High frequency magnetic materials and their manufacturing methods
A rare earth-iron-M-nitrogen magnetic material, combined with ceramics and resins, addresses the limitations of conventional materials by providing high magnetic permeability and low eddy current loss, enabling effective electromagnetic noise absorption and signal amplification across a broad frequency spectrum.
Patent Information
- Application Number
- JP2023509170
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-25
- Filing Date
- 2022-03-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-03-22
AI Technical Summary
Conventional magnetic materials face challenges in achieving high magnetic permeability and resistance to eddy current loss in the high frequency range of 0.001 GHz to 100 GHz, particularly in the ultra-high frequency region, limiting their effectiveness in applications such as electromagnetic noise absorption and signal amplification.
Development of a high-frequency magnetic material using a rare earth-iron-M-nitrogen magnetic material, where M is Ti, V, Mo, Nb, W, Si, Al, or Cr, combined with ceramic and resin materials to enhance magnetic permeability and electrical resistivity, controlling crystal structure and grain size to minimize eddy current loss.
The new magnetic material exhibits high magnetic permeability and low eddy current loss, effectively functioning as electromagnetic wave absorbers and amplifiers across the entire high frequency range, including ultra-high frequencies, while maintaining stability and flexibility.
Smart Images

Figure 0007576881000001 
Figure 0007576881000002 
Figure 0007576881000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a magnetic material used in the high frequency range of 0.001 GHz or more and 100 GHz or less (that is, a high frequency magnetic material) and a manufacturing method thereof. The present invention also relates to a high frequency magnetic material obtained by combining the high frequency magnetic material with other materials (e.g., non-magnetic ceramic materials and / or resins), and particularly to a high frequency magnetic material containing resin and a method for producing the same. [Background technology]
[0002] Examples of magnetic materials for the above-mentioned power equipment and information and communication-related equipment include magnetic materials for transformers, heads, inductors, reactors, yokes, cores (magnetic cores), antennas, microwave elements, magnetostrictive elements, magnetoacoustic elements, magnetic recording elements, and magnetic materials for sensors that use a magnetic field, such as Hall sensors (Hall elements), magnetic sensors, current sensors, rotation sensors, and electronic compasses, and in particular magnetic materials for coil cores and antenna cores used in wireless power supply (also called wireless power transmission or contactless power transmission) systems. Examples of magnetic materials for suppressing damage caused by unwanted electromagnetic interference include magnetic materials for absorbing electromagnetic noise, absorbing electromagnetic waves, and for magnetic shielding; magnetic materials for inductor elements such as noise-removing inductors; magnetic materials for RFID (Radio Frequency Identification) tags; and magnetic materials for noise filters that remove noise from signals at high frequencies.
[0003] Recently, as various types of mobile information and communication devices such as personal computers, mobile phones, and digital cameras have become smaller and more multifunctional, and their processing speeds have increased, the driving frequencies have become increasingly high. The use of high-frequency devices with frequencies between 0.001 GHz and 100 GHz, especially ultra-high frequencies above 1 GHz, has been steadily expanding. In recent years, the demand for devices using microwave electromagnetic waves, such as satellite communications, mobile communications, and car navigation systems, has increased significantly. Technologies such as ETC (Electronic Toll Collection System), short-range wireless communications such as wireless LAN, and millimeter-wave radars for automobiles, such as collision prevention radars, have also begun to spread. In addition, the use of high-frequency devices is also progressing in the field of wireless power supply systems. Low-frequency charging for home appliances such as mobile phones and automatic vacuum cleaners has become widespread, and low-frequency charging for electric vehicles while parked has also been put to practical use. Recently, demonstration tests have been conducted on high-frequency power supply to moving next-generation automobiles, and high-power wireless power supply from power plants using microwaves is being considered. As the trend toward greater use of high frequencies, particularly ultra-high frequencies, progresses, there is a strong demand for magnetic materials that can withstand high-frequency electromagnetic field changes without loss. On the other hand, the deterioration of the electromagnetic environment (specifically, electromagnetic interference to other devices and living organisms) caused by the electromagnetic waves emitted by these high-frequency devices to the outside world is a problem, and currently, public and international organizations are actively promoting legal regulations and voluntary restrictions. In this way, signals (electromagnetic waves) that are useful for individual devices can be interference to other devices and living organisms, making it extremely difficult to address this issue. In order to solve this problem, it is important to establish electromagnetic compatibility (EMC) that takes into account both electromagnetic interference (EMI: Electro-Magnetic Interference) and damage (EMS: Electro-Magnetic Susceptibility) as characteristics of the devices, i.e., not emitting unnecessary electromagnetic waves (electromagnetic noise) and having strong resistance to external noise.
[0004] As an example of the above-mentioned EMC measures, the following will focus on electromagnetic noise absorbing materials that are often used in electronic devices these days. Electromagnetic noise absorbing materials are materials that act to suppress the emission of electromagnetic waves to the outside world near electromagnetic noise sources. In the high-frequency range of several hundred MHz or more, sheet-shaped electromagnetic noise absorbing materials are often used that utilize the natural resonance of Ni-Zn ferrite and other materials to absorb high-frequency electromagnetic noise such as harmonics traveling through lines and convert it into thermal energy to suppress the noise. The magnetic properties required are that the magnetic material has a high relative permeability and a high natural resonance frequency. Ferrite, an oxide magnetic material, has a high electrical resistivity, so performance degradation due to eddy current loss is small and it has been considered a preferable material for use in high-frequency ranges.
[0005] On the other hand, as described in Patent Document 1, the value of the imaginary term of the magnetic permeability of ferrite in the ultra-high frequency region is about 1 to 2 or less, so it is difficult to apply ferrite-based oxide magnetic materials to electromagnetic noise absorption materials in the GHz band (region).For this reason, in recent years, metal-based magnetic materials such as Fe, Fe-Ni alloys, Fe-Ni-Si alloys, sendust, Fe-Cu-Nb-Si alloys, and amorphous alloys, which have larger saturation magnetization values than ferrite-based oxide magnetic materials, have been actively used, and magnetic materials in which magnetic metal particles are dispersed in insulating resins, etc., have been developed as electromagnetic noise absorption materials. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2008 / 136391 Summary of the Invention [Problem to be solved by the invention]
[0007] However, the electrical resistivity of metallic magnetic materials is 10 to 140 μΩcm, while that of ferrite is 4000 to 10 18It is considerably lower than μΩcm. Therefore, it is not possible to achieve high permeability up to high frequencies, making it difficult to use in high frequency ranges. This is because an insulating layer is required to prevent the permeability from starting to decrease in the low frequency range due to eddy current loss, and the non-magnetic portion of the insulating layer lowers the complex relative permeability of the magnetic material-resin composite material in the high frequency range that it originally has. Furthermore, in the ultra-high frequency range exceeding 1 GHz, even such composite materials cannot avoid a decrease in permeability due to the effect of eddy current loss.
[0008] Metal-based magnetic materials with shape anisotropy have also been developed. However, due to considerations similar to those in Patent Document 1, the thickness of the metal-based magnetic material filler must be less than 0.2 μm, and even if a certain degree of filling rate is achieved and magnetic permeability is increased, there is a limit to the applicability to ultra-high frequency applications. For this reason, there has been a strong desire to develop magnetic materials for use as electromagnetic noise absorption materials that have higher magnetic permeability and better electromagnetic noise suppression performance in the high frequency range (especially the ultra-high frequency range), as well as electromagnetic noise absorption materials that are easy to mass-produce and have a wide range of applications that can be used in applications where flexibility is required (for example, magnetic materials that can be dispersed in resin and made into sheets).
[0009] For these reasons, it is important for an excellent high-frequency magnetic material that the value of the real term of the complex relative permeability does not decrease and the value of the imaginary term does not increase up to the high-frequency region (ultra-high-frequency region if necessary), whether it is used as a high-frequency absorbing material for suppressing and absorbing spurious and electromagnetic noise in an electromagnetic noise absorbing material, or as a high-frequency amplifying material for generating a magnetic field or electromagnetic field that is amplified in proportion to the magnetic field or electromagnetic wave of the frequency of use, such as a high-frequency core (magnetic core), a material for RFID tags, or a coil core for a wireless power supply system. In addition, when used as a high-frequency absorbing material, it is important that the value of the imaginary term of the complex relative permeability in the high-frequency region (ultra-high-frequency region if necessary) increases with frequency and is sufficiently large at the desired frequency where unwanted radiation, harmonics, etc. are present, even if the value is close to 0 in the low-frequency region.
[0010] Furthermore, in order to amplify the magnitude of signals in RFID tags for high-frequency signals or coil cores for wireless power supply systems, it is important to realize a high real term of permeability in the frequency range in which signals exist. However, depending on the application, it may also be necessary to absorb and remove noise such as harmonics in the high-frequency to ultra-high-frequency range without absorbing signals on the lower frequency side below a certain frequency. In particular, materials are required that have an imaginary term (μ”) value of the complex relative permeability close to 0 in the frequency range below 1 GHz and a large imaginary term (μ”) value in the high-frequency range (i.e., ultra-high-frequency range) (note that materials with a larger "selective absorption ratio above 1 GHz" as defined below are more suitable for the above purpose). However, as far as the inventors know, only the above-mentioned oxide magnetic materials and metal-based magnetic materials have been used as magnetic materials for high frequency applications in the past. As described above, even if an oxide magnetic material (especially a ferrite-based oxide magnetic material with high electrical resistivity) is used, there is a problem that sufficient magnetic permeability cannot be obtained, even if the problem caused by eddy current loss is small, and even if a metal-based magnetic material is used, there is a problem that eddy current loss occurs in the low frequency range because the magnetic permeability is high but the electrical resistivity is small, and both of these are problems that are not suitable as magnetic materials for high frequency applications. Patent Document 1 attempts to solve this problem by using a nitride material, but the material disclosed in this patent document does not exhibit sufficient performance as a high-frequency amplification material, such as an electromagnetic wave absorption material with high magnetic permeability in the ultra-high frequency range or a magnetic field amplification material used in the high frequency range of 0.001 GHz or more and 0.1 GHz or less. Under these circumstances, there is a demand for the development of new high-frequency magnetic materials that can exhibit better performance than conventional magnetic materials even in the high-frequency range of 0.001 GHz or more and 100 GHz or less.
[0011] The present invention has been made in consideration of the above-mentioned problems, and aims to provide a new high-frequency magnetic material using a nitride-based magnetic material, specifically, a rare earth-iron-M-nitrogen-based magnetic material (wherein M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr) with controlled crystal structure and particle size, as a magnetic material for high-frequency applications, which has a higher magnetization than oxide magnetic materials and therefore can achieve high magnetic permeability, and also has a higher electrical resistivity than metal materials and can solve problems such as the above-mentioned eddy current loss. Moreover, the present invention aims to provide a new nitride-based magnetic material having high performance (specifically, high magnetic permeability) as a high-frequency composite magnetic material, which can further increase the electrical resistivity of the rare earth-iron-M-nitrogen-based magnetic material by compounding the rare earth-iron-M-nitrogen-based magnetic material having a controlled crystal structure and particle size with a resin or a ceramic material, and which can more effectively solve problems such as the eddy current loss described above. Another object of the present invention is to provide a magnetic material for amplifying and absorbing an electromagnetic field used in a high frequency range of 0.001 GHz or more and 100 GHz or less, in particular a magnetic field amplifying material used in a high frequency range of 0.001 GHz or more and 0.1 GHz or less.
[0012] The term "magnetic material for high frequency" in this application refers to a magnetic material that functions as a magnetic material used in a high frequency range (so-called magnetic material for high frequency). Therefore, the term "magnetic material for high frequency" in this application also includes a magnetic material obtained by combining two or more different types of magnetic materials, or one or more types of magnetic materials and a non-magnetic material (for example, a non-magnetic ceramic material and / or a resin), and that functions as a magnetic material used in a high frequency range (so-called magnetic material for high frequency). Such a magnetic material is sometimes referred to as a "composite magnetic material for high frequency" in this application. In this application, "composite" means a state in which, when the magnetic material is composed of two or more different types of magnetic materials, the region occupied by the magnetic material is divided or covered with a different magnetic material, and, when the magnetic material is composed of one or more types of magnetic materials and a non-magnetic material, the region occupied by the magnetic material is divided or covered with a non-magnetic material. Furthermore, among the "high frequency composite magnetic materials", those that contain resin, for example, magnetic materials that function as magnetic materials used in high frequency regions (so-called high frequency magnetic materials) by being composite of one or more types of magnetic materials and resin, or composite of one or more types of magnetic materials, ceramic materials, and resin, may be referred to in this application as "high frequency resin composite magnetic materials". In this way, the above-mentioned "high frequency composite magnetic material" and "high frequency resin composite magnetic material" both function as high frequency magnetic materials, and therefore are "high frequency magnetic materials" in the broad sense. Therefore, the "high frequency magnetic material" in this application includes both the above-mentioned "high frequency composite magnetic material" and "high frequency resin composite magnetic material." In addition, in this application, a magnetic material obtained by combining two or more different types of magnetic materials, or one or more types of magnetic material with a non-magnetic material (e.g., a non-magnetic ceramic material and / or a resin) is simply referred to as a "composite magnetic material," and one that contains resin may be simply referred to as a "resin composite magnetic material." In this application, electromagnetic waves with frequencies between 0.001 GHz and 100 GHz are referred to as "high frequency", and among them, "ultra-high frequency" means high frequency of 1 GHz or more. In this application, unless otherwise specified, "ultra-high frequency" is also included in "high frequency". Therefore, in this application, "high frequency region" refers to the electromagnetic wave region with frequencies between 0.001 GHz and 100 GHz and less, and within that, the electromagnetic wave region with frequencies above 1 GHz refers to the "ultra-high frequency region". In addition, in this application, unless otherwise specified, electromagnetic waves having frequencies lower than the above-mentioned "high frequencies" are referred to as "low frequencies." Furthermore, in this application, the term "high frequency magnetic material" refers to a magnetic material that acts on an electric field, a magnetic field, or an electromagnetic field in the frequency range of 0.001 GHz to 100 GHz to perform a "target function", and includes the "high frequency composite magnetic material". Here, the "target function" refers to the magnetic functions of the magnetic material, such as electromagnetic induction, self-induction, high permeability, high frequency loss, magnetostriction, magnetic domain formation, and semi-hard magnetism, and the "high frequency composite magnetic material" of the present invention is used in elements, parts, devices, etc. that utilize these functions. In this application, magnetic materials that have a target function of high permeability, such as magnetic field amplification materials used in the high frequency range, are sometimes referred to as "high frequency amplification materials", and magnetic materials that have a target function of high high frequency loss are sometimes referred to as "high frequency absorption materials". [Means for solving the problem]
[0013] The present inventors have conducted extensive research into a high-frequency magnetic material with excellent electromagnetic properties that combines the contradictory properties of conventional magnetic materials (specifically, a high-frequency magnetic material with excellent electromagnetic properties that combines the advantages of both metal-based magnetic materials and oxide magnetic materials, namely, high magnetic permeability and high electrical resistivity that can solve the above-mentioned problem of eddy current loss), and have found that a high-frequency magnetic material with extremely high electromagnetic properties that can solve the above-mentioned problems can be obtained by using a rare-earth-iron-M-nitrogen magnetic material (wherein M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr) as the high-frequency magnetic material, adjusting the composition, crystal structure, and particle size of the rare-earth-iron-M-nitrogen magnetic material, and adjusting the blending with ceramics, resins, and other magnetic materials, and have further established a manufacturing method thereof, thereby completing the present invention.
[0014] Specifically, the present invention is as follows. (1) A high-frequency magnetic material whose main phase has a composition represented by the general formula shown in Formula 1 below and is used in the frequency range of 0.001 GHz to 100 GHz. R x Fe (100-x-y-z) M y N z (Formula 1) (R is at least one element selected from the group consisting of rare earth elements including Y, Fe is an iron element, M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, N is a nitrogen element, and x, y, and z satisfy 2 atomic %≦x≦15 atomic %, 0.5 atomic %≦y≦25 atomic %, and 3 atomic %≦z≦50 atomic %). (2) The high frequency magnetic material according to (1) above, wherein 50 atomic % or less of Fe in the formula 1 is substituted with Co or Ni element. (3) The high frequency magnetic material according to (1) or (2) above, wherein R in formula 1 contains 50 atomic % or more of Sm element. (4) The high frequency magnetic material according to any one of (1) to (3) above, wherein the crystal structure of the main phase is tetragonal. (5) A high frequency magnetic material according to any one of (1) to (4) above, wherein the crystal magnetic anisotropy is in-plane magnetic anisotropy. (6) The high frequency magnetic material according to (1) or (2) above, wherein the crystal structure of the main phase is amorphous. (7) The high frequency magnetic material according to any one of (1) to (6) above, wherein less than 50 atomic % of N in the formula 1 is replaced with at least one element selected from the group consisting of H, C, P, Si and S. (8) The high frequency magnetic material according to any one of (1) to (7) above, which is a powder having an average particle size of 0.1 μm or more and 2000 μm or less. (9) A magnetic material for high frequency use according to any one of (1) to (8) above is contained in an amount of 1% by mass or more and 99.999% by mass or less, Metallic Fe, metallic Ni, metallic Co, Fe-Ni alloy, Fe-Ni-Si alloy, sendust, Fe-Si-Al alloy, Fe-Cu-Nb-Si alloy, a At least one selected from the group consisting of amorphous alloy, magnetite, Ni-ferrite, Zn-ferrite, Mn-Zn ferrite, and Ni-Zn ferrite is contained in an amount of 0.001% by mass or more and 99% by mass or less. High frequency magnetic material. (10) The high frequency magnetic material according to (9) above, wherein the metallic Fe is carbonyl iron powder. (11) A magnetic material for high frequency use according to any one of (1) to (10) above, in an amount of 1% by mass or more and 99.999% by mass or less, Contains ceramic materials in an amount of 0.001% by mass or more and 99% by mass or less; High frequency magnetic material. (12) A magnetic material for high frequency use according to any one of (1) to (11) above, comprising 5% by mass or more and 99.9% by mass or less, Contains resin in an amount of 0.1% by mass or more and 95% by mass or less; High frequency magnetic material. (13) The high frequency magnetic material according to (12) above, wherein the resin contains a segment having a solubility parameter of 10 or more and 15 or less. (14) A high frequency magnetic material according to any one of (1) to (13) above, which is magnetically oriented. (15) A method for producing the high frequency magnetic material according to (1) above, by heat treating an alloy containing R, Fe and M as main components as defined in formula 1 above at a temperature in the range of 100°C to 600°C in a nitriding atmosphere containing ammonia gas. (16) A method for producing the high frequency magnetic material according to the above (12), by kneading the high frequency magnetic material according to the above (1) produced by the production method according to the above (15) with a resin containing a segment having a solubility parameter of 10 or more and 15 or less, followed by compression molding, injection molding, and / or calendar molding. Effect of the Invention
[0015] According to the present invention, it is possible to provide a new magnetic material that can be used as a high frequency magnetic material in the entire high frequency range from 0.001 GHz to 100 GHz. According to the present invention, it is possible to provide a high-frequency magnetic material that has high magnetic permeability and small eddy current loss, and is particularly suitable for use as a high-frequency composite magnetic material that functions as an electromagnetic wave absorber in the ultra-high frequency range (particularly the ultra-high frequency range of 1 GHz or more) or functions as a high-frequency amplifier in the high frequency range (particularly the high frequency range of 0.1 GHz or less). [Brief description of the drawings]
[0016] [Figure 1] 1 is an X-ray diffraction diagram (Co-Kα radiation source) of Sm6.4Fe70.5Ti6.4N16.7 magnetic powder (Example 1) and Sm7.7Fe84.6Ti7.7 raw alloy powder (Comparative Example 1). [Diagram 2] FIG. 1 is a graph showing frequency variations in relative permeability of a high-frequency magnetic material powder (Example 2) obtained by finely pulverizing Sm6.4Fe70.5Ti6.4N16.7 magnetic powder and a Sm7.7Fe84.6Ti7.7 raw alloy powder (Comparative Example 1). [Diagram 3] FIG. 1 is a diagram showing frequency changes in relative magnetic permeability of a Sm7.2Fe72.4V14.5N5.9-based magnetic material (Example 3). [Figure 4] SEM (scanning electron microscope) photographs of the cross section of the Ce7.7Fe84.6Ti7.7 raw alloy before and after annealing. A shows before annealing, and B shows after annealing. The black areas in the figure are the Fe-Ti alloy phase, the gray areas are the CeFe11Ti alloy phase, and the white areas are Ce-rich phases such as the Ce2Fe17 alloy phase. [Diagram 5] 1 is an X-ray diffraction diagram (Co-Kα radiation source) of Ce5.3Fe58.2Ti5.3N31.2 magnetic powder (Example 4) and Ce7.7Fe84.6Ti7.7 raw alloy powder (Comparative Example 2). [Figure 6] FIG. 1 is a graph showing the frequency change of the relative magnetic permeability of a Ce5.3Fe58.2Ti5.3N31.2 magnetic powder (Example 4) and a Ce7.7Fe84.6Ti7.7 raw alloy powder (Comparative Example 2). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below. The "high frequency magnetic material" of the present invention has a main phase composition represented by the following formula 1, i.e., R x Fe (100-x-y-z) M y N z (Formula 1) (R is at least one element selected from the group consisting of rare earth elements including Y, Fe is an iron element, M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, N is a nitrogen element, and x, y, and z satisfy 2 atomic %≦x≦15 atomic %, 0.5≦y≦25 atomic %, and 3≦z≦50 atomic %). It is a high-frequency magnetic material used in the frequency range of 0.001 GHz to 100 GHz. That is, the "high frequency magnetic material" of the present invention uses a "rare earth-iron-M-nitrogen magnetic material" (wherein rare earth means at least one element selected from the group consisting of rare earth elements including Y, Fe means iron element, M means at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn and Cr, and nitrogen means nitrogen element). And the "high frequency magnetic material" of the present invention is one in which the composition of the main phase of the "rare earth-iron-M-nitrogen magnetic material" satisfies the above formula 1. The main form of the "high frequency magnetic material" of the present invention (i.e., the "rare earth-iron-M-nitrogen magnetic material" (here, rare earth means at least one element selected from the group consisting of rare earth elements including Y, Fe means iron element, M means at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, and nitrogen means nitrogen element) whose main phase composition satisfies the above formula 1) is powder, and in the present application, this is also referred to as "high frequency magnetic material powder". The magnetic powder for high frequency is used for various applications as a composite magnetic material for high frequency after adjusting its composition and particle size, and adding components such as ceramics and resins as necessary to form the material. In the composite magnetic material for high frequency, ferromagnetism is mainly borne by the rare earth-iron-M-nitrogen magnetic material components, but when ceramic materials and resins coexist between the material powders, a significant improvement in electrical resistivity is achieved. In addition, by introducing and adjusting nano-ceramic materials or resins having a polarity of solubility parameters of 10 to 15, the isolated dispersion of the rare earth-iron-M-nitrogen magnetic material powder, which is the magnetic material powder for high frequency, is promoted, and a significant improvement in electrical resistivity is achieved. In addition, in this application, "nano" means a scale of 1 nm or more and less than 1000 nm, unless otherwise specified. By using these high-frequency composite magnetic materials, it is possible to obtain electromagnetic wave absorbing materials for use in the high-frequency range of 0.001 GHz to 100 GHz and high-frequency amplifying materials for use in the high-frequency range of 0.001 GHz to 0.1 GHz, with significantly reduced eddy current loss.
[0018] The composition, crystal structure, morphology, and magnetic anisotropy of the "rare earth-iron-M-nitrogen magnetic material" used as the "high frequency magnetic material" of the present invention will be described below. Also, the manufacturing method of these materials (in particular, the method of nitriding rare earth-iron-M-based raw alloy to obtain the rare earth-iron-M-nitrogen magnetic material) will be described. As described above, the "high frequency magnetic material" of the present invention is a "rare earth-iron-M-nitrogen magnetic material" (wherein rare earth means at least one element selected from the group consisting of rare earth elements including Y, Fe means elemental iron, M means at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, and nitrogen means elemental nitrogen). The composition of the main phase of the "rare earth-iron-M-nitrogen magnetic material" used as the "high frequency magnetic material" of the present invention is specifically represented by the general formula described in the above formula 1, and the rare earth element (R) in the above formula 1 may include at least one element selected from the group consisting of the following rare earth elements: Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu. Therefore, a raw material containing a mixture of two or more rare earth elements such as misch metal and didymium may be used, but the preferred rare earth element is at least one element selected from the group consisting of Sm, Y, Ce, La, Pr, Nd, Gd, Dy, Er and Yb. More preferably, it is at least one element selected from the group consisting of Sm, Y and Ce. It is more preferable to contain at least one of Sm, Y, and Ce in 50 atomic % or more of the entire R component, since this provides a material with a magnetic permeability or a "maximum absorbed energy coefficient" defined below exceeding 2 GHz, and further a material with extremely high permeability exceeding 5 GHz. In particular, it is preferable to contain 50 atomic % or more of Sm in terms of the balance between oxidation resistance and cost.
[0019] The crystal structure of the main phase of the above-mentioned "rare earth-iron-Mn-nitrogen magnetic material" used as the "high frequency magnetic material" of the present invention is preferably at least one selected from tetragonal, hexagonal, rhombohedral and amorphous, and is more preferably tetragonal or amorphous. In a rare earth-iron-M-nitrogen magnetic material (hereinafter, this material is also referred to as an "R-Fe-MN magnetic material", and the "R" is also referred to as the "rare earth component" or "R component") having at least one type of crystal structure selected from tetragonal, hexagonal, rhombohedral, and amorphous (particularly tetragonal or amorphous), the content of Sm, Y, or Ce in the rare earth component is preferably 50 atomic % or more in the rare earth component, in view of one of the objects of the present invention to actively utilize in-plane magnetic anisotropy. This is because, in a rare earth-iron-M-nitrogen magnetic material having a tetragonal crystal structure, when the rare earth component is Sm, the uniaxial anisotropy constant K u Since the magnetocrystalline anisotropy is negative, the material has in-plane magnetocrystalline anisotropy. For other elements such as Pr, Nd, Gd, Tb, Dy, Ho, Er, Tm, and Lu, the uniaxial anisotropy constant K u This is because the magnetocrystalline anisotropy of these materials tends to be uniaxial, since the magnetocrystalline anisotropy of the amorphous rare earth-iron-M-nitrogen magnetic material of the present invention is almost isotropic, and the material is suitably used as a high-frequency amplification material such as a magnetic field amplification material used in the range of 0.001 GHz to 0.1 GHz. The rare earth elements used herein may be of a purity that can be obtained by industrial production, and the presence of impurities that are unavoidable during production, such as O, H, C, Al, Si, F, Na, Mg, Ca, and Li, is not a problem.
[0020] The rare earth component (R component) content in the above-mentioned "rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material)" used as the "high frequency magnetic material" of the present invention is preferably 2 atomic % or more and 15 atomic % or less in the magnetic material composition. Setting the R component to 2 atomic % or more is preferable in order to avoid the problem that if the content is less than that amount, the soft magnetic metal phase containing a large amount of iron component will separate beyond the allowable amount even after casting and annealing of the master alloy, and such type of soft magnetic metal phase will have a "maximum absorption frequency" defined later in a low frequency range, reducing the magnetic permeability and hindering the function as a high frequency magnetic material in the high frequency range (especially the ultra-high frequency range), which is one of the objects of the present invention. In addition, it is preferable to set the content of the R component to 15 atomic % or less in order to avoid problems such as a decrease in magnetic permeability and magnetization that would occur if the content exceeded that amount. A more preferable composition range of the R component is 5 atomic % or more and 10 atomic % or less. Iron (Fe) is a basic component of the "rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material)" which is responsible for the ferromagnetism in the present invention, and its content is preferably 10 atomic % or more in the magnetic material composition. The iron component (Fe component) content of 10 atomic % or more is preferable in order to avoid the problem of the magnetic permeability and magnetization becoming small when the content is less than that. In addition, the iron component (Fe component) content of 94.5 atomic % or less in the magnetic material composition is preferable in order to avoid the problem of the soft magnetic metal phase containing a large amount of Fe being separated when the content exceeds that amount, and the above-mentioned problem of the R component being insufficient (i.e., when the R component content is less than 2 atomic %). When the composition range of the iron component (Fe component) is 40 atomic % or more and 85 atomic % or less, a balanced material with high magnetic permeability and a natural resonance frequency or maximum absorption frequency in a more preferable range is obtained, and therefore this composition range is particularly preferable.
[0021] The "M component" in the above "rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material)" used as the "high frequency magnetic material" of the present invention is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn and Cr. The introduction of the M component is essential for producing a rare earth-iron-M-nitrogen magnetic material having a tetragonal crystal structure. In addition, when a nitriding method using a mixed gas of ammonia and hydrogen is applied, the rare earth-iron-M-nitrogen magnetic material can be made into an amorphous material at a relatively low temperature, low partial pressure, and in a short time, and the high frequency magnetic material of the present invention can be produced which is homogeneous, has a high magnetic permeability, and has a high natural resonance frequency or maximum absorption frequency compared to the case where the M component is not included. In the case of tetragonal rare earth-iron-M-nitrogen magnetic materials, there are three types of sites for the M component in the crystal structure: 8i, 8j, and 8f, but the occupancy position varies depending on the M component. Ti, V, Mo, Nb, and W mainly occupy the 8i site, and some rare earth-iron-M-nitrogen magnetic materials containing the M component can be materials with in-plane anisotropy, and become high-frequency magnetic materials with high magnetic permeability in the high-frequency range. Conversely, when the M component is Si or Al, it mainly occupies the 8j and 8f sites. Among R-Fe-MN magnetic materials containing this M component, if the amount of N component exceeds 7 atomic %, it becomes a high-frequency magnetic material that can be used especially in the ultra-high frequency range. When the M component is Mn or Cr, it occupies all of the 8i, 8j, and 8f sites. In particular, when the amount of M component is in the range of more than 7 atomic % to 25 atomic % or less, it has a high maximum absorption frequency. The content of the M component in the above-mentioned "rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material)" must be 0.5 to 25 atomic %. In particular, when preparing a tetragonal rare earth-iron-M-nitrogen magnetic material, the amount of M component is preferably 2 atomic % or more. When preparing an amorphous rare earth-iron-M-nitrogen magnetic material, the amount of M component needs to be 0.5 atomic % or more in order to stabilize the structure. Regardless of the crystal structure, the inclusion of the M component results in a high-frequency magnetic material with extremely high magnetic permeability and maximum absorbed energy coefficient. In addition, if the amount of M component in the rare earth-iron-M-nitrogen magnetic material exceeds 25 atomic %, not only is the magnetic permeability extremely low, which is undesirable, but the preferable crystal structure cannot be maintained. In the description of the present invention in this application, when "iron component" or "Fe component" is written, or when "Fe" or "iron" is written in a formula such as "R-Fe-MN system" or in the context of discussing the composition of a magnetic material, unless otherwise specified, it may also include a composition in which 50 atomic % or less of iron (Fe), which is the basic component of the "rare earth-iron-M-nitrogen-based magnetic material" in the high-frequency composite magnetic material of the present invention, is replaced with a ferromagnetic element such as Co or Ni. In this case, it is preferable to replace 0.01 atomic % or more and 50 atomic % or less of the iron component (Fe component) with Co or Ni, but it is particularly preferable to replace 1 atomic % or more and 50 atomic % or less of the iron component (Fe component) with Co or Ni component in order to obtain high oxidation resistance performance and to realize even higher magnetic permeability. It is preferable to set the amount of substitution of Co or Ni component to 50 atomic % or less of the iron component (Fe component) in order to avoid the problem that if the amount of substitution exceeds this amount, the above-mentioned effect on the increase in manufacturing cost is small, and no gain in cost performance is obtained, and the magnetic properties become unstable. Also, it is preferable to set the amount of substitution of Co or Ni component to 0.01 atomic % or more of the iron component (Fe component) in order to avoid the problem that if the amount of substitution is less than this amount, the effect of substitution is hardly observed.
[0022] As described above, the present invention is characterized by using a "rare earth-iron-M-nitrogen magnetic material" as a high-frequency magnetic material, and is a magnetic material that enables use in high-frequency ranges that are difficult when oxide magnetic materials or metal-based magnetic materials are used. In order to achieve particularly excellent "target functions," it is desirable to set the content of nitrogen (N), which is a basic component of the "rare earth-iron-M-nitrogen magnetic material" used in the present invention, in the range of 3 atomic % to 50 atomic % in the magnetic material composition. Setting the content of the nitrogen (N) component to 50 atomic % or less is preferable in order to avoid the problem that the magnetic permeability is generally reduced when the content exceeds that content. In addition, setting the nitrogen (N) component to 3 atomic % or more is preferable in order to avoid the problem that the magnetic permeability is not improved much in the high-frequency range or the ultra-high-frequency range when the content is less than that content. In the case of tetragonal rare earth-iron-M-nitrogen magnetic materials, the nitrogen content is preferably 3 atomic % or more and 25 atomic % or less, depending on the type and content of the rare earth component and M component, and in the case of amorphous rare earth-iron-M-nitrogen magnetic materials, the nitrogen content is preferably 10 atomic % or more and 50 atomic % or less. Compared with rhombohedral or hexagonal rare earth-iron-M-nitrogen magnetic materials, tetragonal rare earth-iron-M-nitrogen magnetic materials, whose crystals are thermodynamically unstable, are more likely to be amorphized in regions with a smaller nitrogen content, and are nitrided amorphous at low temperatures in a short time, so that the crystal phases such as iron nitride, rare earth nitride, and nitrides of the M component are not separated, and the whole is nitrided amorphous uniformly. This is the reason why it is preferable to use a tetragonal rare earth-iron-M raw material alloy in producing the magnetic material of the present invention. The inclusion of nitrogen in the magnetic material used as the high frequency magnetic material of the present invention is one of the important features of the composition of the high frequency magnetic material of the present invention, and one of the main effects of this is an increase in electrical resistivity. This is because it can solve the problem that when eddy current loss increases, the real term of the complex relative permeability decreases, preventing large electromagnetic wave absorption due to natural resonance in the high frequency range or ultra-high frequency range. This effect is particularly remarkable in the amorphous rare earth-iron-M-nitrogen magnetic material of the present invention.
[0023] In materials with the same magnetic permeability, the higher the electrical resistivity, the higher the critical frequency at which eddy currents occur. Therefore, in the high-frequency magnetic material of the present invention, the electrical resistivity increases by containing a certain amount of nitrogen in the magnetic material, and eddy current loss does not become noticeable until the frequency reaches a high frequency range that is commensurate with the inherently high natural resonance frequency of the R-Fe-MN magnetic material. Therefore, a high complex relative permeability real term can be maintained up to the high frequency range including the ultra-high frequency range, and the effect of natural resonance can be fully exerted in the even higher frequency range, so that a high complex relative permeability imaginary term can be realized in the high frequency range including the ultra-high frequency range. In addition, when used as a high-frequency amplification material at frequencies of 0.001 GHz or more and 0.1 GHz or less, if eddy current loss occurs in that frequency range, the temperature of the material rises or the real term of the magnetic permeability becomes small, which is undesirable as it reduces efficiency. From this perspective, in order to further improve the electrical resistivity of the rare earth-iron-M-nitrogen magnetic material and make it a high-frequency magnetic material that can be suitably used in the ultra-high frequency range of 1 GHz or more, it is more desirable to control the content of nitrogen (N), which is a basic component of the "rare earth-iron-M-nitrogen magnetic material" used in the present invention, to a "high nitriding" range of 7 atomic % to 30 atomic %. From the viewpoint of simplifying the process, a range of 10 atomic % to 25 atomic % in which annealing treatment after the nitriding process is not essential is more preferable, and rare earth-iron-nitrogen magnetic materials with the nitrogen content adjusted to this range have particularly high natural resonance frequencies and electrical resistivities. In addition, this high nitriding region R-Fe-MN magnetic material is produced by using a nitriding process by a gas-phase reaction using a gas containing ammonia. For example, when nitrogen gas is used, it is difficult to obtain a homogeneous highly nitrided material.
[0024] The most preferable range (i.e., the optimum range) of the nitrogen content may vary depending on the intended application, the R-Fe-M composition ratio of the R-Fe-MN magnetic material, the amount ratio of the subphases, and further the crystal structure. For example, Sm 7.7 Fe 84.6 Ti 7.7As the raw material alloy, the optimum nitrogen content is in the range of 5 atomic % to 10 atomic % within the range of 3 atomic % to 50 atomic %. The optimum nitrogen content here is the nitrogen content that optimizes at least one of the oxidation resistance and magnetic or electrical properties of the material, although it differs depending on the purpose.
[0025] Here, "magnetic properties" refers to the permeability (μμ0), relative permeability (μ), and complex permeability (μ r μ0), complex relative permeability (μ r ), its real term (μ'), imaginary term (μ") and absolute value (|μ r |), the maximum value of μ” in any frequency domain in the frequency dependence of the complex relative permeability imaginary term (μ” max ) and the frequency at that time (f a This frequency is called the "maximum absorption frequency"), and the maximum value of μ' in any frequency range in the frequency dependence of the complex relative permeability real term (μ' max ) and the frequency at that time (f t ), the product (fμ”) of the complex relative permeability imaginary term (μ”) at a certain frequency (f) and that frequency (f) is called the “absorbed energy coefficient.” The maximum absorbed energy coefficient (fμ”) is the maximum value of the product (fμ”). max ), magnetization (I s ), uniaxial magnetic anisotropy magnetic field or in-plane magnetic anisotropy magnetic field (H a , H a1 , H a2 ), magnetic anisotropy energy (E a ), the absolute value of the magnetic anisotropy ratio (p / q: when a magnetic material is uniaxially oriented in an orientation magnetic field of 1.2 MA / m, the magnetization in an external magnetic field of 1.0 MA / m in the direction of the applied orientation magnetic field is q, and the magnetization in an external magnetic field of 1.0 MA / m in the perpendicular direction is p), the temperature change rate of magnetic permeability, and the natural resonance frequency with the external AC magnetic field caused by electromagnetic waves, etc. (f r ) means at least one of the following:
[0026] "Electrical properties" refers to the electrical resistivity (= volume resistivity ρ), electrical conductivity (σ), impedance (Z), inductance (L), capacitance (C), reactance (R), dielectric constant (εε0), relative dielectric constant (ε), complex dielectric constant (εr ε0), complex relative permittivity (ε r ), its real term (ε'), imaginary term (ε") and absolute value (|ε r |), the loss term in the complex relative permittivity, which is a combination of dielectric loss and conduction loss (ε t =ε”+σ / ω, this ε t is called the electrical loss term. ω is the angular frequency. The above "magnetic properties" and "electrical properties" are collectively referred to as "electromagnetic properties". Generally, a horizontal line (-) is added to the symbols "μ" and "ε" representing relative permeability and relative dielectric constant, but in this application, relative permeability is represented as "μ" and relative dielectric constant as "ε". The above permeability can be regarded as the absolute value of the complex permeability when f→0, and the dielectric constant can be regarded as the absolute value of the complex dielectric constant when f→0.
[0027] In addition, "magnetic permeability" is the relative magnetic permeability (μ) multiplied by the magnetic permeability of a vacuum (μ0), and "dielectric constant" is the relative dielectric constant (ε) multiplied by the dielectric constant of a vacuum (ε0). In the description of the present invention in this application, for example, when "high magnetic permeability" or the equivalent "high relative magnetic permeability" is expressed, it means not only that the magnetic permeability or relative magnetic permeability of the material is high in a static magnetic field, but also that the absolute value of the complex permeability or complex relative magnetic permeability is high in an AC magnetic field such as when electromagnetic waves are acting, and that if the value of the imaginary term of the complex relative magnetic permeability is close to 0, the value of the real term of the complex relative magnetic permeability is high, and conversely, if the value of the real term of the complex relative magnetic permeability is close to 0, the value of the imaginary term of the complex relative magnetic permeability is high. The above relationship is also true for "permittivity" and "relative dielectric constant", so it can be understood as it is by replacing "permeability" and "relative magnetic permeability" in the above description with "permittivity" and "relative dielectric constant", respectively.
[0028] Next, the state in which the magnetic or electrical characteristics are optimal will be described. The state where the magnetic or electrical properties are optimal means that the values of the permeability, the real or imaginary term in the high frequency range of the complex relative permeability, the magnetization, Curie point, electrical resistivity, dielectric constant, the real or imaginary term in the complex relative dielectric constant, etc. are maximum, and the absolute value of the temperature coefficient of permeability and magnetization, the electrical conductivity, etc. are minimum. The magnetic anisotropy ratio, magnetic anisotropy magnetic field, magnetic anisotropy energy, etc., which are closely related to the natural resonance frequency, are said to be optimal when they are set to values that cause natural resonance at the desired frequency or maximize the absorption of electromagnetic waves. The compositions of the R-Fe-MN magnetic material of the present invention are such that the R component (rare earth component) is in the range of 2 atomic % or more and 15 atomic % or less, the Fe component (iron component) is in the range of 10 atomic % or more and 94.5 atomic % or less, the M component is in the range of 0.5 atomic % or more and 25 atomic % or less, and the N component (nitrogen component) is in the range of 3 atomic % or more and 50 atomic % or less, and all of these are satisfied simultaneously.
[0029] Furthermore, the R-Fe-MN magnetic material obtained by the present invention may contain hydrogen (H) in a content ranging from 0.01 atomic % to 10 atomic % inclusive in the magnetic material composition. When H is contained in the above composition range, the oxidation resistance and magnetic permeability are improved. In this case, the composition of the R-Fe-MN magnetic material of the present invention is represented by the general formula R x Fe (100-x-y-z-α) M y N z H α where x, y, z, and α are in the ranges, in atomic %, of 2≦x / (1-α / 100)≦15, 0.5≦y / (1-α / 100)≦25, 3≦z / (1-α / 100)≦50, and 0.01≦α≦10, respectively, and x, y, z, and α are selected so that these four equations are simultaneously true. Furthermore, depending on the manufacturing method, oxygen (O) may be contained in an amount of 0.1 atomic % or more and 20 atomic % or less, in which case the stability of the magnetic properties is improved and a magnetic material with high electrical resistivity can be obtained. Therefore, a more preferable composition of the R-Fe-MN-HO magnetic material of the present invention is represented by the general formula R x Fe (100-x-y-z-α-β) M y N z H α O βWhen expressed as above, x, y, z, α, and β are in the ranges of 2≦x / {(1-α / 100)(1-β / 100)}≦15, 0.5≦y / {(1-α / 100)(1-β / 100)}≦25, 3≦z / {(1-α / 100)(1-β / 100)}≦50, 0.01≦α / (1-β / 100)≦10, and 0.1≦β≦20 in atomic percent, respectively, and x, y, z, α, and β are selected so that these five formulas are simultaneously satisfied. If this oxygen component is localized on the magnetic powder surface, it is highly effective in improving the electrical resistivity, and for this purpose, it is also effective to add various surface oxidation treatments, including acid treatment, alkali treatment, heat treatment, and coupling treatment, to the powder surface before and after nitriding and before and after fine powder adjustment.
[0030] Less than 50 atomic % of the nitrogen (N) component of the "rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material)" used as the "high frequency magnetic material" of the present invention may be replaced with at least one element selected from the group consisting of H, C, P, Si and S. In this case, it is preferable to replace 0.01 atomic % or more and less than 50 atomic % of the nitrogen (N) component of the rare earth-iron-M-nitrogen magnetic material (R-Fe-MN magnetic material) with at least one element selected from the group consisting of H, C, P, Si and S. When replacing the nitrogen (N) component with at least one of these elements, depending on the type and amount of the replacing element, not all of the N component is replaced with the N component, and it is not necessarily replaced one-to-one. However, depending on the type and amount of the replaced element, it may bring about improvement in electromagnetic properties such as oxidation resistance performance, magnetic permeability, and dielectric constant, and when used in a high frequency resin composite magnetic material, it may be expected that the affinity with the resin component is improved and mechanical properties are improved. It is preferable to replace 0.01 atomic % or more of the nitrogen (N) component with at least one of the above elements in order to avoid the problem that the effect of the above replacement is almost lost if the amount of replacement is less than that amount, and it is preferable to replace less than 50 atomic % of the nitrogen (N) component with at least one of the above elements in order to avoid the problem that the effect of nitrogen in improving the electrical resistivity and optimizing the resonance frequency is hindered if the amount of replacement is more than that amount.
[0031] In the description of the present invention in this application, when the term "nitrogen component" or "N component" is used, or when the term "N" or "nitrogen" is used in formulas such as "rare earth-iron-M-nitrogen-based magnetic material" or "R-Fe-MN-based" or in the context of discussing the composition of a magnetic material, unless otherwise specified, this also includes a composition in which 0.01 atomic % or more and less than 50 atomic % of nitrogen (N), which is a basic component of the "rare earth-iron-M-nitrogen-based magnetic material" in the high frequency magnetic material of the present invention, is replaced with at least one element selected from the group consisting of H, C, P, Si, and S. The "rare earth-iron-M-nitrogen magnetic material" used as the "high frequency magnetic material" of the present invention preferably contains a phase having at least one crystal structure selected from tetragonal, rhombohedral, hexagonal and amorphous as the main phase, and more preferably contains a phase having a tetragonal or amorphous crystal structure. In the present invention, a phase that creates these crystal structures and contains at least R (rare earth), Fe (iron), M (M component) and N (nitrogen) is called the "main phase", and a phase having a composition that creates other crystal structures than the above crystal structures is called the "subphase". The subphase means a phase that is not the main phase and is generated intentionally or unintentionally in the process of producing a rare earth-iron-M-nitrogen (-hydrogen-oxygen) magnetic material from a rare earth-iron raw material. The components of the main phase may include H (hydrogen) and / or O (oxygen) in addition to R (rare earth), Fe (iron), M (M component) and N (nitrogen). An example of a preferred crystal structure of the main phase is ThMn 12 The tetragonal crystal structure is similar to that of Th2Zn. 17 The rhombohedral crystal has a similar crystal structure to Th2Ni 17 Examples of such crystal structures include hexagonal crystals having a crystal structure similar to that of TbCu7, CaZn5, etc., and amorphous crystals (also called amorphous nitride because they are made amorphous in the nitriding process). Among these, ThMn 12 In order to ensure good electromagnetic properties and their stability, it is particularly preferable that the main phase of the magnetic material is or contains a tetragonal or amorphous phase having a similar crystal structure to those mentioned above.
[0032] The R-Fe-MN magnetic material may contain subphases such as an R-Fe-M alloy raw material phase, a hydride phase, a decomposed phase containing Fe nanocrystals, and an amorphous oxide phase, but in order to fully exert the effects of the present invention, the volume fraction of the subphase must be kept lower than the content of the main phase, and therefore it is extremely preferable in practical terms for the content of the main phase to exceed 75 volume % of the entire R-Fe-MN magnetic material. In many cases, the main phase of an R-Fe-MN magnetic material is obtained when nitrogen penetrates between the lattices of the R-Fe-M alloy, which is the main raw material phase, causing the crystal lattice to expand or exceeding this, causing the crystal structure to collapse or begin to collapse, but the crystal structure before becoming amorphous has approximately the same symmetry as the main raw material phase. R-Fe-MN magnetic materials with tetragonal, rhombohedral or hexagonal main raw phases are nitrided using R-Fe-M alloy raw phases with the same symmetry. On the other hand, amorphous R-Fe-MN magnetic materials have a structure in which the tetragonal, rhombohedral or hexagonal main raw phase is nitrided and its crystal structure is destroyed. This phenomenon is called "nitriding amorphization" or "nitriding amorphization". The tetragonal R-Fe-M alloy raw phase is more easily amorphized by nitriding than the rhombohedral or hexagonal R-Fe-M alloy raw phases, and is particularly preferred as a raw material for amorphous R-Fe-MN magnetic materials. The term "volume fraction" used here refers to the ratio of the volume occupied by a certain component to the total volume, including voids, of the magnetic material. In the present application, the term "main raw material phase" refers to a phase that contains at least R (rare earth), Fe, and M components, does not contain N, and has at least one crystal structure selected from tetragonal, hexagonal, and rhombohedral (particularly, rhombohedral or hexagonal) (note that in the present application, a phase that has a composition or crystal structure other than the above and does not contain N is referred to as a "secondary raw material phase").
[0033] The expansion of the crystal lattice due to the intrusion of nitrogen improves the material's oxidation resistance and at least one of its magnetic and electrical properties, making it a practically suitable R-Fe-MN magnetic material. Only after the introduction of nitrogen does it become a suitable high-frequency magnetic material, and it exhibits electromagnetic properties completely different from those of conventional nitrogen-free R-Fe-M alloys and Fe. For example, the main raw material phase of the R-Fe-M master alloy is Sm 7.7 Fe 77.0 Co 3.8 Mo 11.5 When the above is selected, the introduction of nitrogen increases the electrical resistivity, and improves the magnetic properties such as the Curie point, the magnetic permeability, and the absolute value of the magnetic anisotropy energy, as well as the oxidation resistance.
[0034] The rare earth-iron-magnesium-nitrogen magnetic material used as the "high frequency magnetic material" of the present invention is preferably a material that utilizes its in-plane magnetic anisotropy. An in-plane magnetic anisotropy material is a material that is energetically more stable when the magnetic moment exists on the c-plane due to the existence of a magnetic moment on the c-axis. Sm-Fe-MN magnetic materials having a rhombohedral or hexagonal crystal structure are not in-plane magnetic anisotropic materials but uniaxial magnetic anisotropic materials, and their practical use as magnet materials is being considered. However, when such magnet materials that are not in-plane magnetic anisotropic materials but are uniaxial magnetic anisotropic materials are used as magnetic materials for high frequency applications, they often only function in the high ultra-high frequency range exceeding 100 GHz as mentioned above, and the magnetic permeability in the ultra-high frequency range is small. In order to avoid such problems, it is preferable that the content of the Sm-Fe-MN magnetic material is less than 50 volume % of the total magnetic material.
[0035] Similarly to Sm-Fe-MN magnetic materials, known rare earth magnet materials such as Sm-Fe-Ti, Nd-Fe-B and Sm-Co, which are tetragonal but not nitride, have uniaxial magnetic anisotropy instead of in-plane magnetic anisotropy, and cannot be said to be suitable as magnetic materials for high frequencies. The reason is that magnetic materials for Nd-Fe-B and Sm-Co magnets have uniaxial magnetic anisotropy, and are metallic magnetic materials, so that they have low electrical resistivity and show a decrease in magnetic permeability in the high frequency range due to eddy current loss. The rare earth-iron-Mn-nitrogen magnetic material of the present invention is preferably an isotropic amorphous material obtained by nitriding a tetragonal raw alloy, unless it is a material that utilizes in-plane magnetic anisotropy. This material is a nitrided amorphous material containing a large amount of nitrogen, and because of its high electrical resistance, the decrease in magnetic permeability due to eddy current loss is significantly suppressed even if the powder particle size is large. Because of the high nitrogen content, the magnetization value is smaller than that of the rare earth-iron-Mn-nitrogen magnetic material of the present invention that utilizes in-plane anisotropy, but the magnetic permeability remains high up to the ultra-high frequency range.
[0036] When the high frequency magnetic material of the present invention is in the form of a powder, the powder preferably has an average particle size of 0.1 μm to 2000 μm, more preferably 0.2 μm to 200 μm. Here, the term "average particle size" refers to the median diameter calculated based on a volume-equivalent diameter distribution curve obtained by a commonly used particle size distribution measuring device. An average particle size of 0.1 μm or more is preferable in that it is possible to avoid the occurrence of ignition and the complicated manufacturing process, such as handling the powder in a low-oxidizing atmosphere. On the other hand, a particle size of 2000 μm or less is preferable in that it is possible to avoid the difficulty in manufacturing a homogeneous nitride and the resulting material having poor absorption of electromagnetic waves at 0.001 GHz or more. Therefore, the high-frequency magnetic material of the present invention uses powder with an average particle size of 0.1 μm or more and 2000 μm or less. Also, if the average particle size is less than 0.2 μm, the magnetic permeability drops and the magnetic powder aggregates significantly, making it impossible to fully utilize the magnetic properties inherent to the material, and it is in a range that is not suitable for general industrial production, so it cannot be said to be a very appropriate particle size range, but even if it is less than 0.2 μm, it has the advantage that it is suitable for thin or ultra-small high-frequency magnetic materials for special purposes because it has overwhelmingly superior oxidation resistance compared to nitrogen-free metal-based high-frequency magnetic materials. From this perspective, it is preferable that the lower limit of the average particle size in the high-frequency magnetic material of the present invention is 0.1 μm, which is less than 0.2 μm. However, as described above, it is more preferable to set the average particle size to 0.2 μm or more in order to avoid the above-mentioned problems that arise when the average particle size is less than this. Furthermore, it is more preferable to set the average grain size to 200 μm or less in order to avoid the problem of a decrease in magnetic permeability in the high frequency range that occurs when the average grain size exceeds this value. If the average particle size is in the range of 0.5 μm to 10 μm, f a This results in a material with high magnetic permeability in the high frequency range, making it easy to obtain a material with a high selective absorption ratio at frequencies above 0.1 GHz. When the average particle size is in the range of 10 μm or more and 200 μm or less, the magnetic permeability is high and the imaginary term of the magnetic permeability is low, making it easy to obtain a high frequency amplifying material in the range of 0.001 GHz or more and 0.1 GHz or less.
[0037] When the "high frequency magnetic material" of the present invention is an amorphous rare earth-iron-nitrogen magnetic material, because of its high electrical resistance, it can be used as a high frequency amplification material, such as a magnetic field amplification material, used in the range of 0.001 GHz or more and 0.1 GHz or less, even if the average particle size is in the range of 1 μm or more and 200 μm or less.
[0038] The "rare earth-iron-Mn-nitrogen magnetic material" used as the high frequency magnetic material of the present invention includes metal Fe, metal Ni, metal Co, Fe-Ni alloys, Fe-Ni-Si alloys, sendust, Fe-Si-Al alloys, Fe-Cu-Nb-Si alloys, a At least one selected from the group consisting of metallic magnetic materials such as amorphous alloys, garnet-type ferrites such as magnetite, Ni-ferrite, Zn-ferrite, Mn-Zn ferrite, Ni-Zn ferrite, and soft magnetic hexagonal magnetoplumbite-based ferrites, and oxide-based magnetic materials may be mixed (also referred to as blending). In other words, the metallic magnetic materials and oxide-based magnetic materials to be mixed may be one type or two or more types. In addition, there is no particular restriction on the form of the metallic magnetic materials and oxide-based magnetic materials to be mixed. For example, when metallic Fe, metallic Ni, and metallic Co are taken as metallic magnetic materials to be mixed, there is no particular restriction on the form of these, and they may be in the form of, for example, metallic powder or metallic foil. When this mixed material is applied to an electromagnetic wave absorbing material, it is possible to expand the frequency band for absorbing electromagnetic waves from high frequency to low frequency, and to absorb noise in a wide band by imparting broad absorption characteristics even in the high frequency region. In particular, when carbonyl iron having a particle size of 0.1 μm to 100 μm is used as the metallic Fe in the mixed material, it becomes a high frequency magnetic material with a good balance between the magnetic permeability below 1 GHz and the magnetic permeability above 1 GHz. The reasons why carbonyl iron can obtain high characteristics when mixed with rare earth-iron-M-nitrogen-based materials are as follows: [1] the circularity of carbonyl iron is very high, 0.7 to 1, and it has excellent electrical insulation, and [2] when mixed with rare earth-iron-M-nitrogen-based magnetic materials in powder form, the signs of the surface electrostatic charges of the metal powder carbonyl iron and the nitride powder rare earth-iron-M-nitrogen material are different, making it easy to mix homogeneously. In the high frequency magnetic material of the present invention used at ultra-high frequencies, when carbonyl iron is used as the magnetic material (mixed material) to be mixed with the rare earth-iron-M-nitrogen magnetic material, the preferred average particle size of the carbonyl iron powder is in the range of 1 μm or more and 10 μm or less.
[0039] In the high frequency composite magnetic material of the present invention, the amount of material to be mixed with the rare earth-iron-M-nitrogen magnetic material to form a composite (i.e., a magnetic material different from the rare earth-iron-M-nitrogen magnetic material, or a non-magnetic material (e.g., a non-magnetic ceramic material and / or resin)) is preferably 0.001% by mass or more and 99% by mass or less of the total magnetic material in the high frequency composite magnetic material of the present invention. A content of 0.001% by mass or more is preferable because it is advantageous for obtaining the effect of adding a metal-based magnetic material or an oxide-based magnetic material used as a mixing material, and a content of 99% by mass or less is preferable because it is advantageous for obtaining the effect on various electromagnetic properties of the rare earth-iron-M-nitrogen magnetic material of the present invention. Therefore, for example, in the high-frequency composite magnetic material of the present invention, when at least one selected from the group consisting of metal-based magnetic materials such as metal Fe, metal Ni, metal Co, Fe-Ni alloys, Fe-Ni-Si alloys, sendust, Fe-Si-Al alloys, Fe-Cu-Nb-Si alloys, and amorphous alloys, and oxide-based magnetic materials such as garnet-type ferrites such as magnetite, Ni-ferrite, Zn-ferrite, Mn-Zn ferrite, and Ni-Zn ferrite, and soft magnetic hexagonal magnetoplumbite-based ferrites, is mixed as the mixed material, the amount of the rare earth-iron-M-nitrogen-based magnetic material is preferably in the range of 1% by mass or more and 99.999% by mass or less, and the amount of at least one selected from the group consisting of the metal-based magnetic materials and the oxide-based magnetic materials to be mixed is preferably in the range of 0.001% by mass or more and 99% by mass or less. Furthermore, for example, when a ceramic material is used as the mixed material in the high-frequency composite magnetic material of the present invention, it is preferable that the amount of the rare earth-iron-M-nitrogen based magnetic material is 1 mass % or more and 99.999 mass % or less, and the amount of the ceramic material is 0.001 mass % or more and 99 mass % or less. The effect can be more effectively achieved by setting the mass fraction of the amount of metal-based magnetic materials other than the rare earth-iron-Mn-nitrogen-based magnetic materials and oxide-based magnetic materials relative to the total magnetic materials in the range of 0.05 mass % to 75 mass %. Furthermore, when the mass fraction of the amount of metal-based magnetic materials and oxide-based magnetic materials other than the rare earth-iron-M-nitrogen-based magnetic materials relative to the total amount of magnetic materials is 0.01 mass % or more and 50 mass % or less, the characteristics of the electrical properties of the rare earth-iron-M-nitrogen-based magnetic materials can be more effectively exhibited. For this reason, when the mass fraction of the amount of metal-based magnetic materials and oxide-based magnetic materials other than the rare earth-iron-M-nitrogen-based magnetic materials relative to the total amount of magnetic materials is set to be 0.05 mass % or more and 50 mass % or less, the rare earth-iron-M-nitrogen-based magnetic materials can more effectively exhibit both of their characteristics, such as absorption in the ultra-high frequency range, and their electrical properties.
[0040] Among the high frequency composite magnetic materials of the present invention that use rare earth-iron-Mn-nitrogen magnetic materials and among those high frequency resin composite magnetic materials, there are materials whose imaginary term value of the complex dielectric constant, i.e., the value of the electrical loss term, exceeds 10 or even exceeds 50 at frequencies of 1 GHz or above. The typical value of the electrical resistivity of the rare earth-iron-Mn-nitrogen magnetic material itself is in the range of 200 μΩcm or more and 8000 μΩcm or less, which is an appropriate magnitude that lies between nitrogen-free metal magnetic materials and oxide magnetic materials. When an electronic circuit is used as an electromagnetic wave source, the electromagnetic waves in the far field (meaning an area that is more than 1 / 2π of the wavelength from the electromagnetic wave source. Areas that are not in the far field are called the near field) have a sufficiently large electric field E equivalent to the magnetic field H, so the high-frequency composite magnetic material of the present invention, which uses a rare earth-iron-M-nitrogen-based magnetic material, is very suitable for use in ultra-high frequency applications such as absorbing noise exceeding 1 GHz, or as a far-field electromagnetic wave absorber for use in anechoic chambers, because it is a magnetic material with a high dielectric constant. It is preferable to make full use of this feature when compounding (mixing) the above-mentioned metal-based magnetic materials and oxide-based magnetic materials.
[0041] Next, the ceramic material used in the "composite magnetic material" which is the high frequency magnetic material of the present invention will be described. As described above, the electrical and magnetic properties of rare earth-iron-M-nitrogen magnetic materials are intermediate between those of metallic materials and oxide materials, and the chemical properties of the magnetic material surface are also intermediate between the two. Therefore, when mixing the rare earth-iron-M-nitrogen magnetic materials in powder form, by shaking the materials in a container (hereinafter also referred to as "shaking"), the charge states of the powder surfaces of the rare earth-iron-M-nitrogen magnetic material and metallic materials, or the rare earth-iron-M-nitrogen magnetic material and oxide material, will be separated into positive and negative, and the materials can be easily mixed in a homogeneous state. Therefore, for the purpose of providing electrical insulation between the rare earth-iron-Mn-nitrogen magnetic material powders and reducing eddy current loss, it is preferable to use an oxide ceramic material. In particular, if the oxide-based ceramic material is a nanopowder of less than 1 μm, a high-frequency composite magnetic material with high resistance and high filling rate can be realized. In particular, rare earth-iron-M-nitrogen-based magnetic material and nano-oxide-based ceramic material have the advantage that they can be mixed homogeneously in a short time by a simple operation such as shaking, and also have the advantage that magnetic field orientation is possible in the same way as with high-frequency resin composite magnetic materials by performing various magnetic field moldings described later after homogeneous mixing. Representative oxide-based materials include silica, alumina, chromium oxide, zirconia, magnesia, rare earth oxide, etc., and oxides or composite oxides containing at least one selected from the group consisting of rare earth and Fe, which are basic components of rare earth-iron-M-nitrogen magnetic materials, Co, Ni, Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, are preferred. Fe oxide is also a ceramic material that can be used in the present invention. As described above, the ceramic material used in the composite magnetic material of the present invention is preferably a nanoceramic material from the viewpoint of the isolated dispersibility of the rare earth-iron-M-nitrogen magnetic material powder, and therefore is preferably a powder having an average particle size of 1 nm or more and less than 1000 nm. In the present invention, when describing nanoceramic materials, the word "nano" may be added before the material name, such as "nanosilica" for silica having a particle size of 1 nm or more and 1000 nm or less.
[0042] Next, the "high frequency resin composite magnetic material" which is the high frequency magnetic material of the present invention will be described.
[0043] Examples of materials that can be used as the resin component of the high frequency resin composite magnetic material are given below. For example, polyamide-based resins such as 12-nylon, 6-nylon, 6,6-nylon, 4,6-nylon, 6,12-nylon, amorphous polyamide, and semi-aromatic polyamide; polyolefin-based resins such as polyethylene, polypropylene, and chlorinated polyethylene; polyvinyl-based resins such as polyvinyl chloride, polyvinyl acetate, polyvinylidene chloride, polyvinyl alcohol, and ethylene-vinyl acetate copolymer; acrylic-based resins such as ethylene-ethyl acrylate copolymer and polymethyl methacrylate; acrylonitrile-based resins such as polyacrylonitrile and acrylonitrile / butadiene / styrene copolymer; and various polyurethane-based resins. Examples of the resin include fluorine-based resins such as polytetrafluoroethylene; synthetic resins known as engineering plastics, such as polyacetal, polycarbonate, polyimide, polysulfone, polybutylene terephthalate, polyarylate, polyphenylene oxide, polyethersulfone, polyphenylsulfide, polyamideimide, polyoxybenzylene, and polyether ketone; thermoplastic resins including liquid crystal resins, such as wholly aromatic polyester; conductive polymers, such as polyacetylene; thermosetting resins, such as epoxy resin, phenolic resin, epoxy-modified polyester resin, silicone resin, and thermosetting acrylic resin; and elastomers, such as nitrile rubber, butadiene-styrene rubber, butyl rubber, nitrile rubber, urethane rubber, acrylic rubber, and polyamide elastomer.
[0044] The resin component of the high frequency resin composite magnetic material of the present invention is not limited to the resins exemplified above, but if at least one of the resins exemplified above is included, a high frequency resin composite magnetic material having high electrical resistivity, excellent impact resistance, flexibility and moldability can be obtained. The content of the resin component is preferably in the range of 0.1 mass% to 95 mass%. It is preferable to set the content of the resin component to 0.1 mass% or more in order to avoid the problem that if the content is less than that, the effect of the resin, such as impact resistance, is hardly exhibited, and it is preferable to set the content of the resin component to 95 mass% or less in order to avoid the problem that if the content exceeds that, the magnetic permeability and magnetization drop drastically, resulting in poor practical use as a high frequency resin composite magnetic material. Furthermore, when the only component other than the resin material component is a rare earth-iron-M-nitrogen based magnetic material, the ceramic material part does not have an electrical insulating effect, so it may be preferable to further increase the content of the resin component to 1 mass % or more and 95 mass % or less. Furthermore, in cases where the magnetic material component is only a rare earth-iron-Mn-nitrogen based magnetic material, in applications where high magnetic permeability and impact resistance are particularly required, for the same reasons as above, the range of 2 mass % or more and 90 mass % or less is more preferable, and the range of 3 mass % or more and 80 mass % or less is most preferable. The content of the magnetic material component in the high frequency resin composite magnetic material of the present invention is preferably 5% by mass or more and 99.9% by mass or less, more preferably 5% by mass or more and 99% by mass or less, even more preferably 10% by mass or more and 98% by mass or less, and most preferably 20% by mass or more and 97% by mass or less. The content of the magnetic material component of 5% by mass or more is preferable in order to avoid the problem that if the content is less than that amount, the magnetic permeability and magnetization will drop drastically, making the material less practical as a high frequency magnetic material, and the content of 99.9% by mass or less is preferable in order to avoid the problem that if the content exceeds that amount, the effects of the resin, such as impact resistance, will hardly be exhibited. In the high frequency resin composite magnetic material of the present invention, most of the electromagnetic properties are borne by the rare earth-iron-M-nitrogen magnetic material constituting the high frequency composite magnetic material used, and when the high frequency resin composite magnetic material of the present invention is applied to high frequency magnetic materials, electromagnetic noise absorbing materials, electromagnetic wave absorbing materials, RFID tag materials, coil cores for wireless power supply systems, etc., it imparts performance that makes use of the characteristics of resins such as impact resistance, flexibility, moldability, and high electrical resistivity to the high frequency composite magnetic material, thereby improving its practicality. Therefore, any resin component that does not impair the performance of the high frequency composite magnetic material used in the present invention and imparts "some inherent characteristics of the resin" can be said to be a very suitable component of the high frequency resin composite magnetic material of the present invention. The above "some inherent characteristic of the resin" is not limited to the characteristics of the resin exemplified above, but includes the characteristics and performance of all known resins. In addition, the rare earth-iron-M-nitrogen magnetic material used in the present invention can be electrically insulated with a resin component, making it possible to apply it to uses other than high frequency magnetic materials. In particular, when the rare earth component of the rare earth-iron-M-nitrogen magnetic material used in the present invention is limited to 50 atomic % or more of Sm, for example, i) By mixing the rare earth-iron-Mn-nitrogen magnetic material having small and large particle sizes to increase the filling rate and maintaining electrical insulation with resin, it can be used as a low-frequency material with excellent magnetic permeability. ii) Use as a magnetic recording material with increased magnetization by using the rare earth-iron-Mn-nitrogen magnetic material having shape magnetic anisotropy and maintaining electrical insulation with resin. It can be expanded to.
[0045] It is possible to add a titanium-based or silicon-based coupling agent to the high frequency resin composite magnetic material of the present invention. Generally, adding a large amount of titanium-based coupling agent improves flowability and moldability, which allows the amount of magnetic powder to be increased, and when magnetic field orientation is performed, the orientation is improved, resulting in a material with excellent magnetic properties. On the other hand, the use of silicon-based coupling agents increases the mechanical strength, but generally deteriorates flowability. In order to utilize the advantages of both titanium-based coupling agents and silicon-based coupling agents, they can be added in combination. In addition to titanium-based and silicon-based coupling agents, it is also possible to add aluminum-based, zirconium-based, chromium-based, or iron-based coupling agents. Furthermore, various kinds of lubricants, heat-resistant anti-aging agents, and antioxidants can be blended into the high frequency resin composite magnetic material of the present invention. When the high frequency resin composite magnetic material of the present invention is made into a compound powder, the particle size may be in a range that is easy to handle in each molding process such as calendar processing and injection molding, but in the present invention, the lower limit of the particle size is preferably 0.1 μm or more from the viewpoint of the oxidation resistance of the powder and the stability of the magnetic properties, and more preferably 0.2 μm or more to obtain a powder with flowability, and more preferably 10 μm or more to obtain a powder with excellent flowability. There is no particular restriction on the upper limit of the particle size, but if it is too large, the magnetic properties of the molded body will become uneven, so it is preferable to make it 5 cm or less. In particular, if the resin composite magnetic material is made 20 mm or less, the variation in the magnetic properties after molding will be further reduced, and if it is made 2 mm or less, excellent flowability will be imparted.
[0046] In the high-frequency resin composite magnetic material of the present invention, it is difficult to impart magnetism to the matrix resin. Therefore, unlike the ferrite-coated rare earth-iron-Mn-nitrogen material described in Patent Document 1, the high-frequency resin composite magnetic material does not have the function of increasing magnetic permeability and suppressing eddy current loss through "electrical insulation and magnetic coupling". However, when the resin contains a segment having a solubility parameter (also referred to as SP (Solubility Parameter) value) of 10 or more and 15 or less, the high frequency composite magnetic material (hereinafter referred to as "magnetic powder") existing as a powder constituting the high frequency resin composite magnetic material of the present invention is isolated and dispersed, and the connection between the magnetic powder particles is broken by the resin, which is an insulator. Therefore, although it is difficult to realize a real term of extremely high magnetic permeability, eddy current loss can be suppressed over frequencies in the high frequency range (especially the ultra-high frequency range). Therefore, when the high frequency resin composite magnetic material of the present invention is applied as a high frequency amplification material such as a core of a coil for a wireless power supply system of 0.001 GHz or more and 0.1 GHz or less, eddy current loss can be extremely reduced, and further, when the high frequency resin composite magnetic material of the present invention is applied as an electromagnetic wave absorbing material or electromagnetic noise absorbing material used in the ultra-high frequency range exceeding 1 GHz, the maximum absorption frequency (f a ) to increase the maximum absorbed energy coefficient (fμ” max) is prevented from being reduced by eddy currents. The reason for this is expected to be that the resin segments with a high solubility parameter have a high affinity with the rare earth-iron-M-nitrogen powder, so they bond strongly to the interface, separating the magnetic powder particles and isolating them. Here, the "solubility parameter" is a measure of intermolecular forces, and the closer the SP values of two substances are, the greater the affinity. Theoretically, it is calculated from the heat of vaporization of a unit volume of liquid, so it is only defined for solvents with a melting point, but the solubility parameter of a resin is also determined based on the solubility in a solvent with a known SP value. Even for resins without literature values, if the structure is known, the SP value can be calculated based on Fedors' estimation method, and by rounding off to one decimal place, it can be determined whether the resin is effective for the present invention.
[0047] Examples of resin segments having a solubility parameter (SP) of 10 or more and 15 or less include thermoplastic resins such as polyamide (SP value of 13 or more and 14 or less), ester (SP value of 10 or more and 11 or less), and polyurethane (SP value of 10), and thermosetting resins such as epoxy resin (SP value of 10 or more and 11 or less). Segments with low SP values such as polyether (SP value of 9), silicone rubber (SP value of 7 or more and 8 or less), and fluorine rubber (SP value of 7 or more and 8 or less) may be contained by copolymerization or the like. In this case, when the resin is contained in the high-frequency resin composite magnetic material of the present invention, the flexibility of the resin composite magnetic material is imparted, making it suitable for electromagnetic noise absorbing material applications requiring elastomer functions. Among them, when a polyamide ester ether elastomer obtained by copolymerizing a polyamide with an SP value of 13.6 and a polyether with an SP value of 9.0 is used as a resin component, the resin composite magnetic material has excellent surface smoothness, achieves isolated dispersion, has a high imaginary term value of magnetic permeability in the ultra-high frequency range, and is excellent in flexibility and impact resistance. This is believed to be due to the fact that in addition to polyamide and polyether, the material contains ester bonds, and segments with a variety of compatibility parameters. This is because the ester bonds are thought to play a role in smoothly connecting the polyamide components that bond to the surface of the rare earth-iron-M-nitrogen magnetic material and the polyether components that are between the powder and impart flexibility. Furthermore, if the solubility parameter (SP) of the segment is set to 13 or more and 14 or less, further improvement in magnetic permeability is observed, and the value of the imaginary term of the complex relative magnetic permeability in the ultra-high frequency range can be brought into the practical range when the volume fraction of the rare earth-iron-Mn-nitrogen magnetic powder is within the wide range of 30 volume % or more and 80 volume % or less. As described above, when a resin with an adjusted solubility parameter (SP) is used in the high-frequency resin composite magnetic material of the present invention, the chemical properties of the surface come into play, and from this point of view, it is better not to completely cover the resin with ferrite material.
[0048] Next, a method for producing the high frequency magnetic material of the present invention will be described, but the method is not particularly limited thereto. The method for producing a high frequency magnetic material of the present invention also includes a method for producing a high frequency composite magnetic material and a high frequency resin composite magnetic material. Regarding the production method, a specific example will be given of a method for obtaining the "high frequency composite magnetic material" of the present invention. In the description of the present invention in this application, "an alloy substantially consisting of an R component, an Fe component, and an M component" refers to an alloy mainly composed of an R component, an Fe component, and an M component (i.e., the total of the R component, the Fe component, and the M component accounts for 50 atomic % or more of the alloy), but the Fe in the Fe component may be replaced with an atom of Co or Ni. In this application, this alloy is also referred to as a "rare earth-iron-M alloy," "raw alloy," or "master alloy." In addition, a "rare earth-iron-M alloy" is also referred to as an "R-Fe-M alloy."
[0049] (1) Preparation of master alloy Methods for producing R-Fe-M alloys include: (I) high-frequency melting, in which the R, Fe, and M metal components are melted by high-frequency waves and cast into a mold; (II) arc melting (also called the arc button method), in which the metal components are placed in a copper boat or other vessel and melted by arc discharge; (III) drop casting or suction casting, in which the arc-melted molten metal is dropped into a water-cooled mold in one go and quenched; (IV) ultra-rapid cooling, in which high-frequency melted molten metal is dropped onto a rotating copper roll to obtain a ribbon-like alloy; (V) gas atomization, in which high-frequency melted molten metal is atomized with gas to obtain alloy powder; and (VI) powder of the Fe and / or M components or Fe-M alloy powder. (VII) a mechanical alloying method in which each metal component and / or alloy is reacted while being finely pulverized by a ball mill or the like, and (VIII) an HDDR (Hydrogenation Decomposition Desorption Recombination) method in which an alloy obtained by any of the above methods is heated in a hydrogen atmosphere to decompose the R and / or M component hydrides and the Fe and / or M component or the Fe-M alloy, and then the mixture is recombined and alloyed under high temperature and low pressure while hydrogen is expelled.
[0050] When using the high-frequency melting method or the arc melting method, Fe-based components are likely to precipitate when the alloy solidifies from the molten state, and the volume fraction of components with maximum absorption frequencies in the low frequency region increases even after the nitriding process, causing a decrease in absorption in the high frequency and even ultra-high frequency regions. Therefore, in order to eliminate the Fe-based components and increase the crystal structure of tetragonal, rhombohedral, or hexagonal (particularly tetragonal), it is effective to anneal in a gas containing at least one of inert gases such as argon and helium, and hydrogen gas, or in a vacuum at a temperature range of 200°C to 1300°C, preferably 600°C to 1185°C. The alloy produced by this method has a larger crystal grain size, better crystallinity, and high magnetic permeability than those produced by the super-quenching method. Therefore, this alloy contains a large amount of homogeneous main raw material phase, and is preferable as a master alloy for obtaining the magnetic material of the present invention. On the other hand, the super-quenching method and the mechanical alloying method are not suitable for use as a master alloy for obtaining the magnetic material of the present invention. law The master alloy obtained by the method has a fine metal structure, so it can be homogenized by annealing for a short time, which is an advantage. The suction casting method and the drop casting method are examples of alloy manufacturing methods that take advantage of the advantages of both methods. The alloy melting method is the same as the arc melting method, but the cooling rate is faster than the normal arc button method, so the phase separation is fine and the annealing time is generally short.
[0051] (2) Coarse grinding and classification process Although it is possible to directly nitride the alloy ingot, R / D method or HDDR method alloy powder produced by the above method, if the crystal grain size is larger than 2000 μm, the nitriding time will be long, and it is more efficient to perform coarse crushing before nitriding. Coarse crushing to 200 μm or less is particularly preferable because it further improves the nitriding efficiency. Coarse pulverization is carried out using a jaw crusher, hammer, stamp mill, rotor mill, pin mill, cutter mill, etc. In addition, even if a pulverizer such as a ball mill or jet mill is used, it is possible to prepare alloy powder suitable for nitriding depending on the conditions. A method of absorbing hydrogen into the master alloy and then pulverizing it with the above-mentioned pulverizer, or a method of repeatedly absorbing and releasing hydrogen to pulverize the alloy may also be used. Furthermore, after coarse grinding, adjusting the particle size using a classifier such as a sieve, a vibration or sonic classifier, an air sieve, or a cyclone is also effective for more uniform nitriding. After coarse grinding and classification, annealing in an inert gas or hydrogen can remove structural defects, which can be effective in some cases. The above examples show how to prepare the powder or ingot raw material of the R-Fe-M alloy in the manufacturing method of the present invention, but the optimal conditions for nitriding shown below vary depending on the crystal grain size, crushed grain size, surface condition, etc. of these raw materials.
[0052] (3) Nitriding and annealing process Nitridation is a process in which a gas containing a nitrogen source, such as ammonia gas or nitrogen gas, is brought into contact with the R-Fe-M alloy powder or ingot obtained in the above step (1) (preparation of master alloy) or step (1) (preparation of master alloy) and step (2) (crushing and classification) to introduce nitrogen into the crystal structure. In this case, it is preferable to have hydrogen coexist in the nitriding atmosphere gas, since this not only increases the nitriding efficiency but also allows the nitriding to occur while maintaining a stable crystal structure. In addition, in order to control the reaction, inert gases such as argon, helium, and neon may also be coexisted. The most preferable nitriding atmosphere is a mixed gas of ammonia and hydrogen. When the total pressure of ammonia and hydrogen combined is near normal pressure (1 atm), the ammonia partial pressure is particularly controlled to be in the range of 0.1 atm to 0.7 atm, and when the total pressure of ammonia and hydrogen combined is outside normal pressure, the ammonia mole fraction is controlled to be in the range of 0.1 atm to 0.7 atm, which not only increases the nitriding efficiency but also reduces the crystal structure of the rare earth-iron-M-nitrogen magnetic material used in the present invention (specifically, the rare earth-iron-M-nitrogen magnetic material). x Fe (100-x-y-z) M y N zIn the formula, R is at least one element selected from Y, Ce, Pr, Nd, Gd, Tb, Dy, Ho, Er, Tm, Lu, and Sm, Fe is an iron element, M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, N is a nitrogen element, and x, y, and z satisfy 2 atomic %≦x≦15 atomic %, 0.5≦y≦25 atomic %, and 3≦z≦50 atomic %.) a magnetic material that covers the entire nitrogen content range can be produced. The nitriding reaction can be controlled by the gas composition, heating temperature, heat treatment time, and pressure. The heating temperature varies depending on the mother alloy composition and the nitriding atmosphere, but is preferably selected in the range of 100°C to 600°C. A temperature of 100°C or higher is preferable in order to avoid the problem that the nitriding rate is very slow when the temperature is lower than that temperature, and a temperature of 600°C or lower is preferable in order to avoid the problem that the main raw material phase decomposes into nitrides of rare earth nitride, iron nitride, and M component when the temperature is higher than that temperature, and it is not possible to nitride while maintaining at least one crystal structure selected from tetragonal, hexagonal, rhombohedral, and amorphous (particularly, tetragonal or amorphous). In order to increase the nitriding efficiency and the content of the main phase, a more preferable temperature range is 250°C to 500°C. Furthermore, when a tetragonal rare earth-iron-M-nitrogen magnetic material is produced by nitriding, a temperature range of 100°C to 500°C in an ammonia-hydrogen atmosphere is suitable, and when an amorphous rare earth-iron-M-nitrogen magnetic material is produced by nitriding amorphization regardless of the crystal structure of the raw material alloy, a temperature range of 250°C to 600°C in an ammonia-hydrogen atmosphere is suitable. In particular, when an amorphous rare earth-iron-M-nitrogen magnetic material is produced by nitriding amorphization using a tetragonal raw material alloy, a temperature range of 250°C to 500°C is suitable. In addition, annealing in an inert gas and / or hydrogen gas after nitriding is preferable in terms of improving magnetic properties. In particular, manufacturing an R-Fe-MN magnetic material in the high nitriding region with a nitrogen content of 7 atomic % to 30 atomic % and then annealing in an atmosphere containing hydrogen gas is a very preferable method in terms of increasing the magnetic permeability and magnetization by improving the crystallinity and homogeneity of the nitrogen-containing magnetic material. The nitriding and annealing apparatus may be a horizontal or vertical tubular furnace, a rotary reactor, a closed reactor, etc. Although the magnetic material of the present invention can be prepared in any apparatus, it is preferable to use a rotary reactor in order to obtain powder having a uniform nitrogen composition distribution. The gas used in the reaction is supplied by an airflow method in which an airflow of 1 atmosphere (atm) or more is sent to the reactor while keeping the gas composition constant, a sealing method in which the gas is sealed in a container at a pressure in the range of 0.01 atmosphere (atm) to 70 atmospheres (atm), or a combination of these. The R-Fe-MN magnetic material is produced only after going through the above steps, from step (1) (preparation of the master alloy) to the main step (3) "nitriding and annealing step." It is also possible to prepare an R-Fe-MNH magnetic material by carrying out the main step (3) using a gas that serves as a hydrogen source.
[0053] (4) Fine grinding process The fine pulverization process is a process carried out for the purpose of pulverizing the R-Fe-MN magnetic material or R-Fe-MNH magnetic material into finer powder, or for the purpose of introducing O and H components into the R-Fe-MN magnetic material in order to obtain an R-Fe-MNHO magnetic material. As the method of fine pulverization, in addition to the methods mentioned in the above step (2) (coarse pulverization and classification step), dry or wet fine pulverization equipment such as a rotary ball mill, a vibration ball mill, a planetary ball mill, a wet mill, a jet mill, a cutter mill, a pin mill, an automatic mortar, or a combination thereof can be used. When introducing O and H components, the amount of the components introduced can be adjusted to within the range of the present invention by controlling the moisture content or oxygen concentration in the fine pulverization atmosphere. As a method for producing the rare earth-iron-M-nitrogen magnetic material of the present invention, it is preferable to prepare a mother alloy of R-Fe-M composition by the method exemplified in step (1) (preparation of mother alloy), or by the method exemplified in step (1) (preparation of mother alloy) and step (2) (crude grinding and classification), then nitride it by the method shown in step (3) (nitriding and annealing), and finely grind it by the method shown in step (4). In particular, the raw alloy obtained in step (1) (preparation of mother alloy) or the raw alloy obtained by grinding and classifying it by the method shown in step (2) (crude grinding and classification) is heat-treated at 600°C to 1300°C in an atmosphere containing at least one of inert gas and hydrogen gas, and then annealed by heat-treating it at 100°C to 600°C in an atmosphere containing ammonia gas, and then nitriding it, thereby obtaining a magnetic material with extremely small deterioration of magnetic properties due to oxidation inside the powder.
[0054] (5) Ceramic material mixing process This step is a step of mixing a ceramic material with the rare earth-iron-M-nitrogen magnetic material obtained in step (3) (nitriding and annealing step) or step (4) (fine grinding step). A typical mixer such as a V-type mixer, tumbler, vibration mixer, shaker, drum mixer, rocking mixer, shaker, or rotary mixer, or the above-mentioned pulverizer or classifier can be used. In addition, this step (5) can be performed simultaneously with steps (1) to (3). In the present invention, the use of nanoceramic powder as the ceramic material not only makes mixing more efficient, but also leads to improved electromagnetic properties.
[0055] (6) Orientation and molding process The high frequency magnetic material of the present invention can be used for various applications by blending (mixing) a specified rare earth-iron-M-nitrogen magnetic material with other magnetic materials, ceramic materials, and / or resins and molding the material. Among them, blending the above-mentioned resins results in the high frequency resin composite magnetic material of the present invention. In addition, when the high frequency magnetic material of the present invention is an anisotropic material, performing a magnetic field orientation operation at least once in this molding process will result in a magnetic material or resin composite magnetic material with high magnetic properties, and therefore this magnetic field orientation operation is particularly recommended. The method of solidifying the high-frequency composite magnetic material of the present invention obtained by compounding (mixing) a predetermined rare earth-iron-M-nitrogen-based magnetic material with other magnetic materials, ceramic materials, and / or resins and molding the material may be to put the material into a mold, cold-press the material, and use the material as is, or to subsequently mold the material by cold rolling, forging, shock wave compression molding, or the like. In many cases, the material may be molded by sintering the material while heat treating the material at a temperature of 50°C or higher. The heat treatment atmosphere is preferably a non-oxidizing atmosphere, and the heat treatment may be performed in an inert gas such as a rare gas such as argon or helium, or in nitrogen gas, or in a reducing gas containing hydrogen gas. The heat treatment may be performed in the air at a temperature of 500°C or lower. Sintering may also be performed at normal pressure or under pressure, or in a vacuum.
[0056] This heat treatment can be performed simultaneously with the powder compaction, and the magnetic material of the present invention can be formed by pressure sintering methods such as hot pressing, HIP (hot isostatic pressing), and SPS (spark plasma sintering). In order to make the pressure effect of the present invention prominent, it is preferable to set the pressure in the heating and sintering step within the range of 0.0001 GPa to 10 GPa. If the pressure is less than this pressure, the effect of the pressure is poor and there is no difference in the electromagnetic properties from normal pressure sintering, so it is preferable to set the pressure to 0.0001 GPa or more in order to avoid the problem that pressure sintering is disadvantageous in terms of reduced productivity. In addition, it is preferable to set the pressure to 10 GPa or less in order to avoid the problem that if the pressure exceeds this pressure, the pressure effect is saturated and even if the pressure is increased further, the productivity will only decrease. In addition, a large pressure may impart induced magnetic anisotropy to the magnetic material, deteriorating the inherent magnetic properties such as high magnetic permeability, or causing the maximum absorption frequency to deviate from the preferred range. Therefore, the preferred range of pressure is 0.001 GPa to 1 GPa, and more preferably 0.01 GPa to 0.1 GPa.
[0057] Furthermore, in many of the above methods, solidification may be accompanied by some decomposition of the surface of the magnetic material, but among the shock wave compression methods, the well-known underwater shock wave compression method is advantageous as a method that can mold the magnetic material without decomposing it.
[0058] When the powder of rare earth-iron-M-nitrogen magnetic material and / or the powder of composite magnetic material obtained in the above step (3) (nitriding and annealing step), or step (3) (nitriding and annealing step) → step (4) (fine grinding step), or step (3) (nitriding and annealing step) → step (5) (ceramic material mixing step), or step (3) (nitriding and annealing step) → step (4) (fine grinding step) → step (5) (ceramic material mixing step) is applied to a high-frequency resin composite magnetic material, it is mixed with a thermosetting resin or a thermoplastic resin and then compression molded, or kneaded with a thermoplastic resin and then injection molded, or if necessary, further molded by extrusion molding, roll molding, and / or calendar molding. In the above mixing, a casting method in which a resin dissolved in a solvent is mixed with the magnetic powder and then the solvent is removed by vaporization or the like is also effective. For the above kneading, it is also effective to use a kneader or a single-screw or twin-screw extruder.
[0059] For example, when applied to an electromagnetic noise absorbing sheet, the types of sheet shapes include batch-type sheets formed by compression molding with a thickness of 5 μm to 10,000 μm, a width of 5 mm to 5,000 mm, and a length of 0.005 m to 1,000 m, and roll-shaped sheets formed by roll molding or calendar molding. When molding using the above method, if part or all of the process is carried out in a magnetic field, the magnetic particles are magnetically oriented, which may improve the magnetic properties. There are three main types of magnetic field orientation: uniaxial magnetic field orientation, rotating magnetic field orientation, and opposing magnetic pole orientation.
[0060] Uniaxial magnetic field orientation means that a static magnetic field is applied from the outside in any direction to a magnetic material or a composite magnetic material that is in a movable state, and the easy magnetization direction of the magnetic material is aligned to the direction of the external static magnetic field. After this, pressure is usually applied or the resin component is solidified to produce a uniaxial magnetic field oriented molded product. Rotating magnetic field orientation is a method in which a magnetic material or a composite magnetic material that is in a movable state is placed in an external magnetic field that usually rotates in one plane, and the magnetization hardness direction of the magnetic material is aligned in one direction. The rotation method includes a method of rotating the external magnetic field, a method of rotating the magnetic material in a static magnetic field, a method of applying a magnetic field at any time in a sequence in which the strength of multiple magnetic poles is synchronized and changed so that the magnetic material feels as if the magnetic field is rotating, and even a combination of the above methods. In extrusion molding and roll molding, a method in which two or more magnetic poles are arranged in the extrusion direction, the strength or polarity of the magnetic field is changed, and the composite magnetic material or resin composite magnetic material is arranged and oriented so that it feels the rotating magnetic field when it passes through is also a rotating magnetic field orientation in a broad sense.
[0061] Opposite magnetic pole orientation is a method of placing a magnetic material or a composite magnetic material in an environment where magnetic poles of the same polarity are facing each other, or moving it in a rotational or translational motion, or a combination of these, to align the direction of hard magnetization in one direction. Uniaxial magnetic field orientation of a magnetic material or composite magnetic material with in-plane magnetic anisotropy improves the magnetic permeability by 1% to 50%, while rotational magnetic field orientation or opposing magnetic pole orientation improves the magnetic permeability by 1% to 200%. In order to sufficiently orient the magnetic material, the magnetic field molding is carried out in a magnetic field of preferably 8 kA / m or more, more preferably 80 kA / m or more, and most preferably 400 kA / m or more. The strength and time of the magnetic field required for magnetic field orientation are determined by the shape of the magnetic material powder, and in the case of a resin composite magnetic material, the viscosity of the matrix and the affinity with the magnetic material powder.
[0062] Generally, the stronger the magnetic field used, the shorter the orientation time, so for magnetic field orientation in roll molding or calendar molding, where the molding time is short and the viscosity of the matrix resin is high, it is desirable to use a magnetic field of 400 kA / m or more. EXAMPLES
[0063] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. For example, the present invention discloses in detail the electromagnetic properties in the range of 0.001 GHz to 3 GHz in the examples, and demonstrates that the magnetic material of the present invention has excellent "target functions," but the use of the material of the present invention is not limited to this range.
[0064] [Examples 1 and 2 and Comparative Example 1] The ingots produced by the suction casting method were annealed at 1000°C for 2 hours to produce Sm as a raw material for rare earth-iron-M alloys. 7.7 Fe 84.6 Ti 7.7 A raw material alloy having the following composition was prepared. This raw alloy was further crushed in a cutter mill in an argon atmosphere, and then crushed into Sm alloys with an average particle size of about 60 μm. 7.7 Fe 84.6 Ti 7.7 A raw alloy powder (Comparative Example 1) was obtained. This raw alloy powder was charged into a horizontal tubular furnace and heat-treated at 390°C for 30 minutes in a mixed gas flow with an ammonia partial pressure of 0.33 atm and a hydrogen gas partial pressure of 0.67 atm. 6.4 Fe 70.5 Ti 6.4 N 16.7A magnetic powder (Example 1) having the composition was prepared. The magnetic material of this powder was analyzed by X-ray diffraction (Co-Kα radiation source), and diffraction lines indicating tetragonal crystals were observed as shown in FIG. 1. The X-ray diffraction diagram of the raw alloy (Comparative Example 1) before nitriding is also shown in FIG. 1, and diffraction lines indicating tetragonal crystals were observed as in Example 1. However, each diffraction line was shifted to a lower angle by nitriding, and nitrogen was inserted between the lattices, which resulted in the formation of ThMn 12 It was found that the tetragonal crystal lattice of the structure expands, increasing the lattice volume. The powder of the rare earth-iron-Mn-nitrogen magnetic material of Example 1 (specifically, Sm 6.4 Fe 70.5 Ti 6.4 N 16.7 The magnetization value of the magnetic material of this composition was 112 emu / g, and the magnetic anisotropy field was 4.32 T. This magnetic material also had in-plane magnetic anisotropy. From this result, it was found that the rare earth-iron-Mn-nitrogen based magnetic material obtained in Example 1 can be used as a high frequency magnetic material. Next, the powder of the rare earth-iron-Mn-nitrogen magnetic material obtained above (specifically, the Sm 6.4 Fe 70.5 Ti 6.4 N 16.7 A powder of a magnetic material having the composition (a powder of a magnetic material having the composition) was finely pulverized in a ball mill for 4 hours to produce a powder of a Sm-Fe-Ti-N magnetic material having an average particle size of about 4 μm (Example 2). This was mixed with 8 mass% of an epoxy resin having a solubility parameter value of 11 and kneaded, and cured overnight at 50°C to produce a toroidal resin composite magnetic material having an inner diameter of 3.1 mm, an outer diameter of 8 mm, and a thickness of 1 mm. The density of the produced resin composite magnetic material was 4.9 g / cm 3 The volume fraction of the magnetic material was 62% by volume. The rare earth-iron-Mn-nitrogen magnetic powder of Example 2 (specifically, the Sm 6.4 Fe 70.5 Ti 6.4 N 16.7The frequency change of the relative permeability (μ) of a resin composite magnetic material using magnetic powder (finely pulverized in a ball mill) is shown in Figure 2. From Figure 2, the value of the real term (μ') of the relative permeability (μ) in the range of 0.001 GHz to 0.1 GHz is almost constant within the range of 2.9 to 2.7, and the complex relative permeability (μ r The imaginary term (μ") of the complex permeability at 3 GHz is small, ranging from 0 to 0.6, and it has been confirmed that the material can be used as a high-frequency amplification material in this range. r ) have values of 1.3 and 0.4, respectively, and the maximum absorbed energy coefficient at that frequency reaches 13 GHz. Therefore, it is found to be a high-frequency composite magnetic material suitable as an electromagnetic noise absorbing material in the ultra-high frequency region around 3 GHz. Furthermore, by extrapolating the frequency change of the relative permeability in Figure 2 to the high frequency side, it is found to be suitable as an electromagnetic noise absorbing material even above 3 GHz. The volume resistivity of this toroid is 10 7 The magnetic resistance was found to be extremely good at insulating and dispersing isolated regions, making it a suitable resin composite magnetic material for high frequencies. In addition, the Sm before nitriding 7.7 Fe 84.6 Ti 7.7 The raw alloy powder having the composition (Comparative Example 1) was processed in the same manner as in Example 2 to prepare a toroidal specimen (density 4.9 g / cm 31 also shows the results of measuring the frequency change of the relative permeability (μ) when the volume fraction of the magnetic powder is 58% by volume. The real term (μ') of the relative permeability (μ) in the range of 0.001 GHz to 0.1 GHz is almost constant at 1.2, and the imaginary term (μ") is almost constant at 0. It is not significantly different from the permeability of a vacuum, and shows a permeability change specific to uniaxial magnetic anisotropy materials. In the frequency range from 0.001 GHz to 3 GHz, the magnetic field is hardly amplified (μ' times) and electromagnetic noise is not absorbed (the amount of absorbed energy is proportional to μ"), so it was found that it is not suitable as a high-frequency magnetic material. Note that the magnetic material of Comparative Example 1 was found to exhibit uniaxial magnetic anisotropy by the magnetic field orientation experiment, but in Example 2, when considered together with the results of the X-ray diffraction method, it was revealed that the magnetic anisotropy changes dramatically from uniaxial to in-plane as nitrogen penetrates between the lattices of the tetragonal crystal structure, and the high-frequency characteristics are also dramatically improved. Thus, it was found that the rare earth-iron-M-nitrogen based resin composite magnetic material obtained in Example 2 can be used as a high frequency magnetic material.
[0065] [Example 3] In the same manner as in Example 1, Sm 7.2 Fe 72.4 V 14.5 N 5.9 A rare earth-iron-Mn-nitrogen magnetic material powder (Example 3) was produced. The powder rare earth-iron-Mn-nitrogen magnetic material (specifically, the powder of Example 3) 7.2 Fe 72.4 V 14.5 N 5.9 The magnetization value of the resin composite magnetic material (based magnetic material) was 132 emu / g and the magnetic anisotropy field was 7.25 T. This magnetic material also had in-plane magnetic anisotropy. This powder was not finely pulverized. 8% by mass of epoxy resin with a solubility parameter value of 11 was mixed and kneaded, and cured overnight at 50°C to produce a toroidal resin composite magnetic material with an inner diameter of 3.1 mm, an outer diameter of 8 mm, and a thickness of 1 mm. The density of the produced resin composite magnetic material was 5.0 g / cm 3 The volume fraction of the magnetic material was 61% by volume. The frequency change of the relative permeability (μ) of the rare earth-iron-Mn-nitrogen based resin composite magnetic material obtained in this example is as shown in FIG. 3. In the range of 0.001 GHz to 0.1 GHz, the value of the real term (μ') of the relative permeability (μ) is almost constant, ranging from 5.0 to 3.8, and the complex relative permeability (μ r The imaginary term (μ”) of the lattice constant was small, ranging from 0 to 1.4, indicating that the material can be used as a high-frequency amplifier in this region. In addition, the maximum absorbed energy coefficient was 3.9 GHz at a frequency of 3 GHz. Therefore, it was found that this is a high-frequency composite magnetic material suitable as an electromagnetic noise absorbing material in the ultra-high frequency region around 3 GHz, and further, by extrapolating the frequency change of the relative permeability in Figure 3 to the high frequency side, it was found that it is also suitable as an electromagnetic noise absorbing material even at frequencies above 3 GHz. Thus, it was found that the rare earth-iron-M-nitrogen based resin composite magnetic material obtained in Example 3 can be used as a high frequency magnetic material.
[0066] [Example 4 and Comparative Example 2] The ingots produced by the suction casting method were annealed at 1000°C for 2 hours to obtain Ce as a raw material for rare earth-iron-M alloys. 7.7 Fe 84.6 Ti 7.7 A raw alloy with the composition was prepared. SEM (scanning electron microscope) photographs of the cross section of the raw alloy before and after annealing are shown in Figure 4. Because the suction casting method was used, the phase separation immediately after casting (Figure 4A, before annealing) was small, and a homogeneous raw alloy (Figure 4B, after annealing) was produced by annealing at 1000°C for 2 hours. Note that the black area in Figure 4 is the Fe-Ti alloy phase with a bcc structure that has a cubic crystal structure, and the gray area is the ThMn alloy phase with a tetragonal crystal structure. 12 Structure of CeFe 11 Ti alloy phase. The white area is Th2Zn with a rhombohedral crystal structure. 17 Structure of CeFe 17 A combined analysis using SEM and EDX revealed that the phase was a Ce-rich phase, such as an alloy phase. The raw alloy was pulverized in an argon atmosphere using a cutter mill to obtain Ce with an average particle size of 60 μm. 7.7 Fe 84.6 Ti 7.7A raw alloy powder (Comparative Example 2) was obtained. This raw alloy powder was charged into a horizontal tubular furnace and heat-treated at 390° C. for 30 minutes in a mixed gas flow with an ammonia partial pressure of 0.33 atm and a hydrogen gas partial pressure of 0.67 atm to obtain Ce with an average particle size of 40 μm. 5.3 Fe 58.2 Ti 5.3 N 31.2 A magnetic powder having the composition of Example 4 was prepared. The rare earth-iron-M-nitrogen magnetic material (specifically, Ce 5.3 Fe 58.2 Ti 5.3 N 31.2 The magnetization value of the magnetic material of the composition was 104 emu / g, and the material was magnetically isotropic. The results of analyzing the magnetic powders of Comparative Example 2 and Example 4 by X-ray diffraction (Co-Kα radiation source) are shown in Figure 5. It was found from this figure that the raw material powder of the comparative example had a tetragonal crystal structure. It was also revealed that the magnetic powder of Example 4 had become homogeneously amorphous, with the tetragonal crystal structure of the raw material being destroyed by amorphization through nitriding. From this result, it was found that the rare earth-iron-Mn-nitrogen based magnetic material obtained in Example 4 can be used as the high frequency magnetic material of the present invention. Next, 8% by mass of epoxy resin with a solubility parameter value of 11 was mixed and kneaded into this rare earth-iron-Mn-nitrogen magnetic material, and cured overnight at 50°C to produce a toroidal resin composite magnetic material with an inner diameter of 3.1 mm, an outer diameter of 8 mm, and a thickness of 1 mm. The density of the produced resin composite magnetic material was 5.4 g / cm. 3 The volume fraction of the magnetic material was 66% by volume. The frequency change of the relative permeability (μ) of the rare earth-iron-magnesium-nitrogen based resin composite magnetic material obtained in this example is shown in FIG. 6. The real term (μ') of the relative permeability (μ) in the range of 0.001 GHz to 0.03 GHz was an extremely high value of 13.2. r The value of the imaginary term (μ") of the complex permeability (μ) at 0.001 GHz to 0.005 GHz was almost 0. Therefore, it was found that it can be used as a magnetic field amplification material in this region. r ) was 5.7, indicating that the material can be used as an electromagnetic noise absorbing material in this range. Ce before nitridation 7.7 Fe 84.6 Ti 7.7 A raw alloy having the composition (Comparative Example 2) was prepared in the same manner as in Example 4, and a toroidal specimen (density 5.0 g / cm 3 The magnetic powder volume fraction was adjusted to 59% by volume. The frequency change of the relative permeability (μ) is also shown in FIG. 6. The real term (μ') of the relative permeability (μ) of Comparative Example 1 in the frequency range of 0.001 GHz to 0.03 GHz was in the range of approximately 2.8 to 1.9, which was a lower value than that of Example 4. Furthermore, the imaginary term (μ") of the relative permeability (μ) of Comparative Example 1 in the frequency range of 0.001 to 0.003 GHz was in the range of 1 to 0.5, which was found to be too lossy to be used as a magnetic field amplification material compared to Example 4 and therefore unable to be used as a high frequency amplification material. In this way, it was found that the rare earth-iron-M-nitrogen based resin composite magnetic material obtained in Example 4 can also be used as a high frequency magnetic material. [Industrial Applicability]
[0067] The present invention relates to magnetic materials used in magnetic field-mediated sensors such as transformers, heads, inductors, reactors, yokes, and cores (magnetic cores) used in high frequency regions, which are mainly used in power equipment and information and communication-related equipment; antennas, microwave elements, magnetostrictive elements, magnetoacoustic elements, and magnetic recording elements; Hall elements, magnetic sensors, current sensors, rotation sensors, and electronic compasses; among others, coil cores and antenna cores used in wireless power supply (also called wireless power transmission or contactless power transmission) systems; magnetic materials for suppressing interference caused by unnecessary electromagnetic interference, such as electromagnetic noise absorbing materials, electromagnetic wave absorbing materials, and magnetic shielding materials; materials for inductor elements such as noise removing inductors; and magnetic materials for removing noise from signals in the high frequency region, such as materials for RFID (Radio Frequency Identification) tags and noise filter materials.
Claims
1. A high-frequency magnetic material having a composition of a main phase represented by the general formula shown in Formula 1 below, and used in a frequency range of 0.001 GHz to 100 GHz. R x Fe (100-x-y-z) M y N z (Formula 1) (R is at least one element selected from the group consisting of rare earth elements including Y, Fe is an iron element, M is at least one element selected from the group consisting of Ti, V, Mo, Nb, W, Si, Al, Mn, and Cr, N is a nitrogen element, and x, y, and z satisfy 2 atomic %≦x≦15 atomic %, 0.5 atomic %≦y≦25 atomic %, and 3 atomic %≦z≦50 atomic %).
2. 2. The high frequency magnetic material according to claim 1, wherein 50 atomic % or less of Fe in said formula 1 is substituted with Co or Ni element.
3. 3. The high frequency magnetic material according to claim 1, wherein R in formula 1 contains 50 atomic % or more of Sm element.
4. 4. The high frequency magnetic material according to claim 1, wherein the crystal structure of the main phase is a tetragonal system.
5. 5. The high frequency magnetic material according to claim 1, wherein the crystal magnetic anisotropy is an in-plane magnetic anisotropy.
6. 3. The high frequency magnetic material according to claim 1, wherein the main phase has an amorphous crystal structure.
7. 7. The high frequency magnetic material according to claim 1, wherein less than 50 atomic % of N in the formula 1 is replaced with at least one element selected from the group consisting of H, C, P, Si and S.
8. 8. The high frequency magnetic material according to claim 1, which is a powder having an average particle size of 0.1 μm or more and 2000 μm or less.
9. The high frequency magnetic material according to any one of claims 1 to 8 is contained in an amount of 1 mass% to 99.999 mass%, at least one selected from the group consisting of metallic Fe, metallic Ni, metallic Co, an Fe—Ni based alloy, an Fe—Ni—Si based alloy, sendust, an Fe—Si—Al based alloy, an Fe—Cu—Nb—Si based alloy, an amorphous alloy, magnetite, Ni-ferrite, Zn-ferrite, an Mn—Zn ferrite, and an Ni—Zn ferrite, in an amount of 0.001% by mass or more and 99% by mass or less; High frequency magnetic material.
10. 10. The high frequency magnetic material according to claim 9, wherein the metallic Fe is carbonyl iron powder.
11. The high frequency magnetic material according to any one of claims 1 to 10 is contained in an amount of 1 mass% to 99.999 mass%. Contains a ceramic material in an amount of 0.001% by mass or more and 99% by mass or less; High frequency magnetic material.
12. The high frequency magnetic material according to any one of claims 1 to 11 is contained in an amount of 5 mass% to 99.9 mass%. Contains 0.1 to 95% by mass of resin; High frequency magnetic material.
13. 13. The high frequency magnetic material according to claim 12, wherein the resin contains a segment having a solubility parameter of 10 or more and 15 or less.
14. The high frequency magnetic material according to claim 1 , which is magnetically oriented.
15. 2. A method for producing the high frequency magnetic material according to claim 1, comprising heat treating an alloy mainly composed of R, Fe, and M as defined in formula 1 in a nitriding atmosphere containing ammonia gas at a temperature in the range of 100° C. to 600° C.
16. A method for producing the high frequency magnetic material according to claim 12, comprising kneading the high frequency magnetic material according to claim 1 produced by the production method according to claim 15 with a resin containing a segment having a solubility parameter of 10 or more and 15 or less, and subjecting the mixture to compression molding, injection molding, and / or calendar molding.
Citation Information
Patent Citations
Soft-magnetic material and its production
JP1991153851A
Ultra-microcrystalline alloy excellent in corrosion resistance
JP1992045247A
Production of nitrogen interstitial rare earth compound alloy
JP1994088169A
Magnetic material
JP1994235051A
Plated film and electromagnetic shielding material
JP2002194586A