Laminated glass including an interlayer film to which ink has been applied
By applying ink with specific pH and ion concentrations on polyvinyl acetal interlayers without direct glass contact, the issues of adhesion and optical distortions in laminated glass production are resolved, achieving efficient and high-quality colored laminated glass.
Patent Information
- Application Number
- JP2022502943
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-18
- Filing Date
- 2020-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-09
AI Technical Summary
Current methods for producing colored laminated glass using polyvinyl acetal interlayers face issues such as adhesion problems between the glass plate and interlayer, incompatibility with ink materials, and undesirable optical distortions due to multiple layers, leading to inefficiencies in production and quality.
The use of an ink with a pH greater than or equal to 7 and limited concentrations of potassium, magnesium, and calcium ions on a polyvinyl acetal interlayer film, applied without direct contact with the glass, enhances adhesion and reduces interference with the interlayer material, allowing for improved laminated glass production.
This approach results in laminated glass with enhanced adhesion, reduced optical distortions, and improved production efficiency, meeting automotive and architectural requirements for opacity and color without compromising mechanical properties.
Smart Images

Figure 0007577110000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated glass comprising two glass sheets bonded together by an adhesive interlayer film having a particular ink applied to at least one surface of the interlayer. [Background technology]
[0002] Laminated glass has advantageous characteristics such as penetration resistance and fragment retention after breakage and is used in many applications in the automotive and building industries. Polyvinyl acetal, especially polyvinyl butyral (PVB), is a material frequently used between the layers of laminates.
[0003] In the building industry, glazings of various colors are increasingly required, especially for decorative purposes and shading against excess sunlight. Currently, pigments are blended into PVB and then co-extruded to obtain colored PVB films. This technology has several drawbacks. For example, PVB film manufacturers must blend PVB resin with each individual color separately, then extrude the individual colored films, and then clean the entire production line to remove traces of pigment before using them in clear or other colored films. Due to the large number of different colors possible and the increasing demand for specific colors, e.g., colors of specific corporate designs, film manufacturers must produce a large number of different colors and store them (most of them in refrigerated conditions) until sale. As a solution to this challenge, it is known to stack several sheets of PVB film extruded with different base colors to create a laminate of a specific color. However, applying several layers of base colors can lead to unacceptable thicknesses of the glass laminate. Furthermore, stacking different colored PVB layers can result in undesirable optical distortion effects and problems in the degassing process before the lamination step.
[0004] In the automotive industry, at least one of the two glass panes in a windshield is typically provided with an opaque frame to protect the sealant or adhesive that mechanically connects the windshield to the chassis from UV radiation, and sometimes the other glass pane is provided with such an opaque frame to hide electrical connections from view.
[0005] The current standard process in the industry is to use sintered enamel on one of the glass surfaces, which entails some drawbacks due to the high processing temperatures. WO 2019 / 038043 A1 describes laminated glass with non-transparent areas that are coated or printed onto the PVB interlayer film using ink. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2019 / 038043 Summary of the Invention [Problem to be solved by the invention]
[0007] However, it has now surprisingly been found that many commercially available inks have certain drawbacks in the lamination process, since their application to the interlayer film can result in adhesion problems between the glass sheets and the interlayer and / or incompatibility with the polyvinyl acetal interlayer material.
[0008] An object of the present invention was therefore an improved laminated glass, using, for example, a more economical process in terms of time and / or costs, a more flexible process, and / or a laminated glass having improved properties, in particular improved adhesion. [Means for solving the problem]
[0009] These and other problems are solved by the present invention.
[0010] The present invention relates to a laminated glass obtained by laminating between two glass sheets at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, in which film A comprises on at least one surface an area in which an ink has been applied (or painted) to the surface, the pH value of the ink being equal to or greater than 7 before its application. Preferably, the pH of the ink is above 7.5, more preferably above 8.0, even more preferably above 8.5. The pH of the ink is also preferably between 7 and 12, more preferably between 7.5 and 10, most preferably between 8 and 9 or less.
[0011] The pH value shall be determined by standard method DIN 19268:2007-05.
[0012] The invention also provides a laminated glass obtained by laminating, between two glass panes, at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, in which film A comprises, on at least one surface, an area in which an ink has been applied to the surface, and in which, before its application, the content of potassium, magnesium or calcium ions in the ink is less than or equal to 200 mg / l.
[0013] The concentrations of ions will be determined by inductively coupled plasma optical emission spectroscopy after sample preparation by microwave digestion per EPA Method 3052.
[0014] In the context of the present invention, the concentrations of the components in the ink are given as the concentrations before application of the ink to the surface of film A. The term "pre-application" therefore refers to the state of the ink before it is applied to at least one surface of film A. [Brief description of the drawings]
[0015] [Figure 1]FIG. 1 shows a preferred embodiment of the laminated glass structure of the present invention, where a and b refer to the two glass sheets, c refers to film A, d refers to the surface area of film A where ink has been applied, and e refers to optional film B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferably, the laminated glass further comprises at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB between the two glass sheets, and at least one surface of film A to which the ink is applied faces film B. Thus, the ink does not directly contact the glass sheets, to reduce possible adhesion problems between the ink and the glass surface.
[0017] Surprisingly, the inventors have found that certain components of commercially available inks interfere with adhesion between the polyvinyl acetal interlayer and the glass surface, even when the surface to which the ink is applied is not in direct contact with the glass surface, for example, when the ink is applied to a surface that is in contact with another polyvinyl acetal surface, particularly when the ink is sandwiched between film A and film B. Without wishing to be bound by theory, it is believed that those components from the ink that interfere with adhesion migrate through the polyvinyl acetal to the glass surface. Such a diffusion process is believed to be facilitated by small amounts of molecules, such as certain organic acids, that are generated in small amounts by hydrolysis of plasticizer molecules. For example, if film A and film B contain different amounts of plasticizer, the amount of plasticizer equilibrates during and after lamination. It is believed that this migration of plasticizer and its cleavage products aids in the diffusion of ink components that affect adhesion.
[0018] It is known that alkali and alkaline earth ions, especially calcium, magnesium and potassium salts, have a significant effect on the adhesion of polyvinyl acetal films to glass surfaces. On the other hand, many commercially available inks contain significant amounts of alkali and / or alkaline earth ions. The ions are either introduced intentionally, for example as counterions of the ink's components, or unintentionally as impurities of one of the components, for example as an ionic load of the water used as the main solvent in aqueous inks.
[0019] By using an ink having a concentration of these cations of 200 mg / l or less, the adhesion is improved. Preferably, the concentrations of potassium ions, magnesium ions and calcium ions in the ink are 200 mg / l or less, more preferably 100 mg / l or less, even more preferably 50 mg / l or less, specifically 10 mg / l or less. In the case of potassium, the concentration in the ink is preferably 20 mg / l or less, more preferably 10 mg / l or less, particularly 2.5 mg / l or less. In the case of magnesium, the concentration in the ink is preferably 50 mg / l or less, more preferably 25 mg / l or less, particularly 10 mg / l or less. In the case of calcium, the concentration in the ink is preferably 250 mg / l or less, more preferably 100 mg / l or less, most preferably 50 mg / l or less, particularly 10 mg / l or less.
[0020] There is no lower limit to the concentration of these ions in the ink, except for the minimum concentration that is technically achievable.
[0021] The ink according to the invention is in either liquid or paste form and contains pigments and / or dyes. Suitable pigments and dyes include carbon black, iron oxides, spinel pigments, organic colored pigments or dyes (diazo dyes, phthalocyanines, perylenes, anthraquinones, anthrapyrimidines, quinophthalones, perinones, quinacridones, diketopyrrolopyrroles, monoazo dyes such as Thermoplastrot 454, Macrolexgelb G, Sandoplast Rot G or Solvaperm Rot G), and / or inorganic pigments (such as zinc chromate, cadmium sulfide, chromium oxide, ultramarine pigments, metal flake barium sulfate and titanium dioxide).
[0022] The ink according to the invention is preferably an aqueous ink, which is preferred over printing inks based on organic solvents, since printing inks based on organic solvents do not swell or dissolve film A, which may result in film defects.
[0023] The term "water-based ink" refers to any ink that uses water as the solvent base.
[0024] For water-based inks, it is especially preferred to use inks made with deionized water (DI water), ie, water that has had almost all of its ions removed.
[0025] However, the use of inks made with deionized water can result in degradation of the polyvinyl acetal film, especially if the ink-containing film is exposed to high temperatures for extended periods of time, such as when the ink provides a high degree of light absorption. It is believed that such degradation may be caused by the residual acidity of the deionized water, which can result in hydrolysis of the acetal groups. Distilled water dissolves carbon dioxide from the air to form carbonic acid. For example, the absorption of carbon dioxide can reduce the pH of ultrapure water to 4.5.
[0026] It is therefore preferable to control the pH of the ink. Examples of pH control agents include alkanolamines such as mono-, di- and triethanolamine, sodium hydroxide and lithium hydroxide.
[0027] The aqueous ink according to the present invention may optionally contain a water-soluble organic solvent. Examples of water-soluble organic solvents include alkyl alcohols having 1 to 4 carbon atoms, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, and isobutyl alcohol; ketones or ketone alcohols, such as acetone and diacetone alcohol; ethers, such as tetrahydrofuran (THF) and dioxane; alkylene glycols, such as ethylene glycol, propylene glycol, diethylene glycol, and triethylene glycol; polyalkylene glycols, such as polyethylene glycol and polypropylene glycol; lower alkyl ethers of polyhydric alcohols, such as ethylene glycol monoethyl ether, propylene glycol monomethyl ether, diethylene glycol monoethyl ether, and triethylene glycol monoethyl ether; lower alkyl ether acetates, such as polyethylene glycol monomethyl ether acetate; glycerol; and pyrrolidones, such as 2-methylpyrrolidone and N-methyl-2-pyrrolidone. Glycols are particularly preferred. The amount of these organic solvents is not particularly limited, but is usually in the range of 1 to 50% by weight, preferably 2 to 10% by weight.
[0028] Furthermore, the water-based ink of the present invention may optionally contain a water-soluble resin (e.g., a low condensation product of vinylpyrrolidone), a water-soluble acrylic resin, an alcohol-soluble resin (e.g., a phenolic resin, etc.), an acrylic resin, a styrene-maleic acid resin, a polyurethane resin, a polyvinyl acetal resin, a polyvinyl alcohol resin, or a ketone resin. Polyvinyl acetal, particularly PVB resin, is preferred. The amount of these resins is not particularly limited, but is usually in the range of 10 to 50% by weight, preferably 20 to 30% by weight.
[0029] It is particularly preferable to use ink that has low concentrations of sodium ions, potassium ions, magnesium ions and calcium ions and a pH of 7 or higher.
[0030] Particularly for automotive applications, the ink according to the invention is preferably black and the laminated glass is opaque in the areas where the ink has been applied to the surface of film A. Preferably, the ink has a colour other than black and the laminated glass is opaque in the areas where the ink has been applied to the surface of film A.
[0031] In particular architectural applications, the ink has a color other than black and the laminated glass is transparent in the areas where the ink has been applied to the surface of Film A. Alternatively, the ink has a color other than black and the laminated glass is opaque in the areas where the ink has been applied to the surface of Film A.
[0032] The term "color" is intended to indicate that the surface may appear in colors other than black and the colors of standard commercial grades of PVB that have not been modified for the purpose of displaying a particular color. Colors may be selected from any possible color in the visible light spectrum as a single color or a mixture of different colors. Additionally, "color" shall also refer to metallic effects, areas of white, or any possible shades.
[0033] The term "opaque" refers to any area of a film having a light transmission in the visible spectrum of 5% or less. The term "transparent" refers to any area of a film having a light transmission in the visible spectrum of greater than 5%. In variations, the "opaque areas" may fade to transparency. In such variations, at least a portion of the "opaque areas" of the film have a light transmission in the visible spectrum of less than 5%.
[0034] The opaque areas may be fully opaque and / or partially interrupted and / or may have a transition area from a fully opaque edge to a transparent area. Interrupted printing may be achieved in the form of a speckle pattern. The opaque areas may fade-in continuously from transparent to opaque black or gray.
[0035] The shape of the opaque areas may be rectangular or may follow the contour of the finished laminated glass.
[0036] The inks can be applied via techniques commonly known in the printing industry, such as offset, rotogravure, flexography, and screen printing, typically followed by a drying step. Preferably, multiple ink layers are superimposed on top of one another. Also preferably, superimposition occurs after the previous ink layer has been at least partially dried.
[0037] To avoid wrinkling and / or deformation of film A due to excessive heating during the drying process, it is important that film A is not exposed to temperatures above its glass transition temperature, measurable as Tg by DSC method. Thus, it is preferred that the temperature of film A during the drying process be maintained at least 3° C., or at least 5° C., or at least 10° C., or at least 15° C., or most preferably at least 20° C. below the Tg of the film.
[0038] The dry film thickness of the ink layer in the printed area is 0.5-50 μm depending on the printing technique and the required opacity. Usually, the dry film thickness is 1-30 μm, preferably 2-20 μm. When several ink layers are superimposed, the dry film thickness refers to the total thickness of the superimposed layers.
[0039] The thickness of film A in the starting state before lamination is 10 to 250 μm, preferably 20 to 160 μm, preferably 30 to 120 μm, preferably 40 to 100 μm, and most preferably 50 to 80 μm. This thickness range does not include additional coating layers and ink layers on the film. In the above laminated glass, the plasticizer from film B migrates, allowing the film thickness to be increased.
[0040] Film A is produced separately from Film B (e.g., extruded or solvent cast) and contains no plasticizer or a sufficiently small proportion of plasticizer so as not to adversely affect subsequent functionalization and processing.
[0041] Film B may be any plasticized PVB film known in the art. Films A and B may contain, in their starting state before lamination and / or in the stack prepared for lamination between glass sheets, a single plasticizer as well as a mixture of plasticizers, both of different and identical composition. The term "different composition" refers both to the type of plasticizer in the mixture and its proportion. Films A and B after lamination, i.e. the finished laminated glass, preferably have the same plasticizers WA and WB. However, in a preferred variant, film A does not contain any plasticizer in its starting state and contains plasticizer WB in an equilibrium amount after lamination.
[0042] The plasticizer-containing film B used according to the invention contains, in the starting state before lamination, at least 22% by weight, for example 22.0 to 45.0% by weight, preferably 25.0 to 32.0% by weight, in particular 26.0 to 30.0% by weight, of plasticizer.
[0043] The film A used according to the invention may contain less than 22 wt.% (e.g. 21.9 wt.%), less than 18 wt.%, less than 16 wt.%, less than 12 wt.%, less than 8 wt.%, less than 4 wt.%, less than 2 wt.%, less than 1 wt.% or no plasticizer (0 wt.%) in the starting state before lamination. In a preferred embodiment of the invention, the film A having a low plasticizer content preferably contains 0-8 wt.%, most preferably 0-4 wt.% plasticizer.
[0044] Also preferably, the laminated glass according to the invention has, before lamination, an amount of plasticizer WA in film A of less than 22 wt.-% and an amount of plasticizer WB in film B of at least 22 wt.-%. More preferably, before lamination, the amount of plasticizer WA in film A is less than 5 wt.-% and in particular film A does not contain any intentionally added plasticizer.
[0045] The term "pre-lamination" refers to the state of Films A and B before they are brought into contact with one another. For example, this term refers to the composition of each film being separately formed and wound separately onto individual rolls.
[0046] Film A or B preferably contains polyvinyl acetal having the same or different proportion of polyvinyl acetate groups, which is 0.1 to 20 mol %, preferably 0.5 to 3 mol % or 5 to 8 mol %.
[0047] The thickness of film B in the initial state is 450 to 2500 μm, preferably 600 to 1000 μm, preferably 700 to 900 μm. In the present invention, a plurality of films B may be stacked on top of each other or may be separated by films A.
[0048] <Polyvinyl acetal> The films A and B used according to the invention contain polyvinyl alcohol or polyvinyl acetal prepared by acetalization of ethylene-vinyl alcohol copolymers.
[0049] The films may contain polyvinyl acetals each having a different polyvinyl alcohol content, degree of acetalization, residual acetate content, ethylene percentage, molecular weight and / or different chain length of the aldehyde of the acetal group.
[0050] In particular, the aldehyde or keto compound used to prepare the polyvinyl acetal can be linear or branched (i.e., "n" or "iso" type) containing from 2 to 10 carbon atoms resulting in a corresponding linear or branched acetal group. Thus, polyvinyl acetal is also referred to as "polyvinyl (iso)acetal" or "polyvinyl (n) acetal."
[0051] The polyvinyl acetals used according to the invention result in particular from the reaction of at least one polyvinyl alcohol with one or more aliphatic unbranched keto compounds containing 2 to 10 carbon atoms. For this purpose, n-butyraldehyde is preferably used, and the polyvinyl acetal PA and the polyvinyl acetal PB are both polyvinyl butyrals.
[0052] Film A or B preferably contains polyvinyl acetal having the same or different proportion of polyvinyl acetate groups, which is 0.1 to 20 mol %, preferably 0.5 to 3 mol % or 5 to 8 mol %.
[0053] The polyvinyl alcohol content of the polyvinyl acetal PA used in film A can be 6 to 26% by weight, 8 to 24% by weight, 10 to 22% by weight, 12 to 21% by weight, 14 to 20% by weight, 16 to 19% by weight, preferably 16 to 21% by weight or 10 to 16% by weight.
[0054] Independently of film A, the polyvinyl alcohol content of the polyvinyl acetal PB used in film B can be 14-26% by weight, 16-24% by weight, 17-23% by weight, preferably 18-21% by weight.
[0055] In a preferred embodiment of the present invention, film A contains polyvinyl acetal PA having a proportion of vinyl alcohol groups of 6 to 26% by weight, and film B contains polyvinyl acetal B having a proportion of vinyl alcohol groups of 14 to 26% by weight.
[0056] <Plasticizer> The films A and / or B used according to the invention may contain, as plasticizers, one or more compounds selected from the following group: esters of polyhydric aliphatic or aromatic acids, for example dialkyl adipates, such as dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, mixtures of heptyl and nonyl adipate, diisononyl adipate, heptylnonyl adipate, and cycloaliphatic esters of adipic acid, and esters of adipic acid with ester alcohols, including ester alcohols or ether compounds, dialkyl sebacates, such as dibutyl sebacate, and also esters of sebacic acid with ester alcohols, including cycloaliphatic ester alcohols or ether compounds, esters of phthalic acid, such as butyl benzyl phthalate or bis-2-butoxyethyl phthalate. - esters or ethers of polyhydric aliphatic or aromatic alcohols or oligoether glycols with one or more unbranched or branched aliphatic or aromatic substituents, such as esters of glycerol, diglycol, triglycol or tetraglycol with linear or branched aliphatic or cycloaliphatic carboxylic acids; examples of the latter group include diethylene glycol-bis-(2-ethylhexanoate), triethylene glycol-bis-(2-ethylhexanoate), triethylene glycol-bis-(2-ethylbutanoate), tetraethylene glycol-bis-n-heptanoate, triethylene glycol-bis-n-heptanoate, triethylene glycol-bis-n-hexanoate, tetraethylene glycol dimethyl ether and / or dipropylene glycol benzoate. - phosphates with aliphatic or aromatic ester alcohols, such as tris(2-ethylhexyl) phosphate (TOF), triethyl phosphate, diphenyl-2-ethylhexyl phosphate and / or tricresyl phosphate - Esters of citric acid, succinic acid and / or fumaric acid.
[0057] By definition, a plasticizer is an organic liquid with a high boiling point. Therefore, additional types of organic liquids with boiling points above 120° C. can also be used as plasticizers.
[0058] It is particularly preferred that film A in the variant in which a plasticizer WA is present in film A at the start, and also film B, contain 1,2-cyclohexanedicarboxylic acid diisononyl ester (DINCH) or triethylene glycol-bis-2-ethylhexanoate (3GO or 3G8) as plasticizer.
[0059] Furthermore, films A and B may contain further additives such as residual amounts of water, UV absorbers, antioxidants, adhesion modifiers, optical brighteners or fluorescent additives, stabilizers, colorants, processing aids, inorganic or organic nanoparticles, pyrogenic silicic acid and / or surface-active substances.
[0060] <Lamination process> The present invention also relates to a method for producing the above-mentioned penetration-resistant glass laminate, in which film A is placed on a glass sheet, then covered with at least one film B, and then a second glass sheet is applied.
[0061] Alternatively, film B can be placed on a glass plate and then covered with at least one film A and a second glass plate can be applied.
[0062] The invention further relates to a method for producing laminated glass, in which a stack is provided comprising at least one film A and at least one film B, the stack being placed on a first glass sheet and then a second glass sheet being applied.
[0063] According to the invention, it is possible to first melt film A onto a glass sheet over the entire area or locally by increasing the temperature, and then cover it with film B. Alternatively, films A and B can be placed together between two glass sheets and melted at high temperature.
[0064] The lamination step for producing laminated glass is preferably carried out by disposing films A and B between two glass plates, and pressing the prepared layered body under increased or reduced pressure and at elevated temperature to form a laminate.
[0065] To laminate the layers, methods familiar to those skilled in the art can be used with or without prior preparation of a pre-laminate.
[0066] The so-called "autoclave process" is carried out at a pressure of about 10-15 bar and at a temperature of 100-150°C for about 2 hours. The vacuum bag or vacuum ring process, for example according to EP 1 235 683 B1, works at about 200 mbar and 130-145°C.
[0067] Vacuum laminators may also be used. These consist of a chamber that can be heated and evacuated, in which the laminated glazing can be laminated within 30-60 minutes. Reduced pressures of 0.01-300 mbar and temperatures of 100-200 ° C, in particular 130-160 ° C, have proven to be of value in practice.
[0068] In the simplest case, to produce a laminated glass laminate, a film A or B is placed on a glass sheet and a further film B or A is placed synchronously or subsequently. A second glass sheet is then applied, producing a laminate of glass sheets. Any pre-lamination method known to the skilled artisan can then be used to remove excess air. Here, the layers are also already initially lightly adhesively bonded to each other and to the glass.
[0069] The glass film laminate may then be subjected to an autoclave process. Film A is preferably placed on the first glass sheet and covered by a thicker film B before the second glass sheet is applied. The method can be carried out in many conceivable and in principle practical variants. For example, film A is easily removed from a roll of suitable width, while film B is pre-tailor-cut to the size of the laminated glass to be produced. This is particularly advantageous in the case of windscreens and other automotive glazing parts. In this case, it is particularly advantageous to further stretch the thicker film B before tailor-cutting it. This allows a more economical use of the film or, if film B has a tint, allows its curvature to be adapted to the upper sheet edge.
[0070] The thin film A is generally produced in the form of an extrusion or blown film using a cast film line. Here, the surface roughness can also be produced by controlled melt breakage or by a cast film method using additionally structured chill rolls and / or structured back rolls. Alternatively, a solvent casting method can be used to produce the film A before functionalization and use it in the described penetration-resistant glass laminate. The film used according to the invention preferably has a one-sided surface structure with a roughness Rz of 0 to 25 μm, preferably a roughness Rz of 1 to 20 μm, particularly preferably a roughness Rz of 3 to 15 μm, in particular a roughness Rz of 4 to 12 μm. It is particularly preferred that the surface roughness Rz of the side of film A in contact with the glass sheet is not more than 20% of its thickness.
[0071] Another embodiment of the present invention is a film comprising a polyvinyl acetal PA, optionally at least one plasticizer WA and, on at least one surface, an area to which an ink has been applied, wherein the pH value of the ink before application is greater than or equal to 7 and the concentration of potassium, magnesium or calcium ions in the ink before application is less than or equal to 200 mg / l.
[0072] The use of inks having a pH value of 7 or greater and / or a concentration of potassium, magnesium or calcium of 200 mg / l or less in a printing or coating process on the surface of a polyvinyl acetal film is also disclosed.
[0073] An embodiment of the present invention is a method for producing a laminated glass according to the present invention disclosed above, characterized in that at least one surface area of a film A is printed or coated with an ink, then placed on a first glass sheet, covered with at least one film B, covered with a second glass sheet, and then laminated at a temperature of 100°C or higher. Preferred aspects of the present invention include the following. [1] A laminated glass obtained by laminating, between two glass sheets, at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, 1. A laminated glass, characterized in that film A comprises, on at least one surface, an area in which an ink has been applied to the surface, and prior to its application, the pH value of said ink is 7 or greater. [2] A laminated glass obtained by laminating, between two glass sheets, at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, 1. A laminated glass, characterized in that film A comprises on at least one surface an area to which ink has been applied, and prior to its application the concentration of potassium ions, magnesium ions or calcium ions in said ink is less than or equal to 200 mg / l. [3] The laminated glass according to [1] or [2], obtained by laminating, between two glass sheets, at least one film A comprising polyvinyl acetal PA and optionally at least one plasticizer WA, and at least one film B comprising polyvinyl acetal PB and at least one plasticizer WB, wherein at least one surface of film A to which the ink is applied faces film B. [4] Before lamination, The amount of plasticizer WA in film A is less than 22% by weight; The amount of plasticizer WB in film B is at least 22% by weight; The laminated glass according to any one of [1] to [3]. [5] The laminated glass according to any one of [1] to [4], wherein the amount of the plasticizer WA in the film A before lamination is less than 5% by weight. [6] The laminated glass according to any one of [1] to [5], wherein the concentrations of potassium ions, magnesium ions and calcium ions in the ink before application are 200 mg / L or less, preferably 100 mg / L or less, and more preferably 50 mg / L or less. [7] The laminated glass according to any one of [1] to [6], wherein the pH of the ink before application is greater than 7.5, preferably greater than 8.0. [8] The laminated glass according to any one of [1] to [7], wherein the polyvinyl acetal PA and the polyvinyl acetal PB are polyvinyl butyral. [9] The laminated glass according to any one of [1] to [8], wherein the laminated glass is opaque in an area where the ink is applied to the surface of film A.
[10] The laminated glass according to any one of [1] to [9], wherein the laminated glass is colored in an area where the ink is applied to the surface of film A.
[11] The laminated glass according to any one of [1] to
[10] , wherein the ink is a water-based ink.
[12] A film comprising a polyvinyl acetal PA, optionally at least one plasticizer WA, and on at least one surface an area to which an ink has been applied, wherein the pH value of said ink before application is greater than or equal to 7, and the concentration of potassium ions, magnesium ions or calcium ions in said ink before application is less than or equal to 200 mg / l.
[13] A method for producing the laminated glass according to any one of [1] to
[11] , comprising printing or coating at least one surface area of film A with ink, placing the film A on a first glass plate, covering the film A with at least one film B, covering the film A with a second glass plate, and laminating the resulting glass at a temperature of 100°C or higher. EXAMPLES
[0074] PVB resin powder (commercial grade Mowital® B 60 H from Kuraray Europe GmbH) was fed into the inlet funnel of a co-rotating twin-screw type laboratory extruder. Potassium acetate and magnesium acetate tetrahydrate aqueous solutions at 0.525 wt. % with respect to the polymer resin were simultaneously dosed into the extruder inlet zone resulting in 350 ppm potassium acetate and 175 ppm magnesium acetate tetrahydrate, respectively, in the degassed melt. The melt was extruded through a 34 cm wide slit die onto a chilled chill roll to form a thin plasticizer-free film approximately 50 μm thick and 30 cm wide, which was subsequently wound up (used and evaluated as Film A with ACA).
[0075] The film was printed with an opaque black strip that was the same length as the film and 5 cm wide.
[0076] Prior to analytical determination of moisture content (Karl-Fischer method) and metal content (ion chromatography), the rolls were stored in a conditioned area with a constant climate of 23° C. / 28% RH.
[0077] A commercially available automotive grade PVB film with reduced adhesion (TROSIFOL® VG R10 0.76 from Kuraray Europe GmbH = example of Film B) was conditioned in the same climate before producing the test laminates.
[0078] Test stacks of dimensions 30×30 cm were obtained by combining standard thickness clear glass (2×Planiclear® 2.1 mm) washed with deionized water <5 μS with films A and B in the following stacking order:
[0079] For adhesion testing and penetration resistance in combination with automotive grade PVB: bottom glass (air side) - film A - ink layer, if present - VG R10 - (tin side) top glass.
[0080] The sandwich was passed through a commercial flat glass laminating nipper line to produce a prelaminate. Lamination was accomplished by using an autoclave at standard conditions (90 minutes with a 30 minute hold time at 140° C. and 12 bar).
[0081] The laminates were allowed to sit at ambient conditions at 23° C. for one week before further mechanical evaluation.
[0082] The penetration resistance of the laminate construction was tested according to ECE 43R (2.26 kg steel ball at 23°C, 226 g steel ball at -20°C and +40°C). The laminate construction (2 x 2.1 mm) safely fulfilled the requirements laid down in ECE R43 for windscreen glazing.
[0083] <Example 1> Printing was achieved by digital inkjet printing using commercially available inkjet inks. To prevent ink attack on the polymer, the color strength of a single printing step was selected to achieve a semi-transparent film. The required opacity was achieved by overprinting already printed parts and then drying the film at 22°C before applying the next layer of printing ink.
[0084] <Comparative Example> Printing was achieved by using an aqueous printing ink suitable for flexographic printing, based on polyacrylate as binder and carbon black as pigment. Similar printing inks are commercially available, for example, from Siegwerk Druckfarben AG&Co. KGaA, Siegburg. The ink was analyzed to contain 62 ppm calcium, 8 ppm magnesium and 12 ppm potassium metals. In order to reach a total dry layer thickness close to 9 μm with sufficiently high opacity, the black printing layer was overprinted twice (3 ink layers in total). After drying, the moisture content of film A in the printed areas was measured to be 2%.
[0085] As film B a commercial automotive grade PVB film with reduced adhesion (TROSIFOL® VG R10 0.76 from Kuraray Europe GmbH) was used.
[0086] The laminate containing the printed film A obtained as described showed well-defined edges between the transparent and opaque black areas. No blurring or distortion of the printed areas could be observed. The opacity was measured to be significantly below 5% visible light transmittance.
[0087] <Adhesion test> The adhesion of the interlayer film to glass was tested using the "Pummel test". This test is well known to those skilled in the art and is described in the literature. The pummel values provided within the scope of the present invention were determined by the pummel test described in WO 03 / 033583 A1.
[0088] When a pummel test was performed to evaluate the adhesion between the PVB and the inner glass surface, the following was observed: In the unprinted areas, the interface between the glass and VG R10 exhibited an adhesion of 3 pummel units, while the opposite interface between Film A and the glass exhibited an adhesion of 4 pummel units. In the printed area, the interface between the glass and VG R10 showed an adhesion of 3.5 pummel units, while the opposite interface between Film A and the glass showed an adhesion of 0 pummel units (the glass was largely delaminated).
[0089] <Example 2> Printing was achieved by using an aqueous printing ink suitable for flexographic printing, based on polyacrylate as binder and carbon black as pigment. Deionized water was used for the preparation of this ink composition instead of regular tap water. The ink was analyzed to contain 3 ppm calcium, 1 ppm magnesium and 8 ppm potassium metals. To reach a total dry layer thickness close to 9 μm with sufficiently high opacity, the black printing layer was overprinted twice (3 ink layers in total). After drying, the moisture content of film A in the printed areas was measured to be 2%.
[0090] As film B a commercial automotive grade PVB film with reduced adhesion (TROSIFOL® VG R10 0.76 from Kuraray Europe GmbH) was used.
[0091] The laminate containing the printed film A obtained as described showed well-defined edges between the transparent and opaque black areas. No blurring or distortion of the printed areas could be observed. The opacity was measured to be significantly below 5% visible light transmittance.
[0092] When a pummel test was performed to evaluate the adhesion between the PVB and the inner glass surface, the following was observed: In the unprinted areas, the interface between the glass and VG R10 exhibited an adhesion of 3 pummel units, while the opposite interface between Film A and the glass exhibited an adhesion of 3.5 pummel units. In the printed area, the interface between the glass and VG R10 exhibited an adhesion of 3.5 pummel units, while the opposing interface between Film A and the glass exhibited an adhesion of 2.5 pummel units.
[0093] Additionally, the laminate was subjected to a heat soak test at 100°C for 7 days. Neither the printed nor the unprinted areas showed any air bubbles or other visible defects. The laminate samples were subjected to a 3000 hour xenon test in an Atlas Ci65 Xenon Weather-Ometer using the method specified in ASTM D2565 in accordance with ANSI Z97.1-2009. The laminate was oriented with Film A facing the xenon radiation source. The black color remained almost unchanged after 3000 hours, but small air bubbles could be observed at the interface of Film A and the ink layer. It is speculated that traces of acid from the ink layer led to partial decomposition of the acid-sensitive polyvinyl butyral.
[0094] <Example 3> Printing was achieved by using an aqueous printing ink suitable for flexographic printing, based on polyacrylate as binder and carbon black as pigment. Deionized water was used for the preparation of this ink composition instead of regular tap water. The ink was analyzed to contain 3 ppm calcium, 1 ppm magnesium and 8 ppm potassium metals. Furthermore, the pH value of the ink was controlled at a value of 8.5 by the addition of sodium hydroxide. In order to reach a total dry layer thickness close to 9 μm with sufficiently high opacity, the black printing layer was overprinted twice (3 ink layers in total). After drying, the moisture content of film A in the printed areas was measured to be 2%.
[0095] As film B a commercial automotive grade PVB film with reduced adhesion (TROSIFOL® VG R10 0.76 from Kuraray Europe GmbH) was used.
[0096] The laminate containing the printed film A obtained as described showed well-defined edges between the transparent and opaque black areas. No blurring or distortion of the printed areas could be observed. The opacity was measured to be significantly below 5% visible light transmittance.
[0097] When a pummel test was performed to evaluate the adhesion between the PVB and the inner glass surface, the following was observed: In the unprinted areas, the interface between the glass and VG R10 exhibited an adhesion of 3 pummel units, while the opposite interface between Film A and the glass exhibited an adhesion of 3.5 pummel units. In the printed area, the interface between the glass and VG R10 exhibited an adhesion of 3 pummel units, while the opposite interface between Film A and the glass exhibited an adhesion of 3.5 pummel units.
[0098] Additionally, the laminate was subjected to a heat soak test at 100°C for 7 days. Neither the printed nor the unprinted areas showed any air bubbles or other visible defects. The laminate samples were subjected to a 3000 hour xenon test in an Atlas Ci65 Xenon Weather-Ometer using the method specified in ASTM D2565 in accordance with ANSI Z97.1-2009. The laminate was oriented with Film A facing the xenon radiation source. The black color remained nearly unchanged after 3000 hours, and no air bubbles were now observed at the interface between Film A and the ink layer.
Claims
1. A laminated glass obtained by laminating, between two glass sheets, at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, Film A comprises, on at least one surface, an area to which ink has been applied, the ink having a pH value of 7 or greater prior to its application; 1. A laminated glass comprising film A, on at least one surface thereof, an area to which ink has been applied, and wherein prior to its application, the concentration of potassium ions in said ink is 20 mg / l or less, the concentration of magnesium ions in said ink is 50 mg / l or less, and the concentration of calcium ions in said ink is 50 mg / l or less.
2. 2. The laminated glass according to claim 1, obtained by laminating, between two glass sheets, at least one film A comprising a polyvinyl acetal PA and optionally at least one plasticizer WA, and at least one film B comprising a polyvinyl acetal PB and at least one plasticizer WB, at least one surface of film A to which the ink has been applied faces film B.
3. Before lamination, The amount of plasticizer WA in film A is less than 22% by weight, The amount of plasticizer WB in film B is at least 22% by weight; The laminated glass according to claim 1 or 2.
4. The laminated glass according to any one of claims 1 to 3, wherein the amount of plasticizer WA in film A before lamination is less than 5 wt%.
5. 5. The laminated glass according to claim 1, wherein the total concentration of potassium ions, magnesium ions and calcium ions in the ink before application is 50 mg / L or less.
6. The laminated glass according to any one of claims 1 to 5, wherein the pH of the ink before application is greater than 7.5 before application.
7. The laminated glass according to any one of claims 1 to 6, wherein the polyvinyl acetal PA and the polyvinyl acetal PB are polyvinyl butyral.
8. 8. The laminated glass according to claim 1, wherein in the areas where the ink is applied to the surface of Film A, the laminated glass is opaque.
9. 9. The laminated glass according to claim 1, wherein in the areas where the ink is applied to the surface of film A, the laminated glass is colored.
10. The laminated glass according to any one of claims 1 to 9, wherein the ink is a water-based ink.
11. A film comprising a polyvinyl acetal PA, optionally at least one plasticizer WA, and on at least one surface an area to which an ink has been applied, wherein, prior to its application, the pH value of said ink is greater than or equal to 7, and, prior to its application, the concentration of potassium ions in said ink is less than or equal to 20 mg / l, the concentration of magnesium ions in said ink is less than or equal to 50 mg / l and the concentration of calcium ions in said ink is less than or equal to 50 mg / l.
12. A method for producing the laminated glass according to any one of claims 1 to 10, characterized in that at least one surface area of film A is printed or coated with ink, then placed on a first glass sheet, covered with at least one film B, covered with a second glass sheet and then laminated at a temperature of at least 100°C.
Citation Information
Patent Citations
Aqueous pigment dispersion and production method thereof, coloring composition, ink composition, and inkjet recording method
JP2016069629A
laminated safety glass
JP2017500271A
Laminated glass comprising interlayer film layers with a pigmented frame
WO2019038043A1