Surface-modified crosslinked polyaspartic acid composition
By utilizing an aspartic acid composition with controlled impurities, the polymerization rate of polysuccinimide is enhanced, resulting in high molecular weight crosslinked polyaspartic acid compositions with improved water retention.
Patent Information
- Application Number
- JP2024111345
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-29
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-31
AI Technical Summary
The polymerization reaction rate of polysuccinimide, an intermediate in the production of polyaspartic acid, is slow, and there is a need for an efficient method to produce crosslinked polyaspartic acid with high water retention.
An aspartic acid composition containing specific impurities such as amino acids and organic acids within predetermined ranges is used to enhance the polymerization reaction, leading to the formation of high molecular weight polysuccinimide and crosslinked polyaspartic acid compositions.
The method accelerates the polymerization process and results in the production of crosslinked polyaspartic acid compositions with high water retention capabilities.
Smart Images

Figure 0007576740000004 
Figure 0007576740000001 
Figure 0007576740000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an aspartic acid composition, a polyaspartic acid composition, a crosslinked polyaspartic acid composition, a surface-modified crosslinked polyaspartic acid composition, and a method for producing the same. It also relates to a polysuccinimide composition, a crosslinked polysuccinimide composition, and a method for producing the same. It also relates to a crosslinked polyaspartic acid-containing product, and a method for producing a crosslinked polyaspartic acid-containing product. This application claims priority based on Japanese Patent Application No. 2021-107638, filed on June 29, 2021, the contents of which are incorporated herein by reference. [Background technology]
[0002] Polyaspartic acid is a biodegradable polycarboxylic acid, and its chemical structure is similar to that of polyacrylic acid. Therefore, polyaspartic acid is expected to be a biodegradable material with high water retention to replace polyacrylic acid. Known methods for obtaining polyaspartic acid include a method in which polysuccinimide is obtained by a dehydration condensation reaction of aspartic acid, and then the polysuccinimide is subjected to alkaline hydrolysis (Patent Document 1).
[0003] Aspartic acid, which is a raw material for polysuccinimide, is industrially synthesized using aspartase from petroleum-derived fumaric acid and ammonia. However, due to problems such as the depletion of petroleum resources, a method for producing aspartic acid by a bioprocess using microorganisms has been investigated (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-176312 [Patent Document 2] International Publication No. 2020 / 208842 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors recognized that in the process of obtaining polyaspartic acid from aspartic acid, the polymerization reaction rate of the intermediate polysuccinimide is slow. In order to improve the efficiency of the process of obtaining polyaspartic acid from aspartic acid, it is desirable to increase the polymerization reaction rate of the intermediate polysuccinimide to obtain a polymer with a high molecular weight. In addition, it is desirable to efficiently obtain crosslinked polyaspartic acid with high water retention by using aspartic acid.
[0006] Therefore, an object of the present invention is to provide an aspartic acid composition that can be used for efficient production of a crosslinked polyaspartic acid composition, and also to provide a polysuccinimide composition containing a high molecular weight polysuccinimide, a crosslinked polyaspartic acid composition having high water retention, and the like, which are obtained from the aspartic acid composition. [Means for solving the problem]
[0007] The present invention includes the following aspects. [1] An aspartic acid composition comprising aspartic acid and impurities, the impurities including at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof, and the content of the impurities being 0.02% by mass or more and 1.1% by mass or less. [2] The aspartic acid composition according to [1], wherein the impurities include amino acids other than aspartic acid. [3] The aspartic acid composition according to [1] or [2], wherein the aspartic acid is produced by a microorganism. [4] A method for producing polysuccinimide, comprising carrying out a polymerization reaction of aspartic acid using the aspartic acid composition according to any one of [1] to [3]. [5] The method for producing polysuccinimide according to [4], wherein the polymerization reaction is carried out in a kneading apparatus. [6] A polysuccinimide composition comprising: polysuccinimide; and impurities, wherein the impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof, and the content of the impurities is 0.001% by mass or more and 1.1% by mass or less. [7] The polysuccinimide composition according to [6], wherein the impurities include an amino acid other than aspartic acid. [8] A polysuccinimide composition, which is a polymerization reaction product of the aspartic acid composition according to any one of [1] to [3]. [9] A polyaspartic acid composition which is a hydrolysate of the polysuccinimide composition according to any one of [6] to [8].
[10] A polyaspartic acid composition comprising polyaspartic acid and impurities, the impurities including at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof, and the content of the impurities being 0.001% by mass or more and 1.1% by mass or less.
[11] The polyaspartic acid composition according to
[10] , wherein the impurities include an amino acid other than the aspartic acid or a salt thereof.
[12] A crosslinked polyaspartic acid composition, which is a crosslinking reaction product of the polyaspartic acid composition according to any one of [9] to
[11] .
[13] A crosslinked polysuccinimide composition, which is a crosslinking reaction product of the polysuccinimide composition according to any one of [6] to [8].
[14] A crosslinked polyaspartic acid composition which is a hydrolysate of the crosslinked polysuccinimide composition according to
[13] .
[15] A surface-modified crosslinked polyaspartic acid composition comprising particles of the crosslinked polyaspartic acid composition according to
[12] or
[14] , the surfaces of the particles being modified with inorganic particles.
[16] A crosslinked polyaspartic acid-containing product comprising the crosslinked polyaspartic acid composition according to
[12] or
[14] , or the surface-modified crosslinked polyaspartic acid composition according to
[15] .
[17] The crosslinked polyaspartic acid-containing product according to
[15] , which is a surfactant, a thickener, a viscosity reducer, a swelling agent, a water absorbent, a gelling agent, a binder, a film-forming agent, a flocculant, an adhesive, a surface modifier, or a sustained-release agent.
[18] A method for producing a polyaspartic acid composition, comprising: a step of using the aspartic acid composition according to any one of [1] to [3] to perform a polymerization reaction of the aspartic acid to obtain a polysuccinimide composition containing polysuccinimide; and a step of using the polysuccinimide composition to perform a hydrolysis reaction of the polysuccinimide to obtain a polyaspartic acid composition containing polyaspartic acid.
[19] A method for producing a crosslinked polyaspartic acid composition, comprising: obtaining a polyaspartic acid composition by the method for producing a polyaspartic acid composition according to the method described in
[18] ; and using the polyaspartic acid composition to perform a crosslinking reaction of the polyaspartic acid, thereby obtaining a crosslinked polyaspartic acid composition containing crosslinked polyaspartic acid.
[20] A method for producing a crosslinked polyaspartic acid composition, comprising the steps of: using the aspartic acid composition according to any one of [1] to [3] to perform a polymerization reaction of the aspartic acid to obtain a polysuccinimide composition containing polysuccinimide; using the polysuccinimide composition to perform a crosslinking reaction of the polysuccinimide to obtain a crosslinked polysuccinimide composition containing crosslinked polysuccinimide; and using the crosslinked polysuccinimide composition to perform a hydrolysis reaction of the crosslinked polysuccinimide to obtain a crosslinked polyaspartic acid composition containing crosslinked polyaspartic acid.
[21] A method for producing a crosslinked polyaspartic acid-containing product, comprising the steps of: obtaining a crosslinked polyaspartic acid composition by the method for producing a crosslinked polyaspartic acid composition according to the above item
[19] or
[20] ; and producing a crosslinked polyaspartic acid-containing product using the crosslinked polyaspartic acid composition.
[22] The method for producing a crosslinked polyaspartic acid-containing product according to
[21] , wherein the crosslinked polyaspartic acid-containing product is a surfactant, a thickener, a viscosity reducer, a swelling agent, a water absorbent, a gelling agent, a binder, a film-forming agent, a flocculant, an adhesive, a surface modifier, or a sustained-release agent. Effect of the Invention
[0008] According to the present invention, since the aspartic acid composition contains a predetermined amount of impurities such as amino acids and organic acids, a polysuccinimide composition containing a high molecular weight polysuccinimide can be obtained by carrying out a polymerization reaction using the aspartic acid composition. In addition, a crosslinked polyaspartic acid composition having high water retention can be obtained from the polysuccinimide composition. [Brief description of the drawings]
[0009] [Figure 1] 1 shows the results of measuring the weight average molecular weight (Mw) of polysuccinimide produced by the polymerization reaction of an aspartic acid composition over time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in more detail below. Note that the present invention is not limited to the embodiments shown below. In this specification, "to" means equal to or greater than the value before "to" and equal to or less than the value after "to". [Aspartic acid composition] In one aspect, the present invention provides an aspartic acid composition for producing polysuccinimide. The aspartic acid composition includes aspartic acid and impurities. The impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof. The content of the impurities in the aspartic acid composition is 0.02% by mass or more and 1.1% by mass or less.
[0011] "Aspartic acid composition" refers to a composition containing aspartic acid as a main component. The aspartic acid composition is used in the production of polysuccinimide. The aspartic acid composition contains aspartic acid and impurities.
[0012] <Impurities> The term "impurities" in the aspartic acid composition refers to components other than aspartic acid contained in the aspartic acid composition. In one embodiment, the impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof.
[0013] An "amino acid" is an organic substance having both an amino group and a carboxy group. The amino acids contained as impurities in the aspartic acid composition are amino acids other than aspartic acid. The amino acids contained as impurities may be any of α-amino acids, β-amino acids, γ-amino acids, and δ-amino acids. The amino acids may be in the L-form, the D-form, or a mixture thereof. In one embodiment, the amino acids are in the L-form. The impurities preferably include amino acids other than aspartic acid.
[0014] Examples of amino acids as impurities include alanine, arginine, asparagine, cysteine, glutamine, glutamic acid, glycine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, and valine. Among them, the impurities preferably include at least one selected from the group consisting of glutamic acid, alanine, and valine, and more preferably include glutamic acid and / or valine.
[0015] The content of amino acids as impurities is preferably 0 parts by mass or more and 1.1 parts by mass or less relative to 100 parts by mass of aspartic acid, and the lower limit may be 0.001 parts by mass or more, 0.005 parts by mass or more, 0.010 parts by mass or more, 0.015 parts by mass or more, 0.02 parts by mass or more, 0.03 parts by mass or more, 0.05 parts by mass or more, 0.07 parts by mass or more, 0.09 parts by mass or more, or 0.10 parts by mass or more. , 0.15 parts by mass or more, 0.18 parts by mass or more, 0.20 parts by mass or more, or 0.25 parts by mass or more, and the upper limit may be 1.1 parts by mass or less, 1.0 parts by mass or less, 0.98 parts by mass or less, 0.95 parts by mass or less, 0.90 parts by mass or less, 0.80 parts by mass or less, 0.75 parts by mass or less, 0.70 parts by mass or less, 0.50 parts by mass or less, or 0.30 parts by mass or less. Any combination of these upper and lower limit values may be used. The content of amino acids as impurities may be, relative to 100 parts by mass of aspartic acid, 0 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.0 parts by mass or less, 0.001 parts by mass or more and 0.98 parts by mass or less, 0.005 parts by mass or more and 0.95 parts by mass or less, 0.010 parts by mass or more and 0.90 parts by mass or less, 0.020 parts by mass or more and 0.80 parts by mass or less, 0.05 parts by mass or more and 0.70 parts by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less.
[0016] The amino acid as an impurity may be in the form of a salt. Examples of the salt of an amino acid include salts with alkali metals (sodium, potassium, lithium, etc.) and salts with alkaline earth metals (calcium, magnesium, etc.). The content ranges exemplified above for the amino acid as an impurity also apply when the amino acid as an impurity is in the form of a salt. When both an amino acid and an amino acid salt are included as impurities, the content ranges exemplified above apply to the total content of both.
[0017] An "organic acid" is an organic substance that exhibits acidity. In one embodiment, the organic acid is a carboxylic acid. When used herein, the term "organic acid" excludes amino acids.
[0018] Examples of organic acids as impurities include pyruvic acid, maleic acid, fumaric acid, malic acid, acetic acid, and succinic acid.
[0019] The content of organic acid as an impurity is preferably 0 parts by mass or more and 1.1 parts by mass or less, and the upper limit may be 0.02 parts by mass or more, 0.03 parts by mass or more, 0.05 parts by mass or more, 0.07 parts by mass or more, 0.09 parts by mass or more, 0.10 parts by mass or more, 0.15 parts by mass or more, 0.18 parts by mass or more, 0.20 parts by mass or more, or 0.25 parts by mass or more, and the upper limit may be 1.1 parts by mass or less, 1.0 parts by mass or less, 0.98 parts by mass or less, 0.95 parts by mass or less, 0.90 parts by mass or less, 0.80 parts by mass or less, 0.75 parts by mass or less, 0.70 parts by mass or less, 0.50 parts by mass or less, or 0.30 parts by mass or less. These upper and lower limit values may be used in any combination. The content of organic acid as an impurity may be, relative to 100 parts by mass of aspartic acid, 0 parts by mass or more and 1.1 parts by mass or less, 0.001 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.0 parts by mass or less, 0.001 parts by mass or more and 0.98 parts by mass or less, 0.005 parts by mass or more and 0.95 parts by mass or less, 0.010 parts by mass or more and 0.90 parts by mass or less, 0.020 parts by mass or more and 0.80 parts by mass or less, 0.05 parts by mass or more and 0.70 parts by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less.
[0020] The organic acid as an impurity may be in the form of a salt. Examples of the salt of the organic acid include salts with alkali metals (sodium, potassium, lithium, etc.) and salts with alkaline earth metals (calcium, magnesium, etc.). The content ranges exemplified above for the organic acid as an impurity also apply when the organic acid as an impurity is in the form of a salt. When both an organic acid and a salt of an organic acid are contained as impurities, the content ranges exemplified above apply to the total content of both.
[0021] The aspartic acid composition contains impurities in an amount of 0.02% by mass or more and 1.1% by mass or less, based on the total mass of all components of the aspartic acid composition. The content of impurities is preferably 0.021% by mass or more and 1.08% by mass or less, based on the total mass of all components of the aspartic acid composition, and the lower limit may be 0.021% by mass or more, 0.025% by mass or more, 0.03% by mass or more, 0.035% by mass or more, 0.04% by mass or more, 0.045% by mass or more, 0.05% by mass or more, 0.07% by mass or more, 0.09% by mass or more, or 0.10% by mass or more. The upper limit may be 1.05 mass% or less, 1.0 mass% or less, 0.98 mass% or less, 0.95 mass% or less, 0.90 mass% or less, 0.80 mass% or less, 0.75 mass% or less, 0.70 mass parts or less, 0.50 mass parts or less, or 0.30 mass parts or less. Any combination of these upper and lower limit values may be used. The content of impurities may be, relative to the total mass of all components of the aspartic acid composition, 0.021% by mass or more and 1.1% by mass or less, 0.025% by mass or more and 1.1% by mass or less, 0.02% by mass or more and 1.0% by mass or less, 0.02% by mass or more and 0.98% by mass or less, 0.02% by mass or more and 0.95% by mass or less, 0.02% by mass or more and 0.90% by mass or less, 0.020% by mass or more and 0.80% by mass or less, 0.02% by mass or more and 0.70% by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less. By keeping the content of impurities within the above range, the polymerization reaction of aspartic acid is promoted, and a high molecular weight polysuccinimide can be obtained.
[0022] The impurities may include components other than amino acids other than aspartic acid, organic acids, and their salts, such as sulfates.
[0023] <Aspartic acid> Aspartic acid may be in the L-form, in the D-form, or in a mixture thereof. In one embodiment, aspartic acid is in the L-form. Aspartic acid may be produced by a microorganism or may be produced without using a microorganism. Examples of a method for producing aspartic acid without using a microorganism include a method of reacting fumaric acid with ammonia in the presence of an enzyme such as aspartase. The content of aspartic acid in the aspartic acid composition is 98.9% by mass or more and 99.98% by mass or less, based on the total mass of all components of the aspartic acid composition. The content of aspartic acid may be 98.95% by mass or more and 99.97% by mass or less, 99.00% by mass or more and 99.96% by mass or less, 99.02% by mass or more and 99.95% by mass or less, or 99.05% by mass or more and 99.93% by mass or less, based on the total mass of all components of the aspartic acid composition. Any combination of these upper and lower limit values may be used.
[0024] <Method of producing aspartic acid composition> The aspartic acid composition can be produced by a known method, for example, a method of reacting fumaric acid with ammonia in the presence of an enzyme such as aspartase, a method of using a microorganism capable of producing aspartic acid, such as a Corynebacterium bacterium, etc.
[0025] (Method using microorganisms) In this specification, the term "microorganism" should be taken literally, and more specifically, the "microorganism" may be a prokaryote such as an archaea, a cyanobacteria, or a bacteria, or a eukaryote such as a fungus. In this embodiment, the "microorganism" is preferably a fungus or a bacteria, and more preferably a bacteria.
[0026] Examples of fungi include Saccharomyces genus yeast (e.g., Saccharomyces cerevisiae), Schizosaccharomyces genus yeast (e.g., Schizosaccharomyces pombe), Pichia genus yeast (e.g., Pichia pastoris), Kluyveromyces genus yeast (Kluyveromyces lactis), Hansenula polymorpha, Yarrowia genus yeast (e.g., Yarrowia lipolytica), Cryptococcus genus fungi (e.g., Cryptococcus sp. S-2), Aspergillus genus fungi (e.g., Aspergillus oryzae), Pseudozyma genus fungi (e.g., Pseudozyma antarctica), etc. Saccharomyces cerevisiae, Schizosaccharomyces pombe, Pichia pastoris, etc. can be conveniently used in the present invention because gene recombination techniques and heterologous protein expression systems have been established.
[0027] Examples of bacteria include bacteria of the genus Escherichia (e.g., Escherichia coli), Bacillus (e.g., Bacillus subtilis), Lactobacillus (e.g., Lactobacillus acidophilus), Clostridium (e.g., Clostridium thermocellum, Clostridium acetobutylicum), Rhodopseudomonas (e.g., Rhodopseudomonas palustris), Rhodobacter (Rhodobacter capsulatus), and bacteria belonging to the coryneform bacteria described in detail below. In the present specification, the "microorganism" is preferably an Escherichia or coryneform bacterium for which recombinant gene technology and protein expression systems have already been established and which enables substance production under reducing conditions in which cells do not substantially grow, more preferably an Escherichia coli or coryneform bacterium, and most preferably a Corynebacterium bacterium.
[0028] Here, the term "Coryneform bacteria" refers to a group of microorganisms defined in Bargeys Manual of Determinative Bacteriology (Vol. 8, p. 599, 1974). More specifically, examples of coryneform bacteria include bacteria of the genus Corynebacterium, Brevibacterium, Arthrobacter, Mycobacterium, Micrococcus, and Microbacterium.
[0029] An example of the Corynebacterium genus is Corynebacterium glutamicum.
[0030] When using a microorganism, the microorganism may be cultured using a medium that is generally used for culturing heterotrophic bacteria. Examples of the medium include media containing a carbon source, a nitrogen source, a phosphorus source, trace elements, vitamins, and the like. Examples of carbon sources include sugars (glucose, sucrose, lactose, fructose, maltose, molasses, starch, and the like), fatty acids (palmitic acid, stearic acid, linoleic acid, and the like), alcohols (glycerol, ethanol, and the like), and organic acids (acetic acid, and the like). Examples of nitrogen sources include nitrogen-containing organic compounds (peptone, yeast extract, meat extract, urea, amino acids, and the like), inorganic ammonium salts, inorganic nitrates, and the like. Examples of phosphorus sources include potassium dihydrogen phosphate, dipotassium hydrogen phosphate, and the like. Examples of trace elements include magnesium, iron, zinc, and the like. Examples of vitamins include biotin, thiamine, and the like.
[0031] The culture conditions can be appropriately selected depending on the type of microorganism. The pH condition is, for example, pH 6 to 9, and more preferably pH 7 to 8.5. The temperature conditions are, for example, 20 to 40°C, and preferably 25 to 37°C. The culture is preferably performed by shaking culture or aeration culture.
[0032] The culture time is not particularly limited and can be appropriately set depending on the type of microorganism and the amount of medium, and may be, for example, 15 to 50 hours, or 20 to 40 hours.
[0033] After the culture, the cells are removed from the culture medium by centrifugation or filtration, and the culture supernatant is collected. The culture supernatant contains various substances such as medium components and by-products of the microorganisms in addition to the aspartic acid produced by the microorganism. Therefore, the aspartic acid may be purified from the culture supernatant by a method commonly used for separation and purification such as concentration, isoelectric crystallization, recrystallization, activated carbon treatment, and washing. The aspartic acid composition can be obtained by reducing the content of impurities to 0.02% by mass or more and 1.1% by mass or less through the purification treatment. The aspartic acid composition obtained by purifying the culture supernatant of the microorganism usually contains at least one impurity selected from the group consisting of amino acids other than aspartic acid and organic acids.
[0034] When the aspartic acid composition is obtained by a method of reacting fumaric acid with ammonia in the presence of an enzyme catalyst to produce aspartic acid, the reaction solution after the reaction is recovered and the aspartic acid is purified. The aspartic acid composition can be obtained by reducing the content of impurities to 0.02% by mass or more and 1.1% by mass or less through the purification process.
[0035] When the content of impurities in the composition becomes less than 0.02% by mass as a result of the purification treatment of aspartic acid, at least one component selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof may be added to adjust the content of impurities to 0.02% by mass or more and 1.1% by mass or less. In this case, it is preferable to add an amino acid other than aspartic acid.
[0036] Due to problems such as the depletion of petroleum resources, it is preferable that petroleum-derived products are replaced by those produced using microorganisms, etc. The aspartic acid composition used in the production of polysuccinimide is also preferably produced using microorganisms. However, since the culture supernatant of a microorganism contains many impurities other than aspartic acid, it is difficult to purify it to the same purity as petroleum-derived products (for example, 99.9% by mass or more). On the other hand, the aspartic acid composition of this embodiment can obtain polysuccinimide with a sufficiently high molecular weight at a lower purity than petroleum-derived products. Furthermore, by using the aspartic acid composition of this embodiment, the polymerization rate of aspartic acid is accelerated (see FIG. 1). Therefore, the purification cost of aspartic acid can be reduced, and conversion to an efficient process using microorganisms can be expected.
[0037] When the aspartic acid composition of this embodiment is used, the polymerization environment is improved due to the presence of a certain amount of impurities such as amino acids and organic acids, and it is therefore believed that the polymerization rate of aspartic acid is increased compared to petroleum refined products, which have a higher purity of aspartic acid.
[0038] [Method of producing polysuccinimide] In one embodiment, the present invention provides a method for producing polysuccinimide, comprising carrying out a polymerization reaction of aspartic acid using the aspartic acid composition.
[0039] The polymerization reaction of aspartic acid can be carried out by a known method. The polymerization reaction of aspartic acid can be carried out in the presence of an acid catalyst or without a catalyst. Examples of the acid catalyst include phosphoric acid, phosphorous acid, phosphite ester, and p-toluenesulfonic acid. The amount of the acid catalyst used is not particularly limited, but can be, for example, 0.001 to 500 parts by mass, preferably 0.01 to 100 parts by mass, and more preferably 0.1 to 70 parts by mass, relative to 100 parts by mass of the aspartic acid composition.
[0040] The polymerization reaction of aspartic acid may be carried out by solid-phase polymerization or solution polymerization.
[0041] (Solid-state polymerization) Solid-phase polymerization is a polymerization method that does not use a reaction solvent. When the polymerization reaction is carried out under a catalyst, it is preferable to add the catalyst to the aspartic acid composition and mix thoroughly before carrying out the polymerization reaction. The mixing temperature is not particularly limited as long as it is 150°C or less at which the polymerization reaction does not occur. The mixing temperature is, for example, 20 to 120°C. The mixing time is, for example, 0.01 to 50 minutes.
[0042] The solid-state polymerization can be carried out using a kneading device after adding a catalyst to the aspartic acid composition. The acid catalyst may be added in its entirety at once or in small portions. The kneading device is not particularly limited, but is preferably equipped with an agitating blade so that the process after polymerization can be easily carried out. The agitating blade can crush the polymer during the polymerization reaction while stirring. Examples of the type of the agitating blade include a screw blade, a helical ribbon blade, a horizontal two-shaft blade, and a Banbury blade, and among these, a screw blade is preferable. Examples of the kneading device include a kneader, an extruder, a planetary mixer, a helical blade mixer, and a screw mixer. The kneading device may be of a batch type or a continuous type.
[0043] The polymerization reaction can be carried out by charging the aspartic acid composition or a mixture of the aspartic acid composition and an acid catalyst into a reactor and heating the mixture. The polymerization temperature is, for example, 100 to 400°C, preferably 150 to 350°C, and more preferably 150 to 280°C.
[0044] The pressure during the polymerization reaction is not particularly limited, and the polymerization reaction may be carried out under negative pressure or normal pressure. The pressure may be, for example, 1 to 100 kPa.
[0045] The polymerization time is not particularly limited as long as it is a time sufficient for producing a polysuccinimide having a desired length. The polymerization time is, for example, 0.5 to 100 hours, preferably 1 to 50 hours, and more preferably 1 to 20 hours.
[0046] The polymerization reaction may be carried out under a stream of an inert gas such as nitrogen or argon, etc. Furthermore, various additives such as a chain extender and a reaction accelerator may be used.
[0047] After the polymerization reaction, the reaction mixture may be pulverized and washed with a solvent such as methanol, or may be washed with distilled water or the like. After washing, the polysuccinimide powder can be obtained by drying, which can be achieved by natural drying, heat drying, vacuum drying, or the like.
[0048] (Solution Polymerization) Solution polymerization is a polymerization method using a reaction solvent. Examples of the reaction solvent include aromatic hydrocarbons, halogenated hydrocarbons, ethers, esters, and aprotic polar solvents. The reaction solvent is preferably a solvent having a boiling point of 100° C. or higher, preferably a solvent having a boiling point of 130° C. or higher. Examples of the aromatic hydrocarbons include cumene and mesitylene. Examples of the halogenated hydrocarbons include chlorotoluene and chlorobenzene. Examples of the ethers include anisole. Examples of the esters include n-amyl acetate. Examples of the aprotic polar solvents include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, tetramethylurea acid, dimethylsulfoxide, sulfolane, and hexamethylphosphoramide. The reaction solvent may be used alone or in a mixed solvent of two or more kinds. Among these, as the reaction solvent, cumene, chlorotoluene, xylene, mesitylene, pseudocumene, 1,3-dimethyl-2-imidazolidinone, sulfolane, and a mixed solvent of two or more of these are preferable because they have an appropriate boiling point. The amount of the reaction solvent used is not particularly limited, but may be, for example, 1 to 5,000 parts by mass, preferably 5 to 1,000 parts by mass, and more preferably 10 to 500 parts by mass, per 100 parts by mass of the aspartic acid composition.
[0049] The polymerization reaction can be carried out by charging a mixture of the aspartic acid composition, the acid catalyst, and the reaction solvent into a reactor, and heating the mixture while removing the generated water. The polymerization temperature is, for example, 100 to 400°C, preferably 120 to 350°C, and more preferably 120 to 280°C.
[0050] The pressure during the polymerization reaction is not particularly limited, and the polymerization reaction may be carried out under negative pressure or under normal pressure.
[0051] The polymerization time is not particularly limited as long as it is a time sufficient for producing a polysuccinimide having a desired length. The polymerization time is, for example, 0.5 to 100 hours, preferably 1 to 75 hours, and more preferably 1 to 50 hours.
[0052] The polymerization reaction may be carried out under a stream of an inert gas such as nitrogen or argon, etc. Furthermore, various additives such as a chain extender and a reaction accelerator may be used.
[0053] After the polymerization reaction, the reaction product may be washed with a solvent such as methanol, and then may be washed with distilled water or the like. After washing, the polysuccinimide powder can be obtained by drying, which can be achieved by natural drying, heat drying, vacuum drying, or the like.
[0054] The weight average molecular weight (Mw) of the polysuccinimide obtained by the polymerization reaction of the aspartic acid composition is not particularly limited. The polymerization reaction can be terminated when polysuccinimide having a desired weight average molecular weight is produced. The Mw of the polysuccinimide is, for example, 50,000 or more, or 60,000 or more. The Mw range of the polysuccinimide is, for example, 10,000 to 200,000, or 20,000 to 200,000. Mw is a polystyrene equivalent value measured by the GPC method.
[0055] In the method of this embodiment, the aspartic acid composition is used to carry out a polymerization reaction of aspartic acid. Therefore, a high molecular weight polysuccinimide can be obtained. In addition, since the polymerization reaction of aspartic acid is promoted, the polymerization reaction time can be shortened.
[0056] [Polysuccinimide composition] In one aspect, the present invention provides a polysuccinimide composition. The polysuccinimide composition includes polysuccinimide and impurities. The impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof. The content of the impurities in the polysuccinimide composition is 0.001% by mass or more and 1.1% by mass or less.
[0057] The term "polysuccinimide composition" refers to a composition containing polysuccinimide as a main component. The polysuccinimide composition can be obtained by a polymerization reaction of the aspartic acid composition. For example, the polysuccinimide composition can be obtained by carrying out the method for producing polysuccinimide. The polysuccinimide composition can also be said to be a polymerization reaction product of the aspartic acid composition.
[0058] The polysuccinimide composition contains polysuccinimide and impurities. The "impurities" in the polysuccinimide composition refer to components other than polysuccinimide contained in the polysuccinimide composition. In one embodiment, the impurities contain at least one selected from the group consisting of amino acids other than aspartic acid and organic acids. The impurities preferably contain amino acids other than aspartic acid.
[0059] The amino acid as an impurity may be the same as the amino acid as an impurity in the aspartic acid composition. The content of the amino acid as an impurity is preferably 0 to 1.1 parts by mass, more preferably 0.001 to 1.1 parts by mass, more preferably 0.001 to 0.5 parts by mass, more preferably 0.001 to 0.3 ... The amino acid as an impurity may be in the form of a salt. Examples of the salt of the amino acid include the same as those mentioned above. The content range exemplified for the amino acid as an impurity is also applied when the amino acid as an impurity is in the form of a salt. When both the amino acid and the salt of the amino acid are included as impurities, the content range exemplified above is applied to the total content of both.
[0060] The organic acid as an impurity may be the same as the organic acid as an impurity in the aspartic acid composition. The content of the organic acid as an impurity is preferably 0 to 1.1 parts by mass, more preferably 0.001 to 0.5 parts by mass, and even more preferably 0.001 to 0.3 parts by mass, relative to 100 parts by mass of polysuccinimide. The organic acid as an impurity may be in the form of a salt. Examples of the salt of the organic acid include the same as those mentioned above. The range of the content exemplified for the organic acid as an impurity is also applied when the organic acid as an impurity is in the form of a salt. When both an organic acid and a salt of an organic acid are contained as impurities, the range of the content exemplified above is applied to the total content of both.
[0061] By keeping the content of the impurities within the above range, the hydrolysis reaction and / or crosslinking reaction of the polysuccinimide is promoted without any problems, and as a result, a desired crosslinked polyaspartic acid composition can be obtained.
[0062] The Mw of the polysuccinimide contained as the main component of the polysuccinimide composition is not particularly limited. The Mw of the polysuccinimide is, for example, 50,000 or more, or 60,000 or more. The Mw of the polysuccinimide is, for example, 50,000 to 200,000, or 60,000 to 200,000.
[0063] The impurities may include components other than amino acids other than aspartic acid, organic acids, and their salts, such as, for example, sulfates.
[0064] The content of polysuccinimide in the polysuccinimide composition is, for example, 99 mass % or more and 99.999 mass % or less based on the total mass of all components of the polysuccinimide composition.
[0065] The polysuccinimide composition can be used in the production of polyaspartic acid.
[0066] [Polyaspartic acid composition and method for producing polyaspartic acid composition] In one embodiment, the present invention provides a polyaspartic acid composition that is a hydrolyzate of the polysuccinimide composition.
[0067] By hydrolyzing the polysuccinimide composition, the polysuccinimide in the polysuccinimide composition is hydrolyzed to become polyaspartic acid. Therefore, a polyaspartic acid composition can be obtained as a hydrolyzate of the polysuccinimide composition. In the polyaspartic acid composition, the polyaspartic acid is usually present in the form of a salt. In this specification, the term "polyaspartic acid" also includes salts of polyaspartic acid, unless otherwise specified. The polyaspartic acid composition is a hydrolysate of the succinimide composition, and therefore may contain the same impurities as those in the succinimide composition.
[0068] The amino acid as an impurity may be the same as the amino acid as an impurity in the aspartic acid composition. The content of the amino acid as an impurity may be 0 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.0 parts by mass or less, 0.001 parts by mass or more and 0.98 parts by mass or less, 0.005 parts by mass or more and 0.95 parts by mass or less, 0.010 parts by mass or more and 0.90 parts by mass or less, 0.020 parts by mass or more and 0.80 parts by mass or less, 0.05 parts by mass or more and 0.70 parts by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less, relative to 100 parts by mass of polyaspartic acid. These upper and lower limit values may be used in any combination. The amino acid as an impurity may be in the form of a salt. Examples of the salt of the amino acid include the same as those mentioned above. The content range exemplified for the amino acid as an impurity is also applied when the amino acid as an impurity is in the form of a salt. When both the amino acid and the salt of the amino acid are included as impurities, the content range exemplified above is applied to the total content of both.
[0069] The content of the organic acid as an impurity may be 0 parts by mass or more and 1.1 parts by mass or less, 0.001 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.1 parts by mass or less, 0.02 parts by mass or more and 1.0 parts by mass or less, 0.001 parts by mass or more and 0.98 parts by mass or less, 0.005 parts by mass or more and 0.95 parts by mass or less, 0.010 parts by mass or more and 0.90 parts by mass or less, 0.020 parts by mass or more and 0.80 parts by mass or less, 0.05 parts by mass or more and 0.70 parts by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less, relative to 100 parts by mass of polyaspartic acid. Any combination of these upper and lower limit values may be used. The organic acid as an impurity may be in the form of a salt. Examples of the salt of the organic acid include the same as those mentioned above. The range of the content exemplified for the organic acid as an impurity is also applied when the organic acid as an impurity is in the form of a salt. When both an organic acid and a salt of an organic acid are contained as impurities, the range of the content exemplified above is applied to the total content of both.
[0070] The polyaspartic acid composition contains impurities in an amount of 0.02% by mass or more and 1.1% by mass or less, based on the total mass of all components of the polyaspartic acid composition. The content of impurities may be 0.021% by mass or more and 1.1% by mass or less, 0.025% by mass or more and 1.1% by mass or less, 0.02% by mass or more and 1.0% by mass or less, 0.02% by mass or more and 0.98% by mass or less, 0.02% by mass or more and 0.95% by mass or less, 0.02% by mass or more and 0.90% by mass or less, 0.020% by mass or more and 0.80% by mass or less, 0.02% by mass or more and 0.70% by mass or less, 0.05 parts by mass or more and 0.50 parts by mass or less, or 0.05 parts by mass or more and 0.30 parts by mass or less, based on the total mass of all components of the polyaspartic acid composition. Any combination of these upper and lower limit values may be used.
[0071] Therefore, in one aspect, the present invention provides a method for producing a polyaspartic acid composition, comprising: a step of using the aspartic acid composition to perform a polymerization reaction of the aspartic acid to obtain a polysuccinimide composition containing polysuccinimide (hereinafter also referred to as "step (i)"); and a step of using the polysuccinimide composition to perform a hydrolysis reaction of the polysuccinimide to obtain a polyaspartic acid composition containing polyaspartic acid (hereinafter also referred to as "step (ii)").
[0072] <Process (i)> Step (i) is a step of carrying out a polymerization reaction of the aspartic acid using the aspartic acid composition to obtain a polysuccinimide composition containing polysuccinimide. Step (i) can be carried out in the same manner as the method described in the above section [Method for producing polysuccinimide].
[0073] <Process (ii)> Step (ii) is a step of using the polysuccinimide composition to carry out a hydrolysis reaction of the polysuccinimide to obtain a polyaspartic acid composition containing polyaspartic acid.
[0074] The hydrolysis reaction of the polysuccinimide in the polysuccinimide composition can be carried out by a known method. The hydrolysis reaction can be carried out under alkaline conditions. For example, the hydrolysis reaction of the polysuccinimide can be carried out by adding a base to the polysuccinimide composition and reacting it with the polysuccinimide.
[0075] Examples of the base include hydroxides of alkali metals, carbonates of alkali metals, hydroxides of alkaline earth metals, carbonates of alkaline earth metals, and ammonia. Examples of the alkali metals include potassium, sodium, and lithium. Examples of the alkaline earth metals include calcium and magnesium. Among them, hydroxides of alkali metals are preferred, NaOH, KOH, LiOH, and the like are more preferred, and an aqueous solution of NaOH is even more preferred. The base is preferably added to the polysuccinimide composition as an aqueous alkaline solution. The aqueous alkaline solution has a pH of preferably 10 to 14, and more preferably 12 to 14 at 25° C. The concentration of the base in the aqueous alkaline solution is not particularly limited, and may be, for example, 0.5 to 50% by mass.
[0076] The amount of the base used may be sufficient to hydrolyze the polysuccinimide in the polysuccinimide composition to polyaspartic acid. For example, the number of moles of the base may be within the range of 90 to 120% of the total number of moles of the carboxyl group and the imide group of the polysuccinimide in the polysuccinimide composition.
[0077] The temperature in the hydrolysis reaction may be any temperature that does not cause hydrolysis of the polymer main chain. The temperature in the hydrolysis reaction is, for example, preferably 10 to 70°C, and more preferably 40 to 60°C. The time of the hydrolysis reaction is not particularly limited, and may be selected appropriately depending on the amount of the polysuccinimide composition, so long as it is a time sufficient for hydrolyzing the polysuccinimide in the polysuccinimide composition to polyaspartic acid. The time of the hydrolysis reaction may be, for example, 1 minute to 100 hours, preferably 30 minutes to 50 hours, and more preferably 1 hour to 10 hours.
[0078] The polyaspartic acid in the polyaspartic acid composition obtained in step (ii) is in the form of a salt. When an alkali metal hydroxide or carbonate is used as the base, the polyaspartic acid is in the form of a salt with the alkali metal. When an alkaline earth metal hydroxide or carbonate is used as the base, the polyaspartic acid is in the form of a salt with the alkaline earth metal. When ammonia is used as the base, the polyaspartic acid is in the form of the ammonium salt. The polyaspartic acid salt may be neutralized with an acid as appropriate to give polyaspartic acid that does not form a salt.
[0079] The polyaspartic acid composition may contain a polymer in which some of the succinimide structural units remain. For example, the polyaspartic acid composition may contain a polymer having an aspartic acid structural unit and a polysuccinimide structural unit. The proportion of the succinimide structural unit in the polymer is preferably 3 mol % or less, more preferably 1 mol % or less, based on the total structural units of the polymer.
[0080] [Crosslinked polyaspartic acid composition and method for producing crosslinked polyaspartic acid composition] In one aspect, the present invention provides a crosslinked polyaspartic acid composition which is a crosslinking reaction product of the polyaspartic acid composition.
[0081] By carrying out a crosslinking reaction of the polyaspartic acid composition, the polyaspartic acid in the polyaspartic acid composition is crosslinked to become a crosslinked polyaspartic acid. Therefore, a crosslinked polyaspartic acid composition can be obtained as a crosslinking reaction product of the polyaspartic acid composition. In the crosslinked polyaspartic acid composition, the crosslinked polyaspartic acid may or may not be in the form of a salt. In this specification, the term "crosslinked polyaspartic acid" also includes salts of crosslinked polyaspartic acid. The crosslinked polyaspartic acid composition is a crosslinking reaction product of the polyaspartic acid composition, and therefore may contain the same impurities as the polyaspartic acid composition.
[0082] Therefore, in one aspect, the present invention provides a method for producing a crosslinked polyaspartic acid composition, comprising: a step of obtaining a polyaspartic acid composition by the method for producing a polyaspartic acid composition (hereinafter also referred to as "step (iii)"); and a step of using the polyaspartic acid composition to perform a crosslinking reaction of the polyaspartic acid to obtain a crosslinked polyaspartic acid composition containing crosslinked polyaspartic acid (hereinafter also referred to as "step (iv)").
[0083] <Step (iii)> Step (iii) is a step of obtaining a polyaspartic acid composition by the method for producing a polyaspartic acid composition. Step (iii) can be performed in the same manner as described in the section [Polyaspartic acid composition, method for producing a polyaspartic acid composition].
[0084] <Process (iv)> The step (iv) is a step of carrying out a crosslinking reaction of the polyaspartic acid using the polyaspartic acid composition to obtain a crosslinked polyaspartic acid composition containing crosslinked polyaspartic acid.
[0085] The crosslinking reaction of the polyaspartic acid in the polyaspartic acid composition can be carried out by a known method. The crosslinking reaction can be carried out using a crosslinking agent. For example, the crosslinking reaction of the polyaspartic acid can be carried out by adding a crosslinking agent to the polyaspartic acid composition and reacting it with the polyaspartic acid. Alternatively, the crosslinking reaction of the polyaspartic acid can be carried out by irradiating the polyaspartic acid composition with gamma rays.
[0086] The crosslinking agent is not particularly limited, and any known crosslinking agent can be used. Examples of the crosslinking agent include polyfunctional epoxy compounds and basic polyamino acid compounds.
[0087] Examples of the polyfunctional epoxy compound include polyglycidyl ethers of alkane polyols (e.g., having 2 to 6 carbon atoms) and poly(alkylene glycols) (e.g., having 2 to 6 carbon atoms), such as ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, and butanediol diglycidyl ether; sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ether, erythritol polyglycidyl ether, trimethylolethane, and the like. Examples of the polyglycidyl ether include polyglycidyl ethers of alkane polyols (e.g., having 2 to 6 carbon atoms) and poly(alkylene glycols) (e.g., having 2 to 6 carbon atoms), such as triglycidyl ether and trimethylolpropane polyglycidyl ether; diepoxy alkanes (e.g., having 4 to 8 carbon atoms), such as 1,2,3,4-diepoxybutane, 1,2,4,5-diepoxypentane, 1,2,5,6-diepoxyhexane, 1,2,7,8-diepoxyoctane, 1,4- and 1,3-divinylbenzene epoxide; and polyphenol polyglycidyl ethers (e.g., having 6 to 15 carbon atoms), such as 4,4'-isopropylidenediphenol diglycidyl ether (bisphenol A diglycidyl ether) and hydroquinone diglycidyl ether. The polyfunctional epoxy compounds may be used alone or in combination of two or more kinds.
[0088] Examples of basic polyamino acid compounds include dimers containing basic amino acids such as glycine-lysine, lysine-glycine, alanine-lysine, and lysine-phenylalanine; polylysine, polyarginine, copolymers of lysine and arginine, and copolymers of basic amino acids and other amino acids. The basic polyamino acid compounds may form salts with inorganic acids, organic acids, and the like. The basic polyamino acid compounds may be used alone or in combination of two or more kinds.
[0089] The amount of the crosslinking agent used may be sufficient to crosslink the polyaspartic acid in the polyaspartic acid composition. The amount of the crosslinking agent used may be appropriately selected depending on the degree to which the polyaspartic acid is crosslinked. The amount of the crosslinking agent used is not particularly limited, but may be, for example, 0.5 to 50 parts by mass, preferably 1 to 20 parts by mass, and more preferably 10 to 10 parts by mass, relative to 100 parts by mass of the polyaspartic acid composition.
[0090] The temperature in the crosslinking reaction can be appropriately selected depending on the type of crosslinking agent. When the crosslinking agent is a polyfunctional epoxy compound, the temperature in the crosslinking reaction is, for example, preferably 10 to 120°C, more preferably 20 to 60°C. When the crosslinking agent is a basic polyamino acid compound, the temperature in the crosslinking reaction is preferably 10 to 120°C, more preferably 30 to 80°C. The time of the crosslinking reaction is not particularly limited, and may be selected appropriately according to the amount of the polyaspartic acid composition, as long as it is sufficient for the polyaspartic acid in the polyaspartic acid composition to be crosslinked. The time of the crosslinking reaction may be, for example, 1 minute to 100 hours. The time of the crosslinking reaction is not particularly limited, but is preferably, for example, 1 minute to 50 hours, and more preferably, 1 minute to 10 hours.
[0091] The polyaspartic acid in the polyaspartic acid composition used in step (iv) may be in the form of a salt or may not be in the form of a salt. When a polyaspartic acid composition in the form of a salt is used in step (iv), the crosslinked polyaspartic acid in the resulting crosslinked polyaspartic acid composition is in the form of a salt. When a polyaspartic acid composition not in the form of a salt is used in step (iv), the crosslinked polyaspartic acid in the resulting crosslinked polyaspartic acid composition is not in the form of a salt. When the crosslinked polyaspartic acid in the crosslinked polyaspartic acid is in the form of a salt, it may be appropriately neutralized with an acid to form a crosslinked polyaspartic acid not in the form of a salt.
[0092] [Crosslinked polysuccinimide composition and method for producing crosslinked polysuccinimide composition] In one embodiment, the present invention provides a crosslinked polysuccinimide composition which is a crosslinking reaction product of the polysuccinimide composition. In one embodiment, the present invention provides a crosslinked polyaspartic acid composition which is a hydrolysate of the crosslinked polysuccinimide composition.
[0093] By carrying out the crosslinking reaction of the polysuccinimide composition, the polysuccinimide in the polysuccinimide composition is crosslinked to become a crosslinked polysuccinimide, so that a crosslinked polysuccinimide composition can be obtained as a crosslinking reaction product of the polysuccinimide composition. The crosslinked polysuccinimide composition is a crosslinking reaction product of the polysuccinimide composition, and therefore may contain the same impurities as the polysuccinimide composition.
[0094] By carrying out the hydrolysis reaction of the crosslinked polysuccinimide composition, the crosslinked polysuccinimide in the crosslinked polysuccinimide composition is hydrolyzed to become crosslinked polyaspartic acid. Therefore, a crosslinked polyaspartic acid composition can be obtained as a hydrolyzate of the crosslinked polysuccinimide composition. In the crosslinked polyaspartic acid composition, the crosslinked polyaspartic acid is usually present in the form of a salt. In this specification, the term "crosslinked polyaspartic acid" also includes salts of crosslinked polyaspartic acid, unless otherwise specified. The crosslinked polyaspartic acid composition is a hydrolysate of the crosslinked polysuccinimide composition, and therefore may contain the same impurities as those in the crosslinked polysuccinimide composition.
[0095] Therefore, in one aspect, the present invention provides a method for producing a crosslinked polyaspartic acid composition, comprising the steps of: using the aspartic acid composition to carry out a polymerization reaction of the aspartic acid to obtain a polysuccinimide composition containing polysuccinimide (hereinafter also referred to as "step (I)"); using the polysuccinimide composition to carry out a crosslinking reaction of the polysuccinimide to obtain a crosslinked polysuccinimide composition containing crosslinked polysuccinimide (hereinafter also referred to as "step (II)"); and using the crosslinked polysuccinimide composition to carry out a hydrolysis reaction of the crosslinked polysuccinimide to obtain a crosslinked polyaspartic acid composition containing crosslinked polyaspartic acid (hereinafter also referred to as "step (III)").
[0096] <Process (I)> Step (I) is a step of carrying out a polymerization reaction of the aspartic acid using the aspartic acid composition to obtain a polysuccinimide composition containing polysuccinimide. Step (I) can be carried out in the same manner as the method described in the above section [Method for producing polysuccinimide].
[0097] <Process (II)> Step (II) is a step of using the polysuccinimide composition to carry out a crosslinking reaction of the polysuccinimide to obtain a crosslinked polysuccinimide composition containing a crosslinked polysuccinimide.
[0098] The crosslinking reaction of the polysuccinimide in the polysuccinimide composition can be carried out by a known method. The crosslinking reaction can be carried out using a crosslinking agent. For example, the crosslinking reaction of the polysuccinimide can be carried out by adding a crosslinking agent to the polysuccinimide composition and reacting it with the polysuccinimide. Alternatively, the crosslinking reaction of the polysuccinimide can be carried out by irradiating the polysuccinimide composition with gamma rays.
[0099] The crosslinking agent is not particularly limited, and any known crosslinking agent can be used, such as an amine compound, hydrazine, chitosan, etc.
[0100] The amine compound may, for example, be an organic compound having two or more amino groups. The amino group may, for example, be a primary amino group or a secondary amino group. The amino group is preferably a primary amino group because it has high reactivity with polysuccinimide and is easy to adjust the degree of crosslinking. The amino group is preferably an amino group that substitutes a hydrogen atom of an aliphatic hydrocarbon group because it has high reactivity with polysuccinimide. Specific examples of the amino group include, for example, an alkylamino group, an aralkylamino group, a benzylamino group, and the like. Examples of the amine compound include aliphatic polyamines such as ethylenediamine, propylenediamine, 1,4-butanediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, tetradecamethylenediamine, hexadecamethylenediamine, 1-amino-2,2-bis(aminomethyl)butane, tetraaminomethane, diethylenetriamine, and triethylenetetramine; alicyclic polyamines such as norbornenediamine, 1,4-diaminocyclohexane, 1,3,5-triaminocyclohexane, and isophoronediamine; aromatic polyamines such as phenylenediamine, tolylenediamine, and xylylenediamine; polyamines such as basic amino acids or esters thereof; and polyamines such as a compound in which one or more molecules of a monoamino compound are bonded by one or more disulfide bonds (e.g., cystamine) or a derivative thereof. The amine compound may be an amino acid having two or more amino groups, such as lysine, cystine, or ornithine, or a salt or ester thereof.
[0101] Furthermore, specific examples of trifunctional or higher functional amine compounds include 1,1,1-tris(2'-aminomethyl)ethane, tetrakis(2'-aminomethyl)methane, 1,1,1-tris(2'-aminoethyl)ethane, tetrakis(2'-aminoethyl)methane, 1,1,1-tris(2'-aminopropyl)ethane, tetrakis(2'-aminopropyl)methane, 1,1,1-tris(2'-aminobutyl)ethane, tetrakis(2'-aminobutyl)methane, 1,2,3-tris(aminomethyl)benzene, 1,2,4-tris(aminomethyl)benzene, and 1,3,5-tris(aminomethyl)benzene.
[0102] The crosslinking agent may be a polymer of an amine compound. Specific examples of crosslinking agents that are polymers include dipeptides having a basic amino acid at the C-terminus, such as glycine-lysine, alanine-lysine, glycine-ornithine, and alanine-ornithine; dipeptides having a basic amino acid at the N-terminus, such as lysine-glycine, lysine-alanine, ornithine-glycine, ornithine-alanine, lysine-lysine, ornithine-lysine, lysine-ornithine, and ornithine-ornithine; glycine-glycine-lysine, glycine-lysine-glycine, glycine-glycine-ornithine, and glycine-ornithine-glycine. , oligopeptides containing at least one basic amino acid such as lysine-lysine-lysine, ornithine-ornithine-ornithine, glycine-glycine-glycine-lysine, and glycine-ornithine-glycine-glycine; polypeptides such as polylysine, polyarginine, a copolymer of lysine and arginine, a copolymer of lysine and aspartic acid, a copolymer of lysine and glutamic acid, and a copolymer of a basic amino acid and another amino acid; and polymers of amino group-containing monomers such as polyethyleneimine, polyallylamine, chitosan, and peptides. When the crosslinking agent is a polymer, the degree of polymerization of the polymer is not particularly limited and can be appropriately selected in consideration of the solubility in the organic solvent used in the reaction, etc.
[0103] Examples of crosslinking agents that are highly biodegradable and have excellent reactivity with polysuccinimide include ethylenediamine, propylenediamine, 1,4-butanediamine, heptamethylenediamine, hexamethylenediamine, lysine, ornithine, and cystamine.
[0104] The amount of the crosslinking agent used may be sufficient to crosslink the polysuccinimide in the polysuccinimide composition. The amount of the crosslinking agent used may be appropriately selected depending on the degree to which the polysuccinimide is crosslinked. The amount of the crosslinking agent used is not particularly limited, but may be, for example, 0.5 to 50 parts by mass, preferably 1 to 20 parts by mass, and more preferably 10 to 10 parts by mass, relative to 100 parts by mass of the polysuccinimide composition.
[0105] The temperature in the crosslinking reaction can be appropriately selected depending on the type of crosslinking agent, and is preferably, for example, 10 to 120°C, and more preferably 20 to 60°C. The time of the crosslinking reaction is not particularly limited, and may be selected appropriately according to the amount of the polysuccinimide composition, as long as it is a time sufficient for the polysuccinimide in the polysuccinimide composition to crosslink. The time of the crosslinking reaction may be, for example, 1 minute to 100 hours. The time of the crosslinking reaction is not particularly limited, but is preferably, for example, 1 minute to 50 hours, and more preferably, 1 minute to 10 hours. The crosslinking reaction may be carried out in an organic solvent or in an aqueous solution. Examples of the solvent used in the crosslinking reaction include water; alcohols such as methanol, ethanol, propanol, isopropanol, butanol, pentanol, hexanol, heptanol, octanol, 2-methoxyethanol, and 2-ethoxyethanol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, and dipropylene glycol; glycosolves such as methyl glycosolve and ethyl glycosolve; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; cyclic ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as petroleum ether, pentane, hexane, heptane, octane, cyclohexane, and decalin; aromatic hydrocarbons such as benzene, toluene, ethylbenzene, and xylene; aromatic ethers such as diphenyl ether and anisole; and phenols such as cresol. Further, examples of the solvent used in the crosslinking reaction include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, N,N'-dimethylimidazolidinone, dimethylsulfoxide, sulfolane, etc. These solvents may be used alone or in combination of two or more.
[0106] <Process (III)> The step (III) is a step of using the crosslinked polysuccinimide composition to carry out a hydrolysis reaction of the crosslinked polysuccinimide to obtain a crosslinked polyaspartic acid composition containing a crosslinked polyaspartic acid.
[0107] The hydrolysis reaction of the crosslinked polysuccinimide in the crosslinked polysuccinimide composition can be carried out by a known method. The hydrolysis reaction can be carried out under alkaline conditions. For example, the hydrolysis reaction of the crosslinked polysuccinimide can be carried out by adding a base to the crosslinked polysuccinimide composition and reacting it with the crosslinked polysuccinimide.
[0108] Examples of the base include hydroxides of alkali metals, carbonates of alkali metals, hydroxides of alkaline earth metals, carbonates of alkaline earth metals, ammonia, organic amine compounds (triethylamine, N-methylmorpholine, triethanolamine, diisopropylethylamine, etc.), etc. Examples of the alkali metals and alkaline earth metals include the same as those mentioned above.
[0109] The amount of base used may be sufficient to hydrolyze the crosslinked polysuccinimide in the crosslinked polysuccinimide composition to crosslinked polyaspartic acid. For example, the number of moles of the base may be within the range of 90 to 120% of the total number of moles of the carboxyl group and the imide group of the crosslinked polysuccinimide in the crosslinked polysuccinimide composition.
[0110] The temperature in the hydrolysis reaction may be any temperature that does not cause hydrolysis of the polymer main chain. The temperature in the hydrolysis reaction is, for example, preferably 10 to 70°C, and more preferably 40 to 60°C. The time of hydrolysis reaction is not particularly limited, and it is sufficient to hydrolyze the crosslinked polysuccinimide in the crosslinked polysuccinimide composition to crosslinked polyaspartic acid, and can be appropriately selected according to the amount of the crosslinked polysuccinimide composition. The time of hydrolysis reaction can be, for example, 1 minute to 100 hours. 30 minutes to 50 hours is preferable, and 1 hour to 10 hours is more preferable.
[0111] The crosslinked polyaspartic acid in the crosslinked polyaspartic acid composition obtained in step (III) is in the form of a salt. When a hydroxide or carbonate of an alkali metal is used as the base, the crosslinked polyaspartic acid is in the form of a salt with the alkali metal. When a hydroxide or carbonate of a crosslinked alkaline earth metal is used as the base, the crosslinked polyaspartic acid is in the form of a salt with the alkaline earth metal. When ammonia is used as the base, the crosslinked polyaspartic acid is in the form of the ammonium salt. When an organic amine is used as the base, the crosslinked polyaspartic acid is in the form of a salt with the organic amine. The salt of the crosslinked polyaspartic acid may be neutralized with an acid as appropriate to form a crosslinked polyaspartic acid that does not form a salt.
[0112] The crosslinked polyaspartic acid composition may contain a polymer in which some of the succinimide structural units remain. For example, the crosslinked polyaspartic acid composition may contain a polymer having an aspartic acid structural unit and a polysuccinimide structural unit. The proportion of the succinimide structural unit in the polymer is preferably 3 mol % or less, more preferably 1 mol % or less, based on the total structural units of the polymer.
[0113] [Surface modified crosslinked polyaspartic acid composition] In one aspect, the present invention provides a surface-modified cross-linked polyaspartic acid composition comprising particles of the cross-linked polyaspartic acid composition, the surfaces of the particles being modified with inorganic particles.
[0114] The crosslinked polyaspartic acid composition may be in the form of particles, and the surface of the particles may be modified with inorganic particles. The inorganic particles are preferably water-insoluble inorganic particles. Examples of the inorganic particles include metal oxides such as aluminum oxide, titanium oxide, zinc oxide, and silicon dioxide. The crosslinked polyaspartic acid composition particles can be obtained by physically pulverizing the dried crosslinked polyaspartic acid composition. The surface-modified crosslinked polyaspartic acid composition can be obtained by reacting the crosslinked polyaspartic acid composition particles with inorganic particles such as fumed silica. The reaction between the crosslinked polyaspartic acid composition particles and the inorganic particles can be carried out by heating to, for example, 100 to 200°C. The reaction time is not particularly limited, but may be, for example, 10 to 60 minutes.
[0115] [Products containing cross-linked polyaspartic acid] In one aspect, the present invention provides a crosslinked polyaspartic acid-containing product comprising a crosslinked polyaspartic acid composition.
[0116] In one aspect, the present invention provides a method for producing a crosslinked polyaspartic acid-containing product, comprising the steps of obtaining a crosslinked polyaspartic acid composition by the method for producing a crosslinked polyaspartic acid composition, and producing a crosslinked polyaspartic acid-containing product using the crosslinked polyaspartic acid composition.
[0117] The crosslinked polyaspartic acid composition obtained as described above can be used for various applications. "Crosslinked polyaspartic acid-containing product" refers to a product containing the crosslinked polyaspartic acid composition. The crosslinked polyaspartic acid-containing product is not particularly limited as long as it contains the crosslinked polyaspartic acid composition. Examples of crosslinked polyaspartic acid-containing products include, but are not limited to, surfactants, thickeners, viscosity reducers, swelling agents, water absorbents, gelling agents, binders, film-forming agents, flocculants, adhesives, surface modifiers, or sustained release agents.
[0118] Examples of products using the surface active effect of the crosslinked polyaspartic acid composition include emulsifiers, emulsion breakers, dispersants, flocculants, antistatic agents, etc. Examples of dispersants include pigment dispersants, dispersants for agricultural chemical granules, dispersants for pulverized coal, cement dispersants, concrete admixtures, cleaning dispersants for lubricating oils, pour point depressants, plastic coloring aids, compatibilizers, etc. Examples of flocculants include polymer flocculants, drainage and retention improvers, sludge coagulants, etc. Examples of products using the surface active effect of the crosslinked polyaspartic acid composition also include leveling agents, retarders, foaming agents, foam boosters, foam boosters, foam stabilizers, soap bubble solutions, defoamers, solubilizers, agents for extending the life of cut flowers, lubricants, etc.
[0119] Examples of products which utilize the thickening effect of the crosslinked polyaspartic acid composition include stabilizers, poultices, polymers for quenching oils, polymers for hydraulic fluids, polymers for increasing crude oil production (e.g., polymers used in mining or well drilling (e.g., temporary sealing materials, dispersions for oil drilling assistance, flow control materials, or polymers in well treatment fluids), printing pastes, etc. Examples of products which utilize the thickening effect of the crosslinked polyaspartic acid composition include plasticizers, etc.
[0120] Examples of products that utilize the swelling action of the crosslinked polyaspartic acid composition include, for example, drug carriers, drug volatilizers, drug holders, electrical equipment related materials such as waterproofing materials for communication cables, gaskets and packings, civil engineering sealants, architectural sealants, lost circulation prevention agents for shield construction, water-swelling toys, sealants, and artificial snow.
[0121] Examples of products using the water absorbing action of the crosslinked polyaspartic acid composition include, for example, moisturizers, dehumidifiers, humidity conditioners, moisture absorbents, water retaining materials, etc. Furthermore, examples of products using these include sanitary products, diapers, breast milk pads, incontinence pads, medical underpads, disposable dustcloths, pet sheets, portable toilets, disposable warmers, wound protection dressings, medical blood absorbers, sweat absorbent fibers, wet tissues, deodorizing and dehumidifying sheets, food freshness preserving agents, dehydrating agents in the food field, food packaging materials such as drip absorbent sheets, transport materials such as water absorbent sheets for transporting fresh vegetables, construction materials for preventing condensation, recording paper for ink jets, moisture-proof coating agents for printed wiring boards, waterproofing agents for concrete, dehydrating agents for gasoline, moisture removers for gasoline, dehydrating agents for oils, moisture removers for oils, etc. Examples of agricultural products include water retention materials, soil conditioners, floral foams (materials for fixing cut flowers), seedling beds, hydroponic vegetation sheets, seed tapes, fluid sowing media, agricultural sheets for preventing condensation, and irrigation solutions.
[0122] Examples of products that utilize the gelling action of the crosslinked polyaspartic acid composition include deodorants, odor eliminators, cooling materials, oil absorbing polymers, and the like.
[0123] Examples of products which utilize the binding action of the crosslinked polyaspartic acid composition include scale inhibitors, tartar inhibitors, heavy metal elution inhibitors, heavy metal immobilizing agents, selenium treatment agents, epoxy resin hardeners, builders, resin strengtheners, dye fixing agents, textile dye-resistant processing agents, fabric processing agents, and deodorizing and antibacterial finishing agents for laundry.
[0124] Examples of products that utilize the film-forming action of the crosslinked polyaspartic acid composition include, for example, rust inhibitors, packaging materials (e.g., packaging materials for food, medicines, electronic materials, etc.), general industrial films, films for packaging materials, coating agents, paints, inks, inkjet inks, water-based inks, inks for ballpoint pens, metallic glossy colored inks, erasable inks, refills for writing instruments, tablet coating agents, seamless capsule bases for storing medicines in the inner space, polymers for floor polish, polymers for paints, masking agents, plastic hard coat agents, polymers for photoresists, coating agents for electromagnetic wave shielding, and fire extinguishing agents.
[0125] Examples of products that utilize the coagulation or adhesion action of the crosslinked polyaspartic acid composition include cultured cell sheets, cohesives, binders for printing inks, water-soluble binders, binders for nonwoven fabrics, binders for plastic reinforcing fibers, binders for electrophotographic toners, binders for magnetic tapes, binders for resin concrete, binders for casting sand, binders for fine ceramics, sealing materials (e.g., sealing materials for electronic devices or optical fibers), adhesives, and the like.
[0126] Examples of products that utilize the surface modifying effect of the crosslinked polyaspartic acid composition include fiber treatment agents, noodle texture improvers, primers, and the like.
[0127] Examples of products that utilize the sustained release effect of the crosslinked polyaspartic acid composition include sustained release agents (such as substrates that sustain the release of active ingredients of cosmetics, medicines, agricultural chemicals, fertilizers, etc.).
[0128] In addition, products containing the above-mentioned products as raw materials can be used for applications such as cosmetics, fragrances, pharmaceuticals, quasi-drugs, pharmaceutical-related materials, medical-related products, health-related products, sanitary products, daily necessities, agricultural materials, food-related materials, civil engineering-related materials, construction-related materials, electrical equipment-related materials, electronic equipment-related materials, writing-related materials, painting-related materials, printing-related materials, electronic printing-related materials, manufacturing process-related materials, analysis-related materials, well-related materials, dyeing-related materials, cloth treatment-related materials, papermaking-related materials, environmental treatment materials, binders, etc.
[0129] The crosslinked polyaspartic acid-containing product can be produced by a known method suitable for the product, using a crosslinked polyaspartic acid composition as a raw material. EXAMPLES
[0130] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples.
[0131] [Evaluation of polymerization reaction using aspartic acid composition] <Preparation of Aspartic Acid Composition> (Example 1, Example 2, Comparative Example 1) Corynebacterium glutamicum was cultured and the culture supernatant was purified to obtain the aspartic acid composition of each example.
[0132] (Reference example 1) L-aspartic acid was purchased from YIXING QIANCHENG BIO-ENGINEERING Co., Ltd. and used as the aspartic acid composition.
[0133] <Analysis of Aspartic Acid Composition> Amino acids were analyzed using an amino acid analyzer. Organic acids were analyzed using high performance liquid chromatography. The composition of the aspartic acid composition of each example is shown in Table 1. The values in Table 1 are mass % relative to the total mass (100 mass %) of the aspartic acid composition. "0.00" indicates less than 0.005 mass %.
[0134] [Table 1]
[0135] <Production of polysuccinimide by solid-state polymerization (1)> Polysuccinimide was synthesized by solid-phase polymerization using the aspartic acid composition of each example. 160 parts by mass of the aspartic acid composition and 97 parts by mass of 85% phosphoric acid were mixed in a mortar, transferred to a tray, and reacted at 190°C and 1.3 kPa for 6 hours. During the reaction, samples were appropriately taken, and the weight average molecular weight (Mw) of the polysuccinimide was measured. The reaction mixture was ground, and then washed with distilled water until the filtrate became neutral. The washed composition was vacuum dried at 80° C. to obtain a polysuccinimide composition.
[0136] <Production of polysuccinimide by solid-state polymerization (2a)> Polysuccinimide was synthesized by solid-phase polymerization using the aspartic acid composition of each example. 160 parts by mass of the aspartic acid composition and 83 parts by mass of 85% phosphoric acid were mixed in a mortar, transferred to a tray, and reacted at 190°C and 1.3 kPa for 6 hours. During the reaction, samples were appropriately taken, and the weight average molecular weight (Mw) of the polysuccinimide was measured. The reaction mixture was ground, and then washed with distilled water until the filtrate became neutral. The washed composition was vacuum dried at 80° C. to obtain a polysuccinimide composition.
[0137] <Production of polysuccinimide by solid-state polymerization using a kneader (2b)> Polysuccinimide was synthesized by solid-phase polymerization using a kneader using the aspartic acid composition of each example. 160 parts by mass of the aspartic acid composition and 97 parts by mass of 85% phosphoric acid were charged into a kneader with a Banbury blade and mixed for 10 minutes. Then, using a heater block attached to the kneader, the mixture was stirred while being heated from room temperature to an internal temperature of 190°C. After reaching 190°C, the mixture was reduced in pressure to 9.3 kPa and reacted for 3 hours. The reaction mixture was pulverized and then washed with distilled water until the filtrate became neutral. The washed composition was vacuum-dried at 80°C to obtain a polysuccinimide composition.
[0138] <Measurement of weight average molecular weight (Mw) of polysuccinimide> The weight average molecular weight (Mw) of polysuccinimide was determined as a polystyrene equivalent value by the GPC method (differential refractometer). For the measurement, a G1000HHR column, a G4000HHR column, and a GMHHR-H column (TSKgel (registered trademark), Tosoh Corporation) were used. Dimethylformamide containing 10 mM lithium bromide was used as the eluent.
[0139] <Result> The results are shown in Figure 1. In the legend of Figure 1, the numbers in parentheses indicate the method for producing polysuccinimide by solid-state polymerization. (1) indicates that the above-mentioned Production (1) method was used, and (2a) indicates that the above-mentioned Production (2a) method was used. Although the aspartic acid compositions of Examples 1 and 2 had a higher impurity content than Reference Example 1, the polymerization reaction proceeded faster than Reference Example 1, and polysuccinimide with a larger Mw was obtained. On the other hand, in Comparative Example 1, the polymerization rate was slower and the Mw of the polysuccinimide was smaller than those in the Examples and Reference Example.
[0140] <Production of polysuccinimide by solution polymerization> Example 3 In a 1L flask equipped with a stirrer, a thermometer, a Dean-Stark trap, and a nitrogen inlet tube, 60 parts by mass of the aspartic acid composition obtained in Example 2, 140 parts by mass of mesitylene, 60 parts by mass of sulfolane, and 2.6 parts by mass of 85% phosphoric acid were charged, and the stirring state was adjusted to make a uniform slurry state. The reaction was continued while removing azeotropic water under heating and reflux in an oil bath. After the reaction was completed, the contents were filtered, washed with methanol, and further washed with distilled water until the filtrate became neutral. The washed composition was vacuum dried at 80°C to obtain a polysuccinimide composition having a weight average molecular weight of 49,000.
[0141] Example 4 Except for changing the reaction solvent to 80 parts by mass of xylene and 100 parts by mass of sulfolane, a polysuccinimide composition was synthesized in the same manner as in Example 3. As a result, a polysuccinimide composition having a weight average molecular weight of 80,000 was obtained.
[0142] Example 5 Except for changing the reaction solvent to 100 parts by mass of xylene and 100 parts by mass of sulfolane, a polysuccinimide composition was synthesized in the same manner as in Example 3. As a result, a polysuccinimide composition having a weight average molecular weight of 111,000 was obtained.
[0143] [Evaluation of Cross-Linked Aspartic Acid Composition] <Production of Crosslinked Polyaspartic Acid Composition> (Examples 6 to 13) A polysuccinimide composition was obtained by the method described in <Production of polysuccinimide by solid-state polymerization (2a)> using the aspartic acid composition of Example 2. A crosslinked polyaspartic acid composition was produced by the following method using the polysuccinimide composition. 100 parts by mass of the polysuccinimide composition was dispersed in 167 parts by mass of ion-exchanged water. While stirring the dispersion, 86 parts by mass of a 48% aqueous sodium hydroxide solution was added dropwise using a dropping funnel. After the dropping was completed, stirring was continued until no more dissolved residue remained, and a polyaspartic acid composition with a non-volatile content (Nonvolatiel: NV) of 40% was obtained. The obtained polyaspartic acid composition was an aqueous solution of sodium polyaspartate. The pH of 150 g of the polyaspartic acid composition was adjusted. Ethylene glycol diglycidyl ether (EGDE; Denacol EX-810, Nagase ChemteX Corporation) was added to the polyaspartic acid composition in the amount shown in Table 2, and reacted at 60°C. After the reaction was continued until gelation was confirmed, the gel was collected, washed with water, and freeze-dried to obtain a solid crosslinked polyaspartic acid composition of each example. In the obtained crosslinked polyaspartic acid composition, the crosslinked polyaspartic acid was present in the form of a sodium salt.
[0144] <Production of Crosslinked Polyaspartic Acid Composition> (Examples 14 and 15) A polysuccinimide composition was obtained by the method described in <Production of polysuccinimide by kneader solid-state polymerization (2b)> using the aspartic acid composition of Example 2. A crosslinked polyaspartic acid composition was produced from the polysuccinimide composition in the same manner as in Examples 6 to 13, except that the polysuccinimide composition was used.
[0145] <Production of Crosslinked Polyaspartic Acid Composition> (Examples 16 to 21) A polysuccinimide composition was obtained by the method described in <Production of polysuccinimide by solid-state polymerization (2a)> using the aspartic acid composition of Example 2. A crosslinked polyaspartic acid composition was produced by the following method using the polysuccinimide composition.
[0146] (Examples 16 and 17) 10 parts by mass of polysuccinimide was mixed with 40 parts by mass of dimethylformamide and dissolved by stirring at 60°C for 5 hours. While heating the solution to 40°C, a solution of 0.24 parts by mass of hexamethylenediamine (HDA) and 2.2 parts by mass of dimethylformamide was dropped and reacted for 48 hours while maintaining the temperature at 40°C. The obtained gel was added to 500 parts by mass of ion-exchanged water and crushed with a mixer. After filtering, it was washed with 150 parts by mass of methanol for 1 hour and vacuum dried at 60°C to obtain 10.1 g of a crosslinked polysuccinimide composition (PCI-1). The degree of crosslinking in this case was 2.0 mol%. 3.0 parts by mass of the crosslinked polysuccinimide composition (PCI-1) obtained above was dispersed in a mixed solvent of 20 parts by mass of methanol and 10 parts by mass of ion-exchanged water. A solution of 2.4 parts by mass of 48% sodium hydroxide and 2.4 parts by mass of methanol was divided into 10 portions and added to the dispersion every 30 minutes, and then reacted for 15 hours. The reaction liquid was poured into 400 parts by mass of methanol, and the precipitate was collected by filtration and further washed with 100 parts by mass of methanol. The mixture was dried in a vacuum at 60°C to obtain 3.0 g of a crosslinked polyaspartic acid composition (crosslinked sodium polyaspartate).
[0147] (Examples 18 and 19) Except for changing the amounts of hexamethylenediamine (HDA) and dimethylformamide used to 0.36 parts by mass and 3.2 parts by mass, respectively, in the same manner as in Examples 16 and 17, a crosslinked polysuccinimide composition (PCI-2) (10.1 g) was obtained. The degree of crosslinking in this case was 3.0 mol%. 3.0 g of a crosslinked polyaspartic acid composition (crosslinked sodium polyaspartate) was obtained in the same manner as in Examples 16 and 17, except that the crosslinked polysuccinimide composition (PCI-2) was used. (Examples 20 and 21) A crosslinked polyaspartic acid composition (crosslinked sodium polyaspartate) 3.0 g was obtained in the same manner as in Examples 16 and 17, except that the amounts of hexamethylenediamine (HDA) and dimethylformamide used were 0.48 parts and 4.3 parts, respectively. The degree of crosslinking in this case was 4.0 mol%.
[0148] Comparative Example 2 Using the aspartic acid composition of Comparative Example 1, a polysuccinimide composition was obtained by the method described in <Production of polysuccinimide by solid-phase polymerization (1)>. A polyaspartic acid composition was obtained by the same method as in Examples 6 to 13 above, except that the polysuccinimide composition was used. The pH of 150 g of the obtained polyaspartic acid composition was adjusted, and EGDE was added in the amount shown in Table 2, and the reaction was carried out at 60°C. Gelation of the reaction solution could not be confirmed, and a solid crosslinked polyaspartic acid composition could not be obtained. This was thought to be because the polymer chain of polyaspartic acid in the polyaspartic acid composition did not have a sufficient length to gel by crosslinking.
[0149] <Surface treatment method for crosslinked polyaspartic acid composition> The crosslinked aspartic acid compositions of Examples 7, 9, 11, 13, 15, 17, 19, and 21 were subjected to surface treatment according to the following method. 0.5 parts by mass of fumed silica (Aerosil 200, manufactured by Nippon Aerosil Co., Ltd.) was added to 100 parts by mass of a crosslinked polyaspartic acid composition that had been crushed in a mortar and passed through a mesh to give a particle size of 150 to 710 μm, and mixed thoroughly. The mixture was then heated at 140° C. for 20 minutes to obtain a solid surface-treated crosslinked polyaspartic acid composition.
[0150] <Evaluation of Water Absorbency of Crosslinked Polyaspartic Acid Composition> The water absorption of the crosslinked polyaspartic acid was evaluated using physiological saline according to the tea bag method (JIS K-7223). The water absorption was calculated using the following formula.
[0151] Water absorption [g-water / g]= {(weight after water absorption)-(blank weight after water absorption)-(sample weight)} / (sample weight)
[0152] <Evaluation of Water Retention Capacity of Crosslinked Polyaspartic Acid Composition> The water retention of the crosslinked polyaspartic acid was evaluated by measuring the amount of water absorption using the tea bag method, then dehydrating the tea bag at 25°C and 150G for 2 minutes in a centrifugal dehydrator, and measuring the weight of the tea bag after dehydration. The water retention was calculated using the following formula.
[0153] Water retention capacity [g-water / g]= {(weight after dehydration)-(blank weight after dehydration)-(sample weight)} / (sample weight)
[0154] <Evaluation of Liquid Permeability of Crosslinked Polyaspartic Acid Composition> The liquid permeability of the crosslinked polyaspartic acid composition was evaluated with reference to the method described in JP 2012-41439 A and the like. Specifically, 0.32 g of the crosslinked polyaspartic acid composition was immersed in 150 mL of physiological saline (NaCl 0.9 mass%) for 30 minutes to prepare swollen gel particles. Next, the prepared swollen gel particles were transferred together with physiological saline into a filtration cylindrical tube having a wire mesh (mesh size 106 μm, JIS Z8801-1:2006) and an openable and closable cock (internal diameter 5 mm, length 10 cm) at the bottom of a vertically standing cylinder (diameter (inner diameter) 25.4 mm, length 40 cm, with graduation lines at 40 mL and 60 mL from the bottom) with the cock closed. Next, a circular wire mesh (mesh size 150 μm, diameter 25 mm) was placed on the swollen gel particles so that the wire mesh and the swollen gel particles were in contact with each other. The circular wire mesh used had a pressure shaft (weight 22 g, length 47 cm) attached perpendicularly to the wire mesh surface. A weight {88.5 g} was then placed on the pressure shaft and left to stand for 1 minute. The stopcock was then opened and the time (T1; seconds) required for the liquid level in the cylindrical filtration tube to drop from the 60 mL graduation line to the 40 mL graduation line was measured. The temperature of the saline solution and the measurement atmosphere was 25°C ± 2°C. The liquid permeability was calculated from the following formula.
[0155] Liquid permeability [mL / min]=20mL×60 / (T1-T2) T1: The time (seconds) for 20 mL of saline to pass through the measurement sample T2: Time (seconds) for 20 mL of saline to pass without a measurement sample
[0156] The evaluation results of the water absorption, water retention, and liquid permeability are summarized in Tables 2 and 3. In Tables 2 and 3, "gelation" indicates whether or not a gelled crosslinked polyaspartic acid composition was obtained (A: gelled; B: not gelled). In Table 2, "ND" indicates below the detection limit.
[0157] [Table 2]
[0158] [Table 3]
[0159] From the results in Tables 2 and 3, it was confirmed that the crosslinked polyaspartic acid compositions of Examples 6 to 21 had excellent water absorbency and water retention. It was confirmed that the surface-treated crosslinked polyaspartic acid compositions of Examples 9, 11, 13, 15, 17, 19, and 21 exhibited excellent liquid permeability. In the surface-treated crosslinked polyaspartic acid composition of Example 7, no improvement in liquid permeability due to the surface treatment was confirmed. This is believed to be because the amount of crosslinking agent required to obtain the crosslinked polyaspartic acid composition was small, so sufficient crosslinking density could not be obtained and only a soft gel could be formed. It is believed that this is why liquid permeability could not be ensured.
[0160] Although preferred embodiments of the present invention have been described and illustrated, it should be understood that they are illustrative of the present invention and should not be considered as limiting. Additions, omissions, substitutions, and other modifications can be made without departing from the spirit or scope of the present invention. Thus, the present invention is not to be considered as limited by the foregoing description, but only by the scope of the appended claims.
Claims
1. A surface-modified crosslinked polyaspartic acid composition comprising particles of a crosslinked polyaspartic acid composition, the surfaces of the particles being modified with inorganic particles, The crosslinked polyaspartic acid composition is a hydrolyzate of a crosslinking reaction product of a polyaspartic acid composition or a crosslinking reaction product of a polysuccinimide composition, the polyaspartic acid composition is a hydrolysate of the polysuccinimide composition, the polysuccinimide composition is a polymerization reaction product of an aspartic acid composition; The aspartic acid composition comprises: Aspartic acid and impurities, The impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof; The content of the impurities is 0.02% by mass or more and 1.1% by mass or less based on the total mass of all components of the aspartic acid composition. Surface-modified cross-linked polyaspartic acid composition.
2. 2. The surface-modified crosslinked polyaspartic acid composition of claim 1, wherein the impurities include an amino acid other than the aspartic acid.
3. 3. The surface-modified crosslinked polyaspartic acid composition according to claim 1, wherein the aspartic acid is produced by a microorganism.
4. A surface-modified crosslinked polyaspartic acid composition comprising particles of a crosslinked polyaspartic acid composition, the surfaces of the particles being modified with inorganic particles, The crosslinked polyaspartic acid composition is a hydrolyzate of a crosslinking reaction product of a polyaspartic acid composition or a crosslinking reaction product of a polysuccinimide composition, the polyaspartic acid composition is a hydrolysate of the polysuccinimide composition, The polysuccinimide composition comprises: polysuccinimide and impurities, The impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof; The content of the impurities is 0.001% by mass or more and 1.1% by mass or less based on the total mass of all components of the polysuccinimide composition. Surface-modified cross-linked polyaspartic acid composition.
5. 5. The surface-modified crosslinked polyaspartic acid composition of claim 4, wherein the impurities include amino acids other than the aspartic acid.
6. A surface-modified crosslinked polyaspartic acid composition comprising particles of a crosslinked polyaspartic acid composition, the surfaces of the particles being modified with inorganic particles, The crosslinked polyaspartic acid composition is a crosslinked reaction product of a polyaspartic acid composition, The polyaspartic acid composition comprises: Polyaspartic acid and impurities, The impurities include at least one selected from the group consisting of amino acids other than aspartic acid, organic acids, and salts thereof; The content of the impurities is 0.001% by mass or more and 1.1% by mass or less based on the total mass of all components of the polyaspartic acid composition. Surface-modified cross-linked polyaspartic acid composition.
7. The surface-modified crosslinked polyaspartic acid composition according to claim 6 , wherein the impurities include an amino acid other than aspartic acid or a salt thereof.
8. A crosslinked polyaspartic acid-containing product comprising the surface-modified crosslinked polyaspartic acid composition of claim 1, 4, or 6.
9. The crosslinked polyaspartic acid-containing product according to claim 8, wherein the crosslinked polyaspartic acid-containing product is a surfactant, a thickener, a viscosity reducer, a swelling agent, a water absorbent, a gelling agent, a binder, a film-forming agent, a flocculant, an adhesive, a surface modifier, or a sustained-release agent.
Citation Information
Patent Citations
Purification of aspartic acid
JP1988233958A
Production of optically active 1-(2,4-dichlorophenyl) ethylamine
JP1996143515A
Production of polyaspartic acid and its salt
JP1997176312A
Production of polysuccinimide
JP1997316196A
Purification of water-absorbing resin
JP1998324750A