Manufacturing method of obliquely stretched film

By controlling take-up tensions and trimming processes, the method addresses breakage and unevenness issues in thin films, ensuring high-quality and stable production of diagonally stretched films for optical devices.

JP7578002B2Active Publication Date: 2024-11-06KONICA MINOLTA INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021002666
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-12
Publication Date
2024-11-06
Estimated Expiration
2041-01-12

AI Technical Summary

Technical Problem

Thin films used in optical devices face issues during trimming processes due to low mechanical strength, leading to breakage, distorted cut surfaces, and display unevenness, affecting productivity and quality.

Method used

A method for producing diagonally stretched films involves controlling the take-up tensions at the leading and non-trimmed areas of the film during trimming, ensuring the ratios of these tensions satisfy specific formulas, and trimming both ends simultaneously or within a specified time frame to prevent breakage and maintain surface quality.

Benefits of technology

The method prevents film breakage during and after trimming, enhances cut surface quality, improves productivity, and reduces display unevenness, resulting in stable film production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578002000004
    Figure 0007578002000004
  • Figure 0007578002000005
    Figure 0007578002000005
  • Figure 0007578002000006
    Figure 0007578002000006
Patent Text Reader

Abstract

To provide a manufacturing method that does not break during and after a trimming process, has excellent quality of a cut surface of a film, can be produced stably with high productivity, and can suppress an occurrence of display irregularity.SOLUTION: A manufacturing method for an oriented film includes: a diagonal stretching process in which both ends of the film in a widthwise direction are gripped by a pair of grips and the film is conveyed with one grip relatively leading and the other relatively lagging, stretching the film in a direction oblique to the widthwise direction; a trimming process to trim an edge of diagonally oriented film that has been stretched by the stretching process; and a film take-up process to take up a trimmed leading edge, a trimmed delayed edge, and a non-trimmed area on the delayed side. If a take-up tension of the leading edge is TIN, a take-up tension of the untrimmed area is TC, a film edge width of the leading edge is widthIN, and a film width of the untrimmed area is widthC, equation (1) is satisfied. Equation (1):[TC / widthC]<[TIN / widthIN]SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an obliquely stretched film, and more particularly to a method for producing an obliquely stretched film which does not break during and after a trimming process, has excellent quality of the cut surface of the film, can be produced stably with high productivity, and can suppress the occurrence of display unevenness. [Background technology]

[0002] As an optical film required for the application of organic electroluminescence display devices and polarized sunglasses, there is a demand for the development of a film in which the in-plane slow axis of the film is inclined at a desired angle with respect to the transmission axis of the polarizer layer. In addition, with the recent evolution of devices such as lighter weight and flexibility, there is an increasing need for thinner optical films. Here, oblique stretching is known as a method for producing a film with an in-plane slow axis tilted at a desired angle. After oblique stretching, the film undergoes a trimming process (also called a "slitting process," "cutting process," or "trimming process") in which unnecessary parts that were gripped with clips during stretching are cut off, and the film is wound up as an optical film and commercialized. Here, the difficulty of trimming the thin film of the obliquely stretched film became evident. This is because a thin film has low mechanical strength, so it is prone to trouble due to disturbances caused by the state of the slit blade and the state of transport, and there was a problem with continuous productivity. In addition, there was a problem of process contamination caused by cutting residue being carried into the next process due to a defective edge of the film, and display unevenness occurred when the thin film was incorporated into a display device, possibly due to uneven stress when the film was cut.

[0003] On the other hand, for example, Patent Document 1 proposes a means for clamping both sides of the film, but if the film tension of a very thin film is weak, the film will not be able to withstand the pressing pressure of the slit blade, and a tearing load will be applied to the film, causing it to break, or even if it does not break, the cut surface will be distorted. If the film is wound up with a distorted cut surface and then unwound in the next process, stress will concentrate due to the distorted area, causing breakage during unwinding, or the distorted area will deform and fold during transport, causing breakage. Also, a technique has been disclosed in which the trimming width (cutting width) is different on the inner peripheral side and the outer peripheral side of the obliquely stretched film in the trimming step (see, for example, Patent Documents 2 and 3), but no description is made about the take-up tension of the film after trimming. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-3368 A [Patent Document 2] International Publication No. 2013 / 118187 [Patent Document 3] International Publication No. 2013 / 125195 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a method for producing an obliquely stretched film which does not break during and after the trimming process, has excellent quality of the cut surface of the film, can be produced stably with high productivity, and can suppress the occurrence of display unevenness. [Means for solving the problem]

[0006] In the course of investigating the causes of the above problems in order to solve the above problems, the inventors discovered that by adjusting the take-up tension in the width direction of the film, i.e., the take-up tension of the leading end and the non-trimming region, to be within a specific range when trimming the end of an obliquely stretched film, it is possible to prevent the film from breaking during and after the trimming process, to have excellent quality cut surfaces, to improve productivity, and to suppress the occurrence of display unevenness, which led to the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.

[0007] 1. An oblique stretching process in which both ends of a film in the width direction are held by a pair of grippers, one of the grippers is moved ahead relatively and the other gripper is moved behind relatively to transport the film, thereby stretching the film in a direction oblique to the width direction; a trimming step of trimming the end portion of the obliquely stretched film obtained by the stretching step; and a film taking-up step of taking up a leading-side end portion which is an end portion of the obliquely stretched film that has been trimmed on the leading side, a delayed-side end portion which is an end portion of the obliquely stretched film that has been trimmed on the delayed side, and a non-trimmed region of the obliquely stretched film, The tension applied to the leading end is T IN , and the take-off tension of the non-trimming area is T C The film end width of the leading end is set to width IN , and the film width of the non-trimming area is C In this case, the following formula (1) is satisfied. death, The tension at the delayed end is T OUT The film end width of the retardation side end is OUT Then, the following formula (2) is satisfied. The method for producing an obliquely stretched film is characterized by the above. Equation (1):[T C / width C ]<[T IN / width IN ] Formula (2): 0.8<[T C / widthC ] / [T OUT / width OUT ]<[T IN / width IN ] / [T C / width C ]<4.0

[0009] 2 In the trimming step, the difference in distance between the trimming start position of the leading side end of the obliquely stretched film and the trimming start position of the lagging side end is within a range of ±200 mm. In the section A method for producing the obliquely stretched film described above.

[0010] 3 In the trimming step, the leading end and the lagging end of the obliquely stretched film are trimmed simultaneously or within ±3 seconds. Paragraph 1 or 2 A method for producing the obliquely stretched film according to claim 1.

[0011] 4 In the trimming step, the widths of the leading end, the lagging end and the non-trimming area to be trimmed satisfy the following formula (3) or (4). 3 Item 10. The method for producing an obliquely stretched film according to any one of items 1 to 9. Formula (3): 15%<(width IN / width C )×100(%)<40% Formula (4): 15%<(width OUT / width C )×100(%)<40%

[0012] 5 In the trimming step, when a contact width between the obliquely stretched film and a support supporting the obliquely stretched film is defined as a contact width A, the following formula (5) is satisfied. 4 Item 10. The method for producing an obliquely stretched film according to any one of items 1 to 9. Formula (5): 0% IN +Width C +Width OUT )×100(%)<10%

[0013] 6 The thickness of the obliquely stretched film is 25 μm or less. 5 Item 10. The method for producing an obliquely stretched film according to any one of items 1 to 9.

[0014] 7 The obliquely stretched film has an NZ coefficient of less than 1.3. 6 Item 10. The method for producing an obliquely stretched film according to any one of items 1 to 9. Effect of the Invention

[0015] According to the above-mentioned means of the present invention, it is possible to provide a method for producing an obliquely stretched film which does not break during and after the trimming process, has excellent quality of the cut surface of the film, can be produced stably with high productivity, and can suppress the occurrence of display unevenness. Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. This was not a big problem with conventional film thicknesses, but by making the film thinner, the film strength decreases, and when the film is taken up with a take-up tension T1 at the leading end IN, non-trim region C, and lagging end OUT after trimming, the film is more likely to break in the non-trim region C starting from the leading end IN during and after the trimming process. This is presumably because the tension T2 immediately after trimming acts in a direction different from the orientation direction H of the film (approximately perpendicular to the orientation direction H) at the leading end IN of the film, making the film more likely to tear (see, for example, FIG. 1(a)). At the lagging side end OUT of the film, the tension T3 immediately after trimming acts in the same direction as the orientation direction H of the film (a direction substantially parallel to the orientation direction H), preventing the film from breaking. ​Therefore, in the present invention, in the trimming process, the take-up tensions of the leading end portion IN and the non-trimming region of the obliquely stretched film are controlled to satisfy the above formula (1). That is, the take-up tension T IN The take-off tension T in the non-trimming area C c It is presumed that by trimming the film so that it is higher than the leading end IN, it is possible to prevent breakage in the non-trimmed region C starting from the leading end IN of the film, resulting in excellent quality of the cut surface of the film and improved productivity (see, for example, Figure 1(b)). [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a schematic diagram for explaining the take-up tension of the leading end, non-trimming region, and lagging end of the film, and the orientation direction of the film in the present invention. [Diagram 2] Schematic top view of an oblique stretching device [Diagram 3] Schematic side view of an oblique stretching device [Figure 4] Schematic diagram showing an example of a rail pattern of an oblique stretching tenter [Diagram 5] Schematic diagram of trimming device [Figure 6] Schematic diagram of trimming device [Figure 7] Schematic diagram of trimming device [Figure 8] FIG. 2 is an exploded perspective view showing a schematic configuration of a polarizing plate. [Figure 9] 1 is an exploded cross-sectional view showing a schematic configuration of an organic EL display device. [Figure 10] FIG. 1 is a cross-sectional view showing a schematic configuration of a liquid crystal display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The method for producing an obliquely stretched film of the present invention includes an oblique stretching step in which both ends of a film in the width direction are held by a pair of grippers, one of the grippers being advanced relatively and the other gripper being delayed relatively, to transport the film and thereby stretch the film in a direction oblique to the width direction, a trimming step in which an end of the obliquely stretched film stretched by the stretching step is trimmed, and a film taking-up step in which a leading-side end which is an end of the obliquely stretched film trimmed on the leading side, a delayed-side end which is an end of the obliquely stretched film trimmed on the delayed side, and a non-trimmed region of the obliquely stretched film are taken up, and the taking-up tension of the leading-side end is set to T IN , and the take-off tension of the non-trimming area is T C The film end width of the leading end is set to width IN , and the film width of the non-trimming area is C In this case, the following formula (1) is satisfied. Equation (1):[T C / width C ]<[T IN / width IN ] This feature is a technical feature common to or corresponding to each of the following embodiments.

[0018] In one embodiment of the present invention, the take-up tension of the delayed side end is T OUT The film end width of the retardation side end is OUT In this case, it is preferable to satisfy the above formula (2) in that non-uniform stress can be prevented when the film is cut.

[0019] In the trimming step, it is preferable that the distance difference between the trimming start position of the leading end and the trimming start position of the lagging end of the obliquely stretched film is within a range of ±200 mm. By setting the distance difference between the trimming start positions of the leading end and the lagging end within a range of ±200 mm, the facility space can be reduced. In addition, the conveyability of the film whose end is held by the clip is in a state where the restricting force of the end is high (the film is thick because the corresponding portion is not stretched), so when trimming is performed in two stages, after the first stage is trimmed, the film tends to move obliquely in the opposite direction to the trimmed side. Therefore, a problem occurs in that the conveying stability of the cut portion trimmed in the second stage becomes unstable, but the above problem does not occur by setting the distance difference between the trimming start positions of the leading end and the lagging end within a range of ±200 mm as described above. In particular, setting the distance difference of the trimming start positions within the above range is effective for thin films. In addition, in the trimming step, it is preferable to trim the leading side end portion and the lagging side end portion of the obliquely stretched film simultaneously or within ±3 seconds, since this makes it possible to keep the distance difference within the range of ±200 mm.

[0020] In the trimming step, when the widths of the leading end, the lagging end, and the non-trimming region to be trimmed satisfy the formula (3) or the formula (4), the stability of the film ends immediately after trimming is excellent, and the production stability of the obliquely stretched film is also improved.

[0021] In the trimming step, when the contact width between the obliquely stretched film and the support supporting the obliquely stretched film is defined as contact width A, it is preferable that the formula (5) is satisfied. In the trimming step, when tension is applied to the obliquely stretched film, if there is a lot of contact between the film and the support supporting the film, the support applies a restricting force, making it difficult to transmit the tension satisfying the formula (1) to the trimmed portion of the obliquely stretched film. Therefore, by making the film and the support satisfy the formula (5) in the trimming step, i.e., by reducing the contact between the film and the support, the tension can be stably transmitted to the trimmed portion.

[0022] Moreover, it is preferable that the thickness of the obliquely stretched film is 25 μm or less in order to accommodate lighter and more flexible devices. Furthermore, it is preferable for the obliquely stretched film to have an NZ coefficient of less than 1.3 in terms of improving the viewing angle.

[0023] The present invention, its components, and embodiments for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as lower and upper limits.

[0024] [Outline of the manufacturing method for obliquely stretched film] The method for producing an obliquely stretched film of the present invention includes an oblique stretching step in which both ends of a film in the width direction are held by a pair of grippers, one of the grippers being advanced relatively and the other gripper being delayed relatively, to transport the film and thereby stretch the film in a direction oblique to the width direction, a trimming step in which an end of the obliquely stretched film stretched by the stretching step is trimmed, and a film taking-up step in which a leading-side end which is an end of the obliquely stretched film trimmed on the leading side, a delayed-side end which is an end of the obliquely stretched film trimmed on the delayed side, and a non-trimmed region of the obliquely stretched film are taken up, and the taking-up tension of the leading-side end is set to T IN , and the take-off tension of the non-trimming area is T CThe film end width of the leading end is set to width IN , and the film width of the non-trimming area is C In this case, the following formula (1) is satisfied. Equation (1):[T C / width C ]<[T IN / width IN ]

[0025] In addition, in the method for producing an obliquely stretched film of the present invention, the take-up tension of the delayed side end portion is T OUT The film end width of the retardation side end is OUT When the thickness is 10 mm or less, it is preferable to satisfy the following formula (2) in order to prevent non-uniform stress when the film is cut. Formula (2): 0.8<[T C / width C ] / [T OUT / width OUT ]<[T IN / width IN ] / [T C / width C ]<4.0 More preferably, the relationship of the following formula (2-1) is satisfied. Formula (2-1): 1.0<[T C / width C ] / [T OUT / width OUT ]<[T IN / width IN ] / [T C / width C ]<3.0

[0026] The "leading end IN" refers to one of the two widthwise ends of the film that has a shorter travel distance for a gripping tool (described later), i.e., the inner portion of the film. The "delayed end OUT" refers to one of the two widthwise ends of the film that has a longer travel distance of a gripping tool, which will be described later, i.e., the outer portion of the film. The "non-trimming area C" refers to the area of ​​the film excluding the leading end IN and the lagging end OUT that is not to be trimmed.

[0027] Here, Fig. 4 is a schematic diagram showing the rail pattern of the oblique stretching tenter, in which the left and right grippers Ci and Co run on asymmetric rails Ri and Ro that connect the inlet of the oblique stretching tenter (position A in Fig. 4) to the position at the end of stretching (position B in Fig. 4). Since the rail pattern in Fig. 4 is for the case where the rail has been turned to the right, the inner circumference side is the rail Ri side, and the outer circumference side is the rail Ro side. Moreover, when the rail pattern is turned to the left, the Ri and Ro are reversed.

[0028] In addition, the above-mentioned "pulling tension at the leading end (T IN ) refers to the tension when the trimmed leading end portion is taken up in the film taking-up step after the trimming step. The above-mentioned "Removal tension of the non-trimming area (T C ) refers to the tension when the non-trimming region is taken up in the film taking-up step after the trimming step. Furthermore, the above-mentioned "pulling tension at the delayed end (T OUT )" refers to the tension when the delayed side end is taken up in the film taking-up process after the trimming process.

[0029] Each of the above take-up tensions (T IN , T C , T OUT An example of a method for measuring the tension is a method of measuring the load applied to the roll. Specifically, a load cell is attached to the bearing part of the roll and the load applied to the roll, i.e., the tension of the film, is measured. The load cell may be a known tension or compression type. In addition, various known measurement methods may be applied.

[0030] The above "film end width at the leading end (width IN "(a)" refers to the film width of the trimmed leading edge in the trimming step, i.e., the distance from the extreme end in the width direction of the trimmed leading edge to the trimmed position. The "width direction" refers to the direction of the short side of the film to be trimmed, that is, the direction from one lateral end to the other of the film. The above-mentioned "film end width at the delay side end (width OUT "(a)" refers to the film width of the trimmed delayed side end in the trimming step, i.e., the distance from the extreme end of the trimmed delayed side end in the width direction to the cut position. The above "film width of the non-trimmed area (width C "(a)" refers to the film width of the trimmed non-trimming region in the trimming step, i.e., the distance between the two ends in the width direction of the trimmed non-trimming region.

[0031] In the trimming step of the present invention, the widths of the leading end, the lagging end and the non-trimming region to be trimmed (width IN ,width C ,width OUT ) satisfies the following formula (3) or formula (4), in that the stability of the film edge immediately after trimming is excellent and the production stability of the obliquely stretched film is also improved. Formula (3): 15%<(width IN / width C )×100(%)<40% Formula (4): 15%<(width OUT / width C )×100(%)<40%

[0032] [Diagonal stretching device] 2 and 3 are schematic diagrams showing oblique stretching apparatuses used in the respective steps of a method for producing an obliquely stretched film according to one embodiment of the present invention, although this is merely an example and the present invention is not limited thereto.

[0033] 2 and 3, the symbols represent the following members, devices, etc.: 1: oblique stretching device, 2: oblique stretching tenter, 3: film unwinding device, 4a: film take-up device at leading end, 4b: film take-up device in non-trimming region, 4c: film take-up device at lagging end, 5 and 8: transport rollers, 6: inner guide rail, 7: outer guide rail, 9a: leading slit, 9b: lagging slit, 11 and 12: guide rail start position, 13 and 14: guide rail end position, 15: long film (original film) or obliquely stretched film.

[0034] <Film forming process> The method for producing an obliquely stretched film of the present invention preferably includes a step of forming a long film containing a resin (hereinafter also referred to as "raw film") prior to the oblique stretching step. The film-forming process can be carried out by various means depending on the type of resin, etc., and will be described in detail later. In the present invention, "long length" refers to a length that is at least about 5 times the width of the film, and preferably 10 times or more, specifically a length that allows the film to be wound into a roll for storage or transportation (film roll).

[0035] <Diagonal stretching process> The oblique stretching step in the production method of the present invention is a step of obliquely stretching an original film by unwinding the original film from a film unwinding device in a specific direction different from the take-up direction of the stretched film, and conveying the original film while holding both ends in the width direction with the grippers of an oblique stretching tenter, thereby imparting an in-plane slow axis at an arbitrary angle greater than 0° and less than 90° with respect to the width direction of the film. Here, the angle with respect to the width direction of the film is an angle within the film plane. Since the slow axis is usually expressed in the stretching direction or in a direction perpendicular to the stretching direction, in the production method according to the present invention, an obliquely stretched film having such a slow axis can be produced by stretching the film at a desired angle that is greater than 0° and less than 90° with respect to the direction perpendicular to the film transport direction.

[0036] (Feeding device) As shown in Figures 2 and 3, the film unwinding device 3 is preferably slidable and rotatable so that the film can be unwound at a predetermined angle relative to the entrance of the oblique stretching tenter. The film unwinding device 3 is preferably slidable and can be unwound to the entrance of the oblique stretching tenter by a conveying direction changing device. By configuring the film unwinding device 3 and the conveying direction changing device in this way, it becomes possible to precisely control the film unwinding position and angle, and it becomes possible to obtain an obliquely stretched film with small variations in film thickness and optical values. In addition, by making the film unwinding device 3 and the conveying direction changing device movable, it is possible to effectively prevent the gripper from biting into the film. The unwound film may be continuously connected to the film-forming process described above, but it is preferable to unwound the film in a roll shape in the film-forming process. By separating the film-forming process from the oblique process, the device can be made compact. When unwound rolls are unwound, high productivity can be ensured by continuously connecting the old film and the new film. The film can be connected by known means, such as a joining tape, heat welding, ultrasonic welding, and laser welding, but joining by heat welding is preferable.

[0037] (Transport roller) The transport rollers 5 are rollers that transport the film fed from the feeding device 3 to the guide rail start positions 11 and 12 . The number of the transport rollers 5 is not particularly limited. A static eliminator for eliminating static electricity from the film may be provided before or after the transport rollers or between multiple transport rollers. The static eliminator may be the same as the static eliminator used in the trimming process described below.

[0038] (Diagonal stretching tenter) In the manufacturing method according to the present embodiment, an oblique stretching tenter is used to impart an oblique orientation to the raw film. The oblique stretching tenter used in the present embodiment is preferably a film stretching device capable of freely setting the orientation angle of the film by changing the rail pattern in various ways. Furthermore, it is preferable that the film stretching device is capable of highly precisely orienting the orientation axis of the film evenly to the left and right across the film width direction, and capable of controlling the film thickness and retardation with high precision.

[0039] 4 is a schematic diagram showing an example of a rail pattern of an oblique stretching tenter used in the method for producing an obliquely stretched film according to an embodiment of the present invention, although this is merely an example and the present invention is not limited thereto. The payout direction D1 of the original film is different from the winding direction D2 of the obliquely stretched film after stretching, and forms a payout angle θi. The payout angle θi can be set to any desired angle in the range of more than 0° and less than 90°. The raw film is held at both ends by left and right grippers at the entrance of the oblique stretching tenter (position A in Fig. 4), and travels with the movement of the grippers. The left and right grippers Ci and Co face each other in a direction approximately perpendicular to the film traveling direction (feed-out direction D1) at the entrance of the oblique stretching tenter (position A in Fig. 4), travel on asymmetric rails Ri and Ro, and release the gripped film at the position at which stretching is completed (position B in Fig. 4). At this time, the left and right gripping tools that faced each other at the entrance of the oblique stretching tenter (position A in Figure 4) move on the asymmetric rails Ri and Ro, and as a result, the gripping tool Ci traveling on the Ri side advances relative to the gripping tool Co traveling on the Ro side. In other words, when the grippers Ci and Co, which were facing each other in a direction approximately perpendicular to the film unwinding direction D1 at the entrance of the oblique stretching tenter (the position where the film grippers start to grip) A, are at position B at the end of the film stretching, the straight line connecting the grippers Ci and Co is inclined at an angle θL with respect to a direction approximately perpendicular to the film winding direction D2. In this manner, the film is obliquely stretched in the direction θL, where "approximately perpendicular" means within the range of 90±1°.

[0040] The oblique stretching tenter can heat the raw film to any temperature at which it can be stretched. The oblique stretching tenter is equipped with a heating zone, a pair of rails on the left and right along which grippers for transporting the film run, and a number of grippers running on the rails. Both ends of the film sequentially supplied to the entrance of the tenter are gripped by the grippers, the film is guided into the heating zone, and the film is released from the grippers at the exit of the tenter. The film released from the grippers is taken up in a take-up process. Each of the pair of rails has an endless continuous track, and the grippers that release their grip on the film at the exit of the tenter run on the outside and are sequentially returned to the entrance.

[0041] The rail pattern of the tenter is asymmetrical on the left and right, and the rail pattern can be adjusted manually or automatically depending on the orientation angle θ and the stretch ratio to be given to the obliquely stretched film to be produced. In the oblique stretching tenter used in the production method according to the embodiment of the present invention, it is preferable that the positions of each rail part and rail connecting part can be freely set and the rail pattern can be arbitrarily changed. In an embodiment of the present invention, the gripping tools of the tenter are adapted to travel at a constant speed while maintaining a constant distance between the gripping tools in front and behind.

[0042] The running speed of the gripping tool can be appropriately selected, but is usually within the range of 1 to 100 m / min. Under high-speed production conditions, the inclination of the orientation angle on the inner circumference side becomes larger, so that the problem of scratches and dents during slitting becomes more prominent. Therefore, the effect of the present invention can be further improved by carrying out the present invention at a running speed in the range of 4 to 75 m / min, and the effect of the present invention can be further improved by carrying out the present invention at a running speed in the range of 10 to 50 m / min.

[0043] The difference in running speed between the pair of left and right grippers is usually 1% or less of the running speed, preferably 0.5% or less, and more preferably 0.1% or less. This is because if there is a difference in the travel speed between the left and right sides of the film at the exit of the stretching process, wrinkles and shifting will occur at the exit of the stretching process, so the speed difference between the left and right grippers is required to be substantially the same. In a typical tenter device, there is speed unevenness on the order of seconds or less depending on the tooth period of the sprocket driving the chain, the frequency of the driving motor, etc., and often causes unevenness of several percent, but these do not fall under the speed difference described in the embodiment of the present invention.

[0044] In the oblique stretching tenter used in the manufacturing method according to the embodiment of the present invention, particularly in the portion where the film is conveyed obliquely, the rails that regulate the path of the gripping tools are often required to have a large bending rate. In order to avoid interference between the gripping tools or local stress concentration due to abrupt bending, it is desirable to make the path of the gripping tools curved at the bending portion.

[0045] In an embodiment of the present invention, at the entrance of the oblique stretching tenter (position A in Fig. 4), the raw film is gripped at both ends by left and right grippers in sequence and travels with the travel of the grippers. At the entrance of the oblique stretching tenter (position A in Fig. 4), the left and right grippers facing each other in a direction approximately perpendicular to the film traveling direction D1 travel on asymmetric rails and pass through a heating zone having a preheating zone, a stretching zone, and a heat setting zone.

[0046] The preheating zone refers to a section at the entrance of the heating zone where the grippers holding both ends run while maintaining a constant distance between them. The stretching zone refers to the section from when the gap between the gripping tools holding both ends starts to widen until it reaches a predetermined gap. At this time, the oblique stretching as described above is carried out, but transverse stretching may be carried out before or after the oblique stretching, if necessary. The heat setting zone refers to a section in which the grippers at both ends run parallel to each other during the period following the stretching zone in which the distance between the grippers becomes constant again. After passing through the heat setting zone, the film may pass through a section (cooling zone) in which the temperature is set to a temperature equal to or lower than the glass transition temperature Tg° C. of the thermoplastic resin constituting the film. At this time, in consideration of shrinkage of the film due to cooling, a rail pattern may be used in advance that narrows the distance between the opposing gripping tools.

[0047] The temperatures of each zone are preferably set, relative to the glass transition temperature Tg of the thermoplastic resin, as follows: the temperature of the preheating zone is Tg to Tg + 30°C, the temperature (stretching temperature) of the stretching zone is Tg to Tg + 50°C, the temperature of the heat setting zone is Tg - 40 to Tg + 50°C, and the temperature of the cooling zone is Tg - 80 to Tg°C. In addition, a temperature difference may be applied in the width direction in the stretching zone to control uneven thickness in the width direction. In order to apply a temperature difference in the width direction in the stretching zone, a method of adjusting the opening of a nozzle that sends hot air into a thermostatic chamber so as to apply a difference in the width direction, or a known method of arranging heaters or hot air generators in the width direction and controlling heating can be used. The lengths of the preheating zone, stretching zone, heat setting zone, and cooling zone can be appropriately selected, and the length of the preheating zone is usually 25 to 150%, the length of the heat setting zone is usually 50 to 200%, and the length of the cooling zone is usually 25 to 150% of the length of the stretching zone.

[0048] The stretching ratio (W / W0) in the oblique stretching step is preferably in the range of 1.1 to 3.0, more preferably 1.5 to 2.8. A stretching ratio in this range is preferable because it reduces thickness unevenness in the width direction. By making a difference in the stretching temperature in the width direction in the stretching zone of the oblique stretching tenter, it is possible to further improve the thickness unevenness in the width direction. W0 represents the width of the raw film before stretching, and W represents the width of the obliquely stretched film after stretching.

[0049] <Trim process> The trimming step according to the production method of the present invention is a step of trimming (cutting) both end portions of the obliquely stretched film after the oblique stretching step described above with a trimming device. Both ends of the obliquely stretched film are deformed by the gripping tools during the oblique stretching process, and therefore it is necessary to cut off both end portions with unstable shapes. In the trimming step according to the present invention, the tension applied to the leading end portion in the film taking-up step described later is set to T IN The take-up tension of the non-trimming area is T C The film end width of the leading end is set to width IN The film width of the non-trimming area is C Then, the following formula (1) is satisfied. Equation (1):[T C / width C ]<[T IN / width IN ]

[0050] FIG. 5 is a schematic diagram of a trimming device for explaining a trimming step according to the present invention, where FIG. 5(a) is a front view as seen from the conveying direction, and FIG. 5(b) is a perspective view. The trimming device of this embodiment is a device that trims both ends of the obliquely stretched film 15 in the direction along the transport direction (the direction of the arrow F in FIG. 5(b)). The trimming device is not limited to the trimming device 90 shown in FIG. 5, and may be any device that can trim both ends of the obliquely stretched film in the transport direction. Specific examples include shear cutting, razor cutting, score cutting, heat cutting, ultrasonic cutting, and laser cutting.

[0051] As shown in FIG. 5, the trimming device 90 is configured to include a leading-side slit 9a and a lagging-side slit 9b that are arranged on the extension lines of the inner guide rail 6 and the outer guide rail 7 of the oblique stretching tenter 2 (see FIGS. 2 and 3), respectively, and a support 10 for supporting the obliquely stretched film 15 from below. The leading-side slit 9a is disposed on the upper side on the inner side of the obliquely stretched film 15, and the delayed-side slit 9b is disposed on the upper side on the outer side of the obliquely stretched film 15.

[0052] The leading-side slit 9a and the delaying-side slit 9b are preferably circular blades rotatably supported on a shaft. Here, the leading-side slit 9a and the delaying-side slit 9b are rotatably supported on a shaft so as to rotate passively in accordance with the transport of the obliquely stretched film 15, and a support 10 described later is rotated by a drive motor (not shown) in accordance with the transport of the obliquely stretched film 15 so as to match the transport speed of the obliquely stretched film 15.

[0053] In addition, both the leading-side slit 9a and the lagging-side slit 9b and the support 10 may be rotated so as to be approximately equal to the transport speed of the obliquely stretched film 15. In addition, either or both of the leading-side slit 9a and the lagging-side slit 9b and the support 10 may be rotated in the opposite direction.

[0054] The leading side slits 9a and the delaying side slits 9b may be so-called dish-shaped blades, bowl-shaped blades, or circular blades of other shapes, but here it is assumed that the leading side slits 9a and the delaying side slits 9b are dish-shaped blades.

[0055] The material of the leading side slit 9a and the delay side slit 9b may be metal or ceramic, but it is preferable to use a cemented carbide or high speed steel. From the viewpoint of the amount of cutting waste and the smoothness of the cut surface, it is preferable to use a cemented carbide blade. It is preferable that the diameter of the leading side slit 9a and the lagging side slit 9b is within a range of 90 to 150 mm, and the thickness is within a range of 1 to 5 mm. The laser cutting device is preferably one that can irradiate laser light with a circular cross section in a direction perpendicular to the laser light irradiation direction. Also, one that can irradiate laser light by providing a focal point in front of the laser light irradiation direction and reducing the diameter of the circle toward the focal point is preferably used. The means for reducing the diameter of the circle of the laser light is not particularly limited, and examples thereof include commonly used means such as lenses, prisms, and mirrors. The laser light is not particularly limited, and known laser light can be used. Examples include CO2 laser, YAG laser, UV laser, etc. When irradiating the laser light, the laser light irradiation time, irradiation intensity, and spot diameter are not particularly limited, and the laser irradiation conditions can be appropriately selected within a range in which the irradiated part does not melt or deform when the film is heated, and the irradiation means may be one-time irradiation or multiple irradiations. The output of the laser irradiation is, for example, 1W to 300W, and preferably 5W to 50W.

[0056] The support 10 is a member that supports the obliquely stretched film 15 from below, and is preferably in the form of a roll, for example. As described above, the support 10 is rotated by a drive motor so as to match the transport speed of the obliquely stretched film 15. In addition, the support 10 shown in Figure 5 is long and rectangular along the width direction of the obliquely stretched film 15, and the support 10 has grooves 10c and 10d formed at positions corresponding to the leading-side slits 9a and the delayed-side slits 9b, into which the leading-side slits 9a and the delayed-side slits 9b can be inserted, respectively, so that when the obliquely stretched film 15 is trimmed, the leading-side slits 9a and the delayed-side slits 9b are inserted into the grooves 10c and 10d.

[0057] In the present invention, when the contact width between the obliquely stretched film 15 and the support 10 supporting the obliquely stretched film 15 is defined as contact width A, it is preferable that the following formula (5) is satisfied. Formula (5): 0% IN +Width C +Width OUT )×100(%)<10% More preferably, the relationship of formula (5-1) is satisfied. Formula (5-1): 1% IN +Width C +Width OUT )×100(%)<5%

[0058] ​​Here, the "contact width A" refers to the width (length) where the support 10 and the obliquely stretched film 15 are in contact with each other, and refers to the width indicated by the symbol A in FIG. 5(a).

[0059] Since it is preferable to satisfy formula (5) as described above, it is more preferable that the support has the form shown in Fig. 6. Fig. 6 is a schematic diagram of another embodiment of the trimming device according to the present invention, where Fig. 6(a) is a front view as seen from the conveying direction, and Fig. 6(b) is a perspective view. In the trimming device 90 shown in FIG. 6, A / (width) represented by the above formula (5) IN +Width C +Width OUT )×100 is 10%, and in the trimming device 90 shown in FIG. IN +Width C +Width OUT ) × 100 is considered to be 100%.

[0060] 6, the inner support 10a is provided at a position corresponding to the leading-side slit 9a, and the outer support 10b is provided at a position corresponding to the lagging-side slit 9b so as to be parallel to the width direction of the obliquely stretched film 15. The contact width A between the two supports 10a and 10b and the obliquely stretched film 15 satisfies the above formula (5).

[0061] The material of the support 10 (inner support 10a and outer support 10b) is preferably metal or rubber, and more preferably metal. When the supports 10, 10a and 10b are made of metal, their surfaces are preferably mirror-finished, grooved or matte-finished, and mirror-finished surfaces are more preferable. In this case, it is preferable that the surfaces of the supports 10, 10a and 10b have an arithmetic mean roughness Ra of 10 nm or less and are free of pinholes and protrusions.

[0062] In the present invention, it is preferable that in the trimming step, a difference in distance between a trimming start position of the leading-side end portion of the obliquely stretched film and a trimming start position of the lagging-side end portion is within a range of ±200 mm.

[0063] FIG. 6(b) is a diagram showing a case where the distance difference between the trimming start position of the leading end and the trimming start position of the lagging end is 0 mm, and FIG. 7 is a diagram showing a case where the distance difference between the trimming start position of the leading end and the trimming start position of the lagging end is less than +200 mm.

[0064] Here, the trimming start position of the leading end refers to the apex X in the height direction perpendicular to the axial direction of the inner support 10a provided at the leading end, as shown in Figures 6(b) and 7. The trimming start position of the delaying end refers to the apex Y in the height direction perpendicular to the axial direction of the outer support 10b provided at the delaying end, as shown in Figures 6(b) and 7. Therefore, the "distance difference between the trimming start position of the leading side end portion and the trimming start position of the lagging side end portion" refers to the shortest distance m along the transport direction F in the interval between the vertex X and the vertex Y. In addition, "the distance difference is within the range of ±200 mm" means the range from a position 200 mm from the apex X in the opposite direction to the film transport direction F to a position 200 mm toward the film transport direction F, with the trimming start position of the leading end (i.e., apex X) as the base, and the opposite direction to the film transport direction F as the negative (-) side. It is preferable that the leading side and the lagging side of the obliquely stretched film are trimmed simultaneously or within ±3 seconds, so that the distance difference can be within the range of ±200 mm.

[0065] In FIG. 6(b), the shortest distance between vertices X and Y in the transport direction F is 0 mm, and the inner support 10a and the outer support 10b are disposed at the same position in the transport direction.

[0066] On the other hand, in FIG. 7, the shortest distance m between vertices X and Y in the transport direction F is less than +200 mm, and the inner support 10a and the outer support 10b are arranged at offset positions in the transport direction F.

[0067] Furthermore, in the present invention, the widths of the leading edge, the lagging edge and the non-trimming area to be trimmed (width IN ,width C ,width OUT ) satisfies the following formula (3) or (4), the stability of the film edge immediately after trimming is excellent, and the production stability of the obliquely stretched film is also improved. Formula (3): 15%<(width IN / width C )×100(%)<40% Formula (4): 15%<(width OUT / width C )×100(%)<40%

[0068] In the trimming step of the present invention, it is preferable to perform trimming under conditions where the temperature of the obliquely stretched film is higher than room temperature. In other words, by heating the film position where the slit blade contacts before the slit blade contacts the film, it becomes possible to perform trimming of the obliquely stretched film under high temperature conditions, and film fragments and residue are less likely to adhere to the slit blade.

[0069] The temperature is preferably adjusted by heating the resin film before cutting using a CO2 laser light irradiation device or a heat generator. The heat generator is not particularly limited as long as it can heat the resin film to a predetermined temperature, and may be, for example, an infrared heater or circulate heated air at a constant temperature to achieve the predetermined temperature.

[0070] The trimming device preferably has a mechanism that follows the stretching direction of the obliquely stretched film. In the oblique stretching tenter, the stretching direction and the winding direction can be set arbitrarily to obtain an obliquely stretched film having an orientation axis inclined as required with respect to the width direction of the film. Therefore, the trimming device according to the present invention is also required to have a mechanism that operates in accordance with the transport in the stretching direction and the winding direction. In this way, the trimming device has the tracking mechanism, so that both ends of the obliquely stretched film can be easily cut. In particular, in the case where the trimming tension is changed according to the width of the leading end and the lagging end as in the present invention, it is not necessary to remove or reconstruct the trimming device when changing the inclination angle of the stretching direction and the take-up direction, which results in excellent productivity.

[0071] A specific example of the follow-up mechanism is, for example, a movable unit that is fixed from the end positions of the guide rails 13 and 14, including the transport roller 8 and the leading-side slits 9a and the lagging-side slits 9b, to the film take-up devices 4a, 4b, and 4c, onto a movable plate or onto a movable rail. In other words, there is a method in which the end positions of the guide rails 13 and 14 and the film take-up devices 4a, 4b, and 4c can be moved together, but this is not particularly limited.

[0072] In addition, the trimming device preferably has a mechanism for checking the angle between the stretching direction of the obliquely stretched film and the traveling direction of the slit blade. By having such a checking mechanism, the trimming device can operate more simply in accordance with the transport in the stretching direction. A specific example of the confirmation mechanism is one in which a light source is provided in the leading-side slit 9a and the lagging-side slit 9b, and the position is confirmed by detecting light from the light source with a sensor provided in the film take-up devices 4a, 4b, and 4c, the heating zone 2, or the like. The light source may be a commercially available one such as a laser, and is not particularly limited.

[0073] Moreover, the trimming device may be provided between the transport rollers 8 as shown in FIGS. 2 and 3, and may be installed anywhere between the transport rollers 8. The number of the transport rollers 8 is not particularly limited, and a step of attaching a protective sheet to protect the obliquely stretched film may be provided midway between the transport rollers. Also, a step of knurling the left and right ends of the film with an embossing ring and a back roll before the film is wound up to provide embossed portions (not shown) on the film ends may be provided.

[0074] In addition, a thickness meter or an optical value measuring instrument capable of online measurement may be disposed in the middle of the transport rollers. Furthermore, a static eliminator for eliminating static electricity from the obliquely stretched film may be provided before or after the transport rollers or between multiple transport rollers.

[0075] The static eliminator can be configured to apply a reverse potential by a static eliminator or a forced charging device during winding so that the charged potential when the original roll is re-unwound is ±2 kV or less, but the forced charging potential can also be configured to be neutralized by a static eliminator that alternates between positive and negative at 1 to 150 Hz. In addition, instead of the static eliminator, an ionizer or a static eliminator bar that generates ion wind can be used. Here, the ionizer static elimination is performed by blowing ion wind toward the film that is wound from the embossing device through the transport roller. The ion wind is generated by a static eliminator. As the static eliminator, a known one can be used without any restrictions.

[0076] <Film removal process> The film taking-up process (hereinafter also simply referred to as the "taking-up process") in the manufacturing method of the present invention is a process of taking up the obliquely stretched film after the trimming process, and specifically, a process of taking up and winding up each of the trimmed leading-side end portion, the trailing-side end portion, and the non-trimmed region of the obliquely stretched film after the trimming process independently. The take-up device used in the film take-up process will be described below.

[0077] (Removal device) As shown in Figures 2 and 3, the leading end, non-trimming area, and lagging end of the film trimmed in the trimming process are independently taken up by film take-up device 4a for the leading end, film take-up device 4b for the non-trimming area, and film take-up device 4c for the lagging end, respectively. These take-up devices 4a, 4b, and 4c are configured to take up the film at a predetermined angle with respect to the outlet of the oblique stretching tenter, which allows for precise control of the take-up position and angle of the film, making it possible to obtain an obliquely stretched film with small variations in film thickness and optical values, and therefore effectively preventing the occurrence of wrinkles in the film.

[0078] The film take-up device 4b is preferably a roll capable of taking up the film. Each of the film take-up devices 4a and 4c may be a roll capable of taking up a film, or may only be a take-up device, and is not particularly limited.

[0079] In the take-up step of the present invention, the take-up tension of the trimmed leading end is T IN The take-up tension of the non-trimming area is T C The film end width of the leading end is set to width IN The film width of the non-trimming area is C When the above formula (1) is satisfied, the film at the leading end, the lagging end and the non-trimming area are taken up. Equation (1):[T C / width C ]<[T IN / width IN ]

[0080] The tension applied to the delayed end is T OUT The film end width of the retardation side end is OUT In this case, it is more preferable to take it out so as to satisfy the relationship of the following formula (2). Formula (2): 0.8<[T C / width C] / [T OUT / width OUT ]<[T IN / width IN ] / [T C / width C ]<4.0

[0081] Specifically, the take-up tension T of the non-trimming area C is within a range of 0.01 to 0.2 N / mm, more preferably 0.02 to 0.15 N / mm, and particularly preferably 0.03 to 0.1 N / mm. The above numerical values ​​are appropriately changed depending on the thickness and resin used.

[0082] The take-up tension T IN , take-up tension T C and take-up tension T OUT A method for controlling the load to within the above range includes measuring the load on the roll, i.e., the tension of the film, and controlling the rotation speed of the take-up roll by a general PID control method so that the value is within the above range. A method for measuring the load includes attaching a load cell to the bearing of the roll and measuring the load on the roll, i.e., the tension of the film. The load cell may be a known tension or compression type.

[0083] The obliquely stretched film after stretching is released from the gripping tools, discharged from the tenter outlet, and after both ends (both sides) of the film are trimmed, it is divided into the trimmed leading end, the trailing end, and the non-trimming region, which are each taken up independently and sequentially by a take-up device. The non-trimming region is sequentially wound up into a roll. The untrimmed region of the film thus wound is used as an obliquely stretched film for various products such as polarizing plates and organic electroluminescence displays.

[0084] In addition, before winding, in order to prevent blocking between the films, a masking film may be overlapped and wound at the same time, or a tape or the like may be attached to at least one end, preferably both ends, of the obliquely stretched film before winding. There are no particular limitations on the masking film as long as it can protect the film, and examples thereof include a polyethylene terephthalate film, a polyethylene film, and a polypropylene film. For removing static electricity during winding of the formed film, the static removing method and static removing device described in the slitting process may be used.

[0085] <Resins used in raw film> The raw film according to the present invention is not particularly limited and may be any film made of a thermoplastic resin. However, for example, when the stretched film is to be used for optical purposes, a film made of a resin having transparency to the desired wavelength is preferred. Examples of such resins include polycarbonate-based resins (PC), polyester-based resins, olefin polymer-based resins having an alicyclic structure (cycloolefin-based resins, COP), polyethersulfone-based resins, polyethylene terephthalate-based resins, polyimide-based resins, polymethyl methacrylate-based resins, polysulfone-based resins, polyarylate-based resins, polyethylene-based resins, polyvinyl chloride-based resins, and cellulose ester-based resins.

[0086] Polycarbonate resins are polyesters of carbonic acid and glycol or dihydric phenols, and are polymers having a carbonate bond of -O-CO-O-. Polymers of bisphenol and carbonate esters are most commonly used, and are commercially available from Teijin Ltd. (Panlite (registered trademark), Pure Ace (registered trademark)), Kaneka Corporation (Elmec (registered trademark)), Mitsubishi Engineering Plastics Corporation (Iupilon (registered trademark)), etc. Of course, polymers copolymerized with monomers having fluorene groups (see, for example, JP-A-2005-189632) show reverse wavelength dispersion of retardation, and such polycarbonates can also be preferably used depending on the application.

[0087] Examples of polyester resins include polyethylene terephthalate (PET) and polyethylene naphthalate (PEN). Polymers copolymerized with monomers having fluorene groups exhibit inverse wavelength dispersion of retardation, and therefore such polyesters may also be preferably used depending on the application.

[0088] As the polyethylene naphthalate-based resin, for example, polyethylene naphthalate produced by polycondensing a lower alkyl ester of naphthalenedicarboxylic acid with ethylene glycol can be suitably used. As a commercially available product, Teonex (manufactured by Teijin Ltd.) can be suitably used.

[0089] The cycloolefin resin is not particularly limited as long as it is a resin having a monomer unit made of a cyclic olefin (cycloolefin). The cycloolefin resin may be either a cycloolefin polymer (COP) or a cycloolefin copolymer (COC). The cycloolefin copolymer refers to a non-crystalline cyclic olefin resin that is a copolymer of a cyclic olefin and an olefin such as ethylene.

[0090] The cyclic olefins include polycyclic cyclic olefins and monocyclic cyclic olefins. Examples of such polycyclic cyclic olefins include norbornene, methylnorbornene, dimethylnorbornene, ethylnorbornene, ethylidenenorbornene, butylnorbornene, dicyclopentadiene, dihydrodicyclopentadiene, methyldicyclopentadiene, dimethyldicyclopentadiene, tetracyclododecene, methyltetracyclododecene, dimethylcyclotetradodecene, tricyclopentadiene, tetracyclopentadiene, etc. Examples of monocyclic cyclic olefins include cyclobutene, cyclopentene, cyclooctene, cyclooctadiene, cyclooctatriene, cyclododecatriene, etc.

[0091] Cycloolefin resins are also available as commercial products, and examples thereof include "ZEONOR" manufactured by Zeon Corporation, "ARTON" manufactured by JSR Corporation, "TOPAS" manufactured by Polyplastics Co., Ltd., and "APEL" manufactured by Mitsui Chemicals, Inc.

[0092] In addition, as the resin constituting the raw film, the resin composition described in JP-A-2006-45369 and the alkoxycinnamic acid ester-based polymer described in JP-A-2016-108544 can also be used. The cycloolefin resin may be blended with specific hydrocarbon resins, for example, those described in JP-A-9-221577 and JP-A-10-287732, or known thermoplastic resins, thermoplastic elastomers, rubbery polymers, organic fine particles, inorganic fine particles, etc., within the scope not impairing the effects of the present invention, and may contain additives such as specific wavelength dispersion agents, sugar ester compounds, antioxidants, peeling promoters, rubber particles, plasticizers, and ultraviolet absorbers.

[0093] <Production method of original film> The raw film may be produced by the solution casting method or the melt casting method, which will be described below. Each method will be described below.

[0094] (Solution casting film method) The solution casting film forming method includes the steps of preparing a dope by dissolving a resin and additives in a solvent, casting the dope onto a belt-shaped or drum-shaped metal support, drying the cast dope as a cast film (web), peeling the web from the metal support, stretching the web or maintaining its width, drying the web, and winding up the finished film.

[0095] The metal support used in the casting process is preferably one with a mirror-finished surface, and a stainless steel belt or a cast drum with a plated surface is preferably used. The surface temperature of the metal support is set to -50°C to a temperature at which the solvent does not boil and foam. A higher support temperature is preferable because the web can be dried faster, but if the support temperature is too high, the web may foam or the flatness may deteriorate.

[0096] The preferred support temperature is appropriately determined in the range of 0 to 100°C, and is more preferably 5 to 30°C. Alternatively, it is also a preferred method to gel the web by cooling it and peel it off from the drum in a state containing a large amount of residual solvent. There are no particular limitations on the method for controlling the temperature of the metal support, but there are methods such as blowing hot or cold air or bringing hot water into contact with the back side of the metal support. Using hot water is preferred because heat is transferred more efficiently and the time required for the temperature of the metal support to become constant is shorter.

[0097] When using hot air, it is sometimes necessary to use hot air above the boiling point of the solvent, taking into account the drop in temperature of the web due to the latent heat of evaporation of the solvent, while also using air at a temperature higher than the desired temperature while preventing foaming.

[0098] In particular, it is preferable to change the temperature of the support and the temperature of the drying air during the period from casting to peeling, so as to perform drying efficiently.

[0099] In order for the resin film to have good planarity, it is preferable that the amount of residual solvent when the web is peeled off from the metal support is within a desired range. Here, the amount of residual solvent is defined by the following formula: Residual solvent amount (mass% or %) = {(MN) / N} x 100 Here, M is the mass (g) of a sample taken at any time during or after the production of the web or film, and N is the mass (g) of M after heating at 115° C. for 1 hour.

[0100] In the film drying process, the roll drying method (a method in which the web is dried by passing it alternately through multiple rolls arranged above and below) or the tenter method, in which the web is dried while being transported, is generally used.

[0101] (Melt casting film method) The melt casting film forming method is a method in which a resin composition containing a resin and additives such as a plasticizer is heated to a temperature at which it exhibits fluidity and melted, and then the fluid molten material is cast to form a film. Methods for forming films by melt casting can be classified into melt extrusion (molding), press molding, inflation, injection molding, blow molding, stretch molding, and the like. Among these, the melt extrusion method is preferred because it can produce films with excellent mechanical strength and surface accuracy. In addition, it is usually preferred that the multiple raw materials used in the melt extrusion method are previously kneaded and pelletized.

[0102] Pelletization may be performed by a known method, for example, by feeding the dry resin, plasticizer, and other additives to an extruder with a feeder, kneading them using a single-screw or twin-screw extruder, extruding them in the form of strands from a die, water-cooling or air-cooling them, and cutting them into pellets.

[0103] The additives may be mixed with the resin before being fed to the extruder, or the additives and the resin may be fed to the extruder by separate feeders. Also, it is preferable to mix small amounts of additives such as particles and antioxidants with the resin in advance in order to mix them uniformly.

[0104] It is preferable that the extruder is capable of pelletizing and processes at a low temperature as much as possible to suppress shearing force and prevent deterioration of the resin (reduction in molecular weight, coloration, gel formation, etc.). For example, in the case of a twin-screw extruder, it is preferable to use deep-groove type screws and rotate them in the same direction. For uniformity of kneading, an intermeshing type is preferable.

[0105] The pellets obtained as described above are used to form a film. Of course, it is also possible to feed the raw material powder directly to an extruder using a feeder without pelletizing, and form a film directly from the powder.

[0106] The above pellets are extruded using a single-screw or twin-screw extruder at a melt temperature of about 200 to 300°C, filtered using a leaf disk type filter or the like to remove foreign matter, and then cast into a film from a T-die. The film is then nipped between a cooling roll and an elastic touch roll and solidified on the cooling roll.

[0107] When the pellets are introduced from the supply hopper into the extruder, it is preferable to carry out the introduction under vacuum, reduced pressure, or in an inert gas atmosphere to prevent oxidative decomposition and the like.

[0108] It is preferable to stabilize the extrusion flow rate by introducing a gear pump, etc. The filter used to remove foreign matter is preferably a stainless steel fiber sintered filter. A stainless steel fiber sintered filter is made by compressing stainless steel fibers into a complex entangled state and sintering the contact points to integrate them. The density can be changed by changing the fiber thickness and the amount of compression, and the filtration accuracy can be adjusted.

[0109] Additives such as plasticizers and particles may be mixed with the resin in advance, or may be kneaded in during the extrusion process. In order to add them uniformly, it is preferable to use a mixing device such as a static mixer.

[0110] When the film is nipped between the cooling roll and the elastic touch roll, the temperature of the film on the touch roll side is preferably set to be equal to or higher than the glass transition temperature (Tg) of the film and equal to or lower than Tg+110° C. As the roll having an elastic surface used for such a purpose, a known roll can be used.

[0111] The elastic touch roll is also called a pressing rotary body. As the elastic touch roll, a commercially available product can be used.

[0112] When the film is peeled off from the cooling roll, it is preferable to control the tension to prevent deformation of the film.

[0113] The raw film produced by each of the above-mentioned film-producing methods may be a single-layered film or a laminated film of two or more layers. The laminated film can be obtained by a known method such as a co-extrusion method, a co-casting method, a film lamination method, or a coating method. Among these, the co-extrusion method and the co-casting method are preferred.

[0114] <Specifications of the original film> The thickness of the raw film before stretching according to the present invention is preferably within the range of 10 to 200 μm, more preferably 20 to 100 μm. In addition, in this embodiment, the thickness unevenness σm in the machine direction (transport direction) of the raw film supplied to the stretching zone described later is preferably less than 0.30 μm, preferably less than 0.25 μm, and more preferably less than 0.20 μm, from the viewpoint of keeping the take-up tension of the film at the inlet of the oblique stretching tenter described later constant and stabilizing optical properties such as orientation angle and retardation. If the thickness unevenness σm in the machine direction of the raw film is 0.30 μm or more, the variation in optical properties such as retardation and orientation angle of the obliquely stretched film may worsen.

[0115] Alternatively, a film having a thickness gradient in the width direction may be supplied as the raw film. The thickness gradient of the raw film can be empirically determined by stretching films with various experimental thickness gradients so that the film thickness at the position where the stretching in the subsequent process is completed can be made as uniform as possible. The thickness gradient of the raw film can be adjusted, for example, so that the thickness of the thick end is about 0.5 to 3% thicker than the thin end.

[0116] The width of the raw film is not particularly limited, but can be within the range of 600 to 2500 mm, preferably 800 to 2000 mm.

[0117] The elastic modulus at the stretching temperature during oblique stretching of the raw film is preferably 0.01 MPa to 5000 MPa, more preferably 0.1 MPa to 500 MPa, expressed as Young's modulus. If the elastic modulus is too low, the shrinkage rate during and after stretching will be low, and wrinkles will be difficult to remove. If the elastic modulus is too high, the tension applied during stretching will be large, making it necessary to increase the strength of the parts holding both side edges of the film, which will increase the load on the tenter in the subsequent process.

[0118] The raw film may be unoriented, or may be a film previously oriented in the longitudinal or transverse direction. If necessary, the orientation of the raw film may be curved, i.e., bowed, in the transverse direction. In short, the orientation state of the raw film can be adjusted so that the film will have a desired orientation at the position where the stretching in the subsequent process is completed.

[0119] <Specifications of obliquely stretched film> The obliquely stretched film obtained by the production method of the present invention (i.e., the film in the non-trimmed region) preferably has a thickness of 25 μm or less, more preferably within the range of 1 to 20 μm, in order to accommodate lighter and more flexible devices.

[0120] The width of the obliquely stretched film according to the present invention is not particularly limited, but is preferably within the range of 1500 to 3000 mm, and more preferably 1700 to 2400 mm.

[0121] Furthermore, it is preferable that the NZ coefficient of the obliquely stretched film according to the present invention is less than 1.3, since this provides the effect of improving the viewing angle. In the present application, the "NZ coefficient" is a value defined as NZ coefficient = (nx-nz) / (nx-ny), where nx, ny, and nz are the maximum in-plane (slow axis direction) refractive index of the retardation film, the refractive index in the direction perpendicular to the slow axis in the retardation film plane (fast axis direction), and the refractive index of the retardation film in the thickness direction, respectively. That is, it is the value of the ratio of Ro to Rt (Rt / Ro+0.5).

[0122] The NZ coefficient can be adjusted to fall within the above range by adding additives, changing the compounding ratio of materials, or changing the film-forming method (casting method, stretching temperature, magnification, film-forming speed, etc.).

[0123] Furthermore, in the obliquely stretched film obtained by the manufacturing method of the present invention, the orientation angle θ is inclined with respect to the winding direction, for example, in the range of greater than 0° and less than 90°, and it is preferable that, over a width of at least 1300 mm, the variation in the in-plane retardation Ro in the width direction is 3 nm or less and the variation in the orientation angle θ is less than 0.6°.

[0124] That is, in the obliquely stretched film, the variation of the in-plane retardation Ro is 3 nm or less, preferably 1 nm or less, in at least 1300 mm in the width direction. By making the variation of the in-plane retardation Ro within the above range, when the obliquely stretched film is bonded to a polarizer layer to form a circular polarizing plate and this is applied to an organic EL display device, color unevenness due to leakage of external reflected light during black display can be suppressed. In addition, when the obliquely stretched film is used as a retardation film for a liquid crystal display device, for example, it is possible to improve the display quality.

[0125] In the obliquely stretched film, the variation in the orientation angle θ is less than 0.6°, and preferably less than 0.4°, over at least 1300 mm in the width direction. When a long obliquely stretched film having a variation in the orientation angle θ of 0.6° or more is bonded to a polarizer layer to form a circular polarizing plate, and the circular polarizing plate is installed in an image display device such as an organic EL display device, light leakage may occur, resulting in a decrease in the light-dark contrast.

[0126] The in-plane retardation Ro of the obliquely stretched film is selected to an optimum value depending on the design of the display device to be used. The Ro is a value obtained by multiplying the difference between the refractive index nx in the in-plane slow axis direction and the refractive index ny in the in-plane direction perpendicular to the slow axis by the average thickness d of the film (Ro=(nx-ny)×d).

[0127] <Polarizing plate> 8 is an exploded perspective view showing a schematic configuration of a polarizing plate 50 of this embodiment. The polarizing plate 50 is configured by laminating a polarizing plate protective film 51, a polarizer layer (also simply referred to as a "polarizer") 52, and a retardation film 53 in this order. The polarizing plate protective film 51 is configured, for example, of a cellulose ester film, but may also be configured of other transparent resin films (for example, cycloolefin resins). The polarizing plate protective film 51 may also be configured of an optical compensation film that compensates for optical properties such as viewing angle expansion.

[0128] A stretched polyvinyl alcohol doped with iodine or a dichroic dye can be used as the polarizer layer 52. The thickness of the polarizer layer is 5 to 40 μm, preferably 5 to 30 μm, and particularly preferably 5 to 20 μm.

[0129] The retardation film 53 is composed of an obliquely stretched film obtained by the manufacturing method of the present invention. The slow axis of the retardation film 53 is inclined at 10 to 80° with respect to one side (for example, side 53a) of the rectangular film outline in the film plane. The side 53a is a side corresponding to the width direction of the long obliquely stretched film. The inclination angle of the slow axis with respect to the side 53a in the film plane is preferably in the range of 30 to 60°, more preferably 45°. The angle between the slow axis of the retardation film 53 and the absorption axis (or transmission axis) of the polarizer layer 52 is, for example, 10 to 80°, preferably 15 to 75°, more preferably 30 to 60°, and even more preferably 45°.

[0130] On the surface of the retardation film 53 opposite to the polarizer layer 52, other layers (for example, a hard coat layer, a low refractive index layer, an antireflection layer, and liquid crystal (positive C-type plate)) may be appropriately provided depending on the application. In addition, an easy-adhesion layer may be provided on the surface of the retardation film 53 on the polarizer layer 52 side.

[0131] The polarizing plate 50 of this embodiment may be a long polarizing plate in which a long polarizing plate protective film 51, a long polarizer layer 52, and a long retardation film 53 (a long obliquely stretched film) are laminated in this order, or may be a sheet-like polarizing plate obtained by cutting the long polarizing plate 50 along the width direction perpendicular to the longitudinal direction.

[0132] The polarizing plate 50 can be produced by a general method. For example, the polarizing plate 50 can be produced by bonding the polarizing layer 52 and the retardation film 53 with an ultraviolet-curing adhesive (UV adhesive). The alkaline saponified retardation film 53 may be attached to one surface of the polarizing layer 52 produced by immersing a polyvinyl alcohol film in an iodine solution and stretching it, using a fully saponified polyvinyl alcohol aqueous solution (water glue). The polarizing layer 52 and the polarizing plate protective film 51 can also be bonded to each other using an ultraviolet-curing adhesive or water glue.

[0133] (Composition of UV-curable adhesive) Known ultraviolet-curable adhesive compositions for polarizing plates include photoradical polymerization-type compositions that utilize photoradical polymerization, photocationic polymerization-type compositions that utilize photocationic polymerization, and hybrid compositions that combine photoradical polymerization and photocationic polymerization.

[0134] Known examples of photoradical polymerization compositions include a composition containing a specific ratio of a radical polymerizable compound containing a polar group such as a hydroxyl group or a carboxyl group and a radical polymerizable compound not containing a polar group, as described in JP-A-2008-009329. In particular, the radical polymerizable compound is preferably a compound having a radically polymerizable ethylenically unsaturated bond. Preferred examples of compounds having a radically polymerizable ethylenically unsaturated bond include compounds having a (meth)acryloyl group. Examples of compounds having a (meth)acryloyl group include N-substituted (meth)acrylamide compounds and (meth)acrylate compounds. (Meth)acrylamide means acrylamide or methacrylamide.

[0135] Further, examples of the photocationic polymerization composition include an ultraviolet-curable adhesive composition containing each of the following components: (α) a cationic polymerizable compound, (β) a photocationic polymerization initiator, (γ) a photosensitizer that exhibits maximum absorption at wavelengths longer than 380 nm, and (δ) a naphthalene-based photosensitizer auxiliary, as disclosed in JP2011-028234A. However, ultraviolet-curable adhesives other than these may also be used.

[0136] (1) Pretreatment process The pretreatment step is a step of carrying out an easy-adhesion treatment on the adhesive surfaces of the retardation film and the polarizing plate protective film (collectively referred to as "protective films" herein) with the polarizer layer. Examples of the easy-adhesion treatment include a corona treatment and a plasma treatment.

[0137] (UV-curing adhesive application process) In the step of applying the ultraviolet curing adhesive, the ultraviolet curing adhesive is applied to at least one of the adhesive surfaces of the polarizer layer and the protective film. When the ultraviolet curing adhesive is applied directly to the surface of the polarizer layer or the protective film, the application method is not particularly limited. For example, various wet application methods such as a doctor blade, a wire bar, a die coater, a comma coater, and a gravure coater can be used. In addition, a method can be used in which the ultraviolet curing adhesive is applied (cast) between the polarizer layer and the protective film, and then the ultraviolet curing adhesive is pressed and spread uniformly with a roller or the like.

[0138] (2)Lamination process After the ultraviolet-curing adhesive is applied by the above method, it is processed in a lamination process. In this lamination process, for example, when the ultraviolet-curing adhesive is applied to the surface of the polarizer layer in the previous application process, a protective film is superimposed thereon. In addition, in the case of a method in which an ultraviolet-curing adhesive is applied to the surface of the protective film, a polarizer layer is superimposed thereon. In addition, when an ultraviolet-curing adhesive is cast between the polarizer layer and the protective film, the polarizer layer and the protective film are superimposed in this state. Then, usually, in this state, pressure is applied by sandwiching the protective film side on both sides with pressure rollers or the like. The pressure rollers can be made of metal, rubber, or the like. The pressure rollers arranged on both sides may be made of the same material or different materials.

[0139] (3) Curing process In the curing step, the uncured ultraviolet-curable adhesive is irradiated with ultraviolet light to cure the ultraviolet-curable adhesive layer containing a cationic polymerizable compound (e.g., an epoxy compound or an oxetane compound) or a radically polymerizable compound (e.g., an acrylate-based compound, an acrylamide-based compound, etc.), and the polarizer layer and the protective film superimposed via the ultraviolet-curable adhesive are bonded together. In the configuration of this embodiment in which protective films are attached to both sides of the polarizer layer, it is advantageous to irradiate ultraviolet light with protective films superimposed on both sides of the polarizer layer via the ultraviolet-curable adhesive, and simultaneously cure the ultraviolet-curable adhesives on both sides.

[0140] Any suitable ultraviolet irradiation conditions can be adopted as long as the ultraviolet-curable adhesive can be cured. The amount of ultraviolet irradiation is preferably in the range of 50 to 1500 mJ / cm2 in terms of integrated light amount, and more preferably in the range of 100 to 500 mJ / cm2.

[0141] When the polarizing plate manufacturing process is carried out on a continuous line, the line speed depends on the curing time of the adhesive, but is preferably in the range of 1 to 500 m / min, more preferably in the range of 5 to 300 m / min, and even more preferably in the range of 10 to 100 m / min. If the line speed is 1 m / min or more, productivity can be ensured, or damage to the protective film can be suppressed, and a polarizing plate with excellent durability can be produced. Also, if the line speed is 500 m / min or less, the ultraviolet-curable adhesive can be sufficiently cured, and a polarizing plate having the desired hardness can be produced. As a result, an ultraviolet-curing adhesive layer with excellent adhesive properties can be formed.

[0142] <Organic EL display device> 9 is an exploded cross-sectional view showing a schematic configuration of an organic EL display device 100, which is an example of the display device of this embodiment. Note that the configuration of the organic EL display device 100 is not limited to this.

[0143] The organic EL display device 100 is constructed by forming a polarizing plate 301 on an organic EL element 101 as a display cell via an adhesive layer 201. The organic EL element 101 is constructed by having, in order, a metal electrode 112, a light-emitting layer 113, a transparent electrode (ITO, etc.) 114, and a sealing layer 115 on a substrate 111 made of glass, polyimide, or the like. The metal electrode 112 may be constructed of a reflective electrode and a transparent electrode.

[0144] The polarizing plate 301 is formed by laminating a λ / 4 retardation film 311, an adhesive layer 312, a polarizer layer 313, an adhesive layer 314, and a protective film 315 in this order from the organic EL element 101 side, and the polarizer layer 313 is sandwiched between the λ / 4 retardation film 311 and the protective film 315. The polarizing plate 301 (circular polarizing plate) is configured by bonding the polarizer layer 313 and the λ / 4 retardation film 311 made of an obliquely stretched film obtained by the manufacturing method of the present invention so that the angle between the transmission axis (or absorption axis) of the polarizer layer 313 and the slow axis of the λ / 4 retardation film 311 is about 45° (or 135°). The protective film 315, the polarizer layer 313, and the λ / 4 retardation film 311 of the polarizing plate 301 correspond to the polarizing plate protective film 51, the polarizer layer 52, and the retardation film 53 of the polarizing plate 50 in FIG. 8, respectively.

[0145] It is preferable that a hardened layer is laminated on the protective film 315. The hardened layer not only prevents scratches on the surface of the organic EL display device, but also prevents warping caused by the polarizing plate 301. Furthermore, an anti-reflection layer may be provided on the hardened layer. The thickness of the organic EL element 101 itself is about 1 μm.

[0146] In the above configuration, when a voltage is applied between the metal electrode 112 and the transparent electrode 114, electrons are injected into the light-emitting layer 113 from the metal electrode 112 or the transparent electrode 114, whichever is the cathode, and holes are injected from the electrode which is the anode, and the two are recombined in the light-emitting layer 113, thereby emitting visible light corresponding to the light-emitting characteristics of the light-emitting layer 113. The light generated in the light-emitting layer 113 is extracted to the outside via the transparent electrode 114 and the polarizing plate 301, either directly or after being reflected by the metal electrode 112.

[0147] In general, in an organic EL display device, a metal electrode, a light-emitting layer, and a transparent electrode are laminated in this order on a transparent substrate to form an element (organic EL element) that is a light-emitting body. Here, the light-emitting layer is a laminate of various organic thin films, and various combinations are known, such as a laminate of a hole injection layer made of a triphenylamine derivative or the like and a light-emitting layer made of a fluorescent organic solid such as anthracene, a laminate of such a light-emitting layer and an electron injection layer made of a perylene derivative, and a laminate of these hole injection layer, light-emitting layer, and electron injection layer.

[0148] Organic EL display devices emit light on the following principle: when a voltage is applied between the transparent electrode and the metal electrode, holes and electrons are injected into the light-emitting layer, and the energy generated by the recombination of these holes and electrons excites the fluorescent material, which emits light when it returns to its ground state. The recombination mechanism is the same as that of a general diode, and as can be expected from this, the current and light emission intensity show strong nonlinearity with rectification with respect to the applied voltage.

[0149] In an organic EL display device, in order to extract light emitted from the light-emitting layer, at least one The anode must be transparent, and a transparent electrode made of a transparent conductor such as indium tin oxide (ITO) is usually used as the anode. On the other hand, to facilitate electron injection and increase luminous efficiency, it is important to use a material with a small work function for the cathode, and metal electrodes such as Mg-Ag and Al-Li are usually used.

[0150] In an organic EL display device with such a configuration, the light-emitting layer is formed of an extremely thin film with a thickness of about 10 nm. Therefore, like the transparent electrode, the light-emitting layer also transmits light almost completely. As a result, when no light is emitted, light enters from the surface of the transparent substrate, passes through the transparent electrode and the light-emitting layer, and is reflected by the metal electrode and exits again from the surface side of the transparent substrate, so that the display surface of the organic EL display device looks like a mirror when viewed from the outside.

[0151] The circular polarizer of this embodiment is suitable for organic EL display devices in which such external light reflection is particularly problematic.

[0152] That is, when the organic EL element 101 is not emitting light, half of the external light incident from outside the organic EL element 101 due to indoor lighting or the like is absorbed by the polarizer layer 313 of the polarizing plate 301, and the remaining half is transmitted as linearly polarized light and enters the λ / 4 retardation film 311. The light incident on the λ / 4 retardation film 311 is converted into circularly polarized light by transmitting through the λ / 4 retardation film 311 because the transmission axis of the polarizer layer 313 and the slow axis of the λ / 4 retardation film 311 intersect at 45° (or 135°).

[0153] The circularly polarized light emitted from the λ / 4 retardation film 311 is mirror-reflected by the metal electrode 112 of the organic EL element 101, and its phase is inverted by 180 degrees, so that the light is reflected as reverse-circularly polarized light. This reflected light is converted into linearly polarized light perpendicular to the transmission axis (parallel to the absorption axis) of the polarizer layer 313 by entering the λ / 4 retardation film 311, and is therefore entirely absorbed by the polarizer layer 313 and is not emitted to the outside. In other words, the polarizing plate 301 can reduce the reflection of external light at the organic EL element 101.

[0154] <Liquid crystal display device> 10 is a cross-sectional view showing a schematic configuration of a liquid crystal display device 400, which is another example of the display device of this embodiment. The liquid crystal display device 400 is configured by disposing a polarizing plate 402 on one side of a liquid crystal cell 401.

[0155] The liquid crystal cell 401 is a display cell in which a liquid crystal layer is sandwiched between a pair of substrates. On the opposite side of the polarizing plate 402 with respect to the liquid crystal cell 401, another polarizing plate arranged in a crossed Nicol state with the polarizing plate 402 and a backlight for illuminating the liquid crystal cell 401 are provided, but are not shown in FIG.

[0156] The liquid crystal display device 400 may also have a front window 403 on the opposite side of the polarizing plate 402 to the liquid crystal cell 401. The front window 403 is an exterior cover of the liquid crystal display device 400, and is made of, for example, cover glass. A filler 404 made of, for example, an ultraviolet-curable resin is filled between the front window 403 and the polarizing plate 402. If the filler 404 is not present, an air layer is formed between the front window 403 and the polarizing plate 402, and the visibility of the displayed image may be reduced due to light reflection at the interfaces between the front window 403 and the polarizing plate 402 and the air layer. However, the filler 404 prevents an air layer from being formed between the front window 403 and the polarizing plate 402, and therefore the visibility of the displayed image may be reduced due to light reflection at the interfaces.

[0157] The polarizing plate 402 has a polarizer layer 411 that transmits a predetermined linearly polarized light. A λ / 4 retardation film 413 and a cured layer 414 made of an ultraviolet curable resin are laminated in this order on one surface side (the side opposite to the liquid crystal cell 401) of the polarizer layer 411 via an adhesive layer 412. A protective film 416 is attached to the other surface side (the liquid crystal cell 401 side) of the polarizer layer 411 via an adhesive layer 415.

[0158] The polarizer layer 411 is obtained by, for example, dyeing a polyvinyl alcohol film with a dichroic dye and stretching it at a high magnification. After the polarizer layer 411 is subjected to an alkali treatment (also called a saponification treatment), a λ / 4 retardation film 413 is attached to one surface side via an adhesive layer 412, and a protective film 416 is attached to the other surface side via an adhesive layer 415. The protective film 416, the polarizer layer 411, and the λ / 4 retardation film 413 of the polarizer 402 correspond to the polarizer protective film 51, the polarizer layer 52, and the retardation film 53 of the polarizer 50 in FIG. 8, respectively. The adhesive layers 412 and 415 are layers made of, for example, a polyvinyl alcohol adhesive (PVA adhesive, water glue), but may be layers made of an ultraviolet-curing adhesive (UV adhesive).

[0159] The λ / 4 retardation film 413 is a layer that imparts an in-plane retardation of about ¼ of the wavelength to transmitted light, and is made of an obliquely stretched film obtained by the manufacturing method of the present invention. The angle (crossing angle) between the slow axis of the λ / 4 retardation film 413 and the absorption axis of the polarizer layer 411 is, for example, 30 to 60°, and more preferably 45°. As a result, the linearly polarized light from the polarizer layer 411 is converted into circularly polarized light or elliptically polarized light by the λ / 4 retardation film 413.

[0160] The cured layer 414 (also called a hard coat layer) is made of an active energy ray curable resin (for example, an ultraviolet ray curable resin).

[0161] The protective film 416 is composed of a resin film made of, for example, a cellulose-based resin (cellulose-based polymer), an acrylic resin, a cyclic polyolefin (COP), or a polycarbonate (PC). The protective film 416 is provided simply as a film for protecting the rear surface side of the polarizer layer 411, but may also be provided as an optical film that also serves as a retardation film having a desired optical compensation function.

[0162] In the case of a liquid crystal display device, another polarizing plate arranged on the opposite side of the polarizing plate 402 with respect to the liquid crystal cell 401 (liquid crystal cell) is configured by sandwiching the surface of a polarizing layer between two optical films, and the above-mentioned polarizing layer and optical films can be the same as the polarizing layer 411 and protective film 416 of the polarizing plate 402.

[0163] An easy-adhesion layer for improving the adhesion of the λ / 4 retardation film 413 may be provided on the adhesive layer 412 side of the λ / 4 retardation film 413. The easy-adhesion layer is formed by performing an easy-adhesion treatment on the adhesive layer 412 side of the λ / 4 retardation film 413. Examples of the easy-adhesion treatment include corona (discharge) treatment, plasma treatment, frame treatment, itro treatment, glow treatment, ozone treatment, and primer coating treatment, and at least one of these treatments may be performed. Among these easy-adhesion treatments, corona treatment and plasma treatment are preferable as the easy-adhesion treatment from the viewpoint of productivity.

[0164] In this manner, in a configuration of the liquid crystal display device 400 in which the polarizing plate 402 is located on the viewing side with respect to the liquid crystal cell 401 and the λ / 4 retardation film 413 of the polarizing plate 402 is located on the opposite side to the liquid crystal cell 401 with respect to the polarizer layer 411, linearly polarized light emitted from the liquid crystal cell 401 and transmitted through the polarizer layer 411 on the viewing side is converted into circularly polarized light or elliptically polarized light by the λ / 4 retardation film 413. For this reason, when a viewer wears polarized sunglasses and views a display image of the liquid crystal display device 400, a component of light parallel to the transmission axis of the polarized sunglasses can be guided to the viewer's eyes, allowing the viewer to view the display image, regardless of the angle between the transmission axis of the polarizer layer 411 and the transmission axis of the polarized sunglasses. EXAMPLES

[0165] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0166] [Production of obliquely stretched film 1] <Preparation of original film B1> An alicyclic olefin polymer resin film (COP film) as raw film B1 was produced by the following production method (melt casting film formation method).

[0167] Under a nitrogen atmosphere, 500 parts by mass of dehydrated cyclohexane were mixed with 1.2 parts by mass of 1-hexene, 0.15 parts by mass of dibutyl ether, and 0.30 parts by mass of triisobutylaluminum in a reactor at room temperature, and then, while maintaining the temperature at 45°C, a norbornene-based monomer mixture consisting of 20 parts by mass of tricyclo[4.3.0.12,5]deca-3,7-diene (dicyclopentadiene, hereinafter abbreviated as DCP), 140 parts by mass of 1,4-methano-1,4,4a,9a-tetrahydrofluorene (hereinafter abbreviated as MTF), and 40 parts by mass of 8-methyl-tetracyclo[4.4.0.12,5.17,10]-dodec-3-ene (hereinafter abbreviated as MTD), and 40 parts by mass of tungsten hexachloride (0.7% toluene solution) were continuously added over a period of 2 hours to polymerize. To the polymerization solution, 1.06 parts by mass of butyl glycidyl ether and 0.52 parts by mass of isopropyl alcohol were added to inactivate the polymerization catalyst and terminate the polymerization reaction.

[0168] Next, 270 parts by mass of cyclohexane was added to 100 parts by mass of the reaction solution containing the obtained ring-opened polymer, and further 5 parts by mass of nickel-alumina catalyst (manufactured by JGC Catalysts and Chemicals Co., Ltd.) was added as a hydrogenation catalyst. The mixture was pressurized to 5 MPa with hydrogen and heated to a temperature of 200°C with stirring, and then reacted for 4 hours to obtain a reaction solution containing 20% ​​hydrogenated polymer of DCP / MTF / MTD ring-opened polymer.

[0169] After removing the hydrogenation catalyst by filtration, a soft polymer (Kuraray Co., Ltd.; Septon 2002) and an antioxidant (Ciba Specialty Chemicals Co., Ltd.; Irganox 1010) were added to the obtained solution and dissolved (0.1 parts by mass per 100 parts by mass of polymer). Next, the solvent cyclohexane and other volatile components were removed from the solution using a cylindrical concentrating dryer (Hitachi Co., Ltd.), and the hydrogenated polymer was extruded in a molten state from an extruder in the form of strands, cooled, and pelletized for recovery. The copolymerization ratio of each norbornene monomer in the polymer was calculated from the residual norbornene composition in the solution after polymerization (by gas chromatography), and was DCP / MTF / MTD = 10 / 70 / 20, which was almost equal to the charged composition. This hydrogenated ring-opening polymer had a weight average molecular weight (Mw) of 31,000, a molecular weight distribution (Mw / Mn) of 2.5, a hydrogenation rate of 99.9%, and a glass transition temperature (Tg) of 134°C.

[0170] The obtained pellets of the hydrogenated ring-opening polymer were dried for 2 hours at 70° C. using a hot air dryer through which air was circulated to remove moisture. The pellets were then melt-extruded using a single-screw extruder having a coat hanger type T-die (manufactured by Mitsubishi Heavy Industries, Ltd.: screw diameter 90 mm, T-die lip material is tungsten carbide, peel strength with molten resin is 44 N) to obtain an alicyclic olefin polymer resin film (COP film) having a thickness of 50 μm and a residual solvent content of 10 ppm as raw film B1.

[0171] <Diagonal stretching process> The raw film B1 obtained above was stretched by the method described below using the oblique stretching device according to the present invention to obtain an obliquely stretched film 1.

[0172] First, the angle (rotation angle) between the film unwinding direction and the winding direction was set to 47°. Then, both ends of the original film B1 sent from the film unwinding device were held by the first clip (inner circumference side of the rail) and the second clip (outer circumference side of the rail).

[0173] When gripping the original film, the clip levers of the first and second clips are moved by the clip closer to grip the original film. When gripping the original film, both ends of the original film are gripped by the first and second clips at the same time, and the film is gripped so that the line connecting the gripping positions of both ends is parallel to the axis parallel to the horizontal direction of the film.

[0174] Next, the unstretched raw film was heated by passing it through the preheating zone, stretching zone, and heat fixing zone in the heating zone by the first and second clips, and stretched in the width direction to obtain an obliquely stretched film. The film transport speed during heating and stretching was 15 m / min, and the stretching temperature was appropriately selected within the range of Tg+10 to Tg+30°C depending on the thickness.

[0175] The stretching ratio of the film was set to 2 before and after stretching, and the thickness of the stretched film was set to 25 μm and the width to 1530 mm. The thickness of the stretched film is the average film thickness measured at 20 mm intervals in the width direction of the film. The average orientation angle of the stretched film, measured at 50 mm intervals in the width direction of the film, was 45°.

[0176] <Trim process> The obliquely stretched film 1 obtained in the oblique stretching step was sent to a trimming device, and both ends of the obliquely stretched film 1 were trimmed. The trimming device used was the device shown in Fig. 5, in which the leading-side slit 9a and the delayed-side slit 9b were circular blades rotatably supported on a shaft, the leading-side slit 9a and the delayed-side slit 9b were rotatably supported on a shaft so as to rotate passively in accordance with the conveyance of the obliquely stretched film, and the support 10 was driven by a drive motor to rotate in accordance with the conveyance of the obliquely stretched film so as to match the conveyance speed of the obliquely stretched film. The material of the leading-side slit 9a and the delayed-side slit 9b was ultra-hard steel, and had a diameter of 100 mm. The support (support roll) 10 was elongated along the width direction of the film, and was made of metal. The support used here was not subjected to mirror finishing or matte finishing. In addition, when the contact width between the film and the support is A, A / (width IN +Width C +Width OUT )×100(%) was set as shown in Table I below. Using such a trimming device, the widths of the leading edge, the non-trimmed area, and the lagging edge of the film (width IN ,width c ,width OUT ) and the difference in distance between the trimming start position of the leading-side end of the obliquely stretched film 1 and the trimming start position of the lagging-side end was as shown in Table I below.

[0177] <Film removal process> The leading end, the non-trimmed region and the lagging end of the obliquely stretched film trimmed in the trimming step were each taken up by a film take-up device. Here, the take-up tensions (T IN , T c , T OUT The load on the roll was controlled so that the film was taken off, with the film being pulled off at a rate as shown in Table I below.

[0178] [Production of obliquely stretched films 2 to 15 and 19 to 21] The obliquely stretched film 1 was produced in the same manner as described above, except for the following changes. In the oblique stretching step, the film was stretched so that the thickness and width of the obliquely stretched film after stretching were as shown in the following Table I. In the production of the obliquely stretched films 2, 20, and 21, the original film B1 was prepared so that the thicknesses were 30 μm, 90 μm, and 24 μm, respectively (i.e., twice the thickness of the obliquely stretched film). In the trimming process, the widths of the leading edge, the non-trimming area, and the lagging edge of the film (widthIN ,width c ,width OUT ) and the difference in distance between the trimming start position of the leading-side end of the obliquely stretched film and the trimming start position of the lagging-side end was as shown in Table I below. In the film taking-up process, the take-up tensions (T IN , T c , T OUT ) as shown in Table I below.

[0179] [Production of Obliquely Stretched Films 16 and 18] The obliquely stretched films 2 to 15 and 19 to 21 were produced in the same manner, except for the following changes. A mirror-finished metal roll (referred to as "support A" in Table I below) was used as the support (support roll) for the trimming device, and the contact width between the film and the support was defined as contact width A. The formula for A / (width IN +Width C +Width OUT )×100(%) was set as shown in Table I below.

[0180] [Production of obliquely stretched film 17] The obliquely stretched films 2 to 15 and 19 to 21 were produced in the same manner, except for the following changes. The support (support roll) of the trimming device is a matte-finished metal roll (represented as "Support B" in Table I below). When the contact width between the film and the support is defined as A, the contact width is expressed as A / (width IN +Width C +Width OUT )×100(%) was set as shown in Table I below.

[0181] [Production of obliquely stretched film 22] The obliquely stretched films 2 to 15 and 19 to 21 were produced in the same manner, except for the following changes. The trimming method for the leading-side slit 9a and the lagging-side slit 9b was to cut the film using a CO2 laser light irradiation device (wavelength 10.6 μm, laser light output 30 W).

[0182] [Production of obliquely stretched film 23] The obliquely stretched film 13 was produced in the same manner, except that the following raw film B2 was used. <Preparation of original film B2> (Cycloolefin resin) As the cycloolefin resin, a cycloolefin resin COP1 was prepared by synthesizing it as follows.

[0183] [ka]

[0184] (Synthesis of cycloolefin resin COP1) 50 g of 8-methoxycarbonyl-8-methyltetracyclo[4.4.0.12,5.17,10]-3-dodecene represented by the above structural formula, 2.3 g of 1-hexene as a molecular weight regulator, and 100 g of toluene were charged into a nitrogen-substituted reaction vessel and heated to 80° C. 0.09 ml of a toluene solution of triethylaluminum (0.6 mol / L) and 0.29 ml of a toluene solution of methanol-modified WCl6 (0.025 mol / L) were added thereto, and the mixture was reacted at 80° C. for 3 hours to obtain a polymer. The obtained ring-opened copolymer solution was then placed in an autoclave, and 100 g of toluene was added. A hydrogenation catalyst, RuHCl(CO)[P(CH)]3, was added at 2500 ppm relative to the amount of monomer charged, and the hydrogen gas pressure was set to 9-10 MPa, and the reaction was carried out at 160-165°C for 3 hours. After the reaction was completed, the mixture was precipitated in a large amount of methanol solution to obtain a hydrogenated product. The cycloolefin resin COP1, which was the hydrogenated product of the obtained ring-opened polymer, had a glass transition temperature (Tg) of 167°C and a weight average molecular weight (Mw) of 13.5×10 4 The molecular weight distribution (Mw / Mn) was 3.06.

[0185] (Preparation of Microparticle Dispersion) 12 parts by mass of fine particles (Aerosil R972V, Nippon Aerosil Co., Ltd.) and 88 parts by mass of ethanol were mixed and stirred in a dissolver for 50 minutes, and then dispersed in a Manton Gauley to prepare a fine particle dispersion. Next, 100 parts by mass of the microparticle dispersion liquid was slowly added to dichloromethane (100 parts by mass) being stirred in a dissolution tank. Further, dispersion was performed using an attritor so that the particle size of the secondary particles became a predetermined size. This was filtered using Finemet NF manufactured by Nippon Seisen Co., Ltd. to prepare a microparticle-added liquid.

[0186] (Preparation of main dope) The main dope of the following composition was prepared. First, dichloromethane and ethanol were added to a pressurized dissolution tank. Cycloolefin resin COP1 and fine particle additive liquid were added to the pressurized dissolution tank containing dichloromethane while stirring. This was heated and stirred to dissolve the resin, and this was filtered using Azumi filter paper No. 244 manufactured by Azumi Filter Paper Co., Ltd. to prepare the main dope. <Composition of main dope> Cycloolefin resin COP1 100 parts by mass Dichloromethane 302 parts by mass Ethanol 18 parts by weight Fine particle additive liquid 10 parts by mass

[0187] (Making of raw film B2) Using the above dope, a raw film B2 having a thickness of 50 μm was produced by a solution casting film-forming method. That is, the dope was cast from a casting die onto a support made of SUS316 and having a thickness of 2 mm, which was driven at a speed of 80 m / min, and the dope was dried on the support to form a casting film. Then, the casting film, which was transported by the movement of the support, was peeled off from the support to obtain the raw film B2.

[0188] [Table 1]

[0189] [Preparation of circular polarizing plates 1 to 23] In the production of the obliquely stretched films 1 to 23, the non-trimmed region of the film taken up in the film taking-up step was used to produce circularly polarizing plates 1 to 23, respectively, as described below. A polyvinyl alcohol film with a thickness of 120 μm was uniaxially stretched (at 110° C. and stretching ratio of 5 times), and then immersed in an aqueous solution of 0.075 g of iodine, 5 g of potassium iodide, and 100 g of water for 60 seconds, and then immersed in an aqueous solution of 6 g of potassium iodide, 7.5 g of boric acid, and 100 g of water at 68° C. After immersion, the film was washed with water and dried to obtain a polarizer layer. Next, the prepared obliquely stretched film 1 was attached to one side of the polarizer layer using a 5% aqueous solution of polyvinyl alcohol as an adhesive. At this time, the film was attached so that the transmission axis of the polarizer layer and the slow axis of the obliquely stretched film 1 were oriented at 45°. Then, an alkali saponified Konica Minolta TAC film KC4UAH (manufactured by Konica Minolta, Inc.) was similarly attached to the other side of the polarizer layer to prepare a circular polarizer 1. Circular polarizers 2 to 23 were also prepared in the same manner using the respective obliquely stretched films 2 to 22.

[0190] [Fabrication of organic EL display devices 1-23] A reflective electrode made of chromium with a thickness of 80 nm was formed on a glass substrate by sputtering. Next, an ITO (indium tin oxide) film with a thickness of 40 nm was formed on the reflective electrode as an anode by sputtering. Next, a poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate (PEDOT:PSS) film with a thickness of 80 nm was formed on the anode as a hole transport layer by sputtering. After that, a shadow mask was used to form the RGB light-emitting layer with a thickness of 100 nm on the hole transport layer. Furthermore, a 4 nm thick film of calcium was formed by vacuum deposition as a first cathode with a low work function that allows electrons to be efficiently injected onto the light-emitting layer. Then, a 2 nm thick film of aluminum was formed on the first cathode as a second cathode. Here, the aluminum used as the second cathode serves to prevent the calcium, which is the first cathode, from chemically altering when a transparent electrode is formed on top of it by sputtering. In this way, an organic light-emitting layer was obtained. Next, a transparent conductive film was formed on the cathode by sputtering to a thickness of 80 nm. ITO was used as the transparent conductive film. Furthermore, a silicon nitride film was formed on the transparent conductive film to a thickness of 200 nm by CVD (chemical vapor deposition) to form an insulating film. This resulted in the fabrication of an organic EL element. The size of the fabricated organic EL element was 1296 mm x 784 mm. On the insulating film of the organic EL element prepared above, a plurality of circularly polarizing plates 1 to 23 prepared as described above were fixed with an adhesive at intervals of 100 m so that the surface of the obliquely stretched film faces the surface of the insulating film of the organic EL element. In this way, organic EL display devices 1 to 23 were prepared.

[0191] [evaluation] <Frequency of breakage> The raw film was continuously processed from the unwinding process to the film take-up process for a length of 100,000 m, and the frequency of film breakage was evaluated according to the following criteria. Ranks 2 to 4 were determined to be acceptable levels for practical use. (standard) Rank 1: Break frequency 10 or more times over 100,000m Rank 2: Break frequency is 4 to 10 times after 100,000m of continuous use Rank 3: Break frequency 1-3 times after 100,000m of continuous use Rank 4: 0 breaks after 100,000m of continuous use

[0192] <Color> For each of the organic EL display devices fabricated above, a color tone evaluation was performed during black display based on the following criteria, with ranks 2 to 4 being regarded as levels that present no practical problems. (standard) Rank 1: Six or more out of 10 images show slight differences in color on the screen, or one or more out of 10 images show significant differences in color on the screen. Rank 2: Three to five out of ten images show slight differences in color on the screen. Rank 3: One or two out of ten images show slight differences in color on the screen. Rank 4: There is no difference in color on the screen for all 10 images.

[0193] [Table 2]

[0194] As shown by the above results, the obliquely stretched film obtained by the manufacturing method of the present invention has a much lower frequency of film breakage than the comparative example, and is effective in preventing breakage after the trimming process, and can be produced stably with high productivity. It is also found that the quality of the organic EL display device manufactured by using such an obliquely stretched film is good. [Explanation of symbols]

[0195] 1. Diagonal stretching device 2. Diagonal stretching tenter 3 Film unwinding device 4a Film take-up device at leading end 4b Film take-up device for non-trimming area 4c Film take-up device at the delayed end 5, 8 Transport rollers 6 Inner guide rail 7 Outer guide rail 9a Leading slit 9b Delay side slit 10 supports 10a Inner support 10b Outer support 10c, 10d groove 11, 12 Guide rail starting position 13, 14 Guide rail end position 15 Raw film or diagonally stretched film 90 Trimming Equipment Ci, Co gripper A Contact width X: Apex of support at leading end Y Apex of support at delayed end IN Leading end C Uncropped area OUT Delay side end 50 Polarizing Plate 52 Polarizer layer 53 Phase difference film (diagonally stretched film) 100 Organic EL display device 101 Organic EL element (display cell) 301 Polarizing plate 311 λ / 4 phase difference film (diagonal stretched film) 313 Polarizer Layer 400 LCD display device 401 Liquid crystal cell (display cell) 402 Polarizing plate 411 Polarizer Layer 413 λ / 4 phase difference film (diagonal stretched film)

Claims

1. an oblique stretching step in which both ends of the film in the width direction are held by a pair of grippers, one of the grippers is moved ahead relatively and the other gripper is moved behind relatively to transport the film, thereby stretching the film in a direction oblique to the width direction; a trimming step of trimming the end portion of the obliquely stretched film obtained by the stretching step; and a film taking-up step of taking up a leading-side end portion which is an end portion of the obliquely stretched film that has been trimmed on the leading side, a delayed-side end portion which is an end portion of the obliquely stretched film that has been trimmed on the delayed side, and a non-trimmed region of the obliquely stretched film, The tension applied to the leading end is T IN , and the take-up tension of the non-trimming area is T C The film end width of the leading end is set to width IN , and the film width of the non-trimming area is C In this case, the following formula (1) is satisfied: A method for producing an obliquely stretched film, characterized in that the following formula (2) is satisfied, where T OUT is the take-up tension at the delayed side end and width OUT is the film end width at the delayed side end. Formula (1): [T C / frame C ]<[T IN / frame IN ] Formula (2): 0.8<[TC / width C] / [TOUT / width OUT]<[TIN / width IN] / [TC / width C]<4.0

2. 2. The method for producing an obliquely stretched film according to claim 1, wherein in the trimming step, a difference in distance between a trimming start position of the leading-side end portion of the obliquely stretched film and a trimming start position of the lagging-side end portion is within a range of ±200 mm.

3. 3. The method for producing an obliquely stretched film according to claim 1, wherein in the trimming step, the leading side end portion and the lagging side end portion of the obliquely stretched film are trimmed simultaneously or within ±3 seconds.

4. 4. The method for producing an obliquely stretched film according to claim 1, wherein each width of the leading end portion, the lagging end portion, and the non-trimming region to be trimmed in the trimming step satisfies the following formula (3) or formula (4). Formula (3): 15%<(width IN / frame C )×100(%)<40% Formula (4): 15% < (width OUT / frame C )×100(%)<40%

5. 5. The method for producing an obliquely stretched film according to claim 1, wherein, in the trimming step, when a contact width between the obliquely stretched film and a support that supports the obliquely stretched film is defined as a contact width A, the following formula (5) is satisfied: Formula (5): 0%<A / (Width IN + frame C + frame OUT )×100(%)<10%

6. 6. The method for producing an obliquely stretched film according to claim 1, wherein the thickness of the obliquely stretched film is 25 μm or less.

7. The method for producing an obliquely stretched film according to any one of claims 1 to 6, characterized in that the obliquely stretched film has an NZ coefficient of less than 1.3.

Citation Information

Patent Citations

  • Optical film, polarizing plate, method for manufacturing these, image display panel, and image display system

    JP2011137860A

  • Trimming apparatus, and manufacturing method of optical film

    JP2015003368A

  • Method and apparatus for manufacturing brittle film

    JP2015182844A

  • Manufacturing method and manufacturing device of optical film

    JP2017109262A

  • Method for producing film

    JP2018047593A