Freeze-transfer method for porous carbon electrodes based on subzero temperatures

The freeze-transfer method using hydrogels at sub-zero temperatures addresses mechanical mismatches in stretchable electrodes, enabling ultra-thin, highly stretchable electrodes for conformal sensors with improved mechanical compatibility and signal acquisition.

JP7576814B1Active Publication Date: 2024-11-01ZHEJIANG UNIV

Patent Information

Application Number
JP2024089047
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-12-07
Filing Date
2024-05-31
Publication Date
2024-11-01
Estimated Expiration
2044-05-31

AI Technical Summary

Technical Problem

Current methods for manufacturing stretchable electrodes are complex, costly, and limited by mechanical property mismatches between brittle carbon electrodes and flexible-elastic bases, resulting in low conductive stretchability and thickness requirements that hinder the development of scalable, conformal, and comfortable electronic devices.

Method used

A freeze-transfer method using hydrogels as an interfacial control system at sub-zero temperatures to transfer porous carbon electrodes onto flexible bases, enhancing interfacial bonding and achieving ultra-thin, conductive, and stretchable electrodes with improved mechanical compatibility.

Benefits of technology

The method enables the production of ultra-thin, conductive electrodes with high stretchability (up to 220%) and maintains the physical and chemical properties of porous carbon materials, facilitating the fabrication of conformal flexible sensors for real-time monitoring of physical, chemical, and electrophysiological signals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576814000001_ABST
    Figure 0007576814000001_ABST
Patent Text Reader

Abstract

A freeze transfer method and sensor for porous carbon electrodes based on subzero temperatures is provided. [Solution] A porous carbon electrode to be transferred is formed on a base, a hydrogel film is introduced between the porous carbon electrode and a flexible / elastic material that is to receive the electrode, the hydrogel film is expanded by low-temperature freezing to structurally bond with the porous carbon, and then the base is peeled off before the electrode fully recovers from the frozen state, completing the transfer of the porous carbon electrode. By using an interface control system as the hydrogel, the transfer of the porous carbon material to a flexible / elastic base in a low-temperature environment is achieved. [Effects] Not only can the porous carbon electrodes be isolated quickly and completely, but the required thickness of the flexible and elastic base is thinner than with conventional transfer peeling techniques, and the composite electrode formed has better conductive elasticity, which helps realize the production of conformal flexible electronics such as ultra-thin flexible sensors.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the technical field of sensor and electrode manufacturing, and relates to a method for manufacturing a stretchable ultra-thin conductive electrode, in particular to a freeze transfer method for a porous carbon electrode based on subzero temperatures and a sensor. [Background technology]

[0002] Skin-like electronic devices can be seamlessly attached to the skin or inside the human body, and have great potential applications in health monitoring, medical research on implantable devices, human-computer interaction, flexible robotics and augmented reality technology. Reducing the thickness and improving the stretchability of the above devices not only improves the wearing comfort but also increases the effective contact between the device and the measured surface, greatly improving the fidelity of signal acquisition of skin and tissue. The development of stretchable electronic devices that are compatible and mechanically compliant with human skin and biological tissue requires properties such as high carrier mobility, low elastic modulus, and wide range of conductive stretchability. However, scalable fabrication and performance of such stretchable electronics remain a challenge, especially when using simple and reproducible methods. Currently reported fabrication methods for stretchable semiconductors include photolithography and thermal evaporation, but they are complicated and costly.

[0003] Laser-induced graphene (LIG), a porous conductive carbon material obtained by high-temperature carbonization on polyimide thin films by laser direct writing technique, has the advantages of convenient digital patterning and controllable physical and chemical properties, and is widely used in the fabrication of various physical, chemical, and electrophysiological sensors. Because polyimide thin films have low ductility and high Young's modulus, LIG ​​is usually transferred to other flexible and elastic bases with low Young's modulus and good stretchability, including but not limited to high molecular weight polymers such as polydimethylsiloxane (PDMS), styrene-ethylene-butylene-styrene block copolymer (SEBS), polyurethane (PU), ecoflex, etc. However, when these high molecular weight flexible and elastic bases are used to transfer LIG electrodes, a larger elastomer thickness (usually more than 45 μm) is required to provide a large interfacial peel force. Meanwhile, the difference in Young's modulus between LIG and elastic polymers is large, limiting the intrinsic stretchable conductivity of the composite electrodes formed by both of them after transfer (usually stretchable rate is about 40%). Summary of the Invention [Problem to be solved by the invention]

[0004] In order to solve the problems described in the background art, the present invention proposes a method and sensor for freezing transfer of porous carbon electrodes based on subzero temperatures. In this method, the transfer of porous carbon materials to flexible and elastic bases in low-temperature environments is realized by using hydrogel as an interface control system. In addition, the hydrogel interface can further improve the problem of mechanical property mismatch between the brittle carbon electrodes and the flexible and elastic bases. The carbon electrodes after successful transfer have small resistance changes and maintain the physical and chemical properties of the porous carbon materials. The thickness of the flexible and elastic base required in the present invention is thin (1-10 microns thick), which is conducive to the realization of the fabrication of ultrathin conformal flexible electronics. In addition, in this method, the device fabricated using viscous hydrogel has a conductive stretchability of up to 220%, which is an increase of more than 5 times compared with the conventional technology. Based on the proposed freezing ultrathin transfer technology, various ultrathin flexible conformal sensors can be designed to realize the real-time monitoring of physical, chemical, and electrophysiological signals.

[0005] The present invention utilizes the characteristics of high water content of hydrogel, combined with the porous structure of conductive carbon electrode, to achieve rapid and complete peeling of carbon electrode under low-temperature freezing conditions. From the perspective of macrostructure, porous carbon electrode can form an interlocking structure with the crystal water of hydrogel surface, thereby ensuring strong interfacial bonding force during peeling process. From the perspective of interaction, van der Waals interaction and electrostatic interaction between the porous carbon surface rich in hydrophilic groups and the hydrogel surface containing crystal water can be significantly enhanced in low temperature environment. Therefore, low temperature enhances the interfacial shear strength, providing excellent conditions for complete transfer of porous carbon electrode. In addition, during the transfer process, flexible / elastomeric material plays a role in supporting the ultra-thin gel layer, which is also an essential condition for successful transfer.

[0006] This low-temperature freeze transfer method is applicable to any hydrogel system and provides a simple, effective, large-area, and versatile method for fabricating soft, conductive, and biocompatible stretchable electronic devices. [Means for solving the problem]

[0007] Specifically, the technical solutions of the present invention are as follows:

[0008] The freeze-transfer method of a porous carbon electrode based on sub-zero temperatures according to the present invention includes the steps of forming a porous carbon electrode to be transferred on a base, introducing a hydrogel film between the porous carbon electrode to be transferred and a flexible / elastic material to receive the electrode, expanding the hydrogel film by low-temperature freezing to structurally bond with the porous carbon material, and then peeling off the base to complete the transfer of the porous carbon electrode before it fully recovers from the frozen state.

[0009] In the above technical solution, furthermore, the porous carbon electrode to be transferred is a laser-induced carbonized graphene material or a porous carbon material produced by any other method. The laser-induced carbonized graphene material may be a porous graphene conductive electrode pattern produced by performing laser scanning on a polymer thin film such as polyimide, and graphene layers of different thicknesses can be produced according to the intensity of the laser incidence. The wavelength of the laser is preferably in the visible band or infrared band, because the thermal effect of the laser treatment in this wavelength range is more significant and contributes to carbonization. Furthermore, the porous carbon electrode material may be graphene or other carbon materials with single-layer or multi-layer porous structure produced by other methods.

[0010] Furthermore, the flexible / elastic material may be a flexible material or an elastic material, or a composite of both, specifically a composite of one or more of polyethylene, polypropylene, vinyl chloride, polystyrene, polyimide, polytetrafluoroethylene, polydimethylsiloxane, styrene-butene copolymer, polybutadiene, polyisoprene, natural rubber, ethylene-propylene rubber, butyl rubber, silicone rubber, polyisobutylene, polyethylene-polybutene, amorphous polyethylene, polyether, polyester, polyurethane, etc. The flexible / elastic material serves as a support layer for the applied hydrogel film and may be thin, less than 10 μm in thickness.

[0011] Furthermore, before the low-temperature freezing, the water content in the hydrogel film is controlled to 10 wt% or more. After the hydrogel film (e.g., the hydrogel is applied), it may be placed in an oven and left to stand or heated. Other methods such as spin coating, spray coating, or brush coating may also be used to apply the hydrogel.

[0012] Additionally, the Young's modulus of the flexible / elastic material is greater than the Young's modulus of the hydrogel film.

[0013] Furthermore, the temperature range of the low-temperature freezing is −196° C. to −1° C. The lower the temperature of the freeze transfer, the shorter the time required for the transfer.

[0014] Furthermore, prior to the introduction of the hydrogel film, the surfaces of both the porous carbon electrode and the flexible / elastomeric material are modified by plasma treatment, which is advantageous for improving the transfer success rate and sample-to-sample reproducibility.

[0015] Furthermore, the plasma treatment is carried out in an oxygen atmosphere.

[0016] The present invention also provides a stretchable conductive electrode produced by any of the above methods, in which the hydrogel used is a viscous hydrogel, which usually has an adhesive strength, i.e., a crosslinking shear strength between the gel and a flexible base (e.g., polyimide, polyethylene terephthalate), of 10 kPa or more.

[0017] The present invention also provides a multi-function sensor and system integration (e.g., four types of sensors and one multimodal flexible sensing system), all of which contain the above-mentioned stretchable conductive electrodes. Through the principles of structural design, combination of multi-sensing mechanisms, etc., it can realize real-time monitoring of physical signals such as strain, temperature, humidity, electrocardiogram, chemical signals, and electrophysiological signals.

[0018] The method of the present invention further improves the problem of mechanical property mismatch between the brittle electrode and the elastic base by using hydrogel as an interface control system. Hydrogels have excellent flexibility, elasticity and biocompatibility due to the abundance of water molecules in their structure. The Young's modulus of common hydrogel films is generally smaller than that of water-free elastomers such as silicone rubber and rubber, and therefore has attracted more attention in the field of bioelectronic devices. By utilizing the characteristics of high water content of hydrogel, structural bonding and high electrostatic interaction with the porous carbon electrode can be generated under sub-zero temperature conditions, and the rapid and complete peeling of the carbon electrode can be finally achieved. As shown in Figure 1, this low-temperature freezing transfer technique can be mainly used to fabricate ultrathin graphene elastomer composite electrodes and ultrathin sensors, and can also improve the problem of mechanical property mismatch between the brittle graphene material and the elastomer. By introducing a hydrogel film between the brittle material and the elastomer, the volume of the hydrogel can be expanded by low-temperature freezing to structurally bond with the porous graphene material, thereby improving the interfacial bonding strength between the graphene and the hydrogel. In addition, as shown in Figures 2-4, by using a viscous hydrogel, the dull crack in the graphene elastomer system (without hydrogel) can be transformed into a flexible crack under the interfacial control of the hydrogel due to the viscosity of the hydrogel, which can greatly improve the conductive stretchability of the graphene elastic composite electrode.

[0019] The main mechanism of this subzero temperature-based transfer method of porous carbon electrodes can be divided into several aspects.

[0020] (1) From the perspective of macrostructure, as shown in Figure 6, the porous carbon material forms an interlocking structure with the crystal water on the gel surface to ensure the stability of the interface during the peeling process.

[0021] (2) From the viewpoint of interaction, as shown in the results of molecular dynamics calculations and peeling characteristics evaluation in Figure 7, in a subzero temperature environment, the interfacial bonding force (including van der Waals interactions and electrostatic interactions) between the porous carbon surface rich in hydrophilic groups and the gel surface containing crystal water is significantly improved, ensuring strong interfacial shear strength during the peeling process.

[0022] (3) During the transfer process, the flexible / elastomeric material plays a supporting role in the mechanical properties of the thin gel layer, which is also an essential condition for successful transfer. Effect of the Invention

[0023] The advantageous effects of the present invention are as follows:

[0024] The method for transferring a porous carbon electrode pattern based on subzero temperatures of the present invention is applicable to rapidly and effectively transfer a porous carbon material onto hydrogels of any system. The conductive pattern after transfer is clear and complete, the resistance change before and after transfer is small, and the transfer efficiency is high. The carbon material after transfer can maintain the porous structure and the physical and chemical properties of the material. Unlike the conventional method of vacuum transfer of conductive graphene, this transfer method is not limited to the thickness or type of gel or elastomer, and can be used to manufacture ultra-thin conductive devices (the base thickness can be less than 10 μm). In addition, the electrodes fabricated with viscous hydrogels based on this freeze transfer method have a conductive stretchability of up to 220%, which is more than 5 times higher than the conventional technology. Based on this ultra-thin porous carbon electrode transfer technology, various conformal flexible sensors that improve the wearing comfort can be designed and manufactured. [Brief description of the drawings]

[0025] [Figure 1] Low-temperature transfer process of porous graphene materials under the action of hydrogel interface. [Diagram 2] FIG. 14. Tensile crack propagation of porous graphene material on the surface of non-viscous and viscous hydrogels. [Diagram 3]FIG. 14. Formation of flexural cracks in porous graphene on the surface of a viscous hydrogel under various tensile conditions. [Figure 4] FIG. 1 illustrates tensile cracking of porous graphene elastic composites with and without a gel layer. [Diagram 5] Reproducibility of elastomer-based sample transfer under oxygen-free and oxygen plasma treatment conditions (total of 50 samples per group). [Figure 6] The interfacial structure diagrams of porous graphene transferred onto a hydrogel surface by cryogenic freezing and onto a PDMS elastomer by vacuum transfer are shown. In the diagram, the porous graphene is partially embedded into the gel by the low-temperature transfer method, and the LIG is completely wrapped in the PDMS elastomer by the vacuum transfer method. [Figure 7] The binding energies of large-defect graphene (LDG) and small-defect graphene (SDG) models at hydrogel interfaces at various temperatures are shown, including the results of molecular dynamics simulation calculations of van der Waals interactions (vdW energy) and electrostatic interactions (electrostatic energy), as well as the results of 180° peel adhesion characterization at various processing temperatures (293 K, 270 K, 223 K, and 77 K). [Figure 8] Transfer effect of hydrogel onto polyethylene terephthalate flexible base. [Figure 9] 1 is an actual working process of freeze-transfer of graphene conductive patterns based on hydrogel. [Figure 10] Conformal attachment of the transferred graphene stretchable electrodes to the surface of curved objects and to skin. [Figure 11] Comparison of the surface morphology of laser-induced graphene before and after freeze-transfer. [Figure 12] Raman characterization of porous graphene before (LIG) and after freeze-transfer (LIG / PPH). [Figure 13] 13 shows the effect of the Young's modulus of the elastomer on the electrode resistance before and after freeze transfer. [Figure 14] The effect of different laser processing energies (laser fluence) on freeze transfer efficiency (TE). [Figure 15] Effect of hydrogel film thickness on the resistance of graphene electrodes before and after freeze-transfer. [Figure 16] FIG. 1 is a diagram showing a strain sensor and its performance. [Figure 17] FIG. 1 is a diagram showing a temperature sensor and its performance. [Figure 18] FIG. 1 illustrates a humidity sensor and its performance. [Figure 19] FIG. 1 illustrates an ECG sensor and its performance. [Figure 20] 1A-1D are schematic diagrams of the manufacturing steps of a multi-modal flexible sensing system. [Figure 21] The results show the real-time monitoring of multiple signals by a multimodal flexible sensing system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present invention will be described in more detail with reference to the drawings and specific examples. The viscous hydrogel used in the embodiments of the present invention may be a hydrogel obtained by mixing a polyvinyl alcohol solution, phytic acid and sugar. Other viscous hydrogels may also be used in the method of the present invention.

[0027] Example 1 (Transfer to a Flexible Base Polyethylene Terephthalate) 1) A PPH hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first prepared, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It is. 3) The surfaces of a polyethylene terephthalate thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 4) The hydrogel solution obtained in 1) was spin-coated onto the treated hydrophilic polyethylene terephthalate at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cure gel was approximately 2.5 μm. 5) The conductive graphene electrode processed in 3) was bonded face-to-face to a thin hydrogel film. 6) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 7) The sample was removed, and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was completely transferred to the surface of the gel.

[0028] Example 2 (Transfer to an Elastomer-Based Polydimethylsiloxane) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a mass ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) In an oxygen atmosphere, the polydimethylsiloxane thin film obtained in 2) and the conductive graphene electrode obtained in 3) were subjected to a surface hydrophilization treatment using plasma. 5) The hydrogel solution obtained in 1) was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cure gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed, and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was completely transferred to the surface of the gel. 9) Finally, when the polyethylene terephthalate substrate underneath the polydimethylsiloxane was peeled off, the resulting composite of conductive graphene, gel, and polydimethylsiloxane was overall stretchable. In Examples 1 and 2, freeze-transfer was performed on two different hydrogel support materials, namely flexible polyethylene terephthalate and elastic polydimethylsiloxane substrates. FIG. 8 shows the transfer effect diagram of hydrogel onto polyethylene terephthalate on a flexible base, from which it can be seen that the conductive graphene pattern after transfer was completely peeled off. FIG. 9 shows the actual working process of freeze-transfer of graphene conductive pattern based on PPH hydrogel, from which the successful peeling and transfer of the conductive pattern can be visually confirmed. FIG. 10 shows the effect of seamlessly attaching the ultrathin graphene conductive stretchable electrode composite that has been successfully freeze-transferred to the surface of an elastic object and skin.

[0029] Example 3 (Effect of Young's modulus of elastic base on transfer efficiency) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a main solution to curing agent ratio of 5:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for curing. The Young's modulus after curing was 0.89 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0030] Example 4 (Effect of Young's modulus of elastic base on transfer efficiency) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a main solution to hardener ratio of 10:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.78 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0031] Example 5 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed, and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was completely transferred to the surface of the gel.

[0032] Example 6 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a main solution to hardener ratio of 40:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.097 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel. In all of Examples 2 to 6, polydimethylsiloxane is used as the support material, so the composites produced are generally elastic. FIG. 10 shows the seamless and conformal application of the conductive elastic composites using elastic materials as the support layer to balloons and human skin. FIG. 11 shows the morphology of the porous surface of the conductive graphene material before and after transfer. FIG. 12 shows a comparison of the Raman characteristic peaks of the conductive graphene material before and after transfer. It is clear from the results of the two groups that the freeze transfer method can well maintain the physical and chemical properties of the conductive material itself. In Examples 2 to 6, the Young's modulus of the hydrogel support material is different, which affects the electrical resistance and transfer efficiency of the freeze transfer. The results of FIG. 13 show that the Young's modulus (0.12 MPa) of the support material in Example 5 is optimal, which can ensure a small difference in electrical resistance before and after transfer and a high transfer efficiency.

[0033] Example 7 (Effect of laser processing energy on transfer effect) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 6.43 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0034] Example 8 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed, and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was completely transferred to the surface of the gel.

[0035] Example 9 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.04 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0036] Example 10 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.85 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 2000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 2.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel. In Examples 7 to 10, the laser processing energy for carbonizing the polyimide thin film was different, which affected the change in electrical resistance before and after transfer and the transfer efficiency. The laser processing energy affected the shape and porosity of the graphene voids, and further affected the interfacial adhesion between the gel and graphene at low temperatures. From the results in FIG. 14, it can be seen that the laser processing energy of 7.24 J / cm -2 It has been shown that when the transfer efficiency is 100%, the change rate of electrical resistance before and after the transfer is less than 50%, and the batch transfer efficiency is optimal, reaching 150%.

[0037] Example 11 (Effect of hydrogel thickness on transfer efficiency) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.04 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 1000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 3 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0038] Example 12 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.04 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 3000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 1.5 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0039] Example 13 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.04 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 4000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately 1.2 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was transferred to the surface of the gel.

[0040] Example 14 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The laser processing energy was 8.04 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 5000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately <1 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was at least partially transferred to the surface of the gel. In Examples 11 to 14, the spin-coating speed of the gel solution was different, and the thickness of the obtained hydrogel was different, which affected the change in electrical resistance before and after transfer and the transfer efficiency. From the results of FIG. 15, it was shown that in Examples 12 and 13, when the thickness of the hydrogel was in the range of 1 to 1.5 μm, that is, when the spin-coating speed was 3000 and 4000 rpm / min, the change in electrical resistance before and after transfer was the smallest, and the effect after transfer was optimal. From these results, it was shown that, in addition to ensuring that the gel was uniform and defects were eliminated, the thinner the gel, the higher the interfacial peel adhesion strength between the gel and graphene at low temperatures.

[0041] Example 15 (Manufacture of a multifunctional flexible sensor) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. 3) Conductive graphene patterns were fabricated by carbonizing polyimide thin films using a carbon dioxide infrared laser in grating mode. The laser processing energy was 7.24 J / cm. -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution obtained in 1) was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 4000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately <1 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was at least partially transferred to the surface of the gel. 9) Based on the above method, in combination with conventional technology, strain sensors, temperature sensors, humidity sensors, and electrocardiogram sensors were manufactured. Examples 1-14 provide the optimal transfer parameters for graphene materials, which are the basis for the technology to fabricate multiple types of sensors in Example 15. Figure 16 shows the performance of the strain sensor, in which the snake-like structure design balances sensitivity and stretchability, with a strain factor (GF) of about 30. Figure 17 shows the performance of the temperature sensor, which exhibits a wide temperature measurement range (10-75°C), linear response with low hysteresis, and good negative temperature coefficient (0.35%°C). -1 ) Figure 18 shows the performance of the humidity sensor, where the gel is the moisture-sensitive material and graphene is the sensing electrode, and the sensitivity of the obtained humidity sensor is 0.81% %RH -1 Figure 19 shows the performance of the electrocardiogram sensor, demonstrating the high degree of conformity between the ultrathin elastomeric composite (LIG / PPH / PDMS) and the skin, which facilitates the detection of electrophysiological signals with high fidelity.

[0042] Example 16 (Multimodal flexible sensor integrated system) 1) A hydrogel with a water content of more than 10% was prepared, i.e., a 10% by weight polyvinyl alcohol solution was first made, and then the polyvinyl alcohol solution, phytic acid, and glucose were mixed in a mass ratio of 5:5:1 and heated at 80°C for use. 2) A polydimethylsiloxane precursor solution with a ratio of main solution to hardener of 20:1 was prepared, and the precursor solution was spin-coated onto a polyethylene terephthalate thin film in one layer at a rotation speed of 1500 rpm / min, and then heated to 90°C for hardening. The Young's modulus after hardening was 0.12 MPa. Two sheets were prepared. 3) A carbon dioxide infrared laser was used in grating mode to carbonize polyimide thin films and fabricate conductive graphene patterns. The four types of sensors in Example 15 were included, and the laser processing energy was 7.24 J / cm -2 It was. 4) The surfaces of a polydimethylsiloxane thin film and a conductive graphene electrode were hydrophilized using plasma in an oxygen atmosphere. 5) The hydrogel solution was spin-coated onto the treated hydrophilic polydimethylsiloxane at a rotation speed of 4000 rpm / min, and then heated at 60°C to rapidly semi-cure the hydrogel so that the thickness of the semi-cured gel was approximately <1 μm. 6) The conductive graphene electrode processed in 4) and the hydrogel thin film in 5) were bonded face-to-face. 7) The bonded sample was held with tweezers and placed in a subzero environment (-196°C to -1°C) to freeze. 8) The sample was removed and the polyimide was carefully peeled off before the sample recovered from the frozen state to the elastic state, and the graphene conductive electrode pattern was at least partially transferred to the surface of the gel. 9) Liquid metal was printed onto the surface of the polydimethylsiloxane (2) by screen printing. 10) Because the humidity sensor and electrocardiogram sensor are in direct contact with the skin, holes were selectively made in the thin film of 9) using a laser cutter to expose the humidity sensor and electrocardiogram sensor. 11) The graphene pattern on the gel in 8) was aligned with the liquid metal electrode in 10) and bonded together, and low-temperature peeling was performed in a liquid nitrogen environment to remove excess polyethylene terephthalate (PET) thin film. According to the embodiment 16, a multimodal flexible sensing system having flexible, ultra-thin and stretchable characteristics can be obtained. The specific manufacturing steps are shown in FIG. 20. The sensing system is conformally attached to the chest of a human body and connected to a flexible printed circuit board, and can monitor respiration rate, electrocardiogram, heart rate, body surface temperature and body surface humidity in real time, in which the respiration rate is obtained by monitoring the expansion and contraction of the chest with a strain sensor, and the heart rate is obtained by analyzing the ECG signal. FIG. 21 shows the results of real-time monitoring of multiple signals by the multimodal flexible sensing system, which can monitor the physiological state of the human body in various states. The above embodiments are merely some preferred embodiments of the present invention and are not used to limit the present invention. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solutions obtained by the method of equivalent substitution or equivalent transformation are within the scope of protection of the present invention.

Claims

1. A freeze transfer method for a porous carbon electrode based on subzero temperatures, comprising: forming a porous carbon electrode to be transferred on a base, introducing a hydrogel film between the porous carbon electrode to be transferred and a flexible / elastic material to receive the electrode, expanding the hydrogel film by low-temperature freezing to structurally bond with the porous carbon, and then peeling off the base before the porous carbon electrode is fully recovered from the frozen state, thereby completing the transfer of the porous carbon electrode; controlling the water content in the hydrogel film to 10 wt % or more before the low-temperature freezing; 2. The method for freeze-transfer of a porous carbon electrode, wherein the flexible / elastic material is a flexible material, an elastic material, or a composite of both.

2. The method for freeze-transferring a porous carbon electrode based on subzero temperatures according to claim 1, characterized in that the porous carbon electrode to be transferred is a laser-induced carbonized graphene material or a porous carbon material manufactured by any other method.

3. 2. The subzero temperature based freeze transfer method of porous carbon electrode of claim 1, wherein the Young's modulus of the flexible / elastic material is greater than the Young's modulus of the hydrogel film.

4. The method for freeze-transfer of a porous carbon electrode based on a subzero temperature according to claim 1, characterized in that the temperature range of the low-temperature freezing is -196°C to -1°C.

5. The freeze transfer method of a porous carbon electrode based on subzero temperatures, as described in claim 1, characterized in that before the hydrogel film is introduced, both the surfaces of the porous carbon electrode and the flexible / elastic material are modified by plasma treatment.

6. 6. The method for freeze-transfer of a porous carbon electrode based on a subzero temperature according to claim 5, wherein the plasma treatment is performed in an oxygen atmosphere.

Citation Information

Patent Citations

  • Conductive composition, conductive member, and device for biological sensing

    JP2017042300A

  • Porous structure provided with pattern that is composed of conductive polymer, and method for producing same

    WO2011118800A1

  • Pellicle film, and pellicle

    WO2014142125A1

Cited By

  • Preparation method of porous carbon material cooperatively regulated by heteroatoms and application of porous carbon material in sodium / potassium ion capacitor

    CN121158763A