Controlled yield ratio steel and method for producing same

A steel with controlled yield ratio and optimized composition and processing achieves ultra-high strength, toughness, and plasticity, addressing the limitations of existing steels in meeting DNV standards for offshore platforms.

JP7576630B2Active Publication Date: 2024-10-31BAOSHAN IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022551534
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-28
Filing Date
2021-02-07
Publication Date
2024-10-31
Estimated Expiration
2041-02-07

AI Technical Summary

Technical Problem

Existing steels fail to meet the requirements of high strength, toughness, and plasticity, particularly in terms of yield ratio, low-temperature impact toughness, and aging impact energy, as specified by DNV classification society standards for offshore platform mooring chains.

Method used

A steel composition with controlled yield ratio, containing specific mass percentages of elements like C, Si, Mn, P, Cr, Mo, Ni, Cu, V, B, Al, Ti, Ca, H, N, and O, combined with a manufacturing process involving refining, casting, heating, rolling, quenching, and tempering, to form a microstructure of tempered martensite and bainite, ensuring ultra-high strength, toughness, and plasticity.

Benefits of technology

The steel achieves a yield ratio of 0.85 to 0.95, tensile strength of 1,100 MPa or more, Charpy impact energy of over 90 J at -20°C, and a strength-toughness product of 115 GPa*J or more, suitable for high-performance offshore platform mooring chains and mechanical structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576630000003
    Figure 0007576630000003
  • Figure 0007576630000004
    Figure 0007576630000004
  • Figure 0007576630000001
    Figure 0007576630000001
Patent Text Reader

Abstract

A steel with a controlled yield ratio and a method for producing the same is disclosed, the steel containing the following components in mass percent: C: 0.245-0.365%, Si: 0.10-0.80%, Mn: 0.20-2.00%, P: ≤ 0.015%, S: ≤ 0.003%, Cr: 0.20-2.50%, Mo: 0.10-0.90%, Nb: 0-0.08%, Ni: 2.30-4.20%, Cu: 0-0.30%, V: 0.01-0.13%, B: The steel contains 0-0.0020%, Al: 0.01-0.06%, Ti: 0-0.05%, Ca:≦0.004%, H:≦0.0002%, N:≦0.013%, O:≦0.0020%, and the balance is Fe and unavoidable impurities, where the components satisfy (8.57*C+1.12*Ni)≧4.8% and 1.2%≦(1.08*Mn+2.13*Cr)≦5.6%. The steel has excellent low-temperature impact toughness and aging impact toughness at -20°C and -40°C, a reasonably controlled yield ratio, and ultra-high strength, toughness, and plasticity, which can be used in applications requiring high strength and toughness, such as offshore platform mooring chains, machine structures, and automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Technical Field The present invention relates to a steel having high strength and high toughness, in particular a steel having excellent low temperature impact toughness and a controlled yield ratio, and a method for producing the same. [Background technology]

[0002] background High strength and high toughness steels, such as ultra-high strength and ultra-high toughness steel bars and steel plates, are utilized in the fields of offshore platforms, giant machine structures, and high strength sheets for automobiles. The strength grades of round steel for offshore platform mooring chains include tensile strength 690 MPa grade R3, tensile strength 770 MPa grade R3S, tensile strength 860 MPa grade R4, tensile strength 960 MPa grade R4S, tensile strength 1,000 MPa grade R5, and tensile strength 1,100 MPa grade R6. In the ship rules issued by DNV classification society in July 2018, R6 was incorporated into the new ship rules. The technical indicators of R6 are specified in the factory certification summary, the certification of manufacturers DNVGL-CP-0237 Offshore Mooring Chains and Accessories (July 2018 edition) and the chain link standard DNVGL-OS-E302 Offshore Mooring Chains (July 2018 edition), but the main technical indicators of R6 include low-temperature impact energy at -20℃ of 60J or more, tensile strength of 1,100MPa or more, yield strength of 900MPa or more, elongation rate of 12% or more, area reduction rate of 50% or more, aging impact energy at -20℃ of 60J or more (after 5% strain, held at 100℃ for 1h), yield ratio of 0.85~0.95, etc. Mooring chains are used to fix offshore platforms, and have requirements such as ultra-high strength, high toughness, and high corrosion resistance. Considering that offshore platforms need to be constructed in cold climates in sea areas at various latitudes and in high latitude sea areas, the impact performance at an environmental temperature of -40℃ needs to be considered at the same time. If the yield ratio of the mooring chain is too high, easy fracture after deformation may occur, which is detrimental to the safety of the offshore platform. Offshore platform mooring chains require ultra-high strength, high toughness and high plasticity at the same time, and therefore the steel needs to have ultra-high strength, ultra-high toughness and ultra-high plasticity. Offshore platform mooring chains can deform during service and need to have good low-temperature impact toughness when deformation occurs. Therefore, the aging impact energy is an important technical indicator for offshore platform mooring chains.

[0003] Much research on steels with ultra-high strength, ultra-high toughness and ultra-high plasticity has been conducted worldwide. Steels with ultra-high strength and ultra-high toughness usually adopt bainite, bainite + martensite, or martensite microstructures. The bainite or martensite structure contains supersaturated carbon atoms, which can change the lattice constant, inhibit dislocation motion, and improve tensile strength. The refined structure ensures that the steel can absorb more energy under stress to achieve higher tensile strength and impact toughness.

[0004] Chinese patent CN102747303A discloses "High-strength steel plate with 1,100MPa-grade yield strength and its manufacturing method". The high-strength steel plate is a steel plate with ultra-high strength and toughness, with a yield strength of 1,100MPa and low-temperature impact energy (-40℃), and contains the following components in mass percent: C: 0.15-0.25%, Si: 0.10-0.50%, Mn: 0.60-1.20%, P: ≦0.013%, S: ≦0.003%, Cr: 0.20-0.55%, Mo: 0.20-0.55%, and C: 0.015-0.025%. .70%, Ni: 0.60-2.00%, Nb: 0-0.07%, V: 0-0.07%, B: 0.0006-0.0025%, Al: 0.01-0.08%, Ti: 0.003-0.06%, H: ≦0.00018%, N: ≦0.0040%, O: ≦0.0030%, and the balance being Fe and unavoidable impurities, where the carbon equivalent satisfies CEQ ≦0.60%. The steel shall have a yield strength of 1,100 MPa or more, a tensile strength of 1,250 MPa or more, and a Charpy impact energy A of 50 J or more. kv The steel plate disclosed in the patent has ultra-high strength, but the impact performance at -40°C cannot stably reach 70J, and has low elongation, but the aging impact performance and yield ratio are not specified.

[0005] Chinese patent CN103898406A discloses "Steel plate with 890Mpa-grade yield strength and low weld crack susceptibility and its manufacturing method", which adopts heat-controlled mechanical rolling and cooling technology to obtain a steel with high strength toughness and ultrafine bainitic lath matrix structure. The steel plate contains the following components in weight percent: C: 0.06-0.13%, Si: 0.05-0.70%, Mn: 1.2-2.3%, Mo: 0-0.25%, Nb: 0.03-0.11%, Ti: 0.002-0.050%, Al: 0.02-0.15%, and B: 0-0.0020%, where the components satisfy 2Si+3Mn+4Mo≦8.5, and the balance is Fe and unavoidable impurities. The steel plate has a yield strength of more than 800 MPa, a tensile strength of more than 900 MPa, and a Charpy impact energy A of more than 150 J. kv However, in the embodiments of the patent, the area reduction is not specified, while the yield ratio, the low temperature impact energy at -40°C and the aging impact energy are not defined.

[0006] Chinese patent CN107794452A discloses "Automotive strip continuous casting with ultra-high strength plastic area and continuous yield and its manufacturing method", containing the following components in weight percent: C: 0.05-0.18%, Si: 0.1-2.0%, Mn: 3.5-7%, Al: 0.01-2%, P: greater than 0 and ≦0.02%, and the balance being Fe and unavoidable impurities, with a ferrite+austenite+martensite microstructure. The patent employs a three-phase composite technology with a soft phase such as ferrite and a hard phase such as martensite and austenite to produce a steel with a yield strength of ≧650 MPa, a tensile strength of 980 MPa, an elongation of ≧20%, and a strength plastic area of ​​≧20 GPa*%. This type of steel can be utilized for automotive exterior panels. However, the product disclosed by the patent has no provision for yield ratio, impact energy and aging impact, that is, it cannot simultaneously satisfy high strength, plasticity and toughness.

[0007] Chinese patent CN103667953A discloses "Marine mooring chain steel with low environmental cracking susceptibility, ultra-high strength and toughness and its manufacturing method". The steel contains: C: 0.12-0.24%, Mn: 0.10-0.55%, Si: 0.15-0.35%, Cr: 0.60-3.50%, Mo: 0.35-0.75%, N: ≦0.006%, Ni: 0.40-4.50%, Cu: ≦0.50%, S: ≦0.005%, P: 0.005-0.025%, O: ≦0.0015%, and H: ≦0.00015%. The mooring chain steel with high strength and toughness is manufactured by adopting the above ingredients and the second quenching process, and has a tensile strength of more than 1,110 MPa, a yield ratio of 0.88 to 0.92, an elongation rate of more than 12%, a reduction in area of ​​more than 50%, and an impact energy (A) at -20°C of more than 50 J. kv According to the patent, the elongations of the mooring chains are 15.5%, 13.5%, 13.5%, and 15.0%, respectively, and the low-temperature impact energy A at -20°C is kv are 67J, 63J, 57J, and 62J, respectively. The low-temperature impact energy of the product disclosed by the patent cannot stably meet the requirements of DNV classification society for Charpy impact energy of 60J or more. After 5% strain, the steel is aged, which increases the dislocation density in the steel and causes the aggregation of interstitial atoms into dislocations, and therefore the aged impact energy is lower than the conventional impact energy. According to the data of the patent, the aged impact energy A at -20℃ is kv The value of 60J also cannot meet the requirement.

[0008] From the analysis of the above prior art, it can be seen that none of them can satisfy the requirements of high strength, toughness and plasticity, specific yield ratio, and high aging impact energy. Summary of the Invention [Means for solving the problem]

[0009] Summary of the Invention The present invention aims to provide a steel with excellent low-temperature impact toughness and a controlled yield ratio, and a method for producing the same. The steel has excellent low-temperature impact toughness and aging impact toughness at -20°C and -40°C, a reasonably controlled yield ratio, and ultra-high strength, toughness, and plasticity. The steel can be used in applications such as offshore platform mooring chains, machine structures, and automobiles that require high strength and toughness of the steel.

[0010] In order to achieve the above objectives, the technical solutions of the present invention are as follows: A steel with a controlled yield ratio and excellent low-temperature impact toughness, containing the following components in mass percent: C: 0.245-0.365%, Si: 0.10-0.80%, Mn: 0.20-2.00%, P: ≦0.015%, S: ≦0.003%, Cr: 0.20-2.50%, Mo: 0.10-0.90%, Nb: 0-0.08%, Ni: 2.30-4.20%, Cu: 0-0.30%, V: 0.01-0.13%, B: 0-0.0020%, Al: 0.01-0.06%. %, Ti: 0~0.05%, Ca:≦0.004%, H:≦0.0002%, N:≦0.013%, O:≦0.0020%, and the balance being Fe and unavoidable impurities, where the components satisfy (8.57*C+1.12*Ni)≧4.8% and 1.2%≦(1.08*Mn+2.13*Cr)≦5.6%; and the yield ratio controlled steel has a yield ratio of 0.85~0.95, a tensile strength of 1,100 MPa or more, and a yield strength of 900 MPa or more.

[0011] The microstructure of the controlled yield ratio steel provided by the present invention is tempered martensite + tempered bainite.

[0012] The steel with a controlled yield ratio provided by the present invention has a Charpy impact energy A at -20°C of 90 J or more after 5% strain and holding at 100°C for 1 h. kv , Charpy impact energy A at -40℃ of 70J or more kv , Charpy impact energy A at -20℃ of 80J or more kvCharpy impact energy A at -40°C of 60J or more after 5% strain and 1h at 100°C kv , Yield ratio of 0.85 to 0.95, tensile strength of 1,100 MPa or more, yield strength of 900 MPa or more, elongation of 15% or more, area reduction of 50% or more, strength toughness product (tensile strength*Charpy impact energy at -20°C A kv ), and strength plastic product (tensile strength * elongation) of 16GPa*% or more. The controlled yield ratio steel can be used for manufacturing high performance offshore platform mooring chains, structural members, etc. with ultra-high strength and toughness.

[0013] The design concept of the composition of the steel with controlled yield ratio provided by the present invention is as follows: C: Carbon element is dissolved in the octahedrons of the austenitic face-centered cubic lattice at a temperature above the austenitizing temperature. In the cooling process, when the cooling rate is relatively slow, a diffusion phase transformation controlled by the diffusion of carbon atoms can occur. When the cooling rate increases, the supersaturation of carbon in ferrite gradually increases. When the cooling rate exceeds the critical cooling rate of martensite phase transformation, a martensite structure can be formed. According to the present invention, the effect of carbon atoms on the diffusion phase transformation is fully utilized to form martensite and bainite structures with a certain amount of supersaturated carbon, thereby controlling the yield ratio of the martensite and bainite composite phase structure, and at the same time, providing the steel with a relatively high strength. Therefore, in the present invention, the C content is controlled to 0.245-0.365%.

[0014] Si: Si is dissolved in steel and plays a role in solid solution strengthening. The solubility of Si in cementite is very low, so carbide-free bainite structure is formed under relatively high Si content, which reduces impact toughness and plasticity. In the comprehensive consideration of the effect of solid solution strengthening and the effect of Si on brittleness in the present invention, the Si content is controlled to 0.10-0.80%.

[0015] Mn: Mn in steel usually exists in the form of solid solution. When the steel is subjected to external force, the Mn atoms dissolved in the steel inhibit dislocation motion and improve the strength of the steel. However, excessively high content of Mn element will worsen the segregation in the steel, resulting in non-uniformity of structure and non-uniformity of performance. Therefore, in the present invention, 0.20-2.00% Mn is incorporated.

[0016] P: P element can segregate at dislocations and grain boundaries in steel, and reduce the binding energy of grain boundaries. When subjected to low-temperature impact, steel with high P content tends to fracture due to the reduction of the binding energy of grain boundaries. By controlling the P content in ultra-high strength steel, it is beneficial to improve the low-temperature impact toughness of the steel. In the present invention, the P content is limited to not exceed 0.015% to ensure low-temperature impact toughness.

[0017] S: S in steel can form relatively large MnS inclusions together with Mn, which can reduce the low-temperature impact toughness of steel. Meanwhile, MnS inclusions can improve the cutting performance of steel. A certain content of S can be added to easy-to-cut steel to reduce the frequency of tool damage in the steel machining process. Because the type of steel provided by the present invention requires good low-temperature impact toughness, and therefore, in the present invention, the S content does not exceed 0.003%.

[0018] Cr: Cr atoms dissolved in steel can inhibit diffusion phase transformation and improve the hardenability of steel, so that the steel forms a high hardness structure. In the tempering process after quenching, Cr can form carbides with C, and the dispersed carbides are beneficial to improving the strength of steel. Excessively high content of Cr element can form coarse carbides, which affects low-temperature impact performance. Therefore, in the present invention, 0.20-2.50% Cr is incorporated to ensure the strength and low-temperature impact performance of steel.

[0019] Mo: The addition of alloying element Mo in steel can effectively inhibit diffusion phase transformation and promote the formation of bainite and martensite. In the tempering process, Mo can form carbides with C. The fine carbides can reduce the degree of dislocation annihilation in the tempering process, improve the strength of the steel, and ensure the low-temperature impact toughness after tempering. Excessively high Mo content can form larger carbides and reduce the impact energy. In the present invention, 0.10-0.90% Mo is incorporated to obtain the corresponding good strength and toughness.

[0020] Nb: Nb can increase the recrystallization temperature of steel, and Nb in the tempering process can form finely dispersed NbC and NbN to improve the strength of steel. When the Nb content is excessively high, the size of Nb carbonitrides is relatively large, which reduces the impact energy of steel. Nb, V, and Ti can form carbonitride complexes with C and N, resulting in a decrease in the strength of steel. In the present invention, 0-0.08% Nb is incorporated to ensure the mechanical performance of steel.

[0021] Ni: The addition of a certain amount of Ni in steel can lower the stacking fault energy of BCC phases in body-centered cubic lattices such as tempered bainite and tempered martensite in steel. Steels containing Ni can deform and absorb more energy under impact load, which improves the impact energy of steel. At the same time, Ni is an austenite stabilizing element. However, a relatively high Ni content can promote an increase in the stability of austenite, so that the final structure may contain excess austenite, which reduces the strength of steel. Therefore, in the present invention, 2.30-4.20% Ni is added to ensure the low-temperature impact toughness and strength of steel.

[0022] Cu: The addition of Cu element in steel will result in the precipitation of ε-Cu in the tempering process, which can improve the strength of the steel. However, since the melting point of Cu element is low, an excessive amount of Cu may cause the aggregation of Cu at the grain boundary during the heating process of the steel billet, thereby reducing the toughness. Therefore, in the present invention, the Cu content cannot exceed 0.30%.

[0023] V: The addition of a certain amount of V to steel will result in the formation and precipitation of V carbonitrides in the tempering process, which can improve the strength of the steel. Nb, V, and Ti are all carbonitride-forming elements, and a relatively high V content can cause the precipitation of coarse VC, which reduces the impact performance. Therefore, in the present invention, in combination with other alloying elements, 0.01-0.13% V is incorporated to ensure the mechanical performance of the steel.

[0024] B: B has a small atomic radius, which exists in the form of interstitial atoms, and aggregates at the grain boundaries of steel to inhibit the nucleation of diffusion phase transformation, so that the steel may form low-temperature phase transformation structures such as bainite or martensite. When the steel contains Mn, Cr, Mo and other alloying elements, the diffusion phase transformation may also be inhibited due to the free energy dissipation effect on the diffusion phase transformation interface. When the B content is excessively high, a large amount of B aggregated at the grain boundaries may reduce the binding energy of the grain boundaries and cause a decrease in impact performance. Therefore, in the present invention, the amount of B incorporated is 0-0.0020%.

[0025] Al: Al is incorporated into steel as a deoxidizing element, and meanwhile, Al can refine grains. If the Al content is too high, relatively large alumina inclusions may be formed, which affects the impact toughness and fatigue life of the steel. Therefore, in the present invention, 0.01-0.06% Al is incorporated to improve the toughness of the steel.

[0026] Ti: Ti in steel can form TiN at high temperature to refine the grains of austenite. If the Ti content is too high, coarse and square TiN can be formed, resulting in local stress concentration and reduced impact toughness and fatigue life. Ti can also form TiC with C in steel during the tempering process to improve strength. In comprehensive consideration of the effects of Ti in grain refinement, strength improvement, and toughness degradation, in the present invention, the Ti content is controlled to 0-0.05%.

[0027] Ca: Ca in steel can spheroidize sulfides to avoid the effect of sulfides on impact toughness, but if the Ca content is too high, inclusions may be formed, and the impact toughness and fatigue performance will be deteriorated. Therefore, the Ca content is controlled to be less than 0.004%.

[0028] H: H in steel can segregate at dislocations, sub-boundaries, and grain boundaries to form hydrogen atoms under the action of edge dislocation hydrostatic stress field. Ultra-high strength steels with tensile strengths of over 900 MPa have high dislocation density, and hydrogen tends to aggregate at dislocations, resulting in hydrogen-induced cracking or delayed cracking during the service of the steel. Control of hydrogen content is an important factor to ensure the safe use of ultra-high strength steels. Therefore, in the present invention, the H content is controlled to not exceed 0.0002%.

[0029] N and O: N in steel can form AlN and TiN with Al and Ti to refine austenite grains. However, if the N content is too high, N will aggregate at dislocations, which will deteriorate the impact performance. Therefore, the N content should be controlled not to exceed 0.013%. Oxygen in steel can form oxides with Al and Ti, which will deteriorate the impact performance. Therefore, the O content should not exceed 0.0020%.

[0030] In particular, in the present invention, 8.57*C+1.12*Ni≧4.8% is satisfied by controlling the contents of C and Ni. The content of dissolved carbon in bainite and the ratio of martensite are controlled by controlling the content of C element, and the impact toughness of the steel is controlled by Ni element, so as to achieve ultra-high strength and good low-temperature impact toughness. By controlling the contents of P, S and H, the segregation of P and H at the grain boundary and the reduction of impact energy are avoided. By controlling the contents of Nb, V, Ti and other alloying elements, dispersed fine carbonitride precipitates are formed, and in the tempering process, on the one hand, a uniform microstructure is formed, and on the other hand, the reduction of strength due to tempering can be avoided. By controlling the contents of Mn, Cr, Mo and other elements, the solid solution strengthening effect of Mn is fully utilized to inhibit the diffusion phase transformation, forming a refined bainite and martensite structure. In the present invention, 1.2%≦1.08*Mn+2.13*Cr≦5.6% is required to optimize the effect of the ratio of Mn and Cr elements on hardenability, i.e., to avoid the case where ultra-high strength structure cannot be obtained due to poor hardenability caused by extremely low contents of Mn and Cr elements, and meanwhile to avoid the formation of too hard martensite structure due to high hardenability caused by excessive contents of Mn and Cr elements, which reduces impact energy and elongation. By utilizing Cr and Mo elements to improve the impact toughness of steel, the hardenability of steel is improved and fine carbide precipitates are formed during the tempering process.

[0031] The method for producing a controlled yield ratio steel having excellent low temperature impact toughness according to the present invention comprises the steps of: 1) Refining and casting, wherein refining and casting are performed according to any one of the compositions in claims 1 to 3 to form a cast billet; 2) heating; Here, the casting billet is heated at a heating temperature of 1,010-1,280°C; 3) Rolled or forged, wherein the final rolling temperature is 720°C or higher, or the final forging temperature is 720°C or higher; and after rolling, air cooling, water cooling or delayed cooling is performed; 4) Quenching heat treatment, wherein the quenching is performed using water quenching or oil quenching at a quenching temperature of 830 to 1,060°C, and the ratio of the quenching time to the thickness or diameter of the steel is 0.25 min / mm or more; and 5) Tempering heat treatment, Here, the tempering temperature is 490-660°C, the ratio of the tempering time to the thickness or diameter of the steel is 0.25min / mm or more, and after tempering, air cooling, delayed cooling or water cooling is carried out.

[0032] According to the present invention, the cast billet is heated and austenitized at a temperature of 1,010 to 1,280 ° C; phenomena such as carbonitride dissolution, austenite grain growth, etc. occur in the billet in the heating process; some or all of the carbides of Cr, Mo, Nb, V, and Ti incorporated in the steel are dissolved in austenite, and the undissolved carbonitrides can be fixed at the grain boundaries of austenite and inhibit the growth of austenite grains. The alloying elements such as Cr, Mo, etc. in the steel that have been solidified can inhibit the diffusion phase transformation in the cooling process and form intermediate and low-temperature transformation structures such as bainite, martensite, etc., which can improve the strength of the steel.

[0033] According to the present invention, the steel is rolled and forged at a temperature of 720 ° C or more. The dynamic recrystallization, static recrystallization, dynamic recovery, static recovery, etc. occurring in the steel promote the formation of refined austenite grains and retain a certain number of dislocations and subgrain boundaries in the austenite grains. In the cooling process, not only carbonitrides but also refined bainite and martensite matrix structures are formed.

[0034] The steel according to the present invention is heated to 830-1,060°C after being rolled and forged, and then held. The steel is then quenched. In the quenching heat treatment process, the carbonitrides of Nb, V, and Ti are partially dissolved, while the carbides of Cr and Mo are also partially dissolved simultaneously with the nitrides of Al, and then the undissolved carbonitrides and carbides fix the austenite grain boundaries and inhibit the growth of austenite grains. In the quenching process after cooling, due to the relatively high cooling rate, finer bainite and martensite structures are formed. Such structures have ultra-high strength and good toughness.

[0035] The steel according to the present invention is then subjected to a tempering heat treatment at a temperature of 490-660 ° C, and in the tempering process, annihilation of unfavorable dislocations and precipitation of carbonitrides occur. The annihilation of dislocations results in a decrease in the internal stress and strength of the steel, and on the other hand, the reduction in the number of micro defects such as dislocations, sub-grain boundaries in the crystals can improve the impact toughness of the steel. The precipitation of fine carbonitrides is beneficial to improve the strength and impact toughness. High temperature tempering is beneficial to improve the uniformity of the steel. When the steel is subjected to plastic deformation, the excellent uniformity can improve the elongation rate. In combination with the component system design of the present invention, using the temperature range of the tempering heat treatment, a steel with ultra-high strength, ultra-high toughness and ultra-high plasticity, as well as good aging impact performance can be formed.

[0036] The controlled yield ratio steel with excellent low temperature impact toughness produced according to the composition and process disclosed in this invention can be used in applications such as offshore platform mooring chains, automotive, and machine structures that require rods with high strength and toughness.

[0037] The present invention has the following advantageous effects: In terms of chemical composition, the present invention adopts an optimized C and Ni content design, and combines with Cr, Mo, and micro-alloying elements such as Nb, V, Ti to form a refined intermediate and low-temperature transformation structure by alloying elements that provide improved hardenability, along with an appropriate amount of Ni to reduce the stacking fault energy of ferrite and improve toughness. In addition, refined tempered bainite and tempered martensite are formed by the quenching and tempering process, which can provide excellent structural uniformity, strength and plasticity. In the tempering process, fine dispersed carbonitrides are formed to improve the strength of the steel and ensure toughness.

[0038] The type of steel provided by the present invention can achieve the corresponding high strength toughness and high strength plasticity by only the first quenching process, which omits the quenching process compared with the second quenching process, thereby reducing the cost and carbon emission of production. Therefore, the steel is also environmentally friendly.

[0039] The steel according to the present invention has a rational composition and process design and a wide process window, which is suitable for carrying out mass commercial production of bars or plates. [Brief description of the drawings]

[0040] [Figure 1] FIG. 1 is an optical microscope image (500X) of the microstructural morphology of a steel bar according to Example 3 of the present invention; and [Diagram 2] FIG. 2 is a scanning electron microscope image (10,000X) of the microstructural morphology of a steel bar according to Example 3 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] Detailed Description The present invention will be further described below in combination with examples and the accompanying drawings. These examples are merely used to describe the best mode for carrying out the present invention, and are not intended to limit the scope of the present invention in any way.

[0042] The composition of the embodiment of the present invention is shown in Table 1. The manufacturing method according to the embodiment of the present invention includes the following steps: refining, casting, heating, forging or rolling, quenching and tempering; in the casting process, die casting or continuous casting is adopted; in the heating process, the heating temperature is 1,010-1,280°C, and the final rolling temperature or final forging temperature is 720°C or higher; and in the rolling process, the steel billet can be directly rolled to the final specification, or the steel billet is rolled to a certain intermediate billet size, and then heated and rolled to the final finished product size. The quenching temperature is 830-1,060°C using water quenching or oil quenching, while the ratio of the quenching heating time to the thickness or diameter of the steel is 0.25min / mm or higher. The tempering temperature is 490-660°C, and the steel is air-cooled, delayed-cooled or water-cooled after tempering.

[0043] Test method: 1. The tensile properties are measured according to Chinese standard GB / T228 Metallic materials--Tensile test at ambient temperature; 2. The impact performance is measured according to GB / T229 Metallic Materials--Charpy Pendulum Impact Test Method; and 3. The strain ageing measurement process is derived from DNV classification rules (Marine Mooring Chains and Accessories. Certification of Manufacturers DNVGL-CP-0237 July 2018 edition).

[0044] The product according to the present invention can be used in applications such as offshore platform mooring chains which require bars with high strength, and the size specification of the bars can reach a diameter of 200mm (the diameter of the round bars in Chinese Patent CN103667953A is only 70-160mm).

[0045] Example 1 Electric furnace or converter refining is carried out according to the composition shown in Table 1, and then casting is carried out to form a continuous casting billet or steel ingot. The continuous casting billet or steel ingot is heated to 1,280°C and rolled at a final rolling temperature of 1,020°C, and the size of the intermediate billet is 260*260mm; after rolling, delayed cooling is carried out; the intermediate billet is then heated to 1,010°C and rolled at a final rolling temperature of 720°C to obtain a finished product bar with a specification of φ20mm; after rolling, air cooling is carried out; the product bar is then heated at 830°C for 35 minutes for quenching, and water quenching treatment is adopted; then tempering is carried out at 490°C for 35 minutes, and air cooling is carried out after tempering.

[0046] Example 2 The implementation process is the same as that of Example 1, except that the heating temperature is 1,220°C; the final rolling temperature is 980°C; the size of the intermediate billet is 260*260mm; and delayed cooling is performed after rolling; the intermediate billet is heated to 1,050°C; the final rolling temperature is 770°C; the specification of the finished product bar is φ60mm, and water cooling is performed after rolling; the finished product bar is heated at 880°C for 70 minutes for quenching, and oil quenching treatment is adopted; then tempering is performed at 540°C for 80 minutes, and delayed cooling is performed after tempering.

[0047] Example 3 The implementation process is the same as that of Example 1, except that the heating temperature is 1,180°C; the final rolling temperature is 940°C; the specification of the finished product bar is φ70 mm, and air cooling is performed after rolling; the finished product bar is heated at 940°C for 90 minutes for quenching, and an oil quenching process is adopted; then tempering is performed at 560°C for 100 minutes, and water cooling is performed after tempering.

[0048] Example 4 The implementation process is the same as that of Example 1, except that the heating temperature is 1,110°C; the final rolling temperature is 920°C, the specification of the finished product bar is φ110mm, and air cooling is performed after rolling; the finished product bar is heated at 960°C for 120 minutes for quenching, and a water quenching process is adopted; and then tempering is performed at 600°C for 180 minutes, and air cooling is performed after tempering.

[0049] Example 5 The implementation process is the same as that of Example 1, except that the heating temperature is 1,080°C; the final rolling temperature is 900°C; the specification of the finished product bar is φ130 mm, and delayed cooling is performed after rolling; the finished product bar is heated at 980°C for 170 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 610°C for 260 minutes, and water cooling is performed after tempering.

[0050] Example 6 The implementation process is the same as that of Example 1, except that the heating temperature is 1,010°C; the final rolling temperature is 870°C; the specification of the finished product bar is φ200mm, and delayed cooling is performed after rolling; the finished product bar is heated at 1,060°C for 350 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 660°C for 350 minutes, and water cooling is performed after tempering.

[0051] Example 7 The implementation process is the same as that of Example 1, except that the heating temperature is 1,230°C; the final rolling temperature is 960°C; the specification of the finished product bar is φ90mm, and air cooling is performed after rolling; the finished product bar is heated at 920°C for 30 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 620°C for 60 minutes, and water cooling is performed after tempering.

[0052] Example 8 The implementation process is the same as that of Example 1, except that the heating temperature is 1,200°C; the final rolling temperature is 980°C, the specification of the finished product bar is φ100mm, and air cooling is performed after rolling; the finished product bar is heated at 920°C for 30 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 600°C for 60 minutes, and water cooling is performed after tempering.

[0053] Comparative Example 1 The implementation process is the same as that of Example 1, except that the heating temperature is 1,150°C; the final rolling temperature is 960°C; the specification of the finished product bar is φ110mm, and air cooling is performed after rolling; the finished product bar is heated at 920°C for 35 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 550°C for 60 minutes, and water cooling is performed after tempering.

[0054] Comparative Example 2 The implementation process is the same as that of Example 1, except that the heating temperature is 1,120°C; the final rolling temperature is 940°C; the specification of the finished product bar is φ130mm, and air cooling is performed after rolling; the finished product bar is heated at 910°C for 40 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 530°C for 70 minutes, and water cooling is performed after tempering.

[0055] Comparative Example 3 The implementation process is the same as that of Example 1, except that the heating temperature is 1,100°C; the final rolling temperature is 900°C; the specification of the finished product bar is φ100mm, and air cooling is performed after rolling; the finished product bar is heated at 870°C for 50 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 520°C for 50 minutes, and water cooling is performed after tempering.

[0056] Comparative Example 4 The implementation process is the same as that of Example 1, except that the heating temperature is 1,040°C; the final rolling temperature is 880°C; the specification of the finished product bar is φ80 mm, and air cooling is performed after rolling; the finished product bar is heated at 930°C for 30 minutes for quenching, and water quenching treatment is adopted; then tempering is performed at 600°C for 40 minutes, and water cooling is performed after tempering.

[0057] The mechanical properties of the steels with controlled yield ratios in Examples 1 to 8 of the present invention and the steels in Comparative Examples 1 to 4 were measured according to the above test methods. The results are shown in Table 2.

[0058] From Tables 1 and 2, it can be seen that C and B in Comparative Example 1 do not satisfy the composition range of the present invention, therefore the refinement effect of C on bainite and ferrite layer structure cannot be fully utilized; and the relatively high B content may cause the segregation of B at the grain boundary, which deteriorates the low-temperature impact performance and results in low strength and low impact energy of the steel. In Comparative Example 2, the steel does not satisfy 8.57*C+1.12*Ni≧4.8%; but the tensile strength of the steel reaches 1,100 MPa, the effect of Ni in lowering stacking fault energy cannot be fully utilized, and the refinement effect of C on bainite layer structure cannot be effectively provided, so the low-temperature impact energy of the steel is rather low. In Comparative Example 3, the contents of Mn and Mo exceed the composition range of the present invention; however, the solid solution strengthening effect of Mn improves the strength of the steel, and produces a tensile strength of more than 1,200 MPa, and Mn segregates toward the grain boundary in the welding process, and the relatively large carbides of Mo tend to reduce the low-temperature toughness of the steel, so the impact energy of the steel of Comparative Example 3 is low. In Comparative Example 4, the steel does not satisfy 1.2%≦1.08Mn+2.13Cr≦5.6%, and the Nb content exceeds the desired composition range of the present invention, so the solid solution strengthening effect of Mn and Cr and the carbide precipitation strengthening effect of Cr cannot be fully utilized, resulting in the formation of coarse NbC precipitation particles, and therefore the steel of Comparative Example 4 only has a yield strength of 890 MPa, a tensile strength not reaching 1,100 MPa, a yield ratio of 0.84, and a low impact energy.

[0059] The steel with a controlled yield ratio provided by the present invention has a Charpy impact energy A of 90 J or more at -20°C. kv , Charpy impact energy A at -40℃ of 70J or more kv Charpy impact energy A at -20℃ of 80J or more after 1h at 100℃ after 5% strain kv Charpy impact energy A at -40°C of 60J or more after 1h at 100°C with 5% strain kv , Yield ratio of 0.85 to 0.95, tensile strength of 1,100 MPa or more, yield strength of 900 MPa or more, elongation of 15% or more, area reduction of 50% or more, strength toughness product (tensile strength*Charpy impact energy at -20°C A kv ), and has a strength plastic product (tensile strength * elongation) of 16GPa*% or more.

[0060] 1 and 2, it can be seen from Fig. 1 and 2 that the microstructure of the steel bar in Example 3 of the present invention is tempered martensite and tempered bainite. The width of the tempered bainite or tempered martensite lath is 0.3-2 μm. Nanoscale carbide precipitates can be seen in the interior of the lath, and fine lamellar shaped cementite precipitates along the interface of the lath with a thickness of 50 nm and a length of about 0.2-2 μm.

[0061] [Table 1]

[0062] [Table 2]

Claims

1. A steel having a controlled yield ratio, comprising the following components in mass percent: C: 0.245-0.365%, Si: 0.10-0.80%, Mn: 0.20-2.00%, P: ≦0.015%, S: ≦0.003%, Cr: 0.20-2.50%, Mo: 0.10-0.90%, Nb: 0-0.08%, Ni: 2.30-4.20%, Cu: 0-0.30%, V: 0.01-0.13%. %, B: more than 0 and 0.0020% or less, Al: 0.01-0.06%, Ti: 0-0.05%, Ca: ≦0.004%, H: ≦0.0002%, N: ≦0.013%, O: ≦0.0020%, and the balance being Fe and unavoidable impurities, wherein the components satisfy (8.57*C+1.12*Ni)≧4.8% and 1.2%≦(1.08*Mn+2.13*Cr)≦5.6%; The controlled yield ratio steel has a yield ratio of 0.85 to 0.95, a tensile strength of 1,100 MPa or more, and a yield strength of 900 MPa or more; and The microstructure of the controlled yield ratio steel is tempered martensite + tempered bainite.

2. The steel with a controlled yield ratio has a Charpy impact energy A of 90 J or more at -20°C. kv Charpy impact energy A at -40°C of 70J or more kv Charpy impact energy A at -20°C of 80J or more after 1h at 100°C after 5% strain kv Charpy impact energy A at -40°C of 60J or more after 1h at 100°C after 5% strain kv , a yield ratio of 0.85 to 0.95, a tensile strength of 1,100 MPa or more, a yield strength of 900 MPa or more, an elongation rate of 15% or more, an area reduction rate of 50% or more, a strength-toughness product (tensile strength*Charpy impact energy at -20°C A kv 2. The controlled yield ratio steel of claim 1, having a strength plastic product (tensile strength * elongation) of 16 GPa*% or more.

3. A method for producing a controlled yield ratio steel, comprising the steps of: 1) Refining and casting, wherein refining and casting are carried out according to the composition in claim 1 or 2 to form a cast billet; 2) heating; Here, the casting billet is heated at a heating temperature of 1,010 to 1,280°C; 3) rolling or forging; wherein the final rolling temperature is 720°C or higher, or the final forging temperature is 720°C or higher; and after rolling or forging, air cooling or water cooling is performed; 4) Quenching heat treatment, wherein the quenching is carried out using water quenching or oil quenching at a quenching temperature of 830-1,060°C, and the ratio of the quenching time to the thickness or diameter of the steel is 0.25 min / mm or more; and 5) Tempering heat treatment, Wherein the tempering temperature is 490-660°C, the ratio of tempering time to the thickness or diameter of the steel is 0.25min / mm or more, and after tempering, air cooling or water cooling is performed; Here, the microstructure of the yield ratio controlled steel is tempered martensite + tempered bainite.

4. The steel with a controlled yield ratio has a Charpy impact energy A of 90 J or more at -20°C. kv Charpy impact energy A at -40°C of 70J or more kv Charpy impact energy A at -20°C of 80J or more after 1h at 100°C after 5% strain kv Charpy impact energy A at -40°C of 60J or more after 1h at 100°C after 5% strain kv , a yield ratio of 0.85 to 0.95, a tensile strength of 1,100 MPa or more, a yield strength of 900 MPa or more, an elongation rate of 15% or more, an area reduction rate of 50% or more, a strength-toughness product (tensile strength*Charpy impact energy at -20°C A kv 4. The method of claim 3, wherein the steel has a strength plastic product (tensile strength * elongation) of 16 GPa*% or more.

Citation Information

Patent Citations

  • Ultrahigh tough steel with tensile strength of 1100 Mpa and manufacturing method thereof

    CN109136737A

  • R6-grade marine mooring chain steel with high strength and ductility suitable for anchor moored positioning cathode protection floating body, and mooring chain thereof

    CN110144516A

  • Tough nitriding steel

    JP1983171558A

  • Production of pressure vessel used in seawater

    JP1991229826A

  • Steel for pressure vessel

    JP1991232946A