Coated Cutting Tools
The (Ti, Al, Cr, Si)N layer on cutting tools, deposited via HIPIMS, addresses the stability and wear issues of existing tools by enhancing thermal stability and wear resistance, resulting in improved tool life for machining hard materials.
Patent Information
- Application Number
- JP2021577463
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-28
- Filing Date
- 2020-06-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-06-24
AI Technical Summary
Existing cutting tools for hard materials like hardened steel and cooled cast iron lack sufficient high-temperature stability and wear resistance, leading to rapid tool degradation during machining.
A coated cutting tool with a (Ti, Al, Cr, Si)N layer deposited using High Power Impulse Magnetron Sputtering (HIPIMS) technology, featuring a cubic phase with multiple unit cell lengths and specific compositional ranges, enhancing hardness, thermal stability, and adhesion to the substrate.
The (Ti, Al, Cr, Si)N layer provides improved high-temperature stability and extended tool life, reducing wear and maintaining performance under harsh cutting conditions.
Smart Images

Figure 0007577082000005 
Figure 0007577082000006 
Figure 0007577082000007
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated cutting tool that is particularly suitable for cutting particularly hard work materials (iso-H materials), the cutting tool having a coating that includes a (Ti,Al,Cr,Si)N layer. [Background technology]
[0002] Generally, cutting tools for metal machining include a substrate of a hard material, such as a cemented carbide, and a thin wear-resistant coating deposited on the surface of the substrate. Examples of cutting tools are cutting inserts, drills or end mills.
[0003] The coating should ideally have a high hardness, but at the same time be tough enough to withstand the harshest cutting conditions possible.
[0004] Depending on the workpiece material to be cut, there are different demands on the cutting tool. In this connection, the properties of the coating on the cutting tool are very important.
[0005] One group of workpiece materials are hardened materials such as hardened steel, cold cast iron and white cast iron. This group of materials is classified as iso-H materials. They are particularly hard and difficult to cut because of the high cutting forces required. Materials belonging to the iso-H group generate a lot of heat during the cutting process. They also have a high level of wear on the cutting edge.
[0006] State of the art coatings used on cutting tools for machining iso-H materials are generally (Ti,Al)N coatings deposited by PVD techniques, which have high hardness and high toughness but lack sufficient high temperature stability.
[0007] US 2015 / 0232978 A1 discloses a coated cutting tool having a coating comprising multiple sublayers of (Ti,Al)N, (Al,Cr)N and (Ti,Si)N, with an average composition of about Ti 0.45 Al 0.40 Cr 0.10 S0.05 N. The coating is deposited by cathodic arc evaporation.
[0008] EP 3434809 A1 discloses a coated cutting tool having a (Ti,Al,Cr,Si)N coating comprising multiple sub-layers of (Ti,Si)N and (Al,Cr)N. The coating is deposited by cathodic arc evaporation. Summary of the Invention
[0009] It is an object of the present invention to provide a coated cutting tool having excellent high temperature stability and improved tool life, especially when cutting iso-H workpiece materials. [Brief description of the drawings]
[0010] [Figure 1] 1 shows an electron diffraction image of a (Ti,Al,Cr,Si)N layer according to the present invention. [Diagram 2] 1 shows the radial intensity distribution curve of an electron diffraction image of a (Ti,Al,Cr,Si)N layer according to the present invention. [Diagram 3] 1 shows the average radial intensity distribution curve of an electron diffraction image of a (Ti,Al,Cr,Si)N layer according to the present invention. [Figure 3a] 1 shows an enlarged portion of the average radial intensity distribution curve of an electron diffraction image of a (Ti,Al,Cr,Si)N layer according to the present invention. [Figure 4] FIG. 2 shows the X-ray θ-2θ diffractogram of a (Ti,Al,Cr,Si)N layer according to the present invention for the cubic (2 0 0) peak. [Diagram 5] FIG. 1 shows the X-ray θ-2θ diffractogram of a HIPIMS deposited (Ti,Al)N layer for the cubic (2 0 0) peak. [Figure 6] Figure 2 shows the X-ray θ-2θ diffractogram of an arc-deposited (Ti,Al,Cr,Si)N layer for the cubic (2 0 0) peak. [Figure 7] 4 shows the X-ray θ-2θ diffractograms of the (Ti,Al)N layers as deposited and after different heat treatment temperatures. [Figure 8]FIG. 1 shows X-ray θ-2θ diffractograms of a (Ti,Al,Cr,Si)N layer according to the invention as deposited and after different heat treatment temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] There is provided herein a coated cutting tool comprising a substrate having a coating comprising a layer of (Ti,Al,Cr,Si)N, the (Ti,Al,Cr,Si)N comprising a cubic phase having a plurality of unit cell lengths.
[0012] Therefore, in this specification, Ti x Al y Cr z S v Disclosed is a coated cutting tool comprising a substrate having a coating including a layer of N, where x is 0.30-0.50, y is 0.25-0.45, z is 0.05-0.15, v is 0.10-0.20, and x+y+z+v=1; the coated cutting tool comprises a cubic phase including a distribution of unit cell lengths in the range of 3.96-4.22 Å for a unit cubic cell, and includes a plurality of intensity maxima in an average radial intensity profile of an electron diffraction pattern within the unit cell length range of 3.96-4.22 Å.
[0013] The average radial intensity profile is obtained from the electron diffraction pattern by taking the average of all the intensities in the diffraction pattern that have the same distance (radius) to the center of the diffraction pattern. The average intensity is then plotted as a function of radius.
[0014] The presence of multiple unit cell lengths results in multiple lattice spacings for a particular (hkl) plane. As an example, the (Ti,Al,Cr,Si)N layer of the present invention comprises a general cubic crystal structure with multiple lattice spacings that give the (2 0 0) reflection.
[0015] The presence of multiple unit cell lengths can be detected by XRD or TEM analysis (electron diffraction). For example, in the radial average intensity profile in electron diffraction, the (2 0 0) reflection intensity is distributed such that three maxima are found in one embodiment (see FIG. 2). The maxima in this embodiment of the invention correspond to d-spacings of 2.01, 2.04 and 2.07 Å. In embodiments of the invention, multiple maxima of other reflections such as (1 1 1), (2 2 0) and (2 2 2) may also be present.
[0016] In θ-2θ XRD analysis, the presence of multiple unit cell lengths affects the shape of the diffraction peak for a particular (hkl) reflection due to the presence of different lattice spacings that cause diffraction.
[0017] In one embodiment, Ti x Al y Cr z S v The N layer contains a cubic phase that contains two to four intensity maxima in the intensity profile of the electron diffraction pattern within the unit cell length range of 3.96 to 4.22 Å.
[0018] In one embodiment, Ti x Al y Cr z S v The N layer contains a cubic phase with three intensity maxima in the intensity profile of the electron diffraction pattern within the unit cell length range of 3.96-4.22 Å, the maxima being located in the ranges of 4.00-4.04 Å, 4.06-4.10 Å, and 4.12-4.16 Å, respectively.
[0019] Ti x Al y Cr z S v In the N layer, x is preferably 0.35 to 0.45, y is preferably 0.30 to 0.40, z is preferably 0.08 to 0.13, v is preferably 0.12 to 0.18, and x+y+z+v=1.
[0020] In one embodiment, Ti x Aly Cr z S v The N layer has a hardness of 3300 to 3700 HV, preferably 3500 to 3700 HV.
[0021] In one embodiment, Ti x Al y Cr z S v The N layer has a reduced Young's modulus of ≧320 GPa, preferably ≧340 GPa.
[0022] In one embodiment, Ti x Al y Cr z S v The N layer has a residual stress of -3 to -6 GPa.
[0023] In one embodiment, Ti x Al y Cr z S v The N layer has a thermal conductivity of less than 3 W / mK, preferably 1.8 to 2.8 W / mK.
[0024] In the case of wear resistant coatings on cutting tools, low thermal conductivity is beneficial to keep the heat load from the cutting process on the tool substrate as low as possible.
[0025] Ti x Al y Cr z S v The thickness of the N layer is suitably 0.5 to 6 μm, preferably 1.5 to 4 μm.
[0026] In one embodiment, the substrate and Ti x Al y Cr z S v Between the layers of Ti and N there is at least one metal nitride layer, suitably a nitride of one or more of Ti, Cr and Zr, optionally together with Al. Preferably the metal nitride layer is a layer of TiN or (Ti,Al)N. x Al y Crz S v It acts as an adhesion enhancing layer between the N layer and the substrate.
[0027] Substrate and Ti x Al y Cr z S v The thickness of the at least one metal nitride layer between the layers of N is suitably 0.1 to 3 μm, preferably 0.5 to 2 μm.
[0028] The substrate of the coated cutting tool may be of any type common in the field of cutting tools for metal machining, suitably selected from cemented carbide, cermet, cBN, ceramic, PCD and HSS.
[0029] In one preferred embodiment, the substrate is a cemented carbide.
[0030] In one preferred embodiment, the coated cutting tool comprises Ti x Al y Cr z S v The present invention relates to a method for producing a cubic phase comprising: a substrate of cemented carbide having a coating including a 0.5-6 μm layer of N, wherein x is 0.30-0.50, y is 0.25-0.45, z is 0.05-0.20, and v is 0.10-0.20, where x+y+z+v=1, and the substrate and Ti include a cubic phase including a distribution of unit cell lengths within the range of 3.96-4.22 Å for the unit cubic cell; x Al y Cr z S v Between the N layers there is a 0.1-3 μm layer of (Ti,Al)N.
[0031] The coated cutting tool can be a coated cutting insert such as a coated cutting insert for turning or a coated cutting insert for milling, or a coated cutting insert for drilling, or a coated cutting insert for thread cutting, or a coated cutting insert for parting and grooving. The coated cutting tool can also be a coated solid tool such as a solid drill, end mill, or tap.
[0032] Tix Al y Cr z S v The layer of N is preferably a sputter deposited layer, most preferably a HIPIMS (High Power Impulse Magnetron Sputtering) deposited layer.
[0033] Ti x Al y Cr z S v When depositing N, it is preferable to use a target containing all of the elements Ti, Al, Cr and Si.
[0034] The method of making a coated cutting tool disclosed herein includes providing a substrate and depositing, preferably in HIPIMS mode, a Ti x Al y Cr z S v and depositing a layer of N, where x is between 0.30 and 0.50, y is between 0.25 and 0.45, z is between 0.05 and 0.20, and v is between 0.10 and 0.20, and x+y+z+v=1. When using HIPIMS mode, the peak power density is suitably >0.2 kW / cm. 2 , preferably >0.4kW / cm 2 , most preferably >0.7kW / cm 2 , and the peak current density is appropriately >0.2A / cm 2 , preferably >0.3A / cm 2 , most preferably >0.4A / cm 2 and the maximum peak voltage is suitably 300 to 1500V, preferably 400 to 900V.
[0035] The substrate temperature during deposition is suitably between 350 and 600°C, preferably between 400 and 550°C.
[0036] The DC bias voltage used in the HIPIMS method is suitably 20 to 100 V, or 30 to 80 V (negative bias).
[0037] The average power density in the HIPIMS method is appropriately 20 to 110 W cm-2 , preferably 30 to 90 W cm -2 It is.
[0038] The pulse length used in the HIPIMS method is suitably 2 μs to 200 ms, preferably 10 μs to 100 ms.
[0039] The deposition process preferably uses one or more targets of TiAlCrSi, followed by targets of the same composition, in one embodiment three targets (one row) are used.
[0040] As is common in PVD deposition of metal nitrides, there may be a slight over-stoichiometry or slight under-stoichiometry of nitrogen in the metal nitride. Thus, the nitrogen content relative to the total metal content in (Ti,Al,Cr,Si)N may be completely outside the 1:1 stoichiometric range and may be a few atomic percentage units above or below 50 atomic %, such as 40-60 atomic % or 50-58 atomic %.
[0041] method XRD Phase Analysis: X-ray diffraction patterns for phase analysis were acquired in the grazing incidence mode (GIXRD) of a diffractometer by Panalytical (Empyrean). CuKα radiation with a line focus was used for the analysis (voltage 40 kV, current 40 mA). The incident beam was defined by a 2 mm mask and a 1 / 8° divergence slit in addition to an X-ray mirror generating a parallel X-ray beam. The lateral divergence was controlled by a Soller slit (0.04°). A 0.18° parallel plate collimator combined with a proportional counter (0D-detector) was used in the diffracted beam path. The measurements were performed in the grazing incidence mode (omega = 1°). The 2θ range was about 28-45° with a step size of 0.03° and a counting time of 10 s. For the XRD line profile analysis, a reference measurement (using LaB6 powder) was performed with the same parameters as above to correct for instrumental broadening.
[0042] TEM analysis Transmission electron microscopy data (selected area diffraction patterns and dark field images) were acquired using a FEI (FEI TITAN80-300) transmission electron microscope. A high voltage of 300 kV was used for the analysis.
[0043] Where electron diffraction experiments are referred to herein, these are TEM measurements made with parallel illumination. Regions of interest were selected with a selected area aperture.
[0044] A FIB (focused ion beam) lift-out was used for TEM sample preparation. For final polishing, the Ga ion beam was adjusted to a current of 200 pA at 5 kV.
[0045] A cross section of the coating was analyzed perpendicular to the surface of the coating.
[0046] Residual Stress: A Seifert / GE diffractometer (PTS3003) was used to analyze the residual stress in the coating. A CuK α X-ray stress analysis was performed using a sin 2 The stress analysis was performed according to the Ψ method. The {111} reflection of cubic TiAlN was used as the stress distribution, s1=-4,910 10 -7 MPa -1 and 0,5s2=2,780·10 -6 MPa -1 The stress was calculated by applying the χ mode in which the χ axis is tilted from -60° to 60°, and the stress was calculated by sin 2 ψ was measured at equidistant intervals.
[0047] Vickers hardness: The Vickers hardness was measured by nanoindentation (load-depth graph) using a Picodentor HM500 from Helmut Fischer GmbH (Sindelfingen, Germany). For the measurements and calculations, the evaluation algorithm of Oliver and Pharr was applied, a Vickers diamond specimen was pressed into the layer and the force-path curve was recorded during the measurement. The maximum load used was 15 mN (HV 0.0015), the load increase and load decrease times were 20 s each, and the hold time (creep time) was 10 s. The hardness was calculated from this curve.
[0048] Reduced Young's Modulus The reduced Young's modulus (equivalent reduced modulus of elasticity) was determined by nanoindentation (load-depth graph) as described for determining Vickers hardness.
[0049] Thermal Conductivity: A time domain thermoreflectance (TDTR) method was used, which has the following characteristics:
[0050] 1. A laser pulse (pump) is used to locally heat the sample.
[0051] 2. Depending on the thermal conductivity and heat capacity, heat energy is transferred from the sample surface to the substrate. The temperature of the surface decreases with time.
[0052] 3. The fraction of the laser that is reflected depends on the surface temperature. A second laser pulse (the probe pulse) is used to measure the temperature drop of the surface.
[0053] 4. Thermal conductivity can be calculated by using mathematical models. (See DG Cahill, Rev. Sci. Instr. 75, 5119 (2004)).
[0054] Thickness: The layer thickness was determined by carrot grinding, whereby a steel ball with a diameter of 30 mm was used to grind the dome-shaped recess, and the ring diameter was measured from which the layer thickness was calculated. The layer thickness measurements on the rake face (RF) of the cutting tool were made at a distance of 2000 μm from the corner, and on the flank face (FF) at the center of the flank. EXAMPLES
[0055] Example 1 (present invention): Composition Ti 0.40 Al 0.60 (Ti,Al)N layers from a target containing were deposited on WC-Co based substrates, milling type cutting inserts and also flat inserts (to facilitate analysis of the coating), using HIPIMS mode in an Oerlikon Balzers instrument using S3p technology.
[0056] The substrate had a composition of 8 wt % Co and balance WC.
[0057] The deposition process was carried out in HIPIMS mode using the following process parameters: Average power: 9.06kW Pulse on time: 7.56ms Temperature: 450℃ Target size: circular, 15cm diameter Target material: Ti40Al60 Total pressure: 0.6Pa Argon pressure: 0.42Pa Bias potential: -40V
[0058] A layer thickness of approximately 1 μm was deposited.
[0059] A layer of (Ti,Al,Cr,Si)N was then deposited on the previously deposited (Ti,Al)N layer using a single target with the composition Ti / Al / Cr / Si 40 / 35 / 10 / 15 (at.%).
[0060] The deposition process was carried out in HIPIMS mode using the following process parameters: Average power per target: 4.8kW Peak pulse power: 60kW Maximum peak voltage: 640V Peak pulse current: 92A Pulse on time: 2ms Temperature: 450℃ Target size: circular, 15 cm diameter (effective plasma area was 1 / 3 of the target area) Target material: Ti40Al35Cr10Si15 Total pressure: 0.62Pa Argon pressure: 0.42Pa Bias potential: -50V (-40V for the first 10 minutes)
[0061] A layer thickness of approximately 2.5 μm was deposited.
[0062] The resulting coated cutting tool is called "Sample 1 (present invention)".
[0063] The content of each element in the (Ti, Al, Cr, Si)N layer was analyzed by energy dispersive X-ray spectroscopy (EDS), and the results are shown in Table 1. TIFF0007577082000001.tif19170
[0064] Example 2 (reference): Composition Ti 0.40 Al 0.60 (Ti,Al)N layers from a target containing were deposited on WC-Co based substrates, milling type cutting inserts and also flat inserts (to facilitate analysis of the coating), using HIPIMS mode in an Oerlikon Balzers instrument using S3p technology.
[0065] The substrate had a composition of 8 wt % Co and balance WC.
[0066] The deposition process was carried out in HIPIMS mode using the following process parameters: Average power: 9.06kW Pulse on time: 7.56ms Temperature: 450℃ Target size: circular, 15cm diameter Target material: Ti40Al60 Total pressure: 0.6Pa Argon pressure: 0.42Pa Bias potential: -40V
[0067] A layer thickness of approximately 3 μm was deposited.
[0068] The resulting coated cutting tool was called "Sample 2 (Reference)".
[0069] Example 3 (reference): Composition Ti 0.33 Al 0.67 (Ti,Al)N layers from a target containing were deposited on WC-Co based substrates, which were milling type cutting inserts and also flat inserts (to facilitate analysis of the coating).
[0070] The substrate had a composition of 8 wt % Co and balance WC.
[0071] The deposition was carried out in an Innova PVD apparatus from the manufacturer Oerlikon-Balzers. The process parameters were as follows: -Target Ti33Al67 -Total pressure: 1Pa N2 -Deposition temperature: 600℃ -DC Bias: -100V -Arc current: 140A -Table (substrate) rotation: 60% -Magnet configuration: Mag10 A layer thickness of approximately 3 μm was deposited.
[0072] The resulting coated cutting tool was called "Sample 3 (Reference)".
[0073] Example 4 (Reference): A (Ti,Al,Cr,Si)N coating according to US 2015 / 023978 was applied to a substrate having a thickness of about Ti 0.50 Al 0.50 N, Al 0.70 Cr 0.30 N and Ti 0.85 S 0.15 N nano multilayers of Ti 0.50 Al 0.50 Target, Al 0.70 Cr 0.30 Target and Ti 0.85 S 0.15 The deposition was by cathodic arc evaporation from a target.
[0074] The coating is made of alternating multilayers AB, where layer A itself is made up of sublayers Al, each about 7 nm thick. 0.70 Cr 0.30 N and Ti 0.85 S 0.15 The thickness of A is about 56 nm.
[0075] Layer B is a Ti layer having a thickness of about 50 nm. 0.50 Al 0.50 This is the N layer.
[0076] The layer sequence AB is repeated 20 times.
[0077] The total coating thickness is about 2 μm.
[0078] The average composition of the (Ti,Al,Cr,Si)N coating is about Ti 0.45 Al 0.40 Cr 0.10 S 0.05 It's N.
[0079] The coatings were deposited on WC-Co based substrates, which were milling type cutting inserts and also flat inserts (to facilitate analysis of the coating). The substrates had a composition of 8 wt.% Co and balance WC. The deposition was carried out in an Innova PVD machine by the manufacturer Oerlikon-Balzers.
[0080] Layer A: 2xTi0.85 S 0.15 N and 2xAl 0.70 Cr 0.30 N (two targets each in the deposition chamber), and the processing conditions are as follows: -N2 pressure: 4Pa -Temperature: 550℃ -Arc current: 160A -DC Bias: -60V -Rotation: 30% -Deposition time: 2 minutes 40 seconds
[0081] Layer B: 2xTi 0.50 Al 0.50 N (two targets in the deposition chamber), processing conditions are as follows: -N2 pressure: 4Pa -Temperature: 550℃ -Arc current: 160A -DC Bias: -120V -Rotation: 30% -Deposition time: 5 minutes 20 seconds Magnet configuration: Ti 0.85 S 0.15 : Mag6, 0.5A Ti 0.50 Al 0.50 : Mag6, 2A Al 0.70 Cr 0.30 : Mag14, 0.5A
[0082] In total [AB] has 20 repetitions.
[0083] The resulting coated cutting tool was called "Sample 4 (Reference)".
[0084] Example 5 (Analysis): Electron diffraction (TEM) analysis was carried out on Sample 1 (the present invention), and Figure 1 shows the resulting electron diffraction pattern.
[0085] FIG. 2 shows the radial intensity distribution profile along line AB of the electron diffraction pattern of sample 1 (invention).
[0086] FIG. 3 shows the average radial intensity distribution profile of the electron diffraction pattern of sample 1 (invention).
[0087] FIG. 3a shows a magnified image of the marked portion corresponding to the cubic (2 0 0) reflection in FIG.
[0088] The average intensity profile of the (2 0 0) reflection is seen to reveal three preferred maxima, implying the presence of multiple preferred d-spacings in the cubic phase, corresponding to the presence of multiple preferred unit cell lengths in (Ti,Al,Cr,Si)N for sample 1 (invention).
[0089] Samples 1, 2 and 4 were further subjected to XRD θ-2θ analysis.
[0090] FIG. 4 shows an X-ray θ-2θ diffraction diagram of Sample 1 (the present invention) in the 2θ range of 40 to 45 degrees, showing a cubic (2 0 0) peak.
[0091] FIG. 5 shows an X-ray θ-2θ diffraction diagram of sample 2 (the present invention), a HIPIMS-deposited (Ti,Al)N layer, in the 2θ range of 40 to 45 degrees showing a cubic (2 0 0) peak.
[0092] Figure 6 shows the X-ray θ-2θ diffractogram of sample 4 (reference), an arc-deposited (Ti,Al,Cr,Si)N layer, in the 2θ range 40-45 degrees exhibiting the cubic (2 0 0) peak.
[0093] It can be seen that the peak for sample 1 (invention) is highly asymmetrical, indicating the presence of multiple preferred d-spacings for the (2 0 0) reflection, whereas the peaks for samples 2 and 4 are highly symmetrical.
[0094] Residual stress was also measured on sample 1 (invention) and showed a value of -5.1±0.3 GPa, ie compressive stress.
[0095] Hardness measurements (15 mN load) were carried out on the flank faces of the coated tools to determine the Vickers hardness and the reduced Young's modulus (EIT), and the results are shown in Table 2. For characterization of the toughness (Young's modulus) of the coatings, Vickers indentation was carried out with a load of 500 mN and cross sections were prepared. TIFF0007577082000002.tif31170
[0096] Finally, for the (Ti,Al,Cr,Si)N layer of sample 1 (invention), the thermal conductivity was determined to be 2.4 W / mK.
[0097] Example 6 (High Temperature Stability): The high temperature stability of the HIPIMS deposited (Ti,Al,Cr,Si)N layer according to the invention present in the coating of sample 1 (invention) was compared with that of sample 3 (reference), i.e. a HIPIMS deposited (S3p technology) (Ti,Al)N coating. The (Ti,Al,Cr,Si)N coating was deposited according to the method of example 1. However, in this coating no inner (Ti,Al)N layer was deposited.
[0098] To analyze the high temperature stability, the coated inserts were placed in a furnace and subjected to an annealing procedure. The temperature was increased to the maximum temperature during one hour and then maintained at that temperature for one hour. There was an argon pressure of about 2 bar in the furnace tube. After the heat treatment there was no active cooling. The experimental equipment was from the manufacturer Nabertherm.
[0099] Hardness measurements were performed by nanoindentation to determine the Martens hardness (GPa). The as-deposited (Ti,Al)N coating had a hardness of 18.7 GPa, whereas the as-deposited (Ti,Al,Cr,Si)N coating had a hardness of 16.4 GPa. Annealing at 1000 °C for 1 h changed the situation. The hardness of the (Ti,Al)N coating decreased to a value of 16.2 GPa, whereas the hardness of the (Ti,Al,Cr,Si)N coating increased slightly to a value of 17.5 GPa. Thus, the (Ti,Al)N coating degrades at 1000 °C, whereas the (Ti,Al,Cr,Si)N does not.
[0100] The high temperature stability of the (Ti,Al,Cr,Si)N coatings is also seen in the XRD analysis. XRD measurements (θ-2θ analysis) were performed on both the as-deposited (Ti,Al)N coatings and the (Ti,Al,Cr,Si)N coatings after annealing at 900°C, 1000°C and 1100°C. Figure 7 shows the diffractogram of the (Ti,Al)N coating and Figure 8 shows the diffractogram for (Ti,Al,Cr,Si)N. There are clear differences between the diffractograms of the different coatings. For example, a splitting of the (2 0 0) peak of TiAlN is observed at 900°C and 1000°C (see Figure 7). By adding Cr and Si, the decomposition is shifted to higher temperatures, i.e., 1100°C (see Figure 8). Also, the (Ti,Al)N coatings obtain the hexagonal AlN (1 0 0) peak at 1100°C, which is not obtained for the (Ti,Al,Cr,Si)N according to the invention.
[0101] Example 7: Cutting test of Sample 1 (invention) and Sample 3 (reference): Sample 1 (invention) and the reference sample were tested in a milling test to measure the interface flank wear. The cutting conditions are summarized in Table 3. Cutting conditions: TIFF0007577082000003.tif53170
[0102] In this test, maximum wear was observed on the flank edge. Two edges of each coating were tested and the average length of cut for each is shown in Table 4. TIFF0007577082000004.tif53170
[0103] It can be concluded that sample 3 (reference) performs much worse than sample 1 (invention).
[0104] Cutting test of sample 4 (reference): Sample 4 (reference) was tested in a separate test round using the same cutting test parameters as in the above tests of Samples 1 and 3, including the same workpiece material. The test had to be stopped already after a cutting length of 76 m due to heavy wear, with an observed VBmax of 0.25 mm.
[0105] It is concluded that sample 4 (reference) performs much worse than sample 1 (invention) tested in the same test described above.
Claims
1. Ti x A y Cr z S v 1. A coated cutting tool comprising a substrate having a coating comprising a layer of N, wherein x is 0.30 to 0.50, y is 0.25 to 0.45, z is 0.05 to 0.15, v is 0.10 to 0.20, and x+y+z+v=1, the coated cutting tool comprising a cubic phase comprising a distribution of unit cell lengths in the range of 3.96 to 4.22 Å for a unit cubic cell, and comprising three intensity maxima in an average radial intensity profile of an electron diffraction pattern within the unit cell length range of 3.96 to 4.22 Å.
2. A coated cutting tool as described in claim 1, wherein three intensity maxima in the intensity profile of the electron diffraction pattern are located within the ranges of 4.00 to 4.04 Å, 4.06 to 4.10 Å and 4.12 to 4.16 Å, respectively.
3. Ti x A y Cr z S v The coated cutting tool according to claim 1 or 2, wherein the N layer has a hardness of 3300 to 3700 HV.
4. Ti x A y Cr z S v A coated cutting tool according to any one of claims 1 to 3, wherein the layer of N has a reduced Young's modulus of ≧320 GPa.
5. Ti x A y Cr z S v The coated cutting tool according to any one of claims 1 to 4, wherein the layer of N has a residual stress of -3 to -6 GPa.
6. Ti x A y Cr z S v The coated cutting tool according to any one of claims 1 to 5, wherein the layer of N has a thermal conductivity of less than 3 W / mK.
7. Ti x A y Cr z S v The coated cutting tool according to any one of claims 1 to 6, wherein the thickness of the N layer is 0.5 to 6 µm.
8. Substrate and Ti x A y Cr z S v A coated cutting tool according to any one of claims 1 to 7, wherein at least one metal nitride layer is present between the layers of N.
9. Substrate and Ti x A y Cr z S v 9. The coated cutting tool of claim 8, wherein there are layers of (Ti,Al)N between layers of N.
10. A coated cutting tool according to any one of claims 1 to 9, wherein the substrate is selected from cemented carbide, cermet, cBN, ceramic, PCD and HSS.
11. Ti x A y Cr z S v A coated cutting tool according to any one of claims 1 to 10, wherein the layer of N is a HIPIMS (High Power Impulse Magnetron Sputtering) deposited layer.
Citation Information
Patent Citations
Special coated tool for processing stainless steel, and preparation method thereof
CN108103465A
PVD method for depositing coatings onto objects and coated objects manufactured therefrom
JP2013505358A
Tools with TiAlCrSiN coating applied by PVD
JP2015530270A