Method for manufacturing light-transmitting laminate
By coating specific areas of the metal thin film with a material to isolate the gas-liquid interface during anodization, the method addresses inefficiencies in existing anodizing processes, achieving uniform and efficient production of transparent laminates with improved safety and reduced processing time.
Patent Information
- Application Number
- JP2020206027
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-11
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing methods for anodizing metal thin films on translucent bases face inefficiencies due to preferential reaction at the gas-liquid interface, leading to non-conductive films and uneven metal layer residuals, with safety risks from hazardous electrolytes and prolonged processing times.
A method involving coating specific portions of the metal thin film with a material like adhesive tape to isolate the gas-liquid interface during anodization, ensuring uniform anodization across the entire immersed area, using controlled electrolytic conditions.
This approach allows for efficient and uniform anodization of the metal thin film on translucent bases in a shorter time, producing high-quality, transparent laminates with consistent properties.
Smart Images

Figure 0007577992000002 
Figure 0007577992000003 
Figure 0007577992000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a light-transmitting laminate. [Background technology]
[0002] A method called anodizing is widely used to improve the corrosion resistance and wear resistance of metals. Anodizing is a method in which an oxide film is artificially generated on the surface of the target metal by electrolytically treating the metal with an anode, and the metal is protected by the oxide film. The film obtained by anodizing is transparent, but if the base metal remains, the overall surface becomes opaque. For this reason, metals that have been anodized in this way have not been used in applications where transparency is required.
[0003] It is possible to produce a transparent material by completely anodizing the underlying metal, and to achieve this, it is sufficient to make the metal layer thin. For example, a light-transmitting laminate having a transparent metal oxide film on a light-transmitting substrate can be produced by using a laminate having a metal thin film on a light-transmitting substrate and immersing the laminate in an electrolyte to completely anodize the metal thin film. Specifically, anodization is carried out by immersing an object to be oxidized, which is a translucent base material having a thin metal film formed thereon, in an electrolytic solution, and applying a voltage between an anode terminal connected to the thin metal film on the portion of the object to be oxidized that is exposed from the electrolytic solution, and a cathode plate provided in the electrolytic solution so as to face the thin metal film but not to come into contact with it.
[0004] In this case, however, the anodization reaction proceeds preferentially at the gas-liquid interface of the electrolyte, and the thin metal film at the gas-liquid interface is completely anodized and becomes non-conductive before other parts. As a result, the current from the anode terminal connected to the part of the thin metal film exposed from the electrolyte that is below the gas-liquid interface does not flow to the thin metal film. This causes a problem that the anodization reaction stops before the thin metal film is completely anodized.
[0005] In order to solve this problem, in Patent Document 1, an oxidized body made of a polypropylene film sputtered with aluminum is gradually immersed in an electrolyte solution while anodizing is performed. Patent Document 1 describes that the aluminum layer of the laminate obtained by this method is completely anodized and is translucent. However, in this method, the immersion speed of the oxidized body in the electrolyte solution is as slow as 2 mm / min, so that the treatment takes a long time, especially when the area of the metal layer of the oxidized body is large, and the productivity is poor. In addition, there is a risk that the residual rate of the metal layer will be uneven due to the influence of the liquid surface shaking at the gas-liquid interface of the electrolyte, and advanced technology is required to make the surface condition of the obtained laminate uniform.
[0006] In Patent Document 2, it is presumed that the oxidized body located at the gas-liquid interface is eliminated by immersing the entire oxidized body in the electrolyte. However, since the electrolyte often contains highly dangerous reagents such as strong acids, this method is undesirable from the standpoint of safety and durability of the equipment because there is a high possibility that the electrolyte will splash on workers and surrounding equipment. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2020 / 067500 [Patent Document 2] Japanese Patent Application Publication No. 2-245328 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a method for producing a light-transmitting laminate, which can uniformly and efficiently anodize almost the entire portion of a metal thin film immersed in an electrolyte solution in a relatively short time by simply carrying out a simple treatment on an object to be oxidized. [Means for solving the problem]
[0009] The above problem is solved by the following configuration.
[0010] [1] A method for producing a light-transmitting laminate having a metal oxide film on a light-transmitting substrate by immersing an oxidizable body consisting of a laminate having a thin metal film on a light-transmitting substrate in an electrolyte and anodizing the thin metal film, the method comprising: covering a specific portion of the thin metal film with a coating material; and immersing the oxidizable body in the electrolyte and anodizing the body so that the gas-liquid interface where the electrolyte comes into contact with the atmosphere is located at the specific portion.
[0011] [2] The method for producing a light-transmitting laminate according to [1], wherein the metal thin film is an aluminum thin film.
[0012] [3] The method for producing a light-transmitting laminate according to [1] or [2], wherein the specific portion is spaced apart from an upper end of the object to be oxidized immersed in the electrolyte and extends linearly in the direction of the gas-liquid interface.
[0013] [4] The method for producing a translucent laminate according to [1] or [2], wherein the specific portion includes a first specific portion spaced apart from an upper end of the object to be oxidized immersed in the electrolyte and extending linearly in a direction toward the gas-liquid interface, a second specific portion that is a left edge of the object to be oxidized, a third specific portion that is a right edge, and a fourth specific portion that is a lower edge, and the gas-liquid interface is located in the first specific portion.
[0014] [5] The method for producing a light-transmitting laminate according to any one of [1] to [4], wherein the covering material is an adhesive tape or a pressure-sensitive adhesive tape.
[0015] [6] The method for producing a light-transmitting laminate according to any one of [1] to [5], wherein the non-anodized portion is removed after the anodization. Effect of the Invention
[0016] According to the present invention, by simply carrying out a simple treatment on the object to be oxidized, it is possible to uniformly and efficiently anodize almost the entire part of the metal thin film immersed in the electrolyte in a relatively short time, and therefore it is possible to efficiently produce a light-transmitting laminate having uniform surface properties and excellent light transmittance. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic cross-sectional view showing an example of a light-transmitting laminate obtained by the present invention. [Diagram 2] FIG. 2 is a schematic front view showing an object to be oxidized coated with a coating material in step (1) according to one embodiment of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing an object to be oxidized immersed in an electrolytic solution according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the method for producing a light-transmitting laminate of the present invention will be described in detail with reference to the drawings. The following embodiments are merely examples for explaining the present invention, and are not intended to limit the present invention to these embodiments. The present invention can be implemented in various forms without departing from the spirit of the present invention.
[0019] The following definitions of terms apply throughout the specification and claims. The symbol "~" indicating a range of numerical values means that the numerical values before and after it are included as the lower limit and upper limit. The dimensional ratios in FIGS. 1 to 3 are different from the actual ones for the sake of convenience of explanation.
[0020] The method for producing a light-transmitting laminate of the present invention is a method for producing a light-transmitting laminate having a metal oxide film on a light-transmitting base by immersing an oxidizable body consisting of a laminate having a metal thin film on a light-transmitting base in an electrolytic solution and anodizing the metal thin film, characterized in that a specific portion of the metal thin film is covered with a coating material, and the body to be oxidized is immersed in the electrolytic solution and anodized so that a gas-liquid interface where the electrolytic solution comes into contact with the atmosphere is located at the specific portion.
[0021] [Transparent laminate] First, a light-transmitting laminate produced by the method for producing a light-transmitting laminate of the present invention (hereinafter, sometimes referred to as "light-transmitting laminate of the present invention") will be described. The light-transmitting laminate of the present invention has a metal oxide film on a light-transmitting substrate. FIG. 1 is a schematic cross-sectional view showing an example of the light-transmitting laminate of the present invention. This light-transmitting laminate 10 has a light-transmitting substrate 1, a metal layer 2 remaining slightly on the light-transmitting substrate 1, and a metal oxide film 3 formed on the surface thereof.
[0022] The light-transmitting substrate 1 is preferably in the form of a sheet, film or plate, but there is no particular limitation on its shape in plan view.
[0023] The material for the light-transmitting substrate 1 may be any material having a total light transmittance greater than 0%, and examples thereof include glass, polyacrylate, polymethacrylate, polyethylene terephthalate (PET), polyethylene, polypropylene, polycarbonate, polystyrene, and nylon. Among these, glass, polyacrylate, polymethacrylate, polyethylene, polypropylene, polycarbonate, polystyrene, and nylon are preferred because they have good light transmittance, glass, polyacrylate, polymethacrylate, polycarbonate, polystyrene, and nylon are more preferred, and glass, polyacrylate, polymethacrylate, and polycarbonate are most preferred.
[0024] There is no particular limitation on the thickness of the light-transmitting substrate 1, and it is appropriately determined depending on the application of the light-transmitting laminate 10. In the case of a light-transmitting substrate 1 made of a resin in general, the thickness is preferably about 10 μm to 3 cm, and in the case of a light-transmitting substrate 1 made of an inorganic material such as glass, the thickness is preferably about 20 μm to 3 cm.
[0025] The metal constituting the thin metal film of the oxidized body (the remaining metal layer 2 in FIG. 1) may be any metal that can form a metal oxide film 3 by anodization. Examples of metals include aluminum, niobium, tantalum, tungsten, titanium, zirconium, hafnium, alloys of two or more of these metals, and alloys of one or more of these metals with other metals. Among these metals, aluminum is preferred because it has excellent workability, is highly safe, and is inexpensive.
[0026] The method for forming the metal thin film on the light-transmitting substrate is not particularly limited, and examples thereof include vacuum deposition, sputtering, etc. When forming the metal thin film by these methods, the light-transmitting substrate may be subjected to a pretreatment in order to improve the adhesion between the metal thin film and the light-transmitting substrate.
[0027] The thickness of the metal thin film before anodization is preferably 30 to 500 nm, more preferably 50 to 300 nm. If the metal thin film is thinner than the lower limit, current cannot be passed through it, and if it is thicker than the upper limit, the anodization reaction does not proceed uniformly, and a uniform light-transmitting laminate may not be obtained.
[0028] It is also possible to use a commercially available metal-deposited film or the like as the material to be oxidized.
[0029] From the viewpoint of the light transmittance of the light-transmitting laminate, it is preferable that the thickness of the metal layer 2 remaining after anodization is thin, but from the viewpoint of its role as a current terminal for anodization, it is difficult to eliminate this metal layer 2 (to have a thickness of 0 nm). In the present invention, completely anodizing the metal thin film means reducing the thickness of this remaining metal layer 2 to 20 nm or less, particularly to 5 nm or less.
[0030] The transparency of the light-transmitting laminate of the present invention is greatly influenced by the transparency of the light-transmitting base material. However, according to the present invention, it is possible to efficiently carry out anodization and productively produce a desired light-transmitting laminate having a total light transmittance of more than 0% and not more than 95%, preferably in the range of 55 to 95%. Moreover, the haze of the light-transmitting laminate can be kept within +5% of the haze of the light-transmitting base material to be oxidized.
[0031] [Method of manufacturing light-transmitting laminate] The method for producing a light-transmitting laminate of the present invention is a method for covering a specific portion of a laminate having a metal thin film on a light-transmitting base material with a coating material, immersing an object to be oxidized in an electrolytic solution so that the gas-liquid interface of the electrolytic solution is located at the specific portion, and then performing anodization. Hereinafter, an embodiment of the method for producing a light-transmitting laminate of the present invention will be described with reference to FIGS.
[0032] The light-transmitting laminate of the present invention can be produced, for example, through the following steps (1) to (3). (1) A step of coating a specific portion of an object to be oxidized, which is a laminate having a metal thin film on a light-transmitting substrate, with a coating material. (2) a step of anodizing the body to be oxidized by immersing the body in an electrolytic solution so that the gas-liquid interface where the electrolytic solution and the atmosphere come into contact is located at the specific portion; (3) A step of removing the remaining metal thin film portion of the transparent laminate produced by anodization, i.e., the non-anodized processed portion. Each step will be described in detail below.
[0033] <Process (1)> This step is a step of coating a specific portion of an object to be oxidized, which is a laminate having a thin metal film on a light-transmitting substrate, with a coating material.
[0034] The covering material used to cover the specific portion may be any material that adheres to the metal thin film of the laminate, and may be a material that has the ability to adhere by itself, or may be a material that is pressed by pressure to adhere to the metal thin film of the laminate. The former may be an adhesive tape, a pressure sensitive adhesive tape, paint, etc., and the latter may be a packing or a suction cup, etc. Among these, adhesive tape or pressure sensitive adhesive tape is preferred from the viewpoint of ease of handling and adhesion. The material of the covering material is not particularly limited, but from the viewpoint of adhesion and acid resistance to the electrolyte, for example, adhesive tape or pressure sensitive adhesive tape is preferably made of an insulating material such as polyester, polypropylene, cellophane, etc.
[0035] The specific portion to be covered is the surface of the thin metal film located at the gas-liquid interface of the electrolyte when the body to be oxidized is immersed in the electrolyte to perform anodic oxidation.
[0036] For example, as shown in Fig. 3, when a light-transmitting substrate 1 on which a metal thin film 3A, which is an object to be oxidized 7, is formed is immersed in the electrolytic solution 4 in an electrolytic cell 6 storing the electrolytic solution 4 to perform anodization, the object to be oxidized 7 is set upright by immersing an upper edge 7A of the object to be oxidized 7 in the electrolytic solution 4 while the lower part is exposed from the upper edge 7A in the electrolytic solution 4, and an anode terminal 8 is connected to the exposed metal thin film 3A. A DC voltage is applied from a power source 20 between a cathode plate 9, which is set upright in the electrolytic solution 4 with a gap therebetween and facing the metal thin film 3A of the object to be oxidized 7, and the anode terminal 8 to perform anodization. In the present invention, the location where the gas-liquid interface 4A of the electrolytic solution 4 is located in this state is designated as the specific portion, and is covered with the covering material 5.
[0037] Therefore, in this case, the specific portion covered with the covering material 5 is a portion spaced from the upper end of the body to be oxidized 7 immersed in the electrolyte 4 and extending linearly in the direction of the gas-liquid interface (horizontal direction). For example, in the case of a rectangular shaped object to be oxidized 7, as shown in FIG. 2(a), it is preferable to provide a coating material 5A in a line parallel to the upper end of the object to be oxidized 7, slightly below the upper edge, ensuring a portion necessary for connecting an anode terminal (there is no particular restriction on the width). In this case, the width of the coating material 5A is preferably large enough to ensure that the gas-liquid interface 4A is located at the position of the coating material 5A even if the liquid level of the gas-liquid interface 4A of the electrolyte fluctuates. On the other hand, since the portion covered with the coating material 5A is not anodized, it is preferable that the width of the coating material 5A is small from the viewpoint of making the area of the metal oxide film as large as possible. From these viewpoints, the width of the coating material 5A is preferably about 10 to 20 mm, and the gas-liquid interface 4A is preferably located on the center line of the coating material 5A.
[0038] The specific portion to be covered with the covering material is not limited to the linear shape as shown in FIG. 2(a). As shown in FIG. 2(b), the metal thin film 3A may be covered with a frame-shaped covering material 5B including a first specific portion 5a spaced from the upper end of the oxidized body 7 immersed in the electrolyte and extending linearly toward the gas-liquid interface 4A, a second specific portion 5b which is the left edge of the oxidized body 7, a third specific portion 5c which is the right edge, and a fourth specific portion 5d which is the lower edge. In other words, when anodizing is performed by immersing the body to be oxidized in an electrolyte, generally the further away from the anode terminal in the body to be oxidized, the worse the conductive path becomes, making it difficult for the anodizing reaction to proceed, and in many cases a uniform metal oxide film is not formed in this area. Therefore, by covering such areas with coating material 5 and ensuring conductivity to the bottom edge, a uniform metal oxide film can be formed only on the exposed surface of the uncoated metal thin film 3A. In this case, the object to be oxidized 7 is immersed in the electrolyte so that the gas-liquid interface 4A is located at the covering material 5a provided on the upper end side of the object to be oxidized 7. Regarding the width of covering material 5B in this case, it is preferable that covering material 5a portion has the same width as covering material 5A shown in FIG. 2(a), but covering materials 5b to 5d portions may be smaller, about 1 to 5 mm.
[0039] 2 shows a method of coating a coating material for an oxidizable object having a rectangular shape in a plan view, but in the case of an oxidizable object having a shape other than a rectangle, for example a circle, a coating material may be provided so as to extend linearly at a position separated from the upper end with the metal thin film surface standing upright in the vertical direction, and the peripheral portion below the linear coating material may be further coated with a coating material in an arc shape.
[0040] <Process (2)> In this process, the laminate provided with the coating material, which is the object to be oxidized, is immersed in an electrolyte so that the gas-liquid interface of the electrolyte is located at the specific portion coated with the coating material, and is anodized. This process is carried out, for example, by the method shown in FIG.
[0041] The method of immersing and fixing the laminate, which is the body to be oxidized, in the electrolyte is not particularly limited as long as the gas-liquid interface of the electrolyte can be maintained at the specific portion covered with the coating material during the anodization reaction.
[0042] The type of electrolyte used for anodization is not particularly limited, and examples thereof include an aqueous solution of sulfuric acid, oxalic acid, phosphoric acid, etc. The acid concentration of the electrolyte is not particularly limited as long as the condition allows the anodization reaction to proceed stably. When an aqueous sulfuric acid solution is used as the electrolyte, the sulfuric acid concentration of the aqueous sulfuric acid solution is usually 0.3M (mol / L) or more, preferably 3M or more, and more preferably 5M or more. By using an aqueous sulfuric acid solution with a sulfuric acid concentration of 5M or more, efficient anodization can be performed. On the other hand, the sulfuric acid concentration is usually 15M or less, and preferably 12M or less. By using an aqueous sulfuric acid solution with a sulfuric acid concentration of 12M or less, a current can be stably passed through the thin metal film during anodization, and a more homogeneous metal oxide film can be formed.
[0043] The temperature of the electrolyte during anodization is preferably 30° C. or lower, more preferably 20° C. or lower, for example, 0 to 17° C., from the viewpoint of reaction stability.
[0044] The anodization reaction is carried out under a certain voltage condition. The voltage at this time is not particularly limited, but for example, when an aqueous sulfuric acid solution is used as the electrolyte, a voltage of 25 to 30 V is preferable because it allows the formation of a homogeneous metal oxide film.
[0045] The current during anodization varies depending on the type and temperature of the electrolyte and the progress of the reaction, but the maximum value is determined by the settings of the DC power supply. This maximum value is preferably in the range of 0.1 to 3.5 A. The thinner the metal thin film formed on the translucent base material is, the smaller the current value is set, and the thicker the metal thin film is, the larger the current value is set, so that a homogeneous metal oxide film can be formed and a high-quality translucent laminate can be obtained.
[0046] <Process (3)> This step is a step of cutting off the non-anodized portion of the manufactured light-transmitting laminate. In the part of the translucent laminate obtained by anodizing the laminate, which is the oxidizable body, that is, the part not immersed in the electrolyte (part exposed from the electrolyte) and the part that was covered with the coating material, a thin metal film that is not anodized remains. Therefore, in the final form of the product, it may be necessary to cut out the part together with the translucent base material. The method for the cutting is not particularly limited, and the cutting can be performed using scissors, a cutter, a band saw, or the like.
[0047] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and various modifications can be made without departing from the gist of the present invention. EXAMPLES
[0048] [Example 1] <Process (1)> A PET film on which aluminum had been previously vapor-deposited (thickness: PET film alone = 75 μm, aluminum layer = 80 nm) was cut into a length of 8 cm length and 5 cm width. The total light transmittance and haze of this aluminum-deposited film, measured before vapor deposition using the method described below, were 82.61% and 58.94%, respectively. When this aluminum vapor deposition film was placed upright with its lengthwise direction facing up and down, approximately 2 cm from the top end was covered with a 1 cm wide masking tape for plating (3M, product number "851A", a polyester tape with an adhesive layer) so that it was parallel to the top edge (Figure 2(a)).
[0049] <Process (2)> Anodization was carried out according to the method shown in FIG. An aluminum plate connected to the negative pole of a DC power supply as a negative electrode was immersed in a 12 M aqueous sulfuric acid solution cooled to 0°C. The aluminum vapor deposition film was connected to the anode of a DC power supply, and was immersed facing the cathode plate so that the center line of the portion covered with the masking tape was at the gas-liquid interface of the electrolyte. Thereafter, a voltage of 25 V and a current of 3.0 A were applied until the current stopped flowing, thereby anodizing the aluminum layer on the aluminum vapor deposition film. The light-transmitting laminate produced by anodization was taken out of the electrolyte and washed with ion-exchanged water. The time required from the start of the anodization to the end of the reaction was 2 minutes and 55 seconds.
[0050] <Process (3)> The masking tape-covered portion of the light-transmitting laminate and the portion above it were cut with scissors.
[0051] <Translucency measurement> As indicators of light transmittance, total light transmittance and haze were measured using NDH4000 manufactured by Nippon Denshoku Industries Co., Ltd., which complies with JIS K7361 and JIS K7136. As a result, the light-transmitting laminate produced in this Example 1 had a total light transmittance of 58.72% and a haze of 58.87%.
[0052] [Example 2] An aluminum-vapor-deposited polypropylene film (thickness: polypropylene alone = 20 μm, aluminum layer = 50 nm) was used as a laminate having a metal thin film on a light-transmitting substrate, and the same operation as in Example 1 was carried out except that the current during anodization was 1.0 A. The time required from the start of anodization to the end of the reaction was 1 minute, and the total light transmittance of the produced light-transmitting laminate was 64.28%, and the haze was 3.24%.
[0053] [Example 3] <Process (1)> An aluminum layer of 200 nm was formed by vacuum deposition on the surface of an acrylic plate (Acrylite L manufactured by Mitsubishi Chemical Corporation) with a thickness of 1.0 mm, length of 8 cm and width of 5 cm, to obtain an aluminum-laminated acrylic plate. The total light transmittance of this acrylic plate alone measured by the above-mentioned method was 93.0%, and the haze was 0.5%. When this aluminum-laminated acrylic plate was stood upright with its longitudinal direction aligned vertically, a section of approximately 2 cm from the top end was covered with the same kind of plating masking tape (manufactured by 3M) used in Example 1 so as to be parallel to the top edge, and then the bottom end and the left and right ends of the aluminum-laminated acrylic plate were similarly covered with masking tape so as to surround the lower surface (Figure 2(b)).
[0054] <Process (2)> Anodization was carried out according to the method shown in FIG. An aluminum plate connected to the negative pole of a DC power supply as a negative electrode was immersed in a 12 M aqueous sulfuric acid solution cooled to 0°C. The aluminum-laminated acrylic plate was connected to the anode of a DC power supply, and was immersed facing the cathode plate so that the center line of the masking tape on the upper covering portion was at the gas-liquid interface of the electrolyte. Thereafter, the aluminum layer on the aluminum-laminated acrylic plate was anodized by passing a current of 3.0 A at a voltage of 25 V until the current stopped flowing. The light-transmitting laminate produced by anodization was taken out of the electrolytic solution and washed with ion-exchanged water. The time required from the start of anodization to the end of the reaction was 3 minutes and 10 seconds.
[0055] <Process (3)> The masking tape-covered portion of the light-transmitting laminate and the portion above the upper masking tape-covered portion were cut off with a band saw.
[0056] <Translucency measurement> The translucency was measured in the same manner as in Example 1. The light-transmitting laminate produced in this Example 3 had a total light transmittance of 88.86% and a haze of 0.38%.
[0057] [Comparative Example 1] The same operation as in Example 1 was carried out except that no masking tape was used in step (1). As a result, the anodization reaction proceeded preferentially at the gas-liquid interface of the electrolyte, resulting in the complete anodization of the aluminum layer. As a result, the anodization reaction hardly proceeded in the area below that, and a translucent laminate could not be obtained.
[0058] [Comparative Example 2] <Process (1)> An oxidizable object was prepared in the same manner as in Example 1, except that the aluminum-deposited PET film was not covered with masking tape.
[0059] <Process (2)> An aluminum plate connected to the negative pole of a DC power supply as a negative electrode was immersed in a 12 M aqueous sulfuric acid solution cooled to 0°C. The aluminum vapor deposition film was attached to a dip coater (Dip Coater YN2-TKB manufactured by Sakigake Semiconductor Co., Ltd.) with the longitudinal direction facing up and down, the upper end was connected to the anode of a DC power supply, and the lower edge was brought into contact with the electrolyte so that it was immersed about 5 mm deep. Thereafter, the aluminum layer on the aluminum vapor-deposited film was anodized by passing a current of 3.0 A at a voltage of 25 V for 30 minutes while the aluminum vapor-deposited film was lowered at a speed of 2 mm per minute. The aluminum vapor-deposited film was anodized in the area between 5 mm and (2 mm / min x 30 min) mm from the bottom end. The obtained light-transmitting laminate was taken out of the electrolytic solution and washed with ion-exchanged water.
[0060] <Process (3)> The non-anodized portion of the transparent laminate was cut with scissors to a length of 5 mm from the lower end and a length of 15 mm from the upper end.
[0061] <Translucency measurement> The translucency was measured in the same manner as in Example 1. The light-transmitting laminate produced in this Comparative Example 2 had a total light transmittance of 58.20% and a haze of 59.86%.
[0062] The results of Examples 1 to 3 and Comparative Examples 1 and 2 are summarized in Table 1.
[0063] [Table 1]
[0064] From the above results, it is evident that according to the present invention, a light-transmitting laminate can be produced efficiently in a short time simply by covering a predetermined portion of an object to be oxidized with a covering material. In Comparative Example 1, in which no coating was applied, it was not possible to continue anodization. In Comparative Example 2, a light-transmitting laminate could be obtained, but the object to be oxidized was lowered at a slow speed, requiring a long treatment time. [Explanation of symbols]
[0065] 1 Translucent base material 2 metal layers 3. Metal oxide film 3A Metal thin film 4 Electrolyte 4A Gas-liquid interface 5,5A,5B Covering material 6 Electrolytic cell 7 Oxidized substance 8 Anode terminal 9 Cathode Plate 10 Translucent laminate 20 Power supply
Claims
1. A method for producing a light-transmitting laminate having a metal oxide film on a light-transmitting substrate, comprising the steps of: immersing an oxidizable body, which is a laminate having a metal thin film on a light-transmitting substrate, in an electrolytic solution; and anodizing the metal thin film, comprising the steps of: a method for anodizing the object to be oxidized by covering a specific portion of the metal thin film with a coating material and immersing the object to be oxidized in the electrolytic solution so that a gas-liquid interface where the electrolytic solution contacts the atmosphere is located at the specific portion, the specific portion includes a first specific portion spaced apart from an upper end of the object to be oxidized immersed in the electrolytic solution and extending linearly in a direction toward the gas-liquid interface, a second specific portion being a left edge portion of the object to be oxidized, a third specific portion being a right edge portion, and a fourth specific portion being a lower edge portion, and the gas-liquid interface is located in the first specific portion.
2. 2. The method for producing a light-transmitting laminate according to claim 1, wherein the metal thin film is an aluminum thin film.
3. 3. The method for producing a light-transmitting laminate according to claim 1, wherein the covering material is an adhesive tape or a pressure-sensitive adhesive tape.
4. 4. The method for producing a light-transmitting laminate according to claim 1, further comprising the step of cutting off a non-anodized portion after the anodization.
Citation Information
Patent Citations
Complex structure
JP1990245328A
Selective chemical treatment
JP1995331459A
Insulator thin film and its production
JP1999172490A
Surface treatment method
JP2009102721A
Antimicrobial material, layered body, antimicrobial layered body, medical member, antimicrobial material production method, antimicrobial layered body production method, and antimicrobial method
WO2020067500A1