Two-component curing composition set, thermally conductive cured product, and electronic device

The two-part curable composition set with epoxy-modified and amino-modified organopolysiloxanes and surfactants addresses issues of heat dissipation degradation and curing failures, providing stable thermal conductivity and handling properties for electronic equipment.

JP7577126B2Active Publication Date: 2024-11-01DENKA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022555439
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-05
Filing Date
2021-10-01
Publication Date
2024-11-01
Estimated Expiration
2041-10-01

AI Technical Summary

Technical Problem

Conventional two-component heat dissipation materials face issues such as degradation in heat dissipation performance due to volatilization, increased viscosity, filler re-agglomeration, and curing failures, especially when exposed to high temperatures, which affect the reliability of electronic equipment.

Method used

A two-part curable composition set comprising epoxy-modified and amino-modified organopolysiloxanes with specific surfactants and thermally conductive fillers, which undergo an addition reaction without a platinum catalyst, maintaining dispersibility and low viscosity even at high temperatures.

Benefits of technology

The composition achieves high uniform curing, low viscosity, and effective heat dissipation with improved handling properties, ensuring reliable thermal conductivity and stability in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577126000001
    Figure 0007577126000001
  • Figure 0007577126000002
    Figure 0007577126000002
  • Figure 0007577126000003
    Figure 0007577126000003
Patent Text Reader

Abstract

A two-part curable composition set that comprises a first agent and a second agent, the first agent including an epoxy-modified organopolysiloxane formed by replacing a portion of the methyl groups of dimethyl silicone with a substituent that has an epoxy group, a thermally conductive filler, and a surfactant, the second agent including an amino-modified organopolysiloxane formed by replacing a portion of the methyl groups of dimethyl silicone with a substituent that has an amino group, a thermally conductive filler, and a surfactant, the surfactants being copolymers that have a (meth)acrylic monomer unit A that has an anionic group, a (meth)acrylic monomer unit B that has a cationic group, and a silicone (meth)acrylic monomer unit C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a two-component curing composition set, a thermally conductive cured product, and an electronic device. [Background technology]

[0002] Room temperature curing liquid silicone rubber exhibits stable performance over a wide temperature range, and is therefore used to improve the reliability of electrical and electronic equipment, such as computer CPUs (central processing units), car batteries, and LED devices.Specifically, it is used as an encapsulant, sealing material, potting material, coating material, and heat dissipation material for various electronic substrates.

[0003] Room temperature curing liquid silicone rubber is mainly classified into one-component and two-component types, and the two-component type is further divided into condensation reaction type and addition reaction type. The addition reaction type has a low shrinkage rate due to curing, high uniform reactivity, and does not generate outgassing, making it suitable for use as a sealant or heat dissipation material for electrical and electronic devices.

[0004] On the other hand, the addition reaction type requires a platinum catalyst, which is a precious metal, but the platinum catalyst is sensitive to temperature, and there is a problem that the catalytic activity is lost during transportation in a high-temperature environment. In addition, there is a problem that poor curing occurs when curing inhibitors such as nitrogen-containing compounds, sulfur-containing compounds, phosphorus-containing compounds, tin-containing compounds, sulfur, and solder flux, and components that can react with the catalyst, such as organic acids such as alcohol, water, and carboxylic acids, are attached to the base material.

[0005] Generally, two-component curing type heat dissipation materials are often compositions in which the above-mentioned addition reaction type liquid silicone rubber is highly filled with thermally conductive inorganic filler. In recent years, with the miniaturization and high output of heat-generating electronic components such as CPUs (central processing units) of personal computers, the amount of heat generated per unit area from these electronic components has become much larger than before, and therefore there is a demand for the above-mentioned heat dissipation materials to have higher performance, such as higher thermal conductivity and improved applicability through lower viscosity.

[0006] As an example of the above-mentioned improvement studies aimed at improving performance, Patent Document 1 reports a silicone grease composition that has high thermal conductivity and maintains excellent fluidity by including an inorganic filler that has been surface-treated with a silane coupling agent having a specific structure in a resin. Patent Document 2 reports a copolymer that contains a polybutadiene structural unit, a structural unit having a hydrolyzable silyl group, and a structural unit having a polysiloxane skeleton as a surface treatment agent other than a silane coupling agent. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2012-52137 A [Patent Document 2] JP 2018-62552 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, when a low molecular weight compound such as a silane coupling agent as disclosed in Patent Document 1 is blended, the silane coupling agent volatilizes with the heat generated by electronic components, generating voids, which causes a problem of reduced heat dissipation performance. In addition, when a high molecular weight surface treatment agent as disclosed in Patent Document 2 is used, the grease viscosity increases and the applicability decreases. Furthermore, it has been found that when a heat dissipation grease using a conventional surface treatment agent or dispersant is kept at high temperatures for a long time, dispersion destruction occurs, and cracks occur due to re-aggregation of the filler, making it impossible to efficiently release heat, and the heat dissipation characteristics decrease. Such a decrease in heat dissipation performance also leads to a decrease in the reliability of electronic devices.

[0009] In addition, addition reaction type liquid silicone rubber, which is generally used as a two-component curing heat dissipation material, has the problem that it will cure poorly if there are components that can react with a catalyst, such as alcohol, water, and organic acids such as carboxylic acids, and this can also cause poor curing depending on the type of silane coupling agent or surface treatment agent used.

[0010] The present invention has been made in consideration of the above problems, and has an object to provide a two-component curing composition set that does not require moisture for the curing reaction, has high uniform curing properties, does not require a platinum catalyst, is less susceptible to curing inhibition, has low viscosity and good handleability, and is capable of maintaining the dispersibility of a thermally conductive filler even when held at high temperatures for long periods of time; a cured product or thermally conductive cured product obtained from the two-component curing composition set; and an electronic device equipped with the thermally conductive cured product. [Means for solving the problem]

[0011] That is, the present invention is as follows. [1] A first agent including an epoxy-modified organopolysiloxane A1 having an epoxy group-containing group, a thermally conductive filler B1, and a surfactant C1; A second agent including an amino-modified organopolysiloxane A2 having an amino group-containing group, a thermally conductive filler B2, and a surfactant C2; The surfactant C1 and the surfactant C2 each contain a copolymer having a (meth)acrylic monomer unit A having an anionic group, a (meth)acrylic monomer unit B having a cationic group, and a silicone (meth)acrylic monomer unit C. Two-part curing composition set. [2] the anionic group includes at least one selected from the group consisting of a carboxyl group, a phosphate group, and a phenolic hydroxyl group; the cationic group includes at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt; The two-component curing composition set according to [1]. [3] The weight average molecular weight of the copolymer is 5,000 to 500,000. The two-component curing composition set according to [1] or [2]. [4] With respect to 100 mol % in total of the (meth)acrylic monomer unit A, the (meth)acrylic monomer unit B, and the silicone (meth)acrylic monomer unit C, The content of the (meth)acrylic monomer unit A is 0.03 to 85 mol %, The content of the (meth)acrylic monomer unit B is 0.05 to 10 mol %, and the content of the silicone (meth)acrylic monomer unit C is 10 to 99.5 mol %. The two-component curing composition set according to any one of [1] to [3]. [5] the content of the surfactant C1 in the first agent is 0.01 to 25 parts by weight with respect to 100 parts by weight of the thermally conductive filler B1 in the first agent; The content of the surfactant C2 in the second agent is 0.01 to 25 parts by weight with respect to 100 parts by weight of the thermally conductive filler B2 in the second agent. The two-component curing composition set according to any one of [1] to [4]. [6] The epoxy group equivalent weight in one molecule of the epoxy-modified organopolysiloxane A1 is 100 to 11,000 g / mol. The two-component curing composition set according to any one of [1] to [5]. [7] The amino group equivalent weight in one molecule of the amino-modified organopolysiloxane A2 is 100 to 8000 g / mol. The two-component curing composition set according to any one of [1] to [6]. [8] The amino-modified organopolysiloxane A2 in the second agent has hydroxyl group-containing groups at both ends. The two-component curing composition set according to any one of [1] to [7]. [9] The thermally conductive filler B1 and the thermally conductive filler B2 each contain at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, copper, silver, and diamond, each of which has a thermal conductivity of 10 W / m·K or more. The two-component curing composition set according to any one of [1] to [8].

[10] The first agent does not contain an organopolysiloxane having at least a vinyl group at the end or in a side chain, and an organopolysiloxane having at least a hydrosilyl group at the end or in a side chain; and The second agent is provided with an organopolysiloxane having at least a vinyl group at the end or in a side chain, and the second agent does not include an organopolysiloxane having at least a hydrosilyl group at the end or in a side chain. The two-component curing composition set according to any one of [1] to [9].

[11] Used as a thermally conductive heat dissipation material, The two-component curing composition set according to any one of [1] to

[10] .

[12] [1] to

[11] , wherein the two-component curing composition set is obtained from a mixture of the first agent and the second agent. cured product.

[13] Used as a thermally conductive heat dissipation material, The cured product according to

[12] .

[14] An electronic component, the cured product according to

[13] , and a housing that accommodates the electronic component and the cured product, The electronic component and the housing are in contact with each other via the cured product. electronic equipment. Effect of the Invention

[0012] According to the present invention, it is possible to provide a two-component curing composition set that does not require moisture for the curing reaction, has high uniform curing properties, does not require a platinum catalyst, is less susceptible to curing inhibition, has low viscosity and good handleability, and is capable of maintaining the dispersibility of a thermally conductive filler even when held at high temperatures for a long period of time; and a cured product or thermally conductive cured product obtained from the two-component curing composition set, as well as an electronic device equipped with the thermally conductive cured product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. However, the present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention.

[0014] [Two-component curing composition set] The two-component curing composition set according to this embodiment comprises a first agent containing an epoxy-modified organopolysiloxane A1 having an epoxy group-containing group, a thermally conductive filler B1, and a surfactant C1, and a second agent containing an amino-modified organopolysiloxane A2 having an amino group-containing group, a thermally conductive filler B2, and a surfactant C2, in which the surfactant C1 and the surfactant C2 contain a copolymer having (meth)acrylic monomer units A having an anionic group, (meth)acrylic monomer units B having a cationic group, and silicone (meth)acrylic monomer units C.

[0015] Conventional two-component curing silicone compositions utilize condensation reactions or addition reactions. However, condensation reactions using organopolysiloxanes having hydroxyl groups or alkoxy groups require moisture for curing, generate reaction by-products (outgassing), and have problems such as high shrinkage. On the other hand, addition reactions using organopolysiloxanes having vinyl groups and organopolysiloxanes having hydrosilyl groups have excellent shrinkage, do not generate outgassing, and do not require moisture, but require an addition reaction catalyst such as a platinum catalyst, and have problems such as curing inhibition caused by coexisting compounds.

[0016] In contrast, in the present embodiment, by using the epoxy-modified organopolysiloxane A1 having an epoxy group-containing group and the amino-modified organopolysiloxane A2 as described above, it is possible to provide a two-component curing composition set that does not require an addition reaction catalyst such as a platinum catalyst, does not cause curing inhibition, does not require moisture for curing, and does not generate outgassing.

[0017] Furthermore, in this embodiment, the use of the specific surfactants C1 and C2 can further improve the dispersion stability of the thermally conductive fillers B1 and B2 contained in the first and second agents. Also, the use of the specific surfactants C1 and C2 can reduce the viscosity of the first and second agents, making it possible to further improve the ease of handling.

[0018] Furthermore, for the reasons described above, in this embodiment, it is preferable that neither the first agent nor the second agent contains an organopolysiloxane having a vinyl group at least at the end or in a side chain, nor an organopolysiloxane having a hydrosilyl group at least at the end or in a side chain.

[0019] Each component contained in the first and second agents will be described in detail below.

[0020] <First agent> The first agent contains an epoxy-modified organopolysiloxane A1 having an epoxy group-containing group, a thermally conductive filler B1, and a surfactant C1, and may contain polydimethylsiloxane D, organosilane E, and a colorant F as necessary.

[0021] (Epoxy modified organopolysiloxane A1) The epoxy-modified organopolysiloxane A1 of this embodiment has a substituent (epoxy group-containing group) having an epoxy group at the end or in the side chain. The organopolysiloxane having an epoxy group is one in which at least a part of the R in the Si-R portion (wherein R is a substituted or unsubstituted monovalent hydrocarbon group) in the organopolysiloxane molecule is a substituent having an epoxy group.

[0022] The epoxy group-containing group is not particularly limited, but examples thereof include an aliphatic epoxy group represented by the following formula (a11) and an alicyclic epoxy group represented by the following formula (a12). Among these, an aliphatic epoxy group such as a glycidyl group is preferred from the viewpoint of curing reactivity, and an alicyclic epoxy group such as an ethylcyclohexene oxide group is preferred from the viewpoint of increasing the glass transition point of the obtained cured product. The epoxy-modified organopolysiloxane A1 may have both an aliphatic epoxy group and an alicyclic epoxy group. [ka] (In the formula, R 1 represents an alkyl group having 1 to 6 carbon atoms.

[0023] The epoxy-modified organopolysiloxane A1 may have any of a linear structure, a branched structure, and a cyclic structure, and may have a structure in which a linear structure and a cyclic structure are combined, or a structure in which a branched structure and a cyclic structure are combined. Among these, a linear structure is preferred from the viewpoint of handling as a liquid, and a branched structure is preferred from the viewpoint of the mechanical properties of the obtained cured product.

[0024] The bonding position of the epoxy group-containing group in the epoxy-modified organopolysiloxane A1 is not particularly limited, and may be a terminal or a side chain, or may be a terminal and a side chain. When the epoxy group-containing group is present in the side chain, the epoxy-modified organopolysiloxane A1 has, for example, a structural unit represented by the following general formula (a1-1) or (a1-2). When the epoxy group-containing group is present in the terminal, the epoxy-modified organopolysiloxane A1 has, for example, a terminal structure represented by the following general formula (a1-3) (wherein n is 1 or more). Furthermore, as a structural unit to which an epoxy group-containing group is not bonded, a structural unit represented by the following general formula (a1-4) can be given. The structural units that the epoxy-modified organopolysiloxane A1 has are not limited to the following, and for example, when the epoxy-modified organopolysiloxane A1 has a branched structure, it may have a branched structural unit, and when the epoxy-modified organopolysiloxane A1 has a cyclic structure, it may not have a terminal structure. [ka] (In the formula, each X independently represents an epoxy group-containing group; R 2 each independently represents a substituted or unsubstituted hydrocarbon group or polyether group having 1 to 12 carbon atoms, and n represents an integer of 0 to 3.

[0025] R 2 The substituted or unsubstituted hydrocarbon group represented by the formula (I) is not particularly limited, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl groups; and halogenated alkyl groups such as chloromethyl, 3,3,3-trifluoropropyl, and 3-chloropropyl groups.

[0026] Also, R 2 The polyether group represented by the formula (I) is not particularly limited, but may be, for example, a polyethylene glycol group (-(C2H4O)l -CH2H5,-(C2H4O) l -CH2H4OH), polypropylene glycol group (-(C3H6O) l -CH3H7,-(C3H6O) l —CH3H6OH), and polyethylene glycol-polypropylene glycol copolymer group. Here, l represents an integer of 2 to 1000.

[0027] Among these, the epoxy-modified organopolysiloxane A1 is preferably an organopolysiloxane having a linear structure and an epoxy-containing group in the side chain. By using such an epoxy-modified organopolysiloxane A1, the reactivity of the first agent and the second agent tends to be further improved.

[0028] The epoxy functional group equivalent of the epoxy-modified organopolysiloxane A1 is preferably 100 to 11000 g / mol, more preferably 200 to 6000 g / mol, and even more preferably 250 to 5000 g / mol. When the epoxy functional group equivalent is within the above range, the reactivity of the first agent and the second agent tends to be further improved.

[0029] The viscosity of the epoxy-modified organopolysiloxane A1 at 25° C. is preferably 5 to 15,000 mm 2 / s, and more preferably 5 to 12000 mm 2 / s, and more preferably 5 to 10,000 mm 2 When the viscosity is within the above range, the handleability of the two-component curing composition set tends to be improved.

[0030] (Thermal conductive filler B1) The thermally conductive filler B1 is, for example, a filler having a thermal conductivity of at least 10 W / m·K. Although there are no particular limitations on such thermally conductive filler B1, examples thereof include aluminum oxide (hereinafter also referred to as "alumina"), aluminum nitride, silica, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, diamond, carbon, indium, gallium, copper, silver, iron, nickel, gold, tin, metallic silicon, and the like.

[0031] Among these, it is preferable to include at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, copper, silver, and diamond, and alumina is more preferable. By using such a thermally conductive filler B1, the filling property is improved, and the thermal conductivity of the obtained cured product tends to be further improved. These thermally conductive fillers B1 may be used alone or in combination of two or more.

[0032] The thermally conductive filler B1 has an average particle size of preferably 0.1 to 120 μm, and more preferably 0.1 to 60 μm. When the average particle size of the thermally conductive filler B1 is within the above range, the fluidity, dispersibility, and filling property tend to be further improved.

[0033] The thermally conductive filler B1 may be a mixture of fillers having different average particle sizes. For example, it is more preferable to use a combination of a thermally conductive filler (B1-1) having an average particle size of 40 to 50 μm and a thermally conductive filler (B1-2) having an average particle size of 1 to 10 μm. In this case, the content of the thermally conductive filler (B1-1) is preferably 40 to 80 mass%, more preferably 50 to 70 mass%, based on the total amount of the thermally conductive filler B1. The content of the thermally conductive filler (B1-1) is preferably 20 to 60 mass%, more preferably 30 to 50 mass%, based on the total amount of the thermally conductive filler B1. By using such a thermally conductive filler B1, the fluidity, dispersibility, and filling property tend to be further improved. The average particle size in this embodiment means D50 (median diameter).

[0034] The content of the thermally conductive filler B1 is preferably 400 to 3000 parts by weight, more preferably 600 to 2800 parts by weight, and even more preferably 700 to 2600 parts by weight, relative to 100 parts by weight of the epoxy-modified organopolysiloxane A1. When the content of the thermally conductive filler is 400 parts by weight or more relative to 100 parts by weight of the epoxy-modified organopolysiloxane A1, the thermal conductivity of the obtained cured product becomes better, and when it is 3000 parts by weight or less, the decrease in fluidity can be more effectively suppressed and the coatability can be ensured.

[0035] (Surfactant C1) The surfactant C1 contains a copolymer (hereinafter referred to as "copolymer C") having an anionic group-containing (meth)acrylic monomer unit A, a cationic group-containing (meth)acrylic monomer unit B, and a silicone (meth)acrylic monomer unit C. By using such surfactant C1, the dispersibility of the thermally conductive filler B1 can be maintained even when the composition is kept at a high temperature for a long period of time, and the viscosity of the first agent can be kept low, thereby further improving the handleability of the composition set as a two-component curing type.

[0036] The content of the surfactant C1 is preferably 0.1 to 7.5 parts by weight, more preferably 0.5 to 5.0 parts by weight, and further preferably 1.0 to 3.0 parts by weight, based on 100 parts by weight of the content of the epoxy-modified organopolysiloxane A1. When the content of the surfactant C1 is within the above range, the dispersibility of the thermally conductive filler B1 at high temperatures is further improved, and the viscosity tends to be further reduced.

[0037] The content of the surfactant C1 is preferably 0.01 to 25 parts by weight, more preferably 0.01 to 15 parts by weight, and further preferably 0.01 to 5.0 parts by weight, relative to 100 parts by weight of the thermally conductive filler B1. When the content of the surfactant C1 is within the above range, the dispersibility of the thermally conductive filler B1 at high temperatures is further improved, and the viscosity tends to be further reduced.

[0038] The copolymer will be described below. In this embodiment, the term "monomer" refers to a monomer having a polymerizable unsaturated bond before polymerization, and the term "monomer unit" refers to a repeating unit that constitutes a part of copolymer C after polymerization and is derived from a specific monomer. In addition, (meth)acrylic includes acrylic and methacrylic, and (meth)acrylic monomers include (meth)acrylate and (meth)acrylamide. Furthermore, in the following, "(meth)acrylic monomer unit A" and the like will also be simply referred to as "unit A" and the like.

[0039] ((Meth)acrylic monomer unit A having an anionic group) The (meth)acrylic monomer unit A is a repeating unit having an anionic group. The anionic group is not particularly limited, but may be, for example, a carboxy group, a phosphoric acid group, a phenolic hydroxy group, or a sulfonic acid group. Among these, it is preferable that the anionic group is at least one selected from the group consisting of a carboxy group, a phosphoric acid group, and a phenolic hydroxy group. By having such a group, the dispersibility of the dispersoid tends to be further improved.

[0040] In addition, it is preferable that the unit A further has an electron-withdrawing group bonded to the anionic group. Such an electron-withdrawing group is not particularly limited as long as it has the effect of stabilizing the anion of the anionic group. For example, an acrylic monomer containing an electron-withdrawing substituent such as a halogen element on the carbon atom at the α-position of the carboxyl group may be used. By having such a group, the dispersibility of the dispersoid tends to be further improved.

[0041] It is preferable that the unit A does not have an electron-donating group bonded to the anionic group or has a group with low electron-donating ability. Such an electron-donating group is not particularly limited as long as it has the effect of destabilizing the anion of the anionic group. For example, an acrylic monomer that does not contain a substituent of an electron-donating group such as a methyl group on the carbon atom at the α-position of the carboxyl group may be used. By adopting such a structure, the dispersibility of the dispersoid tends to be further improved.

[0042] Such (meth)acrylic monomers are not particularly limited, but examples thereof include acrylic acid, methacrylic acid, acid phosphooxypropyl methacrylate, acid phosphooxy polyoxyethylene glycol monomethacrylate, acid phosphooxy polyoxypropylene glycol monomethacrylate, phosphoric acid modified epoxy acrylate, 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 4-hydroxyphenyl acrylate, 4-hydroxyphenyl methacrylate, 2-methacryloyloxyethyl succinic acid, 2-acrylamido-2-methylpropanesulfonic acid, etc. Among these, acrylic acid, 2-methacryloyloxyethyl acid phosphate, 4-hydroxyphenyl methacrylate, and 2-acrylamido-2-methylpropanesulfonic acid are preferred, and acrylic acid is more preferred. By including units derived from such monomers, the affinity to dispersoids is improved, and the dispersibility of dispersoids tends to be improved. The unit A may be used alone or in combination of two or more kinds.

[0043] ((Meth)acrylic Monomer Unit B Having a Cationic Group) The (meth)acrylic monomer unit B is a repeating unit having a cationic group. The cationic group is not particularly limited, but is preferably at least one selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt. Among these, a tertiary amino group is more preferable. By having such a group, the dispersibility of the dispersoid tends to be further improved.

[0044] In addition, the unit B preferably further has an electron-donating group bonded to the cationic group. Such an electron-donating group is not particularly limited as long as it has the effect of stabilizing the cation of the cationic group. For example, an acrylic monomer containing an electron-donating substituent such as a methyl group on the carbon atom at the α-position of the amino group may be used. By having such a group, the dispersibility of the dispersoid tends to be further improved.

[0045] It is preferable that the unit B does not have an electron-withdrawing group bonded to a cationic group or has a group with low electron-withdrawing ability. Such an electron-withdrawing group is not particularly limited as long as it has the effect of destabilizing the cation of the cationic group. For example, an acrylic monomer that does not contain a substituent of an electron-withdrawing group such as a carboxyl group on the carbon atom at the α-position of the amino group may be used. By adopting such a structure, the dispersibility of the dispersoid tends to be further improved.

[0046] Such (meth)acrylic monomers are not particularly limited, but examples thereof include 1-aminoethyl acrylate, 1-aminopropyl acrylate, 1-aminoethyl methacrylate, 1-aminopropyl methacrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, t-butylaminoethyl (meth)acrylate, dimethylaminoethyl methacrylate quaternary salt, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, 2,2,6,6-tetramethyl-4-piperidyl methacrylate, and dimethylaminoethyl acrylate benzyl chloride quaternary salt. Among these, 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and 1-aminoethyl methacrylate are preferred, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate is more preferred. By including units derived from such monomers, the affinity to dispersoids is improved, and the dispersibility of dispersoids tends to be improved. The unit B may be used alone or in combination of two or more kinds.

[0047] ((Meth)acrylic monomer unit C) The (meth)acrylic monomer unit C is a silicone (meth)acrylic monomer unit, which is a (meth)acrylic monomer that does not contain a cationic group or an anionic group in the molecule and has a silicone group.

[0048] In the case where the copolymer C is mixed into a resin composition containing a thermoplastic resin or a thermosetting resin, it is preferable that the (meth)acrylic monomer C has a skeleton having high affinity or compatibility with the resin used in the resin composition. The (meth)acrylic monomer C has a silicone skeleton such as dimethylsiloxane, methylphenylsiloxane, or diphenylsiloxane as such a skeleton. By having such a skeleton, the compatibility with the resin serving as the dispersion medium is improved, and the dispersibility of the dispersoid in the resin composition tends to be improved.

[0049] Such a (meth)acrylic monomer is not particularly limited, but examples thereof include (meth)acrylic monomers having a siloxane skeleton such as α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, etc. The unit C may be used alone or in combination of two or more kinds.

[0050] The number-average molecular weight of the (meth)acrylic monomer C is preferably 300 to 20,000, more preferably 1,000 to 15,000, and even more preferably 3,000 to 12,500. When the number-average molecular weight of the (meth)acrylic monomer C is 300 or more, the affinity to the dispersion medium is improved, and the dispersibility of the dispersoid tends to be improved. In addition, when the number-average molecular weight of the (meth)acrylic monomer C is 20,000 or less, the viscosity of the composition obtained when the copolymer C is mixed with other resins and other components is reduced, and the handleability tends to be improved.

[0051] The total content of the units A and the units B is preferably 0.05 to 90 mol%, more preferably 0.2 to 80 mol%, and even more preferably 0.5 to 75 mol% relative to the total of 100 mol% of the units A, the units B, and the units C. When the total content of the units A and the units B is 0.05 mol% or more, the affinity to the dispersion medium is improved and the dispersibility of the dispersoid tends to be improved. In addition, when the total content of the units A and the units B is 90 mol% or less, the viscosity of the first agent is reduced and the handleability tends to be improved.

[0052] The content of the unit A is preferably 0.03 to 85 mol%, more preferably 0.05 to 80 mol%, and even more preferably 0.10 to 75 mol%, based on 100 mol% in total of the unit A, the unit B, and the unit C. When the content of the unit A is 0.03 mol% or more, the affinity to the dispersion medium is improved and the dispersibility of the dispersoid tends to be improved. Also, when the content of the unit A is 85 mol% or less, the viscosity of the first agent is reduced and the handleability tends to be improved.

[0053] The molar ratio of units A to units B is preferably 0.01 to 150, more preferably 0.05.0 to 50, and further preferably 1.0 to 40. When the molar ratio of units A to units B is within the above range, the affinity to the dispersion medium is further improved, and the dispersibility of the dispersoid tends to be further improved.

[0054] The content of the unit B is preferably 0.05 to 10 mol%, more preferably 0.1 to 7.5 mol%, and even more preferably 0.5 to 5.0 mol%, based on 100 mol% in total of the unit A, the unit B, and the unit C. When the content of the unit B is 0.05 mol% or more, the affinity for the filler tends to be improved. Also, when the content of the unit B is 10 mol% or less, the viscosity of the first agent tends to be reduced, and the handleability tends to be improved.

[0055] The content of the unit C is preferably 10 to 99.5 mol%, more preferably 20 to 99.5 mol%, and even more preferably 25 to 99 mol%, based on 100 mol% in total of the unit A, the unit B, and the unit C. When the content of the unit C is 10 mol% or more, the viscosity of the first agent tends to be further reduced and the handling property tends to be further improved. Also, when the content of the unit C is 99.5 mol% or less, the affinity for the filler tends to be further improved.

[0056] The weight average molecular weight of the copolymer C is preferably 5,000 to 500,000, more preferably 7,000 to 150,000, and further preferably 10,000 to 100,000. By having the weight average molecular weight of the copolymer C of 5000 or more, the dispersibility can be maintained even when the composition is kept at a high temperature for a long time, and the hardness of the composition can be suppressed from increasing. In addition, by having the weight average molecular weight of the copolymer C of 5000 or more, the shape retention of the composition when blended with the thermally conductive filler (c) or a resin is improved, and the resistance to slippage and dripping of the composition when applied to an inclined or vertical surface is improved. In addition, by having the weight average molecular weight of the copolymer C of 500,000 or less, the viscosity of the composition obtained when the copolymer C is mixed with other resins or other components is further reduced, and the handleability tends to be further improved. The weight average molecular weight can be determined by GPC (gel permeation chromatography).

[0057] [Method for producing copolymer C] The method for producing the copolymer C of the present embodiment is not particularly limited, and a known polymerization method for a (meth)acrylic monomer can be used. Examples of the polymerization method include radical polymerization and anionic polymerization. Among these, radical polymerization is preferred.

[0058] The thermal polymerization initiator used in the radical polymerization is not particularly limited, but may be, for example, an azo compound such as azobisisobutyronitrile; an organic peroxide such as benzoyl peroxide, tert-butyl hydroperoxide, or di-tert-butyl peroxide. The photopolymerization initiator used in the radical polymerization is not particularly limited, but may be, for example, a benzoin derivative. In addition, known polymerization initiators used in living radical polymerization such as ATRP or RAFT may also be used.

[0059] The polymerization conditions are not particularly limited, and can be appropriately adjusted depending on the initiator and boiling point of the solvent used, as well as the types of other monomers.

[0060] The order of addition of the monomers is not particularly limited. For example, from the viewpoint of synthesizing a random copolymer, the monomers may be mixed together to initiate polymerization, or from the viewpoint of synthesizing a block copolymer, the monomers may be added sequentially to the polymerization system.

[0061] (Polydimethylsiloxane D) Polydimethylsiloxane D can be added to adjust the viscosity of the first agent and the hardness of the resulting cured product. The viscosity of the polydimethylsiloxane is not particularly limited, and multiple types of polydimethylsiloxanes with different viscosities may be used in combination.

[0062] The content of polydimethylsiloxane D is preferably 0 to 80 parts by weight per 100 parts by weight of the total of the epoxy-modified organopolysiloxane A1 and polydimethylsiloxane D.

[0063] (Organosilane E) Organosilane E can be added to adjust the wettability between the thermally conductive filler B1 and the epoxy-modified organopolysiloxane A1. Although there is no particular limitation on such organosilane, for example, an organosilane represented by the following general formula (e) is preferably used. R 3 a R 4 b Si(OR 5 ) 4-(a+b) (e) (In the formula, R 3 each independently represents an alkyl group having 1 to 15 carbon atoms; R 4 each independently represents an unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms; R 5 each independently represents an alkyl group having 1 to 6 carbon atoms, a is an integer of 1 to 3, b is an integer of 0 to 2, and a+b is an integer of 1 to 3.

[0064] In formula (e), R 3The alkyl group having 1 to 15 carbon atoms represented by is not particularly limited, but examples thereof include a methyl group, an ethyl group, a propyl group, a hexyl group, a nonyl group, a decyl group, a dodecyl group, a tetradecyl group, a 3,3,3-trifluoropropyl group, a 2-(perfluorobutyl)ethyl group, and a 2-(perfluorooctyl)ethyl group. 3 is preferably an alkyl group having 6 to 12 carbon atoms.

[0065] R 4 The unsaturated monovalent hydrocarbon group having 1 to 8 carbon atoms represented by is not particularly limited, and examples thereof include alkenyl groups such as vinyl group, allyl group, etc.; aryl groups such as phenyl group, tolyl group, etc.; aralkyl groups such as 2-phenylethyl group, 2-methyl-2-phenylethyl group, etc.; and halogenated hydrocarbon groups such as p-chlorophenyl group, etc.

[0066] R 5 The alkyl group having 1 to 6 carbon atoms represented by is not particularly limited, but examples thereof include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group. 5 is preferably a methyl group or an ethyl group.

[0067] a is an integer of 1 to 3, and preferably 1. b is an integer of 0 to 2, and preferably 0. a+b is an integer of 1 to 3, and preferably 1.

[0068] The content of the organosilane E is preferably 0.01 to 30 parts by weight, more preferably 0.1 to 5.0 parts by weight, based on 100 parts by weight of the epoxy-modified organopolysiloxane A1. When the content of the organosilane E is within the above range, the wettability can be effectively improved.

[0069] (Colorant F) There is no particular limitation on the colorant F, and examples thereof include any pigment. There is no particular limitation on the content of colorant F, and for example, it is preferably 0.05 to 0.2 parts by weight with respect to 100 parts by weight in total of the first agent and the second agent described below.

[0070] <Second Agent> The second agent contains an amino-modified organopolysiloxane A2 having an amino group-containing group, a thermally conductive filler B2, and a surfactant C2, and may contain additives such as polydimethylsiloxane D, organosilane E, and colorant F, as necessary.

[0071] (Amino-modified organopolysiloxane A2) The amino-modified organopolysiloxane A2 of this embodiment has a substituent (amino group-containing group) having an amino group at the end or in the side chain. The organopolysiloxane having an amino group is one in which at least a part of the R in the Si-R portion (wherein R is a substituted or unsubstituted monovalent hydrocarbon group) in the organopolysiloxane molecule is a substituent having an amino group.

[0072] The amino group-containing group is not particularly limited, and examples thereof include the amino group represented by the following formula (a21): Such an amino group-containing group may be a primary amino group or a secondary amino group, and among these, R 6 is preferably a primary amino group in which R is a hydrogen atom. [ka] (In the formula, R 6 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, the hydrogen atom of which may be substituted with an amino group; R 7 represents an alkyl group having 1 to 6 carbon atoms.

[0073] R 6 R represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, the hydrogen atom of which may be substituted with an amino group. 6 When R is a hydrogen atom, the amino group represented by formula (a21) has a primary amino group at the terminal, such as a 3-aminopropyl group. 6 When R is an alkyl group having 1 to 6 carbon atoms, the amino group represented by formula (a21) has a secondary amino group. 6When the alkyl group represented by formula (a21) is an alkyl group having 1 to 6 carbon atoms in which a hydrogen atom is substituted with an amino group, the amino group represented by formula (a21) is a group having a primary amino group and a secondary amino group, such as an aminoethylaminopropyl group, a group having multiple primary amino groups, or a group having multiple secondary amino groups.

[0074] The amino-modified organopolysiloxane A2 may have any of a linear structure, a branched structure, and a cyclic structure, and may have a structure in which a linear structure and a cyclic structure are combined, or a structure in which a branched structure and a cyclic structure are combined. Among these, a linear structure is preferred from the viewpoint of handling as a liquid, and a branched structure is preferred from the viewpoint of the mechanical properties of the obtained cured product.

[0075] The bonding position of the amino group-containing group in the amino-modified organopolysiloxane A2 is not particularly limited, and may be a terminal or a side chain, or may be a terminal and a side chain. When the amino group-containing group is present in the side chain, the amino-modified organopolysiloxane A2 has, for example, a structural unit represented by the following general formula (a2-1) or (a2-2). When the amino group-containing group is present in the terminal, the amino-modified organopolysiloxane A2 has, for example, a terminal structure represented by the following general formula (a2-3) (wherein m is 1 or more). Furthermore, as a structural unit to which an amino group-containing group is not bonded, a structural unit represented by the following general formula (a2-4) can be given. The structural units that the amino-modified organopolysiloxane A2 has are not limited to the following, and for example, when the amino-modified organopolysiloxane A2 has a branched structure, it may have a branched structural unit, and when the amino-modified organopolysiloxane A2 has a cyclic structure, it may not have a terminal structure. [ka] (In the formula, each Y independently represents an amino group-containing group; R 8 each independently represents a substituted or unsubstituted hydrocarbon group having 1 to 12 carbon atoms, and m represents an integer of 0 to 3.

[0076] R 8The substituted or unsubstituted hydrocarbon group represented by the formula (I) is not particularly limited, and examples thereof include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl groups; and halogenated alkyl groups such as chloromethyl, 3,3,3-trifluoropropyl, and 3-chloropropyl groups.

[0077] Among these, the amino-modified organopolysiloxane A2 is preferably an organopolysiloxane having a linear structure with an amino group-containing group at the end or in the side chain, or an organopolysiloxane having a linear structure with a hydroxyl group at the end and an amino group-containing group in the side chain. By using such an amino-modified organopolysiloxane A2, the reactivity of the first agent and the second agent tends to be further improved.

[0078] The amino functional equivalent of the amino group of the amino-modified organopolysiloxane A2 is preferably 100 to 8000 g / mol, more preferably 200 to 6000 g / mol, more preferably 300 to 4000 g / mol, and even more preferably 300 to 2000 g / mol. When the amino functional equivalent is within the above range, the reactivity of the first agent and the second agent is improved, and the uniform reactivity tends to be improved.

[0079] The viscosity of the amino-modified organopolysiloxane A2 at 25° C. is preferably 5 to 2000 mm 2 / s, more preferably 5 to 1750 mm 2 / s, and more preferably 5 to 1500 mm 2 When the viscosity is within the above range, the handleability of the two-component curing composition set tends to be improved.

[0080] In addition, the amino-modified organopolysiloxane A2 preferably further has a hydroxyl-containing group in which a hydroxyl group is bonded to a silicon atom. The bonding position of the hydroxyl-containing group is not particularly limited, and may be at the end or the side chain, or at the end and the side chain. Among these, the amino-modified organopolysiloxane A2 having a linear structure with amino-containing groups at both ends is preferred. By using such an amino-modified organopolysiloxane A2, the compatibility with the epoxy-modified organopolysiloxane A1 is further improved, and the uniform reactivity tends to be further improved.

[0081] (Thermal conductive filler B2) The thermally conductive filler B2 is, for example, a filler having a thermal conductivity of 10 W / m·K or more, and may be the same as the thermally conductive filler B1. Among these, it is preferable to include at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, copper, silver, and diamond. By using such a thermally conductive filler B2, the filling property is improved, and the thermal conductivity of the obtained cured product tends to be further improved. These thermally conductive fillers B2 may be used alone or in combination of two or more.

[0082] The average particle size and content of the thermally conductive filler B2 may be the same as those of the thermally conductive filler B1, and the above descriptions regarding the thermally conductive filler B1 may be read and applied to the thermally conductive filler B2.

[0083] (Surfactant C2) The surfactant C2 may be the same as the surfactant C1. By using the surfactant C2, the dispersibility of the thermally conductive filler B2 is improved, and the viscosity of the second agent is reduced, which tends to improve the ease of handling.

[0084] The content of surfactant C2 is preferably 0.1 to 7.5 parts by weight, more preferably 0.5 to 5.0 parts by weight, and even more preferably 1.0 to 3.0 parts by weight, based on 100 parts by weight of the content of amino-modified organopolysiloxane A2. When the content of surfactant C2 is within the above range, the dispersibility of thermally conductive filler B2 at high temperatures is further improved, and the viscosity tends to be further reduced.

[0085] The content of surfactant C2 is preferably 0.01 to 25 parts by weight, more preferably 0.01 to 15 parts by weight, and even more preferably 0.01 to 5.0 parts by weight, relative to 100 parts by weight of the content of thermally conductive filler B2. By having the content of surfactant C2 within the above range, the dispersibility of thermally conductive filler B2 at high temperatures is further improved, and the viscosity tends to be further reduced.

[0086] (Additives) In addition, polydimethylsiloxane D, organosilane C, and colorant F that may be contained in the second agent are the same as those in the first agent described above, and the descriptions regarding these in the first agent can be read and applied as those regarding the second agent, so duplicate descriptions will be omitted here.

[0087] In addition, the thermally conductive filler, surfactant, polydimethylsiloxane, organosilane, and colorant as the second agent and the thermally conductive filler, surfactant, polydimethylsiloxane, organosilane, and colorant as the first agent may be of the same type or of different types.

[0088] <Ratio of first and second agent> In the two-component curing composition set of this embodiment, the mixing ratio of the epoxy-modified organopolysiloxane A1 in the first agent and the amino-modified organopolysiloxane A2 in the second agent can be appropriately set depending on the epoxy group content of the epoxy-modified organopolysiloxane A1 in the first agent and the amino group content of the amino-modified organopolysiloxane A2 in the second agent. Epoxy group content = epoxy-modified organopolysiloxane A1 content / functional group equivalent Amino group content = Amino-modified organopolysiloxane A2 content / Functional group equivalent

[0089] The ratio of epoxy group content / amino group content satisfied by the combination of the first agent and the second agent is preferably 70 / 30 to 10 / 90, more preferably 55 / 45 to 20 / 80. When the ratio of epoxy group content to amino group content is within the above range, uniform reactivity is improved, and a cured product with a sufficiently formed crosslinked structure can be obtained.

[0090] <Application> The two-component curing composition set of the present embodiment can be suitably used as a thermally conductive heat dissipating material.

[0091] [Cured product] The cured product according to this embodiment can be obtained, for example, by mixing the first and second parts in the two-part curing composition set described above. More specifically, the cured product (crosslinked cured product) is obtained by mixing the first and second parts in a mixture obtained by mixing the first and second parts, and an addition reaction between the epoxy group of the epoxy-modified organopolysiloxane A1 contained in the first part and the amino group of the amino-modified organopolysiloxane A2 contained in the second part progresses to form a three-dimensional network structure having crosslinked bonds, thereby obtaining the cured product.

[0092] The cured product of the present embodiment may be molded into a desired shape after mixing the first and second parts. In addition, since the cured product of the present embodiment contains a thermally conductive filler, it can be suitably used as a thermally conductive heat dissipation material.

[0093] For mixing, a mixer such as a roll mill, kneader, Banbury mixer, or line mixer is used, and examples of the method include a method of kneading using a universal mixer, hybrid mixer, Trimix (manufactured by Inoue Seisakusho), or a static mixer. The molding method is preferably a doctor blade method, but depending on the viscosity of the resin, an extrusion method, a press method, or a calendar roll method can be used. The reaction conditions for the progression of the addition reaction are not particularly limited, but are usually performed at room temperature (e.g., 25°C) to 150°C for 0.1 to 24 hours.

[0094] The mixing ratio of the first agent and the second agent can be appropriately set depending on the type of the first agent and the second agent used and the purpose of use, but for example, the volume ratio of first agent:second agent may be 1.5:1.0 to 1.0:1.5, or may be 1.0:1.0.

[0095] [Electronic equipment] The electronic device of the present embodiment includes an electronic component, the above-mentioned cured product, and a housing that houses the electronic component and the cured product, the electronic component and the housing being in contact with each other via the cured product.

[0096] Here, the electronic components are not particularly limited, but examples thereof include heat-generating electronic components such as motors, battery packs, circuit boards for on-board power supply systems, power transistors, microprocessors, etc. Furthermore, the metal housing is not particularly limited, but examples thereof include heat sinks configured for the purpose of dissipating or absorbing heat. EXAMPLES

[0097] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.

[0098] [Surfactant synthesis example] <Raw materials> ((Meth)acrylic monomer A having an anionic group) (A-1) Acrylic acid, manufactured by Toagosei Co., Ltd. (A-2) 4-Hydroxyphenyl methacrylate, manufactured by Seiko Chemical Co., Ltd. (A-3) 2-Methacryloyloxyethyl acid phosphate, "Light Ester P-1M" manufactured by Kyoeisha Chemical Co., Ltd. (A-4) 2-acrylamido-2-methylpropanesulfonic acid, manufactured by Tokyo Chemical Industry Co., Ltd. ((Meth)acrylic monomer B having a cationic group) (B-1) 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, "ADEKA STAB LA-82" manufactured by ADEKA Corporation (B-2) 1-aminoethyl methacrylate, manufactured by Tokyo Chemical Industry Co., Ltd. ((Meth)acrylic monomer C) (C-1) α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, JNC Corporation "Silaplane FM-0711" number-average molecular weight 1,000 (C-2) α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane), JNC Corporation "Silaplane FM-0721", number-average molecular weight 5,000 (C-3) α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane, JNC Corporation "Silaplane FM-0725" number-average molecular weight 10,000

[0099] (Copolymer 1) Preparation of surfactant copolymer 1 was carried out by the following method. First, 100 parts by weight of (meth)acrylic monomer consisting of 15 mol% acrylic acid, 0.1 mol% methacrylate-1,2,2,6,6-pentamethyl-4-piperidyl, and 84.9 mol% α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane was added to an autoclave equipped with a stirrer. Next, 0.05 parts by weight of azobisisobutyronitrile (manufactured by Tokyo Chemical Industry Co., Ltd.) was added as an initiator relative to 100 parts by weight of the total of (meth)acrylic monomers, and 1000 parts by weight of a mixed solution of toluene (special reagent grade) and 2-propanol (special reagent grade) in a volume ratio of 7:3 was added as a solvent, and the inside of the autoclave was replaced with nitrogen. After that, the autoclave was heated in an oil bath at 65°C for 20 hours to carry out radical polymerization. After the polymerization was completed, the mixture was degassed at 120°C under reduced pressure for 1 hour to obtain copolymer 1.

[0100] The polymerization rate was 98% or more when analyzed by gas chromatography based on 100% of the monomer charge, which suggested that the ratio of each monomer unit in the copolymer was approximately the same as the monomer charge ratio.

[0101] The weight average molecular weight of the obtained copolymer 1 was determined as a weight average molecular weight converted into standard polystyrene by using a GPC (gel permeation chromatography) method under the following measurement conditions. High-speed GPC equipment: Tosoh Corporation "HLC-8020" Columns: One Tosoh "TSK guardcolumn MP(xL)" 6.0mmID x 4.0cm, and two Tosoh "TSK-GELMULTIPOREHXL-M" 7.8mmID x 30.0cm (16,000 theoretical plates), for a total of three (total theoretical plates: 32,000) Developing solvent: Tetrahydrofuran Detector: RI (Differential Refractometer)

[0102] (Copolymer 2~18) Radical polymerization was carried out in the same manner as for copolymer 1, except that the monomers shown in Table 1 were used, to obtain copolymers 2 to 18. The polymerization rates of the obtained copolymers 2 to 18 were all 98% or more, and the ratios of the monomer units contained in the copolymers were estimated to be approximately the same as the monomer charge ratios. The weight average molecular weights were also determined in the same manner as above.

[0103] The monomer compositions shown in Table 1 are shown as molar ratios (%). The molar ratios were calculated from the amount and molecular weight of each monomer. The molar ratio of α-butyl-ω-(3-methacryloxypropyl)polydimethylsiloxane was calculated based on its weight average molecular weight.

[0104] [Table 1]

[0105] [First agent] The following A1 component to D1 component were mixed based on the compounding ratios (parts by weight) shown in Table 2 to prepare the first agents I-1 to I-21. The mixing of each component was carried out using a hybrid mixer ARE-310 (manufactured by Shin-Kee Co., Ltd., trade name). <A1 component: Organopolysiloxane> A1-1: DOWSIL BY 8411 Fluid (manufactured by Dow Corning Toray Co., Ltd., trade name), epoxy-modified organopolysiloxane, viscosity at 25°C: 8000 mm 2 / s, functional group equivalent of epoxy group: 3300 g / mol, aliphatic type (glycidyl group), epoxy group bonding position: side chain A1-2: DOWSIL SE 1885A (manufactured by Dow Corning Toray Co., Ltd., trade name) organopolysiloxane having a vinyl group (containing a platinum catalyst)

[0106] <B1 component: Thermal conductivity filler> B1-1: Spherical alumina, average particle size: 45 μm, DAW45S (manufactured by Denka Co., Ltd., trade name), thermal conductivity 35 W / mK B1-2: Spherical alumina, average particle size: 5 μm, DAW05 (manufactured by Denka Co., Ltd., trade name), thermal conductivity 35 W / mK

[0107] <C1 component: Surfactant> (C1-1 to C1-18) Copolymers 1 to 18 obtained by the above synthesis examples (C1-19) n-decyltrimethoxysilane: manufactured by Dow Corning Toray Co., Ltd., "DOWSIL Z6210"

[0108] <D1 component: Colorant> D1: Resin Black #442 (manufactured by Resin Color Industry Co., Ltd., trade name)

[0109]

Table 2

[0110] [Second agent] The A2 component to C2 component shown below were mixed based on the compounding ratios (parts by weight) described in Table 3 to prepare the second agents II-1 to II-22. The mixing was carried out using a hybrid mixer ARE-310 (manufactured by Shin-Kee Co., Ltd., trade name).

[0111] <A2 component: Organopolysiloxane> A2-1: DOWSIL BY 16-213 (manufactured by Dow Corning Toray Co., Ltd., trade name), amino-modified organopolysiloxane, viscosity at 25°C: 60 mm 2 / s, functional group equivalent of amino group: 2700 g / mol, primary amine (3-aminopropyl group), amino group bonding position: side chain A2-2: DOWSIL BY 16-892 (manufactured by Dow Corning Toray Co., Ltd., trade name), amino-modified organopolysiloxane, viscosity at 25°C 1400 mm 2 / s, functional group equivalent of amino group 1900 g / mol, primary amine and secondary amine (aminoethylaminopropyl group), amino group bonding position: side chain, both ends OH-containing A2-3: DOWSIL SE 1885B (manufactured by Dow Corning Toray Co., Ltd., trade name) A mixture of an organopolysiloxane having a vinyl group and an organopolysiloxane having a hydrosilyl group

[0112] <B2 component: Thermal conductive filler> B2-1: Spherical alumina, average particle size: 45 μm, DAW45S (manufactured by Denka Co., Ltd., trade name) B2-2: Spherical alumina, average particle size: 5 μm, DAW05 (manufactured by Denka Co., Ltd., trade name)

[0113] <C2 component: Surfactant> (C2-1 to C2-18) Copolymers 1 to 18 obtained by the above synthesis examples (C2-19) n-decyltrimethoxysilane: manufactured by Dow Corning Toray Co., Ltd., "DOWSIL Z6210"

[0114]

Table 3

[0115] [viscosity] The viscosities of the above A1 and A2 components were measured using a "Digital Viscometer DV-1" (product name) manufactured by Brookfield Corp. Specifically, an RV spindle set was used, rotor No. 1 was used, and a container was used that could accommodate the rotor and hold the evaluation sample up to the reference line, and the rotor was immersed in the evaluation sample, and the viscosity was measured at 25°C and 10 rpm.

[0116] In addition, the first and second agents were subjected to 25°C and a shear rate of 10 s -1 The viscosity at 100°C was measured using a rotational rheometer "HANKE MARSIII" manufactured by Thermo Fisher Scientific. Specifically, parallel plates with a diameter of 35 mm were used, with a gap of 0.5 mm, a temperature of 25°C, and a shear rate of 10 s -1 The measurements were performed under the following conditions.

[0117] [Measurement of average particle size] The average particle size of the thermally conductive filler was measured using a laser diffraction particle size distribution analyzer SALD-20 (product name) manufactured by Shimadzu Corporation. For the evaluation sample, 50 ml of pure water and 5 g of the thermally conductive filler powder to be measured were added to a glass beaker, stirred with a spatula, and then dispersed in an ultrasonic cleaner for 10 minutes. The solution of the dispersed thermally conductive filler powder was added drop by drop to the sampler part of the device using a dropper, and measurement was performed when the absorbance stabilized. In the laser diffraction particle size distribution analyzer, the particle size distribution is calculated from the data of the light intensity distribution of the diffraction / scattering holes by the particles detected by the sensor. The average particle size is calculated by multiplying the measured particle size value by the relative particle amount (difference %) and dividing it by the total relative particle amount (100%). The average particle size is the average diameter of the particles, and can be calculated as the cumulative weight average value D50 (or median diameter), which is the maximum value or peak value. The D50 is the particle size with the highest occurrence rate.

[0118] [Cured product] The first and second parts obtained above were mixed in a volume ratio of 50:50 in the combination shown in Table 4 to obtain a mixture. The mixture obtained was held at 150°C for 1 hour to allow the curing reaction to proceed, and a cured product was obtained. The curing reaction was evaluated according to the following methods. The evaluation results are summarized in Tables 3 and 4.

[0119] <Evaluation of uniform reactivity> The mixture of the first and second parts was molded into a shape of about 5 mm thick and 2 cm long and wide, and was held at 150°C for 1 hour to allow the curing reaction to proceed, yielding a cured product. Differences in the cured state depending on the location of the obtained cured product were confirmed, and whether the curing reaction had proceeded uniformly throughout the entire cured product (uniform reactivity) was evaluated according to the following criteria. (Evaluation Criteria) ◎: Completely cured, with the center and edges having the same hardness 〇: Completely cured, but the center was slightly softer than the edges. ×: Not cured

[0120] <Evaluation of dispersion stability> The first and second agents were each stored in a heated state for 100 hours in a dryer at 150° C. The aggregation state of the filler in the first and second agents after the heated storage was confirmed, and the dispersion stability was evaluated according to the following criteria. (Evaluation Criteria) ○: No filler aggregation ×: Filler aggregates

[0121] [Table 4] [Industrial Applicability]

[0122] The two-component curing thermally conductive grease composition of the present invention has industrial applicability as a thermally conductive cured product obtained by mixing and curing the first and second parts, in particular as a thermally conductive grease material used to thermally bond a heating element and a metal housing.

Claims

1. A first agent including an epoxy-modified organopolysiloxane A1 having an epoxy group-containing group, a thermally conductive filler B1, and a surfactant C1; a second agent including an amino-modified organopolysiloxane A2 having an amino group-containing group, a thermally conductive filler B2, and a surfactant C2; the surfactant C1 and the surfactant C2 each comprise a copolymer having (meth)acrylic monomer units A having, as an anionic group, one or more selected from the group consisting of a carboxy group, a phosphate group, and a phenolic hydroxy group, (meth)acrylic monomer units B having, as a cationic group, one or more selected from the group consisting of a primary amino group, a secondary amino group, a tertiary amino group, and a quaternary ammonium salt, and a silicone (meth)acrylic monomer unit C not containing a cationic group or an anionic group in the molecule; The weight average molecular weight of the copolymer is 5,000 to 500,000. Two-part curing composition set.

2. with respect to a total of 100 mol % of the (meth)acrylic monomer unit A, the (meth)acrylic monomer unit B, and the silicone (meth)acrylic monomer unit C, The content of the (meth)acrylic monomer unit A is 0.03 to 85 mol %, The content of the (meth)acrylic monomer unit B is 0.05 to 10 mol %, and the content of the silicone (meth)acrylic monomer unit C is 10 to 99.5 mol %. The two-component curing composition set according to claim 1 .

3. the content of the surfactant C1 in the first agent is 0.01 to 25 parts by weight based on 100 parts by weight of the thermally conductive filler B1 in the first agent; The content of the surfactant C2 in the second agent is 0.01 to 25 parts by weight relative to 100 parts by weight of the thermally conductive filler B2 in the second agent. The two-component curing composition set according to claim 1 or 2.

4. The epoxy group equivalent weight in one molecule of the epoxy-modified organopolysiloxane A1 is 100 to 11,000 g / mol. The two-component curing composition set according to any one of claims 1 to 3.

5. The amino group equivalent weight in one molecule of the amino-modified organopolysiloxane A2 is 100 to 8000 g / mol. The two-component curing composition set according to any one of claims 1 to 4.

6. The amino-modified organopolysiloxane A2 in the second agent has hydroxyl group-containing groups at both ends. The two-component curing composition set according to any one of claims 1 to 5.

7. The thermally conductive filler B1 and the thermally conductive filler B2 each contain at least one selected from the group consisting of aluminum oxide, aluminum nitride, boron nitride, silicon nitride, zinc oxide, aluminum hydroxide, metallic aluminum, magnesium oxide, copper, silver, and diamond, each of which has a thermal conductivity of 10 W / m·K or more. The two-component curing composition set according to any one of claims 1 to 6.

8. The first agent does not contain an organopolysiloxane having at least a vinyl group at the end or in a side chain, and an organopolysiloxane having at least a hydrosilyl group at the end or in a side chain; and The second agent is provided with an organopolysiloxane having at least a vinyl group at the end or in a side chain, and the second agent does not include an organopolysiloxane having at least a hydrosilyl group at the end or in a side chain. The two-component curing composition set according to any one of claims 1 to 7.

9. Used as a thermally conductive heat dissipation material, The two-component curing composition set according to any one of claims 1 to 8.

10. The two-component curing composition set according to any one of claims 1 to 9, wherein the first component and the second component are mixed together, cured product.

11. Used as a thermally conductive heat dissipation material, The cured product according to claim 10.

12. An electronic component, the cured product according to claim 11, and a housing that houses the electronic component and the cured product, The electronic component and the housing are in contact with each other via the cured product. electronic equipment.

Citation Information

Patent Citations

  • Two-component pouring sealant and preparation method thereof

    CN107325782A

  • Liquid silicone rubber composition

    JP1985179417A

  • Fluorine based surfactant having low foaming characteristic

    JP1991030825A

  • Preparation of metal-graphite laminated material

    JP1994321518A

  • Silicone rubber composition and its use

    JP1997296114A