Positive electrode material, positive electrode plate and battery
By employing specific particle size relationships and manganese to iron molar ratios in LMFP materials, the battery's capacity, manganese leaching, and cycling stability are enhanced, addressing the limitations of existing LMFP materials.
Patent Information
- Application Number
- JP2023517872
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-18
- Filing Date
- 2021-09-18
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-09-18
AI Technical Summary
Current lithium manganese iron phosphate (LMFP) materials face challenges in achieving high capacity, low manganese leaching, and high cycling stability due to issues with particle size and manganese to iron molar ratio, leading to poor structural stability and increased diffusion barriers for lithium ions.
Designing positive electrode materials with specific particle size relationships and manganese to iron molar ratios for LMFP materials, including monolithic, dibasic, tribasic, quaternary, and pentavalent forms, to optimize compaction density and electrochemical properties.
The optimized LMFP materials result in batteries with high capacity, low manganese elution, and improved cycling stability, maintaining high structural integrity and efficient lithium ion diffusion.
Smart Images

Figure 0007576692000001 
Figure 0007576692000002 
Figure 0007576692000003
Abstract
Description
[Technical field]
[0001] (Reference to Related Applications) This application claims priority to Chinese Patent Application No. 202010987080.X, entitled “Positive Electrode Material, Positive Electrode Slurry, Positive Electrode Plate and Battery,” filed with the State Intellectual Property Office of the People's Republic of China on September 18, 2020, the entire contents of which are incorporated herein by reference.
[0002] The present application relates to the technical field of batteries, and in particular to positive electrode materials, positive plates and batteries. [Background technology]
[0003] The positive electrode material of lithium-ion batteries is of great importance to the properties of the battery. Commonly used positive electrode materials for power batteries include ternary materials, lithium iron phosphate materials, and lithium manganese iron phosphate materials. Lithium manganese iron phosphate (abbreviated as LMFP) has higher safety and cycle properties than ternary materials, and its potential is much higher than that of lithium iron phosphate (the potential of lithium iron phosphate is 3.4V), which is expected to increase the energy density of the battery. Therefore, the lithium manganese iron phosphate material with higher safety and higher energy density will gradually become the main positive electrode material for power batteries.
[0004] There are two main types of LMFP product forms commonly seen on the current market: pseudo-single crystal and aggregate. Pseudo-single crystal materials are composed of one or a small number (less than five) of primary particles, and have very few internal grain boundaries, while aggregate materials are secondary particle materials in which multiple primary particles are aggregated, and have many internal grain boundaries. Because the primary particles of pseudo-single crystal LMFP materials are large, such materials have a low degree of manganese elution during the battery cycle process, but the capacity that can be achieved with the same metal ratio is low. On the other hand, if the primary particles of the aggregates are small, the specific surface area is large, and the capacity that can be achieved by such materials is high. However, aggregate materials are easily crushed during the compression process, causing the fresh surface of such materials to be exposed to the electrolyte. As a result, serious manganese elution phenomenon occurs during the battery cycle, and the cycle characteristics are deteriorated. In addition, the Mn / Fe molar ratio of LMFP materials is an important factor that affects the structural stability, cycle stability of the battery, rate characteristics, etc. Therefore, it is necessary to provide a completely new LMFP-containing positive electrode material to fabricate a battery with characteristics such as high capacity, low manganese elution, and high cycle stability. Summary of the Invention [Problem to be solved by the invention]
[0005] The present application provides a positive electrode material, a positive electrode plate, and a battery in which, by designing the particle sizes of various LMFP materials with different particle sizes in a positive electrode material, and by designing the morphology and Mn / Fe molar ratio of the LMFP materials with different particle sizes, the positive electrode plate manufactured from the positive electrode material has an appropriate compaction density and each electrochemical characteristic of the battery can be optimized. [Means for solving the problem]
[0006] Specifically, in a first aspect, the positive electrode material according to the present application includes a first lithium manganese iron phosphate material, a second lithium manganese iron phosphate material, a third lithium manganese iron phosphate material, a fourth lithium manganese iron phosphate material, and a fifth lithium manganese iron phosphate material, wherein the first lithium manganese iron phosphate material is an aggregate, the fourth lithium manganese iron phosphate material and the fifth lithium manganese iron phosphate material are both pseudo-single crystals, and the second lithium manganese iron phosphate material and the third lithium manganese iron phosphate material are each an aggregate and / or a pseudo-single crystal, D 50 5 <D 50 4 <D 50 3 <D 50 2 <D 50 1 The particle size relationship of D is satisfied. 50 2 =aD 50 1 , D 50 3 =bD 50 1 , D 50 4 =cD 50 1 , D 50 5 =dD 50 1 and 5 μm≦D 50 1 ≦15 μm, Here, the D 50 1 ~D 50 5 are the particle diameters D of the first lithium manganese iron phosphate material to the fifth lithium manganese iron phosphate material, 50 the value of a is in the range of 0.35 to 0.5, the value of b is in the range of 0.2 to 0.27, the value of c is in the range of 0.17 to 0.18, and the value of d is in the range of 0.15 to 0.16, The molar ratios of manganese to iron in the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material and the fourth lithium manganese iron phosphate material increase in this order, and the molar ratio of manganese to iron in the fifth lithium manganese iron phosphate material is greater than the molar ratio of manganese to iron in the third lithium manganese iron phosphate material.
[0007] In a second aspect, the present application provides a positive electrode slurry comprising the positive electrode material according to the first aspect of the present application, a conductive agent, and a solvent.
[0008] In a third aspect, the present application provides a positive electrode plate comprising a current collector and a positive electrode material layer disposed on the current collector, the positive electrode material layer comprising the positive electrode material as described in the first aspect of the present application or a positive electrode slurry as described in the second aspect of the present application applied to the current collector.
[0009] In a fourth aspect, a battery according to the present application includes a positive plate according to the third aspect of the present application. Effect of the Invention
[0010] The beneficial effects of the present application include the following: The five lithium manganese iron phosphate materials contained in the cathode material of the present application have the above-mentioned specific D 50 When the particle size relationship, the above-mentioned specific morphology requirements, and the size requirements of the specific Mn / Fe molar ratio are satisfied, the packing density of the positive plate made of the positive electrode material is high, and the battery having the positive plate has excellent electrical properties such as high capacity, voltage plateau, cycle stability, and low manganese leaching.
[0011] Additional aspects and advantages of the present application will be set forth in part in the description that follows, and in part will be obvious from the description, or may be learned by practice of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following description is an exemplary embodiment of the present application, and it should be noted that those skilled in the art can make several further improvements and modifications without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
[0013] In a first aspect of the present application, a positive electrode material according to an embodiment of the present application includes a first lithium manganese iron phosphate material, a second lithium manganese iron phosphate material, a third lithium manganese iron phosphate material, a fourth lithium manganese iron phosphate material, and a fifth lithium manganese iron phosphate material, wherein the first lithium manganese iron phosphate material is an aggregate, the fourth lithium manganese iron phosphate material and the fifth lithium manganese iron phosphate material are both pseudo-single crystals, and the second lithium manganese iron phosphate material and the third lithium manganese iron phosphate material are each an aggregate and / or a pseudo-single crystal; D 50 5 <D 50 4 <D 50 3 <D 50 2 <D 50 1 The particle size relationship of D is satisfied. 50 2 =aD 50 1 , D 50 3 =bD 50 1 , D 50 4 =cD 50 1 , D 50 5 =dD 50 1 and 5 μm≦D 50 1 ≦15 μm, Here, D 50 1 ~D 50 5 are the particle diameters D of the first lithium manganese iron phosphate material to the fifth lithium manganese iron phosphate material, respectively. 50The unit is μm, the value of a is in the range of 0.35 to 0.5, the value of b is in the range of 0.2 to 0.27, the value of c is in the range of 0.17 to 0.18, and the value of d is in the range of 0.15 to 0.16; The molar ratios of manganese to iron in the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material and the fourth lithium manganese iron phosphate material increase in this order, and the molar ratio of manganese to iron in the fifth lithium manganese iron phosphate material is greater than the molar ratio of manganese to iron in the third lithium manganese iron phosphate material.
[0014] In this application, the above D 50 1 ~D 50 5 may be regarded as the particle size of each secondary particle in turn (if the LMFP pseudo-single crystal material is composed of one primary particle, it may be regarded as a "secondary particle"). Different morphologies, different particle sizes D 50 LMFP materials having different values of and Mn / Fe molar ratios affect the rate characteristics and cycle stability of the battery, the amount of Mn elution, etc. of the battery. The first lithium manganese iron phosphate material in the form of an aggregate has many grain boundaries and a large energy barrier to overcome when lithium ions diffuse into the aggregate, but the particle size of the primary particles constituting the aggregate is small, the diffusion path of lithium ions therein is short, the Mn / Fe molar ratio is the smallest, and the rate characteristics are high, and it can contribute to reducing the high degree of Mn elution due to the large specific surface area of the material. The fourth and fifth lithium manganese iron phosphate materials in the form of a pseudo single crystal have few grain boundaries and a small diffusion energy barrier, but the particle size of the primary particles is large, the diffusion path of lithium ions therein is long, and the Mn / Fe molar ratio is large, and it can maintain high structural stability and further improve the characteristics such as the voltage plateau and energy density of the battery. Therefore, the above-mentioned specific morphology requirements, D 50Due to the combined effect of the particle size requirements and the Mn / Fe molar ratio, the above five kinds of lithium manganese iron phosphate materials have basically the same charge and discharge capabilities and are all stable in structure. The batteries manufactured using the above positive electrode materials can have excellent properties such as high rate characteristics, high capacity, high cycle stability, and low manganese leaching.
[0015] In addition, the specific D 50 The particle size requirement ensures that the positive plate made of the above positive electrode materials has a good packing density. If the values of a, b, c, and d are not within the above ranges, the particle sizes of the five kinds of lithium manganese iron phosphate materials cannot be well divided, and the packing density of the plate made of them cannot be increased by multi-stage filling of LMFP materials with different particle sizes.
[0016] In one embodiment of the present application, the value range of a is 0.41≦a≦0.45, and the value range of b is 0.21≦b≦0.23. In another embodiment of the present application, a is 0.41, b is 0.23, c is 0.18, and d is 0.16.
[0017] In this application, the first lithium manganese iron phosphate material D 50 1 If the D is too small, even if the above-mentioned various different size particles are combined, the compaction density of the positive plate is still low, and the first lithium manganese iron phosphate material has a D 50 1 If D is too small, the particle size of the primary particles is smaller, the specific surface area of the first lithium manganese iron phosphate material is increased, and side reactions with the electrolyte are increased, resulting in a decrease in the structural stability of the first lithium manganese iron phosphate material during cycling, and an increase in the amount of Mn eluted. 50 1If is too large, the packing density of the positive electrode plate will decrease to a certain extent, and depending on the particle size relationship between the above particles, the particle size of the pseudo single crystal lithium manganese iron phosphate material in this case will also be large, which will lengthen the diffusion path of lithium ions in these two materials, further causing the rate characteristic of the battery to deteriorate.
[0018] In addition, "the second lithium manganese iron phosphate material and the third lithium manganese iron phosphate material are each an aggregate and / or a pseudo-single crystal" can be understood to mean that the second lithium manganese iron phosphate material is an aggregate or a pseudo-single crystal, or contains both an aggregate and a pseudo-single crystal, and similarly, the third lithium manganese iron phosphate material is an aggregate or a pseudo-single crystal, or contains both an aggregate and a pseudo-single crystal.
[0019] In the present application, the Mn / Fe molar ratios of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material and the fourth lithium manganese iron phosphate material increase in this order, the Mn / Fe molar ratios of the fourth and fifth lithium manganese iron phosphate materials are all greater than the Mn / Fe molar ratio of the third lithium manganese iron phosphate material, the Mn / Fe molar ratio of the third lithium manganese iron phosphate material is greater than the Mn / Fe molar ratio of the second lithium manganese iron phosphate material, and the Mn / Fe molar ratio of the second lithium manganese iron phosphate material is greater than the Mn / Fe molar ratio of the first lithium manganese iron phosphate material. The Mn / Fe molar ratio of the fifth lithium manganese iron phosphate material may or may not be equal to the Mn / Fe molar ratio of the fourth lithium manganese iron phosphate material.
[0020] In one embodiment of the present application, the Mn / Fe molar ratio of the first lithium manganese iron phosphate material is 1 to 1.25. The Mn / Fe molar ratio of the second lithium manganese iron phosphate material is 1.5 to 2.33. The Mn / Fe molar ratio of the third lithium manganese iron phosphate material is 2.33 to 4. The Mn / Fe molar ratios of the fourth lithium manganese iron phosphate material and the fifth lithium manganese iron phosphate material are each 4 to 9. When the Mn / Fe molar ratios of the five LMFP materials are within these ranges, the five lithium manganese iron phosphate materials have higher consistency in charge / discharge levels and higher structural stability.
[0021] In one embodiment of the present application, in the positive electrode material, the median diameter of the primary particles of the aggregates is in the range of 100 nm to 500 nm. That is, the median diameter of the primary particles of the first lithium manganese iron phosphate material is in the range of 100 nm to 500 nm, the median diameter of the primary particles of the second lithium manganese iron phosphate material in the form of aggregates is in the range of 100 nm to 500 nm, and the median diameter of the primary particles of the third lithium manganese iron phosphate material in the form of aggregates is in the range of 100 nm to 500 nm.
[0022] In the design of the same particle size of the secondary particles, on the one hand, the aggregates having a median diameter within the above median diameter range can avoid the increase in the specific surface area of the secondary particles due to the increase in the number of primary particles constituting the secondary particles of the LMFP material, and can also avoid the increase in the area where side reactions occur, and can also avoid the problem of reducing the crushing rate of the secondary particles during the compression process of the positive electrode plate, and further avoiding the generation of new interfaces and the deterioration of battery characteristics. On the other hand, the aggregates having a median diameter within the above median diameter range can shorten the diffusion path of lithium ions in the secondary particle material, thereby avoiding the problem of low capacity performance of the LMFP material, increased resistance of the battery, and reduced power characteristics. In addition, when the median diameter of the aggregates is within the above range, it is possible to avoid the increase in side reactions with the electrolyte due to the primary particles of the aggregates being too small, and further to avoid the decrease in structural stability of the aggregates and the increase in the amount of Mn elution. In addition, it is possible to optimize the diffusion path of lithium ions in the aggregates and improve the rate characteristics of the battery.
[0023] In one embodiment of the present application, the particle size of the primary particles of the pseudo single crystal is in the range of 0.5 μm to 2.5 μm. This can prevent the diffusion path of lithium ions from becoming too long due to the primary particles of the pseudo single crystal, which causes the rate characteristics of the battery to decrease. In one specific embodiment of the present application, the particle size of the primary particles of the quaternary lithium manganese iron phosphate material and the quintic lithium manganese iron phosphate material may both be in the range of 1.5 μm to 2.5 μm, the median diameter of the primary particles of the tertiary lithium manganese iron phosphate material in the pseudo single crystal form is in the range of 1.0 μm to 1.5 μm, and the median diameter of the primary particles of the tertiary lithium manganese iron phosphate material in the pseudo single crystal form is in the range of 0.5 μm to 1.0 μm. This can improve the consistency of charge and discharge of the five kinds of lithium manganese iron phosphate materials.
[0024] In the present application, the particle number ratio of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material, the fourth lithium manganese iron phosphate material, and the fifth lithium manganese iron phosphate material may be (0.8-1.2):(0.8-1.2):(1.6-2.4):(6.4-9.6):(6.4-9.6). When the particle number ratio of the five kinds of lithium manganese iron phosphate materials is within the above range, the positive electrode plate manufactured from the positive electrode material has a high compaction density (2.55 g / cm 3 In one embodiment of the present application, the particle number ratio of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material, the fourth lithium manganese iron phosphate material, and the fifth lithium manganese iron phosphate material is 1:1:2:8:8. This allows the positive electrode plate to have an extremely high compaction density (for example, about 2.9 g / cm3). 3 Furthermore, the particle mass ratio of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material, the fourth lithium manganese iron phosphate material, and the fifth lithium manganese iron phosphate material may be 100:14:2.5:0.5:0.3.
[0025] In one embodiment of the present application, the surfaces of the first to fifth lithium manganese iron phosphate materials may each have a carbon coating layer so as to improve the electrical conductivity of each of the lithium manganese iron phosphate materials.
[0026] The LMFP material in the form of aggregates can be produced by a method including the following steps (1) to (4).
[0027] In step (1), raw materials (manganese source, iron source, phosphorus source, lithium source, and carbon source) for synthesizing LMFP are mixed in a certain mass ratio, and the mixed material is wet-ground with water until the particle size of the material becomes 40 nm to 60 nm.
[0028] In step (2), the milled wet material is spray dried to obtain a dry powder.
[0029] In step (3), the dried powder is sintered in an atmosphere with an oxygen concentration of less than 150 ppm. The sintering process includes a first heating stage, a first constant temperature stage, a second heating stage, a second constant temperature stage, and a temperature decreasing stage, in which the first heating stage is a stage in which the temperature is increased from room temperature to a first constant temperature (e.g., 400°C), and the heating time may be 2.5h to 3.5h, the first constant temperature stage is a stage in which the temperature is increased from the first constant temperature (e.g., 400°C) to a second constant temperature (e.g., 700°C), and the heating time may be 2.5h to 4.0h, the second constant temperature stage is a stage in which the temperature is increased from the first constant temperature (e.g., 400°C) to a second constant temperature (e.g., 700°C), and the heating time may be 2.5h to 4.0h, the second constant temperature stage is a stage in which the temperature is decreased from the second constant temperature (e.g., 700°C) to about 50°C, and the temperature decreasing time is 5.5h to 7.5h.
[0030] In step (4), the sintered material is subjected to air-flow crushing, which may be performed at a pressure of 3 MPa to 5 MPa and for a time of 2 h to 3 h, and then sieved and classified to obtain a desired particle size D 50 A material having the formula:
[0031] In one embodiment of the present application, in the step (1), the mixing time may be 0.5 h to 1.5 h, and in another embodiment of the present application, in the step (1), the mixing time may be 0.75 h to 1.2 h.
[0032] In one embodiment of the present application, in step (1), ferric manganese phosphate may be simultaneously selected as a manganese source, an iron source, and a phosphorus source. The lithium source may include, but is not limited to, at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium dihydrogen phosphate, lithium citrate, and lithium acetate. The carbon source may include, but is not limited to, at least one of glucose, sucrose, starch, fructose, citric acid, ascorbic acid, and polyethylene glycol.
[0033] In one embodiment of the present application, in the above step (1), the material is first pulverized with a pulverizing medium having a diameter of 0.6 mm to 0.8 mm until the particle size becomes 50 μm or less, and then the material is pulverized with a pulverizing medium having a diameter of 0.1 mm to 0.3 mm until the particle size becomes 40 nm to 60 nm, In one embodiment of the present application, in step (2) above, the inlet temperature during spray drying may be 150°C to 200°C, and in another embodiment of the present application, the inlet temperature during spray drying may be 160°C to 180°C.
[0034] The manufacturing method of the pseudo single crystal LMFP material is different from the manufacturing method of the aggregate LMFP material in that the first and second constant temperature during sintering are different and the airflow crushing pressure is different.
[0035] When manufacturing a pseudo-single crystal LMFP material, in the sintering process, the first heating step is a step of heating from room temperature to a first constant temperature (e.g., 450°C), and the heating time may be 2.5h to 3.5h, and the first constant temperature step is a constant temperature time of 3.5h to 5.5h, the second heating step is a step of heating from a first constant temperature (e.g., 450°C) to a second constant temperature (e.g., 750°C), and the heating time may be 2.5h to 4.0h, and the second constant temperature step is a constant temperature time of 2.5h to 4.5h, and the temperature decreasing step is a step of decreasing the temperature from the second constant temperature (e.g., 750°C) to about 50°C), and the temperature decreasing time is 6.5h to 8.5h. When producing a LMFP material in a pseudo single crystal form, after the above sintering, air-flow crushing is performed at a pressure of 5 MPa to 8 MPa for 2 to 3 hours, and then sieving and classification are performed to obtain a material having a desired particle size.
[0036] The positive electrode slurry according to the embodiment of the present application includes the above positive electrode material, and further includes a conductive agent, a binder, and a solvent.
[0037] In a second aspect of the present application, the mass ratio of the positive electrode material, the conductive agent, and the binder is 100:(0.5-5):(0.5-5). In another embodiment of the present application, the solid content in the positive electrode slurry is 10 wt % to 80 wt %.
[0038] The conductive agent includes at least one of carbon nanotubes, carbon black, and graphene, and in another embodiment of the present application, the conductive agent includes carbon nanotubes, carbon black, and graphene, and the positive electrode material layer formed from the positive electrode slurry has high conductivity due to the ternary conductive agent. Furthermore, the mass ratio of the carbon nanotubes, the carbon black, and the graphene may be 6:5:2.
[0039] The above binder is a common choice in the field of batteries, and may be, for example, one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene butadiene rubber (SBR), polyacrylonitrile (PAN), polyimide (PI), poly(acrylic acid) (PAA), polyacrylate, polyolefin, sodium carboxymethyl cellulose (CMC) and sodium alginate. PVDF may be a copolymer of vinylidene fluoride and a polar group-containing olefin-based compound, the polar group including at least one of a carboxyl group, an epoxy group, a hydroxyl group and a sulfonic acid group, and the presence of the polar group can improve the peel strength between the positive electrode material layer formed from the positive electrode slurry and the current collector.
[0040] Such solvents are a common choice in the battery field, for example N-methylpyrrolidone (NMP).
[0041] In one embodiment of the present application, the positive electrode slurry may further include a dispersant to further improve the dispersibility and stability of the positive electrode slurry. The dispersant may be polyvinylpyrrolidone (PVP), etc.
[0042] When preparing the above positive electrode slurry, the first LMFP material, the second LMFP material, and the third LMFP material, which have larger particle sizes, are added in their powder form, thereby preventing settling from occurring during mixing, and the fourth LMFP material and the fifth LMFP material, which have smaller particle sizes, may be added in their powder form or in their slurry form, and each of the slurries may contain a dispersant, such as PVP, in addition to the organic solvent.
[0043] In a third aspect of the present application, a positive electrode plate according to the embodiment of the present application includes a current collector and a positive electrode material layer disposed on the current collector, the positive electrode material layer including the positive electrode material or the positive electrode slurry being applied to the current collector, thereby the positive electrode plate containing the positive electrode material has a high compaction density.
[0044] The positive electrode material layer further contains a conductive agent and a binder in addition to the positive electrode material, and is formed by applying the positive electrode slurry to a current collector.
[0045] In a fourth aspect of the present application, a battery according to the present embodiment includes the positive electrode plate, and the battery has excellent electrical properties such as high capacity, low probability of manganese elution, and high cycle stability.
[0046] The present application will now be further described with reference to several examples.
[0047] Regarding the production of positive electrode materials, The first LMFP material to the fifth LMFP material that satisfy the above morphology requirements are referred to as particle 1, particle 2, particle 3, particle 4, and particle 5, respectively, and five types of particles are selected and mixed based on the particle size, quantity, and Mn / Fe molar ratio in Table 1 to obtain positive electrode materials corresponding to different embodiments.
[0048] The measurement methods for each item of each LMFP material are as follows.
[0049] Regarding the method for measuring the particle size of each LMFP material, a laser particle sizer is used as the measuring device, and the standard model is Malvern 2000 / 3000. The measurement method is to disperse each LMFP material in deionized water, ultrasonicate for 10 minutes, set the refractive index of the particles to 1.74, and measure the particle size D of each LMFP material. 50 The aim is to obtain
[0050] The method for measuring the number of particles of LMFP materials with different particle sizes is to make the LMFP materials with different particle sizes approximately spherical, and measure the particle size D 50 and volume density (approx. 3.6 g / cm 3 The method involves calculating the mass of the individual spheres based on the mass of the LMFP material. By controlling the feed mass of the LMFP material with different particle sizes, the number of particles of the LMFP material with different particle sizes is controlled.
[0051] The median diameter of the primary particles of each LMFP material (particle size D 50The measurement method for LMFP material is to take a photograph of each LMFP material at 10,000 times magnification using a scanning electron microscope (SEM), artificially measure the size of approximately 300 primary particles, and create a number distribution to obtain the median diameter of the primary particles.
[0052] For the Mn / Fe molar ratio of each LMFP material, 0.2000g of each LMFP particle is weighed, and analytically pure commercially available hydrochloric acid and nitric acid are added and heated to decompose (the decomposition solution is prepared by taking 1mL of a mixture of commercially available concentrated hydrochloric acid and water with a volume ratio of 1:1 and mixing it with 3mL of commercially available concentrated nitric acid), filtered through filter paper, and the filter paper is rinsed with deionized water at least three times to ensure that the ions are sufficiently contained in the filtrate, and then the volume is adjusted to 100ml. The ion concentrations of Fe and Mn are measured and detected according to GB / T9723-2007 Chemical Reagents: General Principles of Flame Atomic Absorption Spectroscopy (AAS), and the Mn / Fe molar ratio is calculated.
[0053] For the preparation of the positive electrode slurry, a certain ratio of organic solvent NMP and binder PVDF are added to a stirrer, stirred for 1 h, then a conductive agent (specifically, a mixture of carbon tubes, carbon black and graphene with a mass ratio of 0.6:0.5:0.3) is added, stirred for 30 min, particles 1, particles 2 and particles 3 are added in their respective powder forms, stirred for 1.5 h, then a PVP-containing NMP slurry of particles 4 and particles 5 is added, stirred for 1.5 h, and sieved to obtain a positive electrode slurry. In the positive electrode slurry, the mass ratio of the positive electrode material composed of particles 1 to 5, the conductive agent, the binder PVDF and the organic solvent NMP is 100:2:2:30.
[0054] For the preparation of the positive plate, the positive electrode slurry corresponding to each embodiment is applied to both sides of the aluminum foil, respectively, and then dried, and a positive electrode material layer is formed on the aluminum foil to obtain an uncompressed positive plate, and the uncompressed positive plate is cut to a size of 40×100 mm and compressed by a large hydraulic press to obtain a compressed positive plate. Based on the areal density of the positive plate and the thickness after compression, the compaction density of the positive plate is calculated, and the results are summarized in Table 2.
[0055] For the manufacture of the battery, the positive electrode slurry corresponding to each example was mixed with a surface density of 2.0 g / dm 2 The compaction density is 2.65g / cm 3 Each single-sided positive plate is then used to manufacture a 2025 button battery.
[0056] First, the positive electrode slurry corresponding to each example was prepared so that the surface density was 4.0 g / dm 2 The compaction density is 2.65g / cm 3 The positive electrode plate is manufactured on both sides, and the surface density is 2.1g / dm 2 and the compaction density is 1.60g / cm 3 Provide a double-sided negative electrode plate of 0.5 mm and use a PP film as a separator to assemble a 053450 full battery.
[0057] The specific capacity of each button battery was measured, and the median voltage of each battery, the rate characteristics, and the amount of Mn eluted from the negative electrode during cycling were measured. The results are summarized in Table 2.
[0058] The method for measuring the specific capacity was to charge the button battery corresponding to each Example with constant current-constant voltage (CC-CV) at 0.1C until the voltage reached 4.3V and the off current reached 0.05C, and then discharge the battery with constant current-constant voltage at 0.1C until the voltage reached 2.5V. This charge-discharge cycle was repeated three times, and the discharge capacity after the third cycle was taken and divided by the amount of the positive electrode material layer applied to the positive electrode plate to calculate the specific capacity of the battery.
[0059] The median voltage refers to the discharge voltage corresponding to half the discharge capacity in the discharge curve of the battery at 1 / 3 C. The method for measuring the median voltage is to charge all the batteries corresponding to each example at 1 / 3 C with constant current-constant voltage (CC-CV) until the voltage becomes 4.3 V and the off current becomes 0.05 C, and then discharge at 1 / 3 C with constant current-constant voltage (CC-CV) until the voltage becomes 2.5 V, and plot the discharge curve of voltage vs. capacity to find the median voltage.
[0060] The method for measuring the rate characteristics was to charge all batteries corresponding to each Example at a constant current of 0.2C to 4.2V at 25°C, and then discharge them at constant currents of 0.2C and 5C to 2.5V, respectively, calculate the ratio of the discharge capacity at 5C to the discharge capacity at 0.2C, and use this value to evaluate the rate characteristics of the battery.
[0061] The method for measuring the amount of Mn eluted from the negative electrode was to charge all the batteries corresponding to each Example at 45° C. to 4.3 V at 1 C with a constant current and discharge to 2.5 V at 1 C with a constant current. After 500 charge / discharge cycles were performed in this manner, the batteries were disassembled and the Mn content in the negative electrode material of the negative electrode plate was measured. The Mn content was measured by an inductively coupled plasma emission spectrometer (ICP).
[0062] In addition, in order to highlight the beneficial effects of the technical means of the present application, the positive electrode materials of Comparative Examples 1 to 7 are further provided, and the parameters of each LMFP material used therein are summarized in Table 1.
[0063] [Table 1]
[0064] [Table 2] [Table 3] [Table 4]
[0065] As can be seen from Tables 1 and 2, in the positive electrode materials of Examples 1 to 13, when the particle morphology, particle size relationship, and Mn / Fe ratio magnitude relationship all satisfy the requirements described in the present application, the compaction density of the positive electrode plate is 2.65 g / cm 3 Up to 2.86g / cm 3The specific capacity of the battery is basically not significantly decreased, so the battery has a high energy density. In addition, the positive electrode material of each embodiment can provide the battery with a high median voltage, high rate characteristics, and excellent cycle characteristics. For example, the battery manufactured with the positive electrode material of each embodiment has excellent rate characteristics, and the ratio of the discharge capacity at 5C and 0.2C is 84% or more and can reach 91%, which indicates that the continuous output characteristics of the battery are high. After the battery is cycled 500 times at 45°C, the amount of Mn eluted from the negative electrode is low, less than 500 ppm.
[0066] In addition, as can be seen from the comparison between Comparative Examples 1 and 2 and Example 1, the particle diameters D 50 If the ratios a, b, c, and d are not within the above-defined ranges, the packing density of the electrode plate produced therewith will be significantly reduced. As can be seen from a comparison between Comparative Examples 3 to 5 and Example 1, if the particle number ratios of these five types of LMFP materials are not within the above-defined ranges, the packing density of the electrode plate will be significantly reduced. As can be seen from a comparison between Comparative Example 7 and Example 1, if the Mn / Fe molar ratios of the first LMFP material to the fifth LMFP material do not satisfy the magnitude relationship defined in this application, the rate characteristics of the battery will be clearly reduced and the amount of Mn eluted from the negative electrode will be significantly increased.
[0067] The above examples merely illustrate some embodiments of the present application, and although the description is specific and detailed, it should not be understood as limiting the scope of the claims of the present application. However, those skilled in the art can make some further modifications and improvements without departing from the concept of the present application, and all of these fall within the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of the attached claims.
Claims
1. the first lithium manganese iron phosphate material is an aggregate, the fourth lithium manganese iron phosphate material and the fifth lithium manganese iron phosphate material are both pseudo-single crystals, and the second lithium manganese iron phosphate material and the third lithium manganese iron phosphate material are each an aggregate and / or a pseudo-single crystal; D 50 5 <D 50 4 <D 50 3 <D 50 2 <D 50 1 and D 50 2 = aD 50 1 , D 50 3 = bD 50 1 , D 50 4 = CD 50 1 , D 50 5 =dd 50 1 and 5 μm≦D 50 1 ≦15 μm, Here, the D 50 1 ~D 50 5 are the particle diameters D of the first lithium manganese iron phosphate material to the fifth lithium manganese iron phosphate material, 50 The value of a is in the range of 0.35 to 0.5, the value of b is in the range of 0.2 to 0.27, the value of c is in the range of 0.17 to 0.18, and the value of d is in the range of 0.15 to 0.16, the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material and the fourth lithium manganese iron phosphate material have a molar ratio of manganese to iron increasing in this order, and the fifth lithium manganese iron phosphate material has a molar ratio of manganese to iron greater than the molar ratio of manganese to iron in the third lithium manganese iron phosphate material; a particle number ratio of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material, the fourth lithium manganese iron phosphate material, and the fifth lithium manganese iron phosphate material is (0.8 to 1.2):(0.8 to 1.2):(1.6 to 2.4):(6.4 to 9.6):(6.4 to 9.6).
2. 2. The cathode material of claim 1, wherein the first lithium manganese iron phosphate material has a molar ratio of manganese to iron in the range of 1 to 1.25, the second lithium manganese iron phosphate material has a molar ratio of manganese to iron in the range of 1.5 to 2.33, the third lithium manganese iron phosphate material has a molar ratio of manganese to iron in the range of 2.33 to 4, and the fourth lithium manganese iron phosphate material and the fifth lithium manganese iron phosphate material each have a molar ratio of manganese to iron in the range of 4 to 9.
3. The positive electrode material according to claim 1 or 2, wherein the value of a is in the range of 0.41 to 0.45, and the value of b is in the range of 0.21 to 0.
23.
4. The positive electrode material according to any one of claims 1 to 3, wherein a is 0.41, b is 0.23, c is 0.18, and d is 0.
16.
5. The positive electrode material according to any one of claims 1 to 4, wherein a particle number ratio of the first lithium manganese iron phosphate material, the second lithium manganese iron phosphate material, the third lithium manganese iron phosphate material, the fourth lithium manganese iron phosphate material, and the fifth lithium manganese iron phosphate material is 1:1:2:8:
8.
6. The positive electrode material according to any one of claims 1 to 5, wherein the median diameter of the primary particles of the aggregates is in the range of 100 nm to 500 nm.
7. A positive electrode plate comprising a current collector and a positive electrode material layer disposed on the current collector, the positive electrode material layer comprising the positive electrode material according to any one of claims 1 to 6.
8. A battery comprising the positive plate of claim 7.
Citation Information
Patent Citations
Composite cathode material, cathode sheet, preparation method of cathode sheet, and lithium ion battery
CN109962221A
Lithium ion secondary battery and manufacturing method for the same
JP2012212663A
Composition for forming lithium secondary battery electrode, electrode for secondary battery
JP2013232313A
Positive electrode for secondary battery and secondary battery including the same
JP2016530684A
Cathode materials containing olivine structured nanocomposites
US20170170479A1