Sealing resin sheet
The sealing resin sheet addresses the issue of excessive intrusion by using a formulation with controlled viscosity and additives, achieving precise sealing and reduced penetration during curing.
Patent Information
- Application Number
- JP2021532793
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-18
- Filing Date
- 2020-07-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Conventional sealing methods for semiconductor elements and electronic components using thermosetting resins fail to achieve sufficient dimensional accuracy during curing, leading to excessive intrusion of cured material between the elements and the substrate.
A sealing resin sheet with specific viscosity ranges at different shear rates, formulated with thermosetting and thermoplastic resins, including additives like layered silicate compounds, is used to minimize the intrusion of cured material by controlling fluidity during curing.
The resin sheet effectively seals elements while reducing the amount of cured material that penetrates between the element and the substrate, ensuring precise sealing and improved reliability.
Smart Images

Figure 0007577659000004 
Figure 0007577659000005 
Figure 0007577659000006
Abstract
Description
[Technical field]
[0001] The present invention relates to an encapsulating resin sheet, and more particularly to an encapsulating resin sheet for encapsulating an element. [Background technology]
[0002] Conventionally, it is known that a sealing sheet containing a thermosetting resin is used to seal a semiconductor element or an electronic component mounted on a substrate by pressing, and then the thermosetting resin is thermally cured to form a cured body from the sealing sheet (see, for example, Patent Document 1 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-162909 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, with the increasing sophistication of electronic devices, there is a demand for miniaturization of the semiconductor elements and electronic components used in them. Accordingly, there is a demand for improved dimensional accuracy during curing of the resin (cured body) that protects the semiconductor elements and electronic components. Specifically, there is a demand to further reduce the amount of intrusion of the cured body that intrudes between the semiconductor elements and electronic components and the substrate from the side edges of the semiconductor elements and electronic components.
[0005] The present invention provides an encapsulating resin sheet that can sufficiently encapsulate an element and can reduce intrusion of a cured body between an element, typically a semiconductor element or an electronic component, and a substrate. [Means for solving the problem]
[0006] The present invention [1] is a viscosity (ν 0.01 ) but 8×10 5The viscosity at 85°C (ν 0.1 ) but 8×10 5 It is an encapsulating resin sheet having a viscosity of less than Pa·s.
[0007] The present invention [2] is a viscosity (ν 0.01 ) and viscosity (ν 10 ) and the sealing resin sheet according to the above [1], which satisfies the following formula (1): ν 0.01 / ν 10 ≧70 (1) The present invention [3] is a viscosity (ν 10 ) is 0.4 × 10 5 The sealing resin sheet according to the above [1] or [2] has a viscosity of 0.1 Pa·s or less. Effect of the Invention
[0008] In the encapsulating resin sheet of the present invention, the viscosity at 85° C. at a shear rate of 0.01 rad / sec (ν 0.01 ) but 8×10 5 The viscosity at 85°C (ν 0.1 ) but 8×10 5 Less than Pa s.
[0009] Therefore, the elements can be sufficiently encapsulated, and when the encapsulating resin sheet is heated to form a cured body, the amount of the cured body that penetrates between the elements and the substrate can be reduced. [Brief description of the drawings]
[0010] [Figure 1]1A to 1D are cross-sectional views showing the process of manufacturing an electronic element package by encapsulating multiple electronic elements using a first embodiment of the encapsulating resin sheet of the present invention, where FIG. 1A shows the process of preparing an encapsulating resin sheet, FIG. 1B shows the process of preparing electronic elements, FIG. 1C shows the process of pressing the encapsulating resin sheet to form an encapsulated body, and FIG. 1D shows the process of heating the encapsulated body to form a hardened body. [Diagram 2] 2A to 2D are cross-sectional views showing the process of manufacturing an electronic element package by encapsulating multiple electronic elements using a second embodiment of the encapsulating resin sheet of the present invention, where FIG. 2A shows the process of preparing an encapsulating multilayer resin sheet, FIG. 2B shows the process of preparing electronic elements, FIG. 2C shows the process of pressing the encapsulating multilayer resin sheet to form an encapsulated body, and FIG. 2D shows the process of heating the encapsulated body to form a hardened body. [Diagram 3] 3A to 3D are cross-sectional views of steps in a method for measuring the penetration length Y of the hardened body in an embodiment, in which FIG. 3A shows a step (step A) of preparing a sealing multilayer resin sheet, FIG. 3B shows a step (step B) of preparing an electronic element (dummy element), FIG. 3C shows a step (step C) of pressing the sealing multilayer resin sheet to form a sealing body, and FIG. 3D shows a step (step D) of heating the sealing body to form a hardened body. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The encapsulating resin sheet of the present invention has a predetermined viscosity at 85° C. at a predetermined shear rate in a viscoelasticity measurement described later.
[0012] Hereinafter, a first embodiment of such an encapsulating resin sheet (one-layer encapsulating resin sheet) will be described.
[0013] The sealing resin sheet is a resin sheet for sealing an element, and has a generally plate shape (film shape) extending in a plane direction perpendicular to the thickness direction.
[0014] The material of the sealing resin sheet contains, for example, a thermosetting resin and a thermoplastic resin.
[0015] Examples of the thermosetting resin include epoxy resin, silicone resin, urethane resin, polyimide resin, urea resin, melamine resin, and unsaturated polyester resin.
[0016] The thermosetting resins can be used alone or in combination of two or more kinds.
[0017] The thermosetting resin is preferably an epoxy resin. The epoxy resin is prepared as an epoxy resin composition containing a base resin, a curing agent, and a curing accelerator.
[0018] Examples of the base agent include bifunctional epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, modified bisphenol A type epoxy resin, modified bisphenol F type epoxy resin, and biphenyl type epoxy resin, and polyfunctional epoxy resins having three or more functional groups such as phenol novolac type epoxy resin, cresol novolac type epoxy resin, trishydroxyphenylmethane type epoxy resin, tetraphenylolethane type epoxy resin, and dicyclopentadiene type epoxy resin. These base agents can be used alone or in combination of two or more. As the base agent, preferably, bifunctional epoxy resins, more preferably, bisphenol F type epoxy resins, can be used.
[0019] The lower limit of the epoxy equivalent of the base resin is, for example, 10 g / eq., or preferably 100 g / eq. The upper limit of the epoxy equivalent of the base resin is, for example, 300 g / eq., or preferably 250 g / eq.
[0020] The lower limit of the softening point of the base agent is, for example, 50° C., preferably 70° C., more preferably 72° C., and even more preferably 75° C. The upper limit of the softening point of the base agent is, for example, 130° C., preferably 110° C., and more preferably 90° C.
[0021] If the softening point of the base resin is equal to or higher than the above-mentioned lower limit, the encapsulating resin sheet 1 can flow in the step shown in Fig. 1C. Therefore, the time required for the step shown in Fig. 1C can be shortened, and one surface in the thickness direction of the encapsulating resin sheet 1 can be flattened in the step shown in Fig. 2C.
[0022] The lower limit of the ratio of the main agent in the material is, for example, 1 mass%, preferably 2 mass%. The upper limit of the ratio of the main agent in the material is, for example, 30 mass%, preferably 15 mass%. The lower limit of the ratio of the main agent in the epoxy resin composition is, for example, 30 mass%, preferably 50 mass%. The upper limit of the ratio of the main agent in the epoxy resin composition is, for example, 80 mass%, preferably 70 mass%.
[0023] The curing agent is a latent curing agent that cures the above-mentioned base material by heating. For example, the curing agent may be a phenolic resin such as phenol novolac resin. If the curing agent is a phenolic resin, the phenolic resin and the base material together form a cured product having high heat resistance and high chemical resistance. Therefore, the cured product has excellent sealing reliability.
[0024] The ratio of the curing agent is set to the following equivalent ratio. Specifically, the lower limit of the total of the hydroxyl groups in the phenolic resin relative to 1 equivalent of the epoxy group in the base agent is, for example, 0.7 equivalents, preferably 0.9 equivalents. The upper limit of the total of the hydroxyl groups in the phenolic resin relative to 1 equivalent of the epoxy group in the base agent is, for example, 1.5 equivalents, preferably 1.2 equivalents. Specifically, the lower limit of the number of parts of the curing agent contained relative to 100 parts by mass of the base agent is, for example, 20 parts by mass, preferably 40 parts by mass. The upper limit of the number of parts of the curing agent contained relative to 100 parts by mass of the base agent is, for example, 80 parts by mass, preferably 60 parts by mass.
[0025] The curing accelerator is a catalyst (thermal curing catalyst) that accelerates the curing of the base agent by heating. Examples of the curing accelerator include organic phosphorus compounds, such as imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole (2PHZ-PW). Preferably, imidazole compounds are used. The lower limit of the number of parts of the curing accelerator contained relative to 100 parts by mass of the base agent is, for example, 0.05 parts by mass. The upper limit of the number of parts of the curing accelerator contained relative to 100 parts by mass of the base agent is, for example, 5 parts by mass.
[0026] The lower limit of the content of the thermosetting resin in the material (sealing resin sheet) is, for example, 5 mass%, preferably 10 mass%, more preferably 13 mass%. The upper limit of the content of the thermosetting resin in the material (sealing resin sheet) is, for example, 30 mass%, preferably 25 mass%, more preferably 20 mass%.
[0027] Examples of thermoplastic resins include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resin (such as 6-nylon and 6,6-nylon), phenoxy resin, acrylic resin, saturated polyester resin (such as PET), polyamideimide resin, fluororesin, styrene-isobutylene-styrene block copolymer, etc. These thermoplastic resins can be used alone or in combination of two or more kinds.
[0028] As the thermoplastic resin, preferably, an acrylic resin is used from the viewpoint of improving dispersibility in the thermosetting resin.
[0029] Examples of the acrylic resin include a (meth)acrylic acid ester copolymer (preferably a carboxyl group-containing acrylic acid ester copolymer) obtained by polymerizing a monomer component including a (meth)acrylic acid alkyl ester having a linear or branched alkyl group and another monomer (copolymerizable monomer).
[0030] Examples of the alkyl group include alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, propyl, isopropyl, n-butyl, t-butyl, isobutyl, pentyl, and hexyl.
[0031] Examples of other monomers include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; glycidyl group-containing monomers such as glycidyl acrylate and glycidyl methacrylate; acid anhydride monomers such as maleic anhydride and itaconic anhydride; 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, and the like. ) 10-hydroxydecyl acrylate, 12-hydroxylauryl (meth)acrylate, or hydroxyl group-containing monomers such as (4-hydroxymethylcyclohexyl)-methyl acrylate, for example, styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, and other sulfonic acid group-containing monomers, 2-hydroxyethylacryloylphosphate, and other phosphoric acid group-containing monomers, for example, styrene monomers, and for example, acrylonitrile. These may be used alone or in combination of two or more. Preferably, a carboxyl group-containing monomer or a hydroxyl group-containing monomer is used, and more preferably, a carboxyl group-containing monomer is used.
[0032] The other monomers can be used alone or in combination of two or more kinds.
[0033] More preferably, the thermoplastic resin is an acrylic resin containing a carboxyl group, and further preferably, the thermoplastic resin is an acrylic resin containing a carboxyl group.
[0034] The lower limit of the acid value of the acrylic resin containing a carboxyl group is, for example, 18, or preferably 25. The upper limit of the acid value of the acrylic resin is 50, or preferably 40.
[0035] When the acid value is equal to or higher than the lower limit, the fluidity of the encapsulating resin sheet can be reduced when the encapsulating resin sheet is heated to form a cured body (the curing step described later), and an element or substrate can be obtained in which the penetration amount of the cured body falls within a predetermined range when the encapsulating resin sheet is heated to form a cured body (the curing step described later).
[0036] Furthermore, when the acid value is equal to or less than the upper limit, when the encapsulating resin sheet is heated to form a cured body (the curing process described later), the fluidity of the encapsulating resin sheet can be appropriately reduced, and an element or substrate in which the penetration amount of the cured body is within a predetermined range can be obtained.
[0037] The acid value can be measured by a conventional indicator titration method using potassium hydroxide.
[0038] The lower limit of the glass transition temperature Tg of the thermoplastic resin is, for example, −70° C., preferably −50° C., and more preferably −30° C. The upper limit of the glass transition temperature Tg of the thermoplastic resin is, for example, 0° C., preferably 5° C., and more preferably −5° C. The glass transition temperature Tg is a theoretical value calculated by, for example, the Fox equation, and a specific calculation method thereof is described in, for example, JP 2016-175976 A.
[0039] The lower limit of the weight average molecular weight of the thermoplastic resin is, for example, 100,000, preferably 300,000, more preferably 1,000,000, and further preferably 1,100,000. The upper limit of the weight average molecular weight of the thermoplastic resin is, for example, 1,400,000. The weight average molecular weight is measured by gel permeation chromatography (GPC) based on a standard polystyrene equivalent value.
[0040] The lower limit of the proportion of the thermoplastic resin in the material (sealing resin sheet) is, for example, 1 mass%, preferably 5 mass%, more preferably 15 mass%, and the upper limit of the proportion of the thermoplastic resin in the material is, for example, 30 mass%.
[0041] The lower limit of the proportion of the thermoplastic resin relative to the total amount of the thermoplastic resin and the thermosetting resin is, for example, 10 mass%, preferably 20 mass%, and the upper limit of the proportion of the thermoplastic resin relative to the total amount of the thermoplastic resin and the thermosetting resin is, for example, 40 mass%, preferably 30 mass%.
[0042] The material may further contain layered silicate compounds, inorganic fillers (other than layered silicate compounds), pigments, silane coupling agents, and other additives.
[0043] The layered silicate compound is dispersed in the thermosetting resin and the thermoplastic resin (resin matrix) in the material (sealing resin sheet). The layered silicate compound is a flow control agent when forming an encapsulant and a cured body (described later) from the sealing resin sheet. Specifically, the layered silicate compound is a curing flow reducer that reduces the flowability of the cured body when the sealing resin sheet is heated to form the cured body.
[0044] The layered silicate compound is, for example, a silicate having a structure (three-dimensional structure) in which layers extending two-dimensionally (in the plane direction) are stacked in the thickness direction, and is called a phyllosilicate.
[0045] Specifically, examples of the layered silicate compound include smectites such as montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, and stevensite, as well as kaolinite, halloysite, talc, and mica. As the layered silicate compound, smectite is preferably used from the viewpoint of improving the mixability with the thermosetting resin, and montmorillonite is more preferably used.
[0046] The layered silicate compound may be an unmodified one whose surface is not modified, or may be a modified one whose surface is modified with an organic component.Preferably, the layered silicate compound is surface-modified with an organic component from the viewpoint of obtaining excellent affinity with thermosetting resins and thermoplastic resins.Specifically, the layered silicate compound may be an organically modified smectite whose surface is modified with an organic component, or more preferably, an organically modified bentonite whose surface is modified with an organic component.
[0047] Examples of the organic component include organic cations (onium ions) such as ammonium, imidazolium, pyridinium, and phosphonium.
[0048] Examples of ammonium include dimethyl distearyl ammonium, distearyl ammonium, octadecyl ammonium, hexyl ammonium, octyl ammonium, 2-hexyl ammonium, dodecyl ammonium, trioctyl ammonium, etc. Examples of imidazolium include methyl stearyl imidazolium, distearyl imidazolium, methyl hexyl imidazolium, dihexyl imidazolium, methyl octylimidazolium, dioctylimidazolium, methyl dodecyl imidazolium, didodecyl imidazolium, etc. Examples of pyridinium include stearyl pyridinium, hexyl pyridinium, octyl pyridinium, dodecyl pyridinium, etc. Examples of the phosphonium include dimethyl distearyl phosphonium, distearyl phosphonium, octadecyl phosphonium, hexyl phosphonium, octyl phosphonium, 2-hexyl phosphonium, dodecyl phosphonium, and trioctyl phosphonium. The organic cation can be used alone or in combination of two or more kinds. Preferably, ammonium is used, and more preferably, dimethyl distearyl ammonium is used.
[0049] As the organically modified layered silicate compound, preferably, organically modified smectite the surface of which is modified with ammonium, and more preferably, organically modified bentonite the surface of which is modified with dimethyldistearylammonium, is used.
[0050] The lower limit of the average particle size of the layered silicate compound is, for example, 1 nm, preferably 5 nm, more preferably 10 nm. The upper limit of the average particle size of the layered silicate compound is, for example, 100 μm, preferably 50 μm, more preferably 10 μm. The average particle size of the layered silicate compound is determined as a D50 value (cumulative 50% median size) based on the particle size distribution determined by a particle size distribution measurement method in a laser scattering method.
[0051] As the layered silicate compound, commercially available products can be used. For example, commercially available organic bentonite products include the Esben series (manufactured by Hojun Co., Ltd.).
[0052] The lower limit of the content of the layered silicate compound in the material (sealing resin sheet) is, for example, 0.1 mass%, preferably 1 mass%, more preferably 2 mass%, and even more preferably 3 mass%. The upper limit of the content of the layered silicate compound in the material (sealing resin sheet) is, for example, 25 mass%, preferably 15 mass%, more preferably 10 mass%, and even more preferably 7 mass%.
[0053] Examples of inorganic fillers include silicate compounds other than layered silicate compounds such as orthosilicate, sorosilicate, and inosilicate, and silicon compounds (other than layered silicate compounds) such as quartz (silicic acid), silica (anhydrous silicic acid), and silicon nitride. Examples of inorganic fillers include alumina, aluminum nitride, and boron nitride. These can be used alone or in combination of two or more. Preferably, silicon compounds other than layered silicate compounds are used, and more preferably, silica.
[0054] The shape of the inorganic filler is not particularly limited, and examples thereof include a substantially spherical shape, a substantially plate shape, a substantially needle shape, an irregular shape, etc. A substantially spherical shape is preferable.
[0055] The upper limit of the average value of the maximum length of the inorganic filler (synonymous with the average particle diameter if the filler is substantially spherical) is, for example, 50 μm, preferably 20 μm, more preferably 10 μm. The lower limit of the average value of the maximum length of the inorganic filler is, for example, 0.1 μm, preferably 0.5 μm. The average particle diameter of the inorganic filler is determined as the D50 value (cumulative 50% median diameter) based on the particle size distribution determined by, for example, a particle size distribution measurement method in a laser scattering method.
[0056] The inorganic filler may also include a first filler, a second filler having an average maximum length smaller than the average maximum length of the first filler, and a third filler having an average maximum length smaller than the average maximum length of the second filler.
[0057] The lower limit of the average maximum length of the first filler is, for example, 1 μm, or preferably 3 μm.The upper limit of the average maximum length of the first filler is, for example, 50 μm, or preferably 30 μm.
[0058] The upper limit of the average value of the maximum length of the second filler is, for example, 0.9 μm, preferably 0.8 μm.The lower limit of the average value of the maximum length of the second filler is, for example, 0.02 μm, preferably 0.1 μm.
[0059] The upper limit of the average value of the maximum length of the third filler is, for example, 0.015 μm.The lower limit of the average value of the maximum length of the second filler is, for example, 0.001 μm, preferably 0.01 μm.
[0060] The lower limit of the ratio of the average maximum length of the first filler to the average maximum length of the second filler is, for example, 2, preferably 5. The upper limit of the ratio of the average maximum length of the first filler to the average maximum length of the second filler is, for example, 50, preferably 20.
[0061] The lower limit of the ratio of the average maximum length of the second filler to the average maximum length of the third filler is, for example, 10, preferably 20. The upper limit of the ratio of the average maximum length of the second filler to the average maximum length of the third filler is, for example, 60, preferably 50.
[0062] The materials of the first filler, the second filler and the third filler may be the same or different.
[0063] Furthermore, the surface of the inorganic filler may be partially or entirely treated with a silane coupling agent or the like.
[0064] The lower limit of the content of the inorganic filler in the material (sealing resin sheet) is, for example, 30 mass%, preferably 40 mass%, and the upper limit of the content of the inorganic filler in the material (sealing resin sheet) is, for example, 70 mass%, preferably 60 mass%.
[0065] When the content ratio and / or the content number of the inorganic filler is equal to or more than the above-mentioned lower limit, the sealing resin sheet 1 can flow in the step shown in FIG. 1C.
[0066] In the case where the inorganic filler includes the first filler and the second filler (does not include the third filler), the lower limit of the content ratio of the first filler in the material (sealing resin sheet) is, for example, 20 mass%, preferably 30 mass%. The upper limit of the content ratio of the first filler in the material (sealing resin sheet) is, for example, 60 mass%, preferably 50 mass%. The lower limit of the content ratio of the second filler in the material (sealing resin sheet) is, for example, 10 mass%, preferably 15 mass%. The upper limit of the content ratio of the second filler in the material (sealing resin sheet) is, for example, 30 mass%, preferably 25 mass%. The lower limit of the content number of the second filler relative to 100 mass parts of the first filler is, for example, 30 mass parts, preferably 40 mass parts, more preferably 50 mass parts. The upper limit of the number of parts of the second filler contained per 100 parts by mass of the first filler is, for example, 70 parts by mass, preferably 60 parts by mass, and more preferably 55 parts by mass.
[0067] When the inorganic filler includes a first filler, a second filler, and a third filler, the lower limit of the content ratio of the first filler in the material (sealing resin sheet) is, for example, 20 mass%, preferably 30 mass%. The upper limit of the content ratio of the first filler in the material (sealing resin sheet) is, for example, 60 mass%, preferably 50 mass%. The lower limit of the content ratio of the second filler in the material (sealing resin sheet) is, for example, 10 mass%, preferably 15 mass%. The upper limit of the content ratio of the second filler in the material (sealing resin sheet) is, for example, 30 mass%, preferably 25 mass%. The lower limit of the content ratio of the third filler in the material (sealing resin sheet) is, for example, 1 mass%, preferably 3 mass%. The upper limit of the content ratio of the third filler in the material (sealing resin sheet) is, for example, 10 mass%, preferably 5 mass%. The lower limit of the number of parts of the second filler relative to 100 parts by mass of the first filler is, for example, 30 parts by mass, preferably 40 parts by mass, more preferably 50 parts by mass. The upper limit of the number of parts of the second filler relative to 100 parts by mass of the first filler is, for example, 70 parts by mass, preferably 60 parts by mass, more preferably 55 parts by mass. The lower limit of the number of parts of the third filler relative to 100 parts by mass of the second filler is, for example, 10 parts by mass, preferably 15 parts by mass. The upper limit of the number of parts of the third filler relative to 100 parts by mass of the second filler is, for example, 40 parts by mass, preferably 30 parts by mass.
[0068] The pigment may be, for example, a black pigment such as carbon black. The lower limit of the pigment particle size is, for example, 0.001 μm. The upper limit of the pigment particle size is, for example, 1 μm. The pigment particle size is an arithmetic mean diameter determined by observing the pigment with an electron microscope. The lower limit of the ratio of the pigment to the material is, for example, 0.1% by mass. The upper limit of the ratio of the pigment to the material is, for example, 2% by mass.
[0069] Examples of the silane coupling agent include silane coupling agents containing an epoxy group. Examples of the silane coupling agent containing an epoxy group include 3-glycidoxydialkyldialkoxysilanes such as 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxyalkyltrialkoxysilanes such as 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane. Preferably, 3-glycidoxyalkyltrialkoxysilane is used. The lower limit of the content of the silane coupling agent in the material is, for example, 0.1% by mass, preferably 0.5% by mass. The upper limit of the content of the silane coupling agent in the material is, for example, 10% by mass, preferably 5% by mass, more preferably 2% by mass.
[0070] To obtain this sealing resin sheet, the above-mentioned components are mixed in the above-mentioned ratio to prepare a material. When a layered silicate compound is mixed into the material, the above-mentioned components are preferably thoroughly stirred to uniformly disperse the layered silicate compound in the thermosetting resin and the thermoplastic resin.
[0071] If necessary, a solvent (such as a ketone such as methyl ethyl ketone) is further added to prepare a varnish. The varnish is then applied to a release sheet (not shown) and then dried by heating to produce a sealing resin sheet having a sheet shape. On the other hand, a sealing resin sheet can also be formed from the material by kneading and extrusion without preparing a varnish.
[0072] The encapsulating resin sheet thus formed is in a B-stage (semi-cured state), specifically, a state before the C-stage. That is, a state before the complete curing. The encapsulating resin sheet is formed into a B-stage sheet from an A-stage material by heating during the above-mentioned drying or extrusion kneading.
[0073] The lower limit of the thickness of the encapsulating resin sheet is, for example, 10 μm, preferably 25 μm, more preferably 50 μm. The upper limit of the thickness of the encapsulating resin sheet is, for example, 3000 μm, preferably 1000 μm, more preferably 500 μm, and still more preferably 300 μm.
[0074] Next, a method for manufacturing an electronic element package 51 by encapsulating an electronic element, as an example of an element, with an encapsulating resin sheet will be described with reference to FIGS. 1A to 1D.
[0075] In this method, first, an encapsulating resin sheet 1 is prepared (preparation step) as shown in Fig. 1A. The encapsulating resin sheet 1 has one surface and the other surface in the thickness direction that face each other in the thickness direction.
[0076] Separately, an electronic element 21 is prepared as shown in FIG. 1B.
[0077] The electronic elements 21 include electronic components, and are mounted, for example, in multiple numbers on a substrate 22. The multiple electronic elements 21 and the substrate 22 are provided on an element mounting substrate 24 together with bumps 23. In other words, the element mounting substrate 24 includes the multiple electronic elements 21, the substrate 22, and the bumps 23.
[0078] The substrate 22 has a generally flat plate shape extending in a planar direction. On one surface 25 in the thickness direction of the substrate 22, terminals (not shown) to be electrically connected to electrodes (not shown) of the electronic element 21 are provided.
[0079] Each of the electronic elements 21 has a generally flat plate shape (chip shape) extending in a planar direction. The electronic elements 21 are arranged at intervals from one another in the planar direction. The other thickness direction surfaces 28 of the electronic elements 21 are parallel to one thickness direction surface 25 of the substrate 22. An electrode (not shown) is provided on the other thickness direction surface 28 of each of the electronic elements 21. The electrode of the electronic element 21 is electrically connected to a terminal of the substrate 22 via a bump 23, which will be described next. A gap (space) 26 is provided between the other thickness direction surface 28 of the electronic element 21 and one thickness direction surface 25 of the substrate 22.
[0080] The lower limit of the interval between adjacent electronic elements 21 is, for example, 50 μm, preferably 100 μm, and more preferably 200 μm. The upper limit of the interval between adjacent electronic elements 21 is, for example, 10 mm, preferably 5 mm, and more preferably 1 mm. If the interval between adjacent electronic elements 21 is equal to or less than the above upper limit, more electronic elements 21 can be mounted on the substrate 22, and space can be saved.
[0081] The bumps 23 electrically connect the electrodes (not shown) of the multiple electronic elements 21 to the terminals of the substrate 22. The bumps 23 are disposed between the electrodes of the electronic elements 21 and the terminals of the substrate 22. Examples of materials for the bumps 23 include solder and metals such as gold. The thickness of the bumps 23 corresponds to the thickness (height) of the gaps 26. The thickness of the bumps 23 is set appropriately depending on the application and purpose of the element mounting substrate 24.
[0082] 1B, the encapsulating resin sheet 1 is placed on the plurality of electronic elements 21 (placement step). Specifically, the other thickness-wise surface of the encapsulating resin sheet 1 is brought into contact with one thickness-wise surface of the plurality of electronic elements 21.
[0083] 1C, the encapsulating resin sheet 1 and the element mounting board 24 are pressed (encapsulating step). Preferably, the encapsulating resin sheet 1 and the element mounting board 24 are heat-pressed.
[0084] For example, the sealing resin sheet 1 and the element mounting board 24 are sandwiched in the thickness direction and pressed by a press 27 equipped with two flat plates. Note that the flat plates of the press 27 are equipped with, for example, a heat source (not shown).
[0085] The pressing conditions (pressure, time, temperature, and the like) are not particularly limited, and conditions are selected that allow the sealing resin sheet 1 to penetrate between the plurality of electronic elements 21 while not damaging the element mounting substrate 24. More specifically, the pressing conditions are set so that the sealing resin sheet 1 flows and penetrates between the adjacent electronic elements 21, covering the peripheral side surfaces of each of the plurality of electronic elements 21, and contacting one surface 25 in the thickness direction of the substrate 22 that does not overlap with the electronic elements 21 in a plan view.
[0086] Specifically, the lower limit of the pressing pressure is, for example, 0.01 MPa, preferably 0.05 MPa. The upper limit of the pressing pressure is, for example, 10 MPa, preferably 5 MPa. The lower limit of the pressing time is, for example, 0.3 minutes, preferably 0.5 minutes. The upper limit of the pressing time is, for example, 10 minutes, preferably 5 minutes.
[0087] Specifically, the lower limit of the heating temperature is, for example, 40°C, or preferably 60°C. The upper limit of the heating temperature is, for example, 100°C, or preferably 95°C.
[0088] By pressing the encapsulating resin sheet 1, the encapsulating resin sheet 1 is plastically deformed to correspond to the outer shape of the electronic elements 21. The other surface in the thickness direction of the encapsulating resin sheet 1 is deformed into a shape corresponding to one surface in the thickness direction and peripheral side surfaces of the multiple electronic elements 21.
[0089] The sealing resin sheet 1 undergoes plastic deformation while maintaining the B stage.
[0090] As a result, the sealing resin sheet 1 covers the peripheral side surfaces of each of the multiple electronic elements 21, and contacts one surface 25 in the thickness direction of the substrate 22 that does not overlap with the electronic elements 21 in a plan view.
[0091] In this way, the sealing body 31 that seals the electronic element 21 is formed (produced) from the sealing resin sheet 1. One surface in the thickness direction of the sealing body 31 becomes a flat surface.
[0092] At this time, the encapsulant 31 is allowed to slightly intrude into the gap (the gap between the electronic element 21 and the substrate 22) 26. Specifically, the encapsulant 31 is allowed to have an intrusion length X (see FIG. 3C ) of the encapsulant 31 intruding into the gap 26, based on the side edge 75 of the electronic element 21.
[0093] Specifically, the upper limit of the sealant penetration length X is, for example, 20 μm, preferably 10 μm, more preferably 5 μm, further preferably 3 μm, and particularly preferably 1 μm.
[0094] Thereafter, as shown in FIG. 1D, the sealed body 31 is heated to form a hardened body 41 from the sealed body 31 (hardening step).
[0095] Specifically, the sealing body 31 and the element mounting board 24 are removed from the press 27, and then the sealing body 31 and the element mounting board 24 are heated in a dryer under atmospheric pressure.
[0096] The lower limit of the heating temperature (cure temperature) is, for example, 100° C., preferably 120° C. The upper limit of the heating temperature (cure temperature) is, for example, 200° C., preferably 180° C. The lower limit of the heating time is, for example, 10 minutes, preferably 30 minutes. The upper limit of the heating time is, for example, 180 minutes, preferably 120 minutes.
[0097] By heating the above-described sealed body 31, a C-stage (completely cured) hardened body 41 is formed from the sealed body 31. One surface in the thickness direction of the hardened body 41 is an exposed surface.
[0098] The edge of the sealing body 31 that has been allowed to slightly penetrate into the gap is allowed to further penetrate slightly into the gap 26 to become the hardened body 41, but the extent of this is suppressed as small as possible. Specifically, the hardened body 41 can have a small value (YX) (hereinafter referred to as the sealing body penetration amount (YX)) obtained by subtracting the sealing body penetration length X from the hardened body penetration length Y (see FIG. 3D) of the hardened body 41 penetrating into the gap 26, based on the side edge 75 of the electronic element 21.
[0099] Specifically, the upper limit of the hardened body penetration length Y is, for example, 45 μm, preferably 25 μm, more preferably 20 μm, even more preferably 10 μm, particularly preferably 5 μm, and most preferably 1 μm. The lower limit of the hardened body penetration length Y is, for example, −25 μm, preferably −10 μm, and more preferably −5 μm.
[0100] The upper limit of the penetration amount (YX) of the sealant is, for example, 30 μm, preferably 15 μm, more preferably 10 μm, even more preferably 5 μm, particularly preferably 3 μm, and most preferably 1 μm.
[0101] In addition, this sealing resin sheet 1 has a predetermined viscosity at 85° C. and a predetermined shear rate in a viscoelasticity measurement described in detail in an example below.
[0102] Specifically, the viscosity (ν 0.01 ) lower limit is 8×10 5 Pa s, preferably 10 x 10 5 The viscosity (ν 0.01 ) is, for example, 25×10 5 Pa s, preferably 18 x 10 5 Pa·s.
[0103] In addition, the viscosity at 85°C (ν 0.1 ) is capped at 8×10 5 Less than Pa s, preferably 5×105 Viscosity (ν) at 85°C at a shear rate of 0.1 rad / s is less than Pa·s. 0.1 ) is, for example, 1×10 5 Pa·s.
[0104] Viscosity (ν) at 85°C at a shear rate of 0.01 rad / s 0.01 ) is equal to or greater than the lower limit above, and the viscosity at 85°C (ν 0.1 ) is less than the above upper limit, when the encapsulating resin sheet 1 is placed on the electronic element 21 and the encapsulating resin sheet 1 (sealing body 31) is heated to form a cured body 41 as shown in FIG. 1D, the amount of the cured body 41 penetrating into the gap 26 between the electronic element 21 and the substrate 22 can be reduced.
[0105] In detail, the encapsulating resin sheet 1 has a high viscosity when the shear stress (shear rate) is low (specifically, a viscosity (ν 0.01 ) is equal to or higher than the lower limit above), and when the shear stress (shear rate) is high, the viscosity is low (specifically, the viscosity (ν 0.1 ) is less than the above upper limit).
[0106] Such thixotropy allows the viscosity of the sealing resin sheet 1 to be low in the sealing process (when the shear force (shear rate) is high), allowing the sealing resin sheet 1 to penetrate between multiple electronic elements 21, while allowing the viscosity of the sealing resin sheet 1 to be high in the curing process (when the shear force (shear rate) is low), reducing the amount of penetration of the cured body 41 into the gap 26 between the electronic element 21 and the substrate 22.
[0107] On the other hand, the viscosity at 85°C (ν 0.01If the above lower limit is exceeded, the flowability of the encapsulating resin sheet 1 cannot be reduced when the encapsulating resin sheet is heated to form a cured body (curing step). As a result, the amount of the cured body penetrating between the element and the substrate cannot be reduced when the encapsulating resin sheet is heated to form a cured body (curing step).
[0108] In addition, the viscosity at 85°C (ν 0.1 ) is equal to or greater than the upper limit, the sealing resin sheet 1 cannot sufficiently penetrate between the plurality of electronic elements 21.
[0109] Viscosity (ν) at 85°C at a shear rate of 0.01 rad / s 0.01 ) and the viscosity (ν 0.1 ) preferably satisfies the following formula (2), more preferably satisfies the following formula (3), and further preferably satisfies the following formula (4). ν 0.01 / ν 0.1 ≧2 (2) ν 0.01 / ν 0.1 ≧3 (3) ν 0.01 / ν 0.1 ≧4 (4) In addition, the viscosity at 85°C (ν 0.01 ) and the viscosity (ν 0.1 ) preferably satisfies the following formula (5), and more preferably satisfies the following formula (6): ν 0.01 / ν 0.1 <= 6 (5) ν 0.01 / ν 0.1 <=5 (6) Viscosity (ν) at 85°C at a shear rate of 0.01 rad / s 0.01 ) and the viscosity (ν 0.1 ) satisfies the above formula (2), (3), or (4), a thixotropic property sufficient to achieve the above-mentioned effects can be exhibited.
[0110] In addition, the viscosity at 85°C (ν 10 ) is, for example, 0.4×10 5 Pa s, preferably 0.2×10 5 The viscosity (ν 10 ) is, for example, 0.01×10 5 Pa s, preferably 0.05 x 10 5 Pa·s.
[0111] Viscosity (ν 10 ), the viscosity of the encapsulating resin sheet 1 can be reduced in the encapsulating step (when the shear force (shear rate) is high), allowing the encapsulating resin sheet 1 to penetrate between multiple electronic elements 21.
[0112] In addition, the viscosity at 85°C (ν 0.01 ) and viscosity (ν 10 ) preferably satisfies the following formula (7), more preferably satisfies the following formula (8), even more preferably satisfies the following formula (9), and particularly preferably satisfies the following formula (10). ν 0.01 / ν 10 ≧40 (7) ν 0.01 / ν 10 ≧70 (8) ν 0.01 / ν 10 ≧100 (9) ν 0.01 / ν 10 ≧120 (10) In addition, the viscosity at 85°C (ν 0.01 ) and viscosity (ν 10 ) preferably satisfies the following formula (11), and more preferably satisfies the following formula (12): ν 0.01 / ν10 <=200 (11) ν 0.01 / ν 10 <= 150 (12) Viscosity (ν) at 85°C at a shear rate of 0.01 rad / s 0.01 ) and viscosity (ν 10 ) satisfies the above formula (7), (8), (9), or (10) (preferably, satisfies the above formula (8)), a thixotropic property sufficient to achieve the above-mentioned effects can be exhibited.
[0113] Next, a second embodiment (multilayer encapsulating resin sheet) of the present invention will be described.
[0114] In the second embodiment, as shown in Figures 2A to 2D, an electronic element 21 is encapsulated by an encapsulating multilayer resin sheet 11 having an encapsulating resin sheet 1 and a second encapsulating resin sheet 12 in that order on one side in the thickness direction, and then a cured body 41 is formed.
[0115] The encapsulating multilayer resin sheet 11 includes an encapsulating resin sheet 1 and a second encapsulating resin sheet 12 disposed on the entire surface of one surface in the thickness direction of the encapsulating resin sheet 1. Preferably, the encapsulating multilayer resin sheet 11 includes only the encapsulating resin sheet 1 and the second encapsulating resin sheet 12.
[0116] The material of the second sealing resin sheet 12 is the same as the material (thermosetting resin composition) of the sealing resin sheet 1, but does not contain a layered silicate compound. The lower limit of the ratio of the thickness of the second sealing resin sheet 12 to the thickness of the sealing resin sheet 1 is, for example, 0.5, preferably 1, and more preferably 2. The upper limit of the ratio of the thickness of the second sealing resin sheet 12 to the thickness of the sealing resin sheet 1 is, for example, 10, and preferably 5.
[0117] A method for manufacturing an electronic element cured body package 50 by encapsulating a plurality of electronic elements 21 with an encapsulating multilayer resin sheet 11 and then forming a cured body 41 will be described with reference to Figs. 2A to 2D.
[0118] 2A, a sealing multilayer resin sheet 11 is prepared. Specifically, the sealing resin sheet 1 and a second sealing resin sheet 12 are bonded together.
[0119] As shown in FIG. 2B, a plurality of electronic elements 21 to be mounted on a substrate 22 are prepared.
[0120] Next, the encapsulating multilayer resin sheet 11 is placed on the electronic element 21 so that the other surface in the thickness direction of the encapsulating resin sheet 1 contacts one surface in the thickness direction of the electronic element 21 .
[0121] As shown in FIG. 2C, thereafter, the sealing resin sheet 1 and the element mounting board 24 are pressed.
[0122] By pressing, the sealing resin sheet 1, which has the above-mentioned thixotropy, flows and infiltrates between the adjacent electronic elements 21. On the other hand, even when pressed, the fluidity of the second sealing resin sheet 12 does not change significantly and remains low, so that infiltration between the adjacent electronic elements 21 is suppressed.
[0123] As a result, a sealing body 31 for sealing the plurality of electronic elements 21 is formed from the sealing multilayer resin sheet 11 .
[0124] In addition, when the sealing resin sheet 1 contains a filler at a ratio equal to or greater than the above-mentioned lower limit and the second sealing resin sheet 12 contains a filler at a ratio equal to or greater than the above-mentioned lower limit, the sealing resin sheet 1 and the second sealing resin sheet 12 can flow by the press shown in FIG. 2C.
[0125] At this time, the encapsulating resin sheet 1 is in contact with the electronic element 21, while the second encapsulating resin sheet 12 is located on the opposite side of the electronic element 21 with respect to the encapsulating resin sheet 1. In other words, an edge of the encapsulating body 31 facing the gap 26 is formed from the encapsulating resin sheet 1. On the other hand, one surface in the thickness direction of the encapsulating body 31 is formed from the second encapsulating resin sheet 12.
[0126] Thereafter, as shown in FIG. 2D, sealed body 31 is heated to form hardened body 41 from sealed body 31.
[0127] Since the encapsulating multilayer resin sheet 11 includes the above-mentioned encapsulating resin sheet 1, the amount of the cured body 41 that enters the gap 26 can be reduced.
[0128] In particular, if the encapsulating resin sheet 1 and the second encapsulating resin sheet 12 contain a base material of an epoxy resin having a softening point of 50° C. or more and 130° C. or less, the encapsulating resin sheet 1 and the second encapsulating resin sheet 12 can flow in the step shown in Fig. 2C. This allows the time for the step shown in Fig. 2C to be shortened, and allows one surface in the thickness direction of the second encapsulating resin sheet 12 to be flattened in the step shown in Fig. 2C.
[0129] Furthermore, if the sealing resin sheet 1 and the second sealing resin sheet 12 contain a phenol resin as a curing agent together with the epoxy resin as a main agent, the cured body 41 has high heat resistance and high chemical resistance. Therefore, the cured body 41 has excellent sealing reliability.
[0130] 2C, the second sealing resin sheet 12 is fluidized by the pressing force, and one surface in the thickness direction becomes flat. In addition, in the step shown in Fig. 2C, in the sealing multilayer resin sheet 11, as described above, the sealing resin sheet 1 together with the second sealing resin sheet 12 is softened and fluidized by the pressing force, and is deformed to follow the outer shape of the electronic element 21. In the step shown in Fig. 2C, the sealing resin sheet 1 is allowed to enter the gap 26 slightly.
[0131] Variations In the following modified examples, the same reference numerals are used for the same components and steps as those in the first and second embodiments, and detailed descriptions thereof will be omitted. In addition, each modified example can achieve the same effects as those in the first and second embodiments, unless otherwise specified. Furthermore, the first and second embodiments and their modified examples can be appropriately combined.
[0132] In the first embodiment, the electronic element 21 is sealed with one layer of the sealing resin sheet 1. However, although not shown, the electronic element 21 can also be sealed with a plurality of sealing resin sheets 1 (a laminate sheet).
[0133] Moreover, the second sealing resin sheet 12 in the sealing multilayer resin sheet 11 may be multilayered.
[0134] As an example of an element, there is mentioned an electronic element 21 arranged across a gap 26 from one surface 25 in the thickness direction of the substrate 22, which is sealed with the sealing resin sheet 1; however, for example, although not shown, there can also be mentioned an electronic element 21 in contact with one surface 25 in the thickness direction of the substrate 22, which can be sealed with the sealing resin sheet 1.
[0135] Furthermore, although the electronic element 21 has been given as an example of an element, a semiconductor element may also be given. EXAMPLES
[0136] The present invention will be described in more detail below with reference to preparation examples, comparative preparation examples, examples and comparative examples. The present invention is not limited to the preparation examples, comparative preparation examples, examples and comparative examples. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters and the like used in the following description can be replaced with the upper limit (numeric value defined as "less than or equal to" or "less than") or lower limit (numeric value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters and the like described in the above "Form for carrying out the invention".
[0137] The components used in the Preparation Examples and Comparative Preparation Examples are shown below.
[0138] Layered silicate compound: Esben NX manufactured by Hojun Co., Ltd. (organic bentonite whose surface is modified with dimethyl distearyl ammonium) Base material: YSLV-80XY manufactured by Nippon Steel Chemical Co., Ltd. (bisphenol F type epoxy resin, high molecular weight epoxy resin, epoxy equivalent 200g / eq., solid, softening point 80℃) Hardener: Gun-ei Chemical's LVR-8210DL (novolac type phenolic resin, latent hardener, hydroxyl equivalent: 104 g / eq., solid, softening point: 60°C) Acrylic resin 1: HME-2006M manufactured by Negami Chemical Industries, carboxyl group-containing acrylic acid ester copolymer (acrylic resin), acid value: 32, number of functional groups: 736, weight average molecular weight: 1,290,000, glass transition temperature (Tg): -13.9°C, methyl ethyl ketone solution with solid content concentration of 20% by mass Acrylic resin 2: HME-2000M manufactured by Negami Chemical Industries, carboxyl group-containing acrylic acid ester copolymer (acrylic resin), acid value: 20, number of functional groups: 367, weight average molecular weight: 1,030,000, glass transition temperature (Tg): 3.7°C, methyl ethyl ketone solution with a solid content of 20% by mass Acrylic resin 3: HME-2004M manufactured by Negami Chemical Industries, acrylic acid ester copolymer (acrylic resin), acid value: 0, number of functional groups: 0, weight average molecular weight: 1,180,000, glass transition temperature (Tg): -3°C, methyl ethyl ketone solution with a solid content of 20% by mass Silane coupling agent: Shin-Etsu Chemical's KBM-403 (3-glycidoxypropyltrimethoxysilane) First filler: FB-8SM (spherical fused silica powder (inorganic filler), average particle size 7.0 μm) Second filler: Inorganic filler (amorphous silica and surface-treated amorphous silica) obtained by surface-treating SC220G-SMJ (average particle size 0.5 μm) manufactured by Admatechs Co., Ltd. with 3-methacryloxypropyltrimethoxysilane (product name: KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.), inorganic particles surface-treated with 1 part by mass of a silane coupling agent per 100 parts by mass of the inorganic filler Third filler: AEROSIL200 (average particle size 12 nm) manufactured by Nippon Aerosil Co., Ltd., hydrophilic silica particles Curing accelerator: 2PHZ-PW (2-phenyl-4,5-dihydroxymethylimidazole) manufactured by Shikoku Chemical Industry Co., Ltd. Solvent: Methyl ethyl ketone (MEK) Carbon black: Mitsubishi Chemical #20, particle size 50 nm Preparation Examples 1 to 3 and Comparative Preparation Examples 1 to 3 A varnish of the material was prepared according to the compounding recipe shown in Table 1. The varnish was applied to the surface of a release sheet and then dried at 120° C. for 2 minutes to produce an encapsulating resin sheet 1 having a thickness of 65 μm. The encapsulating resin sheet 1 was in the B stage.
[0139] Preparation Example 4 A varnish of the material was prepared according to the compounding recipe shown in Table 2. The varnish was applied to the surface of a release sheet and then dried at 120° C. for 2 minutes to prepare a second sealing resin sheet 12 having a thickness of 195 μm. The second sealing resin sheet 12 was in the B stage.
[0140] Example 1 、2 and Comparative Example 1 to Comparative Example 4 In a combination of preparation examples as shown in Table 3, an encapsulating resin sheet and a second encapsulating resin sheet were laminated together to prepare an encapsulating multilayer resin sheet having a thickness of 260 μm.
[0141] evaluation <Measurement of penetration length of hardened material> The following steps A to E were carried out to measure the penetration length Y of the hardened body.
[0142] Step A: As shown in FIG. 3A, a sample sheet 61 having a length of 10 mm, a width of 10 mm and a thickness of 260 μm is prepared from the encapsulating multilayer resin sheet 11 of each of the Examples and Comparative Examples.
[0143] Step B: As shown in FIG. 3B, a dummy element mounting substrate 74 is prepared in which a dummy element 71 measuring 3 mm in length, 3 mm in width, and 200 μm in thickness is mounted on a glass substrate 72 via a bump 23 having a thickness of 20 μm.
[0144] Step C: As shown in FIG. 3C, the sample sheet 61 is used to seal the dummy elements 71 on the dummy element mounting substrate 74 by vacuum plate pressing at a temperature of 65° C., a pressure of 0.1 MPa, a vacuum degree of 1.6 kPa, and a pressing time of 1 minute, thereby forming a sealed body 31 from the sample sheet 61.
[0145] Step D: As shown in FIG. 3D, the sealed body 31 is thermally cured by heating at 150° C. under atmospheric pressure for 1 hour, and a cured body 41 is formed from the sealed body 31.
[0146] Step E: As shown in the enlarged view of Figure 3D, using the side edge 75 of the dummy element 71 as a reference, the penetration length Y of the hardened body 41 from the side edge 75 into the gap 26 between the dummy element 71 and the glass substrate 72 is measured.
[0147] The hardened body penetration length Y was evaluated according to the following criteria. The results are shown in Table 3. ⊚: The hardened body penetration length Y was 0 μm or more and 25 μm or less. ◯: The hardened body penetration length Y was more than 25 μm and 45 μm or less, or less than 0 μm and −25 μm or more. ×: The hardened body penetration length Y was more than 45 μm or less than −25 μm.
[0148] In the evaluation, "minus" means that a space (see the thick dashed line in FIG. 2D) is formed that protrudes outward from side edge 75 of dummy element 71. The absolute value of "minus" corresponds to the protruding length of the space.
[0149] <Measurement of the penetration length of the sealing body> For the encapsulating multilayer resin sheet 11 of each of the Examples and Comparative Examples, the following step F was further carried out between the above-mentioned steps C and D to measure the encapsulant penetration length X. The results are shown in Table 3.
[0150] Step F: Using side edge 75 of dummy element 71 as a reference, the penetration length X of sealant 31 from side edge 75 into gap 26 between dummy element 22 and glass substrate 72 was measured. The results are shown in Table 3. ⊚: The penetration length X of the sealing body was 0 μm or more and 10 μm or less. ◯: The sealing body penetration length X was more than 10 μm and 20 μm or less. ×: The penetration length X of the sealing body was less than 20 μm.
[0151] <Amount of encapsulant penetration> The penetration amount of the plugged body (YX) was calculated by subtracting the penetration length X of the plugged body obtained by the above method from the penetration length Y of the hardened body obtained by the above method. The results are shown in Table 3. ⊚: The penetration amount (YX) of the sealing body was 0 μm or more and 15 μm or less. ◯: The amount of penetration of the sealing body (YX) was more than 15 μm and 30 μm or less. ×: The penetration amount (YX) of the sealing body exceeded 30 μm.
[0152] <Viscoelasticity measurement> Example 1 、2 , Comparative Example 1 to Comparative Example 4 The viscoelasticity of the sealing resin sheet 1 (B stage) was measured.
[0153] Specifically, the viscoelasticity measurements were carried out using a rheometer (Mars III) (measurement conditions: using an 8 mmφ plate, temperature 85° C., strain amount 0.005%). The results are shown in Table 3.
[0154] Consideration Viscosity (ν) at 85°C at a shear rate of 0.01 rad / s 0.01 ) but 8×10 5 Viscosity (ν ) at 85°C at a shear rate of 0.1 rad / s or more (Pa·s) 0.1 ) but 8×10 5 Example 1: Less than Pa·s , 2 and compare example 4 is the viscosity (ν 0.01) but 8×10 5 It can be seen that the penetration length and penetration amount of the plug are smaller than those of Comparative Example 1 and Comparative Example 2, which are less than Pa·s. In addition, the viscosity (ν 0.1 ) but 8×10 5 In Comparative Example 3, which was Pa·s or more, the sealing resin sheet could not be sufficiently infiltrated between the multiple dummy elements.
[0155] From this, the viscosity (ν 0.01 ) but 8×10 5 Viscosity (ν ) at 85°C at a shear rate of 0.1 rad / s or more (Pa·s) 0.1 ) but 8×10 5 It can be seen that if the viscosity is less than Pa·s, the element can be sufficiently sealed and the amount of the cured body that penetrates between the element and the substrate can be reduced.
[0156] [Table 1]
[0157] [Table 2]
[0158] [Table 3]
[0159] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as being limited. Modifications of the present invention that are obvious to those skilled in the art are included in the scope of the following claims. [Industrial Applicability]
[0160] The sealing resin sheet is used to seal elements. [Explanation of symbols]
[0161] 1 Sealing resin sheet
Claims
1. A composition comprising a thermosetting resin, a thermoplastic resin, and a layered silicate compound, The acid value of the thermoplastic resin is 18 mgKOH / g or more, Viscosity (ν) at 85° C. at a shear rate of 0.01 rad / s 0.01 ) but 8 x 10 5 Pa s or more, Viscosity (ν) at 85° C. at a shear rate of 0.1 rad / s 0.1 ) but 8 x 10 5 A sealing resin sheet having a viscosity of less than Pa·s.
2. Viscosity (ν) at 85° C. at a shear rate of 0.01 rad / s 0.01 ) and viscosity (v 10 2. The encapsulating resin sheet according to claim 1, wherein the above formula (1) is satisfied: ν 0.01 / ν 10 ≧70 (1)
3. Viscosity (ν) at 85° C. at a shear rate of 10 rad / s 10 ) is 0.4 × 10 5 The sealing resin sheet according to claim 1 , wherein the viscosity is equal to or less than Pa·s.
Citation Information
Patent Citations
Resin composition, material for substrate and substrate film
JP2005133055A
Sealing sheet
JP2006321216A
Resin sheet for electronic device sealing use, and method for manufacturing electronic device package
JP2015043378A
Sheet for sealing electronic device and manufacturing method of electronic device package
JP2015061017A
Thermosetting resin sheet for encapsulation, and manufacturing method of hollow package
JP2015179814A