Ultra-high strength cold-rolled steel sheet with excellent bending workability and its manufacturing method
A tailored alloy composition and manufacturing process for cold-rolled steel sheets achieve high strength and ductility, addressing the challenges of ultra-high-strength steel sheets by ensuring a balanced microstructure for improved bending workability and weldability.
Patent Information
- Application Number
- JP2023532517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-03
- Filing Date
- 2021-11-29
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2041-11-29
AI Technical Summary
Existing ultra-high-strength cold-rolled steel sheets face challenges in achieving both high tensile strength of 980 MPa or more and excellent bending workability, particularly in 180° full crimp bending tests, due to issues with microstructure control and composition, leading to poor weldability and increased manufacturing costs.
A specific alloy composition and controlled manufacturing process involving continuous annealing, cooling rates, and overaging treatments to achieve a microstructure of 80-98% tempered martensite, balanced with fresh martensite, bainite, and ferrite, with controlled lath sizes and cooling rates to ensure high strength and ductility.
The solution results in a steel sheet with yield strength of 780-920 MPa, tensile strength of 980-1200 MPa, elongation of 8% or more, and excellent bending workability, meeting the stringent requirements of automotive applications without cracking.
Smart Images

Figure 0007576704000005 
Figure 0007576704000006 
Figure 0007576704000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an ultra-high strength cold-rolled steel sheet having excellent bending workability and a manufacturing method thereof, and more particularly to an ultra-high strength cold-rolled steel sheet having excellent bending workability that can be used for automobiles and a manufacturing method thereof. [Background technology]
[0002] Recently, the strengthening of safety regulations for passengers and pedestrians has led to the obligation to build safety devices, which is a contradictory issue in terms of weight reduction for improving fuel efficiency. Consumers are increasingly interested in hybrid and electric vehicles, which are environmentally friendly and highly fuel-efficient. In order to produce such environmentally friendly and safe vehicles, the weight of the body structure must be reduced and the stability of the body material must be ensured. However, hybrid vehicles are equipped with various devices such as electric engines, electric batteries, and secondary fuel storage tanks in addition to the existing gasoline engine. In addition, as driver comfort continues to improve, the weight of the body increases. Therefore, in order to reduce the weight of the body, it is essential to develop materials that are thin yet have excellent strength, ductility, and bending properties. Therefore, in order to solve this problem, it is necessary to develop giga-class steel sheets that can ensure high strength and high ductility, such as a tensile strength of 980 MPa or more.
[0003] Meanwhile, structural or reinforcing materials protect passengers by absorbing the energy of a collision, but if the strength of the spot welds is insufficient, they will break during a collision and will not be able to absorb enough energy. In addition, most of the parts to which such ultra-high strength steel is mainly applied require bending processing, such as side sills, so even if the elongation is excellent, if the bendability is poor, it cannot be used as a part. Bending workability refers to the minimum bending radius ratio (R / t) per unit thickness, where the minimum bending radius ratio (R) refers to the minimum radius at which cracks do not occur in the outer winding part of the steel sheet after bending test. The requirements for bending workability vary slightly depending on the automobile company, but according to a Japanese automobile company that requires the strictest standard, it requires that R / t≦1 be met for cold-rolled steel sheets with a tensile strength of 980 MPa. However, some customers require not only R / t but also 180° full crimp bending properties to reduce the risk of processing cracks and for excellent bending workability, but in reality it is very difficult to secure these properties with ultra-high strength steel sheets with tensile strengths of 980 MPa or more.Therefore, there is a pressing need to develop ultra-high strength steel sheets with tensile strengths of 980 MPa or more that have high yield strength and excellent bending workability.
[0004] In order to improve bending workability, it is necessary to properly control the composition and fraction of the transformation phases present in the steel material. It is generally known that the lower the strength ratio between the soft phase such as ferrite (F) and the hard phase such as bainite (B) or martensite (M), the better the bending workability. To achieve this, bainite or tempered martensite must be generated instead of martensite, but since such transformation phases have the problem of significantly reducing elongation, it is most important to properly ensure the composition ratio of the transformation phases.
[0005] A conventional technique for improving the workability of the high-tensile steel sheet is disclosed in Patent Document 1. Patent Document 1 relates to a steel sheet having a composite structure mainly composed of tempered martensite, and is characterized in that fine precipitated Cu particles having a particle size of 1 to 100 nm are dispersed inside the structure in order to improve the workability. However, Patent Document 1 has a problem in that the Cu content is excessively increased to 2 to 5% in order to precipitate good fine Cu particles, which may cause red brittleness due to Cu, and also excessively increases the manufacturing cost.
[0006] A typical manufacturing method for increasing the yield strength is to use water cooling during continuous annealing. Heating After that, the steel sheet is immersed in water and tempered to produce a steel sheet in which the microstructure is transformed from martensite to tempered martensite. Patent Document 2 is a representative prior art of such a method. Patent Document 2 relates to a technique for producing a steel material having a martensite volume fraction of 80 to 97% and the remainder being ferrite by continuously annealing a steel material having a carbon content of 0.18 to 0.3%, water cooling to room temperature, and then performing overaging treatment at a temperature of 120 to 300°C for 1 to 15 minutes. When ultra-high strength steel is produced by the tempering method after water cooling in this way, the yield ratio is very high, but there is a problem that the shape quality of the coil deteriorates due to temperature deviations in the width and length directions. Therefore, in order to solve such problems and at the same time ensure an appropriate microstructure, precise control of the temperature and cooling conditions during continuous annealing is required.
[0007] Meanwhile, Patent Document 3 proposes a steel sheet having a fine structure containing 2-10% by area of pearlite in a ferrite matrix, and improved strength by precipitation strengthening and grain refinement mainly by adding carbonitride forming elements such as Ti. Patent Document 3 has the advantage of being able to easily obtain high strength at low manufacturing costs, but has the disadvantage that high-temperature annealing must be performed to cause sufficient recrystallization and ensure ductility, since the recrystallization temperature rises sharply due to fine precipitates. In addition, the existing precipitation strengthened steel, which is strengthened by precipitating carbonitrides in a ferrite matrix, has the problem that it is difficult to obtain high-strength steel of 600 MPa class or more.
[0008] Therefore, there is a demand for development of an ultra-high strength steel material having a tensile strength of 980 MPa or more, which solves the above-mentioned problems and has a high yield ratio and allows cold forming without cracking even in a 180° full crimp bending test. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2005-264176 A [Patent Document 2] Patent No. 2528387 [Patent Document 3] Korean Patent Publication No. 2015-0073844 Summary of the Invention [Problem to be solved by the invention]
[0010] One aspect of the present invention provides an ultra-high strength cold rolled steel sheet having excellent bending workability and a method for producing the same. [Means for solving the problem]
[0011] One embodiment of the present invention provides an ultra-high strength cold rolled steel sheet having excellent bending workability, which contains, by weight %, 0.06-0.17% C, 0.1-0.8% Si, 1.9-2.9% Mn, 0.005-0.07% Nb, 0.004-0.05% Ti, 0.0004-0.005% B, 0.20% or less (excluding 0%) Cr, 0.04-0.45% Mo, the balance being Fe and other unavoidable impurities, and satisfies the following relational expressions 1-3, and the microstructure contains, by area %, 80-98% tempered martensite, the balance being fresh martensite, bainite, ferrite and retained austenite, and the average length of the lath minor axis of the tempered martensite is 500 nm or less. [Relational expression 1]0.40≦C+Mn / 6+(Cr+Mo+V) / 5+(Si+Ni+Cu) / 15≦0.70 [Relationship 2] 110≦48.8+49logC+35.1Mn+25.9Si+76.5Cr+105.9Mo+1325Nb≦210 [Relationship 3] 0.20≦Mo+200B≦0.70 (However, the contents of the alloy components shown in the above Relational Formulas 1 to 3 are expressed in terms of weight percent.)
[0012] Another embodiment of the present invention is a method for producing a slab containing, by weight percent, 0.06-0.17% C, 0.1-0.8% Si, 1.9-2.9% Mn, 0.005-0.07% Nb, 0.004-0.05% Ti, 0.0004-0.005% B, 0.20% or less (excluding 0%) Cr, 0.04-0.45% Mo, the balance being Fe and other unavoidable impurities, and which satisfies the following relations 1 to 3: The heated slab is finish-rolled so that the finish rolling exit temperature is Ar3+50°C to Ar3+150°C to obtain a hot-rolled steel sheet; the hot-rolled steel sheet is cooled to Ms+50°C to Ms+300°C and then coiled; the coiled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet; the cold-rolled steel sheet is continuously annealed in a temperature range of 820 to 860°C; and the continuously annealed cold-rolled steel sheet is heated for 50 to 200 seconds. Heating The processing step; Heatingthe step of primarily cooling the treated cold-rolled steel sheet to 620-700°C at a cooling rate of 1-10°C / s; the step of secondarily cooling the primarily-cooled cold-rolled steel sheet to 360-420°C at a cooling rate of 5-50°C / s; and the step of overaging the secondarily-cooled cold-rolled steel sheet at 370-420°C or overaging after reheating, wherein during the secondary cooling and overaging treatment, the following relational expressions 4 to 8 are satisfied. [Relational expression 1]0.40≦C+Mn / 6+(Cr+Mo+V) / 5+(Si+Ni+Cu) / 15≦0.70 [Relationship 2] 110≦48.8+49logC+35.1Mn+25.9Si+76.5Cr+105.9Mo+1325Nb≦210 [Relationship 3] 0.20≦Mo+200B≦0.70 [Relationship 4] 0≦A≦50 [Relationship 5] 0≦B≦40 [Relationship 6] 0≦2.8A+0.5B≦100 [Relationship 7] 0≦3.1A+2.3B≦200 [Relational expression 8]0.25≦(3.1A+2.3B) / (2.8A+0.5B)≦3.5 (Note that the contents of the alloy components in the above relational expressions 1 to 3 are expressed in terms of weight percent, and in the above relational expressions 4 to 8, A is Ms-secondary cooling end temperature (°C), and B is overaging treatment temperature-secondary cooling end temperature (°C).) Effect of the Invention
[0013] According to one aspect of the present invention, there is provided an ultra-high strength cold rolled steel sheet having excellent bending workability and a method for producing the same. [Brief description of the drawings]
[0014] [Figure 1] 1 is a microstructure photograph of Example 1 according to an embodiment of the present invention, observed using a SEM. [Diagram 2] 1 is a microstructure photograph of Example 1 according to an embodiment of the present invention, observed using a TEM. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an ultra-high strength cold rolled steel sheet having excellent bending workability according to one embodiment of the present invention will be described. First, the alloy composition of the present invention will be described. The content of the alloy composition described below means weight % unless otherwise specified.
[0016] C: 0.06-0.17% Carbon (C) is a very important element added for solid solution strengthening. Carbon also contributes to improving strength by combining with precipitated elements to form fine carbides. If the C content is less than 0.06%, it is very difficult to ensure the desired strength. On the other hand, if the C content exceeds 0.17%, the strength may increase rapidly and bending workability may decrease as martensite is excessively formed during cooling due to an increase in hardening ability. In addition, the weldability is poor, so that welding defects are more likely to occur during part processing at customer companies. Therefore, the C content is preferably in the range of 0.06-0.17%. The lower limit of the C content is more preferably 0.08%, and even more preferably 0.10%. The upper limit of the C content is more preferably 0.165%, even more preferably 0.16%, and most preferably 0.145%.
[0017] Si: 0.1-0.8% Silicon (Si) is one of the five major elements of steel, and a small amount is naturally added during the manufacturing process. The above-mentioned Si contributes to increasing strength and suppresses the formation of carbides during annealing. HeatingIt prevents carbon from being generated as carbide during processing and cooling. In addition, this carbon is distributed and accumulated in the retained austenite, so that the austenite phase remains at room temperature, which is advantageous for ensuring elongation. If the Si content is less than 0.1%, it may be difficult to sufficiently ensure the above-mentioned effects. On the other hand, if the Si content exceeds 0.80%, it may cause surface scale defects, degrade the plating surface quality, and reduce the chemical conversion treatability. Therefore, the Si content is preferably in the range of 0.1 to 0.8%. The lower limit of the Si content is more preferably 0.2%, and even more preferably 0.3%. The upper limit of the Si content is more preferably 0.7%, and even more preferably 0.6%.
[0018] Mn: 1.9-2.9% Manganese (Mn) is an element that completely precipitates sulfur in steel into MnS to prevent hot brittleness due to the formation of FeS, and also solid-solution strengthens steel. If the Mn content is less than 1.9%, it is difficult to ensure the strength targeted in the present invention. On the other hand, if the Mn content exceeds 2.9%, problems such as weldability and hot rolling are likely to occur, and at the same time, the hardening ability may be increased to form martensite more excessively, resulting in a decrease in elongation. In addition, there is a problem that Mn-Bands (bands of Mn oxides) are formed in the microstructure, increasing the risk of processing cracks and sheet breakage, and there is a problem that Mn oxides dissolve on the surface during annealing, greatly impairing galvanic properties. Therefore, the Mn content is preferably in the range of 1.9-2.9%. The lower limit of the Mn content is more preferably 2.0%, and even more preferably 2.1%. The upper limit of the Mn content is more preferably 2.8%, and further preferably 2.7%.
[0019] Nb: 0.005-0.07% Niobium (NB) is an element that segregates at the austenite grain boundary, suppresses the coarsening of austenite grains during annealing heat treatment, and forms fine carbides to contribute to increasing strength. When the Nb content is less than 0.005%, the above-mentioned effects are insufficient. On the other hand, when the Nb content exceeds 0.07%, coarse carbides precipitate, and the amount of carbon dissolved in the steel is reduced, which may result in a decrease in strength and elongation, resulting in an increase in manufacturing costs. Therefore, the Nb content is preferably in the range of 0.005-0.07%. The lower limit of the Nb content is more preferably 0.01%, and even more preferably 0.015%. The upper limit of the Nb content is more preferably 0.06%, and even more preferably 0.05%.
[0020] Ti: 0.004-0.05% Titanium (Ti) is an element for forming fine carbides, and contributes to ensuring yield strength and tensile strength. In addition, Ti is an element for forming nitrides, and has the effect of precipitating N in steel as TiN and suppressing AlN precipitation, which has the advantage of reducing the risk of cracks occurring during continuous casting. If the Ti content is less than 0.004%, it may be difficult to obtain the above-mentioned effects. On the other hand, if the Ti content exceeds 0.05%, coarse carbides are precipitated, and the strength and elongation may be reduced due to the reduction in the amount of solid-solubilized carbon in the steel, which may cause nozzle clogging during continuous casting. Therefore, the Ti content is preferably in the range of 0.004-0.05%. The lower limit of the Ti content is more preferably 0.008%, and even more preferably 0.012%. The upper limit of the Ti content is more preferably 0.04%, and even more preferably 0.03%.
[0021] B: 0.0004-0.005% Boron (B) is an element that contributes greatly to ensuring the hardenability of steel materials, and in order to obtain such an effect, it is preferable to add 0.0004% or more. However, if the content of B exceeds 0.005%, boron carbide is formed at the grain boundary to provide a nucleation site for ferrite, which may actually deteriorate the hardenability. Therefore, the content of B is preferably in the range of 0.0004-0.005%. The lower limit of the content of B is more preferably 0.0006%, and even more preferably 0.0008%. The upper limit of the content of B is more preferably 0.004%, and even more preferably 0.003%.
[0022] Cr: 0.20% or less (excluding 0%) Chromium (Cr) is an element that improves hardenability and increases the strength of steel. However, if the Cr content exceeds 0.2%, a penetration corrosion problem may occur due to non-uniform generation of Cr oxide in a salt water atmosphere. Therefore, the Cr content is preferably in the range of 0.20% or less. The Cr content is more preferably 0.15% or less, and even more preferably 0.10% or less. Meanwhile, in the present invention, since the hardenability and strength improving effect can be obtained even with a small amount, the lower limit of the Cr is not particularly limited.
[0023] Mo: 0.04-0.45% Molybdenum (Mo) is an element that forms carbides, and when added in combination with carbonitride forming elements such as Ti, Nb, and V, it plays a role in maintaining the size of precipitates fine and improving yield strength and tensile strength. In addition, Mo has the advantage of improving the hardening ability of steel and forming fine martensite at grain boundaries, making it possible to control the yield ratio. In order to achieve the above effects, it is preferable that Mo is added in an amount of 0.04% or more. However, since Mo is an expensive element, the higher its content, the more disadvantageous it is in manufacturing, so it is preferable to appropriately control its content. If the Mo content exceeds 0.45%, not only does it cause a sharp increase in manufacturing cost, which reduces the economic efficiency, but also causes a problem of reducing the ductility of the steel due to the excessive grain refinement effect and solid solution strengthening effect. Therefore, the Mo content is preferably in the range of 0.04-0.45%. The lower limit of the Mo content is more preferably 0.06%, and even more preferably 0.08%.The upper limit of the Mo content is more preferably 0.40%, and even more preferably 0.35%.
[0024] On the other hand, the cold-rolled steel sheet of the present invention preferably satisfies the above-mentioned alloy components and also satisfies the following relations 1 to 3. This makes it possible to produce an ultra-high strength steel sheet having an excellent bending workability and a tensile strength of 980 MPa or more, which is the target of the present invention.
[0025] [Relational expression 1]0.40≦C+Mn / 6+(Cr+Mo+V) / 5+(Si+Ni+Cu) / 15≦0.70 The above-mentioned relational formula 1 is a component relational formula for ensuring strength and weldability. If the value of the above-mentioned relational formula 1 is less than 0.40, it is difficult to ensure the material and weld strength targeted by the present invention, and if it exceeds 0.70, the weldability may be poor. Therefore, the value of the above-mentioned relational formula 1 is preferably in the range of 0.40 to 0.70. The lower limit of the value of the above-mentioned relational formula 1 is more preferably 0.45, and even more preferably 0.50. The upper limit of the value of the above-mentioned relational formula 1 is more preferably 0.68, and even more preferably 0.65.
[0026] [Relationship 2] 110≦48.8+49logC+35.1Mn+25.9Si+76.5Cr+105.9Mo+1325Nb≦210 The above-mentioned relational expression 2 is a component relational expression related to the hardenability index for ensuring hardenability. If the value of the above-mentioned relational expression 2 is less than 110, it is difficult to ensure the strength targeted in the present invention due to insufficient hardenability, and if it exceeds 210, the hardenability may be excessively high, resulting in poor bending workability. Therefore, the value of the above-mentioned relational expression 2 is preferably in the range of 100 to 200. The lower limit of the value of the above-mentioned relational expression 2 is more preferably 120, and even more preferably 130. The upper limit of the value of the above-mentioned relational expression 2 is more preferably 200, and even more preferably 190.
[0027] [Relationship 3] 0.20≦Mo+200B≦0.70 The above-mentioned relational formula 3 is a component relational formula for more stably securing the strength targeted by the present invention. If the value of the above-mentioned relational formula 3 is less than 0.20, it is difficult to secure the strength targeted by the present invention due to insufficient hardening ability, and if it exceeds 0.70, there is a drawback that not only the hardening ability is excessively high, resulting in poor bending workability, but also an increase in manufacturing costs. Therefore, the value of the above-mentioned relational formula 3 is preferably in the range of 0.20 to 0.70. The lower limit of the value of the above-mentioned relational formula 3 is more preferably 0.25, and even more preferably 0.30. The upper limit of the value of the above-mentioned relational formula 3 is more preferably 0.65, and even more preferably 0.60.
[0028] The remaining component of the present invention is iron (Fe). However, in normal manufacturing processes, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and this cannot be excluded. Since these impurities are known to anyone skilled in normal manufacturing processes, the contents of all of them are not specifically mentioned in this specification.
[0029] Meanwhile, the above impurities include one or more of P, S, Al, Sb, N, Mg, Sn, Sb, Zn, and Pb as tramp elements, and the total amount of the tramp elements may be 0.1% by weight or less. Tramp elements are impurity elements such as scrap used as raw materials in the steelmaking process, and if the total amount of the tramp elements exceeds 0.1%, it may cause surface cracks in the slab and may deteriorate the surface quality of the steel plate.
[0030] Hereinafter, the microstructure and the like of the ultra-high strength cold rolled steel sheet with excellent bending workability according to one embodiment of the present invention will be described.
[0031] The microstructure of the cold-rolled steel sheet of the present invention preferably includes, in terms of area %, 80 to 98% tempered martensite, and the remainder fresh martensite, bainite, ferrite, and retained austenite. The microstructure of the cold-rolled steel sheet of the present invention includes tempered martensite (hereinafter also referred to as "TM") as a main structure. However, if the fraction of the tempered martensite is less than 80%, it is difficult to ensure the target strength, and if it exceeds 98%, bending workability and elongation may decrease. Therefore, the fraction of the martensite is preferably in the range of 80 to 98%. The lower limit of the fraction of the martensite is more preferably 82%, and even more preferably 84%. The upper limit of the fraction of the martensite is more preferably 97%, and even more preferably 96%. The remaining structures, fresh martensite (hereinafter also referred to as "FM"), bainite (hereinafter also referred to as "B"), ferrite (hereinafter also referred to as "F"), and retained austenite (hereinafter also referred to as "RA"), are microstructures that are inevitably formed during the manufacturing process. However, the remaining structure may also play a positive role in the present invention. The fresh martensite is an advantageous structure for ensuring strength. Thus, the higher the fraction of fresh martensite, the more advantageous it is for ensuring strength, but if it exceeds 11%, the elongation and bending workability may decrease. Therefore, the fraction of fresh martensite is preferably 11% or less. The fraction of fresh martensite is more preferably 10% or less, even more preferably 9% or less, and most preferably 8% or less.
[0032] The bainite can play an important role in improving bending properties by contributing to a reduction in the hardness difference between phases. However, if the fraction exceeds 3%, the fraction of martensite is relatively reduced, making it difficult to ensure the target strength. The ferrite is a structure that is advantageous for ensuring elongation. However, if the fraction exceeds 3%, the fraction of martensite is relatively reduced, making it possible that it is difficult to ensure the target strength. The retained austenite is a structure that is advantageous for ensuring elongation. However, if the fraction exceeds 3%, the fraction of martensite is relatively reduced, making it possible that it is difficult to ensure the target strength. Therefore, it is preferable that the fractions of the bainite, ferrite, and retained austenite are each 3% or less.
[0033] On the other hand, the average length of the lath minor axis of the tempered martensite is preferably 500 nm or less. The narrower the lath spacing of the tempered martensite, the more advantageous it is in terms of ensuring strength and bending workability. However, if the average length of the lath minor axis of the tempered martensite exceeds 500 nm, it is difficult to obtain the above effect. The average length of the lath minor axis is more preferably 400 nm or less, and even more preferably 300 nm or less.
[0034] The cold-rolled steel sheet of the present invention provided as described above can have a yield strength (YS): 780 to 920 MPa, a tensile strength (TS): 980 to 1200 MPa, an elongation (EL): 8% or more, a yield ratio (YS / TS): 0.75 or more, a hole expansion ratio (HER): 40% or more, and a bending workability (YS x EL x HER): 300 GPa%% or more, and has the advantage that no cracks occur during a 180° full crimp bending test. The yield strength is more preferably 790 to 910 MPa, and even more preferably 800 to 900 MPa. The tensile strength is more preferably 990 to 1180 MPa, and even more preferably 1000 to 1160 MPa. The elongation is more preferably 9% or more, and even more preferably 10% or more. The yield ratio is more preferably 0.76 or more, and even more preferably 0.77 or more. The hole expansion ratio is more preferably 45% or more, and even more preferably 50% or more. The bending workability is more preferably 350 GPa% or more, and further preferably 400 GPa% or more. Meanwhile, the 180° full crimp bending test can be performed by first bending the steel sheet to be measured by 90°, then sandwiching another steel sheet having twice the thickness of the steel sheet, and then bending the steel sheet to be measured by 180° again to perform full crimping.
[0035] Hereinafter, a method for producing an ultra-high strength cold rolled steel sheet having excellent bending workability according to one embodiment of the present invention will be described.
[0036] First, a slab satisfying the above-mentioned alloy composition is heated. In the present invention, the slab heating temperature is not particularly limited, but for example, the slab heating can be performed at 1100 to 1300°C. If the slab heating temperature is less than 1100°C, the slab temperature is low and a rolling load may occur during rough rolling, and if it exceeds 1300°C, the structure may become coarse, and there may be disadvantages such as an increase in power costs. The lower limit of the slab heating temperature is more preferably 1125°C, and more preferably 1150°C. The upper limit of the slab heating temperature is more preferably 1275°C, and more preferably 1250°C. Meanwhile, the slab may have a thickness of 230 to 270 mm.
[0037] Thereafter, the heated slab is finish-rolled so that the finish rolling exit temperature is Ar3+50°C to Ar3+150°C to obtain a hot-rolled steel sheet. If the finish rolling exit temperature is less than Ar3+50°C, there is a high possibility that the hot deformation resistance will increase rapidly. If the finish rolling exit temperature exceeds Ar3+150°C, there is a high possibility that not only an excessively thick oxide scale will be generated but also the microstructure of the steel sheet will become coarse. Therefore, the finish rolling exit temperature is preferably in the range of Ar3+50°C to Ar3+150°C. The lower limit of the finish rolling exit temperature is more preferably Ar3+60°C, and more preferably Ar3+70°C. The upper limit of the finish rolling exit temperature is more preferably Ar3+140°C, and more preferably Ar3+130°C.
[0038] Thereafter, the hot-rolled steel sheet is cooled to Ms+50°C to Ms+300°C and then coiled. If the coiling temperature is less than Ms+50°C, excessive martensite or bainite is generated, which leads to an excessive increase in strength of the hot-rolled steel sheet, and problems such as defective shape due to the load during cold rolling may occur. On the other hand, if the coiling temperature exceeds Ms+300°C, the pickling property may decrease due to an increase in surface scale. Therefore, the coiling temperature is preferably in the range of Ms+50°C to Ms+300°C. The lower limit of the coiling temperature is more preferably Ms+60°C, and even more preferably Ms+70°C. The upper limit of the coiling temperature is more preferably Ms+290°C, and even more preferably Ms+270°C. On the other hand, after the coiling, the coiled hot-rolled steel sheet may be cooled to room temperature at a cooling rate of 0.1°C / s or less.
[0039] Thereafter, the coiled and cooled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. The cold rolling can be performed at a reduction of 40 to 70%. If the cold rolling reduction is less than 40%, the driving force for recrystallization is weakened, which may cause problems in obtaining good recrystallized grains, and shape correction is very difficult. If the cold rolling reduction exceeds 70%, cracks are likely to occur at the edge of the steel sheet, and the rolling load may increase rapidly. Therefore, it is preferable that the cold rolling is performed at a reduction of 40 to 70%. Meanwhile, before the cold rolling, pickling may be performed to remove scale and impurities attached to the surface.
[0040] Thereafter, the cold-rolled steel sheet is subjected to continuous annealing in a temperature range of 820 to 860°C. When the continuous annealing temperature is less than 820°C, it is difficult to form sufficient austenite, and it is difficult to ensure the target strength in the present invention. On the other hand, when the temperature exceeds 860°C, the austenite grain size becomes coarse, and bending workability of the final product may decrease. Therefore, the continuous annealing temperature is preferably in the range of 820 to 860°C. The lower limit of the continuous annealing temperature is more preferably 825°C, and even more preferably 830°C. The upper limit of the continuous annealing temperature is more preferably 855°C, and even more preferably 850°C.
[0041] After this, the above-mentioned continuously annealed cold-rolled steel sheet is heated for 50 to 200 seconds. Heating This is to ensure sufficient austenite fraction at the annealing temperature proposed by the present invention, together with recrystallization and grain growth of the cold rolled structure. Heating If the treatment time is less than 50 seconds, the reverse transformation of austenite does not occur sufficiently, and the ferrite fraction in the final structure increases, making it difficult to secure the target strength. Heating If the treatment time exceeds 200 seconds, the austenite grain size becomes coarse, and the bending workability of the final product may deteriorate. Heating The lower limit of the treatment time is more preferably 55 seconds, and even more preferably 60 seconds. Heating The upper limit of the processing time is more preferably 190 seconds, and even more preferably 180 seconds.
[0042] After this, HeatingThe treated cold-rolled steel sheet is primarily cooled to 620-700°C at a cooling rate of 1-10°C / s. The primary cooling step is performed to ensure the equilibrium carbon concentration of ferrite and austenite to increase the ductility and strength of the steel sheet. If the primary cooling end temperature is less than 630°C or exceeds 700°C, it is difficult to ensure the ductility and strength targeted in the present invention. If the cooling rate is less than 1°C / s, it is difficult to ensure the targeted microstructure fraction due to accelerated ferrite transformation, and if it exceeds 10°C / s, it is difficult to ensure the elongation due to excessive martensite transformation.
[0043] Thereafter, the cold-rolled steel sheet subjected to the primary cooling is secondarily cooled to 360 to 420°C at a cooling rate of 5 to 50°C / sec. The secondary cooling is one of the control factors considered important in the present invention, and the secondary cooling end temperature is a very important condition for simultaneously ensuring strength, ductility, and bending workability. If the secondary cooling end temperature is less than 360°C, it is difficult to ensure ductility due to an excessive increase in the martensite fraction, and if it exceeds 420°C, it is difficult to ensure sufficient martensite and therefore difficult to ensure the target strength. Therefore, the secondary cooling end temperature, which is one of the important control factors for ensuring the target physical properties in the present invention, is preferably in the range of 360 to 420°C. The lower limit of the secondary cooling end temperature is more preferably 365°C, and even more preferably 370°C. The upper limit of the secondary cooling end temperature is more preferably 405°C, and even more preferably 400°C. If the secondary cooling rate is less than 5°C / s, ferrite transformation occurs preferentially before martensite and bainite transformation due to the slow cooling rate, and the appropriate amount of fine structure fraction desired by the present invention cannot be obtained, and if it exceeds 50°C / s, the excessive cooling rate can cause shape deterioration, resulting in poor sheet passability and sheet breakage. The lower limit of the secondary cooling rate is more preferably 7.5°C / s, and even more preferably 10°C / s. The upper limit of the secondary cooling rate is more preferably 47.5°C / s, and even more preferably 45°C / s.
[0044] On the other hand, in order to ensure the fraction of tempered martensite, which is an important microstructure in the present invention, at a target level, it is important to precisely control the difference between the Ms temperature and the secondary cooling end temperature. More specifically, it is preferable to satisfy the following relational expression 4. When the difference between Ms and the secondary cooling end temperature, i.e., the value of A, is less than 0, it may be difficult to ensure the target strength due to the small amount of martensite transformation, and when the value of A exceeds 50°C, it is difficult to ensure ductility due to the long residence time in the martensite region and the excessive increase in the fraction of martensite. Therefore, it is preferable that the difference between the Ms and the secondary cooling end temperature, i.e., the value of A, is 0 to 50°C. The lower limit of the A value is more preferably 1°C, and even more preferably 2°C. The upper limit of the A value is more preferably 45°C, and even more preferably 40°C. On the other hand, Ms means the temperature at which martensite transformation begins, and its value can be calculated from the following formula 1. [Relationship 4] 0≦A≦50 (In the above relational expression 4, A is the Ms-secondary cooling end temperature (°C).) [Formula 1] Ms=539-423C-30.4Mn-7.5Si+30Al
[0045] Thereafter, the second-cooled cold-rolled steel sheet is overaged at 370 to 420°C or overaged after reheating. The overaging is preferably performed at a temperature equal to or higher than the temperature at the end of the second cooling. The overaging is a process for promoting the transformation of fresh martensite generated at the end of the second cooling into tempered martensite, and thus high yield strength and bending workability can be stably ensured. Therefore, in order to ensure high bending workability to be obtained in the present invention, the overaging temperature is a very important factor, and in the present invention, the overaging temperature is precisely controlled in the range of 370 to 420°C. If the overaging temperature is less than 370°C, the transformation from fresh martensite to tempered martensite may be small, and bending workability may be reduced. On the other hand, if the overaging temperature exceeds 420°C, it may be difficult to ensure tensile strength due to excessive tempered martensite transformation. Therefore, the overaging temperature is preferably in the range of 370 to 420°C. The lower limit of the overaging treatment temperature is more preferably 375°C, and even more preferably 380°C. The upper limit of the overaging treatment temperature is more preferably 415°C, and even more preferably 410°C.
[0046] On the other hand, in order to ensure the fraction of tempered martensite, which is an important microstructure in the present invention, at a target level, it is important to precisely control the overaging temperature and the secondary cooling end temperature. More specifically, it is preferable to satisfy the following relational expression 5. When the difference between the overaging temperature and the secondary cooling end temperature, i.e., the value of B, is less than 0, it is difficult to obtain the overaging effect, and when the value of B exceeds 40°C, it may be difficult to ensure the target tensile strength due to excessive tempered martensite transformation. Therefore, the difference between the overaging temperature and the secondary cooling end temperature, i.e., the value of B, is preferably 0 to 40°C. The lower limit of the B value is more preferably 2.5°C, and even more preferably 5°C. The upper limit of the B value is more preferably 35°C, and even more preferably 30°C. [Relationship 5] 0≦B≦40 (In the above relational expression 5, B is the overaging treatment temperature-secondary cooling end temperature (°C).)
[0047] In the present invention, in order to achieve the target fine structure fraction and strength level, it is preferable that the following relations 6 to 8 are satisfied during the above-mentioned secondary cooling and overaging treatment.
[0048] [Relationship 6] 0≦2.8A+0.5B≦100 The above-mentioned relational expression 6 is for ensuring the yield strength targeted by the present invention. If the value of the above-mentioned relational expression 6 is less than 0, it is difficult to secure sufficient martensite and to obtain high yield strength, and if it exceeds 100, there is a possibility that a problem of excessively high yield strength may occur due to securing excessive tempered martensite. Therefore, it is preferable that the value of the above-mentioned relational expression 6 is in the range of 0 to 100. The lower limit of the value of the above-mentioned relational expression 6 is more preferably 2, and even more preferably 4. The upper limit of the value of the above-mentioned relational expression 6 is more preferably 90, and even more preferably 80.
[0049] [Relationship 7] 0≦3.1A+2.3B≦200 The above-mentioned relational expression 7 is for ensuring the tensile strength targeted by the present invention. When the value of the above-mentioned relational expression 7 is less than 0, it is difficult to ensure sufficient fresh martensite and therefore difficult to ensure the targeted tensile strength, and when it exceeds 200, transformation to tempered martensite occurs excessively and therefore difficult to ensure the tensile strength. Therefore, it is preferable that the value of the above-mentioned relational expression 7 is in the range of 0 to 200. The lower limit of the value of the above-mentioned relational expression 7 is more preferably 2, and even more preferably 4. The upper limit of the value of the above-mentioned relational expression 7 is more preferably 190, and even more preferably 180.
[0050] [Relational expression 8]0.25≦(3.1A+2.3B) / (2.8A+0.5B)≦3.5 The above-mentioned relational expression 8 is for simultaneously ensuring the yield strength and tensile strength targeted by the present invention. When the value of the above-mentioned relational expression 8 is less than 0.25 or exceeds 3.5, there is a drawback in that it is difficult to ensure the targeted structure fraction and therefore difficult to simultaneously ensure the desired yield strength and tensile strength. Therefore, the value of the above-mentioned relational expression 8 is preferably in the range of 0.25 to 3.5. The lower limit of the value of the above-mentioned relational expression 8 is more preferably 0.50, and even more preferably 0.75. The upper limit of the value of the above-mentioned relational expression 8 is more preferably 3.25, and even more preferably 3.0.
[0051] Meanwhile, the present invention may further include a step of temper rolling the overaged cold rolled steel sheet at an elongation rate of 0.1 to 2.0% after the overaging treatment. In general, temper rolling causes little increase in tensile strength, but increases yield strength by at least 50 MPa or more. If the elongation rate is less than 0.1%, it may be difficult to control the shape, and if it exceeds 2.0%, operability may become significantly unstable due to high elongation work. EXAMPLES
[0052] The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are provided to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.
[0053] (Example) Molten steel having the alloy composition shown in Table 1 below was prepared, and then continuously cast to produce a slab having a thickness of 250 mm. The slab was heated to 1200°C for 12 hours, hot-rolled, and then coiled. At this time, the finish rolling exit temperature during hot rolling was controlled in the range of Ar3+50°C to Ar3+150°C, and the coiling temperature was controlled in the range of Ms+50°C to Ms+300°C. Thereafter, the hot-rolled steel sheet having a thickness of 3.2 mm obtained by the hot rolling was pickled, and then cold-rolled at a cold reduction of 50% to obtain a cold-rolled steel sheet having a thickness of 1.6 mm. This cold-rolled steel sheet was manufactured as a final product using the conditions shown in Tables 2 and 3 below. The microstructure and mechanical properties of the cold-rolled steel sheet manufactured in this manner were measured, and the results are shown in Table 4 below.
[0054] The fraction of the microstructure was measured using Electron Backscatter Diffraction (EBSD) equipment. The average length of the lath minor axis of the tempered martensite was calculated by averaging five randomly taken images at 40,000x magnification using a transmission electron microscope (TEM), measuring the images using Image-Plus Pro software, and calculating the average value. Meanwhile, the measured microstructure is composed of a mixture of tempered martensite, remaining fresh martensite, bainite, ferrite, and retained austenite.
[0055] Tensile strength (TS), yield strength (YS), and elongation (EL) were measured through a tensile test in the horizontal direction after rolling, and the gauge length was 50 mm and the width of the tensile test specimen was 25 mm.
[0056] The hole expansion ratio (HER) was measured according to the ISO 16330 standard, and the holes were sheared using a 10 mm diameter punch with a clearance of 12%.
[0057] In the 180° full crimp bending test, the steel plate to be measured was first bent 90°, and then another steel plate twice as thick as the steel plate was sandwiched between the two plates. The steel plate to be measured was then bent 180° again to be fully crimped, and the presence or absence of cracks was then visually determined. Cases where no cracks occurred were marked with ○, and cases where cracks occurred were marked with ×.
[0058] [Table 1]
[0059] [Table 2]
[0060] [Table 3]
[0061] [Table 4]
[0062] As shown in Tables 1 to 4 above, in the case of Examples 1 to 12, which satisfy the alloy composition and manufacturing conditions proposed by the present invention, it can be seen that excellent mechanical properties are obtained by securing the microstructure that the present invention aims to obtain.
[0063] On the other hand, in the case of Comparative Examples 1 to 17 which do not satisfy the alloy composition or manufacturing conditions proposed by the present invention, it was confirmed that the mechanical properties were deteriorated because the microstructure which the present invention aims to obtain could not be secured.
[0064] Fig. 1 is a microstructure photograph of Example 1 observed by using an SEM, and Fig. 2 is a microstructure photograph of Example 1 observed by using a TEM. As can be seen from Figs. 1 and 2, it can be confirmed that Example 1 has a uniform distribution of tempered martensite, which is the main structure of the present invention.
Claims
1. The steel contains, by weight, C: 0.06-0.17%, Si: 0.1-0.8%, Mn: 1.9-2.9%, Nb: 0.005-0.07%, Ti: 0.004-0.05%, B: 0.0004-0.005%, Cr: 0.20% or less (excluding 0%), and Mo: 0.04-0.45%, with the balance being Fe and other inevitable impurities; The following relations 1 to 3 are satisfied, The microstructure, in terms of area percent, includes tempered martensite: 80-98%, the remainder fresh martensite, bainite, ferrite and retained austenite. The average length of the lath minor axis of the tempered martensite is 500 nm or less. [Relational expression 1] 0.40≦C+Mn / 6+(Cr+Mo+V) / 5+(Si+Ni+Cu) / 15≦0.70 [Relationship 2] 110≦48.8+49 log C+35.1 Mn+25.9 Si+76.5 Cr+105.9 Mo+1325 Nb≦210 [Relationship 3] 0.20≦Mo+200B≦0.70 (However, the contents of the alloy components in the above Relational Formulas 1 to 3 are expressed in weight percent.)
2. The impurities include one or more of P, S, Al, Sb, N, Mg, Sn, Sb, Zn, and Pb as tramp elements, and the total amount thereof is 0.1 wt% or less. The cold-rolled steel sheet according to claim 1.
3. 2. The cold rolled steel sheet according to claim 1, wherein the fresh martensite is 11% or less, the bainite is 3% or less, the ferrite is 3% or less, and the retained austenite is 3% or less.
4. The cold-rolled steel sheet has a yield strength (YS): 780 to 920 MPa, a tensile strength (TS): 980 to 1200 MPa, an elongation (EL): 8% or more, a yield ratio (YS / TS): 0.75 or more, a hole expansion ratio (HER): 40% or more, and a bending workability (YS × EL × HER): 300 GPa%% or more. The cold-rolled steel sheet according to claim 1, wherein no cracks occur during a 180 ° full crimp bending test.
5. a step of heating a slab containing, by weight, 0.06-0.17% C, 0.1-0.8% Si, 1.9-2.9% Mn, 0.005-0.07% Nb, 0.004-0.05% Ti, 0.0004-0.005% B, 0.20% or less (excluding 0%) Cr, and 0.04-0.45% Mo, with the balance being Fe and other unavoidable impurities, and satisfying the following relations 1 to 3; a step of finish rolling the heated slab so that the finish rolling delivery temperature is Ar3+50°C to Ar3+150°C to obtain a hot-rolled steel sheet; cooling the hot-rolled steel sheet to Ms+50°C to Ms+300°C and then coiling it; cold rolling the coiled hot-rolled steel sheet to obtain a cold-rolled steel sheet; continuous annealing the cold-rolled steel sheet at a temperature range of 820 to 860°C; subjecting the continuously annealed cold rolled steel sheet to a soaking treatment for 50 to 200 seconds; a step of primarily cooling the soaked cold-rolled steel sheet to 620 to 700° C. at a cooling rate of 1 to 10° C. / s; secondarily cooling the primarily cooled cold-rolled steel sheet to 360 to 420° C. at a cooling rate of 5 to 50° C. / sec; The second-cooled cold-rolled steel sheet is overaged at 370 to 420° C. or overaged after reheating; The method for producing a cold-rolled steel sheet according to claim 1, wherein the following relations 4 to 8 are satisfied during the secondary cooling and overaging treatment. [Relational expression 1] 0.40≦C+Mn / 6+(Cr+Mo+V) / 5+(Si+Ni+Cu) / 15≦0.70 [Relationship 2] 110≦48.8+49 log C+35.1 Mn+25.9 Si+76.5 Cr+105.9 Mo+1325 Nb≦210 [Relationship 3] 0.20≦Mo+200B≦0.70 [Relationship 4] 0≦A≦50 [Relationship 5] 0≦B≦40 [Relationship 6] 0≦2.8A+0.5B≦100 [Relationship 7] 0≦3.1A+2.3B≦200 [Relational expression 8] 0.25≦(3.1A+2.3B) / (2.8A+0.5B)≦3.5 (Note that the contents of the alloy components described in the above Relational Formulas 1 to 3 are expressed in terms of weight percent, and in the above Relational Formulas 4 to 8, A is Ms-secondary cooling end temperature (°C), and B is overaging treatment temperature-secondary cooling end temperature (°C).)
6. The method for producing a cold rolled steel sheet according to claim 5, wherein the slab heating is performed at 1100 to 1300°C.
7. The method for producing a cold rolled steel sheet according to claim 5, wherein the slab has a thickness of 230 to 270 mm.
8. The method for producing a cold-rolled steel sheet according to claim 5, further comprising the step of cooling the coiled hot-rolled steel sheet to room temperature at a cooling rate of 0.1° C. / s or less after the coiling.
9. The method for producing a cold-rolled steel sheet according to claim 5, wherein the cold rolling is performed at a rolling reduction of 40 to 70%.
10. The method for producing a cold rolled steel sheet according to claim 5, further comprising the step of temper rolling the overaged cold rolled steel sheet at an elongation of 0.1 to 2.0% after the overaging treatment.
Citation Information
Patent Citations
High-strength steel having adequate workability and manufacturing method therefor
JP2005264176A
High-strength cold rolled steel sheet and its production method
JP2006183140A
High-strength cold-rolled steel sheet excellent in steel sheet shape and shape fixability and production method thereof
JP2014196557A
Manufacturing method of ultra-high strength cold-rolled steel sheet with good formability and strip shape
JP2528387B2
High strength steel sheet and method of manufacturing the steel sheet
KR1020130046941A