Semiconductor Device

By employing highly purified oxide semiconductors with large energy gaps in DC conversion circuits, the reliability issues associated with dielectric breakdown are mitigated, ensuring stable operation under high voltages.

JP7576667B2Active Publication Date: 2024-10-31SEMICON ENERGY LAB CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023132772
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2009-12-04
Filing Date
2023-08-17
Publication Date
2024-10-31
Estimated Expiration
2030-11-29

AI Technical Summary

Technical Problem

Conventional DC conversion circuits face reliability issues due to dielectric breakdown when high voltages are applied to transistors, particularly thin film transistors, leading to low reliability.

Method used

The use of an intrinsic or substantially intrinsic semiconductor with a large energy gap, such as an oxide semiconductor, in the channel forming layer of transistors, combined with high purification to minimize hydrogen concentration and oxygen deficiency, thereby reducing defects and enhancing reliability.

Benefits of technology

The implementation of highly purified oxide semiconductors with reduced hydrogen content improves the reliability of DC conversion circuits by minimizing dielectric breakdown and maintaining stable electrical characteristics even under high voltages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576667000001
    Figure 0007576667000001
  • Figure 0007576667000002
    Figure 0007576667000002
  • Figure 0007576667000003
    Figure 0007576667000003
Patent Text Reader

Abstract

To provide a DC conversion circuit having high reliability.SOLUTION: A semiconductor device includes an induction element that generates an electromotive force according to a change in a flowing current, a transistor that has a gate, a source, and a drain and that controls generation of an electromotive force in the induction element by turning on or off, a rectifying element which is in conduction state when the transistor is off, and a control circuit that controls the on state or the off state of the transistor, and the transistor has an oxide semiconductor layer having a hydrogen concentration of 5×1019 atoms / cm3 or less as a channel formation layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] 1. Field of the Invention An embodiment of the present invention relates to a DC converter circuit and a power supply circuit. [Background technology]

[0002] In recent years, in various electronic devices, for example, the power supply voltage has been changed from a voltage with large voltage fluctuations to a stable value. When generating a DC current of a certain value, or when multiple different power supply voltages are required, A circuit that converts a voltage into a different value of DC voltage (also called a DC conversion circuit or DC-DC converter). u) is used.

[0003] The DC conversion circuit is configured using, for example, a coil, a diode, and a transistor. There is a non-insulated DC converter circuit (see, for example, Patent Document 1). The switching circuit has the advantages of a small circuit area and low manufacturing costs. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 58-086868 Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional DC converter circuits have a problem of low reliability. For example, in a DC converter circuit, a relatively high voltage is handled, so When a high voltage above a certain value is applied to a transistor (such as a thin film transistor) This may cause dielectric breakdown of the transistor.

[0006] An object of one embodiment of the present invention is to improve the reliability of a DC converter circuit. [Means for solving the problem]

[0007] One embodiment of the present invention is to obtain a high purity product by removing impurities that act as electron donors as much as possible. It is an intrinsic or substantially intrinsic semiconductor that has been oxidized and has a higher energy gap than silicon semiconductors. A DC converter using a transistor having an oxide semiconductor with a large jump in the channel formation layer This improves the reliability of the DC conversion circuit. The energy gap of the oxide semiconductor used in one embodiment is, for example, 2 eV or more. is set to 2.5 eV or more, more preferably 3 eV or more.

[0008] Note that the term "high purification" refers to removing hydrogen from the oxide semiconductor layer as much as possible and By supplying oxygen to the oxide semiconductor layer, defects due to oxygen deficiency in the oxide semiconductor layer can be reduced. Both are concepts that include the other.

[0009] The hydrogen concentration in the oxide semiconductor is 5×10 19 / cm 3 Less than or equal to 5x 10 18 / cm 3 Less than or equal to 5×10 17 / cm 3 or less, or 1×10 16 / cm 3 In addition, hydrogen or OH groups contained in the oxide semiconductor are removed. The carrier concentration is 1×10 12 / cm 3 Less than 1 x 10 11 / cm 3 less than It is.

[0010] The oxide semiconductor layer is a quaternary metal oxide film of In-Sn-Ga-Zn-O or a ternary metal oxide film of In-Sn-Ga-Zn-O. Metal oxide films such as In-Ga-Zn-O, In-Sn-Zn-O, and In-Al-Zn- O film, Sn-Ga-Zn-O film, Al-Ga-Zn-O film, Sn-Al-Zn-O film, Binary metal oxide films such as In-Zn-O, Sn-Zn-O, Al-Zn-O, and Zn -Mg-O film, Sn-Mg-O film, In-Mg-O film, In-Sn-O film, In-O film The insulating film can be formed using an oxide semiconductor film such as a Sn—O film or a Zn—O film. The oxide semiconductor film may contain SiO2. The n-Ga-Zn-O film is made of indium (In), tin (Sn), gallium (Ga), and zinc The term "oxide film containing Zn" refers to an oxide film containing Zn, and the stoichiometric ratio is not particularly important.

[0011] The oxide semiconductor layer is InMO3(ZnO) m The membrane is formed using the formula (m>0). Here, M is one or more selected from Ga, Al, Mn, and Co. For example, M can be Ga, Ga and Al, Ga and Mn, or Ga and Co. InMO3(ZnO) m Oxide semiconductors with structures represented by (m>0) The oxide semiconductor containing Ga as M in the above-mentioned In-Ga-Zn-O This is called an oxide semiconductor, and the film is also called an In-Ga-Zn-O film.

[0012] In this way, by using a highly purified oxide semiconductor for a channel formation region of a transistor, For example, when the drain voltage is in the range of 1V to 10V, When the voltage between the gate and source is within the range of 0 V or less, the off-state current ( The current that flows between the source and drain when -13 A or less, or off current density The off-state current (the value obtained by dividing the off-state current by the channel width of the transistor) is 100aA (a (atom) is 1 0 -18 ) / μm or less, preferably 10 aA / μm or less, and more preferably 1 aA / μm or less.

[0013] A highly purified oxide semiconductor layer in which the hydrogen concentration is sufficiently reduced is used as the channel formation layer. By using such transistors, it is possible to realize a highly reliable DC conversion circuit. do.

[0014] One aspect of the present invention is a semiconductor device that includes an inductive element that generates an electromotive force in response to a change in the flowing current, a gate, a switch, and a The inductive element has a source and a drain, and is turned on or off to A transistor that controls the generation of electromotive force and a transistor that is conductive when the transistor is off. and a control circuit that controls an on / off state of the transistor, The transistor is formed with a hydrogen concentration of 5×10 19 atoms / cm 3 The following is a DC converter circuit including an oxide semiconductor layer.

[0015] In one embodiment of the present invention, the control circuit is a control circuit having an input signal of the voltage at the second terminal of the inductive element. A signal is input, the input signal is compared with a reference voltage, and a pulse is generated according to the comparison result. A hysteresis loop that outputs a pulse signal with a set width to the gate of a transistor as an output signal. The configuration may include a comparator.

[0016] In one embodiment of the present invention, the hysteresis comparator is configured using a logic circuit. The logic circuit is a channel-forming layer with a hydrogen concentration of 5×10 19 atoms / cm 3 is less than or equal to The semiconductor device may be formed using a transistor including an oxide semiconductor layer.

[0017] One aspect of the present invention is a method for manufacturing a semiconductor device comprising the steps of: It has an inductive element that generates an electromotive force in response to changes in current, a gate, a source, and a drain. A transistor that controls the generation of electromotive force in an inductive element by being in an on or off state. A transistor is a rectifier that is conductive when the transistor is off. and a control circuit for controlling the on or off state of the capacitor. The control circuit receives an input signal A signal, which is the voltage at the second terminal of the inductive element, is input, and the input signal and the reference voltage are The output signal is a pulse signal with a pulse width set according to the comparison result. The DC converter has a hysteresis comparator that outputs to the gate of the inverter.

[0018] In one embodiment of the present invention, the transistor has a channel formation layer having a hydrogen concentration of 5×10 1 9 atoms / cm 3 It may be the following.

[0019] One aspect of the present invention is a coil having a first terminal and a second terminal, and a voltage at the second terminal is an output voltage. A gate, a source, and a drain, and either the source or the drain is a coil. a transistor electrically connected to the first terminal of the transistor, and an input voltage is applied to the other of the source and drain of the transistor. A transistor has a first electrode and a second electrode, the first electrode being electrically connected to the second terminal of the coil. a capacitance element having an anode and a cathode, the anode of which is electrically connected to the cathode of the first electrode of the capacitor, and a low power supply voltage is applied to the second electrode of the capacitor; A low power supply voltage is applied to the anode, and the cathode is connected to the source and drain of the transistor. A diode electrically connected to one of the inputs and the second terminal of the coil as the input signal. The voltage at the second terminal of the coil is input, and a pulse signal with a duty ratio set according to the voltage at the second terminal of the coil is generated. a hysteresis comparator for outputting the signal to a gate of a transistor; The transistor is equipped with a channel formation layer having a hydrogen concentration of 5×10 19 atoms / cm 3 The following is a DC converter circuit including an oxide semiconductor layer.

[0020] In one embodiment of the present invention, a hysteresis comparator includes a first input terminal, a second input terminal, a first reference voltage is applied to the first input terminal and a second reference voltage is applied to the second input terminal a first comparator to which the voltage of the second terminal of the coil is input as an input signal; a first input terminal, a second input terminal, and an output terminal; and a coil A second capacitor is connected to the second terminal of the first capacitor and a second reference voltage is applied to the second input terminal of the second capacitor. a first comparator having an input terminal and an output terminal, the input terminal being connected to the output terminal of the first comparator; a first inverter electrically connected to the second inverter, the first inverter having an input terminal and an output terminal, the input terminal being connected to the second inverter; a second inverter electrically connected to the output terminal of the comparator; and a first input terminal; A first inverter has a second input terminal and an output terminal, the first input terminal being connected to the output terminal of the first inverter. a first NOR transistor electrically connected to the gate of the transistor; A gate, a first input terminal, a second input terminal, and an output terminal, the first input terminal being a the second input terminal of the second inverter is electrically connected to the output terminal of the first NOR gate; an output terminal electrically connected to the second input terminal of the first NOR gate; and a second NOR gate connected to the first NOR gate.

[0021] In one embodiment of the present invention, a first comparator, a second comparator, a first inverter , the second inverter, the first NOR gate, and the second NOR gate are transistors The transistor includes a gate, a source, a drain, and a channel forming layer. Hydrogen concentration is 5×10 19 atoms / cm 3 The present invention has a structure including an oxide semiconductor layer having the following structure. It is also possible.

[0022] In one embodiment of the present invention, the capacitance element is an electric double layer capacitor, a redox capacitor, Alternatively, it may be a lithium ion capacitor.

[0023] One embodiment of the present invention is a DC converter circuit as described above, and a storage device electrically connected to the DC converter circuit. and a power supply circuit having a power supply device.

[0024] In one embodiment of the present invention, the power storage device includes a photoelectric conversion device, a lithium ion secondary battery, and a The present invention may be any one or more of the lithium ion capacitors. Effect of the Invention

[0025] According to one embodiment of the present invention, the reliability of a DC converter circuit can be improved. [Brief description of the drawings]

[0026] [Figure 1] FIG. 2 is a circuit diagram showing an example of a circuit configuration of a DC conversion circuit. [Diagram 2] FIG. 2 is a circuit diagram showing an example of a circuit configuration of a DC conversion circuit. [Diagram 3] FIG. 2 is a circuit diagram showing an example of a circuit configuration of a DC conversion circuit. [Figure 4] FIG. 1 is a circuit diagram showing an example of a circuit configuration of a hysteresis comparator. [Diagram 5] 6 is a timing chart for explaining an example of the operation of a hysteresis comparator. [Figure 6] 1A to 1C are diagrams illustrating transistors. [Figure 7] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 8] 1A to 1C are diagrams illustrating transistors. [Figure 9] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 10] 1A to 1C are diagrams illustrating transistors. [Figure 11] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 12] FIG. 1 is a longitudinal cross-sectional view of an inverted staggered transistor including an oxide semiconductor. [Figure 13] FIG. 13 is an energy band diagram (schematic diagram) taken along the line A-A' of FIG. [Figure 14] 1A shows a state in which a positive potential (+Vg) is applied to the gate electrode 1001. FIG. 1B shows a state in which a negative potential (-Vg) is applied to the gate electrode 1001. [Figure 15] A diagram showing the relationship between the vacuum level, the work function of a metal (φM), and the electron affinity of an oxide semiconductor (χ). [Figure 16] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 17] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 18] 1A to 1C illustrate a method for manufacturing a transistor. [Figure 19] 1A to 1C are diagrams illustrating transistors. [Figure 20] FIG. 2 is a diagram illustrating a power supply circuit. [Figure 21]1A to 1C are diagrams illustrating electronic devices. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] An embodiment of the present invention will be described below with reference to the drawings. The present invention is not limited to the above description, and the embodiments and details thereof are not limited to those described above without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that the above may be modified in various ways. The present invention should not be construed as being limited to the description of the embodiments.

[0028] (Embodiment 1) In this embodiment, an example of a DC converter circuit according to one embodiment of the present invention will be described.

[0029] An example of the configuration of a DC converter circuit according to this embodiment will be described with reference to FIG. 1 is a circuit diagram showing an example of a configuration of a DC conversion circuit according to an embodiment of the present invention.

[0030] The DC converter circuit shown in FIG. 1 includes an inductive element 101, a transistor 102, and a rectifying element (RC T) 103.

[0031] In this specification, a transistor is defined as a transistor having at least a gate, a source, and a drain. As the transistor, for example, a gate insulating type transistor can be used. do.

[0032] The term "gate" refers to a gate electrode and a part or the whole of a gate wiring. The term "gate electrode of at least one transistor is electrically connected to another electrode or another wiring" means that The term "gate electrode" refers to the wiring that connects the gate electrodes to each other. The conductive layer may have a function as a gate electrode and a gate wiring.

[0033] The source refers to the source electrode and a part or the whole of the source wiring. The source wiring is a conductive layer that functions as a source. A wiring that electrically connects the source electrode of a transistor to another electrode or wiring. In addition, the source electrode and the source wiring are not distinguished from each other, and one conductive layer is used for both the source electrode and the source wiring. It is also possible to configure the wiring to function as a bus line.

[0034] The drain refers to the drain electrode and a part or the whole of the drain wiring. The electrode refers to a conductive layer that functions as a drain. To electrically connect the drain electrode of one transistor to another electrode or another wiring In addition, the drain electrode and the drain wiring are not distinguished from each other, and one conductive layer is used. It may also be configured to function as a drain electrode and a drain wiring.

[0035] In this specification, the source and drain of a transistor are used to determine the structure and operation of the transistor. Since they are interchangeable depending on the operating conditions, it is difficult to determine which is the source or drain. Therefore, in this document (specification, claims, drawings, etc.), Either the source or the drain is referred to as the source or drain, and the other is referred to as the source. and the other of the drain.

[0036] The inductive element 101 generates an electromotive force in response to changes in the current flowing through it due to electromagnetic induction. As shown in FIG. 1, the inductive element 101 has a first terminal and a second terminal. The inductive element 101 may be, for example, a coil.

[0037] The transistor 102 is turned on or off to control the inductive element 101. The transistor 102 has a function of controlling the generation of electromotive force. For example, as shown in FIG. One of the source and the drain is connected to either the first terminal or the second terminal of the inductive element 101. are electrically connected.

[0038] Generally speaking, voltage refers to the difference in electric potential between two points (also called the potential difference). However, voltage and potential values ​​are often expressed in volts (V) in circuit diagrams and other places. Therefore, in this specification, unless otherwise specified, The potential difference between the potential at the point and the reference potential (also called the reference potential) is used as the voltage at that point. There are cases.

[0039] In this specification, the signal may be an analog signal using, for example, a voltage or a digital signal. For example, a signal using a voltage (also called a voltage signal) can be It is preferred to use a signal having at least a first voltage state and a second voltage state, e.g. For example, a high-level voltage state may be used as the first voltage state and a low-level voltage state may be used as the second voltage state. A digital signal having a voltage state can be used. Voltage V H Or simply V H Also called a low level, the voltage at the low level is V L Or simply V L and The voltages of the first voltage state and the second voltage state are also referred to as "voltages of the first voltage state and the second voltage state." The voltage in the first voltage state may vary depending on the signal and may be affected by noise, etc. The voltage in the first voltage state and the voltage in the second voltage state do not have to be constant, but may be within a certain range. stomach.

[0040] For example, as shown in FIG. 1, the rectifying element 103 has a first terminal and a second terminal. Either the first terminal or the second terminal of the inductive element 101 is connected to either the first terminal or the second terminal of the inductive element 101. are electrically connected.

[0041] The rectifying element 103 may be, for example, a diode. For example, a PN diode or a PIN diode can be used. The transistor 102 may be used as the transistor having a gate and a drain. The use of transistors with their inputs electrically connected (also called diode-connected) As a diode-connected transistor, the function of the channel formation layer is and a hydrogen concentration in a channel formation layer is 5×10 19 atoms / c m 3 Less than or equal to 5×10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / cm 3 The carrier concentration is 1×10 12 / cm 3 Less than, preferred 1×10 11 / cm 3 A transistor having a capacitance of less than 100 .mu.m can be used.

[0042] Furthermore, the DC converter circuit shown in Figure 1 is capable of determining which terminal is given the input voltage and which terminal is given the voltage. For example, the first and second terminals of the inductive element 101 are An input voltage is applied to the other of the first and second terminals of the rectifier element 103, and a voltage is output from the other of the first and second terminals of the rectifier element 103. When a current flows from the first terminal to the second terminal of the rectifying element 103, the direct current shown in FIG. The current converter circuit functions as a boost circuit. An input voltage is applied to the other of the first and second terminals of the inductive element 101. When a current flows from the first terminal to the second terminal of the rectifier element 103 as shown in FIG. The DC converter circuit functions as a step-down circuit.

[0043] Furthermore, in the DC converter circuit of this embodiment, the on and off states of the transistor 102 are The DC converter circuit of this embodiment may have a control circuit for controlling the DC converter. An example of the configuration will be described with reference to FIG. 2. In the DC conversion circuit shown in FIG. For parts having the same configuration as the DC converter circuit shown in FIG. To quote.

[0044] The DC conversion circuit shown in FIG. 2 includes a control circuit 104 in addition to the components shown in FIG.

[0045] The control circuit 104 has a function of controlling the on / off state of the transistor 102. The control circuit 104 receives the output voltage of the DC converter as an input signal, and controls the DC converter The ripple of the output voltage of the The pulse signal is output to the gate of the transistor 102. The off state is controlled.

[0046] The control circuit 104 is configured using, for example, a hysteresis comparator. The comparator is configured using, for example, a plurality of logic circuits, each of which has For example, the transistor is configured using a channel forming layer. and the hydrogen concentration in the oxide semiconductor layer is 5×10 19 atoms / cm 3 Less than or equal to 5×10 18 atoms / cm 3 The following are more preferred Or 5×10 17 atoms / cm 3 The carrier concentration is 1×10 12 / cm 3 Less than 1 x 10 11 / cm 3 It is also possible to use transistors with This reduces voltage fluctuations caused by transistor leakage current in each logic circuit. Therefore, the voltage state of the pulse signal can be stabilized. The control circuit 104 is formed by combining a hysteresis comparator with another arithmetic circuit. It is preferable.

[0047] As shown in FIG. 1 and FIG. 2, an example of a DC converter circuit according to the present embodiment includes a transistor and an inductor. The configuration includes a conductive element and a rectifying element.

[0048] The DC converter circuit of this embodiment has a capacitance element for smoothing the output voltage. By providing a capacitance element, the output voltage can be made close to a constant value. Cut.

[0049] Further, in the DC converter circuit of the present embodiment, a channel forming layer and and the hydrogen concentration in the oxide semiconductor layer is 5×1019 a toms / cm 3 Less than or equal to 5×10 18 atoms / cm 3 The following is more preferable: 5×10 17 atoms / cm 3 The carrier concentration is 1×10 12 / cm 3 Less than 1 x 10 11 / cm 3 The transistors used should be less than 1000 .mu.m. The transistor has the following advantages over conventional silicon transistors: It has a low off-state current and a high dielectric strength. Therefore, it is used as a transistor that configures a DC conversion circuit. This allows the transistor to operate without damage even when a high voltage is applied between its terminals. This can suppress damage to the capacitor.

[0050] Next, as an example of the operation of the DC converter circuit of this embodiment, the operation of the DC converter circuit shown in FIG. An example of the above will be described.

[0051] As a DC conversion method of the DC conversion circuit of this embodiment, for example, a nonlinear control method is used. The nonlinear control scheme alternates the state of the transistor 102 between an on state and an off state. By switching between these two, the voltage input to the DC converter circuit is converted into a pulse signal, and In this method, the output voltage is generated using a pulse signal. The state is set by, for example, the duty ratio of a pulse signal input to the gate. The pulse signal input to the transistor 102 is, for example, an output voltage of a DC converter circuit. is generated.

[0052] An example of the operation of the DC converter circuit shown in FIG. 2 can be mainly divided into a period T1 and a period T2. , the input is made by alternately performing the operation in the period T1 and the operation in the period T2. The voltage is increased or decreased. Each period is explained below.

[0053] During the period T1, the transistor 102 is turned on in response to the pulse signal, and the rectifying element 10 In addition, the inductive element 3 is turned off depending on the value of the input voltage input to the DC converter circuit. A current flows through inductive element 101. At this time, electromotive force V1 is generated in inductive element 101.

[0054] In the period T2, the transistor 102 is turned off in response to the pulse signal. In the conductive element 101, in order to suppress the change in its own magnetic field, an electromotive force in the opposite direction to the electromotive force V1 is generated. V2 is generated, the rectifier element 103 becomes conductive, and the inductive element 101 and the rectifier element 103 When current flows through the converter, the output voltage changes. The voltage value is the value at which the input voltage has changed. The output voltage value is the value at which the input voltage has changed between the period T1 and the period T2. T2, in other words, the duty ratio of the pulse signal. In periods T1 and T2, when the output voltage is greater than the desired value, the duty cycle of the pulse signal is The ratio is set to be low by the control circuit 104. Also, if the output voltage is lower than the desired value, If the duty ratio of the pulse signal is smaller than the threshold voltage, the duty ratio of the pulse signal is set to be higher by the control circuit 104. In this way, in the DC converter circuit shown in FIG. 2, the output voltage per unit period is set by the control circuit. By feeding back to 104, the output voltage after feedback is made to approach the desired value. It can be done.

[0055] As described above, the DC converter circuit of the present embodiment is an example of a DC converter circuit that converts a pulse signal input from a control circuit into a A transistor electrically connected to the inductive element 101 is turned on in accordance with the duty ratio of the signal. and off states to convert the input voltage to a different value to generate an output voltage. This allows the circuit to function as a voltage step-up circuit or a voltage step-down circuit.

[0056] (Embodiment 2) In this embodiment, an example of a DC converter circuit according to one embodiment of the present invention will be described. The most typical conversion methods for the conversion circuit are the linear method and the switching method. The DC conversion circuit of this type has excellent conversion efficiency and is therefore suitable for reducing the power consumption of electronic devices. In the embodiment, a switching type, particularly a chopper type, DC conversion circuit will be described. .

[0057] An example of the configuration of the DC converter circuit in this embodiment will be described with reference to FIG. 3. 1 is a circuit diagram showing an example of a configuration of a DC conversion circuit according to an embodiment of the present invention.

[0058] The DC conversion circuit shown in FIG. 3 includes a coil 201, a transistor 202, and a diode 203. a capacitance element 204, and a hysteresis comparator (also called HCMP) 205. Prepare.

[0059] The coil 201 has a first terminal and a second terminal. The coil 201 functions as an inductive element. has.

[0060] The transistor 202 has one of a source and a drain electrically connected to the first terminal of the coil 201. Connected.

[0061] The transistor 202 is, for example, a semiconductor having a function as a channel formation layer. The hydrogen concentration in the channel forming layer is 5×10 19 atoms / cm 3 Hereinafter, preferably 5×10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / cm 3 The carrier concentration is 1×10 12 / cm 3 Less than 1 x 10 11 / c m 3 A transistor having a capacitance of less than 100 .mu.m can be used.

[0062] The diode 203 has an anode and a cathode, and the anode is connected to a low power supply voltage (voltage VSS or simply VSS) is applied, and the cathode is electrically connected to the first terminal of the coil 201. The diode 203 functions as a rectifying element.

[0063] As the diode 203, for example, a PN diode or a PIN diode can be used. In addition, a transistor applicable to the transistor 202, for example, a diode The connected transistor can also be used as a diode 203. As an example of such a transistor, an oxide semiconductor having a function as a channel formation layer is used. The hydrogen concentration in the oxide semiconductor layer is 5×10 19 atoms / cm 3 The following is preferably is 5 x 10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / c m 3 The carrier concentration is 1×10 12 / cm 3Less than 1 x 10 11 / cm 3 A transistor having a capacitance of less than 100 .mu.m can be used.

[0064] The capacitor 204 is provided between a first electrode, a second electrode, and the first electrode and the second electrode. a dielectric layer formed on the first electrode of the coil 201; and a first electrode electrically connected to the second terminal of the coil 201. A low power supply voltage is applied to the second electrode. The capacitor 204 has a function as a smoothing capacitor. , has the function of smoothing the voltage of node N2 shown in FIG.

[0065] The capacitor 204 is formed using, for example, the oxide semiconductor layer used in the transistor 202. MIS capacitor, electric double layer capacitor, redox capacitor, or lithium ion capacitor In the DC converter circuit according to one embodiment of the present invention, By alternately switching the transistor 202 on and off, a boost operation or The charge / discharge rate of the capacitance element 204 to which the boosted or stepped-down voltage is applied in order to perform the step-down operation If the voltage is low, the voltage step-up or step-down operation may be delayed. By using a lithium ion capacitor, which is said to be fast, the delay of the voltage step-up or step-down operation is In addition, the present invention is not limited to the lithium ion capacitor, and the capacitance element 2 04, other alkali metal ions or alkaline earth metal ions are used as mobile ions. For example, a sodium ion capacitor may be used. This allows the manufacturing cost to be reduced. It is preferable that the capacitance of the capacitance element 204 is large. By increasing the capacitance of the capacitance element 204, Therefore, the output voltage of the DC converter circuit can be smoothed.

[0066] The hysteresis comparator 205 receives as an input signal the output voltage of the DC converter circuit shown in FIG. The voltage is input, the ripple of the input signal is detected, and the duty ratio is adjusted according to the detected ripple. A preset pulse signal is generated, and the generated pulse signal is used as a control signal to drive the transistor 20. It has the function of outputting to gate 2.

[0067] The hysteresis comparator 205 is configured using a logic circuit. This allows the number of steps to be reduced. can be reduced.

[0068] Here, the circuit of the hysteresis comparator (hysteresis comparator 205) shown in FIG. An example of the circuit configuration will be described with reference to FIG. 4. FIG. 4 shows the hysteresis comparator shown in FIG. FIG. 2 is a circuit diagram showing an example of a circuit configuration of a regulator.

[0069] The hysteresis comparator shown in FIG. 4 includes a comparator 221 and a comparator 222. , inverter 223, inverter 224, NOR gate 225, and NOR gate 22 6 and.

[0070] The comparator 221 has a first input terminal, a second input terminal, and an output terminal. A reference high voltage (reference voltage Vref H Or just Vref H (also called) is given A signal S22 is input to the second input terminal.

[0071] The comparator 222 has a first input terminal, a second input terminal, and an output terminal. A signal S22 is input to the input terminal, and a low voltage (reference voltage Vre f L Or just Vref L The reference voltage Vref L The value of is the base Reference voltage Vref H is less than the value of

[0072] The inverter 223 has an input terminal and an output terminal. The input terminal is connected to the output terminal of the comparator 221. The input terminal is electrically connected to the power terminal.

[0073] The inverter 224 has an input terminal and an output terminal. The input terminal is connected to the output terminal of the comparator 222. The input terminal is electrically connected to the power terminal.

[0074] The NOR gate 225 has a first input terminal, a second input terminal, and an output terminal. The input terminal is electrically connected to the output terminal of the inverter 223. The connection point between the first input terminal of inverter 5 and the output terminal of inverter 223 is referred to as node S.

[0075] NOR gate 226 has a first input terminal, a second input terminal, and an output terminal. The input terminal is electrically connected to the output terminal of the NOR gate 225, and the second input terminal is the output terminal of the NOR gate 224 is electrically connected to the second input of the NOR gate 225. The first input terminal of the NOR gate 226 is electrically connected to the inverter 2 The connection point with the output terminal of 24 is node R.

[0076] In addition, the comparator 221, the comparator 222, the inverter 223, and the inverter 224 , NOR gate 225, and NOR gate 226 are each formed of a transistor. The transistor is provided with, for example, an oxide semiconductor having a function as a channel forming layer. The oxide semiconductor layer has a hydrogen concentration of 5×10 19 atoms / cm 3 The following are the preferred Or 5×10 18 atoms / cm 3 Less than 5×10, more preferably 17 atoms / cm 3 The carrier concentration is 1×10 12 / cm 3 Less than 1 x 10 1 1 / cm 3 In this embodiment, a transistor having a capacitance of less than 100 Ω can be used. Each logic circuit can be constructed using transistors of the same conductivity type. By constructing each logic circuit using transistors of the same conductivity type, the manufacturing process is simplified. It can be simplified.

[0077] As shown in Figure 4, the hysteresis comparator shown in Figure 3 has two comparators. The configuration has two comparators, and the voltage of the signal input to each of the two comparators is (The output voltage of the DC conversion circuit shown in Figure 3) and the reference voltage (reference voltage Vref H Or base Reference voltage Vref L ) is compared with and a pulse signal with a duty ratio set according to the comparison result is generated. Output the number.

[0078] Next, an example of the operation of the hysteresis comparator shown in FIG. 4 will be described.

[0079] An example of the operation of the hysteresis comparator shown in Figure 4 is as follows: The voltage at node N2 (voltage V N2 Or simply VN2 (also called the reference voltage Vref H twist If high (V N2 >Vref H ), voltage V N2 is the reference voltage Vref L Higher, reference voltage Vref H If lower (Vref H >V N2 >Vref L ), voltage V N2 is the reference voltage V ref L If lower (Vref L >V N2 ) In each case This will be explained below.

[0080] V N2 >Vref H When the potential of node S is V H The potential of node R becomes V L Become At this time, the potential of node Q becomes V L The output of the hysteresis comparator shown in Figure 4 is Signal (Signal OUT HCMP (also called the "current-transmitting" signal) will be at a low level.

[0081] Vref H >V N2 >Vref L When the potential of node S is V L The potential of node R becomes V L In this case, node Q maintains the state of node Q in the previous period. For example, if the potential of node Q was V H In this case, the potential of node Q is V H and The output signal of the hysteresis comparator also remains at high level, and the The potential of Q is V L When the potential of node Q is V L The signal remains OUTHCMP Moro It remains at the - level.

[0082] Vref L >V N2 When the potential of node S is V L The potential of node R becomes V H Become At this time, the potential of node Q is V H The output signal of the hysteresis comparator becomes It becomes an extreme level.

[0083] Further, an example of the operation of the hysteresis comparator of this embodiment will be described with reference to FIG. FIG. 5 illustrates an example of the operation of the hysteresis comparator according to the present embodiment. This is a timing chart for setting the voltage V N2 , the voltage of node S (V NS Also called , the voltage at node R (V NR ), and the waveform of the output signal of the hysteresis comparator are shown respectively.

[0084] As shown in Figure 5, for example, the voltage V N2 If is a triangular wave, Vref L >V N2 During The voltage of node S is kept at low level. Then, Vref L >V N2 From Vref L <V N2 When this happens, the voltage at node R goes from high to low, and Vref H >V N2 >Vref L During this time, the signal is OUT HCMP Furthermore, Vre is maintained at a high level. f H >V N2 >Vref L From V N2 >Vref HWhen this happens, the voltage of node S becomes low. The signal OUT HCMP goes from high to low. V N 2>Vref H During this time, the voltage of node S is maintained at a high level. N2 >V ref H From Vref H >V N2 When this happens, the voltage at node S changes from high to low. In addition, Vref H >V N2 >Vref L During this time, the signal is OUT HCMP Low level In this way, the voltage V N2 A pulse signal based on The above is an example of the operation of the hysteresis comparator shown in FIG.

[0085] As described above, as an example shown in FIG. 2 to FIG. 4, an example of the DC converter circuit of the present embodiment is an inductor. A coil that functions as a conductive element and a transistor that functions as a switching element. A capacitor having a function as a smoothing capacitor is used. a hysteresis comparator for controlling the on or off state of the transistor; , the configuration is provided with:

[0086] Further, in the DC converter circuit of this embodiment, an oxide having a function as a channel forming layer is provided. The oxide semiconductor layer has a hydrogen concentration of 5×10 19 atoms / cm 3 below , preferably 5 x 10 18 atoms / cm 3 Less than 5×10, more preferably 17 at oms / cm 3The carrier concentration is 1×10 12 / cm 3 Less than 1x, preferably 10 11 / cm 3 The transistor may be configured to have a capacitance less than 100 Ω. Compared to conventional silicon-based transistors, for example, the transistors have a lower off-state current and are highly insulating. High voltage resistance. Therefore, by using it as a transistor that configures a DC conversion circuit, This prevents the transistor from being destroyed even when a high voltage is applied between the terminals of the transistor. This can be done.

[0087] Next, an example of the operation of the DC conversion circuit shown in FIG. 3 will be described.

[0088] The DC conversion method of the DC converter circuit of this embodiment is a pulse width modulation control method. An example of the operation of the DC converter circuit shown in FIG. 3 can be divided into a period T51 and a period T52. The operation in the period T51 and the operation in the period T52 are repeated alternately. The respective periods are explained below.

[0089] In the period T51, the trigger is generated in accordance with the pulse signal input from the hysteresis comparator 205. The transistor 202 is turned on, and the voltage of the node N1 becomes the input voltage of the DC converter circuit shown in FIG. The voltage at node N1 becomes equal to the voltage at node N2, and diode 203 becomes non-conductive. When the input voltage becomes equal to the input voltage, a current flows through the coil 201. At 1, an electromotive force is generated.

[0090] During the period T52, the transistor is turned on by the pulse signal input from the hysteresis comparator 205. At this time, the magnetic field generated in the coil 201 is In order to suppress the change, an electromotive force V2 in the opposite direction to the electromotive force V1 is generated, and the diode 203 When the diode 203 is turned on, a current flows through the coil 201. By repeating the periods T51 and T52, the voltage of the node N2 decreases. The output voltage of the DC converter shown in FIG. 3 is smaller than the input voltage. The value of the output voltage is The ratio of the length of period T51 to the length of period T52, in other words, the duty ratio of the pulse signal. For example, in periods T51 and T52, if the output voltage is greater than the desired value, the pulse The duty cycle of the signal is set low by the hysteresis comparator 205. Also, if the output voltage is less than the desired value, the duty ratio of the pulse signal is set to hysteresis. It is set high by the lysis comparator 205. Thus, the In the DC conversion circuit, the output voltage for each unit period is fed to the hysteresis comparator 205. By backing up the output voltage, the output voltage can be adjusted to the desired value during the following period. do.

[0091] As shown in FIG. 3, an example of the DC converter circuit of the present embodiment is a DC converter circuit that receives an input from a control circuit. A transistor electrically connected to the first terminal of the coil in response to the duty ratio of the input pulse signal The input voltage is converted to a different value by switching the transistor alternately on and off. By generating an output voltage, it can function as a voltage booster circuit or a voltage drop circuit.

[0092] This embodiment mode can be appropriately combined with or replaced by other embodiment modes. do.

[0093] (Embodiment 3) This embodiment can be applied to the transistors constituting the DC conversion circuit disclosed in this specification. An example of a transistor will be shown.

[0094] One embodiment of a transistor and a manufacturing method of the transistor according to this embodiment will be described with reference to FIGS. I will explain this in more detail.

[0095] 6(A) and (B) show examples of the planar and cross-sectional structures of a transistor. The transistor 410 shown is one with a top-gate structure.

[0096] FIG. 6A is a plan view of a transistor 410 having a top-gate structure, and FIG. FIG. 2 is a cross-sectional view taken along line C1-C2 of (A).

[0097] The transistor 410 includes an insulating layer 407, an oxide semiconductor layer 412, a source electrode layer 415a, a drain electrode layer 415b, a gate insulating layer 402, and The gate electrode layer 411 is included, a wiring layer 414a is in contact with a source electrode layer 415a, and a drain electrode The wiring layer 414b contacts the pole layer 415b.

[0098] In addition, in FIGS. 6A and 6B, a transistor having a single gate structure is used as the transistor 410. The transistor in this embodiment will be described using a transistor having a channel formation region. A transistor having a multi-gate structure having a plurality of transistors may be used.

[0099] Hereinafter, a process of manufacturing a transistor 410 on a substrate 400 will be described with reference to FIGS. Explain.

[0100] There is no significant limitation on the substrate that can be used for the substrate 400 having an insulating surface. In both cases, the substrate must have sufficient heat resistance to withstand heat treatment. 00 includes glass substrates such as barium borosilicate glass and aluminoborosilicate glass. can be used.

[0101] Instead of the above glass substrate, an insulating substrate such as a ceramic substrate, a quartz substrate, or a sapphire substrate may be used. Alternatively, a substrate made of an insulating material may be used. Alternatively, a crystallized glass substrate or the like may be used. Plastic substrates and the like can also be used as appropriate. A semiconductor substrate of the above type may also be used.

[0102] First, an insulating layer 407 is formed as a base film on a substrate 400 having an insulating surface. 07 includes a silicon oxide layer and a silicon oxynitride layer (SiO x N y Also called, however, x>y>0), an oxide insulating layer such as an aluminum oxide layer or an aluminum oxynitride layer The insulating layer 407 is preferably formed by a plasma CVD method or a sputtering method. However, it is necessary to prevent a large amount of hydrogen from being contained in the insulating layer 407. To achieve this, the insulating layer 407 is preferably formed by a sputtering method.

[0103] In this embodiment, a silicon oxide layer is formed as the insulating layer 407 by a sputtering method. The substrate 400 is transferred to a processing chamber, where hydrogen and moisture are removed and a high-purity sputtering agent containing oxygen is applied. A targeting gas is introduced, and a silicon semiconductor target is used to oxidize the insulating layer 407. A silicon layer is formed on the substrate 400. In addition, when forming the insulating layer 407, the substrate 40 0 may be at room temperature or may be heated.

[0104] In this embodiment, for example, quartz (preferably The substrate temperature was 108°C, and the distance between the substrate and the target (TS distance) was 10 60 mm, pressure 0.4 Pa, high frequency power supply 1.5 kW, oxygen and argon (oxygen flow rate 25 The deposition was performed by RF sputtering under an atmosphere of argon (25 sccm: argon flow rate 1:1). A silicon oxide film is formed. The thickness of the silicon oxide film is 100 nm. Instead of quartz (preferably synthetic quartz), a silicon oxide film is formed using a target. A silicon target can be used as the sputtering gas. Alternatively, a mixture of oxygen and argon gas can be used.

[0105] When the insulating layer 407 is formed using any of the above materials and methods, It is preferable to form the insulating layer 407 while removing residual moisture. This is to prevent the inclusion of hydroxyl groups or moisture.

[0106] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium It is preferable to use a sublimation pump. As an exhaust means, for example, a turbocharger is used. A cryopump equipped with a cold trap can be used. In the deposition chamber that has been evacuated, hydrogen atoms and compounds containing hydrogen atoms (such as water) are present. Since the exhaust gas is exhausted, the insulating layer 407 formed by film formation in the film formation chamber is The concentration of impurities (especially hydrogen) can be reduced.

[0107] The sputtering gas used in forming the insulating layer 407 is hydrogen, water, or hydroxide. High purity, with impurities such as bases or hydrides removed to concentrations of about ppm or ppb. It is preferable to use a gas.

[0108] In addition, the sputtering method uses RF sputtering, which uses a high-frequency power source as the sputtering power source. The sputtering method uses a direct current power source, the DC sputtering method uses a pulsed bias, and The RF sputtering method is mainly used for forming insulating films. The DC sputtering method is mainly used for depositing metal films.

[0109] In addition, the sputtering equipment is a multi-target sputtering system that can accommodate multiple targets of different materials. Multi-target sputtering equipment is a type of equipment that deposits different material films in the same chamber. It is possible to deposit layers or to deposit films by discharging multiple types of materials simultaneously in the same chamber. can.

[0110] The sputtering device is a magnetron with a magnet mechanism inside the chamber. Sputtering equipment that uses the sputtering method and microwaves that do not use glow discharge There is a sputtering device that uses the ECR sputtering method using generated plasma. .

[0111] In addition, in the sputtering method, a target material and a sputtering gas component are mixed during film formation. Reactive sputtering is a method of forming thin films of these compounds by chemically reacting them with each other, and film formation is also used. There is also a bias sputtering method in which a voltage is applied to the substrate as well.

[0112] The insulating layer 407 may have a laminated structure. For example, the insulating layer 407 may have a nitride insulating layer and a The nitride insulating layer may have a laminated structure with an oxide insulating layer. , silicon oxynitride (SiN x O y (x>y>0) layer, aluminum nitride As the oxide insulating layer, an aluminum layer, an aluminum nitride oxide layer, or the like can be used. a silicon oxynitride layer, a silicon oxynitride layer, an aluminum oxide layer, or an aluminum oxynitride layer etc. can be used.

[0113] For example, a high-purity sputtering gas containing nitrogen and from which hydrogen and moisture have been removed is introduced. A silicon nitride layer is formed on the substrate using a cone target, and an oxide layer is formed on the silicon nitride layer. In this case, the silicon layer is formed. In the same manner as the silicon oxide layer, the residual silicon in the processing chamber is removed. It is preferable to form the silicon nitride layer while removing moisture.

[0114] In addition, when forming the silicon nitride layer, the substrate 400 may be heated.

[0115] When a silicon nitride layer and a silicon oxide layer are laminated as the insulating layer 407, forming a silicon nitride layer and a silicon oxide layer using a common silicon target in a semiconductor device; First, nitrogen-containing sputtering gas is introduced to the silicon wafer mounted in the processing chamber. A silicon nitride layer is formed using a silicon target, and then the sputtering gas is changed to an oxygen-containing Switch to sputtering gas and form silicon oxide layer using same silicon target This allows the silicon nitride layer and the silicon oxide layer to be formed without exposing the substrate 400 to the atmosphere. Since the silicon nitride layer can be continuously formed, impurities such as hydrogen and moisture on the surface of the silicon nitride layer can be prevented. It is possible to prevent the adhesion of the particles.

[0116] Next, an oxide semiconductor film is formed over the insulating layer 407 to a thickness of 2 nm to 200 nm.

[0117] In order to prevent hydrogen, a hydroxyl group, and moisture from being contained in the oxide semiconductor film as much as possible, As a pretreatment, the substrate 400 on which the insulating layer 407 is formed is placed in a preheating chamber of a sputtering device. The substrate 400 is preheated at 400 to remove impurities such as hydrogen and moisture adsorbed on the substrate 400 and then exhausted. As the exhaust means provided in the preheating chamber, for example, a cryopump is preferable. It is preferable to omit this preheating process. This may be performed on the substrate 400 prior to the formation of the gate insulating layer 402 to be formed later, or on the substrate 400 prior to the formation of the gate insulating layer 402 to be formed later. The same procedure was carried out on the substrate 400 on which the source electrode layer 415a and the drain electrode layer 415b were formed. This is also fine.

[0118] Note that before the oxide semiconductor film is formed by a sputtering method, argon gas is introduced. Reverse sputtering is performed to generate plasma, and the film formed during film formation that adheres to the surface of the insulating layer 407 is It is preferable to remove the powdery material (also called particles or dust) that is generated. This means that no voltage is applied to the target side, and a high-frequency power source is used on the substrate side in an argon atmosphere. This method involves applying a voltage to the substrate to generate plasma near the substrate and modifying the surface. Instead of the argon atmosphere, nitrogen, helium, oxygen, etc. may be used.

[0119] The oxide semiconductor film can be formed by a sputtering method. Examples of the oxides include In-Sn-Ga-Zn-O, which is a quaternary metal oxide, and In-Sn-Ga-Zn-O, which is a ternary metal oxide. In-Ga-Zn-O film, In-Sn-Zn-O film, In-Al-Zn-O film, Sn- Ga-Zn-O film, Al-Ga-Zn-O film, Sn-Al-Zn-O film, and binary metal oxide film In-Zn-O film, Sn-Zn-O film, Al-Zn-O film, Zn-Mg-O film , Sn-Mg-O film, In-Mg-O film, In-Sn-O film, In-O film, Sn-O film In addition, an oxide semiconductor film such as a Zn-O film can be used. SiO2 may be included.

[0120] In addition, as the oxide semiconductor film, InMO3(ZnO) m Using a membrane represented by (m>0) Here, M is one or more selected from Ga, Al, Mn, and Co. Metal element. For example, M is Ga, Ga and Al, Ga and Mn, or Ga and C. Examples include o.

[0121] In this embodiment, as an example, an oxide semiconductor film is an In-Ga-Zn-O based metal oxide substrate. The oxide semiconductor film is formed by a sputtering method using a target. Typically, the mixture is heated under an atmosphere of argon, oxygen, or a rare gas (typically argon) and oxygen. The film can be formed by sputtering in a nitrogen-mixed atmosphere. When using the ring method, a target containing 2% to 10% by weight of SiO2 is used. Film formation may also be performed.

[0122] The sputtering gas used in forming the oxide semiconductor film is hydrogen, water, a hydroxyl group, or is a high-purity gas in which impurities such as hydrides have been removed to concentrations of about ppm or ppb. It is preferable to use:

[0123] The oxide semiconductor film was prepared by sputtering using targets such as In, Ga , and a metal oxide target containing Zn (composition ratio: In2O3:Ga2O3:Zn O=1:1:1[mol%] or In:Ga:Zn=1:1:0.5[atom%]) It should be noted that the total volume of the metal oxide target to be produced is The ratio of the volume of the material to the volume of the material excluding the space occupied by voids, etc. (also called the filling rate) is 90 % or more, preferably 95% or more. Use a metal oxide target with a high filling rate. As a result, the formed oxide semiconductor film becomes a dense film.

[0124] In this embodiment, as an example, a substrate is held in a processing chamber that is maintained in a reduced pressure state. The remaining moisture in the metal is removed, and a sputtering gas from which hydrogen and moisture have been removed is introduced. An oxide semiconductor film is formed on the substrate 400 using an oxide as a target. To remove the residue, it is preferable to use an adsorption type vacuum pump. Examples of pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a cold trap in the turbo pump as the exhaust means. The deposition chamber evacuated by the cryopump can be, for example, , hydrogen atoms, water (H2O) and other compounds containing hydrogen atoms (preferably compounds containing carbon atoms) Since the oxides formed by film formation in the film formation chamber are exhausted, The concentration of impurities in the oxide semiconductor film can be reduced. Heating may also be performed.

[0125] An example of the deposition conditions is: substrate temperature at room temperature, distance between substrate and target at 60 mm, pressure at 0. 4 Pa, direct current (DC) power supply 0.5 kW, oxygen and argon (oxygen flow rate 15 sccm: argon The conditions were as follows: a 30 sccm gas flow rate atmosphere was used. By using the oxide semiconductor film, particles can be reduced and the film thickness distribution can be made uniform. The thickness of the oxide semiconductor film is preferably 5 nm to 30 nm. Since the thickness varies depending on the oxide semiconductor material to be used, the thickness may be appropriately selected depending on the material. .

[0126] Next, the oxide semiconductor film is subjected to a first photolithography process to form an island-shaped oxide semiconductor layer 41. 2 (see FIG. 7A). The resist mask may be formed by an inkjet method. By forming the conductive layer by this method, the manufacturing cost can be reduced.

[0127] The etching of the oxide semiconductor film may be performed by dry etching or wet etching. The oxide semiconductor film can be etched by dry etching. Both dry and wet etching may be used.

[0128] The etching gas used in dry etching is a gas containing chlorine (chlorine-based gas, e.g. For example, chlorine (Cl2), boron chloride (BCl3), silicon chloride (SiCl4), carbon tetrachloride (CC l4) etc.) are preferred.

[0129] In addition, the etching gas used in dry etching is a gas containing fluorine (fluorine-based Gases, such as carbon tetrafluoride (CF4), sulfur hexafluoride (SF6), nitrogen trifluoride (NF3), trifluoromethane (CHF3), hydrogen bromide (HBr), or oxygen (O2), These gases are mixed with rare gases such as helium (He) and argon (Ar). can be used.

[0130] Dry etching methods include, for example, parallel plate RIE (Reactive Ion Etching) tching) method, ICP (Inductively Coupled Plasma) (Inductively coupled plasma) etching method can be used. Etching to the desired processed shape. In order to allow for the etching to be performed, the etching conditions (the amount of power applied to the coil-shaped electrode, The amount of power applied, the temperature of the electrode on the substrate side, etc. are adjusted appropriately.

[0131] The etching solution used for wet etching is, for example, a mixture of phosphoric acid, acetic acid, and nitric acid. In addition, the etching solution used for wet etching is I TO07N (manufactured by Kanto Chemical Co., Ltd.) may also be used.

[0132] In addition, the etching solution after wet etching contains the material removed by etching. The removed material is then removed by cleaning. The waste etching solution containing the removed material is purified and The material removed by etching may be reused. By recovering and reusing materials such as indium contained in the oxide semiconductor layer from the waste liquid, This allows for more efficient use of resources and reduces manufacturing costs.

[0133] In addition, during etching, the material is adjusted to the desired shape. The etching conditions (etching solution, etching time, temperature, etc.) are adjusted appropriately.

[0134] In this embodiment, as an example, a solution of phosphoric acid, acetic acid, and nitric acid is used as the etching solution. The oxide semiconductor film was processed into an island-shaped oxide semiconductor layer 412 by wet etching. do.

[0135] Next, first heat treatment is performed on the oxide semiconductor layer 412. The temperature of the first heat treatment is 400 The temperature is set to 750° C. or higher, preferably 400° C. or higher but lower than the distortion point of the substrate. The substrate is placed in an electric furnace, which is one of heat treatment apparatuses, and the oxide semiconductor layer is heated in a nitrogen atmosphere. After heat treatment at 450℃ for 1 hour in an atmosphere, the sample was oxidized without contacting with the air. This first heat treatment prevents water and hydrogen from entering the oxide semiconductor layer, and obtains an oxide semiconductor layer. In this manner, the oxide semiconductor layer 412 can be dehydrated or dehydrogenated.

[0136] When the temperature of the heat treatment apparatus is lowered from the heat treatment temperature, the atmosphere may be changed to oxygen. When the temperature is decreased, the atmosphere is switched to oxygen, and oxygen is replenished to the oxygen vacancies in the oxide semiconductor layer. Oxygen vacancies generate carriers, but their disappearance results in a significant increase in the number of carriers. Thus, an oxide semiconductor layer having an extremely low carrier concentration can be obtained.

[0137] The heat treatment device is not limited to an electric furnace, and may be a heat treatment device using heat conduction or heat radiation from a heating element such as a resistance heating element. The apparatus may be equipped with a device for heating the object to be treated by irradiation. For example, a GRTA (Gas Rapid Thermal Anneal) equipment, LRTA (Lamp Rapid Thermal Annealing (RTA) equipment The LRTA device can be used with halogen lamps, metal halide lamps, etc. lamp, xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure A device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a mercury lamp. The GRTA device is a device that uses high-temperature gas for heat treatment. An inert gas that does not react with the workpiece during heat treatment, such as a rare gas such as argon or nitrogen. A gas is used.

[0138] In the first heat treatment, the substrate is placed in an inert gas heated to 650°C to 700°C. After heating for several minutes, the substrate is removed from the inert gas heated to a high temperature for GRTA treatment. GRTA processing allows high-temperature heat treatment in a short period of time.

[0139] In the first heat treatment, the atmosphere during the heat treatment (nitrogen, helium, neon, or rare gas such as argon) does not contain water, hydrogen, etc., or The purity of nitrogen or rare gases such as helium, neon, or argon introduced into the treatment equipment is , 6N (99.9999%) or more, preferably 7N (99.99999%) or more (i.e. It is preferable to keep the impurity concentration at 1 ppm or less, and preferably at 0.1 ppm or less.

[0140] The first heat treatment is performed on an oxide semiconductor film before it is processed into an island-shaped oxide semiconductor layer. In that case, after the first heat treatment, the substrate is taken out of the heating device and is then heated with a photo A lithography process is carried out.

[0141] The heat treatment for dehydrating and dehydrogenating the oxide semiconductor layer is performed in the oxide semiconductor layer formation. After that, a source electrode layer and a drain electrode layer are stacked on the oxide semiconductor layer, and then a source electrode After forming a gate insulating layer over the gate electrode layer and the drain electrode layer, stomach.

[0142] Next, a conductive film is formed over the insulating layer 407 and the oxide semiconductor layer 412. The conductive film may be formed by sputtering or vacuum deposition. An element selected from chromium, copper, tantalum, titanium, molybdenum, and tungsten, An alloy mainly composed of the element or an alloy film combining the above elements can be used. The conductive film can be made of manganese, magnesium, zirconium, beryllium, etc. Alternatively, a material selected from one or more of aluminum, yttrium, and the like may be used. The film may have a single-layer structure or a laminated structure of two or more layers. A single layer structure of aluminum film containing conductors is also available. A two-layer structure in which a titanium film is laminated on an aluminum film, and a titanium film and an aluminum film overlapping the titanium film are laminated. Examples include a three-layer structure with an aluminum film and a titanium film on top of that. Titanium, tantalum, tungsten, molybdenum, chromium, neodymium, scandium A film made of a single or multiple combinations of elements selected from the group consisting of aluminum, an alloy film, or a nitride film. This is also fine.

[0143] Next, a resist mask is formed on the conductive film by a second photolithography process. After etching the silicon nitride film to form the source electrode layer 415a and the drain electrode layer 415b, The resist mask is removed (see FIG. 7B). The end portion of the drain electrode layer 415b is preferably tapered. Thus, a gate insulating layer is laminated on the source electrode layer 415a and the drain electrode layer 415b. This is preferable because it improves the covering property.

[0144] In this embodiment, a titanium film having a thickness of 150 nm is formed by sputtering. A resist mask is formed on the titanium film, and the titanium film is selectively etched to form the source electrode. A layer 415a and a drain electrode layer 415b are formed.

[0145] Note that when the conductive film is etched, the oxide semiconductor layer 412 is removed, and the insulating layer The conductive film and the oxide semiconductor film were formed using different materials and etching methods so that the conductive film and the oxide semiconductor film 407 were not exposed. Adjust conditions accordingly.

[0146] In this embodiment, as an example, a titanium film is used as the conductive film and an I A n-Ga-Zn-O oxide semiconductor film was used, and ammonia water (AH) was used as the etchant. A mixture of ammonia, water, and hydrogen peroxide is used.

[0147] Note that in the second photolithography step, only a part of the oxide semiconductor layer is etched. In some cases, the oxide semiconductor layer 412 may have a groove (a recess). 15a, a resist mask for forming the drain electrode layer 415b is formed by an ink-jet method. If the resist mask is formed by the inkjet method, a photomask is not used. This reduces manufacturing costs.

[0148] The exposure to light used to form the resist mask in the second photolithography process is ultraviolet light or KrF laser. The source electrode layers adjacent to each other on the oxide semiconductor layer 412 are exposed to the laser beam or the ArF laser beam. The width of the gap between the end of the drain electrode layer and the bottom end of the drain electrode layer determines the channel width of the transistor to be formed later. When performing exposure with a channel length L of less than 25 nm, the channel length L is determined by the channel length L. Extreme ultraviolet rays have extremely short wavelengths of up to several tens of nanometers. The resist mask is formed in the second photolithography process using the ultraviolet light. Line exposure has high resolution and a large depth of focus. It is also possible to set the channel length L to 10 nm or more and 1000 nm or less, and the operating speed of the circuit is The off-current value can be made extremely small, resulting in low power consumption. It is also possible to achieve this.

[0149] Next, the insulating layer 407, the oxide semiconductor layer 412, the source electrode layer 415a, and the drain electrode layer 4 A gate insulating layer 402 is formed over 15b (see FIG. 7C).

[0150] The gate insulating layer 402 is formed by depositing silicon oxide using a plasma CVD method or a sputtering method. A silicon layer, a silicon nitride layer, a silicon oxynitride layer, a silicon oxynitride layer, or an aluminum oxide layer. The gate insulating layer 402 may be formed as a single layer or a stacked layer. In order to prevent a large amount of from being contained, the gate insulating layer 402 is formed by a sputtering method. In the case where the silicon oxide film is formed by the sputtering method, for example, For example, a silicon target or a quartz target is used as the target, and The treatment is carried out using oxygen or a mixed gas of oxygen and argon.

[0151] The gate insulating layer 402 is, for example, HfO x (x>0) etc. can also be used. The gate insulating layer 402 is made of HfO x By using the above, from the oxide semiconductor layer side The leakage current flowing toward the gate electrode can be reduced.

[0152] The gate insulating layer 402 is also covered with an oxide film from the source electrode layer 415a and the drain electrode layer 415b side. Alternatively, a silicon oxide layer and a silicon nitride layer may be laminated. For example, the first gate A silicon oxide layer (SiO x (x>0) A second gate insulating layer is formed on the first gate insulating layer by a sputtering method. A silicon nitride layer (SiN y (y>0)) to form a film The gate insulating layer may be 100 nm thick. In this embodiment, as an example, Pa, high frequency power supply 1.5 kW, oxygen and argon (oxygen flow rate 25 sccm: argon flow rate A 100 nm thick oxide film was deposited by RF sputtering under a 25 sccm (1:1) atmosphere. A recon layer is formed.

[0153] Next, a resist mask is formed by a third photolithography process, and selective etching is performed. A part of the gate insulating layer 402 is removed by etching to form a source electrode layer 415a and a drain electrode Openings 421a and 421b are formed reaching layer 415b (see FIG. 7(D)).

[0154] Next, a conductive film is formed over the gate insulating layer 402, the opening 421a, and the opening 421b, and then A gate electrode layer 411, a wiring layer 414a, and a wiring layer 41 The resist mask 4b may be formed by an ink-jet method. If the mask is formed by an inkjet method, the manufacturing cost can be reduced.

[0155] The gate electrode layer 411, the wiring layer 414a, and the wiring layer 414b are made of molybdenum, titanium, or the like. Tantalum, chromium, tantalum, tungsten, aluminum, copper, neodymium, scandium, etc. It is formed in a single layer or laminated form using any metal material or alloy material that contains these as the main component. It is possible.

[0156] For example, a two-layer laminate structure of a gate electrode layer 411, a wiring layer 414a, and a wiring layer 414b may be used. For example, a two-layer structure with a molybdenum layer laminated on an aluminum layer, or a molybdenum layer laminated on a copper layer Two-layer structure with a butene layer laminated on top of a copper layer, and two-layer structure with a titanium nitride layer or tantalum nitride layer laminated on top of a copper layer A layered structure or a two-layered structure in which a titanium nitride layer and a molybdenum layer are laminated is preferred. The three-layer laminate structure is a tungsten layer or a tungsten nitride layer and an aluminum layer. A layer of an alloy of aluminum and silicon or an alloy of aluminum and titanium, and a layer of titanium nitride or a layer of titanium. It is preferable that the gate electrode has a laminated structure in which a light-transmitting conductive film is used. A light-transmitting gate electrode layer 411 and wiring layers 414a and 414b can also be formed. The conductive film may be, for example, a transparent conductive oxide.

[0157] In this embodiment, as an example, a titanium film having a thickness of 150 nm is formed by sputtering. A gate electrode layer 411, a wiring layer 414a, and a wiring layer 41 Form 4b.

[0158] Next, a second heat treatment (preferably 200 The temperature is from 250° C. to 350° C., for example. A second heat treatment is performed in a nitrogen atmosphere at 250° C. for 1 hour. Even if a protective insulating layer or a planarizing insulating layer is formed on the transistor 410 and then the second heat treatment is performed, good.

[0159] Through the above steps, the oxide semiconductor layer 41 in which the concentrations of hydrogen, moisture, hydrides, and hydroxides are reduced is obtained. A transistor 410 having a first conductivity type and a second conductivity type can be formed (see FIG. 7E).

[0160] A protective insulating layer or a planarization insulating layer for planarization may be provided over the transistor 410. For example, a silicon oxide layer, a silicon nitride layer, a silicon oxynitride layer, The silicon nitride oxide layer or the aluminum oxide layer can be formed as a single layer or a stacked layer. do.

[0161] The planarizing insulating layer may be made of polyimide, acrylic, benzocyclobutene, or polyamide. Heat-resistant organic materials such as epoxy can be used. Other materials include low-k materials, siloxane resins, PSG (phosphorus glass), and B It is possible to use PSG (polysilicon boron glass) and other materials. A planarization insulating layer may be formed by stacking a plurality of insulating films.

[0162] The siloxane-based resin is a Si-O- formed material that is formed from a siloxane-based material. This corresponds to a resin containing Si bonds. Siloxane-based resins have organic groups (e.g., aryl groups) as substituents. The organic group may be a fluoro group. It is okay to do so.

[0163] The method for forming the flattening insulating layer is not particularly limited. Depending on the material, the method may be a sputtering method, a SO G method, spin coating, dip, spray coating, droplet ejection method (inkjet method, screen Printing methods such as doctor knife, roll printing, and offset printing can also be used. The coating can be performed using a roll coater, curtain coater, knife coater, or the like.

[0164] When the oxide semiconductor film is formed as described above, moisture remaining in the atmosphere during the film formation is removed. As a result, the concentrations of hydrogen and hydride in the oxide semiconductor film can be reduced. This makes it possible to stabilize the characteristics of the star.

[0165] As described above, in a DC converter circuit including a transistor including an oxide semiconductor layer, It is possible to provide a highly reliable DC conversion circuit having stable electrical characteristics.

[0166] This embodiment mode can be combined with or replaced with any of the other embodiment modes as appropriate.

[0167] (Embodiment 4) This embodiment can be applied to the transistors constituting the DC conversion circuit disclosed in this specification. Another example of a transistor will be described. Note that the transistor may have the same parts as those in the third embodiment or parts having similar functions. The steps and operations may be the same as those in the third embodiment, and the repeated explanations will be omitted as appropriate. Detailed explanations of the same parts will also be omitted as appropriate.

[0168] One embodiment of a transistor and a manufacturing method of the transistor of this embodiment will be described with reference to FIGS. I will explain this in more detail.

[0169] 8(A) and (B) show examples of the planar and cross-sectional structures of a transistor. The transistor 460 shown is one with a top-gate structure.

[0170] FIG. 8A is a plan view of a transistor 460 having a top-gate structure, and FIG. 8(A) is a cross-sectional view taken along line D1-D2 of FIG. 8(A).

[0171] The transistor 460 includes an insulating layer 457, a source electrode layer 458, and a gate insulating layer 459 on a substrate 450 having an insulating surface. and the electrode layer 465a1 or 465a2 which becomes one of the drain electrode layers, an oxide semiconductor the layer 462, an electrode layer 465b which is the other of the source and drain electrode layers, and a wiring layer 468 , a gate insulating layer 452, a gate electrode layer 461 (461a, 461b), and an electrode layer 46 5a (465a1, 465a2) is electrically connected to the wiring layer 464 via the wiring layer 468. Although not shown, the electrode layer 465b is also provided on the gate insulating layer 452. Electrical connection is made to the wiring layer in the opening.

[0172] Hereinafter, a process of manufacturing a transistor 460 on a substrate 450 will be described with reference to FIGS. Explain.

[0173] First, an insulating layer 457 serving as a base film is formed over a substrate 450 having an insulating surface.

[0174] In this embodiment, the substrate 450 is transferred to a processing chamber, where hydrogen and moisture are removed and oxygen-containing High purity sputtering gas is introduced and a silicon target or quartz (preferably synthetic quartz) is used. Using the above, a silicon oxide film was formed on the substrate 450 as an example of an insulating layer 457 by a sputtering method. The sputtering gas is oxygen or a mixture of oxygen and argon. A mixture of gases is used.

[0175] In this embodiment, for example, the purity is 6N, and quartz (preferably synthetic quartz) is used as the target. The substrate temperature was 108°C, and the distance between the substrate and the target (TS distance) was 60 mm. , pressure 0.4 Pa, high frequency power supply 1.5 kW, oxygen and argon (oxygen flow rate 25 sccm: Silicon oxide was deposited by RF sputtering in an argon atmosphere (flow rate 25 sccm = 1:1). The thickness of the silicon oxide film is 100 nm. Instead of quartz, a silicon target is used as a target for depositing silicon oxide film. A t can be used.

[0176] In the case where the insulating layer 457 is formed using any of the above materials and methods, It is preferable to form the insulating layer 457 while removing residual moisture. This is to prevent the inclusion of acid groups or moisture.

[0177] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium pumps. It is preferable to use a sublimation pump. A cryopump equipped with a cold trap can be used. The deposition chamber that has been evacuated contains, for example, hydrogen atoms and compounds that contain hydrogen atoms (such as water). Since the gas is evacuated, the concentration of impurities contained in the insulating layer 457 by forming the film in the film forming chamber is can be reduced.

[0178] The sputtering gas used in forming the insulating layer 457 may be hydrogen, water, a hydroxyl group, or High-purity gas in which impurities such as hydrides have been removed to concentrations of ppm or ppb. It is preferable to use

[0179] The insulating layer 457 may have a laminated structure. For example, the insulating layer 457 may have a nitride insulating layer and an oxide insulating layer. The nitride insulating layer may be a laminated layer of, for example, silicon nitride. A silicon layer, a silicon oxynitride layer, an aluminum nitride layer, or an aluminum oxynitride layer, etc. The oxide insulating layer may be a silicon oxide layer, a silicon oxynitride layer, or an oxide An aluminum layer, an aluminum oxynitride layer, or the like can be used.

[0180] For example, a high-purity sputtering gas containing nitrogen and from which hydrogen and moisture have been removed is introduced. A silicon nitride layer is formed on the substrate using a cone target, and an oxide layer is formed on the silicon nitride layer. In this case, the silicon layer is formed. In the same manner as the silicon oxide layer, the residual silicon in the processing chamber is removed. It is preferable to form the silicon nitride layer while removing moisture.

[0181] Next, a conductive film is formed over the insulating layer 457, and the conductive film is A resist mask is formed on the electrode layers 465a1 and 465a2 by selectively etching the resist mask. After the electrode layers 465a1 and 465b2 are formed, the resist mask is removed (see FIG. 9A). Although 65a2 is shown as being divided in the cross-sectional view, it is a continuous film. When the ends of the source electrode layer and the drain electrode layer are tapered, the gate insulating layer This is preferable because it improves the covering property.

[0182] The material of the electrode layers 465a1 and 465a2 may be aluminum, chromium, copper, tantalum, An element selected from titanium, molybdenum, and tungsten, or an alloy containing the above elements as the main component Alternatively, an alloy film of a combination of the above elements can be used. Materials for 5a1 and 465a2 include manganese, magnesium, zirconium, and beryllium. Alternatively, a material selected from one or more of aluminum, yttrium, and the like may be used. The film may have a single-layer structure or a laminated structure of two or more layers. A single layer structure of an aluminum film containing silicon is also available. A two-layer structure in which a titanium film is laminated on an aluminum film, and a titanium film and an aluminum film are laminated on the titanium film. Examples include a three-layer structure in which a tungsten film is laminated on top of the titanium film. , aluminum, titanium, tantalum, tungsten, molybdenum, chromium, neodymium, A film of a single or a combination of elements selected from scandium, An alloy film in which several elements are combined, or a nitride film in which one or several of the elements are combined may be used. good.

[0183] In this embodiment, the electrode layers 465a1 and 465a2 are formed by sputtering to a thickness of 15 A 0 nm titanium film is formed.

[0184] Next, an oxide semiconductor film is formed over the insulating layer 457 to a thickness of 2 nm to 200 nm.

[0185] Next, an oxide semiconductor film is formed, and an island-shaped oxide semiconductor is formed by a second photolithography process. The oxide semiconductor film is processed into a layer 462 (see FIG. 9B). The film is formed by sputtering using a Ga-Zn-O metal oxide target.

[0186] In this embodiment, as an example, a substrate is held in a processing chamber that is maintained in a reduced pressure state. The remaining moisture in the metal is removed, and a sputtering gas from which hydrogen and moisture have been removed is introduced. An oxide semiconductor film is formed on the substrate 450 using an oxide as a target. To remove the residue, it is preferable to use an adsorption type vacuum pump. Examples of pumps include cryopumps, ion pumps, and titanium sublimation pumps. As an exhaust means, a turbo pump equipped with a cold trap is preferably used. The deposition chamber evacuated by the cryopump can be filled with, for example, water. Compounds containing hydrogen atoms, such as water (H2O), are more preferable. Compounds containing carbon atoms Since the exhaust gas such as fluorine and the like is exhausted, the oxide semiconductor film is formed in the deposition chamber. The concentration of impurities contained in the oxide semiconductor film can be reduced. .

[0187] In addition, the sputtering gas used in forming the oxide semiconductor film is hydrogen, water, or water. High purity, with impurities such as acid groups or hydrides removed to concentrations of ppm or ppb. It is preferable to use a high-temperature gas.

[0188] An example of the deposition conditions is: substrate temperature at room temperature, distance between substrate and target at 60 mm, pressure at 0. 4 Pa, direct current (DC) power supply 0.5 kW, oxygen and argon (oxygen flow rate 15 sccm: argon The conditions were as follows: a 30 sccm gas flow rate atmosphere was used. By using the oxide semiconductor film, particles can be reduced and the film thickness distribution can be made uniform. The thickness of the oxide semiconductor film is preferably 5 nm to 30 nm. Since the thickness varies depending on the oxide semiconductor material to be used, the thickness may be appropriately selected depending on the material. .

[0189] In this embodiment, as an example, a solution of phosphoric acid, acetic acid, and nitric acid is used as the etching solution. The oxide semiconductor film is processed into an island-shaped oxide semiconductor layer 462 by wet etching. do.

[0190] Next, first heat treatment is performed on the oxide semiconductor layer 462. The temperature of the first heat treatment is 400 The temperature is set to 750° C. or higher, preferably 400° C. or higher but lower than the distortion point of the substrate. The substrate is placed in an electric furnace, which is one of heat treatment apparatuses, and the oxide semiconductor layer is heated in a nitrogen atmosphere. After heat treatment at 450℃ for 1 hour in an atmosphere, the sample was oxidized without contacting with the air. This first heat treatment prevents water and hydrogen from entering the oxide semiconductor layer, and obtains an oxide semiconductor layer. In this manner, the oxide semiconductor layer 462 can be dehydrated or dehydrogenated.

[0191] When the temperature of the heat treatment apparatus is lowered from the heat treatment temperature, the atmosphere may be changed to oxygen. When the temperature is decreased, the atmosphere is switched to oxygen, and oxygen is replenished to the oxygen vacancies in the oxide semiconductor layer. Oxygen vacancies generate carriers, but their disappearance significantly reduces the number of carriers. In this way, an oxide semiconductor layer with an extremely low carrier concentration can be obtained.

[0192] The heat treatment device is not limited to an electric furnace, and may be a heat treatment device using heat conduction or heat radiation from a heating element such as a resistance heating element. The apparatus may be equipped with a device for heating the object to be treated by irradiation. For example, a GRTA device, a LR device, etc. For example, a TA apparatus or other RTA apparatus can be used as the first heat treatment. The substrate is placed in an inert gas atmosphere heated to a high temperature of 0°C to 700°C, and after heating for several minutes, GRTA may be performed by moving the plate out of the inert gas heated to a high temperature. The use of this material makes it possible to carry out high-temperature heat treatment in a short period of time.

[0193] In the first heat treatment, nitrogen or a rare gas such as helium, neon, or argon is used. It is preferable that the nitrogen introduced into the heat treatment device does not contain water, hydrogen, etc. The purity of rare gases such as helium, neon, and argon is 6N (99.9999%) or higher. Preferably, the concentration of impurities is 7N (99.99999%) or more (i.e., the impurity concentration is 1 ppm or less, It is preferable to keep the concentration of the EDTA concentration at 0.1 ppm or less.

[0194] In addition, the first heat treatment of the oxide semiconductor layer is performed on the oxide semiconductor layer before it is processed into the island-shaped oxide semiconductor layer. In this case, the substrate is removed from the heating device after the first heat treatment. The substrate is then taken out and subjected to a photolithography process.

[0195] The heat treatment for dehydrating and dehydrogenating the oxide semiconductor layer is performed in the oxide semiconductor layer formation. After the formation of the oxide semiconductor layer, a source electrode layer and a drain electrode layer are further laminated on the oxide semiconductor layer. After forming the gate insulating layer on the source electrode layer and the drain electrode layer, It is also possible.

[0196] Next, a conductive film is formed over the insulating layer 457 and the oxide semiconductor layer 462, and then a third photolithography is performed. A resist mask is formed on the conductive film by a lithography process, and selective etching is performed to form a conductive film. After the electrode layer 465b and the wiring layer 468 are formed, the resist mask is removed (see FIG. 9(C)). The electrode layer 465b and the wiring layer 468 are made of the same material and process as the electrode layers 465a1 and 465a2. It is sufficient to form the

[0197] In this embodiment, as an example, a titanium film having a thickness of 150 nm is formed by sputtering. Then, a resist mask is formed on the titanium film by a third photolithography process. Then, etching is performed to form the electrode layer 465b and the wiring layer 468. Since the same titanium film is used for the pole layers 465a1, 465a2 and the electrode layer 465b, There is no selective ratio between 465a1, 465a2 and the electrode layer 465b in the etching. Therefore, the electrode layers 465a1 and 465a2 are etched when the electrode layer 465b is etched. In order to prevent the wiring layer 468 from being covered with the oxide semiconductor layer 462, the wiring layer 468 is provided on the electrode layer 465a2. The electrode layers 465a1 and 465a2 and the electrode layer 465b are provided with a ferroelectric film in an etching process. When a different material having a high selectivity is used, the electrode layer 465a2 is removed during etching. The protective wiring layer 468 is not necessarily provided.

[0198] Note that the conductive film is etched so that the oxide semiconductor layer 462 is not removed. The materials and etching conditions of the oxide semiconductor film and the oxide semiconductor film are adjusted as appropriate.

[0199] In this embodiment, as an example, a titanium film is used as the conductive film and an I A n-Ga-Zn-O oxide semiconductor film was used, and ammonia water (AH) was used as the etchant. A mixture of ammonia, water, and hydrogen peroxide is used.

[0200] Note that in the third photolithography step, part of the oxide semiconductor layer 462 is etched. In some cases, the oxide semiconductor layer 462 may have a groove (a depression). b. A resist mask for forming the wiring layer 468 may be formed by an inkjet method. If the resist mask is formed by the inkjet method, no photomask is used, so manufacturing Costs can be reduced.

[0201] Next, the insulating layer 457, the oxide semiconductor layer 462, the electrode layers 465a1 and 465a2, and the electrode layer 4 65 b , a gate insulating layer 452 is formed on the wiring layer 468 .

[0202] The gate insulating layer 452 is formed by depositing silicon oxide using a plasma CVD method or a sputtering method. A silicon layer, a silicon nitride layer, a silicon oxynitride layer, a silicon oxynitride layer, or an aluminum oxide layer. The gate insulating layer 452 may be formed as a single layer or a stacked layer. In order to prevent a large amount of SiO2 from being contained, the gate insulating layer 452 is formed by sputtering. In the case where the silicon oxide film is formed by the sputtering method, for example, For example, a silicon target or a quartz target is used as the target, and a sputtering gas The heating is carried out using oxygen or a mixed gas of oxygen and argon.

[0203] The gate insulating layer 452 is, for example, HfO x etc. can also be used. Gate HfO as insulating layer 452 x By using the above, the gate electrode can be formed from the oxide semiconductor layer side. Therefore, the leakage current flowing toward the

[0204] The gate insulating layer 452 is made of silicon oxide from the electrode layers 465a1, 465a2, and 465b side. A structure in which a silicon layer and a silicon nitride layer are laminated may also be used. The pressure was 0.4 Pa, the high frequency power supply was 1.5 kW, and oxygen and argon (oxygen flow rate 25 sccm A 1000 nm thick film was deposited by RF sputtering under an argon atmosphere (flow rate 25 sccm = 1:1). 1. Form a 0 nm silicon oxide layer.

[0205] Next, a resist mask is formed by a fourth photolithography process, and selective etching is performed. A part of the gate insulating layer 452 is removed by etching to form an opening 423 reaching the wiring layer 468. Although not shown, when the opening 423 is formed, the electrode layer 465b is In this embodiment, for example, an opening to the electrode layer 465b may be formed. Further, an example in which an interlayer insulating layer is formed after laminating, and a wiring layer for electrical connection is formed in the opening is also available. do.

[0206] Next, a conductive film is formed over the gate insulating layer 452 and the opening 423, and then a fifth photolithography is performed. A gate electrode layer 461 (461a, 461b) and a wiring layer 464 are formed by a lithography process. The resist mask may be formed by an ink-jet method. Forming it by the coujet method can reduce manufacturing costs.

[0207] In addition, a conductive layer for forming a gate electrode layer 461 (461a, 461b) and a wiring layer 464 is formed. The film is made of molybdenum, titanium, chromium, tantalum, tungsten, aluminum, copper, neodymium, etc. A single layer is formed using metal materials such as zinc and scandium, or alloy materials that contain these as the main components. Alternatively, it may be formed by laminating.

[0208] In this embodiment, as an example, a titanium film having a thickness of 150 nm is formed by sputtering. Then, the gate electrode layers 461a and 461b and the wiring layer 46 Form 4.

[0209] Next, a second heat treatment (preferably 200 The temperature is from 250° C. to 350° C., for example. A second heat treatment is performed in a nitrogen atmosphere at 250° C. for 1 hour. This may be performed after forming a protective insulating layer or a planarizing insulating layer.

[0210] Through the above steps, the oxide semiconductor layer 46 in which the concentrations of hydrogen, moisture, hydrides, and hydroxides are reduced is formed. A transistor 460 having a first conductivity type and a second conductivity type can be formed (see FIG. 9E).

[0211] A protective insulating layer or a planarization insulating layer for planarization may be provided over the transistor 460. Although not shown, the gate insulating layer 452, the protective insulating layer, and the planarizing insulating layer are covered with the electrode layer 46. An opening is formed that reaches the electrode layer 465b, and a wiring layer that is electrically connected to the electrode layer 465b is formed in the opening. Complete.

[0212] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0213] As described above, when forming an oxide semiconductor film, it is necessary to remove residual moisture in the atmosphere during the film formation. As a result, the concentrations of hydrogen and hydride in the oxide semiconductor film can be reduced. This can stabilize the oxide semiconductor film.

[0214] As described above, in a DC converter circuit including a transistor including an oxide semiconductor layer, It is possible to provide a highly reliable DC conversion circuit having stable electrical characteristics.

[0215] (Embodiment 5) This embodiment can be applied to a transistor included in a DC converter circuit according to one embodiment of the present invention. An example of such a transistor will be described. The components or parts having similar functions and steps are the same as those in the third or fourth embodiment. The detailed explanation of the same part will be omitted as appropriate. do.

[0216] An example of a transistor of this embodiment will be described with reference to FIG.

[0217] An example of a cross-sectional structure of a transistor is shown in FIG. The transistors 425 and 426 each have a structure in which an oxide semiconductor layer is sandwiched between a conductive layer and a gate electrode layer. It is one of the transistors.

[0218] In addition, in FIG. 10(A) and (B), a silicon substrate is used as the substrate. Transistors 425 and 426 are provided on an insulating layer 422 provided on a plate 420. It is being done.

[0219] In FIG. 10A, an insulating layer 422 and an insulating layer 407 are provided on a silicon substrate 420. A conductive layer 427 is provided between the oxide semiconductor layer 412 and the insulating layer 424 so as to overlap with at least the entire oxide semiconductor layer 412. do.

[0220] In FIG. 10B, the conductive layer between the insulating layer 422 and the insulating layer 407 is the conductive layer 424. The oxide semiconductor layer 412 is processed by etching so as to have a channel region. This is an example that overlaps with part of the

[0221] The conductive layers 427 and 424 can be made of any metal material that can withstand the heat treatment temperature in the subsequent process. Commonly, titanium, tantalum, tungsten, molybdenum, chromium, neodymium, scandium An element selected from the above, or an alloy containing the above elements, or a combination of the above elements An alloy film or a nitride containing the above-mentioned element can be used. 427 and 424 may be a single layer structure or a laminated structure, for example, a single layer of tungsten or a single layer of nitride. The tungsten nitride layer and the tungsten layer may be laminated to form a laminate structure.

[0222] The conductive layers 427 and 424 have a potential different from that of the gate electrode layer 41 of the transistors 425 and 426. 1 may be the same as or different from the first gate electrode layer, and may also function as a second gate electrode layer. The potential of the conductive layers 427 and 424 may be a fixed potential such as GND or 0V. stomach.

[0223] The conductive layers 427 and 424 control the electrical characteristics of the transistors 425 and 426. can be done.

[0224] In addition, the present invention is not limited to the structure in which the second gate electrode layer is formed by providing a conductive layer. For example, when a semiconductor substrate is used as the substrate, the substrate is thermally oxidized to form a The deposited region can also function as a second gate electrode layer.

[0225] This embodiment mode can be combined with or replaced with any of the other embodiment modes as appropriate.

[0226] (Embodiment 6) In this embodiment, a transistor included in a DC converter circuit according to one embodiment of the present invention can be used. An example of a transistor that can be used will be described below.

[0227] An example of a transistor and a manufacturing method of the transistor of this embodiment will be described with reference to FIGS. explain.

[0228] An example of a method for manufacturing a transistor is shown in FIGS. The transistor shown in Fig. 1 has a bottom-gate structure and is also called an inverted staggered transistor. cormorant.

[0229] In addition, the transistor 390 is a transistor having a single gate structure. The transistor is a multi-gate transistor having a plurality of channel formation regions. This is also fine.

[0230] Hereinafter, a process for fabricating a transistor 390 on a substrate 394 will be described with reference to FIGS. 11(A) to 11(E). Explain the process.

[0231] First, a conductive film is formed on a substrate 394 having an insulating surface, and then a first photolithography process is performed. A resist mask is formed on the conductive film by a process, and the conductive film is selectively etched. In this way, a gate electrode layer 391 is formed. Note that the end portion of the gate electrode layer 391 is tapered. When the end of the gate electrode layer 391 is tapered, the The coating of the gate insulating layer that is to be formed is improved. The manufacturing cost can be reduced by forming the resist mask by an inkjet method. .

[0232] There is no significant limitation on the substrate that can be used for the substrate 394 having an insulating surface, but at least In any case, the substrate 394 must have a heat resistance sufficient to withstand the heat treatment. For example, a glass substrate such as barium borosilicate glass or aluminoborosilicate glass is used. It can be used.

[0233] Instead of the above glass substrate, an insulating substrate such as a ceramic substrate, a quartz substrate, or a sapphire substrate may be used. A substrate made of an insulating material may be used. Alternatively, a substrate made of crystallized glass may be used. Alternatively, a semiconductor substrate such as silicon may be used as the substrate. A solid substrate may also be used.

[0234] In addition, an insulating film serving as a base film may be provided between the substrate 394 and the gate electrode layer 391. The base film has a function of preventing the diffusion of impurity elements from the substrate 394. a silicon oxide film, a silicon nitride film, or a silicon oxynitride film; It can be formed by a laminated structure using films.

[0235] The material of the gate electrode layer 391 is molybdenum, titanium, chromium, tantalum, tungsten, or the like. Metallic materials such as zinc, aluminum, copper, neodymium, and scandium, or materials containing these as the main components The insulating film 10 can be formed as a single layer or a laminated layer using an alloy material.

[0236] For example, the two-layer stacked structure of the gate electrode layer 391 is a molybdenum layer stacked on an aluminum layer. A two-layer structure with a molybdenum layer on a copper layer, a two-layer structure with a titanium nitride layer on a copper layer A two-layer structure with a titanium nitride layer or a tantalum nitride layer laminated thereon, and a titanium nitride layer and a molybdenum layer laminated thereon or a two-layer structure in which a tungsten nitride layer and a tungsten layer are laminated. The three-layer laminate structure is preferably a tungsten layer or a tungsten nitride layer, and an aluminum layer. A layer of an alloy of aluminum and silicon or an alloy of aluminum and titanium, and a layer of titanium nitride or titanium. It is preferable that the gate electrode is formed by stacking a light-transmitting conductive film. A layer 391 can also be formed. As the conductive film having a light-transmitting property, a light-transmitting conductive oxide can be used. The following can be cited as examples.

[0237] Next, a gate insulating layer 397 is formed over the gate electrode layer 391 .

[0238] Here, the oxide semiconductor (high-temperature oxide semiconductor) that has been made i-type or substantially i-type by removing impurities is Since the gate oxide semiconductor (a purified oxide semiconductor) is extremely sensitive to the interface state and the interface charge, The interface between the gate insulating layer and the highly purified oxide semiconductor layer is important. The insulating layer (GI) is required to be of high quality.

[0239] For example, high-density plasma CVD using microwaves (2.45 GHz) produces dense, high-insulation-voltage It is preferable that a highly purified oxide semiconductor layer and a high-quality insulating film can be formed. By closely contacting the gate insulating layer, the interface state can be reduced and the interface characteristics can be improved. The high-density plasma device used here is 1×10 11 / cm 3 Any device capable of achieving the above plasma density can be used.

[0240] For example, a microwave power of 3kW to 6kW is applied to generate plasma, and the formation of an insulating film is performed. The chamber is filled with monosilane gas (SiH4) and nitrous oxide (N2 O) and rare gas are introduced to generate high-density plasma at a pressure of 10 Pa to 30 Pa. An insulating film is formed on a substrate having an insulating surface such as a silicon wafer. Then, the supply of monosilane gas is stopped. Nitrous oxide (N2O) and rare gases are introduced without exposing the insulating film to the atmosphere. Plasma treatment may be performed. At least nitrous oxide (N2O) and rare gases are introduced to provide insulation. The plasma treatment on the film surface is performed after the formation of the insulating film. The flow ratio of nitrous oxide gas (N2O) to silane gas (SiH4) is 1:10 to 1:20. The rare gas introduced into the chamber is helium, argon, chlorine, etc. Lipton, xenon, etc. can be used, but argon is the most inexpensive. is preferred.

[0241] Of course, if a good insulating film can be formed as the gate insulating layer 397, sputtering is possible. Other film formation methods such as the ring method and plasma CVD method can be applied. The quality of the gate insulating film and the interface characteristics with the oxide semiconductor are improved by heat treatment. In any case, it goes without saying that the quality of the film as a gate insulating film is good. Any material may be used as long as it can reduce the interface state density with the oxide semiconductor and form a good interface.

[0242] For example, at 85°C, 2 x 10 6 V / cm, 12-hour gate bias and thermal stress test (B In the T test, when impurities are added to an oxide semiconductor, The bonds between the main component of are broken by a strong electric field (B: bias) and high temperature (T: temperature), The dangling bonds formed induce a drift in the threshold voltage (Vth). The transistor used in the DC converter circuit according to one embodiment of the present invention is a transistor that is formed by removing impurities from an oxide semiconductor, particularly In order to improve the interface characteristics with the gate insulating layer, hydrogen and water must be removed as much as possible. This makes it possible to obtain a transistor that is stable even during BT testing.

[0243] The gate insulating layer 397 may be a silicon oxide layer, a silicon nitride layer, or a silicon oxynitride layer. A silicon nitride layer, a silicon oxide nitride layer, or an aluminum oxide layer is formed as a single layer or a stacked layer. can be done.

[0244] The gate insulating layer 397 is, for example, HfO x etc. can also be used. Gate HfO as insulating layer 397 x By using the above, the gate electrode can be formed from the oxide semiconductor layer side. Therefore, the leakage current flowing toward the

[0245] The gate insulating layer 397 is formed by laminating a silicon oxide layer and a silicon nitride layer. In this embodiment, as an example, a high density gas is generated at a pressure of 30 Pa and a microwave power of 6 kW. A silicon oxynitride layer with a thickness of 100 nm is formed by plasma CVD. The flow rate ratio of monosilane gas (SiH4) and nitrous oxide (N2O) introduced into the chamber is: The range is 1:10 to 1:200.

[0246] In addition, the gate insulating layer 397 and the oxide semiconductor film 393 contain hydrogen, a hydroxyl group, and moisture as much as possible. In order to prevent the gate electrode layer 391 from being mixed with the substrate, the substrate on which the gate electrode layer 391 is formed is treated as a pretreatment for the film formation. 394, or the substrate 394 on which the gate insulating layer 397 has been formed, is pre-insulated from the sputtering device. Preliminary heating in a preheating chamber removes impurities such as hydrogen and moisture adsorbed on the substrate 394, and exhausts the gas. The preheating temperature is preferably 100° C. or higher and 400° C. or lower. The temperature is 150° C. or more and 300° C. or less. In addition, the exhaust means provided in the preheating chamber may be, for example, A cryopump is preferable. This preheating process can be omitted. The preheating was performed before the formation of the oxide insulating layer and after the formation of the source electrode layer and the drain electrode layer. Substrate 394 may be treated similarly.

[0247] Next, an oxide semiconductor film 393 with a thickness of 2 nm to 200 nm is formed over the gate insulating layer 397. (See FIG. 11(A)).

[0248] Note that before the oxide semiconductor film 393 is formed, argon gas is introduced to generate plasma. The particles adhering to the surface of the gate insulating layer 397 are removed by reverse sputtering. It is preferable to remove it.

[0249] The oxide semiconductor film 393 is formed by, for example, a sputtering method. Examples include In-Sn-Ga-Zn-O films, which are quaternary metal oxides, and ternary metal oxides. In-Ga-Zn-O film, In-Sn-Zn-O film, In-Al-Zn-O film, S n-Ga-Zn-O film, Al-Ga-Zn-O film, Sn-Al-Zn-O film, and binary metal Metal oxide films such as In-Zn-O, Sn-Zn-O, Al-Zn-O, and Zn-Mg- O film, Sn-Mg-O film, In-Mg-O film, In-Sn-O film, In-O film, Sn- The oxide semiconductor film may be an oxide semiconductor film such as an O film or a Zn-O film. The film may contain SiO2.

[0250] The oxide semiconductor film 393 is InMO3(ZnO) m (m>0) Here, M is one or more selected from Ga, Al, Mn, and Co. indicates multiple metal elements. For example, M can be Ga, Ga and Al, Ga and Mn, or G Examples include a and Co.

[0251] In this embodiment, as an example, the oxide semiconductor film 393 is an In—Ga—Zn—O-based metal oxide film. The oxide semiconductor film 393 is formed by a sputtering method using an oxide target. , in a rare gas (typically argon) atmosphere, in an oxygen atmosphere, or in a rare gas (typically argon) atmosphere. The film can be formed by sputtering in an atmosphere of fluorine and oxygen. When using the sputtering method, the target contains 2% to 10% by weight of SiO2. The film may be formed using the following.

[0252] In addition, an oxide semiconductor film 393 was formed by a sputtering method using an oxide A target of a metal oxide mainly composed of zinc oxide can be used. Other examples of targets include metal oxide targets containing In, Ga, and Zn. The composition ratio is In2O3:Ga2O3:ZnO=1:1:1[mol%] or In:Ga Zn=1:1:0.5[atom%]) can be used. Metal oxide target The filling rate of the metal oxide target is 90% or more, preferably 95% or more. By using the above-mentioned oxide semiconductor film, the formed oxide semiconductor film becomes dense.

[0253] In this embodiment, as an example, the substrate is held in a processing chamber maintained in a reduced pressure state. The process is heated to room temperature or a temperature less than 400° C. Then, hydrogen is introduced into the process chamber while removing the remaining moisture in the process chamber. A sputtering gas from which moisture has been removed is introduced, and the substrate is sputtered using a metal oxide as a target. An oxide semiconductor film 393 is formed on the substrate 394. In order to remove residual moisture in the treatment chamber, It is preferable to use an adsorption type vacuum pump. It is preferable to use a lion pump, an ion pump, or a titanium sublimation pump. As the exhaust means, for example, a turbo pump equipped with a cold trap is used. The deposition chamber evacuated using a cryopump contains, for example, hydrogen atoms, water (H2 O) and other compounds containing hydrogen atoms (and more preferably compounds containing carbon atoms). Therefore, the concentration of impurities in the oxide semiconductor film is reduced by forming the oxide semiconductor film in the deposition chamber. The degree of oxidation can be reduced. In addition, the cryopump removes the moisture remaining in the processing chamber while the By performing the sputtering deposition, the substrate temperature during deposition of the oxide semiconductor film 393 is changed from room temperature to The heating temperature can be from 100°C to less than 400°C.

[0254] As an example of the deposition conditions, the distance between the substrate and the target is 60 mm, the pressure is 0.6 Pa, and the direct current ( The conditions are DC power supply 0.5kW and oxygen (oxygen flow rate 100%) atmosphere. In addition, by using a pulsed direct current (DC) power supply, particles can be reduced and the film thickness distribution becomes uniform. The thickness of the oxide semiconductor film is preferably from 5 nm to 30 nm. Note that the appropriate thickness of the oxide semiconductor film varies depending on the oxide semiconductor material to be used. The thickness may be appropriately selected depending on the material.

[0255] Next, the oxide semiconductor film is subjected to a second photolithography process to form an island-shaped oxide semiconductor layer 39. 9 (see FIG. 11B). The resist mask may be formed by an ink-jet method. Forming it by the PET method can reduce manufacturing costs.

[0256] In addition, when a contact hole is formed in the gate insulating layer 397, the process is performed using an oxide semiconductor This can be done when layer 399 is formed.

[0257] Note that the etching of the oxide semiconductor film 393 here is performed by dry etching or wafer etching. The oxide semiconductor film 393 can be etched by hot etching. In the case of the etching, both dry etching and wet etching may be used.

[0258] The etching gas used in dry etching is a gas containing chlorine (chlorine-based gas, e.g. For example, chlorine (Cl2), boron chloride (BCl3), silicon chloride (SiCl4), carbon tetrachloride (CC l4) etc.) are preferred.

[0259] In addition, the etching gas used in dry etching is a gas containing fluorine (fluorine-based Gases, such as carbon tetrafluoride (CF4), sulfur hexafluoride (SF6), nitrogen trifluoride (NF3), trifluoromethane (CHF3), hydrogen bromide (HBr), or oxygen (O2), These gases are mixed with rare gases such as helium (He) and argon (Ar). can be used.

[0260] As a dry etching method, parallel plate type RIE (Reactive Ion Etch) ing method and ICP (Inductively Coupled Plasma) A combined plasma etching method can be used. It is possible to etch into the desired shape. The etching conditions (the amount of power applied to the coil-type electrode, the amount of power applied to the electrode on the substrate side) were set so that The amount of power used, the temperature of the electrode on the substrate, etc. are adjusted appropriately.

[0261] The etching solution used for wet etching is, for example, a mixture of phosphoric acid, acetic acid, and nitric acid. Alternatively, ITO07N (manufactured by Kanto Chemical Co., Ltd.) may be used.

[0262] In addition, the etching solution after wet etching is washed away together with the etched material. The waste etching solution containing the removed material is purified to remove the contained material. The indium and other components contained in the oxide semiconductor layer may be recycled from the waste liquid after the etching. By recovering and reusing materials, we can make effective use of resources and reduce costs. do.

[0263] In addition, during etching, the material is adjusted to the desired shape. The etching conditions (etching solution, etching time, temperature, etc.) are adjusted appropriately.

[0264] In this embodiment, reverse sputtering is performed before forming a conductive film in the next step, and oxidation is performed. Resist residues and the like adhering to the surfaces of the compound semiconductor layer 399 and the gate insulating layer 397 are removed. It is preferable to do so.

[0265] Next, a conductive film is formed over the gate insulating layer 397 and the oxide semiconductor layer 399. The conductive film can be formed by sputtering or vacuum deposition. An element selected from the group consisting of aluminum, chromium, copper, tantalum, titanium, molybdenum, and tungsten, Alternatively, an alloy film containing the above elements or an alloy film containing a combination of the above elements may be used. The conductive film may be made of manganese, magnesium, zirconium, or the like. Alternatively, a material selected from one or more of the following may be used: SiO 2 , beryllium, and yttrium. The conductive film may have a single layer structure or a stacked structure of two or more layers. For example, a single layer structure of an aluminum film containing silicon can be used. The structure is a two-layer structure in which a titanium film is laminated on an aluminum film, or a Ti film and a Examples include a three-layer structure in which an aluminum film is laminated on top of the aluminum film and a Ti film is then formed on top of that. In addition, titanium, tantalum, tungsten, molybdenum, chromium, nickel, A film made of a single or a combination of elements selected from the group consisting of ZnO, ZnO, and Scandium, or an alloy film in which a plurality of elements are combined, or a nitride film in which a single element or a plurality of elements are combined It may be used.

[0266] Next, a resist mask is formed on the conductive film by a third photolithography process. After etching the source electrode layer 395a and the drain electrode layer 395b, Remove the dysplasia mask (see Figure 11(C)).

[0267] In the third photolithography process, ultraviolet light or KrF laser is used for exposure when forming the resist mask. The source electrode layers adjacent to each other on the oxide semiconductor layer 399 are exposed to the laser beam or the ArF laser beam. The width of the gap between the end of the drain electrode layer and the bottom end of the drain electrode layer determines the channel width of the transistor to be formed later. When performing exposure with a channel length L of less than 25 nm, the channel length L is determined by the channel length L. Extreme ultraviolet rays have extremely short wavelengths of up to several tens of nanometers. The third photolithography process uses ultraviolet light to form a resist mask. Line exposure has high resolution and a large depth of focus. It is also possible to set the channel length L to 10 nm or more and 1000 nm or less, and the operating speed of the circuit is The off-current value can be made extremely small, which also contributes to low power consumption. can be done.

[0268] Note that the conductive film is etched so that the oxide semiconductor layer 399 is not removed. The materials and etching conditions of the oxide semiconductor film and the oxide semiconductor film are adjusted as appropriate.

[0269] In this embodiment, for example, a titanium film is used as the conductive film and the oxide semiconductor layer 399 is An In-Ga-Zn-O oxide semiconductor layer was used as the etchant, and ammonia hydrogen peroxide was used as the etchant. Uses water (a mixture of ammonia, water, and hydrogen peroxide).

[0270] Note that in the third photolithography step, part of the oxide semiconductor layer 399 is etched. In some cases, the oxide semiconductor layer 399 may have a groove (a recess). A resist mask for forming the drain electrode layer 395a and the drain electrode layer 395b is formed by an inkjet method. If the resist mask is formed by an ink-jet method, the manufacturing cost can be reduced. Cut.

[0271] In order to reduce the number of photomasks and steps used in the photolithography process, The resist pattern is formed by a multi-tone mask, which is an exposure mask that allows the light to be projected at multiple intensities. The etching process may be performed using a resist mask formed using a multi-tone mask. The mask has a shape with multiple film thicknesses, and the shape can be further deformed by etching. This allows for multiple etching processes to be performed to create different patterns. Therefore, one multi-tone mask can handle at least two different patterns. Therefore, the number of exposure masks can be reduced. Since the corresponding photolithography process can also be eliminated, the process can be simplified.

[0272] Plasma treatment with gases such as N2O, N2, or Ar removes the exposed oxide semiconductor. Water adsorbed on the surface of the conductor layer may be removed. A mixed gas of oxygen and argon may also be used. The plasma treatment may be carried out using

[0273] When plasma treatment is performed, the protective layer in contact with a part of the oxide semiconductor layer is not exposed to the air. An oxide insulating layer 396 is formed as an oxide insulating layer to be an insulating layer (see FIG. 11D). In this embodiment, the oxide semiconductor layer 399 is a source electrode layer 395a and a drain electrode layer 39 In a region not overlapping with 5b, the oxide semiconductor layer 399 and the oxide insulating layer 396 are in contact with each other. It is formed as follows.

[0274] In this embodiment, the oxide insulating layer 396 includes an island-shaped oxide semiconductor layer 399 and a source The substrate 394 on which the electrode layer 395a and the drain electrode layer 395b have been formed is heated at room temperature or below 100° C. The gas is heated to a temperature of 1000° C., hydrogen and moisture are removed, and a high-purity sputtering gas containing oxygen is introduced. A silicon oxide layer containing defects is formed using a silicon semiconductor target.

[0275] In this embodiment, for example, a silicon target having a purity of 6N and doped with boron is used. The distance between the substrate and the target (TS distance) was set to 89 m. m, pressure 0.4 Pa, direct current (DC) power supply 6 kW, oxygen (oxygen flow rate 100%) atmosphere A silicon oxide film is formed by pulse DC sputtering. The thickness is set to 300 nm. In addition, a silicon oxide film is formed instead of a silicon target. Quartz (preferably synthetic quartz) can be used as a target for sputtering. The deposition gas used is, for example, oxygen or a mixed gas of oxygen and argon.

[0276] When the oxide insulating layer 396 is formed using any of the above materials and methods, the process It is preferable to form the oxide insulating layer 396 while removing residual moisture in the chamber. In order to prevent hydrogen, hydroxyl groups, or moisture from being contained in the oxide insulating layer 399 and the oxide insulating layer 396, It is.

[0277] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. Also, as the exhaust means, a turbo pump with a coupling is used. The deposition chamber is evacuated using a cryopump. The chamber is evacuated, for example, of hydrogen atoms and compounds containing hydrogen atoms (such as water), By forming the oxide insulating layer 396 in the deposition chamber, the impurity concentration in the oxide insulating layer 396 can be reduced. do.

[0278] Note that, as the oxide insulating layer 396, a silicon oxynitride layer or an oxide An aluminum layer, an aluminum oxynitride layer, or the like can also be used.

[0279] Further, the oxide insulating layer 396 and the oxide semiconductor layer 399 are heated at 100° C. to 40° C. in a state where the oxide insulating layer 396 and the oxide semiconductor layer 399 are in contact with each other. Heat treatment may be performed at 0° C. The oxide insulating layer 396 in this embodiment has many defects. Therefore, hydrogen, moisture, and hydroxyl groups contained in the oxide semiconductor layer 399 are removed by this heat treatment. Alternatively, impurities such as hydride are diffused into the oxide insulating layer 396, and then the oxide semiconductor layer 399 is The amount of the impurities contained can be further reduced.

[0280] Through the above steps, the oxide semiconductor layer 39 in which the concentrations of hydrogen, moisture, hydroxyl groups, or hydrides are reduced is formed. A transistor 390 having a first conductivity type and a second conductivity type can be formed (see FIG. 11E).

[0281] When the oxide semiconductor film is formed as described above, moisture remaining in the atmosphere during the film formation is removed. As a result, the concentrations of hydrogen and hydride in the oxide semiconductor film can be reduced. The oxide semiconductor film can be further stabilized.

[0282] Note that a protective insulating layer may be provided over the oxide insulating layer. In this embodiment, the protective insulating layer 39 8 is formed on the oxide insulating layer 396. The protective insulating layer 398 may be a silicon nitride film, a nitride A silicon oxide film, an aluminum nitride film, an aluminum nitride oxide film, or the like is used.

[0283] In this embodiment, as an example, the substrate 394 on which the oxide insulating layer 396 is formed is It is heated to a temperature of ℃ ~ 400 ℃, and hydrogen and moisture are removed, and it is a high-purity sputtering By introducing a silicon nitride gas and using a silicon semiconductor target, In this case, similarly to the oxide insulating layer 396, The protective insulating layer 398 is preferably formed while removing moisture remaining in the treatment chamber.

[0284] When the protective insulating layer 398 is formed, the protective insulating layer 398 is formed at a temperature of 100° C. to 400° C. The plate 394 is heated to oxidize hydrogen or moisture contained in the oxide semiconductor layer 399. In this case, after the oxide insulating layer 396 is formed, In addition, no heat treatment is required.

[0285] In addition, a silicon oxide layer is formed as the oxide insulating layer 396, and a nitride layer is formed as the protective insulating layer 398. When stacking silicon layers, the silicon oxide layer and the silicon nitride layer are simultaneously processed in the same processing chamber. The sputtering process can be performed by using a silicon target that contains oxygen. Gas is introduced to form a silicon oxide layer using a silicon target mounted in the processing chamber. Then, the sputtering gas was switched to a nitrogen-containing sputtering gas and the same silicon A silicon nitride layer is formed using a silicon oxide target. Since it can be formed continuously without exposure to the atmosphere, hydrogen and moisture are not present on the silicon oxide layer surface. In this case, the oxide insulating layer 396 can be made of oxide. After forming a silicon layer and laminating a silicon nitride layer as a protective insulating layer 398, an oxide semiconductor A heat treatment ( The heating temperature is preferably 100°C to 400°C.

[0286] In addition, when an oxide semiconductor layer having a channel formation region is formed over a gate insulating layer, The residual moisture in the air is removed to reduce the concentrations of hydrogen and hydride in the oxide semiconductor layer. It is possible.

[0287] The above process is carried out at temperatures below 400℃, so the thickness is less than 1mm and the length is 1m on each side. It can also be applied to manufacturing processes that use glass substrates at temperatures above 400°C. All steps can be carried out at processing temperature.

[0288] Furthermore, the conduction mechanism of a transistor using an oxide semiconductor will be described with reference to FIGS. In the following explanation, an ideal situation is assumed for ease of understanding. Not all of them necessarily reflect the real world. Also, the following explanation is only a rough guide. Please note that this is merely speculation.

[0289] FIG 12 is a longitudinal cross-sectional view of an inverted staggered transistor including an oxide semiconductor. An oxide semiconductor layer 1003 is provided on a gate insulating film 1002. A source electrode 1004a and a drain electrode 1004b are provided on the source electrode 1004a. An oxide insulating layer 1005 is provided on the drain electrode 1004b, and the oxide insulating layer 10 A conductive layer 1006 is provided over the oxide semiconductor layer 1003 with the insulating film 1005 sandwiched therebetween.

[0290] FIG. 13 shows an energy band diagram (schematic diagram) in the A-A' cross section shown in FIG. 13(A) shows the case where the voltage between the source and drain is equipotential (Vd = 0 V), and Fig. 13(B) applies a positive potential (Vd>0) to the drain relative to the source, and a positive potential to the gate This shows the case where (Vg>0) is added.

[0291] FIG. 14 is an energy band diagram (schematic diagram) in the cross section taken along line B-B' in FIG. FIG. 14(A) shows a state in which a positive potential (+Vg) is applied to the gate (G1), and the source The figure shows the on-state where carriers (electrons) flow between the gate and drain. is the state in which a negative potential (-Vg) is applied to the gate (G1), and the transistor is in the off state (minority capacitance This shows the case where the rear does not flow.

[0292] Figure 15 shows the relationship between the vacuum level, the work function of a metal (φM), and the electron affinity of an oxide semiconductor (χ). Shows.

[0293] Since metals are degenerate, the Fermi level is located in the conduction band. The body is generally N-type, in which case the Fermi level (Ef) is located in the middle of the band gap. The Fermi level (Ei) is located closer to the conduction band than the intrinsic Fermi level (Ei). In the case of a conductor, although it depends on the deposition method, the oxide semiconductor layer contains a small amount of hydrogen or water. It is known that some of these electrons act as donors, which is one of the reasons for the n-type structure. It is being done.

[0294] In contrast, the oxide semiconductor used in the transistor of the DC converter circuit of one embodiment of the present invention is The N-type impurity hydrogen is removed from the oxide semiconductor, and impurities other than the main components of the oxide semiconductor are removed. By purifying the material to the extent possible, it is possible to obtain an intrinsic (I type) or substantially intrinsic semiconductor. In other words, instead of adding impurities to create I-type, hydrogen, water, etc. By removing impurities as much as possible, it is a highly purified I-type (intrinsic semiconductor) or close to it. This makes the Fermi level equal to the intrinsic Fermi level. It can be up to.

[0295] When the band gap (Eg) of an oxide semiconductor is 3.15 eV, the electron affinity (χ) is The specification of titanium (Ti) that constitutes the source and drain electrodes is 4.3 eV. The electron affinity function is approximately equal to the electron affinity of the oxide semiconductor. In this case, the metal-oxide semiconductor interface In this case, no Schottky barrier is formed for electrons.

[0296] In other words, when the work function of a metal and the electron affinity of an oxide semiconductor are equal, An energy band diagram (schematic diagram) as shown in FIG. 13(A) is shown.

[0297] In FIG. 13(B), the black circles (●) represent electrons. When a positive potential is applied to the drain, Electrons cross the barrier (h) and are injected into the oxide semiconductor, where they flow toward the drain. In the case of a positive drain, the barrier height (h) changes depending on the gate voltage and the drain voltage. When a rain voltage is applied, the barrier height in FIG. 13(A) without voltage application, i.e. In other words, the barrier height (h) is smaller than half the band gap (Eg).

[0298] At this time, the electrons pass through the gate insulating film and the highly purified oxide semiconductor as shown in FIG. The electrons move through the lowest energetically stable portion on the oxide semiconductor side at the interface with the body.

[0299] In FIG. 14B, a negative potential (reverse bias) is applied to the gate electrode 1001. Since the number of holes, which are minority carriers, is essentially zero, the current is close to zero. value.

[0300] For example, if the channel width W of a transistor is 1×10 4 The device has a channel length of 3 μm. However, the off-state current is -13 A or less, and the subthreshold swing value (S value) is 0.1V / dec. (gate insulating film thickness 100nm).

[0301] Thus, simply applying oxide semiconductors with a wide band gap to transistors In addition, impurities such as hydrogen that form donors are reduced as much as possible, and the carrier density is preferably 1 ×10 12 / cm 3 less than 1.45×10 10 / cm 3 Less than By doing so, thermally excited carriers can be eliminated at practical operating temperatures, and the The transistor can be operated only by the injected carriers. Off current 1×10 -13 A or less, and the off-state current is almost It is possible to obtain a transistor that operates extremely stably with almost no change.

[0302] As described above, a transistor including an oxide semiconductor layer has stable electrical characteristics. It is possible to provide a highly reliable transistor.

[0303] This embodiment mode can be appropriately combined with or replaced by other embodiment modes. do.

[0304] (Embodiment 7) This embodiment can be applied to a transistor included in a DC converter circuit according to one embodiment of the present invention. An example of such a transistor will be described.

[0305] An example of a transistor and a manufacturing method of the transistor of this embodiment will be described with reference to FIGS. explain.

[0306] An example of a method for manufacturing a transistor is shown in FIGS. The transistor shown in Fig. 1 has a bottom-gate structure and is also called an inverted staggered transistor. cormorant.

[0307] In addition, the transistor 310 has a single gate structure. The transistor is a multi-gate transistor having a plurality of channel formation regions. This is also fine.

[0308] Hereinafter, a process for fabricating a transistor 310 on a substrate 300 will be described with reference to FIGS. Explain the process.

[0309] First, a conductive film is formed on a substrate 300 having an insulating surface, and then a first photolithography process is performed. A gate electrode layer 311 is formed by a process. If the resist mask is formed by an inkjet method, the manufacturing cost can be reduced. do.

[0310] There is no significant limitation on the substrate that can be used for the substrate 300 having an insulating surface. In both cases, the substrate 3 must have sufficient heat resistance to withstand the heat treatment. 00 includes glass substrates such as barium borosilicate glass and aluminoborosilicate glass. can be used.

[0311] Instead of the above glass substrate, an insulating substrate such as a ceramic substrate, a quartz substrate, or a sapphire substrate may be used. A substrate made of an insulating material may be used. Alternatively, a substrate made of crystallized glass may be used. The substrate may be a semiconductor substrate such as silicon.

[0312] An insulating film serving as a base film may be provided between the substrate 300 and the gate electrode layer 311. , which has the function of preventing the diffusion of impurity elements from the substrate 300. A laminate structure of one or more films selected from a silicon nitride oxide film or a silicon oxynitride film. It can be formed.

[0313] The gate electrode layer 311 may be made of any of molybdenum, titanium, chromium, tantalum, tungsten, Metallic materials such as aluminum, copper, neodymium, and scandium, or alloys containing these as their main components The gold material can be used to form a single layer or a multilayer structure.

[0314] For example, the gate electrode layer 311 may have a two-layer laminate structure of molybdenum on an aluminum layer. Two-layer laminate structure with a molybdenum layer on a copper layer, two-layer laminate structure with a molybdenum layer on a copper layer, A two-layer laminate structure with a titanium nitride layer or tantalum nitride layer laminated on top, a titanium nitride layer and a tantalum nitride layer A two-layer structure consisting of a tungsten nitride layer and a tungsten layer, or a tungsten nitride layer and a tungsten layer A two-layer laminate structure is preferable. A three-layer laminate structure is preferably a tungsten layer or a nitride layer. a tungsten nitride layer, an aluminum-silicon alloy layer or an aluminum-titanium alloy layer, It is preferable to form a laminate having a titanium nitride layer and a titanium layer.

[0315] Next, the gate insulating layer 302 is formed on the gate electrode layer 311 .

[0316] Here, the oxide semiconductor (high-temperature oxide semiconductor) that has been made i-type or substantially i-type by removing impurities is Since the gate oxide semiconductor (a purified oxide semiconductor) is extremely sensitive to the interface state and the interface charge, The interface between the gate insulating layer and the highly purified oxide semiconductor layer is important. The insulating layer (GI) is required to be of high quality.

[0317] For example, high-density plasma CVD using microwaves (2.45 GHz) produces dense, high-insulation-voltage It is preferable that a highly purified oxide semiconductor layer and a high-quality insulating film can be formed. By closely contacting the gate insulating layer, the interface state can be reduced and the interface characteristics can be improved. The high-density plasma device used here is 1×10 11 / cm 3 Any device capable of achieving the above plasma density can be used.

[0318] For example, a microwave power of 3kW to 6kW is applied to generate plasma, and the formation of an insulating film is performed. The chamber is filled with monosilane gas (SiH4) and nitrous oxide (N2 O) and rare gas are introduced to generate high-density plasma at a pressure of 10 Pa to 30 Pa. An insulating film is formed on a substrate having an insulating surface such as a silicon wafer. Then, the supply of monosilane gas is stopped. Nitrous oxide (N2O) and rare gases are introduced without exposing the insulating film to the atmosphere. Plasma treatment may be performed. At least nitrous oxide (N2O) and rare gases are introduced to provide insulation. The plasma treatment on the film surface is performed after the formation of the insulating film. The flow ratio of nitrous oxide gas (N2O) to silane gas (SiH4) is 1:10 to 1:20. The rare gas introduced into the chamber is helium, argon, chlorine, etc. Lipton, xenon, etc. can be used, but argon is the most inexpensive. is preferred.

[0319] Of course, if a good insulating film can be formed as the gate insulating layer 302, sputtering is also possible. Other film formation methods such as the ring method and plasma CVD method can be applied. The quality of the gate insulating film and the interface characteristics with the oxide semiconductor are improved by heat treatment. In any case, it goes without saying that the quality of the film as a gate insulating film is good. Any material may be used as long as it can reduce the interface state density with the oxide semiconductor and form a good interface.

[0320] Furthermore, at 85°C, 2 × 10 6 V / cm, 12-hour gate bias and thermal stress test (B In the T test, when impurities are added to an oxide semiconductor, The bonds between the main component of are broken by a strong electric field (B: bias) and high temperature (T: temperature), The resulting dangling bonds induce a drift in the threshold voltage (Vth). The transistor used in the DC converter circuit of one embodiment of the present invention is an oxide semiconductor transistor. Impurities, especially hydrogen and water, are removed as much as possible to improve the interface characteristics with the gate insulating layer as described above. By doing so, it is possible to obtain a transistor that is stable even in BT tests. .

[0321] The gate insulating layer 302 may be a silicon oxide layer, a silicon nitride layer, or a silicon oxynitride layer. A silicon nitride layer, a silicon oxide nitride layer, or an aluminum oxide layer is formed as a single layer or a stacked layer. can be done.

[0322] The gate insulating layer 302 is, for example, HfO x etc. can also be used. Gate Insulating layer 302: HfO x By using the above, the gate electrode can be formed from the oxide semiconductor layer side. Therefore, the leakage current flowing toward the

[0323] The gate insulating layer 302 is formed by laminating a silicon oxide layer and a silicon nitride layer. In this embodiment, as an example, a high density gas is generated at a pressure of 30 Pa and a microwave power of 6 kW. A silicon oxynitride layer with a thickness of 100 nm is formed by plasma CVD. The flow rate ratio of monosilane gas (SiH4) and nitrous oxide (N2O) introduced into the chamber is: The range is 1:10 to 1:200.

[0324] Next, an oxide semiconductor film 330 having a thickness of 2 nm to 200 nm is formed on the gate insulating layer 302. Form.

[0325] Before the oxide semiconductor film 330 is formed by a sputtering method, argon gas is introduced. The reverse sputtering is performed by introducing the metal into the gate insulating layer 302 to generate plasma, and the metal is deposited on the surface of the gate insulating layer 302. It is preferable to remove particles that may be present in the argon atmosphere. Alternatively, oxygen or the like may be used.

[0326] The oxide semiconductor film 330 is a quaternary metal oxide film, In-Sn-Ga-Zn-O film. and ternary metal oxide films such as In-Ga-Zn-O, In-Sn-Zn-O, and In- Al-Zn-O film, Sn-Ga-Zn-O film, Al-Ga-Zn-O film, Sn-Al-Z In-Zn-O films, Sn-Zn-O films, and Al-Zn -O film, Zn-Mg-O film, Sn-Mg-O film, In-Mg-O film, In-Sn-O film, In addition, an oxide semiconductor film such as an In—O film, an Sn—O film, or a Zn—O film can be used. In addition, the oxide semiconductor film may contain SiO2.

[0327] The oxide semiconductor film 330 is InMO3(ZnO) m (m>0) Here, M is one or more selected from Ga, Al, Mn, and Co. indicates multiple metal elements. For example, M can be Ga, Ga and Al, Ga and Mn, or G Examples include a and Co.

[0328] In addition, an oxide semiconductor film 330 was formed by sputtering using an oxide A target of a metal oxide mainly composed of zinc oxide can be used. Other examples of targets include metal oxide targets containing In, Ga, and Zn. The composition ratio is In2O3:Ga2O3:ZnO=1:1:1[mol%] or In:Ga Zn=1:1:0.5[atom%]) can be used. In, Ga, and As a metal oxide target containing In and Zn, In:Ga:Zn=1:1:1 [atom% ], or a target having a composition ratio of In:Ga:Zn=1:1:2 [atom%] was used. The filling rate of the metal oxide target is 90% or more, preferably 95% or more. By using a metal oxide target with a high filling rate, the oxide semiconductor film formed The film becomes a dense film.

[0329] The sputtering gas used in forming the oxide semiconductor film 330 is hydrogen, water, or water. High purity, with impurities such as acid groups or hydrides removed to concentrations of ppm or ppb. It is preferable to use a high-temperature gas.

[0330] The substrate is held in a processing chamber maintained in a reduced pressure state, and the substrate temperature is preferably maintained at 100° C. or more and 600° C. or less. The temperature is preferably 200° C. or higher and 400° C. or lower. In addition, the concentration of impurities in the oxide semiconductor film can be reduced. Damage caused by etching is reduced. In addition, hydrogen and moisture are removed while removing residual moisture in the processing chamber. The removed sputtering gas is introduced, and metal oxide is used as a target to deposit on the substrate 300. The oxide semiconductor film 330 is formed. In order to remove the residual moisture in the processing chamber, an adsorption type evaporator is used. It is preferable to use an air pump. As an adsorption type vacuum pump, for example, a cryopump is used. It is preferable to use an ion pump or a titanium sublimation pump. The stage may be, for example, a turbo pump equipped with a cold trap. The deposition chamber evacuated using a cryopump contains hydrogen atoms, water (H2O), and other hydrogen gases. Because compounds containing atoms (and more preferably compounds containing carbon atoms) are exhausted By forming the oxide semiconductor film in the deposition chamber, the concentration of impurities in the oxide semiconductor film can be reduced. .

[0331] An example of the deposition conditions is as follows: the distance between the substrate and the target is 100 mm, the pressure is 0.6 Pa, and the direct current is The conditions are: DC power supply 0.5 kW, oxygen (oxygen flow rate 100%) atmosphere. In addition, if a pulsed direct current (DC) power supply is used, particles can be reduced and the film thickness distribution becomes uniform. The thickness of the oxide semiconductor film is preferably from 5 nm to 30 nm. Note that the appropriate thickness of the oxide semiconductor film varies depending on the oxide semiconductor material used. The thickness can be appropriately selected depending on the material.

[0332] Next, the oxide semiconductor film 330 is subjected to a second photolithography process to form an island-shaped oxide semiconductor In addition, a resist mask for forming an island-shaped oxide semiconductor layer is formed by ink jet printing. The resist mask may be formed by an inkjet method. can be reduced.

[0333] Next, the oxide semiconductor layer is subjected to a first heat treatment. The temperature of the first heat treatment is 400° C. or higher. The temperature is set to 750° C. or lower, preferably 400° C. or higher but lower than the distortion point of the substrate. The substrate is placed in an electric furnace, which is a type of heat treatment device, and the oxide semiconductor layer is heated under a nitrogen atmosphere. After heat treatment at 450℃ for 1 hour, the oxide semiconductor was The intrusion of water and hydrogen into the oxide layer is prevented, and an oxide semiconductor layer 331 is obtained (see FIG. 16(B)).

[0334] When the heat treatment apparatus is cooled from the heat treatment temperature, the atmosphere may be changed to oxygen. When the temperature is decreased, the atmosphere is switched to oxygen, and oxygen is replenished to the oxygen vacancies in the oxide semiconductor layer. Oxygen vacancies generate carriers, but their disappearance significantly reduces the number of carriers. Thus, an oxide semiconductor layer having an extremely low carrier concentration can be obtained.

[0335] The heat treatment device is not limited to an electric furnace, and may be a heat treatment device using heat conduction or heat radiation from a heating element such as a resistance heating element. The apparatus may be equipped with a device for heating the object to be treated by irradiation. For example, a GRTA device, a LR device, etc. The RTA device can be used with a halogen lamp, a meter, or a similar device. Tal halide lamps, xenon arc lamps, carbon arc lamps, high pressure sodium lamps The material to be treated is heated by the radiation of light (electromagnetic waves) emitted from lamps such as high-pressure mercury lamps. The GRTA device is a device that uses high-temperature gas for heat treatment. The body contains rare gases such as argon or nitrogen that react with the material being treated by heat treatment. An inert gas that is not harmful to the environment is used.

[0336] For example, the first heat treatment is performed by subjecting the substrate to a base in an inert gas heated to a high temperature of 650° C. to 700° C. The plate is moved and heated for several minutes, after which the substrate is moved and taken out of the inert gas heated to a high temperature. Using the GRTA, high-temperature heat treatment can be performed in a short time.

[0337] In the first heat treatment, nitrogen or a rare gas such as helium, neon, or argon is used. It is preferable that the nitrogen introduced into the heat treatment device does not contain water, hydrogen, etc. The purity of rare gases such as helium, neon, and argon is 6N (99.9999%) or higher. Preferably, the concentration of impurities is 7N (99.99999%) or more (i.e., the impurity concentration is 1 ppm or less, It is preferable to keep the concentration of the EDTA concentration at 0.1 ppm or less.

[0338] In addition, the first heat treatment of the oxide semiconductor layer is performed on the oxide semiconductor layer before it is processed into the island-shaped oxide semiconductor layer. The semiconductor film 330 may be subjected to the first heat treatment. In that case, the semiconductor film 330 may be heated by the heating device after the first heat treatment. The substrate is taken out and a photolithography process is performed.

[0339] The heat treatment for dehydrating and dehydrogenating the oxide semiconductor layer is performed in the oxide semiconductor layer formation. After that, a source electrode layer and a drain electrode layer are stacked on the oxide semiconductor layer, and then a source electrode The deposition may be performed either after a protective insulating layer is formed over the drain electrode layer or after a protective insulating layer is formed over the drain electrode layer.

[0340] In addition, when a contact hole is formed in the gate insulating layer 302, the process is performed using an oxide semiconductor. This may be done before or after membrane 330 is subjected to a dehydration or dehydrogenation treatment.

[0341] Note that the etching of the oxide semiconductor film here is not limited to wet etching and may be dry etching. Etching may also be used.

[0342] In order to etch the desired shape, the etching conditions (etching Adjust the etching conditions (liquid, etching time, temperature, etc.) as appropriate.

[0343] Next, a conductive film is formed over the gate insulating layer 302 and the oxide semiconductor layer 331. For example, The conductive film may be formed by sputtering or vacuum deposition. An element selected from the group consisting of aluminum, chromium, copper, tantalum, titanium, molybdenum, and tungsten. Alternatively, alloys containing the above elements or alloy films made of a combination of the above elements may be used. The conductive film is made of manganese, magnesium, zirconium, beryllium, etc. Alternatively, a material selected from one or more of the following may be used. The conductive film may have a single layer structure or a laminated structure of two or more layers. A single layer structure of an aluminum film containing silicon can be used. A two-layer structure in which a titanium film is laminated on an aluminum film, and a Ti film and an aluminum film are laminated on the Ti film. Examples include a three-layer structure in which an aluminum film is laminated and a Ti film is further formed on top of that. Minium, titanium, tantalum, tungsten, molybdenum, chromium, neodymium, scandium A film made of a single or multiple combinations of elements selected from the group consisting of tin, nickel, and tin, an alloy film, or a nitride film is used. It's fine.

[0344] When a heat treatment is performed after the conductive film is formed, the conductive film must have heat resistance to withstand the heat treatment. It is preferable that

[0345] A resist mask is formed on the conductive film by a third photolithography process, and selective etching is performed. After forming the source electrode layer 315a and the drain electrode layer 315b by etching, a resist The mask is removed (see FIG. 16(C)).

[0346] In the third photolithography process, ultraviolet light or KrF laser is used for exposure when forming the resist mask. The source electrode layers adjacent to each other on the oxide semiconductor layer 331 are exposed to the ion beam. The width of the gap between the end of the drain electrode layer and the bottom end of the drain electrode layer determines the channel width of the transistor to be formed later. When performing exposure with a channel length L of less than 25 nm, the channel length L is determined by the channel length L. Extreme ultraviolet rays have extremely short wavelengths of up to several tens of nanometers. The third photolithography process uses ultraviolet light to form a resist mask. Line exposure has high resolution and a large depth of focus. It is also possible to set the channel length L to 10 nm or more and 1000 nm or less, and the operating speed of the circuit is The off-current value can be made extremely small, which also contributes to low power consumption. can be done.

[0347] Note that in order to prevent the oxide semiconductor layer 331 from being removed during etching of the conductive film, The materials and etching conditions of the oxide semiconductor film and the oxide semiconductor film are adjusted as appropriate.

[0348] In this embodiment, for example, a titanium film is used as the conductive film, and the oxide semiconductor layer 331 is An In-Ga-Zn-O oxide semiconductor layer was used as the etchant, and ammonia hydrogen peroxide was used as the etchant. Uses water (a mixture of ammonia, water, and hydrogen peroxide).

[0349] Note that in the third photolithography step, part of the oxide semiconductor layer 331 is etched. In some cases, the source electrode layer 315 may have a groove (a recess). a) A resist mask for forming the drain electrode layer 315b is formed by an inkjet method. If the resist mask is formed by an ink-jet method, the manufacturing cost can be reduced.

[0350] Further, an oxide conductive layer is formed between the oxide semiconductor layer and the source electrode layer and the drain electrode layer. The oxide conductive layer and the metal layer for forming the source and drain electrode layers may be The oxide conductive layer can function as a source region and a drain region.

[0351] The oxide conductive layer is formed as a source region and a drain region, and the oxide semiconductor layer is formed as a source electrode layer and a drain region. By providing the source region and the drain electrode layer, the resistance of the source region and the drain region can be reduced. This makes it possible to achieve high speed operation of the transistor.

[0352] In order to reduce the number of photomasks and steps used in the photolithography process, The resist pattern is formed by a multi-tone mask, which is an exposure mask that allows the light to be projected at multiple intensities. The etching process may be performed using a resist mask formed using a multi-tone mask. The mask has a shape with multiple film thicknesses, and the shape can be further deformed by etching. This allows for multiple etching processes to be performed to create different patterns. Therefore, one multi-tone mask can handle at least two different patterns. Therefore, the number of exposure masks can be reduced. Since the corresponding photolithography process can also be eliminated, the process can be simplified.

[0353] Next, a plasma treatment is performed using a gas such as N2O, N2, or Ar. Water adsorbed on the surface of the oxide semiconductor layer exposed by the treatment is removed. The plasma treatment may be performed using a mixed gas of oxygen and argon.

[0354] After the plasma treatment, the protective insulating film in contact with a part of the oxide semiconductor layer is removed without being exposed to the air. An oxide insulating layer 316 is formed to serve as an insulating film.

[0355] The oxide insulating layer 316 has a thickness of at least 1 nm and is formed by an oxide method such as a sputtering method. The insulating layer 316 can be formed by using a method that does not allow impurities such as water and hydrogen to be mixed in. When hydrogen is contained in the oxide insulating layer 316, the hydrogen penetrates into the oxide semiconductor layer, Alternatively, oxygen in the oxide semiconductor layer is extracted by hydrogen, and the backchannel of the oxide semiconductor layer is formed. The resistance of the panel becomes low (N-type), and a parasitic channel may be formed. In order to form the oxide insulating layer 316 as a film containing as little hydrogen as possible, hydrogen is not used in the deposition method. It is important that there is no

[0356] In this embodiment, as an example, a silicon oxide film having a thickness of 200 nm is used as the oxide insulating layer 316. The substrate temperature during film formation is set to room temperature or higher and 300°C or lower. In this embodiment, the temperature is set to 100° C. Formation of a silicon oxide film by sputtering The method is carried out under a rare gas (typically argon) atmosphere, an oxygen atmosphere, or a rare gas (typically argon) atmosphere. The reaction can be carried out in an atmosphere of argon and oxygen. For example, a silicon target can be used. A silicon oxide film can be formed by sputtering in an atmosphere of oxygen and nitrogen. The oxide semiconductor layer is in an oxygen-deficient state and has low resistance, i.e., is N-type. The insulating layer 316 is resistant to moisture, hydrogen ions, and OH - It does not contain impurities such as An inorganic insulating film that blocks the intrusion of silicon is used, typically a silicon oxide film or a silicon oxynitride film. A film made of aluminum, an aluminum oxide film, an aluminum oxynitride film, or the like is used.

[0357] In this case, the oxide insulating layer 316 is formed while removing residual moisture in the processing chamber. It is preferable that the oxide semiconductor layer 331 and the oxide insulating layer 316 contain hydrogen, a hydroxyl group, or moisture. This is to prevent it from being swallowed up.

[0358] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, of hydrogen atoms and compounds containing hydrogen atoms (such as water), By forming the oxide insulating layer 316 in the deposition chamber, the impurity concentration in the oxide insulating layer 316 can be reduced. do.

[0359] The sputtering gas used in forming the oxide insulating layer 316 is hydrogen, water, hydroxide, or the like. High purity, with impurities such as bases or hydrides removed to concentrations of about ppm or ppb. It is preferable to use a gas.

[0360] Next, a second heat treatment (preferably 200 ℃ or higher and 400 ℃ or lower, for example, 250 ℃ or higher and 350 ℃ or lower). For example, in a nitrogen atmosphere The second heat treatment is performed at 250° C. for 1 hour. is heated in contact with the oxide insulating layer 316 .

[0361] Through the above steps, the oxide semiconductor film after deposition is dehydrated or dehydrogenated. After the resistance of the oxide semiconductor film is reduced by performing heat treatment for the purpose of the present invention, a part of the oxide semiconductor film is selectively made into an oxygen-excess state. As a result, the channel formation region 313 overlapping with the gate electrode layer 311 becomes an I-type. , a low-resistance source region 314a overlapping the source electrode layer 315a, and a drain electrode layer 315b The low-resistance drain region 314b overlapping the transistor 314 is formed in a self-aligned manner. A resistor 310 is formed (see FIG. 16(D)).

[0362] Note that the oxide semiconductor layer overlapping with the drain electrode layer 315b (and the source electrode layer 315a) forming a low-resistance drain region 314b (or a low-resistance source region 314a) in This improves the reliability of the transistor. By forming the region 314b, the low-resistance drain region 314 b) A structure in which the conductivity can be changed stepwise toward the channel formation region 313. Therefore, the wiring for supplying the high power supply potential VDD to the drain electrode layer 315b is When the gate electrode layer 311 and the drain electrode layer 315b are connected and operated, a high electric field is generated between the gate electrode layer 311 and the drain electrode layer 315b. Even if a high electric field is applied, the low-resistance drain region acts as a buffer to prevent a local high electric field from being applied. This allows the transistor to have an improved dielectric strength.

[0363] A protective insulating layer may be further formed over the oxide insulating layer 316. For example, A silicon nitride film is formed using the RF sputtering method. The RF sputtering method is suitable for mass production. The protective insulating layer is preferably formed by the method described above. , O.H. - Inorganic insulation that does not contain impurities such as these and blocks their intrusion from the outside Using the film, silicon nitride film, aluminum nitride film, silicon oxynitride film, aluminum oxynitride film, In this embodiment, a nitride film or the like is used as the protective insulating layer. It is formed using a silicon film (see FIG. 16(E)).

[0364] In this embodiment, the substrate 300 on which the oxide insulating layer 316 has been formed is heated at 100° C. to 400° C. The temperature is then increased to 100° C., hydrogen and moisture are removed, and a high-purity sputtering gas containing nitrogen is introduced. A silicon nitride film is formed as the protective insulating layer 303 using a silicon semiconductor target. In this case, as in the case of the oxide insulating layer 316, moisture remaining in the treatment chamber is removed. It is preferable to deposit a protective insulating layer 303 while performing the above-mentioned process.

[0365] In addition, a planarization insulating layer for planarization may be provided over the protective insulating layer 303.

[0366] In addition, an oxide film is formed on the protective insulating layer 303 (on the planarizing insulating layer if a planarizing insulating layer is provided). A conductive layer may be provided to overlap the semiconductor layer. It may be the same as or different from the first gate electrode layer 311 and serves as a second gate electrode layer. The potential of the conductive layer may be a fixed potential such as GND or 0V. .

[0367] The conductive layer can control the electrical characteristics of the transistor 310 .

[0368] As described above, a transistor including an oxide semiconductor layer has stable electrical characteristics. It is possible to provide a highly reliable transistor.

[0369] This embodiment mode can be combined with or replaced with any of the other embodiment modes as appropriate.

[0370] (Embodiment 8) This embodiment can be applied to a transistor included in a DC converter circuit according to one embodiment of the present invention. An example of such a transistor will be described.

[0371] An example of a transistor and a manufacturing method of the transistor of this embodiment will be described with reference to FIGS. explain.

[0372] An example of a method for manufacturing a transistor is shown in FIGS. The transistor shown in Figure 1 is a type called a channel-protection type (also called a channel-stop type). It is one of the Tom gate structures and is also called an inverted staggered transistor.

[0373] In addition, the transistor 360 has a single gate structure. The transistor is a multi-gate transistor having a plurality of channel formation regions. This is also fine.

[0374] Hereinafter, a process for fabricating a transistor 360 on a substrate 320 will be described with reference to FIGS. Explain the process.

[0375] First, a conductive film is formed on a substrate 320 having an insulating surface, and then a first photolithography process is performed. A gate electrode layer 361 is formed by a process. If the resist mask is formed by the inkjet method, a photomask is not used. This reduces manufacturing costs.

[0376] The gate electrode layer 361 may be made of any of molybdenum, titanium, chromium, tantalum, tungsten, Metallic materials such as aluminum, copper, neodymium, and scandium, or alloys containing these as their main components The gold material can be used to form a single layer or a multilayer structure.

[0377] Next, the gate insulating layer 322 is formed on the gate electrode layer 361 .

[0378] Here, the oxide semiconductor (high-temperature oxide semiconductor) that has been made i-type or substantially i-type by removing impurities is Since the gate oxide semiconductor (a purified oxide semiconductor) is extremely sensitive to the interface state and the interface charge, The interface between the gate insulating layer and the highly purified oxide semiconductor layer is important. The insulating layer (GI) is required to be of high quality.

[0379] For example, high-density plasma CVD using microwaves (2.45 GHz) produces dense, high-insulation-voltage It is preferable that a highly purified oxide semiconductor layer and a high-quality insulating film can be formed. By closely contacting the gate insulating layer, the interface state can be reduced and the interface characteristics can be improved. The high-density plasma device used here is 1×10 11 / cm 3 Any device capable of achieving the above plasma density can be used.

[0380] For example, a microwave power of 3kW to 6kW is applied to generate plasma, and the formation of an insulating film is performed. The chamber is filled with monosilane gas (SiH4) and nitrous oxide (N2 O) and rare gas are introduced to generate high-density plasma at a pressure of 10 Pa to 30 Pa. An insulating film is formed on a substrate having an insulating surface such as a silicon wafer. Then, the supply of monosilane gas is stopped. Nitrous oxide (N2O) and rare gases are introduced without exposing the insulating film to the atmosphere. Plasma treatment may be performed. At least nitrous oxide (N2O) and rare gases are introduced to provide insulation. The plasma treatment on the film surface is performed after the formation of the insulating film. The flow ratio of nitrous oxide gas (N2O) to silane gas (SiH4) is 1:10 to 1:20. The rare gas introduced into the chamber is helium, argon, chlorine, etc. Lipton, xenon, etc. can be used, but argon is the most inexpensive. is preferred.

[0381] Of course, if a good insulating film can be formed as the gate insulating layer 322, sputtering is also possible. Other film formation methods such as the ring method and plasma CVD method can be applied. The quality of the gate insulating film and the interface characteristics with the oxide semiconductor are improved by heat treatment. In any case, it goes without saying that the quality of the film as a gate insulating film is good. Any material may be used as long as it can reduce the interface state density with the oxide semiconductor and form a good interface.

[0382] Furthermore, at 85°C, 2 × 10 6 V / cm, 12-hour gate bias and thermal stress test (B In the T test, when impurities are added to an oxide semiconductor, The bonds between the main component of are broken by a strong electric field (B: bias) and high temperature (T: temperature), The resulting dangling bonds induce a drift in the threshold voltage (Vth). The transistor used in the DC converter circuit of one embodiment of the present invention is an oxide semiconductor transistor. Impurities, especially hydrogen and water, are removed as much as possible to improve the interface characteristics with the gate insulating layer as described above. By doing so, it is possible to obtain a transistor that is stable even in BT tests. .

[0383] The gate insulating layer 322 may be a silicon oxide layer, a silicon nitride layer, or a silicon oxynitride layer. A silicon nitride layer, a silicon oxide nitride layer, or an aluminum oxide layer is formed as a single layer or a stacked layer. can be done.

[0384] The gate insulating layer 322 is, for example, HfO x etc. can also be used. Gate HfO as the insulating layer 322 x By using the above, the gate electrode can be formed from the oxide semiconductor layer side. Therefore, the leakage current flowing toward the

[0385] The gate insulating layer 322 is formed by laminating a silicon oxide layer and a silicon nitride layer. In this embodiment, as an example, a high density gas is generated at a pressure of 30 Pa and a microwave power of 6 kW. A silicon oxynitride layer with a thickness of 100 nm is formed by plasma CVD. The flow rate ratio of monosilane gas (SiH4) and nitrous oxide (N2O) introduced into the chamber is: The range is 1:10 to 1:200.

[0386] Next, an oxide semiconductor film having a thickness of 2 nm to 200 nm is formed over the gate insulating layer 322. The oxide semiconductor layer is then processed into an island shape by a second photolithography process. In one embodiment, sputtering was performed using an In-Ga-Zn-O metal oxide target. An oxide semiconductor film is formed by a deposition method.

[0387] In this case, it is preferable to form the oxide semiconductor film while removing residual moisture in the treatment chamber. This is to prevent hydrogen, a hydroxyl group, or moisture from being contained in the oxide semiconductor film.

[0388] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a pump for the exhaust. For example, a turbo pump is used as the exhaust means. A deposition chamber evacuated using a cryopump may be provided with a cold trap. For example, hydrogen atoms and compounds containing hydrogen atoms (such as water) are exhausted. By forming the oxide semiconductor film in the deposition chamber, the concentration of impurities contained in the oxide semiconductor film can be reduced.

[0389] The sputtering gas used in forming the oxide semiconductor film is hydrogen, water, a hydroxyl group, or is a high-purity gas in which impurities such as hydrides have been removed to concentrations of about ppm or ppb. It is preferable to use:

[0390] Next, the oxide semiconductor layer is subjected to first heat treatment. The temperature of the first heat treatment is 400° C. or higher. The temperature is set to 750° C. or lower, preferably 400° C. or higher but lower than the distortion point of the substrate. The substrate was placed in an electric furnace, which is one of the equipment used for the deposition of oxide semiconductor layers, and the temperature was raised to 450°C in a nitrogen atmosphere. After the heat treatment for 1 hour at 300° C., the oxide semiconductor layer was cooled to room temperature without being exposed to the air. Thus, the oxide semiconductor layer 332 is obtained (see FIG. 17A).

[0391] Next, a plasma treatment is performed using a gas such as N2O, N2, or Ar. Water adsorbed on the surface of the oxide semiconductor layer exposed by the treatment is removed. The plasma treatment may be performed using a mixed gas of oxygen and argon.

[0392] Next, an oxide insulating layer is formed over the gate insulating layer 322 and the oxide semiconductor layer 332. A resist mask is formed by a third photolithography process, and selective etching is performed. After the oxide insulating layer 366 is formed, the resist mask is removed.

[0393] In this embodiment, a silicon oxide film having a thickness of 200 nm is used as an example of the oxide insulating layer 366. The substrate temperature during film formation should be between room temperature and 300°C. In this embodiment, the temperature is set to 100° C. Gas (typically argon) atmosphere, oxygen atmosphere, or rare gas (typically argon) atmosphere ) and in an oxygen atmosphere. For example, a silicon target can be used to irradiate oxygen. In addition, a silicon oxide film can be formed by a sputtering method under a nitrogen atmosphere. The oxide insulating layer 366 formed in contact with the low-resistance oxide semiconductor layer is resistant to moisture, hydrogen ions, and the like. N, OH - It is an inorganic insulator that does not contain impurities such as chlorine and blocks them from entering from the outside. An insulating film is used, typically a silicon oxide film, a silicon oxynitride film, an aluminum oxide film, or An aluminum oxynitride film or the like is used.

[0394] In this case, the oxide insulating layer 366 is formed while removing residual moisture in the processing chamber. It is preferable that the oxide semiconductor layer 332 and the oxide insulating layer 366 contain hydrogen, a hydroxyl group, or moisture. This is to prevent it from being swallowed up.

[0395] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, of hydrogen atoms and compounds containing hydrogen atoms (such as water), By forming the oxide insulating layer 366 in the deposition chamber, the impurity concentration in the oxide insulating layer 366 can be reduced. do.

[0396] The sputtering gas used in forming the oxide insulating layer 366 is hydrogen, water, hydroxide, or the like. High purity, with impurities such as bases or hydrides removed to concentrations of about ppm or ppb. It is preferable to use a gas.

[0397] Next, a second heat treatment (preferably 200 ℃ or higher and 400 ℃ or lower, for example, 250 ℃ or higher and 350 ℃ or lower) may be performed. For example, The second heat treatment is performed at 250° C. for 1 hour in a SiO 2 atmosphere. A part of the semiconductor layer (channel formation region) is heated in a state in contact with the oxide insulating layer 366.

[0398] In this embodiment, an oxide semiconductor layer 366 is further provided and a part of the oxide semiconductor layer 366 is exposed. The layer 332 is subjected to a heat treatment under a nitrogen or inert gas atmosphere or under reduced pressure. The exposed areas of the oxide semiconductor layer 332 that are not covered by the border layer 366 are filled with nitrogen, indium, and other impurities. The resistance can be reduced by performing a heat treatment in an active gas atmosphere or under reduced pressure. For example, Then, heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere.

[0399] Heat treatment in a nitrogen atmosphere on the oxide semiconductor layer 332 provided with the oxide insulating layer 366 As a result, the exposed region of the oxide semiconductor layer 332 has a low resistance, and the region with a different resistance (FIG. 17( In FIG. 1B, the oxide semiconductor layer 362 has a region indicated by hatched areas and a region indicated by white areas.

[0400] Next, a conductive film is formed on the gate insulating layer 322, the oxide semiconductor layer 362, and the oxide insulating layer 366. After forming the film, a resist mask is formed by a fourth photolithography process, and selective After etching the source electrode layer 365a and the drain electrode layer 365b, Remove the dystomask (see Figure 17(C)).

[0401] The source electrode layer 365a and the drain electrode layer 365b are made of aluminum, chromium, or the like. , copper, tantalum, titanium, molybdenum, tungsten, or any of the above elements. The alloys may be made of a single element or a combination of the elements mentioned above. The conductive film may have a single layer structure or a laminated structure of two or more layers.

[0402] Through the above steps, the oxide semiconductor film after deposition is dehydrated or dehydrogenated. After the resistance of the oxide semiconductor film is reduced by performing heat treatment for the purpose of the present invention, a part of the oxide semiconductor film is selectively made into an oxygen-excess state. As a result, the channel formation region 363 overlapping with the gate electrode layer 361 becomes I-shaped. A low-resistance source region 364a overlapping the source electrode layer 365a and a drain electrode layer 365 The low-resistance drain region 364b overlapping the transistor 364b is formed in a self-aligned manner. A transistor 360 is formed.

[0403] Note that the oxide semiconductor layer overlapping with the drain electrode layer 365b (and the source electrode layer 365a) forming a low-resistance drain region 364b (or a low-resistance source region 364a) in This improves the reliability of the transistor. By forming the region 364b, the low resistance drain region 364b and the channel It is possible to provide a structure in which the conductivity can be changed stepwise from the first region to the second region. Therefore, the drain electrode layer 365b is connected to a wiring that supplies a high power supply potential VDD. When the device is operated, a high electric field is applied between the gate electrode layer 361 and the drain electrode layer 365b. Even if the transistor is turned on, the low-resistance drain region acts as a buffer to prevent a local high electric field from being applied. It is possible to provide a configuration in which the withstand voltage of the semiconductor device is improved.

[0404] A protective insulating layer 3 is formed on the source electrode layer 365a, the drain electrode layer 365b, and the oxide insulating layer 366. In this embodiment, the protective insulating layer 323 is formed using a silicon nitride film. (See Figure 17(D)).

[0405] Note that a thin film is further formed over the source electrode layer 365 a, the drain electrode layer 365 b, and the oxide insulating layer 366. An oxide insulating layer may be formed and a protective insulating layer 323 may be stacked over the oxide insulating layer.

[0406] As described above, a transistor including an oxide semiconductor layer has stable electrical characteristics. It is possible to provide a highly reliable transistor.

[0407] Note that this embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0408] (Embodiment 9) In this embodiment, a transistor included in a DC converter circuit according to one embodiment of the present invention can be used. An example of a transistor that can be used will be described below.

[0409] An example of a transistor and a manufacturing method of the transistor of this embodiment will be described with reference to FIGS. 18A to 18C are cross-sectional views illustrating a method for manufacturing a transistor of this embodiment.

[0410] In addition, the transistor 350 has a single gate structure. The transistor is a multi-gate transistor having a plurality of channel formation regions. This is also fine.

[0411] Hereinafter, a process for fabricating a transistor 350 on a substrate 340 will be described with reference to FIGS. Explain the process.

[0412] First, a conductive film is formed on a substrate 340 having an insulating surface, and then a first photolithography process is performed. In this embodiment, the gate electrode layer 351 is formed by a process. A tungsten film with a thickness of 150 nm was deposited by sputtering as a conductive film for forming the GaN- ... and form it.

[0413] Next, the gate insulating layer 342 is formed on the gate electrode layer 351 .

[0414] Here, the oxide semiconductor (high-temperature oxide semiconductor) that has been made i-type or substantially i-type by removing impurities is Since the gate oxide semiconductor (a purified oxide semiconductor) is extremely sensitive to the interface state and the interface charge, The interface between the gate insulating layer and the highly purified oxide semiconductor layer is important. The insulating layer (GI) is required to be of high quality.

[0415] For example, high-density plasma CVD using microwaves (2.45 GHz) produces dense, high-insulation-voltage It is preferable that a highly purified oxide semiconductor layer and a high-quality insulating film can be formed. By closely contacting the gate insulating layer, the interface state can be reduced and the interface characteristics can be improved. The high-density plasma device used here is 1×10 11 / cm 3 Any device capable of achieving the above plasma density can be used.

[0416] For example, a microwave power of 3kW to 6kW is applied to generate plasma, and the formation of an insulating film is performed. The chamber is filled with monosilane gas (SiH4) and nitrous oxide (N2 O) and rare gas are introduced to generate high-density plasma at a pressure of 10 Pa to 30 Pa. An insulating film is formed on a substrate having an insulating surface such as a silicon wafer. Then, the supply of monosilane gas is stopped. Nitrous oxide (N2O) and rare gases are introduced without exposing the insulating film to the atmosphere. Plasma treatment may be performed. At least nitrous oxide (N2O) and rare gases are introduced to provide insulation. The plasma treatment on the film surface is performed after the formation of the insulating film. The flow ratio of nitrous oxide gas (N2O) to silane gas (SiH4) is 1:10 to 1:20. The rare gas introduced into the chamber is helium, argon, chlorine, etc. Lipton, xenon, etc. can be used, but argon is the most inexpensive. is preferred.

[0417] Of course, if a good insulating film can be formed as the gate insulating layer 342, sputtering is also possible. Other film formation methods such as the ring method and plasma CVD method can be applied. The quality of the gate insulating film and the interface characteristics with the oxide semiconductor are improved by heat treatment. In any case, it goes without saying that the quality of the film as a gate insulating film is good. Any material may be used as long as it can reduce the interface state density with the oxide semiconductor and form a good interface.

[0418] Furthermore, at 85°C, 2 × 10 6 V / cm, 12-hour gate bias and thermal stress test (B In the T test, when impurities are added to an oxide semiconductor, The bonds between the main component of are broken by a strong electric field (B: bias) and high temperature (T: temperature), The resulting dangling bonds induce a drift in the threshold voltage (Vth). The transistor used in the DC converter circuit of one embodiment of the present invention is an oxide semiconductor transistor. Impurities, especially hydrogen and water, are removed as much as possible to improve the interface characteristics with the gate insulating layer as described above. By doing so, it is possible to obtain a transistor that is stable even in BT tests. .

[0419] The gate insulating layer 342 may be a silicon oxide layer, a silicon nitride layer, or a silicon oxynitride layer. The silicon layer (SiO x N y where x>y>0), silicon oxynitride layer (SiN x O y (where x>y>0), or aluminum oxide layers formed as a single layer or multilayers It is possible.

[0420] The gate insulating layer 342 is, for example, HfO x etc. can also be used. Gate HfO as the insulating layer 342 x By using the above, the gate electrode can be formed from the oxide semiconductor layer side. Therefore, the leakage current flowing toward the

[0421] The gate insulating layer 342 is formed by laminating a silicon oxide layer and a silicon nitride layer. In this embodiment, as an example, a high density gas is generated at a pressure of 30 Pa and a microwave power of 6 kW. A silicon oxynitride layer with a thickness of 100 nm is formed by plasma CVD. The flow rate ratio of monosilane gas (SiH4) and nitrous oxide (N2O) introduced into the chamber is: The range is 1:10 to 1:200.

[0422] Next, a conductive film is formed on the gate insulating layer 342, and a conductive film is formed by a second photolithography process. A resist mask is formed on the conductive film, and selective etching is performed to form a source electrode layer 355a. After the drain electrode layer 355b is formed, the resist mask is removed (see FIG. 18A). .

[0423] Next, an oxide semiconductor film 345 is formed (see FIG. 18B). The semiconductor film 345 is formed by sputtering using an In-Ga-Zn-O metal oxide target. The oxide semiconductor film 345 is formed into an island by a third photolithography process. The oxide semiconductor layer is then processed into a shaped oxide semiconductor layer.

[0424] In this case, the oxide semiconductor film 345 is formed while removing moisture remaining in the treatment chamber. In order to prevent hydrogen, a hydroxyl group, or moisture from being contained in the oxide semiconductor film 345, This is the case.

[0425] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, of hydrogen atoms and compounds containing hydrogen atoms (such as water), By forming the oxide semiconductor film 345 in the deposition chamber, the impurity concentration in the oxide semiconductor film 345 can be reduced. Cut.

[0426] The oxide semiconductor film 345 is formed using a sputtering gas such as hydrogen, water, or water. High purity, with impurities such as acid groups or hydrides removed to concentrations of ppm or ppb. It is preferable to use a high-temperature gas.

[0427] Next, the oxide semiconductor layer is subjected to first heat treatment. The temperature of the first heat treatment is 400° C. or higher. The temperature is set to 750° C. or lower, preferably 400° C. or higher but lower than the distortion point of the substrate. The substrate was placed in an electric furnace, which is one of the equipment used for the deposition of oxide semiconductor layers, and the temperature was raised to 450°C in a nitrogen atmosphere. After the heat treatment for 1 hour, the oxide semiconductor layer was exposed to air and water or moisture was not allowed to enter the oxide semiconductor layer. In the first heat treatment, the oxide semiconductor layer 346 is obtained (see FIG. 18C). This results in dehydration or dehydrogenation.

[0428] In the first heat treatment, the substrate is immersed in an inert gas heated to a high temperature of 650°C to 700°C. After heating for a few minutes, the substrate is removed from the heated inert gas. GRTA may be used, which allows high-temperature heat treatment in a short period of time.

[0429] Furthermore, an oxide insulating layer 356 serving as a protective insulating film in contact with the oxide semiconductor layer 346 is formed. .

[0430] The oxide insulating layer 356 has a thickness of at least 1 nm and is formed by an oxide method such as a sputtering method. The insulating layer 356 can be formed by using a method that does not allow impurities such as water and hydrogen to be mixed in. When hydrogen is contained in the oxide insulating layer 356, the hydrogen penetrates into the oxide semiconductor layer, Alternatively, oxygen in the oxide semiconductor layer is extracted by hydrogen, and the backchannel of the oxide semiconductor layer is formed. The resistance of the panel becomes low (N-type), and a parasitic channel may be formed. In order to form the oxide insulating layer 356 as a film containing as little hydrogen as possible, hydrogen is not used in the deposition method. It is important that there is no

[0431] In this embodiment, a silicon oxide film having a thickness of 200 nm is formed by sputtering as the oxide insulating layer 356. The substrate temperature during film formation should be between room temperature and 300°C. In the embodiment, the temperature is set to 100° C. The silicon oxide film is formed by sputtering using a rare gas ( Typically, under an atmosphere of argon), under an oxygen atmosphere, or under a rare gas atmosphere (typically, argon) and The deposition can be carried out in an oxygen atmosphere. The target is a silicon oxide target or For example, a silicon target can be used to oxidize oxygen and A silicon oxide film can be formed by sputtering in a nitrogen atmosphere. The oxide insulating layer 356 is formed in contact with the oxide semiconductor layer that has become an N-type oxide semiconductor layer and has a low resistance. is water, hydrogen ions, OH -It does not contain impurities such as these, and prevents them from entering from the outside. A blocking inorganic insulating film is used, typically a silicon oxide film, a silicon oxynitride film, or an oxide An aluminum film, an aluminum oxynitride film, or the like is used.

[0432] In this case, the oxide insulating layer 356 is formed while removing residual moisture in the processing chamber. It is preferable that the oxide semiconductor layer 346 and the oxide insulating layer 356 contain hydrogen, a hydroxyl group, or moisture. This is to prevent it from being swallowed up.

[0433] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, to hydrogen atoms and compounds containing hydrogen atoms such as water (H2O). Therefore, the impurity concentration in the oxide insulating layer 356 formed in the deposition chamber can be reduced.

[0434] The sputtering gas used in forming the oxide insulating layer 356 is hydrogen, water, hydroxide, or the like. High purity, with impurities such as bases or hydrides removed to concentrations of about ppm or ppb. It is preferable to use a gas.

[0435] Next, a second heat treatment (preferably 200 ℃ or higher and 400 ℃ or lower, for example, 250 ℃ or higher and 350 ℃ or lower). For example, in a nitrogen atmosphere The second heat treatment is performed at 250° C. for 1 hour. The insulating layer 356 is heated while a part of the insulating layer 356 (channel formation region) is in contact with the insulating layer 356 .

[0436] As described above, by performing heat treatment for dehydration or dehydrogenation, the oxide semiconductor layer The oxide semiconductor layer is then oxidized to make it in contact with the oxide semiconductor layer. By forming the oxide insulating layer, the oxide semiconductor layer is made in an oxygen-excess state. Through the above steps, the transistor 350 is formed. will be done.

[0437] A protective insulating layer may be further formed on the oxide insulating layer 356. For example, In this embodiment mode, a silicon nitride film is formed as a protective insulating layer. The edge layer 343 is formed using a silicon nitride film (see FIG. 18(D)).

[0438] Further, a planarization insulating layer for planarization may be provided over the protective insulating layer 343.

[0439] As described above, a transistor including an oxide semiconductor layer has stable electrical characteristics and is reliable. This makes it possible to provide a highly reliable transistor.

[0440] This embodiment mode can be combined with or replaced with any of the other embodiment modes as appropriate.

[0441] (Embodiment 10) This embodiment can be applied to a transistor included in a DC converter circuit according to one embodiment of the present invention. An example of such a transistor will be described.

[0442] In this embodiment, a manufacturing process of a transistor is partially different from that in Embodiment 7, as shown in FIG. Figure 19 is the same as Figure 16 except for some differences in the process, so the same parts are Reference numerals will be used and detailed explanations of the same parts will be omitted.

[0443] First, a gate electrode layer 381 is formed on a substrate 370, and a first gate insulating layer 372a and a second gate insulating layer 372b are formed on the gate electrode layer 381. In this embodiment, the gate insulating layer has a two-layer structure. The first gate insulating layer 372a is a nitride insulating layer, and the second gate insulating layer 372b is an oxide insulating layer. A border layer is used.

[0444] The oxide insulating layer may be, for example, a silicon oxide layer, a silicon oxynitride layer, or an aluminum oxide layer. An aluminum layer, an aluminum oxynitride layer, or the like can be used. Examples of the layer include a silicon nitride layer, a silicon oxynitride layer, an aluminum nitride layer, and an aluminum oxynitride layer. A minium layer or the like can be used.

[0445] The first gate insulating layer 372a or the second gate insulating layer 372b is, for example, H fO x The first gate insulating layer 372a or the second gate insulating layer 372b may be used. 372b HfO x By using the above, it is possible to form a gate electrode from the oxide semiconductor layer side. The leakage current that may flow can be reduced.

[0446] In this embodiment, a silicon nitride layer and a silicon oxide layer are stacked from the gate electrode layer 381 side. The first gate insulating layer 372a is formed by sputtering to a thickness of 50 nm. A silicon nitride layer (SiN y (y> 0)) and a film as a second gate insulating layer 372b is formed on the first gate insulating layer 372a. A silicon oxide layer (SiO x (x>0) is laminated to form a gate insulating layer with a thickness of 150 nm.

[0447] Next, an oxide semiconductor film is formed, and the oxide semiconductor film is divided into islands by a photolithography process. In this embodiment, an In-Ga-Zn-O based oxide semiconductor layer is used as an example. An oxide semiconductor film is formed by a sputtering method using a metal oxide target.

[0448] In this case, it is preferable to form the oxide semiconductor film while removing residual moisture in the treatment chamber. This is to prevent hydrogen, a hydroxyl group, or moisture from being contained in the oxide semiconductor film.

[0449] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, to hydrogen atoms and compounds containing hydrogen atoms such as water (H2O). Therefore, the impurity concentration in the oxide semiconductor film formed in the deposition chamber can be reduced.

[0450] The sputtering gas used in forming the oxide semiconductor film is hydrogen, water, a hydroxyl group, or is a high-purity gas in which impurities such as hydrides have been removed to concentrations of about ppm or ppb. It is preferable to use:

[0451] Next, the oxide semiconductor layer is dehydrated or dehydrogenated. The temperature of the heat treatment is 400°C or higher and 750°C or lower, preferably 425°C or higher and 750°C or lower. If the temperature is 425°C or higher, the heat treatment time may be 1 hour or less. In this case, the heat treatment time is set to be longer than one hour. The substrate is placed in an electric furnace, and the oxide semiconductor layer is subjected to heat treatment in a nitrogen atmosphere. After the above steps, the oxide semiconductor layer is prevented from being exposed to the air and from being contaminated by water or hydrogen. In the same furnace, high-purity oxygen gas, high-purity N2O gas, or ultra-dry air (dew point below -40℃) Cooling is performed by introducing oxygen gas or N2O gas into the reactor at a temperature of 300°C or lower, preferably at -60°C or lower. It is preferable that hydrogen and the like are not included. Alternatively, oxygen gas or N2 The purity of O gas is 6N (99.9999%) or more, preferably 7N (99.99999%). ) or more (i.e., impurity concentration in oxygen gas or N2O gas is 1 ppm or less, preferably 0. It is preferable to keep the concentration at 1 ppm or less.

[0452] The heat treatment device is not limited to an electric furnace, and may be, for example, a GRTA device, a LRTA device, or the like. The TA device can be used. The LRTA device uses halogen lamps, metal halide lamps, etc. xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp It is a device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a In addition, the heat generated by the LRTA device, lamps, and other heat sources such as resistance heating elements may also be used. A device that heats the workpiece by radiation may be used. GRTA is a device that uses high-temperature gas. The gas used is a rare gas such as argon or a gas with a high thermal conductivity such as nitrogen. An inert gas that does not react with the workpiece during heat treatment is used. Heat treatment may be performed at 0° C. to 750° C. for several minutes.

[0453] After the first heat treatment for dehydration or dehydrogenation, the temperature is preferably 200° C. or higher and 400° C. or lower. Heat treatment is usually performed at temperatures between 200°C and 300°C in an oxygen or N2O gas atmosphere. You may go.

[0454] In addition, the first heat treatment of the oxide semiconductor layer is performed on the oxide semiconductor layer before it is processed into the island-shaped oxide semiconductor layer. In this case, the substrate is removed from the heating device after the first heat treatment. The substrate is then taken out and subjected to a photolithography process.

[0455] By going through the above steps, the entire oxide semiconductor layer is made into an oxygen-excess state, and thus a high resistance As a result, the oxide semiconductor layer 382 which is entirely i-type can be obtained.

[0456] Next, a conductive film is formed over the oxide semiconductor layer 382 and then is subjected to a resist process by a photolithography process. A mask is formed, and selective etching is performed to form the source electrode layer 385a and the drain electrode layer 385b. A layer 385b is formed, and an oxide insulating layer 386 is formed by a sputtering method.

[0457] In this case, the oxide insulating layer 386 is formed while removing residual moisture in the processing chamber. It is preferable that the oxide semiconductor layer 382 and the oxide insulating layer 386 contain hydrogen, a hydroxyl group, or moisture. This is to prevent it from being swallowed up.

[0458] In order to remove residual moisture from within the processing chamber, it is preferable to use an adsorption type vacuum pump. Examples of adsorption type vacuum pumps include cryopumps, ion pumps, and titanium sublimation pumps. It is preferable to use a displacement pump. As the exhaust means, for example, a turbo pump is used. The deposition chamber may be equipped with a cold trap. The chamber is evacuated, for example, to hydrogen atoms and compounds containing hydrogen atoms such as water (H2O). Therefore, the impurity concentration in the oxide insulating layer 386 formed in the deposition chamber can be reduced.

[0459] The sputtering gas used in forming the oxide insulating layer 386 is hydrogen, water, a hydroxyl group, or water. Uses high-purity gas in which impurities such as chlorine have been removed to concentrations of ppm or ppb. It is preferable that

[0460] Through the above steps, the transistor 380 can be formed.

[0461] Note that in order to reduce variations in electrical characteristics of the transistors, Heat treatment (preferably at 150° C. or higher and lower than 350° C.) may be performed in a nitrogen gas atmosphere. For example, a heat treatment is performed at 250° C. for 1 hour in a nitrogen atmosphere.

[0462] In addition, heat treatment is performed in air at 100°C to 200°C for 1 hour to 30 hours. In this embodiment, heat treatment is performed at 150° C. for 10 hours. Heat treatment may be performed by holding the material at a heating temperature, or by heating the material from room temperature to a temperature of 100°C or higher and 200°C or lower. Heat treatment may be performed by repeatedly increasing the temperature to a heating temperature and decreasing the temperature from the heating temperature to room temperature. Heating under reduced pressure can shorten the heating time. In this case, hydrogen is absorbed from the oxide semiconductor layer into the oxide insulating layer, and the transistor becomes normally off. Therefore, the reliability of the transistor can be improved.

[0463] The protective insulating layer 373 is formed over the oxide insulating layer 386. In this embodiment, the protective insulating layer 3 As the film 73, a silicon nitride film is formed to a thickness of 100 nm by using a sputtering method.

[0464] The protective insulating layer 373 and the first gate insulating layer 372a made of a nitride insulating layer are resistant to moisture and water. It does not contain impurities such as hydrogen, hydrides, or hydroxides, and blocks these from entering from the outside. It has the effect of checking.

[0465] Therefore, in the manufacturing process after the protective insulating layer 373 is formed, impurities such as moisture from the outside This can prevent the intrusion of foreign matter and improve the long-term reliability of the device.

[0466] In addition, a protective insulating layer 373 made of a nitride insulating layer and a first gate insulating layer 372a are provided between the protective insulating layer 373 and the first gate insulating layer 372a. A part of the insulating layer to be removed is formed so that the protective insulating layer 373 and the first gate insulating layer 372a are in contact with each other. The structure may be such that:

[0467] Therefore, impurities such as moisture, hydrogen, hydrides, and hydroxides in the oxide semiconductor layer can be eliminated as much as possible. and preventing the inclusion of the impurities, thereby maintaining the impurity concentration in the oxide semiconductor layer low. It is possible.

[0468] Further, a planarization insulating layer for planarization may be provided over the protective insulating layer 373.

[0469] A conductive layer overlapping with the oxide semiconductor layer may be provided over the protective insulating layer 373. The potential may be the same as that of the gate electrode layer 381 of the transistor 380 or may be different. The conductive layer may also function as a second gate electrode layer. It may be a fixed potential of V.

[0470] The conductive layer can control the electrical characteristics of the transistor 380 .

[0471] As described above, a transistor including an oxide semiconductor layer has stable electrical characteristics. It is possible to provide a highly reliable transistor.

[0472] This embodiment mode can be combined with or replaced with any of the other embodiment modes as appropriate.

[0473] (Embodiment 11) The DC converter circuit according to one embodiment of the present invention can be combined with various other power storage devices to form a power supply circuit. In this embodiment, a power supply using a DC converter circuit according to one embodiment of the present invention can be constructed. The power supply circuit will now be described.

[0474] An example of the configuration of the power supply circuit of this embodiment will be described with reference to FIG. 1 is a block diagram showing an example of a configuration of a power supply circuit according to an embodiment;

[0475] The power supply circuit shown in FIG. 20 includes a power storage device 601 and a DC conversion circuit 602.

[0476] The power storage device 601 has a function of supplying power. Conversion device, lithium ion secondary battery, lithium ion capacitor, electric double layer capacitor , and redox capacitors, or any one or more thereof. For example, By using a lithium-ion secondary battery and a lithium-ion capacitor in combination, high-speed charging and discharging It is possible to provide a power storage device that can store a large amount of power and can supply power for a long period of time. The power storage device 601 is not limited to a lithium ion secondary battery, and may be any other alkaline metal A secondary battery using lithium ions or alkaline earth metal ions as mobile ions may also be used. In addition, the power storage device 601 is not limited to a lithium ion capacitor, and may be any other alkaline. A capacitor using lithium metal ions or alkaline earth metal ions as mobile ions is used. It's fine.

[0477] The DC conversion circuit 602 is electrically connected to the power storage device 601. For example, the DC converter circuit described in the above embodiment 1 or 2 can be used. Cut.

[0478] As shown in FIG. 20, an example of the power supply circuit of this embodiment has a power storage device and a DC conversion circuit. The power supplied from the power storage device is boosted or stepped down by the DC conversion circuit, It generates a power supply voltage that is suitable for the specifications of the device to which the power is supplied. In a power supply circuit of the present invention, a DC converter circuit according to one embodiment of the present invention is used as a DC converter circuit. This makes it possible to improve the reliability of the power supply circuit.

[0479] This embodiment mode can be appropriately combined with or replaced by other embodiment modes. do.

[0480] (Embodiment 12) This embodiment mode will describe an electronic device to which the power supply circuit shown in the above embodiment mode 11 can be applied. An example will be described with reference to FIG.

[0481] FIG. 21A shows a notebook personal computer, which includes a main body 3001 and a housing 300 2, a display unit 3003, a keyboard 3004, etc. In order to generate the power supply voltage for the notebook personal computer shown in A), The power supply circuit of the eleventh embodiment can be applied.

[0482] FIG. 21B shows a mobile phone, which is composed of two housings, a housing 2800 and a housing 2801. The housing 2801 includes a display panel 2802, a speaker 2803, a microphone, and a 2804, pointing device 2806, camera lens 2807, external connection terminal The housing 2800 also includes a solar cell for charging the mobile phone. The housing 28 is provided with an antenna, a memory slot 2810, and an external memory slot 2811. It is built into the 01.

[0483] The display panel 2802 is equipped with a touch panel, and in FIG. The multiple operation keys 2805 are indicated by dotted lines. The solar cell 2810 and the voltage output from the solar cell 2810 are required for each circuit. The power supply circuit is configured using a DC conversion circuit that converts the input voltage into a desired voltage.

[0484] As described above, the power supply circuit according to the eleventh embodiment can be applied to various electronic devices. In addition, by applying the power supply circuit according to the eleventh embodiment to electronic equipment, It is possible to provide high-quality electronic equipment.

[0485] This embodiment mode can be appropriately combined with or replaced by other embodiment modes. do. [Explanation of symbols]

[0486] 101 Inductive element 102 Transistor 103 Rectifier 104 Control circuit 201 Coil 202 Transistor 203 Diode 204 Capacitive element 205 Hysteresis Comparator 221 Comparator 222 Comparator 223 Inverter 224 Inverter 225 NOR Gate 226 NOR Gate 300 Substrates 302 Gate insulating layer 303 Protective insulation layer 310 Transistor 311 Gate electrode layer 313 Channel formation region 314a Low resistance source region 314b Low-resistance drain region 315a Source electrode layer 315b Drain electrode layer 316 Oxide insulating layer 320 Substrate 322 Gate Insulation Layer 323 Protective Insulation Layer 330 Oxide Semiconductor Film 331 Oxide semiconductor layer 332 Oxide semiconductor layer 340 Substrate 342 Gate Insulation Layer 343 Protective Insulation Layer 345 Oxide Semiconductor Film 346 Oxide Semiconductor Layer 350 Transistors 351 Gate electrode layer 352 Oxide semiconductor layer 355a Source electrode layer 355b Drain electrode layer 356 Oxide insulating layer 360 Transistor 361 Gate electrode layer 362 Oxide semiconductor layer 363 Channel Formation Region 364a Low resistance source region 364b Low-resistance drain region 365a Source electrode layer 365b Drain electrode layer 366 Oxide Insulating Layer 370 Substrate 372a Gate insulating layer 372b Gate insulating layer 373 Protective Insulation Layer 380 Transistors 381 Gate electrode layer 382 Oxide semiconductor layer 385a Source electrode layer 385b Drain electrode layer 386 Oxide Insulating Layer 390 Transistors 391 Gate electrode layer 392 Oxide semiconductor layer 393 Oxide Semiconductor Film 394 Substrate 395a Source electrode layer 395b Drain electrode layer 396 Oxide Insulating Layer 397 Gate Insulation Layer 398 Protective Insulation Layer 399 Oxide Semiconductor Layer 400 Substrates 402 Gate insulating layer 407 Insulating Layer 410 Transistor 411 Gate electrode layer 412 Oxide semiconductor layer 414a wiring layer 414b wiring layer 415a Source electrode layer 415b Drain electrode layer 420 Silicon substrate 421a aperture 421b aperture 422 Insulating layer 423 Aperture 424 Conductive layer 425 Transistor 426 Transistor 427 Conductive Layer 450 Substrate 452 Gate insulation layer 457 Insulating Layer 460 Transistors 461 Gate electrode layer 461a Gate electrode layer 461b Gate electrode layer 462 Oxide Semiconductor Layer 464 Wiring layer 465a Electrode layer 465b Electrode layer 465a1 Electrode layer 465a2 Electrode layer 468 Wiring layer 601 Electricity storage device 602 DC conversion circuit 1001 Gate electrode 1002 Gate insulating film 1003 Oxide semiconductor layer 1004a Source electrode 1004b Drain electrode 1005 Oxide insulating layer 1006 Conductive layer 2800 Chassis 2801 Case 2802 Display Panel 2803 Speaker 2804 Microphone 2805 Operation key 2806 Pointing Device 2807 Camera lenses 2808 External connection terminal 2810 Solar Cell 2811 External memory slot 3001 Main unit 3002 Case 3003 Display section 3004 Keyboard

Claims

1. A first conductive layer; and a semiconductor layer disposed above the first conductive layer and having a channel formation region of a transistor; a second conductive layer electrically connected to the semiconductor layer and disposed above the semiconductor layer; a third conductive layer electrically connected to the semiconductor layer and the first conductive layer and disposed above the semiconductor layer; a fourth conductive layer having a function as a gate electrode of the transistor and overlapping the semiconductor layer with an insulating layer therebetween; a fifth conductive layer having a region in contact with the third conductive layer and disposed above the third conductive layer and above the insulating layer; the third conductive layer overlaps with the first conductive layer via the semiconductor layer; The fourth conductive layer overlaps with the first conductive layer via the insulating layer and the semiconductor layer.

2. A first conductive layer; and a semiconductor layer disposed above the first conductive layer and having a channel formation region of a transistor; a second conductive layer electrically connected to the semiconductor layer and disposed above the semiconductor layer; a third conductive layer electrically connected to the semiconductor layer and the first conductive layer and disposed above the semiconductor layer; a fourth conductive layer having a function as a gate electrode of the transistor and overlapping the semiconductor layer with an insulating layer therebetween; a fifth conductive layer having a region in contact with the third conductive layer and disposed above the third conductive layer and above the insulating layer; the second conductive layer and the third conductive layer are disposed in the same layer; the third conductive layer overlaps with the first conductive layer via the semiconductor layer; The fourth conductive layer overlaps with the first conductive layer via the insulating layer and the semiconductor layer.

3. A first conductive layer; and a semiconductor layer disposed above the first conductive layer and having a channel formation region of a transistor; a second conductive layer electrically connected to the semiconductor layer and disposed above the semiconductor layer; a third conductive layer electrically connected to the semiconductor layer and the first conductive layer and disposed above the semiconductor layer; a fourth conductive layer having a function as a gate electrode of the transistor and overlapping the semiconductor layer with an insulating layer therebetween; a fifth conductive layer having a region in contact with the third conductive layer and disposed above the third conductive layer and above the insulating layer; the third conductive layer overlaps with the first conductive layer via the semiconductor layer; the fourth conductive layer overlaps with the first conductive layer via the insulating layer and the semiconductor layer; A semiconductor device, wherein an area of ​​a region where the first conductive layer and the semiconductor layer overlap is larger than an area of ​​a region where the second conductive layer and the semiconductor layer overlap.

4. A first conductive layer; and a semiconductor layer disposed above the first conductive layer and having a channel formation region of a transistor; a second conductive layer electrically connected to the semiconductor layer and disposed above the semiconductor layer; a third conductive layer electrically connected to the semiconductor layer and the first conductive layer and disposed above the semiconductor layer; a fourth conductive layer having a function as a gate electrode of the transistor and overlapping the semiconductor layer with an insulating layer therebetween; a fifth conductive layer having a region in contact with the third conductive layer and disposed above the third conductive layer and above the insulating layer; the second conductive layer and the third conductive layer are disposed in the same layer; the third conductive layer overlaps with the first conductive layer via the semiconductor layer; the fourth conductive layer overlaps with the first conductive layer via the insulating layer and the semiconductor layer; A semiconductor device, wherein an area of ​​a region where the first conductive layer and the semiconductor layer overlap is larger than an area of ​​a region where the second conductive layer and the semiconductor layer overlap.

5. In any one of claims 1 to 4, A semiconductor device, wherein a region of the third conductive layer that contacts the fifth conductive layer does not overlap with the semiconductor layer.

6. In any one of claims 1 to 5, The second conductive layer does not overlap with the first conductive layer.

Citation Information

Patent Citations

  • Non-insulation type l-c resonance converter

    JP1983086868A

  • Thin-film transistor and display device

    JP2006024610A

  • Semiconductor device and manufacturing method thereof

    JP2007134687A

  • Semiconductor device and manufacturing method therefor

    JP2008270773A