrate on the side of the second substrate.
6. 6. The light emitting device according to claim 1, wherein the thermal expansion coefficient of the light-transmitting member is not less than 3×10 −6 / ° C. and not more than 5×10 −6 / ° C.
7. 7. The light emitting device according to claim 1, wherein the thickness of the thermal oxide film on the upper surface of the substrate other than the bonding portion is 0.8 [mu]m or more and 1.2 [mu]m or less.
8. 4. The light emitting device according to claim 2, wherein the thermal oxide film formed on the inner surface of the through hole has a thickness of 0.8 μm or more and 1.2 μm or less.
9. 8. The light emitting device according to claim 1, wherein the thickness of the thermal oxide film at the junction is at least 0.5 times the thickness of the thermal oxide film other than the junction.
10. A method for manufacturing a light emitting device, comprising the steps of: a step of preparing a composite substrate having a first substrate made of single crystal silicon, an oxide film made of silicon oxide formed on the first substrate, and a second substrate made of single crystal silicon bonded onto the first substrate via the oxide film, the composite substrate having a plurality of element mounting regions on an upper surface thereof defined by lattice-shaped parting lines; a hole forming step of forming a plurality of columnar holes extending from a lower surface of the composite substrate to the oxide film in one of the plurality of element mounting regions; a recess forming step of forming a plurality of recesses in the upper surface of the composite substrate in each of the plurality of element mounting regions, the recesses extending from the upper surface of the composite substrate to the oxide film and having a bottom surface in a region including the one region; an oxide film removing step of removing the oxide film exposed on the bottom surface of each of the plurality of recesses to connect the plurality of holes to the bottom surface of each of the plurality of recesses; a thermal oxide film forming step of forming a thermal oxide film having a thickness of 0.8 μm to 1.2 μm on a lower surface of the composite substrate, on the upper surface of the composite substrate, and on inner surfaces of each of the plurality of holes; a through electrode forming step of forming a columnar through electrode by electrolytic plating so as to fill the inside of each of the plurality of holes; a die bonding step of mounting a light emitting element on the bottom surface of each of the plurality of recesses; a light-transmitting member bonding process for placing a light-transmitting member made of glass having a frit glass layer on one surface facing the top surface of the composite substrate so as to cover each of the plurality of recesses, and bonding the light-transmitting member to the top surface of the composite substrate by scanning a laser from above on the frit glass layer along the periphery of each of the plurality of recesses; a dicing step of cutting the composite substrate along the dividing lines to separate the composite substrate, a thickness of a thermal oxide film at a joint portion of an upper surface of the composite substrate with the light-transmitting member being 0.5 times or more a thickness of a thermal oxide film at a portion other than the joint portion of the upper surface of the composite substrate after the light-transmitting member joining step.
11. A method for manufacturing a light emitting device, comprising the steps of: providing a substrate made of single crystal silicon and having a device mounting area with a recess; a thermal oxide film forming step of forming a thermal oxide film on an upper surface of the substrate; a die bonding step of mounting a light emitting element in the recess; a transparent member bonding process for disposing a transparent member made of glass having a glass frit layer on the upper surface of the substrate so as to cover the recessed portion and to face the glass frit layer side of the substrate, and melting the glass frit layer to bond the transparent member to the upper surface of the substrate; Including, a thickness of the thermal oxide film at the bonding portion is 0.5 times or more the thickness of the thermal oxide film other than the bonding portion, the thickness of the thermal oxide film at the bonding portion being 0.5 times or more the thickness of the thermal oxide film other than the bonding portion, the thickness of the thermal oxide film at the bonding portion being 0.5 times or more the thickness of the thermal oxide film other than the bonding portion,
Citation Information
Patent Citations
Light-emitting device
JP2008270707A
Substrate manufacturing method
JP2009076752A
Light emitting device
JP2010278317A
Light emission device and manufacturing method for the same
JP2016127249A
Wiring board, substrate, through electrode substrate, optical device, and display device
JP2018148068A