Carbon-based metal adsorbent
The carbon-based metal adsorbent with controlled surface area, carboxy groups, and nitrogen content improves metal adsorption performance, addressing the inefficiencies of existing adsorbents and enhancing the removal of metals from wastewater.
Patent Information
- Application Number
- JP2022136073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-29
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-08-29
AI Technical Summary
Existing adsorbents do not effectively adsorb metals from wastewater, leading to environmental pollution and health risks, and there is a need for improved metal adsorption performance.
A carbon-based metal adsorbent with a specific surface area of 100-4000 m²/g, carboxy group amount of 0.6-5.0 meq/g, nitrogen content of 3-100 μeq/g based on basic functional groups, and controlled ratios of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen, along with appropriate pore volume and average pore diameter, enhances metal adsorption.
The carbon-based metal adsorbent exhibits superior metal adsorption performance, particularly for metals in Groups 3 to 15 of the periodic table, outperforming conventional adsorbents in terms of metal adsorption capacity.
Smart Images

Figure 0007576596000003 
Figure 0007576596000004 
Figure 0007576596000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon-based metal adsorbent. [Background technology]
[0002] Even trace amounts of metals contained in wastewater from factories can cause river and soil pollution, and also have adverse effects on the human body. Metals must be removed as impurities from liquids such as cleaning water used in the manufacturing process of products. For this reason, porous adsorbents such as activated carbon are used as a means of removing metals from liquids such as purified water and wastewater.
[0003] In recent years, techniques have been proposed for further improving the metal adsorption performance by modifying porous adsorbents. For example, Patent Document 1 discloses activated carbon obtained by activating a carbonaceous material with an acidic gas, and further treating the activated carbon with an oxidizing agent to control the total amount of acidic functional groups and the amount of acidic functional groups derived from carboxylic acids. Patent Document 2 discloses a porous body in which a nitrogen-containing organic compound is introduced into the pores of a metal oxide porous body and the organic compound is thermally decomposed to form a skeleton in the pores of the body consisting of carbon and nitrogen atoms. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-315243 A [Patent Document 2] JP 2004-168587 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide an adsorbent having excellent adsorption performance for metals. [Means for solving the problem]
[0006] The metal adsorbent of the present invention has the following configuration. [1] Specific surface area is 100 to 4000 m 2 / g, The amount of carboxyl group is 0.6 to 5.0 meq / g, and The nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups is 3 to 100 μeq / g; A carbon-based metal adsorbent.
[0007] [2] The ratio of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen obtained by elemental analysis of the carbon-based metal adsorbent is 1 to 20 mass%; and The amount of the basic functional group is more than 0.17 meq / g and 0.60 meq / g or less, The carbon-based metal adsorbent according to [1].
[0008] [3] The total amount of acidic functional groups is 1.5 to 5.0 meq / g, and The ratio of carboxyl groups to the total amount of acidic functional groups is 31-100%. The carbon-based metal adsorbent according to [1].
[0009] [4] The carbon-based metal adsorbent according to [1], wherein the carbon-based metal adsorbent is an alkali-activated activated carbon.
[0010] [5] The carbon-based metal adsorbent according to [1], wherein the metal is a metal belonging to Groups 3 to 15 of the periodic table.
[0011] [6] A metal remover or a metal carrier using the carbon-based metal adsorbent according to any one of [1] to [5]. Effect of the Invention
[0012] According to the present invention, it is possible to provide a carbon-based metal adsorbent having excellent adsorption performance for metals, particularly metals belonging to Groups 3 to 15 of the periodic table. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the amounts of metal adsorption in Example 1 and Comparative Example 2. [Diagram 2] FIG. 2 is a graph showing the amount of metal adsorption in Example 2 and Comparative Examples 3 and 5. [Diagram 3] FIG. 3 is a graph showing the amounts of metal adsorption in Example 3 and Comparative Example 4. [Figure 4] FIG. 4 is a graph showing the amounts of metal adsorption in Example 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The carbon-based metal adsorbent of the present invention has a specific surface area of 100 to 4000 m 2 / g, the amount of carboxy groups is 0.6 to 5.0 meq / g, and the nitrogen content in the amount of basic functional groups in the carbon-based metal adsorbent is 3 to 100 μeq / g. The nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups is the value obtained by multiplying the amount of basic functional groups by the ratio of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen obtained by elemental analysis of the carbon-based metal adsorbent. In particular, the carbon-based metal adsorbent of the present invention exhibits superior metal adsorption performance by appropriately controlling (I) the amount of carboxyl groups and (II) the nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups, as compared with conventional adsorbents in which these are not controlled.
[0015] Carbon-based metal adsorbent The carbon-based metal adsorbent of the present invention is an adsorbent mainly composed of carbon. The term "mainly composed of carbon" means that the ratio of carbon to the total amount of carbon, nitrogen, hydrogen, and oxygen obtained by analyzing the carbon-based metal adsorbent with an elemental analyzer is preferably 50% by mass or more, more preferably 55% by mass or more, even more preferably 60% by mass or more, and even more preferably 65% by mass or more. The carbon-based metal adsorbent is a porous body having pores, and metals are adsorbed in the pores. A preferred carbon-based metal adsorbent having such properties is alkali-activated activated carbon (sometimes called alkali-activated carbon). The excellent metal adsorption performance of the present invention means a larger amount of metal adsorption compared to a conventional porous adsorbent having a comparable specific surface area. Since the metal adsorption amount of an adsorbent increases with increasing specific surface area, the comparison is made with the specific surface area being the same. The metal to be adsorbed is not particularly limited, but is preferably a metal belonging to Groups 3 to 15 of the periodic table, more preferably Groups 3 to 14 of the periodic table, even more preferably Groups 3 to 11 of the periodic table, and even more preferably Groups 8 to 11 of the periodic table. The metal to be adsorbed in the present invention may be a metal belonging to Groups 8 to 14 of the periodic table. Alternatively, the metal to be adsorbed in the present invention may be preferably any one or more heavy metals, more preferably any one or more transition metals, and even more preferably at least one selected from the group consisting of cobalt, iron, copper, and lead.
[0016] specific surface area The specific surface area of the carbon-based metal adsorbent of the present invention is 100 to 4000 m 2 / g. Increasing the specific surface area increases the contact area with the medium to be treated, such as a metal-containing solution, thereby improving the treatment performance and increasing the amount of metal adsorption. On the other hand, if the specific surface area is too large, the amount of acidic functional groups such as carboxyl groups decreases, and the nitrogen content in the carbon-based metal adsorbent decreases, so that the desired metal adsorption performance may not be achieved. The specific surface area of the carbon-based metal adsorbent is preferably 250 m 2 / g or more, more preferably 1000m 2 / g or more, more preferably 1500m 2 / g or more, and even more preferably 2000m 2 / g or more, preferably 3500m 2 / g or less, more preferably 3000m 2 / g or less.
[0017] Pore volume In the present invention, it is also a preferred embodiment to appropriately control the pore volume of the carbon-based metal adsorbent. If the pore volume is too small, sufficient metal adsorption capacity may not be ensured, whereas if the pore volume is too large, the material becomes bulky, reducing the loading amount during use and increasing the number of fine pores that are not suitable for metal adsorption, which may result in reduced metal adsorption performance. The pore volume of the carbonaceous metal adsorbent is preferably 0.05 ml / g or more, more preferably 0.1 ml / g or more, and is preferably 2.5 ml / g or less, more preferably 2.0 ml / g or less.
[0018] Average pore size In the present invention, it is also a preferred embodiment to appropriately control the average pore size of the carbon-based metal adsorbent. If the average pore size is too small, the metals are difficult to enter the pores, and sufficient adsorption performance may not be obtained. On the other hand, if the average pore size is too large, the material becomes bulky and the loading amount during use may decrease. The average pore diameter of the carbon-based metal adsorbent is preferably 0.5 nm or more, more preferably 1.0 nm or more, even more preferably 1.5 nm or more, and preferably 4 nm or less, more preferably 3.5 nm or less, even more preferably 3.0 nm or less, and even more preferably 2.5 nm or less.
[0019] Total acidic functional group amount The total acidic functional groups include all acidic functional groups, such as carboxyl groups, carbonyl groups, phenol groups, lactone groups, etc., which are measured by the method described in the Examples. In the present invention, it is also a preferred embodiment to appropriately control the total amount of acidic functional groups in the carbon-based metal adsorbent. When the total amount of acidic functional groups increases, the content of carboxyl groups that can be ion-exchanged with metal ions increases, and the carbon-based metal adsorbent exhibits excellent metal adsorption performance. If the total amount of acidic functional groups is too small, it may not be possible to ensure a sufficient amount of carboxyl groups. On the other hand, if the total amount of acidic functional groups is too large, the nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups may decrease. The total amount of acidic functional groups contained in the carbon-based metal adsorbent of the present invention is preferably 1.5 meq / g or more, more preferably 1.7 meq / g or more, even more preferably 2.0 meq / g or more, even more preferably 2.2 meq / g or more, and most preferably 2.5 meq / g or more, and is preferably 5.0 meq / g or less, more preferably 4.0 meq / g or less, even more preferably 3.5 meq / g or less, and even more preferably 3.0 meq / g or less.
[0020] Carboxylic acid content The amount of carboxy groups contained in the carbon-based metal adsorbent of the present invention is 0.6 to 5.0 meq / g. A high carboxyl group content improves the metal adsorption performance, whereas an excessively high carboxyl group content reduces the nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups, resulting in a decrease in the metal adsorption performance. The carboxy group content is preferably 0.61 meq / g or more, more preferably 0.65 meq / g or more, even more preferably 0.69 meq / g or more, still more preferably 0.7 meq / g or more, and is preferably 4.0 meq / g or less, more preferably 3.5 meq / g or less, even more preferably 3.0 meq / g or less, still more preferably 2.5 meq / g or less, and most preferably 2.0 meq / g or less.
[0021] Ratio of carboxyl groups to total acidic functional groups In the present invention, it is also a preferred embodiment to appropriately control the ratio of the amount of carboxyl groups to the total amount of acidic functional groups in the carbon-based metal adsorbent. The higher the ratio of the amount of carboxyl groups, the more improved the metal adsorption performance. The ratio of the amount of carboxy groups to the amount of all acidic functional groups is preferably 31% or more, more preferably 32% or more, and is preferably 100% or less, more preferably 80% or less, even more preferably 60% or less, and even more preferably 40% or less.
[0022] Amount of basic functional groups In the present invention, it is also a preferred embodiment to appropriately control the amount of basic functional groups contained in the carbon-based metal adsorbent. The basic functional group is a functional group having a positive charge, such as an amino group, and includes all basic functional groups that can be measured by the method described in the Examples. If the content of basic functional groups is too low, the nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups falls outside the above range, and the metal adsorption performance may decrease. On the other hand, if the amount of basic functional groups is too high, the amount of carboxy groups decreases, and the adsorption performance for metals may decrease. The content of basic functional groups is preferably more than 0.17 meq / g, more preferably 0.2 meq / g or more, even more preferably 0.3 meq / g or more, still more preferably 0.35 meq / g or more, and is preferably 0.60 meq / g or less, more preferably 0.5 meq / g or less, even more preferably 0.4 meq / g or less.
[0023] Nitrogen ratio In the present invention, it is also a preferred embodiment to control the ratio of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen obtained by elemental analysis of the carbon-based metal adsorbent. Increasing the nitrogen ratio in the carbon-based metal adsorbent increases the nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups, improving the metal adsorption performance. If the nitrogen ratio is too high, the specific surface area and the amount of carboxyl groups may decrease, resulting in an imbalance and a decrease in the metal adsorption performance. The nitrogen ratio is calculated by analyzing the carbon-based metal adsorbent with an elemental analyzer to calculate the ratio of the nitrogen amount to the total amount of carbon, nitrogen, hydrogen, and oxygen. The oxygen amount is a value calculated based on the formula described in the examples. The ratio of the amount of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen is preferably 1 mass% or more, more preferably 1.5 mass% or more, even more preferably 2.0 mass% or more, and is preferably 20 mass% or less, more preferably 18 mass% or less, even more preferably 16 mass% or less, and still more preferably 15 mass% or less.
[0024] Nitrogen content in carbon-based metal adsorbents relative to the amount of basic functional groups In the carbon-based metal adsorbent of the present invention, the nitrogen content in the basic functional group amount in the carbon-based metal adsorbent is 3 to 100 μeq / g. When the amount of carboxyl groups is within the above-mentioned range, and the nitrogen content in the amount of basic functional groups in the carbon-based metal adsorbent is within a specified range, the carbon-based metal adsorbent exhibits excellent metal adsorption performance. The more the nitrogen content in the amount of basic functional groups in the carbon-based metal adsorbent is, the more the metal adsorption performance improves, but if it is too high, the carboxyl group content decreases and the metal adsorption performance decreases. The nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups is preferably 4 μeq / g or more, more preferably 5 μeq / g or more, even more preferably 7 μeq / g or more, still more preferably 10 μeq / g or more, and is preferably 80 μeq / g or less, more preferably 70 μeq / g or less, even more preferably 60 μeq / g or less, and still more preferably 50 μeq / g or less.
[0025] The carbon-based metal adsorbent of the present invention may be formed into a shape according to the application, and examples of such shapes include powder, granules, crushed (granular), fibrous, etc. Furthermore, the carbon-based metal adsorbent may be formed into any shape, such as a cylinder, sphere, sheet, etc., together with a binder or other adsorbent as necessary.
[0026] The carbon-based metal adsorbent of the present invention may be of any size and can be pulverized to a desired size using a pulverizing device such as a ball mill. The pulverization may be carried out during or after the production process.
[0027] The carbon-based metal adsorbent of the present invention has excellent adsorption performance for metal components present in a liquid phase. Examples of the liquid phase include water, organic solvents, and other liquids depending on various applications, and the carbon-based metal adsorbent exhibits extremely excellent adsorption performance in removing metal components contained in the liquid. The carbon-based metal adsorbent of the present invention is useful, for example, for removing impurities in a plating solution and recovering metals from metal-containing waste liquid. The carbon-based metal adsorbent of the present invention may be used to form a metal remover. Also, the carbon-based metal adsorbent of the present invention may be used as a metal support for catalysts and other applications by adsorbing a desired metal.
[0028] Hereinafter, a method for producing alkali-activated activated carbon, which is a preferred embodiment of the carbon-based metal adsorbent of the present invention, will be described, but the production method of the present invention is not limited to the following production method as long as the desired physical properties are obtained, and the production conditions can be changed as appropriate. Note that the following production conditions indicate preferred ranges, and each production condition must be appropriately adjusted to obtain the desired physical properties.
[0029] (Activating materials) The activation raw material of the present invention is a carbonaceous material carbide containing nitrogen. In the present invention, by using the carbonaceous material carbide containing nitrogen as the activation raw material, the nitrogen content in the carboxyl group amount and basic functional group amount of the carbonaceous metal adsorbent obtained by activation can be controlled within the above range. The nitrogen content of the activation raw material is preferably 3% by mass or more, more preferably 5% by mass or more, even more preferably 7% by mass or more, still more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and still more preferably 20% by mass or less.
[0030] Examples of nitrogen-containing carbonaceous materials include nitrogen-containing resins such as melamine resins, guanidine resins, urea resins, aniline resins, sulfonamide resins, imide resins, urethane resins, nitrile resins such as polyacrylonitrile, polybenzimidazole resins, carbazole resins, acridine resins, pyridine resins, and pyrrole resins. In particular, polyacrylonitrile resins are preferred because they contain a large amount of nitrogen in the activated carbon after activation. The nitrogen-containing resin may be a copolymer containing a nitrogen-containing monomer as the main component and other monomers as subcomponents. The nitrogen-containing resins may be used alone or in combination of two or more kinds.
[0031] (Carbonization process) The activation raw material is obtained by carbonizing the nitrogen-containing carbonaceous material before activation. The carbonization treatment is performed by heat treating the nitrogen-containing carbonaceous material in an inert gas such as nitrogen, for example by holding it at 400°C to 1000°C for 1 hour to 3 hours.
[0032] (Alkaline activation treatment process) The activation treatment step of the present invention is an alkali activation treatment in which an activator containing an alkali metal compound is mixed with an activation raw material and heated in an inert gas to obtain activated carbon. In the alkali activation treatment step of the present invention, an alkali metal compound is used as an alkali activator. Examples of the alkali metal compound include alkali metal hydroxides such as potassium hydroxide and sodium hydroxide, alkali metal carbonates such as potassium carbonate and sodium carbonate, and alkali metal sulfates such as potassium sulfate and sodium sulfate. An alkali metal hydroxide is preferred, and potassium hydroxide is more preferred.
[0033] Regarding the amount of activator used, the higher the mixing ratio of the activator to the activation raw material, the larger the specific surface area of the activated carbon tends to be. On the other hand, if the mixing ratio of the activator is too high, the density of the activated carbon tends to decrease. In the present invention, the mixing ratio of the activator may be adjusted so as to obtain the above-mentioned specific surface area, and the mass ratio of the activator to the activation raw material (mass of activator / mass of activation raw material) is preferably 0.5 or more, more preferably 1.0 or more, even more preferably 2.0 or more, and preferably 10.0 or less, more preferably 5.0 or less, even more preferably 4.0 or less. The alkali activation treatment of the present invention is carried out in an atmosphere of any inert gas such as argon, helium, or nitrogen.
[0034] If the alkali activation treatment temperature of the present invention is too low, a sufficient specific surface area and amount of carboxyl groups cannot be secured, whereas if the activation temperature is too high, nitrogen and carboxyl groups are released and the desired amounts cannot be secured. The heating temperature during the alkali activation treatment is preferably 350° C. or higher, more preferably 400° C. or higher, and is preferably 800° C. or lower, more preferably 750° C. or lower, and further preferably 700° C. or lower. The rate of temperature rise to the above heating temperature is preferably 1° C. / min or more, more preferably 5° C. / min or more, and is preferably 20° C. / min or less, more preferably 15° C. / min or less. The activation treatment time in the above heating temperature range is preferably 1 hour or more, more preferably 2 hours or more, and is preferably 10 hours or less, more preferably 5 hours or less.
[0035] (Cleaning process) The washing step is a step in which the activated carbon after the alkali activation treatment is washed with water or with an inorganic acid to remove the alkali metals remaining in the activated carbon. The rate of alkali metal removal can be increased by repeating the washing step multiple times. (Water cleaning treatment) The temperature of the water used in the water washing treatment is preferably 20° C. or higher, more preferably 30° C. or higher, and is preferably 100° C. or lower, more preferably 95° C. or lower. The water washing treatment is desirably performed by repeating water washing and filtration multiple times until the pH of the filtrate becomes 7.0 or lower.
[0036] (Inorganic acid cleaning treatment) In the inorganic acid washing treatment, hydroacids such as hydrochloric acid and hydrofluoric acid, and oxygen acids such as sulfuric acid, nitric acid, phosphoric acid, and perchloric acid can be used as inorganic acids, and hydrochloric acid is preferred. From the viewpoint of increasing the alkali metal removal rate while maintaining the physical properties of the activated carbon, it is preferred to adjust the inorganic acid concentration so that the inorganic acid is 10 to 100 parts by mass per 100 parts by mass of activated carbon. The liquid temperature of the inorganic acid aqueous solution is preferably set to a temperature range that can increase the alkali metal removal efficiency in the activated carbon while suppressing the volatilization of the inorganic acid, and is preferably 20°C or higher, more preferably 30°C or higher, and preferably 100°C or lower, more preferably 95°C or lower. In the inorganic acid washing treatment, washing and filtration are repeated multiple times, and it is preferred to perform the treatment until the amount of potassium remaining in the activated carbon is 5000mg / kg or less (more than 0mg / kg), more preferably the amount of alkali metal remaining in the activated carbon is 2500mg / kg or less (more than 0mg / kg), and even more preferably 1000mg / kg or less (more than 0mg / kg). The amount of alkali metal remaining can be measured by an ICP emission spectrometer.
[0037] (Water washing process) As a post-treatment step following the inorganic acid washing treatment, a water washing treatment is carried out to remove inorganic acids remaining in the activated carbon. In order to increase the efficiency of removing inorganic acids, the temperature of the water used in the water washing treatment is preferably 20° C. or higher, more preferably 30° C. or higher, and even more preferably 50° C. or higher, and is preferably 100° C. or lower, and more preferably 95° C. or lower. The water washing treatment is desirably carried out by repeating water washing and filtration multiple times until the pH of the filtrate becomes 6.5 or higher.
[0038] (Drying process) After the washing treatment, the activated carbon may be dried by a drying treatment. The drying may be performed under conditions that can remove the moisture remaining in the activated carbon, and it is preferable to heat the activated carbon in the air (for example, at 100 to 150° C.) for 0.5 to 24 hours. In the present invention, the alkaline activated carbon obtained by the activation treatment is not subjected to a high-temperature heat treatment (for example, above 150° C.). If the alkaline activated carbon is subjected to a high-temperature heat treatment, the amount of acidic functional groups and the specific surface area are reduced, and the metal adsorption performance is reduced.
[0039] The alkali activated carbon obtained by appropriately adjusting each production condition has the above-mentioned configuration as the carbon-based metal adsorbent of the present invention. EXAMPLES
[0040] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and it is possible to carry out the present invention by making appropriate modifications within the scope of the above and below-mentioned aims, and all of these modifications are included in the technical scope of the present invention.
[0041] Example 1 Activation raw materials Polyacrylonitrile (PAN) resin was charged into a muffle furnace (manufactured by Koyo Thermos) as a carbonaceous material, and the temperature inside the furnace was raised to 650°C (heating rate: 10°C / min) under a nitrogen atmosphere and held at that temperature for 2 hours. The resulting PAN resin carbonized material was used as the activation raw material. Activation treatment process A commercially available alkaline activator (48.5% potassium hydroxide aqueous solution) was added as an activator to the obtained PAN resin carbonized material so that the mass ratio ([mass of alkaline component of activator] / [mass of activation raw material]: hereinafter referred to as KOH / C ratio) was 2.0, and the temperature was raised to 400°C in a nitrogen atmosphere and maintained at that temperature for 3.75 hours to obtain alkaline activated carbon.
[0042] Water washing process The obtained alkali activated carbon was repeatedly washed with warm water at 60°C until the pH of the filtrate became 7.0 or less. Inorganic acid washing process The alkali-activated carbon was then washed with a 5.25 wt % aqueous hydrochloric acid solution for 1 hour, and then subjected to suction filtration. Post-processing process (washing process) Furthermore, the alkali activated carbon after filtration was repeatedly washed with hot water at 60°C until the pH of the filtrate reached 6.5 or higher. Drying process The obtained alkali activated carbon was dried for 24 hours in a dryer set at 115° C. to obtain Activated Carbon 1.
[0043] Example 2 Activated carbon 2 was obtained in the same manner as in Example 1, except that the activation temperature was 600° C. and the KOH / C ratio was 3.0.
[0044] Example 3 Activated carbon 3 was obtained in the same manner as in Example 1 except that the activation temperature was 650° C. and the KOH / C ratio was 2.5.
[0045] Comparative Example 1 The activated carbon No. 2 was placed in a small furnace and heated to 450° C. in a nitrogen atmosphere (heating rate: 10° C. / min).
[0046] Comparative Example 2 Comparative activated carbon 2 was obtained in the same manner as in Example 1, except that the carbonaceous material was changed from PAN resin to petroleum coke (DPC) and the KOH / C ratio was set to 1.0.
[0047] Comparative Example 3 Comparative activated carbon 3 was obtained in the same manner as in Example 1, except that the carbonaceous material was changed from PAN resin to petroleum coke, the activation temperature was set to 600° C., and the KOH / C ratio was set to 5.0.
[0048] Comparative Example 4 Comparative activated carbon 4 was obtained in the same manner as in Example 1, except that the carbonaceous material was changed from PAN resin to petroleum coke, the activation temperature was set to 650° C., and the KOH / C ratio was set to 3.0.
[0049] Comparative Example 5 Activation raw materials Phenolic resin was charged into a muffle furnace (manufactured by Koyo Thermos) as a carbonaceous material, and the temperature inside the furnace was raised to 700°C (heating rate: 10°C / min) under a nitrogen atmosphere and held at that temperature for 2 hours. The resulting spherical phenolic resin carbonized material was used as the activation raw material. Activation treatment process The activated carbon of Comparative Example 5 was obtained in the same manner as in Example 1, except that the activation temperature was 600° C. and the KOH / C ratio was 3.0.
[0050] evaluation Each of the above activated carbons was pulverized in a disk mill so that the particle size at 50% cumulative frequency on a volume basis (D50) was about 8 to 12 μm, and then subjected to each analysis. The particle size of the pulverized activated carbon (sample) was measured using a laser diffraction particle size distribution analyzer (Shimadzu Corporation, SALD (registered trademark)-2200). A volume-based cumulative frequency curve was calculated from the particle size distribution measurement results, and the particle size at 50% cumulative frequency (D50) was defined as the average particle size.
[0051] specific surface area Activated carbon (0.2 g) was vacuum-dried at 250°C, and then the amount of nitrogen gas adsorbed in a liquid nitrogen atmosphere (-196°C) was measured using a nitrogen adsorption apparatus (Micromeritics ASAP-2420) to obtain a nitrogen adsorption isotherm, and the specific surface area (m2 / g) was calculated using the BET method.
[0052] Total Pore Volume The total pore volume (mL / g) was calculated from the amount of nitrogen adsorbed at a relative pressure (P / P0) of 0.93 from the nitrogen adsorption isotherm.
[0053] Average pore diameter (4V / A) The pores of the activated carbon were assumed to be cylindrical, and the average pore diameter was calculated based on the following formula. Average pore diameter (nm) = 4 × total pore volume (mL / g) / specific surface area (m 2 / g) x 1000
[0054] Total acidic functional groups The total amount of acidic functional groups was determined according to the Boehm method (reference: HP Boehm, Adzan. Catal, 16, 179 (1966)). Specifically, 50 mL of sodium ethoxide aqueous solution (0.1 mol / L) was added to 1 g of activated carbon, stirred at 500 rpm for 2 hours, and then left for 24 hours. After 24 hours, the mixture was stirred for an additional 30 minutes and filtered. 0.1 mol / L hydrochloric acid was added dropwise to 25 mL of the obtained filtrate, and the amount of hydrochloric acid titrated when the pH reached 4.0 was measured. As a blank test, 0.1 mol / L hydrochloric acid was added dropwise to 25 mL of the sodium ethoxide aqueous solution (0.1 mol / L) to measure the amount of hydrochloric acid titrated when the pH reached 4.0. The total amount of acidic functional groups (meq / g) was calculated using the following formula. Total acidic functional group amount (meq / g)=[(ab)×0.1] / [(S×25) / 50] a: Hydrochloric acid titration volume in blank test (mL) b: Amount of hydrochloric acid titrated when the sample was reacted (mL) S: Sample weight (g)
[0055] Individual acidic functional groups The 0.1 mol / 1000 mL aqueous solution of sodium ethoxide (NaOEt) was changed to 0.1 mol / 1000 mL NaOH, 0.05 mol / 1000 mL Na2CO3, or 0.1 mol / 1000 mL NaCO3, and the evaluation was carried out in the same manner as for the total amount of acidic functional groups. In addition, the calculation of each acidic functional group was performed using the following formula.
[0056] [Table 1]
[0057] The method for quantifying the amount of functional groups in activated carbon is generally known and is based on [Hymen, 34[2](1996) Otoha p.62] or [Catal.,1966
[16] (USA) p.179]. Specifically, 1g of activated carbon is placed in a 100mL Erlenmeyer flask, 50mL each of N / 10 alkaline reagents ((a) sodium bicarbonate, (b) sodium carbonate, (c) caustic soda, (d) sodium ethoxide) are added, and the mixture is shaken for 24 hours, after which the unreacted alkaline reagent is titrated with N / 10 hydrochloric acid. The amount of functional groups is quantified by subtracting the titration amount of each, since the carboxyl group reacts with all of the reagents (a)-(d), the lactone group reacts with the reagents (b)-(d), the hydroxyl group reacts with the reagents (c)-(d), and the quinone group reacts with the reagent (d).
[0058] Basic Functional Group The amount of basic functional groups was determined by back titration when measuring the total amount of acidic functional groups. Specifically, 50 mL of hydrochloric acid (0.1 mol / L) was added to 1 g of activated carbon, and the mixture was stirred at 500 rpm for 2 hours, and then left for 24 hours. After 24 hours, the mixture was stirred for another 30 minutes and separated by filtration. 0.1 mol / L sodium hydroxide was dropped into 25 mL of the obtained filtrate, and the amount of sodium hydroxide titrated when the pH became 8.0 was measured. In addition, as a blank test, 0.1 mol / L sodium hydroxide was dropped into 25 mL of the hydrochloric acid (0.1 mol / L) and the amount of sodium hydroxide titrated when the pH became 8.0 was measured. The amount of basic functional groups (meq / g) was then calculated by the following formula. Amount of basic functional group (meq / g) = [(cd) x 0.1] / [(S x 25) / 50] c: Sodium hydroxide titration amount in blank test (mL) d: The amount of sodium hydroxide titrated when the sample was reacted (mL) S: Sample mass (g)
[0059] Carbon, Hydrogen, Nitrogen, Oxygen The mass percentages (mass%) of carbon (C), hydrogen (H), and nitrogen (N) contained in the sample were measured using a CHN coder (JM1000HCN, manufactured by J Science Labs). The amount of oxygen (O) in the sample (mass%) was calculated from the obtained percentages (mass%) of C, H, and N according to the following formula. O amount (mass %) = 100 mass % - C amount (mass %) - H amount (mass %) - N amount (mass %)
[0060] Carboxy group The ratio of the amount of carboxyl groups to the total amount of acidic functional groups was calculated from the total amount of acidic functional groups (meq / g) and the amount of carboxyl groups (R-COOH groups) (meq / g) according to the following formula. Carboxylic group ratio = Carboxylic group amount (meq / g) / Total acidic functional group amount (meq / g) × 100
[0061] Basic nitrogen functional group The amount of basic nitrogen functional groups was calculated based on the amount of basic functional groups (meq / g) and the amount of N (mass%) obtained by elemental analysis according to the following formula. Amount of basic nitrogen functional group = Amount of basic functional group (meq / g) × Amount of N (mass%) / 100 × 1000 (unit adjustment)
[0062] metal-containing aqueous solution The metal reagent was added to a 1-L measuring flask so that the initial concentration C0 (mg / L) was 100 mg / L, and then the solution was made up to the mark with pure water to prepare each metal-containing aqueous solution. The following reagents were used to prepare the metal-containing aqueous solutions. Cobalt (Co)-containing aqueous solution: CoCl2·hexahydrate (Kishida Chemical Co., Ltd., special grade, purity 99%) Iron (Fe)-containing aqueous solution: FeCl3·hexahydrate (Kishida Chemical Co., Ltd., special grade, purity 99%) ·Copper (Cu) containing aqueous solution: CuSO4 pentahydrate (manufactured by Kishida Chemical Co., Ltd., special grade, purity 99.5%) ·Lead (Pb) containing aqueous solution: PbCl2 (manufactured by Kishida Chemical Co., Ltd., special grade, purity 98%)
[0063] Metal adsorption amount 0.1 g of activated carbon dried for 2 hours in a dryer set at 115 ° C. was added to a 100 mL Erlenmeyer flask, and 100 mL of the above metal-containing aqueous solution prepared so that the initial concentration C0 (mg / L) was 100 mg / L was added, and the mixture was stirred at 500 rpm for 24 hours in a thermostatic bath at 25 ° C. After stirring for 24 hours, the activated carbon was filtered off with a syringe filter, and the obtained filtrate was measured using an ICP emission spectrometer (manufactured by Thermo Electron Co., Ltd.) to quantify the metal concentration C1 (mg / L) remaining after adsorption. The amount of metal adsorption (mg / g) per weight of activated carbon was calculated from the metal concentrations (mg / L) before and after adsorption based on the following formula. Metal adsorption amount (mg / g)=[(C0(mg / L)-C1(mg / L))×0.1(L)] / 0.1(g)
[0064] [Table 2]
[0065] Since the amount of adsorption varies depending on the specific surface area, the results of comparing the Examples and Comparative Examples for each specific surface area based on the above results are shown in Figures 1 to 4. Note that from the left in the figure, the amounts of adsorption of Co, Fe, Cu, and Pb are shown. As shown in FIG. 1, Comparative Example 2 had a larger specific surface area than Example 1, but the adsorption amount of each metal was smaller. Similarly, as shown in FIGS. 2 to 4, Examples 2 and 3 also had larger adsorption amounts of each metal than Comparative Examples 1, 3, 4, and 5, which had equivalent specific surface areas. The reason why the adsorption amount of Pb is prominent is that the atomic weight of Pb is larger than those of Co, Fe, and Cu, and the difference is significant when the adsorption amount is converted to mg / g.
[0066] From the above results, the activated carbons 1 to 3 of the present invention, in which the nitrogen content in the carbon-based metal adsorbent relative to the amount of carboxyl groups and basic functional groups is appropriately controlled, exhibited superior metal adsorption performance to the comparative activated carbons 1 to 5, which did not satisfy either or both of the above requirements.
Claims
1. Specific surface area is 100 to 4000 m 2 / g, The amount of carboxyl group is 0.6 to 5.0 meq / g, and The nitrogen content in the carbon-based metal adsorbent relative to the amount of basic functional groups is 3 to 100 μeq / g; A carbon-based metal adsorbent.
2. The ratio of nitrogen to the total amount of carbon, nitrogen, hydrogen, and oxygen obtained by elemental analysis of the carbon-based metal adsorbent is 1 to 20 mass%; and The amount of the basic functional group is more than 0.17 meq / g and 0.60 meq / g or less, 2. The carbon-based metal adsorbent according to claim 1,
3. The total amount of acidic functional groups is 1.5 to 5.0 meq / g, and The ratio of the amount of carboxyl groups to the amount of all acidic functional groups is 31 to 100%, 2. The carbon-based metal adsorbent according to claim 1,
4. The carbon-based metal adsorbent according to claim 1 , wherein the carbon-based metal adsorbent is an alkali-activated carbon.
5. 2. The carbon-based metal adsorbent according to claim 1, wherein the adsorbed metal of the carbon-based metal adsorbent is a metal belonging to Groups 3 to 15 of the periodic table.
6. A metal remover or a metal carrier using the carbon-based metal adsorbent according to any one of claims 1 to 5.
Citation Information
Patent Citations
Preparation and application of nitrogen-rich porous activated carbon adsorbent derived from microporous polymer
CN112892477A
Method of activating electrode constituting substance
JP1979000478A
Nitrogen-containing carbon-based porous body and its manufacturing method
JP2004168587A
Activated carbon and method for manufacturing the same
JP2004315243A
Active carbon fiber and method of producing the same
JP2017172099A