Substrate with multilayer reflective film for EUV mask blank, manufacturing method thereof and EUV mask blank

By integrating a Si/N layer between Si and Mo layers and a Ru protective layer, the multilayer reflective film in EUV mask blanks maintains high reflectance despite heat exposure, addressing interdiffusion issues and ensuring consistent performance.

JP7577486B2Active Publication Date: 2024-11-05SHIN ETSU CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020151705
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-10
Publication Date
2024-11-05
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

The multilayer reflective film in EUV mask blanks experiences a decrease in reflectance due to interdiffusion between Mo and Si layers, which is exacerbated by heat during processing or exposure, leading to reduced performance.

Method used

Incorporating a layer containing Si and N between the Si and Mo layers, and using a Ru-containing protective layer on top, along with specific sputtering methods to form the multilayer reflective film, prevents interdiffusion and maintains high reflectance.

Benefits of technology

The solution maintains a high reflectance of 65% or more for EUV light even after heat treatment, ensuring consistent performance of the EUV mask blanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007577486000001
    Figure 0007577486000001
  • Figure 0007577486000002
    Figure 0007577486000002
  • Figure 0007577486000003
    Figure 0007577486000003
Patent Text Reader

Abstract

SOLUTION: To provide a substrate with a multilayer reflection film for an EUV mask blank that includes a substrate and a multilayer reflection film formed on the substrate, wherein the multilayer reflection film includes a Si / Mo laminated portion in which Si layers and Mo layers are alternately laminated, wherein a layer containing Si and N is formed at one or more portions between the Si layer and the Mo layer of the Si / Mo laminated portion, so as to be in contact with both of the Si layer and the Mo layer.EFFECT: It is possible to provide a substrate with a multilayer reflection film for an EUV mask blank, having the multilayer reflection film that has high reflectance and barely shows a decrease in reflectance even when it is heated, and provide the EUV mask blank.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an EUV mask blank that is a material for EUV masks used in the manufacture of semiconductor devices such as LSIs, a multilayer reflective film-coated substrate for an EUV mask blank that is used in the manufacture of the EUV mask blank, and a method for manufacturing the same. [Background technology]

[0002] In the manufacturing process of semiconductor devices (semiconductor device), photolithography technology is repeatedly used, in which exposure light is irradiated onto a transfer mask, and the circuit pattern formed on the mask is transferred onto a semiconductor substrate (semiconductor wafer) via a reduced projection optical system. Conventionally, the wavelength of the exposure light has mainly been 193 nm using argon fluoride (ArF) excimer laser light, and a process called multi-patterning, which combines exposure processes and processing processes multiple times, has been used to ultimately form patterns with dimensions smaller than the exposure wavelength.

[0003] However, as the device patterns continue to become finer, the formation of even finer patterns is required, and thus EUV lithography technology using EUV (Extreme Ultra Violet) light, which has a shorter wavelength than ArF excimer laser light, as exposure light has been developed. EUV light is light with a wavelength of, for example, about 10 to 20 nm, more specifically, light with a wavelength of about 13.5 nm. This EUV light has extremely low permeability to materials, and conventional transmission type projection optical systems and masks cannot be used, so reflective optical elements are used. For this reason, reflective masks have been proposed as masks for pattern transfer. In a reflective mask, a multilayer reflective film that reflects EUV light is formed on a substrate, and an absorber film that absorbs EUV light is formed in a pattern on the multilayer reflective film. On the other hand, a mask in a state before patterning the absorber film (including a state in which a resist layer is formed) is called a reflective mask blank, and this is used as a material for a reflective mask. In general, a reflective mask and a reflective mask blank that reflect EUV light are called an EUV mask and an EUV mask blank, respectively.

[0004] The EUV mask blank has a basic structure including a low thermal expansion substrate, a multilayer reflective film formed thereon to reflect EUV light, and an absorber film formed thereon to absorb EUV light. As the multilayer reflective film, a Mo / Si multilayer reflective film is usually used, which obtains the necessary reflectance for EUV light by alternately laminating molybdenum (Mo) films and silicon (Si) films. Furthermore, as a protective film for protecting the multilayer reflective film, a ruthenium (Ru) film or a film made of a mixture of Ru with niobium (Nb) or zirconium (Zr) is formed on the outermost layer of the multilayer reflective film. On the other hand, as the absorber film, a material mainly composed of tantalum (Ta) or chromium (Cr), which has a relatively large extinction coefficient for EUV light, is used. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2005-516182 [Patent Document 2] International Publication No. 2015 / 012151 Summary of the Invention [Problem to be solved by the invention]

[0006] Multilayer reflective films are required to have high reflectance against EUV light, but in the area where Mo layers and Si layers are alternately laminated, an interdiffusion layer is formed between the Mo layers and the Si layers, which is a mixture of the components of both layers, Si and Mo, and only a low reflectance is obtained that deviates from the theoretical reflectance obtained by laminating Mo layers and Si layers. In addition, if heat is applied to the multilayer reflective film during the mask processing process or exposure to EUV light using a mask, the interdiffusion layer will thicken or change, resulting in a further decrease in reflectance.

[0007] The present invention has been made to solve the above-mentioned problems, and has an object to provide a multilayer reflective film-coated substrate for an EUV mask blank, which has a multilayer reflective film that has high reflectance and is not prone to decrease in reflectance even when heat is applied, a manufacturing method thereof, and an EUV mask blank. [Means for solving the problem]

[0008] As a result of extensive investigations to solve the above-mentioned problems, the inventors have found that a Si / Mo laminate portion constituting a multilayer reflective film used in an EUV mask blank is configured by alternately laminating Si layers and Mo layers, and a layer containing Si and N is formed in contact with both the Si layer and the Mo layer at least one between the Si layer and the Mo layer, and preferably, the multilayer reflective film is configured to include such a Si / Mo laminate portion and a protective layer containing Ru formed in contact with the Si / Mo laminate portion as an uppermost layer of the multilayer reflective film, thereby providing a multilayer reflective film-coated substrate for an EUV mask blank and an EUV mask blank having a multilayer reflective film that has high reflectivity and is resistant to deterioration in reflectivity even when heat is applied, and have thus completed the present invention.

[0009] Therefore, the present invention provides the following multilayer reflective film-coated substrate for an EUV mask blank, a manufacturing method thereof, and an EUV mask blank. 1. A substrate and a multilayer reflective film provided on the substrate, the multilayer reflective film having a Si / Mo laminated portion in which Si layers and Mo layers are alternately laminated, and a layer containing Si and N is formed in contact with both the Si layer and the Mo layer at least one of the Si layers and the Mo layer of the Si / Mo laminated portion. And, the multilayer reflective film further includes a protective layer containing Ru in contact with the Si / Mo stacked portion as an uppermost layer of the multilayer reflective film, a layer of the Si / Mo laminated portion in contact with the protective layer is a Mo layer; an uppermost portion of the multilayer reflective film is composed of, from the side remote from the substrate, the protective layer, the Mo layer, the layer containing Si and N, and the Si layer; At the top, the Mo layer has a thickness of 1 nm or less. Yes A multilayer reflective film-coated substrate for an EUV mask blank, comprising: 2. The multilayer reflective film-coated substrate for an EUV mask blank according to 1, wherein the layer containing Si and N has a thickness of 2 nm or less. 3 At the top, the thickness of the protective layer is 4 nm or less. ,above The layer containing Si and N has a thickness of 2 nm or less, and the Si layer has a thickness of 4 nm or less. 1 or 2 2. A multilayer reflective film-coated substrate for an EUV mask blank according to claim 1. 4 The Si / Mo laminated portion includes 30 or more three-layer laminated structure units each including, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, and a Mo layer formed in contact with the layer containing Si and N, or a Mo layer, from the substrate side, a layer containing Si and N formed in contact with the Mo layer, and a Si layer formed in contact with the layer containing Si and N. 3 2. A multilayer reflective film-coated substrate for an EUV mask blank according to claim 1 . 5 The Si / Mo laminated portion includes 30 or more four-layer laminated structure units each including, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, a Mo layer formed in contact with the layer containing Si and N, and a layer containing Si and N formed in contact with the Mo layer. 3 2. A multilayer reflective film-coated substrate for an EUV mask blank according to claim 1 . 6 The multilayer reflective film has a peak reflectance of 65% or more at an incident angle of 6° for EUV light having a wavelength of 13.4 to 13.6 nm. 5 2. A multilayer reflective film-coated substrate for an EUV mask blank according to claim 1 . 7 .1 to 6 A method for producing a multilayer reflective film-coated substrate for an EUV mask blank according to any one of the above claims, (A) A step of forming the Si / Mo laminated portion by sputtering The sputtering step comprises: One or more Mo targets and one or more Si targets can be mounted. Power can be applied separately to the Mo target and the Si target; The substrate and each target are disposed in an offset arrangement, There is no shielding member between each target and the substrate, The substrate can be rotated along its major surface; and Nitrogen-containing gas can be introduced A method for producing a multilayer reflective film-coated substrate for an EUV mask blank, characterized in that the method is carried out in a magnetron sputtering apparatus equipped with a chamber. 8 . 1 7. A method for producing a multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 6, comprising the steps of: (A) forming the Si / Mo laminate by sputtering; and (B) forming the protective layer by sputtering Including, A method for producing a multilayer reflective film-coated substrate for an EUV mask blank, characterized in that after the step (A), the step (B) is carried out without bringing the Si / Mo laminate portion formed in the step (A) into contact with a gas that reacts with the Si / Mo laminate portion. 9 The above-mentioned (A) step is carried out in one sputtering chamber, the substrate on which the above-mentioned Si / Mo laminated portion is formed is moved from the one sputtering chamber to another sputtering chamber, and the above-mentioned (B) step is carried out in the other sputtering chamber. 8 The manufacturing method described in 10 A transfer chamber is provided between the first and second sputtering chambers, which can communicate with each sputtering chamber individually or simultaneously with both sputtering chambers, and the substrate on which the Si / Mo laminated portion is formed is transferred from the first sputtering chamber to the second sputtering chamber via the transfer chamber. 9 The manufacturing method described in 11The transfer from the one sputtering chamber to the transfer chamber and the transfer from the transfer chamber to the other sputtering chamber are both performed under vacuum. 10 The manufacturing method described in 12 The Si / Mo laminated portion includes 30 or more three-layer laminated structure units each consisting of, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, and a Mo layer formed in contact with the layer containing Si and N, or 30 or more three-layer laminated structure units each consisting of, from the substrate side, a Mo layer, a layer containing Si and N formed in contact with the Mo layer, and a Si layer formed in contact with the layer containing Si and N. 8 ~ 11 13. The method for producing a semiconductor device according to any one of the preceding claims. 13 The Si / Mo laminated portion includes 30 or more four-layer laminated structure units each including, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, a Mo layer formed in contact with the layer containing Si and N, and a layer containing Si and N formed in contact with the Mo layer. 8 ~ 11 13. The method for producing a semiconductor device according to any one of the preceding claims. 14 The multilayer reflective film has a peak reflectance of 65% or more at an incident angle of 6° for EUV light having a wavelength in the range of 13.4 to 13.6 nm. 8 ~ 13 13. The method for producing a semiconductor device according to any one of the preceding claims. 15 .1 to 6 13. An EUV mask blank comprising an absorber film containing Ta or Cr on the multilayer reflective film of the multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 12. 16 .1 to 6 1. An EUV mask blank comprising: an absorber film containing Ta but not containing Cr on the multilayer reflective film of the multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 9; and a hard mask film containing Cr on the absorber film, the hard mask film functioning as an etching mask when dry etching the absorber film. Effect of the Invention

[0010] According to the present invention, it is possible to provide a multilayer reflective film-coated substrate for an EUV mask blank, which has a multilayer reflective film that has high reflectance and is resistant to deterioration in reflectance even when heat is applied, and an EUV mask blank. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a partial cross-sectional view, omitted from the middle, showing an example of a multilayer reflective film-coated substrate for an EUV mask blank of the present invention. [Diagram 2] FIG. 1 is a partial cross-sectional view, omitted from the middle, illustrating a multilayer reflective film-coated substrate for an EUV mask blank, having a multilayer reflective film composed of an ideal Si / Mo stacked portion and a protective layer. [Diagram 3] FIG. 1 is a partial cross-sectional view, omitted from the middle, showing a multilayer reflective film-coated substrate for an EUV mask blank, having a conventional multilayer reflective film consisting of a Si / Mo stacked portion and a protective layer. [Figure 4] FIG. 1 is a conceptual diagram showing an example of a sputtering apparatus suitable for forming a multilayer reflective film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will now be described in further detail. The substrate with a multilayer reflective film for an EUV mask blank of the present invention has a substrate and a multilayer reflective film formed on the substrate (on one main surface (front surface)) that reflects exposure light, specifically, a multilayer reflective film that reflects EUV light. The multilayer reflective film may be provided in contact with one main surface of the substrate, and an undercoat film may be provided between the substrate and the multilayer reflective film. The wavelength of EUV light used in EUV lithography using EUV light as exposure light is 13 to 14 nm, and is usually light having a wavelength of about 13.5 nm (for example, 13.4 to 13.6 nm).

[0013] 1 is a partial cross-sectional view, omitted from the middle, showing an example of a multilayer reflective film-coated substrate for an EUV mask blank of the present invention. This multilayer reflective film-coated substrate for an EUV mask blank 10 has a multilayer reflective film 2 formed on one main surface of a substrate 1 in contact with the one main surface.

[0014] The substrate preferably has low thermal expansion characteristics for EUV light exposure, and has a thermal expansion coefficient of, for example, ±2×10 -8 / ℃, preferably within ±5×10 -9 / °C. It is preferable to use a substrate having a sufficiently flat surface, and the surface roughness of the main surface of the substrate is preferably 0.5 nm or less, particularly 0.2 nm or less, in terms of RMS value. Such a surface roughness can be obtained by polishing the substrate, for example.

[0015] The multilayer reflective film is a film that reflects EUV light, which is exposure light, in an EUV mask. In the present invention, the multilayer reflective film has a Si / Mo laminated portion composed of a multilayer in which Si (silicon) layers and Mo (molybdenum) layers are alternately laminated. In this Si / Mo laminated portion, a layer of Si, which is a material having a relatively high refractive index to EUV light, and a layer of Mo, which is a material having a relatively low refractive index to EUV light, are periodically laminated. Here, the Si layer and the Mo layer are layers formed of simple silicon and simple molybdenum, respectively. The number of laminated Si layers and Mo layers is preferably, for example, 40 periods or more (40 layers or more for each) and 60 periods or less (60 layers or less for each). The thicknesses of the Si layers and Mo layers in the Si / Mo laminated portion are appropriately set according to the exposure wavelength, and the thickness of the Si layer is preferably 5 nm or less, and the thickness of the Mo layer is preferably 4 nm or less. The lower limit of the thickness of the Si layer is not particularly limited, but is usually 1 nm or more, and the lower limit of the thickness of the Mo layer is not particularly limited, but is usually 1 nm or more. The thicknesses of the Si layer and the Mo layer may be set so as to obtain a high reflectance to EUV light. The thicknesses of the Si layer and the Mo layer may be constant or may differ from one layer to another. The total thickness of the Si / Mo laminate is usually about 250 to 450 nm.

[0016] In the present invention, the Si / Mo laminated portion is formed such that a layer containing Si and N is in contact with both the Si layer and the Mo layer at least one between the Si layer and the Mo layer. The layer containing Si and N is preferably free of oxygen. Specifically, the layer containing Si and N is preferably a SiN (here, SiN means that the constituent elements are only Si and N) layer. The N content of the layer containing Si and N is preferably 1 atomic % or more, particularly 5 atomic % or more, and is preferably 60 atomic % or less, particularly 57 atomic % or less. The thickness of the layer containing Si and N is preferably 2 nm or less, more preferably 1 nm or less. The lower limit of the thickness of the layer containing Si and N is not particularly limited, but is preferably 0.1 nm or more.

[0017] The layer containing Si and N is provided at least in one location between the Si layer and the Mo layer constituting the Si / Mo laminated portion. The layer containing Si and N may be provided on a part or all of the substrate side (lower side) of the Mo layer, or on a part or all of the side (upper side) of the Mo layer away from the substrate, but it is particularly preferable to provide the layer all over the space between the Si layer and the Mo layer constituting the Si / Mo laminated portion.

[0018] In particular, from the viewpoint of obtaining a high reflectance, it is preferable that the Si / Mo laminated portion contains 30 or more, particularly 40 or more three-layered laminated structural units consisting of a Si layer, a layer containing Si and N formed in contact with the Si layer, and a Mo layer formed in contact with the layer containing Si and N from the substrate side, or a Mo layer, a layer containing Si and N formed in contact with the Mo layer, and a Si layer formed in contact with the layer containing Si and N from the substrate side. It is also more preferable that the Si / Mo laminated portion contains 30 or more, particularly 40 or more four-layered laminated structural units consisting of a Si layer, a layer containing Si and N formed in contact with the Si layer, a Mo layer formed in contact with the layer containing Si and N, and a layer containing Si and N formed in contact with the Mo layer from the substrate side. The upper limit of both the three-layered laminated structural units and the four-layered laminated structural units is preferably 60 or less.

[0019] In the present invention, specific examples of the Si / Mo laminated portion include those shown in Fig. 1. In the multilayer reflective film 2 of the multilayer reflective film-coated substrate 10 for EUV mask blank shown in Fig. 1, a Si / Mo laminated portion 21 is formed in contact with the substrate 1. In the Si / Mo laminated portion 21, Si layers 211 and Mo layers 212 are alternately laminated, and in this case, the Si layer 211 is on the side closest to the substrate 1, and the Mo layer 212 is on the side furthest from the substrate 1. A layer 213 containing Si and N is formed between the Si layer 211 and the Mo layer 212 and in contact with both the Si layer 211 and the Mo layer 212. Therefore, in this case, from the substrate side, a three-layer stacked structure unit of Si layer 211, layer 213 containing Si and N, and Mo layer 212 is included, and from the substrate side, a three-layer stacked structure unit of Mo layer 212, layer 213 containing Si and N, and Si layer 211 is included, and further, from the substrate side, a four-layer stacked structure unit of Si layer 211, layer 213 containing Si and N, Mo layer 212, and layer 213 containing Si and N is included.

[0020] The Si / Mo laminated portion of the multilayer reflective film is formed by alternately laminating Si layers and Mo layers. FIG. 2 is a partial cross-sectional view, omitted from the middle, for explaining an EUV mask blank multilayer reflective film-coated substrate having a multilayer reflective film consisting of an ideal Si / Mo laminated portion and a protective layer. FIG. 3 is a partial cross-sectional view, omitted from the middle, showing an EUV mask blank multilayer reflective film-coated substrate having a conventional multilayer reflective film consisting of a Si / Mo laminated portion and a protective layer. When the Si / Mo laminated portion 21 of the multilayer reflective film 2 of the EUV mask blank multilayer reflective film-coated substrate 10 is formed by directly laminating Si layers and Mo layers alternately on the substrate 1, it is ideal that the Si / Mo laminated portion 21 is formed only by the Si layer 211 and the Mo layer 212 in which the Si layer and the Mo layer are in contact with each other, as shown in FIG. 2. With such a Si / Mo laminated portion 21, the theoretical reflectance due to the Si / Mo laminated portion consisting only of the Si layer and the Mo layer can be obtained.

[0021] However, although it is not impossible in principle to form a Si / Mo laminated portion having such a configuration, when it is formed by a practical method, in reality, as shown in FIG. 3, Si and Mo are mixed at the contact portion between the Si layer 211 and the Mo layer 212, and an interdiffusion layer 21a made of Si and Mo is unintentionally formed at this portion. When such an interdiffusion layer made of Si and Mo is formed, the reflectance is reduced from the theoretical value obtained by the Si / Mo laminated portion made of only the Si layer and the Mo layer. Furthermore, when heat is applied to the multilayer reflective film during the mask processing process or exposure to EUV light using a mask, the interdiffusion layer made of Si and Mo becomes thicker or changes, resulting in a further reduction in reflectance.

[0022] On the other hand, when a layer containing Si and N is formed between the Si layer and the Mo layer in contact with both the Si layer and the Mo layer, the formation of an interdiffusion layer consisting of Si and Mo between the Si layer and the Mo layer, which causes a decrease in reflectance, is suppressed, so that the decrease in reflectance from the theoretical value obtained in the Si / Mo laminated portion consisting of only the Si layer and the Mo layer is suppressed, and a higher reflectance is achieved than in the past. Note that, between the Si layer and the Mo layer where the layer containing Si and N is not formed, the above-mentioned interdiffusion layer consisting of Si and Mo is usually formed in contact with both the Si layer and the Mo layer, but in the Si / Mo laminated portion of the multilayer reflective film of the present invention, the formation of an interdiffusion layer consisting of Si and Mo is suppressed between the Si layer and the Mo layer where the layer containing Si and N is formed, so that the decrease in reflectance due to heat is suppressed compared to the conventional multilayer reflective film in which the interdiffusion layer consisting of Si and Mo is formed all between the Si layer and the Mo layer. From this viewpoint, the layer containing Si and N may be formed only partially between the Si layer and the Mo layer, but it is more advantageous to form the layer in most of the space between the Si layer and the Mo layer, and it is particularly advantageous to form the layer in the entire space between the Si layer and the Mo layer.

[0023] In the present invention, the multilayer reflective film preferably has a protective layer in contact with the Si / Mo laminated portion as the top layer of the multilayer reflective film. If the top layer of the multilayer reflective film is a Si layer or a Mo layer, it will be etched by dry etching using a gas containing fluorine, so it is effective to provide a protective layer on the Si / Mo laminated portion. The protective layer is also called a capping layer, and functions as an etching stopper when an absorber pattern is formed from an absorber film formed thereon. For this reason, a material having etching characteristics different from those of the absorber film is used for the protective layer. In addition, it is preferable that the protective layer is also effective for protecting the multilayer reflective film when the absorber pattern is corrected.

[0024] In the present invention, a specific example of the protective layer is as shown in Fig. 1. In the multilayer reflective film 2 of the multilayer reflective film-coated substrate 10 for EUV mask blank shown in Fig. 1, a protective layer 22 is formed in contact with a Si / Mo laminated portion 21.

[0025] The protective layer is made of a material containing ruthenium (Ru). The material containing Ru is preferably Ru alone or a compound in which niobium (Nb) or zirconium (Zr) is added to Ru. The thickness of the protective layer is usually 5 nm or less, and preferably 4 nm or less. The lower limit of the thickness of the protective layer is usually 2 nm or more.

[0026] In the Si / Mo laminated portion, the layer closest to the substrate of the multilayer reflective film may be either a Si layer or a Mo layer. On the other hand, the layer farthest from the substrate may be either a Si layer or a Mo layer, but is preferably a Mo layer, and it is preferable that the layer in contact with the protective layer of the Si / Mo laminated portion is a Mo layer.

[0027] When the layer in contact with the protective layer of the Si / Mo laminate is a Si layer, if a protective layer of a material containing Ru is directly laminated on the Si / Mo laminate, it is ideal that the Si layer 211 of the Si / Mo laminate 21 and the protective layer 22 are in contact with each other as shown in Fig. 2. In this state, the decrease in reflectance of the multilayer reflective film 2 caused by the protective layer 22 is limited, and a high reflectance can be obtained.

[0028] However, although it is not impossible in principle to achieve such a state, when it is formed by a practical method, in reality, as shown in FIG. 3, Si and Ru are mixed at the portion where the Si layer 211 and the protective layer 22 contact each other, and an interdiffusion layer 21b made of Si and Ru is unintentionally formed at this portion. When such an interdiffusion layer made of Si and Ru is formed, the interdiffusion layer 21b made of Si and Ru reduces the reflectance. Furthermore, when heat is applied to the multilayer reflective film during a mask processing process or exposure to EUV light using a mask, the interdiffusion layer made of Si and Ru becomes thicker or changes, and further, when the protective layer made of a material containing Ru is exposed to the atmosphere, not only the protective layer but also the Si layer is oxidized, resulting in a further reduction in reflectance.

[0029] In contrast, as shown in FIG. 1, when the layer in contact with protective layer 22 of Si / Mo laminate 21 is Mo layer 212, no interdiffusion layer of Si and Ru that would cause a decrease in reflectance is formed between the Si / Mo laminate and the protective layer of a material containing Ru, and therefore a higher reflectance is achieved than when the layer in contact with the protective layer of the Si / Mo laminate is a Si layer.

[0030] When the layer in contact with the protective layer of the Si / Mo laminated portion is a Mo layer, it is preferable that a layer containing Si and N is formed between the Si layer closest to this Mo layer and the Mo layer in contact with the protective layer, in contact with both the Si layer and the Mo layer. Specifically, it is preferable that the top of the multilayer reflective film is composed of a protective layer, a Mo layer, a layer containing Si and N, and a Si layer, from the side away from the substrate. The area between the Si layer closest to the Mo layer in contact with the protective layer of the Si / Mo laminated portion and the Mo layer in contact with the protective layer is easily affected by the protective layer, and when heat is applied to the multilayer reflective film, it is most easily affected by heat, so that an interdiffusion layer made of Si and Mo is most likely to be formed. Therefore, it is particularly effective to form a layer containing Si and N between the Si layer and the Mo layer at the top of the multilayer reflective film in order to obtain a high reflectance.

[0031] In this case, when a layer containing Si and N is formed, even if a Mo layer in contact with a protective layer formed of a material containing Ru is formed thin, if a protective layer formed of a material containing Ru is formed on the Mo layer, the protective layer formed of a material containing Ru will be in a stable state having a crystalline dense structure, even if the protective layer formed of a material containing Ru is a relatively thin film. Therefore, the thickness of the Mo layer in contact with the protective layer formed of a material containing Ru is preferably 2 nm or less, more preferably 1 nm or less. In particular, when the top of the multilayer reflective film is composed of a protective layer, a Mo layer, a layer containing Si and N, and a Si layer from the side away from the substrate, it is preferable that the thickness of the protective layer is 4 nm or less, the thickness of the Mo layer is 1 nm or less, the thickness of the layer containing Si and N is 2 nm or less, and the thickness of the Si layer is 4 nm or less.

[0032] In the present invention, the reflectance of the multilayer reflective film can be made 65% or more as the peak reflectance at an incident angle of 6° for EUV light having a wavelength in the range of 13.4 to 13.6 nm. Even when the multilayer reflective film is subjected to a heat treatment, for example, a heat treatment at 200°C for 10 minutes in an air atmosphere, the change (decrease) in reflectance is small, and the peak reflectance can be maintained at 65% or more even after the heat treatment.

[0033] The method of forming the Si / Mo laminated part includes the sputtering method, in which power is supplied to a target, the atmospheric gas is turned into plasma (ionized) by the supplied power, and the ion beam sputtering method, in which an ion beam is irradiated onto the target. The sputtering method includes the DC sputtering method, in which a direct current voltage is applied to the target, and the RF sputtering method, in which a high frequency voltage is applied to the target. The sputtering method is a film formation method in which a voltage is applied to the target with the sputtering gas introduced into the chamber, the gas is ionized, and the sputtering phenomenon caused by the gas ions is utilized. In particular, the magnetron sputtering method is advantageous in terms of productivity. The power applied to the target may be DC or RF, and DC also includes pulse sputtering, in which the negative bias applied to the target is reversed for a short period of time to prevent the target from charging up.

[0034] The Si / Mo laminated portion can be formed by a sputtering method using, for example, a sputtering device capable of mounting multiple targets. Specifically, a silicon (Si) target for forming a Si layer and a layer containing Si and N, and a molybdenum (Mo) target for forming a Mo layer are used. When forming a Si layer and a Mo layer, a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas is used as a sputtering gas. When forming a layer containing Si and N, a rare gas and a nitrogen-containing gas such as nitrogen gas (N2 gas) are used. The substrate and each target are arranged in an offset arrangement (a vertical line passing through the center of the sputtering surface of each target does not coincide with a vertical line passing through the center of the film formation surface of the substrate), and the Si target and the Mo target are sputtered in sequence to sequentially form a Si layer, a layer containing Si and N, and a Mo layer. Sputtering is preferably performed while rotating the substrate along the main surface. In this case, it is preferable that no member such as a shutter is provided in the chamber to shield the target from the substrate. The layer containing Si and N may be formed by reactive sputtering using a nitrogen-containing gas, or may be formed by using a silicon compound target such as a silicon nitride target.

[0035] The Si / Mo laminated section is (A) A process for forming a Si / Mo laminate by sputtering In this case, it is particularly preferable to carry out this sputtering using a magnetron sputtering apparatus that can mount one or more Mo targets and one or more Si targets, can apply power separately to the Mo targets and the Si targets, has an offset arrangement between the substrate and each target, does not have a shielding member between each target and the substrate, can rotate the substrate along its main surface, and is equipped with a chamber into which a nitrogen-containing gas can be introduced.

[0036] The protective layer can be formed by a sputtering method such as ion beam sputtering or magnetron sputtering, as in the case of the Si / Mo laminated portion, but magnetron sputtering is advantageous as in the case of the Si / Mo laminated portion.

[0037] The protective layer can be formed by a sputtering method using, for example, a sputtering device capable of mounting one or more targets. Specifically, a ruthenium (Ru) target and, if necessary, one or more element targets selected from niobium (Nb) and zirconium (Zr) are used, and rare gases such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, and xenon (Xe) gas are used as sputtering gas. The target and the main surface of the substrate are opposed to each other (for example, in an arrangement in which a vertical line passing through the center of the sputtering surface of the target coincides with a vertical line passing through the center of the film formation surface of the substrate), and a single target is used for sputtering, or the substrate and each target are placed in an offset arrangement, and multiple targets are simultaneously sputtered. Sputtering is preferably performed while rotating the substrate along the main surface.

[0038] When the protective layer is formed of a compound containing an element other than a metal, it can be formed by reactive sputtering using a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas together with a rare gas as a sputtering gas. The target may also be a compound.

[0039] In this way, the multilayer reflective film has the following properties: (A) forming a Si / Mo laminate by sputtering; (B) forming a protective layer by sputtering; In this case, for example, the step (A) can be performed in one sputtering chamber, and the substrate on which the Si / Mo laminated portion is formed can be moved from the one sputtering chamber to another sputtering chamber, and the step (B) can be performed in the other sputtering chamber. However, if the Si / Mo laminated portion is exposed to an atmosphere containing oxygen, such as the air, when moving from the step (A) to the step (B), an unnecessary oxide layer is formed between the Si / Mo laminated portion and the protective layer, which may cause a decrease in reflectance and peeling between layers. Therefore, when moving to the step (B) after the step (A), it is preferable to move to the step (B) and perform the step (B) without contacting the Si / Mo laminated portion formed in the step (A) with a gas that reacts with the Si / Mo laminated portion, particularly a gas containing oxygen, such as oxygen gas (O2 gas) (more specifically, without exposing it to the air).

[0040] As a method for carrying out step (B) without contacting the Si / Mo laminated portion formed in step (A) with a gas that reacts with the Si / Mo laminated portion, specifically, step (A) is carried out in one sputtering chamber, the substrate on which the Si / Mo laminated portion is formed is moved from the one sputtering chamber to another sputtering chamber, and step (B) is carried out in the other sputtering chamber, a transfer chamber that can communicate with each sputtering chamber individually or simultaneously with both sputtering chambers is provided between the one and other sputtering chambers, and the substrate on which the Si / Mo laminated portion is formed is moved from the one sputtering chamber to the other sputtering chamber via the transfer chamber. In this case, it is preferable that the transfer from the one sputtering chamber to the transfer chamber and the transfer from the transfer chamber to the other sputtering chamber are both carried out under an inert gas atmosphere or vacuum at normal pressure (atmospheric pressure) or reduced pressure (pressure lower than normal pressure).

[0041] 4 is a conceptual diagram showing an example of a sputtering apparatus suitable for forming the multilayer reflective film of the present invention. This sputtering apparatus 100 is composed of a sputtering chamber 101 for forming a Si / Mo laminated portion by sputtering, a sputtering chamber 102 for forming a protective layer by sputtering, a transfer chamber 103 connected to both the sputtering chambers 101 and 102, and a load lock chamber 104 connected to the transfer chamber 103. An openable and closable partition wall (not shown) is provided between the transfer chamber 103 and the load lock chamber 104, and a partition wall (not shown) is provided between the sputtering chambers 101 and 102. Transport chamber 103 Between the two, a partition that can be opened or closed as required can be provided.

[0042] When a multilayer reflective film is formed by such a sputtering apparatus, for example, first, a substrate is introduced into a load lock chamber 104, and after the pressure inside the load lock chamber 104 is reduced, the partition is opened, and the substrate is moved to the sputtering chamber 101 via the transfer chamber 103, and a Si / Mo laminated portion is formed in the sputtering chamber 101. Next, the substrate on which the Si / Mo laminated portion has been formed is moved from the sputtering chamber 101 via the transfer chamber 103 to the sputtering chamber 102, and a protective layer is formed in the sputtering chamber 102. Next, the substrate on which the Si / Mo laminated portion and the protective layer (multilayer reflective film) have been formed is moved from the sputtering chamber 102 via the transfer chamber 103 to the load lock chamber 104, the partition is closed, the pressure inside the load lock chamber 104 is returned to normal pressure, and the substrate on which the multilayer reflective film has been formed is taken out, whereby a substrate with a multilayer reflective film for an EUV mask blank can be obtained. By forming the multilayer reflective film in this manner, step (B) can be carried out without bringing the Si / Mo laminated portion formed in step (A) into contact with a gas that reacts with the Si / Mo laminated portion.

[0043] The multilayer reflective film-coated substrate for an EUV mask blank becomes an EUV mask blank by forming an absorber film on the multilayer reflective film.

[0044] The EUV mask blank of the present invention has an absorber film that absorbs exposure light formed on the multilayer reflective film of the multilayer reflective film-coated substrate for EUV mask blank, specifically, an absorber film that absorbs EUV light and reduces reflectance. The absorber film is preferably provided in contact with the protective layer. The EUV mask blank may further have a hard mask film on the absorber film that functions as an etching mask when dry etching the absorber film. On the other hand, a conductive film used for electrostatically chucking the EUV mask to an exposure device may be provided under the other main surface (back surface) that is the surface opposite to the one main surface of the substrate, preferably in contact with the other main surface. In the present invention, the one main surface of the substrate is the front surface and the upper side, and the other main surface is the back surface and the lower side, but the front and back and the top and bottom of both are defined for convenience, and the one main surface and the other main surface are either of the two main surfaces (film formation surfaces) of the substrate, and the front and back and the top and bottom are interchangeable.

[0045] From an EUV mask blank (mask blank for EUV exposure), an EUV mask (mask for EUV exposure) having an absorber pattern (pattern of the absorber film) formed by patterning an absorber film is manufactured. The EUV mask blank and the EUV mask are reflective mask blanks and reflective masks.

[0046] The absorber film is formed on top of the multilayer reflective film and absorbs the EUV light, which is the exposure light, to reduce the reflectance of the exposure light. In the EUV mask, a transfer pattern is formed due to the difference in reflectance between the area where the absorber film is formed and the area where the absorber film is not formed.

[0047] The material of the absorber film is not limited as long as it absorbs EUV light and can be patterned. Examples of the material of the absorber film include materials containing tantalum (Ta) or chromium (Cr). In addition, materials containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), etc. Examples of materials containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0048] The absorber film can be formed by sputtering, and the sputtering is preferably magnetron sputtering. Specifically, it can be formed by sputtering using a metal target such as a chromium (Cr) target or a tantalum (Ta) target, or a metal compound target such as a chromium compound target or a tantalum compound target (a target containing a metal such as Cr or Ta and oxygen (O), nitrogen (N), carbon (C), boron (B), etc.), and using a rare gas such as helium (He) gas, argon (Ar) gas, krypton (Kr) gas, or xenon (Xe) gas as a sputtering gas, or by reactive sputtering using a reactive gas such as an oxygen-containing gas, a nitrogen-containing gas, or a carbon-containing gas together with a rare gas.

[0049] A hard mask film (an etching mask film for the absorber film) having etching characteristics different from those of the absorber film may be provided on the side of the absorber film that is away from the substrate, preferably in contact with the absorber film. This hard mask film functions as an etching mask when the absorber film is dry etched. After the absorber pattern is formed, the hard mask film may be left as a reflectance reduction layer for reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection, as a part of the absorber film, or may be removed so as not to remain on the EUV mask. Materials for the hard mask film include materials containing chromium (Cr). A hard mask film formed of a material containing Cr is particularly suitable when the absorber film is formed of a material containing Ta and not containing Cr. When a layer (reflectance reduction layer) that mainly serves the function of reducing the reflectance at the wavelength of light used in an inspection such as a pattern inspection is formed on the absorber film, the hard mask film can be formed on the reflectance reduction layer of the absorber film. The hard mask film can be formed by, for example, a magnetron sputtering method. The thickness of the hard mask film is not particularly limited, but is usually about 5 to 20 nm.

[0050] The conductive film preferably has a sheet resistance of 100Ω / □ or less, and there is no particular restriction on the material. Examples of the material of the conductive film include materials containing tantalum (Ta) or chromium (Cr). Furthermore, materials containing Ta or Cr may contain oxygen (O), nitrogen (N), carbon (C), boron (B), and the like. Examples of materials containing Ta include Ta alone and tantalum compounds such as TaO, TaN, TaON, TaC, TaCN, TaCO, TaCON, TaB, TaOB, TaNB, TaONB, TaCB, TaCNB, TaCOB, and TaCONB. Examples of materials containing Cr include Cr alone and chromium compounds such as CrO, CrN, CrON, CrC, CrCN, CrCO, CrCON, CrB, CrOB, CrNB, CrONB, CrCB, CrCNB, CrCOB, and CrCONB.

[0051] The thickness of the conductive film is not particularly limited as long as it functions as an electrostatic chuck, but is usually about 5 to 100 nm. The thickness of the conductive film is preferably formed so that the film stress is balanced with the multilayer reflective film and the absorber pattern after forming the EUV mask, that is, after forming the absorber pattern. The conductive film may be formed before forming the multilayer reflective film, or after forming all the films on the multilayer reflective film side of the substrate, or after forming a part of the film on the multilayer reflective film side of the substrate, the conductive film may be formed, and then the remaining film on the multilayer reflective film side of the substrate may be formed. The conductive film can be formed, for example, by magnetron sputtering.

[0052] Furthermore, the EUV mask blank may have a resist film formed on the side farthest from the substrate. The resist film is preferably an electron beam (EB) resist. EXAMPLES

[0053] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0054] [Example 1] Thermal expansion coefficient is ±5.0×10 -9 A multilayer reflective film consisting of a Si / Mo laminate and a protective layer containing Ru was formed on a substrate made of a low thermal expansion material in the range of 0.1 nm to 1.5 nm / °C, with the main surface having a surface roughness of 0.1 nm or less in RMS value and a main surface flatness of 100 nm in TIR value.

[0055] The Si / Mo laminated portion was formed by magnetron sputtering using a Si target and a Mo target as targets and Ar gas and N2 gas as sputtering gas. One Si target and one Mo target were attached to the magnetron sputtering device, and the substrate and each target were offset from each other, and the substrate was rotated to form the laminate. First, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 3.0 nm. Next, Ar gas and N2 gas were flowed into the sputtering chamber, and only the Si target was discharged, forming a SiN layer with a thickness of 1.0 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged, forming a Mo layer with a thickness of 3.0 nm. The formation of the Si layer, SiN layer, and Mo layer constitutes one cycle, and the formation of these three layers was repeated for a total of 40 cycles. After that, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 2.8 nm. Next, Ar gas and N2 gas were flowed into the sputtering chamber, and only the Si target was discharged, forming a SiN layer with a thickness of 1.0 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged, forming a Mo layer with a thickness of 0.5 nm, forming a Si / Mo laminated section.

[0056] The protective layer was formed by magnetron sputtering using a Ru target as the target and Ar gas as the sputtering gas. One Ru target was attached to a magnetron sputtering device other than the magnetron sputtering device that formed the Si / Mo laminated portion, and the substrate and the target were arranged facing each other, and the protective layer was formed while rotating the substrate. The substrate on which the Si / Mo laminated portion was formed was moved under vacuum from the magnetron sputtering device that formed the Si / Mo laminated portion to the magnetron sputtering device that formed the protective layer, via a transfer chamber that communicated with both sputtering chambers. Ar gas was introduced into the sputtering chamber. S The Ru target was discharged and a Ru layer was formed with a thickness of 2.5 nm as a protective layer.

[0057] When the cross section of the obtained multilayer reflective film was observed with a transmission electron microscope (TEM), a Ru layer with a thickness of 2.5 nm, a Mo layer with a thickness of 0.5 nm, a SiN layer with a thickness of 1.0 nm, a Si layer with a thickness of 2.6 nm, an interdiffusion layer of Si and Mo with a thickness of 0.5 nm, a Mo layer with a thickness of 2.3 nm, and a SiN layer with a thickness of 0.9 nm were observed on the upper part of the multilayer reflective film, in that order from the surface side (the side away from the substrate). In addition, a multilayer reflective film obtained by the same method was subjected to a heat treatment at 200°C for 10 minutes in an air atmosphere, and the cross section of the multilayer reflective film was observed in the same manner, and was the same as before the heat treatment. In addition, the peak reflectance at an incident angle of 6° for EUV light in the wavelength range of 13.4 to 13.6 nm was measured before and after the heat treatment, and it was 67% before the heat treatment and 65% after the heat treatment, and both were high reflectances of 65% or more.

[0058] [Example 2] Thermal expansion coefficient is ±5.0×10 -9 A multilayer reflective film consisting of a Si / Mo laminate and a protective layer containing Ru was formed on a substrate made of a low thermal expansion material in the range of 0.1 nm to 1.5 nm / °C, with the main surface having a surface roughness of 0.1 nm or less in RMS value and a main surface flatness of 100 nm in TIR value.

[0059] The Si / Mo laminated portion was formed by magnetron sputtering using a Si target and a Mo target as targets and Ar gas and N2 gas as sputtering gas. One Si target and one Mo target were attached to the magnetron sputtering device, and the substrate and each target were offset from each other, and the substrate was rotated to form the laminate. First, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 3.0 nm. Next, Ar gas and N2 gas were flowed into the sputtering chamber, and only the Si target was discharged, forming a SiN layer with a thickness of 0.5 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged, forming a Mo layer with a thickness of 3.0 nm. Next, Ar gas and N2 gas were flowed into the sputtering chamber, and only the Si target was discharged, forming a SiN layer with a thickness of 0.5 nm. The formation of the Si layer, SiN layer, Mo layer, and SiN layer constitutes one cycle, and the formation of these four layers was repeated a total of 40 cycles. After that, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 2.4 nm. Next, Ar gas and N2 gas were flowed into the sputtering chamber, and only the Si target was discharged, forming a SiN layer with a thickness of 0.5 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged, forming a Mo layer with a thickness of 0.5 nm, forming a Si / Mo laminated section.

[0060] The protective layer was formed by magnetron sputtering using a Ru target as the target and Ar gas as the sputtering gas. One Ru target was attached to a magnetron sputtering device other than the magnetron sputtering device that formed the Si / Mo laminated portion, and the substrate and the target were arranged facing each other, and the protective layer was formed while rotating the substrate. The substrate on which the Si / Mo laminated portion was formed was moved from the magnetron sputtering device that formed the Si / Mo laminated portion to the magnetron sputtering device that formed the protective layer through a transfer chamber that communicated with both sputtering chambers, and moved under vacuum. Ar gas was flowed into the sputtering chamber, and the Ru target was discharged, forming a Ru layer with a thickness of 2.5 nm, which was used as the protective layer.

[0061] When the cross section of the obtained multilayer reflective film was observed with a transmission electron microscope (TEM), a Ru layer with a thickness of 2.7 nm, a Mo layer with a thickness of 0.5 nm, a SiN layer with a thickness of 0.5 nm, a Si layer with a thickness of 2.5 nm, a SiN layer with a thickness of 0.5 nm, a Mo layer with a thickness of 2.5 nm, and a SiN layer with a thickness of 0.5 nm were observed on the upper part of the multilayer reflective film, in order from the surface side (the side away from the substrate). In addition, a multilayer reflective film obtained by the same method was subjected to a heat treatment at 200°C for 10 minutes in an air atmosphere, and the cross section of the multilayer reflective film was observed in the same manner, and was the same as before the heat treatment. In addition, the peak reflectance at an incident angle of 6° for EUV light in the wavelength range of 13.4 to 13.6 nm was measured before and after the heat treatment, and it was 67% before the heat treatment and 65% after the heat treatment, and both were high reflectances of 65% or more.

[0062] [Comparative Example 1] Thermal expansion coefficient is ±5.0×10 -9 A multilayer reflective film consisting of a Si / Mo laminate and a protective layer containing Ru was formed on a substrate made of a low thermal expansion material in the range of 0.1 nm to 1.5 nm / °C, with the main surface having a surface roughness of 0.1 nm or less in RMS value and a main surface flatness of 100 nm in TIR value.

[0063] The Si / Mo laminated portion was formed by magnetron sputtering using a Si target and a Mo target as targets and Ar gas and N2 gas as sputtering gas. One Si target and one Mo target were attached to the magnetron sputtering device, and the substrate and each target were offset from each other, and the substrate was rotated to form the laminate. First, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 4.0 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged, forming a Mo layer with a thickness of 3.0 nm. The formation of these Si and Mo layers was counted as one cycle, and the formation of these two layers was repeated for a total of 40 cycles. After that, only Ar gas was flowed into the sputtering chamber, and only the Si target was discharged, forming a Si layer with a thickness of 3.0 nm. Next, only Ar gas was flowed into the sputtering chamber, and only the Mo target was discharged to form a Mo layer with a thickness of 1.0 nm, forming a Si / Mo laminated portion.

[0064] The protective layer was formed by magnetron sputtering using a Ru target as the target and Ar gas as the sputtering gas. One Ru target was attached to a magnetron sputtering device other than the magnetron sputtering device that formed the Si / Mo laminated portion, and the substrate and the target were arranged facing each other, and the protective layer was formed while rotating the substrate. The substrate on which the Si / Mo laminated portion was formed was moved from the magnetron sputtering device that formed the Si / Mo laminated portion to the magnetron sputtering device that formed the protective layer through a transfer chamber that communicated with both sputtering chambers, and moved under vacuum. Ar gas was flowed into the sputtering chamber, and the Ru target was discharged, forming a Ru layer with a thickness of 2.5 nm, which was used as the protective layer.

[0065] When the cross section of the obtained multilayer reflective film was observed with a transmission electron microscope (TEM), the following were observed in the upper part of the multilayer reflective film, in order from the surface side (the side away from the substrate): a 2.5 nm thick Ru layer, a 1.2 nm thick interdiffusion layer of mixed Si and Mo, a 2.8 nm thick Si layer, a 0.5 nm thick interdiffusion layer of mixed Si and Mo, a 2.7 nm thick Mo layer, and a 1.3 nm thick interdiffusion layer of mixed Si and Mo. In addition, a multilayer reflective film obtained by the same method was subjected to a heat treatment at 200°C for 10 minutes in an air atmosphere, and the cross section of the multilayer reflective film was observed in the same manner. As a result, a Ru layer having a thickness of 2.5 nm, an interdiffusion layer of Si and Mo having a thickness of 1.6 nm, a Si layer having a thickness of 2.6 nm, an interdiffusion layer of Si and Mo having a thickness of 0.5 nm, a Mo layer having a thickness of 2.6 nm, and an interdiffusion layer of Si and Mo having a thickness of 1.6 nm were observed in the upper part of the multilayer reflective film, in that order from the surface side (the side away from the substrate). In addition, the peak reflectance at an incident angle of 6° for EUV light having a wavelength of 13.4 to 13.6 nm was measured before and after the heat treatment, and it was 65% before the heat treatment and 62% after the heat treatment, resulting in a low reflectance of less than 65% after the heat treatment. [Explanation of symbols]

[0066] 1 Board 10 Multilayer reflective film substrate for EUV mask blanks 2 Multilayer reflective film 21 Si / Mo laminate 211 Si layer 212 Mo layer Layer containing 213Si and N 21a Interdiffusion layer consisting of Si and Mo 21b Interdiffusion layer consisting of Si and Ru 22 Protective layer 100 Sputtering equipment 101, 102 Sputtering chamber 103 Transport chamber 104 Load Lock Chamber

Claims

1. a substrate; and a multilayer reflective film provided on the substrate, the multilayer reflective film having a Si / Mo laminated portion in which a Si layer and a Mo layer are alternately laminated, and a layer containing Si and N is formed in contact with both the Si layer and the Mo layer at least one of the Si layers and the Mo layer of the Si / Mo laminated portion; the multilayer reflective film further includes a protective layer containing Ru, as a top layer of the multilayer reflective film, in contact with the Si / Mo laminated portion, a layer of the Si / Mo laminated portion in contact with the protective layer is a Mo layer; an uppermost portion of the multilayer reflective film is composed of, from the side remote from the substrate, the protective layer, the Mo layer, the layer containing Si and N, and the Si layer; At the top, the Mo layer has a thickness of 1 nm or less. A multilayer reflective film-coated substrate for an EUV mask blank, comprising:

2. 2. The multilayer reflective film-coated substrate for an EUV mask blank according to claim 1, wherein the layer containing Si and N has a thickness of 2 nm or less.

3. 3. The multilayer reflective film-coated substrate for an EUV mask blank as described in claim 1 or 2, characterized in that, at the uppermost portion, the protective layer has a thickness of 4 nm or less, the layer containing Si and N has a thickness of 2 nm or less, and the Si layer has a thickness of 4 nm or less.

4. 4. The multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 3, characterized in that the Si / Mo laminate portion contains 30 or more three-layer laminate structure units each composed of, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, and a Mo layer formed in contact with the layer containing Si and N, or 30 or more three-layer laminate structure units each composed, from the substrate side, of a Mo layer, a layer containing Si and N formed in contact with the Mo layer, and a Si layer formed in contact with the layer containing Si and N.

5. 4. The substrate with a multilayer reflective film for an EUV mask blank according to any one of claims 1 to 3, characterized in that the Si / Mo laminate portion contains 30 or more four-layer laminate structure units each composed of, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, a Mo layer formed in contact with the layer containing Si and N, and a layer containing Si and N formed in contact with the Mo layer.

6. 6. The multilayer reflective film-coated substrate for an EUV mask blank according to claim 1, wherein the peak reflectance of the multilayer reflective film is 65% or more at an incident angle of 6° for EUV light having a wavelength in the range of 13.4 to 13.6 nm.

7. A method for producing a multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 6, comprising the steps of: (A) A step of forming the Si / Mo laminated portion by sputtering The sputtering step comprises: One or more Mo targets and one or more Si targets can be attached. Power can be applied to the Mo target and the Si target separately; The substrate and each target are disposed in an offset arrangement, There is no shielding member between each target and the substrate, The substrate can be rotated along its major surface; and Nitrogen-containing gas can be introduced A method for producing a multilayer reflective film-coated substrate for an EUV mask blank, the method being carried out in a magnetron sputtering apparatus equipped with a chamber.

8. A method for producing a multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 6, comprising the steps of: (A) forming the Si / Mo laminate by sputtering; and (B) forming the protective layer by sputtering Including, A method for producing a multilayer reflective film-coated substrate for an EUV mask blank, characterized in that after the step (A), the step (B) is carried out without bringing the Si / Mo laminate portion formed in the step (A) into contact with a gas that reacts with the Si / Mo laminate portion.

9. 9. The manufacturing method according to claim 8, characterized in that the step (A) is carried out in one sputtering chamber, the substrate on which the Si / Mo laminated portion is formed is moved from the one sputtering chamber to another sputtering chamber, and the step (B) is carried out in the other sputtering chamber.

10. The manufacturing method described in claim 9, characterized in that a transfer chamber is provided between the one and another sputtering chambers, the transfer chamber being capable of communicating with each sputtering chamber individually or with both sputtering chambers simultaneously, and the substrate on which the Si / Mo laminated portion is formed is moved from the one sputtering chamber to the other sputtering chamber via the transfer chamber.

11. 11. The method according to claim 10, wherein the transfer from the one sputtering chamber to the transfer chamber and the transfer from the transfer chamber to the other sputtering chamber are both performed under vacuum.

12. 12. The manufacturing method according to claim 8, wherein the Si / Mo laminate portion contains 30 or more three-layer laminate structure units each composed of, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, and a Mo layer formed in contact with the layer containing Si and N, or 30 or more three-layer laminate structure units each composed, from the substrate side, of a Mo layer, a layer containing Si and N formed in contact with the Mo layer, and a Si layer formed in contact with the layer containing Si and N.

13. 12. The manufacturing method according to claim 8, wherein the Si / Mo laminate portion includes 30 or more four-layer laminate structure units each composed of, from the substrate side, a Si layer, a layer containing Si and N formed in contact with the Si layer, a Mo layer formed in contact with the layer containing Si and N, and a layer containing Si and N formed in contact with the Mo layer.

14. 14. The method according to claim 8, wherein the peak reflectance of the multilayer reflective film is 65% or more at an incident angle of 6° for EUV light having a wavelength in the range of 13.4 to 13.6 nm.

15. 7. An EUV mask blank comprising an absorber film containing Ta or Cr on the multilayer reflective film of the multilayer reflective film-coated substrate for an EUV mask blank according to claim 1.

16. 7. An EUV mask blank comprising: an absorber film containing Ta and not containing Cr on the multilayer reflective film of the multilayer reflective film-coated substrate for an EUV mask blank according to any one of claims 1 to 6; and a hard mask film containing Cr on the absorber film, the hard mask film functioning as an etching mask when dry etching the absorber film.

Citation Information

Patent Citations

  • Method of depositing multilayer film, reflecting mirror, and exposure device

    JP2004331998A

  • Passivation overcoat double layer

    JP2005516182A

  • Substrate with multilayer reflection film, reflective mask blank, and method of manufacturing them

    JP2011192693A

  • Reflective mask with light blocking region, reflective mask blank, method of manufacturing reflective mask