Thermally conductive silicone rubber composition
The thermally conductive silicone rubber composition addresses the challenges of low thermal conductivity and brittleness in heat dissipation by using specific organopolysiloxanes and fillers, achieving high thermal conductivity and strength with low-molecular-weight siloxane removal, ensuring easy mounting and preventing contact failure.
Patent Information
- Application Number
- JP2021183716
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-11-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-11-10
AI Technical Summary
Existing heat dissipation methods for electronic components face challenges such as low thermal conductivity, reduced elasticity, and difficulty in mounting due to high-temperature curing, which leads to brittleness and contact failure from low-molecular-weight siloxane volatilization.
A thermally conductive silicone rubber composition comprising specific organopolysiloxanes and thermal conductive fillers, cured at low temperatures to achieve high thermal conductivity, sufficient low-molecular-weight siloxane removal, and adequate strength, preventing embrittlement and contact failure.
The composition provides a heat-dissipating molded article with excellent thermal conductivity, strength, and insulation properties, easily mountable on electronic components, while minimizing low-molecular-weight siloxane content to prevent contact failure.
Smart Images

Figure 0007577048000010 
Figure 0007577048000001 
Figure 0007577048000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat-conductive silicone rubber composition and a heat-radiating molded article using the composition. [Background technology]
[0002] Semiconductors such as transistors and diodes used in electronic devices such as converters and power supplies generate large amounts of heat themselves as they become more powerful, faster, smaller, and more integrated. This can cause equipment to malfunction or break down if the temperature of the equipment rises. For this reason, many heat dissipation methods have been proposed to suppress the temperature rise of semiconductors during operation, as well as heat dissipation materials used for these methods.
[0003] For example, in order to suppress the temperature rise of semiconductors during operation in electronic devices, heat sinks made of metal plates with high thermal conductivity such as aluminum and copper are used. These heat sinks conduct the heat generated by the semiconductor and release the heat from their surface due to the temperature difference with the outside air. On the other hand, the semiconductor and the heat sink must be electrically insulated, and for this reason, a plastic film or the like is interposed between the heat-generating electronic component and the heat sink. However, the plastic film has an extremely low thermal conductivity, which significantly impedes the transfer of heat to the heat sink.
[0004] Therefore, in order to make the sheet less likely to break and have thermal conductivity, a thermally conductive sheet has been developed in which a thermally conductive resin is laminated on a glass cloth. For example, there is a thermally conductive sheet in which silicone rubber containing boron nitride powder and spherical silica powder as thermally conductive fillers is laminated on a glass cloth (Patent Document 1). However, when a flat-shaped heat dissipation sheet is arranged, there is a problem that the creepage distance for insulation becomes too large.
[0005] For the above reasons, a proposal has been made to encase electronic components using a heat-dissipating molded product molded into a tube or cap shape (Patent Document 2). However, when a high amount of heat-conductive filler is added to increase thermal conductivity, the elasticity and elongation of the molded product decreases, and there is a problem that the molded product may break, crack, or be cut when attached to an electronic component. In addition, when applying a heat-dissipating molded product to an electronic component, in order to prevent contact failure caused by low-molecular-weight siloxane, it is necessary to perform a high-temperature post-cure on the heat-dissipating molded product to remove the low-molecular-weight siloxane. However, this post-cure further embrittles the molded product, making it difficult to attach it to an electronic component. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-199880 [Patent Document 2] Japanese Utility Model Application Publication No. 57-2666 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention has been made in view of the above circumstances, and has an object to provide a heat-conductive silicone rubber composition that has high thermal conductivity and can be post-cured at low temperatures to give a cured product that has sufficient low-molecular-weight siloxane removal effect and strength. Another object is to provide a heat-dissipating molded article that uses this heat-conductive silicone rubber composition, has a low low-molecular-weight siloxane content, and can be easily mounted on electronic components. [Means for solving the problem]
[0008] In order to solve the above problems, the present invention provides (A) 100 parts by mass of an organopolysiloxane having an average degree of polymerization of 3,000 to 10,000 and a total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms of 500 ppm or less, (B) an organopolysiloxane having an average degree of polymerization of 2 to 2,000 and having alkenyl groups only at both molecular chain terminals: 10 to 100 parts by mass, (C) thermally conductive filler: 500 to 2,700 parts by mass, and (D) Hardener: Effective amount The present invention provides a thermally conductive silicone rubber composition comprising:
[0009] The thermally conductive silicone rubber composition of the present invention has high thermal conductivity and can be post-cured at low temperatures to give a cured product that is sufficiently effective in removing low molecular weight siloxanes and has sufficient strength.
[0010] The thermally conductive silicone rubber composition of the present invention further comprises (E) (E1) Formula (1): R 2 b R 3 c Si(OR 4 ) 4-b-c (1) (In the formula, R 2 are independently alkyl groups having 6 to 15 carbon atoms; R 3 are independently alkyl groups having 1 to 5 carbon atoms; R 4 are independently an alkyl group having 1 to 4 carbon atoms, b is an integer of 1 to 3, and c is 0, 1 or 2, with the proviso that b+c is 1 to 3. and an alkoxysilane represented by the formula: (E2) Formula (2): [ka] (In the formula, R 5 are independently an alkyl group having 1 to 4 carbon atoms, and d is an integer of 5 to 100. Dimethylpolysiloxane having one end blocked with a trialkoxysilyl group, represented by It is preferable that one or more selected from the above be contained in an amount of 0.01 to 30 mass % based on the total amount of the organosilicon compound components.
[0011] With such a thermally conductive silicone rubber composition, it becomes easy to fill the organosilicon compound component with a non-spherical thermally conductive filler, and the resulting cured product has sufficient strength.
[0012] In the present invention, the thermally conductive silicone rubber composition preferably has a plasticity of 100-800.
[0013] Such a thermally conductive silicone rubber composition is not sticky, is easy to handle by roll work, and can be easily kneaded.
[0014] The present invention also provides a cured product obtained by curing the above-mentioned thermally conductive silicone rubber composition.
[0015] Such a cured product has high thermal conductivity and is capable of achieving sufficient low molecular weight siloxane removal effect and strength through post-curing at low temperatures.
[0016] The present invention further provides a heat-radiating molded article made from the above cured product, wherein the cured product has a thermal conductivity of 1.5 W / m·K or more.
[0017] Such a heat dissipating molded article has favorable heat dissipation performance, contains a small amount of low-molecular-weight siloxane, and can be easily mounted on electronic components.
[0018] The heat-radiating molded article of the present invention preferably has a Type A durometer hardness of 60 to 96 as defined in JIS K6253-3:2012 for the cured product.
[0019] With such a heat-dissipating molded product, the surface of the cured material layer is less likely to be scratched during handling, the surfaces of the cured material do not fuse together or deform during molding, and the molded product has excellent flexibility and does not crack when handled.
[0020] The heat-radiating molded article preferably has a withstand voltage of 4.5 kV or more when the cured product has a thickness of 0.45 mm.
[0021] With such a heat dissipating molded article, when the molded article is mounted on an electronic component, the sheet will not suffer dielectric breakdown under high voltage.
[0022] Furthermore, the heat-radiating molded article preferably has a content of diorganocyclopolysiloxane having 3 to 10 silicon atoms of 100 ppm or less after post-curing at 150° C. for 1 hour.
[0023] Such a heat-dissipating molded article can effectively prevent the occurrence of contact failure caused by the volatilization of low-molecular-weight siloxane over time. Effect of the Invention
[0024] The heat conductive silicone rubber composition of the present invention can sufficiently reduce the low molecular weight siloxane content even when subjected to a low temperature post-cure process. In addition, the heat dissipating molded article made of a cured product molded using this composition can be prevented from becoming embrittled due to high temperature post-cure. The obtained heat dissipating molded article has excellent thermal conductivity, strength, and insulation properties, and has a low low molecular weight siloxane content, making it easy to mount on electronic components and preventing contact failure. [Brief description of the drawings]
[0025] [Figure 1] FIG. 2 is a diagram showing the shape of a cover for a heat-generating electronic component produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that by molding a heat-conductive molded article using a heat-conductive silicone rubber composition in which a heat-conductive filler is added and mixed with an organopolysiloxane having a low molecular weight siloxane content below a certain value, and then post-curing the composition at a low temperature, it is possible to obtain a heat-conductive molded article which does not become embrittled and has a sufficiently reduced low molecular weight siloxane content, which has led to the completion of the present invention.
[0027] That is, the present invention is a thermally conductive silicone rubber composition characterized by containing the following (A) to (D): (A) Organopolysiloxane having an average degree of polymerization of 3,000 to 10,000 and a total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms of 500 ppm or less: 100 parts by mass (B) Organopolysiloxane having an average degree of polymerization of 2 to 2,000 and having alkenyl groups only at both ends of the molecular chain: 10 to 100 parts by mass (C) Thermally conductive filler: 500 to 2,700 parts by mass (D) Hardener: Effective amount
[0028] The heat conductive silicone rubber composition and heat dissipating molded article of the present invention are described in detail below, but the present invention is not limited to these.
[0029] The present invention provides a low temperature curable thermally conductive silicone rubber composition. The thermally conductive silicone rubber composition of the present invention is characterized by containing the specific components (A) to (D) described below. If necessary, it may further contain other components. These components will be described below.
[0030] [(A) Organopolysiloxane with an average degree of polymerization of 3,000 to 10,000] Component (A) is the main component of the thermally conductive silicone rubber composition and preferably has the average composition formula shown in formula (3) below. R n SiO (4-n) / 2 (3)
[0031] In the above formula (1), R is independently a monovalent hydrocarbon group having 1 to 8 carbon atoms, and examples thereof include alkyl groups such as methyl, ethyl, and propyl groups, alkenyl groups such as vinyl and allyl groups, aryl groups such as phenyl and tolyl groups, and cycloalkyl groups such as cyclohexyl and cyclopentyl groups. In addition, some or all of the hydrogen atoms directly bonded to the carbon atoms of these groups may be substituted with halogen atoms such as chlorine and fluorine. Preferred are methyl, phenyl, trifluoropropyl, and vinyl groups. In addition, n is a positive number of 1.85 to 2.10.
[0032] The organopolysiloxane preferably has a linear molecular structure, but may have a partially branched structure in the molecule.Furthermore, the organopolysiloxane preferably has a molecular chain end blocked with a triorganosilyl group or a hydroxyl group.Examples of the triorganosilyl group include a trimethylsilyl group, a dimethylvinylsilyl group, a trivinylsilyl group, a methylphenylvinylsilyl group, a methyldiphenylsilyl group, a dimethylphenylsilyl group, and a dimethylhydroxysilyl group.
[0033] The average degree of polymerization of the component (A) is from 3,000 to 10,000, and preferably from 5,000 to 10,000.
[0034] The average degree of polymerization referred to in this specification refers to the average degree of polymerization determined from the number average molecular weight by gel permeation chromatography (GPC) using polystyrene as the standard substance.
[0035] In component (A), the total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms is 500 ppm or less, and more preferably 300 ppm or less. If the total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms exceeds 500 ppm, high-temperature post-cure is required to remove low molecular weight compounds from the molded product, which may cause the molded product to become brittle, and low molecular weight siloxanes may volatilize from the molded product over time, resulting in contact failure. In this specification, the total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms can be determined by subjecting the measurement subject to gas chromatography analysis.
[0036] [(B) Organopolysiloxane having an average degree of polymerization of 2 to 2,000 and having alkenyl groups only at both ends of the molecular chain] The (B) component is a component that is subjected to a crosslinking reaction in the thermally conductive silicone rubber composition. It is an organopolysiloxane having an average degree of polymerization of 2 to 2,000 and having alkenyl groups only at both ends of the molecular chain. The alkenyl group is preferably an alkenyl group having 2 to 8 carbon atoms, such as a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a butenyl group, a hexenyl group, a cyclohexenyl group, etc. Among them, a lower alkenyl group having 2 to 4 carbon atoms such as a vinyl group or an allyl group is preferred, and a vinyl group is particularly preferred. The organopolysiloxane of the (B) component may be used alone or in combination of two or more types having different average degrees of polymerization.
[0037] The average degree of polymerization of the component (B) is from 2 to 2,000, and preferably from 10 to 2,000.
[0038] The blending amount of the component (B) is preferably 10 to 100 parts by mass, and more preferably 30 to 70 parts by mass, per 100 parts by mass of the component (A).
[0039] Specific examples of the component (B) include those represented by the following general formula (4). [ka] (In the formula, R 1 are independently monovalent hydrocarbon groups having no aliphatic unsaturated bonds, X is an alkenyl group, and a is a number from 0 to 1998.
[0040] In the above formula, R 1Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cycloheptyl; aryl groups such as phenyl, tolyl, xylyl, naphthyl, and biphenylyl; and aralkyl groups such as benzyl, phenylethyl, phenylpropyl, and methylbenzyl, each of which has 1 to 10 carbon atoms, and particularly 1 to 6 carbon atoms. In addition, groups in which some or all of the hydrogen atoms bonded to the carbon atoms of these groups are substituted with halogen atoms such as fluorine and chlorine may be used. Examples include chloromethyl, 3-chloropropyl, 3,3,3-trifluoropropyl, chlorophenyl, fluorophenyl, and 3,3,4,4,5,5,6,6,6-nonafluorohexyl groups. Among these, preferred are alkyl groups having 1 to 3 carbon atoms, such as a methyl group, an ethyl group, a propyl group, a chloromethyl group, and a 3,3,3-trifluoropropyl group, and aryl groups, such as a phenyl group, a chlorophenyl group, and a fluorophenyl group. 1 may all be the same or different.
[0041] Examples of the alkenyl group for X include those having about 2 to 8 carbon atoms, such as a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a butenyl group, a hexenyl group, and a cyclohexenyl group. Of these, lower alkenyl groups such as a vinyl group and an allyl group are preferred, and a vinyl group is particularly preferred.
[0042] In general formula (4), a is a number from 0 to 1998, preferably a number that satisfies 10≦a≦1998, and more preferably a number that satisfies 10≦a≦1,000. The organopolysiloxane represented by general formula (4) is preferably added in an amount of 10 to 100 parts by mass, and particularly 30 to 70 parts by mass, per 100 parts by mass of the organopolysiloxane of component (A).
[0043] [(C) Thermally conductive filler] The component (C) is a component used as a filler that imparts thermal conductivity to the thermally conductive silicone rubber composition. The component (C) may be any material that has thermal conductivity, and preferably has electrical insulation. Although not particularly limited, for example, materials that are generally considered to be thermally conductive fillers, such as metal oxides such as alumina, silica, magnesia, red iron oxide, beryllia, titania, and zirconia, metal nitrides such as aluminum nitride, silicon nitride, and boron nitride, metal hydroxides such as magnesium hydroxide, artificial diamond, and silicon carbide, can be used.
[0044] The blending amount of the component (C) is preferably 500 to 2,700 parts by mass, and more preferably 600 to 2,500 parts by mass, per 100 parts by mass of the component (A).
[0045] These thermally conductive fillers may be surface-treated with a silane coupling agent or a partial hydrolysate thereof, an alkylalkoxysilane or a partial hydrolysate thereof, an organic silazanes, an organopolysiloxane oil, an organopolysiloxane containing a hydrolyzable functional group, etc. Such treatment may be performed by previously treating the thermally conductive filler itself, or may be performed when mixing the organopolysiloxane of component (A) or component (B) with the thermally conductive filler (C).
[0046] In the thermally conductive silicone rubber composition, the thermally conductive filler is particularly (1) A powder having an average particle size of 5 to 60 μm, preferably 5 μm or more and less than 50 μm, and (2) Powder with an average particle size of 0.5 to 4 μm, preferably 0.5 μm or more and less than 3 μm The ratio of component (1) to component (2) is preferably (1):(2)=9:1 to 4:6, and more preferably 8:2 to 5:5. When the ratio of component (1) to component (2) is within this range, the thermally conductive filler can be effectively dispersed and filled in the silicone, and the plasticity of the thermally conductive silicone rubber composition can be kept within a range that provides good workability. In addition, the surface of the heat-dissipating molded article can be made smoother.
[0047] The above average particle size is usually the cumulative volume average diameter D 50 Specifically, it can be calculated as the cumulative 50% particle diameter (D) on a volume basis measured using a particle size distribution analyzer MT3000II manufactured by Microtrack Bell Co., Ltd. 50 ) value.
[0048] [(D) Hardener] Component (D) is a component necessary for curing the thermally conductive silicone rubber composition. The curing agent is appropriately selected depending on the mechanism of the crosslinking reaction of the composition.
[0049] When curing is carried out by addition reaction, an organohydrogenpolysiloxane is used as the curing agent (D) and the reaction is carried out in the presence of a platinum catalyst. When curing by peroxide, an organic peroxide is used as the curing agent (D).
[0050] When the composition is cured by an addition reaction (hydrosilylation reaction), the curing agent is comprised of an organohydrogenpolysiloxane having an average of two or more silicon-bonded hydrogen atoms per molecule and a platinum catalyst.
[0051] Examples of groups bonded to silicon atoms in this organohydrogenpolysiloxane include linear alkyl groups, branched alkyl groups, cyclic alkyl groups, aryl groups, aralkyl groups, and halogenated alkyl groups, with alkyl groups and aryl groups being preferred, and methyl and phenyl groups being particularly preferred. The kinetic viscosity of this organohydrogenpolysiloxane at 25°C is not particularly limited, but is preferably 5 to 300 mm 2 / s, and particularly preferably 10 to 200 mm 2 / s range. In the present invention, the kinematic viscosity refers to a value measured at 25° C. using a Cannon-Fenske viscometer described in JIS Z8803:2011.
[0052] The molecular structure of this organohydrogenpolysiloxane is not limited, and examples thereof include linear, branched, partially branched linear, cyclic, and dendritic (dendrimer) structures. This organohydrogenpolysiloxane may be, for example, a homopolymer having these molecular structures, a copolymer consisting of these molecular structures, or a mixture thereof.
[0053] Examples of such organohydrogenpolysiloxanes include dimethylpolysiloxanes blocked at both molecular chain terminals with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers blocked at both molecular chain terminals with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers blocked at both molecular chain terminals with dimethylhydrogensiloxy groups, and the formula: (CH3)3SiO 1 / 2 Siloxane units represented by the formula: (CH3)2HSiO 1 / 2 Siloxane units represented by the formula: SiO 4 / 2 and mixtures of two or more of these.
[0054] In the thermally conductive silicone rubber composition, the content of this organohydrogenpolysiloxane is the amount (effective amount) necessary for curing the composition, and specifically, the amount is preferably within the range of 0.8 to 10 moles of silicon-bonded hydrogen atoms in this component per mole of silicon-bonded alkenyl groups in the thermally conductive silicone rubber composition, more preferably within the range of 1 to 8 moles, and particularly preferably within the range of 1.2 to 5 moles. If the content of this component is at or above the lower limit of the above range, curing is sufficient to obtain sufficient sheet strength and oil bleeding can be suppressed, and if it is at or below the upper limit of the above range, the sheet does not become embrittled or foaming does not occur.
[0055] The platinum catalyst is a catalyst for accelerating the curing of the present composition, and examples thereof include chloroplatinic acid, an alcohol solution of chloroplatinic acid, an olefin complex of platinum, an alkenylsiloxane complex of platinum, and a carbonyl complex of platinum.
[0056] In addition, when the present composition is cured by a free radical reaction with an organic peroxide, the curing agent is an organic peroxide, such as benzoyl peroxide, di(p-methylbenzoyl) peroxide, di(o-methylbenzoyl) peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, di-t-butyl peroxide, and t-butyl peroxybenzoate.
[0057] The content of this organic peroxide is the amount (effective amount) necessary for curing the composition, and specifically, it is preferably an amount of 0.5 to 20 parts by mass, and particularly preferably an amount of 1 to 10 parts by mass, per 100 parts by mass of the organosilicon compound component. If the content of this component is at or above the lower limit of the above range, curing is sufficient, sufficient sheet strength is obtained, and oil bleeding can be suppressed, while if it is at or below the upper limit of the above range, the sheet does not become embrittled or foaming occurs.
[0058] [(E) component] The thermally conductive silicone rubber composition according to the present invention may further contain the following component (E) as an organosilicon compound component. Component (E) is one or more selected from components (E1) and (E2) below. Component (E) improves, for example, the wettability of the non-spherical thermally conductive filler (C), making it easier to fill the organosilicon compound component with the thermally conductive filler, and therefore can increase the loading amount of the thermally conductive filler.
[0059] (Component (E1)) The component (E1) is an alkoxysilane represented by the following formula (1). R 2 b R 3 c Si(OR 4 ) 4-b-c (1) (In the formula, R 2 are independently alkyl groups having 6 to 15 carbon atoms; R3 are independently an alkyl group having 1 to 5 carbon atoms; R 4 are independently an alkyl group having 1 to 4 carbon atoms, b is an integer of 1 to 3, and c is 0, 1 or 2, with the proviso that b+c is 1 to 3.
[0060] In the above formula (1), R 2 Examples of the alkyl group represented by the formula (I) include a hexyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, and a tetradecyl group. 2 When the alkyl group represented by the formula (I) has 6 to 15 carbon atoms, the wettability of the non-spherical thermally conductive filler (C) is sufficiently improved, making it easier to fill the thermally conductive filler into the thermally conductive silicone rubber composition, and the low-temperature properties of the composition are also improved.
[0061] R 3 Examples of the alkyl group represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a t-butyl group, a pentyl group, a neopentyl group, etc. In particular, an alkyl group having 1 to 3 carbon atoms, such as a methyl group, an ethyl group, a propyl group, etc., is preferred.
[0062] R 4 Examples of the alkyl group represented by the formula (I) include alkyl groups having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, a propyl group, and a butyl group.
[0063] b is an integer of 1 to 3, and c is 0, 1 or 2, provided that b+c is 1 to 3.
[0064] ((E2) component) Component (E2) is a dimethylpolysiloxane in which one molecular chain end is blocked with a trialkoxysilyl group, as represented by the following formula (2). [ka] (In the formula, R 5 are independently an alkyl group having 1 to 4 carbon atoms, and d is an integer of 5 to 100.
[0065] R 5 The alkyl group represented by the formula (1) is 4 The alkyl group may be the same as the alkyl group represented by the following formula:
[0066] d is an integer of 5 to 100, and preferably an integer of 10 to 50.
[0067] When component (E) is added, the amount of component (E) is preferably 0.01 to 30% by mass, more preferably 1 to 20% by mass, based on the total amount of the organosilicon compound components. If the amount is equal to or greater than the lower limit, the non-spherical thermally conductive filler can be easily filled into the organosilicon compound components. If the amount is equal to or less than the upper limit, the strength of the resulting cured product is sufficient.
[0068] [Component (F)] The thermally conductive silicone rubber composition according to the present invention may further contain the following component (F) as an organosilicon compound component. Component (F) is a plasticizer, and is a dimethylsiloxane represented by the following formula (5). [ka] (In the formula, e is an integer of 5 to 500, preferably an integer of 50 to 400.)
[0069] When component (F) is blended, the blending amount is preferably 0.5 to 20 mass% of the total amount of the organosilicon compound components, and more preferably 1 to 15 mass%. If the amount is equal to or more than the lower limit, the sheet does not become too hard and brittle. If the amount is equal to or less than the upper limit, sufficient sheet strength is obtained and oil bleeding is suppressed.
[0070] [Other ingredients] The heat conductive silicone rubber composition of the present invention may further contain other components as required, such as reinforcing silica, silicone oil, silicone wetter, flame retardant, addition reaction regulator, colorant, heat resistance improver, and internal release agent, as described below.
[0071] [Preparation of Thermally Conductive Silicone Rubber Composition] The above-mentioned heat-conductive silicone rubber composition can be prepared as follows. The components (A), (B), and (C), and when added, the components (E) and (F), etc., are kneaded using a mixer such as a kneader or a Banbury mixer while heating to a temperature of 100°C or higher as necessary. In this kneading process, reinforcing silica such as fumed silica and precipitated silica; silicone oil, silicone wetter, etc.; flame retardants such as platinum, titanium oxide, and benzotriazole, etc. may be added as desired. The homogeneous mixture obtained in the kneading process is cooled to room temperature, filtered through a strainer, etc., and then a required amount of curing agent (D) is added to the mixture using a two-roll mill, a kneader, a Banbury mixer, etc., and kneaded again. In this second kneading process, acetylene compound-based addition reaction inhibitors such as 1-ethynyl-1-cyclohexanol, colorants such as organic pigments and inorganic pigments, heat resistance improvers such as iron oxide and cerium oxide, and internal release agents may be added as desired.
[0072] The curing conditions for the above-mentioned heat-conductive silicone rubber composition are, for example, in the case of curing by addition reaction, preferably at 80 to 180°C, particularly 100 to 160°C, for 30 seconds to 20 minutes, particularly 1 minute to 10 minutes, and in the case of curing by organic peroxide, preferably at 100 to 180°C, particularly 110 to 170°C, for 30 seconds to 20 minutes, particularly 1 minute to 10 minutes. Furthermore, it is preferable to perform post-cure at 100 to 170°C as necessary. If the post-cure temperature is too high, the molded product may become brittle due to reduced elongation.
[0073] In this way, the thermally conductive silicone rubber composition of the present invention can be cured at low temperatures of 180°C or less, whether cured by addition reaction or by organic peroxide, and there is no need to remove low molecular weight siloxanes at high temperatures, so that it has a low molecular weight siloxane removal effect sufficient to prevent contact failure, and it is possible to obtain a cured product (molded product, particularly a heat-dissipating molded product) that has high thermal conductivity and excellent strength.
[0074] The plasticity of the thermally conductive silicone rubber composition is preferably 100 to 800. If the plasticity is within the above range, the composition will not be sticky and difficult to handle by roll work, etc., and the composition will be easily kneaded. The plasticity can be measured by a method conforming to JIS K6249:2003 using an automatic Williams Plastometer VR-6155 manufactured by Ueshima Seisakusho Co., Ltd.
[0075] The cured product of the thermally conductive silicone rubber composition has a thermal conductivity of at least 1.5 W / m K, more preferably at least 1.8 W / m K, and even more preferably at least 2.0 / m K. The thermal conductivity can be measured by the hot disk method (in accordance with ISO 22007-2) using a TPS-2500S manufactured by Kyoto Electronics Manufacturing Co., Ltd.
[0076] The type A durometer hardness of the cured product of the thermally conductive silicone rubber composition described above is in the range of 60 to 96, more preferably 70 to 93, as described in JIS K6253-3:2012. If the hardness is 60 or more, the surface of the cured product layer is unlikely to be scratched during handling, and the surfaces of the cured product are unlikely to fuse together or deform during molding. On the other hand, if the hardness is 96 or less, the flexibility is excellent, and no cracks occur during handling of the molded product.
[0077] When the thickness of the cured product of the thermally conductive silicone rubber composition is 0.45 mm, the withstand voltage is 4.5 kV or more. If the withstand voltage is 4.5 kV or more, when the molded product is mounted on an electronic component, the sheet will not break down under high voltage. The withstand voltage is approximately proportional to the thickness of the cured product. The withstand voltage can be measured by a method conforming to JIS C2110-1:2016.
[0078] The cured product of the above thermally conductive silicone rubber composition has a content of diorganocyclopolysiloxane having 3 to 10 silicon atoms of 100 ppm or less, more preferably 50 ppm or less, after post-curing for 1 hour at 150° C. If the content of diorganocyclopolysiloxane having 3 to 10 silicon atoms is 100 ppm or less, the occurrence of contact failure due to volatilization of low molecular weight siloxane over time can be prevented.
[0079] As described above, the heat-conductive silicone rubber composition of the present invention can be cured at low temperatures even in a highly filled system by reducing the amount of low molecular weight siloxane, and can provide molded products with good dimensional stability during molding. For this reason, the composition is suitable for producing heat-dissipating molded articles such as covers for heat-generating electronic components. EXAMPLES
[0080] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The average degree of polymerization was determined from the number average molecular weight measured by GPC using polystyrene as the standard substance. The average particle size was determined from the cumulative volume average diameter D 50 The measurements were performed using a particle size distribution analyzer MT3000II manufactured by Microtrack Bell Co., Ltd.
[0081] [Preparation of Thermally Conductive Silicone Rubber Composition] (1) The following components (A) to (C) and optional components (E) and (F) were placed in a 5 L heat treatment kneader (manufactured by Inoue Seisakusho) and mixed for 30 minutes at 25 to 40° C. The kneader was then heated, and after it was confirmed that the temperature of the composition had reached 170° C., heating and stirring was continued for an additional 2 hours.
[0082] (A) Component: (A-1) Dimethylpolysiloxane having an average degree of polymerization of 8,000 and both ends blocked with dimethylvinyl groups; total content of diorganocyclopolysiloxane having 3 to 10 silicon atoms; 100 ppm (A-2) Dimethylpolysiloxane having an average degree of polymerization of 8,000 and both ends blocked with dimethylvinyl groups; total content of diorganocyclopolysiloxane having 3 to 10 silicon atoms: 4700 ppm The total content of the diorganocyclopolysiloxanes having 3 to 10 silicon atoms was measured by gas chromatography analysis, which will be described later.
[0083] (B) Ingredients: Dimethylpolysiloxane with an average degree of polymerization of 1,000, both ends of which are blocked with dimethylvinyl groups.
[0084] (C) Thermally conductive filler: (C-1) Average particle size: 1 μm: crushed alumina (C-2) Average particle size: 1 μm: spherical alumina (C-3) Average particle size: 10 μm: spherical alumina (C-4) Average particle size: 45 μm: spherical alumina (C-5) Average particle size: 9.3 μm: crushed aluminum hydroxide (C-6) Average particle size: 1.3 μm: crushed aluminum hydroxide
[0085] Component (E): A dimethylpolysiloxane represented by the following formula (6), having an average degree of polymerization of 30 and one end blocked with a trimethoxysilyl group. [ka]
[0086] Component (F): Dimethylpolysiloxane represented by the following formula (7) [ka] (In the formula, f=300)
[0087] (2) After heating and stirring, the mixture was cooled to about room temperature (25°C) and the kneaded compound was taken out. Furthermore, using a two-roll mill (Daishin Machinery Co., Ltd.), the compound was kneaded with the following (D) as a curing agent to obtain a thermally conductive silicone rubber composition.
[0088] Component (D): an organic peroxide represented by the following formula (8): [ka]
[0089] [Plasticity measurement] The plasticity of the resulting thermally conductive silicone rubber composition was measured according to a method in accordance with JIS K6249:2003 using an automatic Williams Plastometer VR-6155 manufactured by Ueshima Seisakusho Co., Ltd. The results are shown in Table 1.
[0090] [Thermal conductivity measurement] The obtained heat-conductive silicone rubber composition was placed in a 60 mm × 60 mm × 6 mm mold, and the pressure was adjusted so that the thickness after curing would be 6 mm. Then, using a high-pressure press (manufactured by Shoji Iron Works Co., Ltd.), the composition was pressed at 165°C and 100 kgf / cm 2 The sheets were press cured at 400°C for 10 minutes to produce sheets with a thickness of 6 mm. The sheets were then post-cured at 150°C for 1 hour or 200°C for 1 hour, and then cooled to room temperature. Two of the 6 mm thick sheets were used to measure the thermal conductivity at 25°C using a probe placed between the two sheets by the hot disk method (compliant with ISO 22007-2). The results are shown in Table 1.
[0091] [Hardness] The obtained heat-conductive silicone rubber composition was placed in a 60 mm × 60 mm × 6 mm mold, and the pressure was adjusted so that the thickness after curing would be 6 mm. Then, using a high-pressure press (manufactured by Shoji Iron Works Co., Ltd.), the composition was pressed at 165°C and 100 kgf / cm 2 The sheets were press cured at 400°C for 10 minutes to produce sheets with a thickness of 6 mm. The sheets were then subjected to secondary curing at 150°C for 1 hour or 200°C for 1 hour, and then cooled to room temperature. Two of the 6 mm thick sheets were stacked together to produce a test piece, and their hardness was measured using a durometer A hardness tester. The results are shown in Table 1.
[0092] [Voltage resistance] The obtained heat-conductive silicone rubber composition was placed in a mold of 100 mm × 100 mm × 0.45 mm, and the pressure was adjusted so that the thickness after curing would be 0.45 mm. Then, using a high-pressure press (manufactured by Shoji Iron Works Co., Ltd.), the composition was pressed at 165°C and 100 kgf / cm 2The resulting sheets were press cured at 40°C for 10 minutes to produce sheets with a thickness of 0.45 mm. The sheets were then post-cured at 150°C for 1 hour or 200°C for 1 hour, and then cooled to room temperature. The air dielectric strength of the 0.45 mm sheets was measured in accordance with JIS C2110-1:2016. The results are shown in Table 1.
[0093] [Low molecular weight siloxane content] The obtained heat-conductive silicone rubber composition was placed in a mold of 100 mm × 100 mm × 0.45 mm, and the pressure was adjusted so that the thickness after curing would be 0.45 mm. Then, using a high-pressure press (manufactured by Shoji Iron Works Co., Ltd.), the composition was pressed at 165°C and 100 kgf / cm 2 The mixture was press cured at 40°C for 10 minutes to produce a sheet with a thickness of 0.45 mm. Further, secondary vulcanization (post curing) was performed at 150°C / 1 hour or 200°C / 1 hour, and then cooled to room temperature. A small piece of this sheet was taken and immersed in acetone to extract low molecular weight siloxanes, and the total content (ppm by mass) of diorganocyclopolysiloxanes having 3 to 10 silicon atoms was measured by gas chromatography analysis. The results are shown in Table 1.
[0094] [Strength] The obtained heat-conductive silicone rubber composition was placed in a 100 mm × 100 mm × 2 mm mold, the pressure was adjusted so that the thickness after curing would be 2 mm, and the composition was pressed at 165°C and 100 kgf / cm using a high-pressure press (manufactured by Shoji Iron Works Co., Ltd.). 2 The resulting mixture was press cured at 40°C for 10 minutes to produce a 2 mm thick sheet. It was then post-cured at 150°C for 1 hour or 200°C for 1 hour, and then cooled to room temperature. The tensile strength, elongation at break, and tear strength of the 2 mm thick sheets produced were measured in accordance with JIS K6249:2003. The results are shown in Table 1.
[0095] [Molding covers for heat-generating electronic components] The heat-conductive silicone rubber composition after mixing was transferred to a transfer molding machine (manufactured by PRC Corporation) consisting of a piston, pot, middle mold, and lower mold, and was then molded at 165°C and 100 kgf / cm. 2The molded product was molded by hot pressing at 150°C for 10 minutes. After demolding, the molded product was subjected to secondary vulcanization at 150°C for 1 hour to produce a cover for heat-generating electronic parts. The shape of the cover for heat-generating electronic parts is shown in Figure 1. The dimensions (unit: mm) are also shown in the figure.
[0096] [Crack resistance when molding is installed] The heat-generating electronic component covers produced in Examples 1 to 3 and Comparative Examples 2 and 3 were attached to an electrode (manufactured by Safe Co., Ltd.) measuring 15 mm x 4.5 mm x 20 mm in height, and a voltage of 4.5 kV was applied for 10 seconds to measure the presence or absence of leakage current. If cracks occur during attachment, leakage current will occur. Thirty pieces were measured, and the number of pieces that had cracks is shown in Table 1.
[0097] [Table 1]
[0098] As shown in Table 1, in Examples 1 to 3, the strength and crack resistance during installation of the molded body were good, and the low molecular weight siloxane content was low. In Comparative Example 1, the amount of the heat conductive filler was too large, so a heat conductive silicone rubber composition was not obtained. In Comparative Example 2, the amount of low molecular weight siloxane could not be reduced to the desired amount even after post-cure (150°C for 1 hour), and the tensile strength was poor. On the other hand, in Comparative Example 3, the sheet was embrittled due to the high-temperature post-cure (200°C for 1 hour) for preventing contact failure caused by low molecular weight siloxane, and cutting and cracking occurred during installation and handling of the molded body, resulting in leakage current. In other words, in Comparative Examples 2 and 3, contact failure caused by low molecular weight siloxane cannot be prevented.
[0099] Thus, the thermally conductive silicone rubber composition of the present invention can be cured at low temperatures, and even when a post-cure step is performed at low temperatures, the low molecular weight siloxane content can be sufficiently reduced. Therefore, the thermally conductive silicone rubber composition of the present invention can obtain a sufficient low molecular weight siloxane removal effect even when no post-cure step is performed or when the post-cure step is performed at a low temperature, and can give a cured product (molded product) with high thermal conductivity and excellent strength. In addition, the heat-dissipating molded article made of the cured product molded using this composition can be prevented from becoming embrittled due to high-temperature post-cure. The obtained heat-dissipating molded article has excellent thermal conductivity, strength, and insulation properties, and contains a small amount of low-molecular-weight siloxane, making it easy to mount on electronic components and preventing contact failure.
[0100] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
Claims
1. (A) 100 parts by mass of an organopolysiloxane having an average degree of polymerization of 3,000 to 10,000 and a total content of diorganocyclopolysiloxanes having 3 to 10 silicon atoms of 500 ppm or less, (B) an organopolysiloxane having an average degree of polymerization of 2 to 2,000 and having alkenyl groups only at both molecular chain terminals: 10 to 100 parts by mass, (C) thermally conductive filler: 500 to 2,700 parts by mass, and (D) Curing agent: effective amount A thermally conductive silicone rubber composition comprising:
2. moreover (E) (E1) The following formula (1): R 2 b R 3 c Si(OR 4 ) 4-b-c (1) (In the formula, R 2 are independently alkyl groups having 6 to 15 carbon atoms; R 3 are independently alkyl groups having 1 to 5 carbon atoms; R 4 are independently an alkyl group having 1 to 4 carbon atoms, b is an integer of 1 to 3, and c is 0, 1 or 2, with the proviso that b+c is 1 to 3. and an alkoxysilane represented by the formula: (E2) The following formula (2): 【Chemistry 1】 (In the formula, R 5 are independently an alkyl group having 1 to 4 carbon atoms, and d is an integer of 5 to 100. Dimethylpolysiloxane having one end blocked with a trialkoxysilyl group, represented by 2. The thermally conductive silicone rubber composition according to claim 1, characterized in that the composition contains 0.01 to 30 mass % of the total amount of the organosilicon compound components, of one or more selected from the following:
3. 3. The thermally conductive silicone rubber composition according to claim 1, wherein the thermally conductive silicone rubber composition has a plasticity of 100 to 800 as measured by a method in accordance with JIS K6249:2003.
4. A cured product obtained by curing the thermally conductive silicone rubber composition according to any one of claims 1 to 3.
5. A heat-dissipating molded article comprising the cured product according to claim 4, wherein the cured product has a thermal conductivity of 1.5 W / m·K or more.
6. The heat-dissipating molded article according to claim 5, wherein the cured product has a type A durometer hardness according to JIS K6253-3:2012 in the range of 60 to 96.
7. 7. A heat-radiating molded article according to claim 5 or 6, characterized in that the withstand voltage of the cured article is 4.5 kV or more when the thickness of the cured article is 0.45 mm.
8. A heat-dissipating molded body according to any one of claims 5 to 7, characterized in that the content of diorganocyclopolysiloxane having 3 to 10 silicon atoms after post-curing at 150°C for 1 hour is 100 ppm or less.
Citation Information
Patent Citations
JP1982002666U
Heat dissipating sheet
JP1997199880A
Heat-conductive silicone rubber composition
JP2011153252A
Thermally conductive silicone composition and cured product of the same
JP2015071662A
Method for manufacturing reinforcement layer-including thermally conductive silicone composite sheet
JP2021089908A