Thermally conductive silicone composition
A thermally conductive silicone composition with tailored aluminum nitride and inorganic particles addresses the challenge of combining high thermal conductivity and slip resistance, enhancing heat dissipation and stability in semiconductor devices.
Patent Information
- Application Number
- JP2021172352
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-10-21
AI Technical Summary
Existing thermally conductive materials for semiconductor devices face challenges in achieving both high thermal conductivity and slip resistance, leading to inadequate heat dissipation and potential device damage due to slippage and fluidity issues.
A thermally conductive silicone composition comprising specific sizes and shapes of aluminum nitride particles and inorganic particles, along with organopolysiloxane components, to enhance thermal conductivity and slip resistance.
The composition achieves high thermal conductivity and improved slip resistance, ensuring effective heat dissipation and stability under thermal shock conditions.
Smart Images

Figure 0007577046000001 
Figure 0007577046000002 
Figure 0007577046000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermally conductive silicone composition. [Background technology]
[0002] It is widely known that semiconductor elements generate heat during use and the resulting decrease in performance, and various heat dissipation technologies are used as a means of solving this problem. In general, a cooling member (such as a heat sink) is placed near the heat-generating part, and the two are placed in close contact with each other, and heat is efficiently removed from the cooling member to dissipate heat. In this case, if there is a gap between the heat-generating part and the cooling member, the heat conductivity decreases due to the presence of air with low thermal conductivity, and the temperature of the heat-generating part does not decrease sufficiently. To prevent this phenomenon, heat-dissipating materials with good thermal conductivity and conformability to the surface of the part, such as heat-dissipating grease and heat-dissipating sheets, are used.
[0003] In recent years, the amount of heat generated by high-grade semiconductors, such as server CPUs and vehicle drive IGBTs, is increasing. As the amount of heat generated increases, the heat dissipation performance required for thermal grease and thermal sheets is also improving. Thermal grease is useful as a heat dissipation material for such semiconductor elements because of its low contact thermal resistance. However, when the viscosity of thermal grease is reduced to obtain good application performance, the thermal grease may slip off due to thermal shock of the element or external vibration, resulting in insufficient heat dissipation and potentially damaging the element.
[0004] Patent Document 1 proposes a high thermal conductivity grease that combines a metal oxide and a metal nitride to achieve both slippage resistance and application performance, but does not disclose anything with a thermal conductivity of 7.5 W / m·K or more, and the heat dissipation performance is insufficient.On the other hand, Patent Documents 2 and 3 blend insulating inorganic fillers in a specific ratio to improve the discharge performance of the heat dissipation grease, achieving low viscosity and high thermal conductivity of 7.5 W / m·K or more, but the high fluidity results in insufficient slippage resistance. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-063365 A [Patent Document 2] Patent No. 6246986 [Patent Document 3] International Publication No. 2020 / 262449 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in view of the above circumstances, and has as its object to provide a thermally conductive silicone composition that combines high thermal conductivity with resistance to misalignment. [Means for solving the problem]
[0007] In order to solve the above problems, the present invention provides a thermally conductive silicone composition, comprising: (C) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 4 μm or more and less than 50 μm; (D) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 50 μm or more and 150 μm or less; And, (E) Inorganic particles with an average particle size of 0.1 μm or more and less than 4.0 μm Contains the total amount of the (C) component and the (D) component is 20% by mass or more and less than 80% by mass of the total amount of the composition; The present invention provides a thermally conductive silicone composition in which the blending amount of the component (E) is 20% by mass or more and less than 50% by mass of the entire composition, and the ratio of the component (D) to the total amount of the component (C) and the component (D) is 5% by mass or more and less than 50% by mass.
[0008] This thermally conductive silicone composition combines high thermal conductivity with resistance to misalignment.
[0009] In the present invention, the component (C) is preferably rounded aluminum nitride particles.
[0010] Such component (C) can impart higher thermal conductivity to the thermally conductive silicone composition.
[0011] In the present invention, the component (C) is 150 parts by mass of the component (C) and has a kinematic viscosity of 1,000 mm at 25°C. 2 When a paste obtained by mixing 100 parts by mass of dimethylpolysiloxane of 1,000 parts by mass of dimethylpolysiloxane having a thickness of 300 μm is pressed at 25° C. and 0.1 MPa for 60 minutes, the thickness of the paste is preferably 10 μm to 100 μm.
[0012] Within this range, the viscosity of the thermally conductive silicone composition can be reduced, resulting in superior workability.
[0013] In the present invention, the component (E) is preferably at least one type selected from metal oxide particles and metal nitride particles.
[0014] Such inorganic particles provide the thermally conductive silicone composition with better thermal conductivity and resistance to misalignment.
[0015] In this case, the component (E) is preferably at least one selected from the group consisting of alumina particles, aluminum nitride particles, and zinc oxide particles.
[0016] Such inorganic particles provide the thermally conductive silicone composition with improved thermal conductivity and resistance to shear.
[0017] In this case, the component (E) is preferably amorphous zinc oxide particles.
[0018] Such inorganic particles provide the thermally conductive silicone composition with even better thermal conductivity and resistance to shearing.
[0019] In the present invention, further, (A) a kinetic viscosity at 25°C of 10 to 100,000 mm 2 It is preferable that the organopolysiloxane contains an organopolysiloxane having the formula:
[0020] If the viscosity of component (A) is within the specified range, bleeding out of the organopolysiloxane from the thermally conductive silicone composition is suppressed, and the thermally conductive silicone composition is more stretch It has excellent malleability.
[0021] In this case, the component (A) is preferably an organopolysiloxane having one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms in each molecule.
[0022] As the component (A) used in the present invention, the above-mentioned are preferred.
[0023] Also, at this time, (F) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in one molecule; (G) platinum group metal catalyst, And, (H) Reaction control agent It is preferable that the composition contains
[0024] By including such a component, an addition reaction type thermally conductive silicone composition can be obtained, and the resistance to misalignment can be improved.
[0025] In this case, it is preferable that the composition contains a hydrosilylation reaction product of the components (A) and (F).
[0026] By including such a component, it is possible to further improve the slippage resistance.
[0027] In the present invention, it is preferable that for each aliphatic unsaturated hydrocarbon group bonded to a silicon atom in one molecule of component (A), there are 4.0 to 20.0 hydrogen atoms bonded to silicon atoms in one molecule of component (F).
[0028] Within such a range, the thermally conductive silicone composition can have improved resistance to slippage.
[0029] In the present invention, it is preferable that the composition further contains (I) an organic peroxide.
[0030] By including this component (I), the thermally conductive silicone composition can have improved resistance to misalignment due to the radical reaction that occurs between components (A).
[0031] In the present invention, it is preferable that the composition further contains (B) a hydrolyzable organopolysiloxane containing an alkoxysilyl group.
[0032] This component can improve the fluidity when components (C), (D), and (E) are filled.
[0033] In this case, it is preferable that the composition further contains a condensation catalyst (J).
[0034] By including this component (J), the condensation reaction of component (B) can be carried out, thereby further improving the slippage resistance of the thermally conductive silicone composition. Effect of the Invention
[0035] According to the present invention, it is possible to obtain a thermally conductive silicone composition that has high thermal conductivity and excellent resistance to misalignment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] As described above, there has been a need for the development of a thermally conductive silicone composition that combines high thermal conductivity with resistance to misalignment.
[0037] As a result of extensive investigations conducted by the present inventors in order to achieve the above object, they discovered that a thermally conductive silicone composition containing aluminum nitride particles and inorganic particles having a specific particle size and shape has high thermal conductivity and excellent resistance to misalignment, and have completed the present invention.
[0038] That is, the present invention provides a thermally conductive silicone composition, (C) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 4 μm or more and less than 50 μm; (D) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 50 μm or more and 150 μm or less; And, (E) Inorganic particles with an average particle size of 0.1 μm or more and less than 4.0 μm Contains the total amount of the (C) component and the (D) component is 20% by mass or more and less than 80% by mass of the total amount of the composition; The amount of the component (E) blended is equal to or greater than 20% by mass and less than 50% by mass of the entire composition, and the proportion of the component (D) relative to the total amount of the component (C) and the component (D) is equal to or greater than 5% by mass and less than 50% by mass.
[0039] The present invention will be described in detail below, but the present invention is not limited thereto.
[0040] [Thermal conductive silicone composition] The thermally conductive silicone composition of the present invention contains (C) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral shapes having an average particle size of 4 μm or more and less than 50 μm, (D) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral shapes having an average particle size of 50 μm or more and 150 μm or less, and (E) inorganic particles having an average particle size of 0.1 μm or more and less than 4.0 μm, and the total amount of the (C) component and the (D) component is 20 mass% or more and less than 80 mass% of the entire composition, the blending amount of the (E) component is 20 mass% or more and less than 50 mass% of the entire composition, and the ratio of the (D) component to the total amount of the (C) component and the (D) component is 5 mass% or more and less than 50 mass%. In addition, the thermally conductive silicone composition of the present invention can contain the following components (A), (B), (F) to (J), and other components. Each component will be described below.
[0041] [(C) component] Component (C) is one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral shapes with an average particle size of 4 μm or more and less than 50 μm, preferably 4 μm or more and 30 μm or less. The shape of component (C) is preferably rounded, and the rounded shape referred to here means that the particles have few corners and are rounded and smooth, and does not include spherical shapes. The rounded shape is clearly different from the spherical shape in that it has corners. Spherical aluminum nitride is not preferred because it has poor thermal conductivity.
[0042] If the average particle size of component (C) is less than 4 μm, the thermal conductivity of the heat-conductive silicone will decrease, and if it is 50 μm or more, the resulting silicone composition may not be uniform. In the present invention, the average particle size is the cumulative average diameter D 50 (median diameter) and can be measured, for example, by Microtrac MT330OEX manufactured by Nikkiso Co., Ltd.
[0043] The aluminum nitride particles of component (C) and component (D) described below can be synthesized by known direct nitridation methods, reduction nitridation methods, etc., and can be adjusted to any particle size range by pulverization, etc. Also, rounded aluminum nitride particles can be obtained by heat treating amorphous or polyhedral aluminum nitride in a non-oxidizing atmosphere at 1,600°C to 2,000°C.
[0044] The component (C) is a mixture of 150 parts by mass of component (C) and a kinetic viscosity of 1,000mm at 25°C. 2 When a paste made by mixing 100 parts by mass of dimethylpolysiloxane having a molecular weight of 1000 / s is pressed at 25° C. and 0.1 MPa for 60 minutes, the thickness of the paste is preferably 10 μm or more and 100 μm or less, and more preferably 10 μm or more and 50 μm or less. If component (C) is within this range, the viscosity of the thermally conductive silicone composition can be reduced, further improving workability.
[0045] The component (C) may be used alone or in combination of two or more types.
[0046] [(D) component] Component (D) is one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 50 μm to 150 μm, preferably 60 μm to 120 μm, and more preferably 70 μm to 120 μm. Spherical aluminum nitride particles are not preferred because they have poor thermal conductivity.
[0047] If the average particle size of component (D) is less than 50 μm, the thermal conductivity of the resulting thermally conductive silicone composition will decrease, whereas if it exceeds 150 μm, the resulting thermally conductive silicone composition will tend to be non-uniform.
[0048] The component (D) may be used alone or in combination of two or more types.
[0049] The total amount of components (C) and (D) is 20% by mass or more and less than 80% by mass, preferably 50 to less than 80% by mass, based on the total amount of the composition. If the total amount of components (C) and (D) is less than 20% by mass, the thermal conductivity of the resulting thermally conductive silicone composition will decrease. If the total amount of components (C) and (D) is 80% by mass or more, the thermally conductive silicone composition will not be uniform.
[0050] Furthermore, the proportion of component (D) relative to the total amount of components (C) and (D) is from 5% to less than 50% by mass. If it is less than 5% by mass, the thermal conductivity of the thermally conductive silicone composition will be poor, and if it is 50% by mass or more, the slippage resistance of the thermally conductive silicone composition will be poor.
[0051] [(E) component] Component (E) is inorganic particles with an average particle size of 0.1 μm or more and less than 4.0 μm, preferably 0.4 μm or more and 2.0 μm or less. If the particle size is less than 0.1 μm, the viscosity of the thermally conductive silicone composition increases and handling becomes poor, while if the particle size is 4.0 μm or more, the thermally conductive silicone composition will not be uniform.
[0052] The inorganic particles are preferably metal oxide particles or metal nitride particles, specifically, aluminum oxide particles, aluminum nitride particles, zinc oxide particles, etc., and are preferably at least one selected from aluminum oxide particles, aluminum nitride particles, and zinc oxide particles, and are particularly preferably amorphous zinc oxide particles.
[0053] The blending amount of component (E) is from 20% to less than 50% by mass, and preferably from 25 to 40% by mass, of the entire thermally conductive silicone composition. If component (E) is less than 20% by mass, the thermally conductive silicone composition will not be homogeneous, and if it is 50% by mass or more, the viscosity of the thermally conductive silicone composition will increase, making it difficult to handle.
[0054] The component (E) may be used alone or in combination of two or more types.
[0055] [Component (A)] The thermally conductive silicone composition of the present invention further comprises: (A) a kinetic viscosity at 25°C of 10 to 100,000 mm 2 / s, preferably 30 to 10,000 mm 2 / s, and more preferably 100 to 8,000 mm 2 When the viscosity is within the specified range, bleeding out of the organopolysiloxane from the thermally conductive silicone composition is suppressed, and the thermally conductive silicone composition is more stretch In the present invention, the kinetic viscosity is a value measured at 25° C. using an Ostwald viscometer.
[0056] The molecular structure of the organopolysiloxane of component (A) is not particularly limited and may be linear, branched, cyclic, or the like. In particular, it is preferable for the main chain to be composed of repeating diorganosiloxane units, and for it to have a linear structure in which both ends of the molecular chain are blocked with triorganosiloxy groups. The organopolysiloxane may be used alone or in combination of two or more.
[0057] The organopolysiloxane can be represented by the following average composition formula (1). R 1 a SiO (4-a) / 2 (1)
[0058] In the above average composition formula (1), R 1are each independently a saturated or unsaturated, unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 14. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl, cycloalkyl groups such as cyclopentyl and cyclohexyl, alkenyl groups such as vinyl and allyl, aryl groups such as phenyl and tolyl, aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl, and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or with a cyano group, for example, a 3,3,3-trifluoropropyl group, a 2-(perfluorobutyl)ethyl group, a 2-(perfluorooctyl)ethyl group, and a p-chlorophenyl group, and the like are preferred.
[0059] In the above average composition formula (1), a is a number within the range of 1.8 to 2.2, and particularly within the range of 1.9 to 2.1. By having a within this range, the resulting thermally conductive silicone composition can have a good viscosity.
[0060] As the organopolysiloxane represented by the above average composition formula (1), a linear organopolysiloxane represented by the following formula (2) is preferred. [ka]
[0061] In the above formula, R 2 are each independently a saturated or unsaturated, unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 14 carbon atoms. Examples of the monovalent hydrocarbon group include the groups described above. Furthermore, at least one R 2 is preferably a vinyl group. m is a value that indicates that the kinetic viscosity of the organopolysiloxane at 25° C. is 10 to 100,000 mm 2 / s, preferably 30 to 10,000 mm 2 / s, and more preferably 100 to 8,000 mm2 / s.
[0062] The blend amount of the component (A) is preferably 0.1 to 60 mass %, and more preferably 0.1 to 10 mass %, of the total composition. The component (A) may be blended either alone or in combination of two or more.
[0063] The component (A) is preferably an organopolysiloxane having one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms in each molecule.
[0064] [(B) Component] Component (B) is a hydrolyzable organopolysiloxane containing an alkoxysilyl group. Component (B) acts as a surface treatment agent for the above components (C) to (E). Therefore, by adding component (B), the thermally conductive silicone composition can maintain its fluidity even when components (C) to (E) are added in large amounts to the composition. At the same time, deterioration of heat dissipation performance caused by oil separation and pump-out over time can be suppressed. Examples of component (B) include organopolysiloxanes represented by the following general formula (3). Among them, it is preferable to contain a trifunctional hydrolyzable organopolysiloxane. [ka] (In the formula, R 3 X is independently an unsubstituted or substituted monovalent hydrocarbon group. 1 , X 2 , X 3 is R 3 Or -(R 4 ) n -SiR 5 d (OR 6 ) 3-d may be different, but at least one of them is -(R 4 ) n -SiR 5 d (OR 6 ) 3-d R 4 is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, R5 are independently unsubstituted or substituted monovalent hydrocarbon groups containing no aliphatic unsaturated bonds, R 6 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group or an acyl group having 1 to 4 carbon atoms, n is 0 or 1, and d is an integer of 0 to 2. b and c are 1≦b≦1,000 and 0≦c≦1,000, respectively.
[0065] In the above general formula (3), R 3 are independently unsubstituted or substituted monovalent hydrocarbon groups having preferably 1 to 10 carbon atoms, more preferably 1 to 6 carbon atoms, and even more preferably 1 to 3 carbon atoms, examples of which include linear alkyl groups, branched alkyl groups, cyclic alkyl groups, alkenyl groups, aryl groups, aralkyl groups, halogenated alkyl groups, and the like. Examples of linear alkyl groups include methyl groups, ethyl groups, propyl groups, hexyl groups, and octyl groups. Examples of branched alkyl groups include isopropyl groups, isobutyl groups, tert-butyl groups, and 2-ethylhexyl groups. Examples of cyclic alkyl groups include cyclopentyl groups and cyclohexyl groups. Examples of alkenyl groups include vinyl groups and allyl groups. Examples of aryl groups include phenyl groups and tolyl groups. Examples of aralkyl groups include 2-phenylethyl groups and 2-methyl-2-phenylethyl groups. Examples of halogenated alkyl groups include a 3,3,3-trifluoropropyl group, a 2-(nonafluorobutyl)ethyl group, and a 2-(heptadecafluorooctyl)ethyl group. 3 As the alkyl group, a methyl group, a phenyl group, and a vinyl group are preferred.
[0066] X 1 , X 2 , X 3 is R 3 Or -(R 4 ) n -SiR 5 d (OR 6 ) 3-d may be different, but at least one of them is -(R 4 ) n -SiR5 d (OR 6 ) 3-d It is.
[0067] R 4 is an oxygen atom or an alkylene group having 1 to 4 carbon atoms, and R 4 Examples of the alkylene group having 1 to 4 carbon atoms include a methylene group, an ethylene group, a propylene group, and a butylene group. 5 are independently unsubstituted or substituted monovalent hydrocarbon groups not containing an aliphatic unsaturated bond, preferably having 1 to 10 carbon atoms, more preferably 1 to 6, and even more preferably 1 to 3. Examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl groups, cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl groups, aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl groups, aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl groups, and groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine, chlorine, and bromine, or with cyano groups, etc.
[0068] Above R 6 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group having 1 to 4 carbon atoms. 6 Examples of the alkyl group include R 3 Examples of the alkoxyalkyl group include a methoxyethyl group and a methoxypropyl group. Examples of the alkenyl group include a vinyl group and an allyl group. 6 The acyl group of R is preferably one having 2 to 8 carbon atoms, and examples of the acyl group include an acetyl group and an octanoyl group. 6 is preferably an alkyl group, and particularly preferably a methyl group or an ethyl group.
[0069] b and c are 1≦b≦1,000 and 0≦c≦1,000, respectively, but preferably b+c is 10 to 1,000, more preferably 10 to 300. n is 0 or 1, and d is an integer of 0 to 2, preferably 0. In addition, if OR 6 The number of groups is preferably 1 to 6, and particularly preferably 3 or 6. The bonding order of the siloxane units shown in parentheses is not limited to the following order.
[0070] Specific examples of suitable components (B) include the following: [ka]
[0071] The blend amount of the component (B) is preferably 0.1 to 60 mass %, and more preferably 1 to 10 mass %, of the total composition. The component (B) may be blended either alone or in combination of two or more.
[0072] In the thermally conductive silicone composition of the present invention, when the above-mentioned component (A) is an organopolysiloxane that has one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms per molecule, the thermally conductive silicone composition can be made into an addition reaction type thermally conductive silicone composition by further adding the following components (F) to (H).
[0073] [Component (F)] Component (F) is an organohydrogenpolysiloxane having two or more, and preferably at least 3 but less than 40, hydrogen atoms bonded to silicon atoms (SiH groups) per molecule, i.e., an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms per molecule, and the hydrogen atoms bonded to silicon atoms in the molecule undergo an addition reaction with aliphatic unsaturated hydrocarbon groups in the composition in the presence of a platinum group metal catalyst described below, to form a crosslinked structure.
[0074] The molecular structure of the component (F) is not particularly limited and may be, for example, linear, branched, or cyclic, and can be represented by the average composition formula (4) below. R 7 e H f SiO (4-e-f) / 2 (4)
[0075] In the average composition formula (4), R 7 are each independently a saturated or unsaturated, unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms, preferably 1 to 14, excluding aliphatic hydrocarbon groups. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl, cycloalkyl groups such as cyclopentyl and cyclohexyl, alkenyl groups such as vinyl and allyl, aryl groups such as phenyl and tolyl, aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl, and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, bromine, and chlorine, or cyano groups, such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, and p-chlorophenyl. 7 As the alkyl group, a methyl group and a phenyl group are particularly preferred.
[0076] e is a positive number of 1.0 to 3.0, preferably 0.5 to 2.5, f is 0.005 to 2.0, preferably 0.01 to 1.0, and e+f is a positive number of 0.5 to 3.0, preferably 0.8 to 2.5.
[0077] The amount of component (F) is preferably such that the number of hydrogen atoms bonded to silicon atoms in one molecule of component (F) is 4.0 to 20.0, more preferably 8.0 to 20.0, per one aliphatic unsaturated hydrocarbon group bonded to silicon atoms in one molecule of component (A).Within such a range, the slippage resistance is improved.Finally, the component (F) may be blended alone or in combination of two or more kinds.
[0078] In the present invention, it is preferable to contain a hydrosilylation reaction product of the component (A) and the component (F). By containing such a component, it is possible to further improve the slippage resistance.
[0079] [(G) component] Component (G) is a platinum group metal catalyst, which is a catalyst for promoting the hydrosilylation reaction between the aliphatic unsaturated hydrocarbon group bonded to a silicon atom in component (A) and the SiH group in component (F). The platinum group metal catalyst may be any of those conventionally known for addition reactions. Examples include platinum-based, palladium-based, and rhodium-based catalysts, among which platinum or platinum compounds, which are relatively easy to obtain, are preferred. Examples include platinum alone, platinum black, chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, and platinum coordination compounds.
[0080] The amount of component (G) blended is preferably within the range of 1 to 2,000 ppm, and more preferably 2 to 1,000 ppm, calculated as the mass of platinum group metal atoms relative to the organopolysiloxane of component (A), which ensures an appropriate reaction rate for the addition reaction.
[0081] The component (G) may be used alone or in combination of two or more different compounds.
[0082] [(H) component] The component (H) is a reaction inhibitor that suppresses the progress of the hydrosilylation reaction at room temperature and functions to extend shelf life and pot life. The reaction inhibitor can be a conventional reaction inhibitor used in addition curing silicone compositions. Examples of the reaction inhibitor include acetylene compounds such as acetylene alcohols (e.g., ethynylmethyldecylcarbinol, 1-ethynyl-1-cyclohexanol, 3,5-dimethyl-1-hexyn-3-ol), various nitrogen compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole, organic phosphorus compounds such as triphenylphosphine, oxime compounds, and organic chloro compounds.
[0083] [Component (I)] In the thermally conductive silicone composition of the present invention, when the above-mentioned component (A) is an organopolysiloxane that has one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms per molecule, the inclusion of an organic peroxide (I) can enhance the resistance to misalignment of the composition through a radical reaction between components (A).
[0084] As the organic peroxide, known organic peroxides used in radical reactions can be used, for example, acyl organic peroxides such as benzoyl peroxide and bis(p-methylbenzoyl)peroxide, alkyl organic peroxides such as di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide and dicumyl peroxide, and ester organic peroxides such as tert-butyl perbenzoate.
[0085] [(J) component] When the thermally conductive silicone composition of the present invention contains the above-mentioned component (B), it can further contain a condensation catalyst (J) to form a thermally conductive silicone composition that undergoes a condensation reaction, and the condensation reaction of component (B) can further enhance the shear resistance of the thermally conductive silicone composition.
[0086] Condensation catalyst can be used known ones used in condensation reaction.For example, metal catalysts such as titanium esters such as tetrabutyl titanate, tetrapropyl titanate, etc.; organic tin compounds such as dibutyltin dilaurate, dibutyltin maleate, dibutyltin diacetate, etc.; tin carboxylates such as tin octoate, tin naphthenate, tin laurate, tin fersaticate, etc.; reaction product of dibutyltin oxide and phthalic acid ester; dibutyltin diacetylacetonate; organic aluminum compounds such as aluminum triacetylacetonate, aluminum trisethylacetoacetate, diisopropoxyaluminum ethylacetoacetate, etc.; chelate compounds such as diisopropoxy-bis(ethyl acetoacetate)titanium, zirconium tetraacetylacetonate, titanium tetraacetylacetonate, etc.; lead octoate; iron naphthenate; bismuth compounds such as bismuth-tris(neodecanoate) and bismuth-tris(2-ethylhexanoate). Furthermore, known amine catalysts such as laurylamine may be used. Among these, particularly preferred are tin carboxylates or organic tin compounds such as dibutyltin dilaurate, dibutyltin maleate, dibutyltin diacetate, tin octylate, tin naphthenate, tin laurate, and tin fersaticate; a reaction product of dibutyltin oxide and a phthalic acid ester; tin catalysts such as dibutyltin diacetylacetonate; and chelate compounds such as diisopropoxy-bis(ethyl acetoacetate)titanium.
[0087] [Other ingredients] The thermally conductive silicone composition of the present invention may contain a non-reactive organo(poly)siloxane such as methylpolysiloxane for the purpose of adjusting the elastic modulus and viscosity. In addition, in order to prevent deterioration of the thermally conductive silicone composition, a known antioxidant such as 2,6-di-t-butyl-4-methylphenol may be contained as necessary. Furthermore, dyes, pigments, flame retardants, anti-settling agents, thixotropy improvers, etc. may be blended as necessary.
[0088] [Thermal Conductivity] The thermal conductivity of the thermally conductive silicone composition of the present invention, as measured by the hot disk method in accordance with ISO 22007-2, is preferably at least 7.5 W / m K. There is no upper limit to the thermal conductivity, but it is preferably no greater than 13.0 W / m K. The thermal conductivity was measured by the method described in the Examples below.
[0089] The thermally conductive silicone composition of the present invention is resistant to slippage, making it an ideal thermally conductive silicone composition. The method for measuring slippage resistance is as described in the Examples below.
[0090] [Method of producing thermally conductive silicone composition] The method for producing the thermally conductive silicone composition of the present invention will now be described, but is not limited to this.
[0091] The method for producing the thermally conductive silicone composition of the present invention may be according to the conventional method for producing a thermally conductive silicone composition, and is not particularly limited. For example, the composition can be obtained by mixing the above-mentioned components (A) to (J) and, if necessary, other optional components. The mixing device is not particularly limited, and mixers such as Trimix, Twinmix, Planetary Mixer (all registered trademarks of mixers manufactured by Inoue Seisakusho Co., Ltd.), Ultra Mixer (registered trademarks of mixers manufactured by Mizuho Kogyo Co., Ltd.), and Hivis Dispermix (registered trademarks of mixers manufactured by Tokushu Kika Kogyo Co., Ltd.) can be used. In addition, a three-roll finishing treatment or the like may be performed to break down the aggregation of the thermally conductive fillers (C), (D), and (E).
[0092] When the thermally conductive silicone composition of the present invention contains component (A) which is an organopolysiloxane having one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms per molecule, and also contains components (F) and (G), it is preferable to stir the mixture at a temperature of 100°C or higher for 30 minutes or longer. This allows components (A) and (F) to be sufficiently crosslinked via a hydrosilylation reaction, and allows the thermally conductive silicone composition to have a more appropriate viscosity. EXAMPLES
[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following, the kinematic viscosity is a value measured at 25°C using an Ostwald viscometer (manufactured by Shibata Scientific Co., Ltd.). The thickness of component (C) after pressing was determined by using 150 parts by mass of component (C) and a kinematic viscosity of 1,000 mm at 25°C. 2 A paste (thickness 300 μm) made by mixing 100 parts by mass of dimethylpolysiloxane of 12.6 parts by mass of 100% by mass of dimethylpolysiloxane of 12.6 parts ...
[0094] The components used were as follows: [Component (A)] A-1: Both ends are blocked with trimethylsilyl groups, and the kinetic viscosity at 25°C is 5,000mm 2 / s Dimethylpolysiloxane A-2: Both ends are blocked with dimethylvinylsilyl groups, and the kinetic viscosity at 25°C is 600mm 2 / s dimethylpolysiloxane (vinyl group amount 0.015mol / g) A-3: The ends are blocked with dimethylvinylsilyl and trimethylsilyl groups, and the kinetic viscosity at 25°C is 700mm 2 / s dimethylpolysiloxane (vinyl group amount 0.005mol / g)
[0095] [(B) Component] B-1: Hydrolyzable organopolysiloxane represented by the following formula: [ka]
[0096] [(C) component] C-1: Round aluminum nitride particles with D50 of 20.0 μm (Thickness after pressing: 54 μm) C-2: Round aluminum nitride particles with D50 of 11.0 μm (Thickness after pressing: 32 μm) C-3: Round aluminum nitride particles with D50 of 5.0 μm (Thickness after pressing: 14 μm) C-4: Spherical alumina particles with D50 of 10.0 μm (Thickness after pressing: 25 μm) (Comparative component)
[0097] [(D) component] D-1: Round aluminum nitride particles with D50 of 70.0 μm D-2: Round aluminum nitride particles with D50 of 100.0 μm D-3: Round aluminum nitride particles with D50 of 120.0 μm D-4: Spherical aluminum nitride particles with D50 of 60.0 μm (comparative component) D-5: Spherical alumina particles with D50 of 100.0 μm (comparative component)
[0098] [(E) component] E-1: Irregular zinc oxide particles with D50 of 1.2 μm E-2: Irregular zinc oxide particles with D50 of 0.4 μm E-3: Round aluminum nitride particles with D50 of 0.7 μm E-4: Irregular alumina particles with D50 of 1.3 μm
[0099] [Component (F)] F-1: Both ends are blocked with trimethylsilyl groups, and the kinetic viscosity at 25°C is 100mm 2 / s and SiH content of 0.0055 mol / g
[0100] [(G) component] G-1: A solution of platinum-divinyltetramethyldisiloxane complex dissolved in the same dimethylpolysiloxane as A-2 (platinum atom content: 1% by mass)
[0101] [(H) component] H-1: Ethynylcyclohexanol
[0102] [Examples 1 to 14, Comparative Examples 1 to 5] Preparation of Thermally Conductive Silicone Composition The above components (A) to (H) were blended in the amounts shown in Tables 1 to 3 below, by the method described below, to prepare thermally conductive silicone compositions. Components (A) to (H) were added to a 5-liter planetary mixer (manufactured by Inoue Seisakusho Co., Ltd.) and mixed at 150°C for 4 hours. The mixture was then cooled to 25°C to prepare a thermally conductive silicone composition. The viscosity, thermal conductivity, and slippage resistance of each composition obtained by the above method were evaluated according to the following methods. The results are shown in Tables 1 to 3.
[0103] [viscosity] The viscosity of the thermally conductive silicone composition was measured using a spiral viscometer (Type PC-1T) manufactured by Malcom Co., Ltd., and was measured at 25° C. (rotor A at 10 rpm, shear rate 6 [1 / s]).
[0104] [Thermal Conductivity] Each composition was wrapped in kitchen wrap to form a pouch, and the thermal conductivity of the pouch was measured using a Kyoto Electronics Manufacturing Co., Ltd. TPA-501.
[0105] [Slip resistance] A test piece was prepared by sandwiching 1.0 g of the composition between an aluminum plate and a glass plate of 60 mm x 60 mm with a spacer to a thickness of 0.5 mm. The test piece was vertically left at 25 ° C for 12 hours, and then the composition was marked with × if it had moved, and marked with ◯ if it had not moved. The test piece was then placed vertically in a thermal tester with one cycle of -40 ° C for 30 minutes and 120 ° C for 30 minutes, and marked with ⊚ if the composition had not moved after 1,000 cycles.
[0106] [Table 1]
[0107] [Table 2]
[0108] [Table 3]
[0109] The results in Tables 1 to 3 show that the thermally conductive silicone compositions of Examples 1 to 14, which met the requirements of the present invention, were able to achieve both high thermal conductivity and resistance to displacement due to thermal shock.
[0110] On the other hand, Comparative Example 1, in which the ratio of component (D) to the total amount of components (C) and (D) was 50% by mass or more, was inferior in slippage resistance. Comparative Example 2, in which spherical particles were used instead of component (C) of the present invention, and Comparative Examples 3 and 4, in which spherical particles were used instead of component (D) of the present invention, were inferior in thermal conductivity, and Comparative Example 5, which did not contain component (E) of the present invention, had a non-uniform composition and was extremely inferior in handleability.
[0111] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. A thermally conductive silicone composition comprising: (C) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 4 μm or more and less than 50 μm; (D) one or more types of aluminum nitride particles selected from amorphous, rounded, and polyhedral particles having an average particle size of 50 μm or more and 150 μm or less; And, (E) One or more particles selected from aluminum nitride particles having an average particle size of 0.1 μm or more and less than 4.0 μm, and zinc oxide particles. Contains the total amount of the (C) component and the (D) component is 20% by mass or more and less than 80% by mass of the total composition, a thermally conductive silicone composition, characterized in that the blending amount of said component (E) is equal to or greater than 20% by mass and less than 50% by mass of the entire composition, and the proportion of said component (D) relative to the combined amount of said component (C) and said component (D) is equal to or greater than 5% by mass and less than 50% by mass.
2. 2. The thermally conductive silicone composition according to claim 1, wherein component (C) is rounded aluminum nitride particles.
3. The component (C) is 150 parts by mass of the component (C) and has a kinetic viscosity of 1,000 mm at 25° C. 2 3. The thermally conductive silicone composition according to claim 1, wherein when a paste obtained by mixing 100 parts by mass of a dimethylpolysiloxane having a molecular weight of 100 or more and ...
4. 4. The thermally conductive silicone composition according to claim 1, wherein component (E) is amorphous zinc oxide particles.
5. Furthermore, (A) a kinetic viscosity at 25°C of 10 to 100,000 mm 2 5. The thermally conductive silicone composition according to claim 1, which contains an organopolysiloxane in which the formula (I) is a hydroxy group or a hydroxy group.
6. 6. The thermally conductive silicone composition according to claim 5, wherein component (A) is an organopolysiloxane having one or more aliphatic unsaturated hydrocarbon groups bonded to silicon atoms per molecule.
7. moreover, (F) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms in each molecule; (G) platinum group metal catalyst, And, (H) Reaction inhibitor The thermally conductive silicone composition according to claim 6, which comprises
8. 8. The thermally conductive silicone composition according to claim 7, which contains a hydrosilylation reaction product of said component (A) and said component (F).
9. 9. The thermally conductive silicone composition according to claim 7, wherein for each aliphatic unsaturated hydrocarbon group bonded to a silicon atom in one molecule of component (A), there are 4.0 to 20.0 hydrogen atoms bonded to silicon atoms in one molecule of component (F).
10. 10. The thermally conductive silicone composition according to any one of claims 6 to 9, further comprising (I) an organic peroxide.
11. 11. The thermally conductive silicone composition according to claim 1, further comprising (B) a hydrolyzable organopolysiloxane that contains an alkoxysilyl group.
12. 12. The thermally conductive silicone composition according to claim 11, further comprising (J) a condensation catalyst.
Citation Information
Patent Citations
Aluminum nitride substrate and manufacture
JP1987046986A
Thermally conductive silicone composition and cured product of the same
JP2017210518A
Thermal conductive silicone composition and production method thereof
JP2020063365A
Thermally conductive composition
WO2016190189A1
Silicone composition and method for producing same
WO2020137970A1