Resin composition
A resin composition combining a polyimide resin with a polycyclic aromatic hydrocarbon skeleton and epoxy resin improves mechanical properties of inorganic-filled cured products, addressing brittleness and thermal expansion issues, resulting in high peel strength and low roughness for insulating layers.
Patent Information
- Application Number
- JP2022206973
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-04-24
- Filing Date
- 2022-12-23
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2038-04-10
AI Technical Summary
Existing resin compositions containing inorganic fillers with small average particle sizes or large specific surface areas result in brittle cured products with high roughness and thermal expansion, compromising peel strength and mechanical integrity.
Incorporating a polyimide resin with a polycyclic aromatic hydrocarbon skeleton and specific surface area, along with an epoxy resin and active ester curing agent, to create a resin composition that maintains flexibility and reduces roughness and thermal expansion while enhancing peel strength.
The composition achieves a cured product with low ten-point average roughness, low linear thermal expansion, and high peel strength, suitable for insulating layers in printed wiring boards and semiconductor devices.
Smart Images

Figure 0007578131000012 
Figure 0007578131000001 
Figure 0007578131000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. The present invention further relates to a resin sheet containing the resin composition, and a printed wiring board and a semiconductor device each containing an insulating layer formed of a cured product of the resin composition. [Background technology]
[0002] As a manufacturing technique for printed wiring boards, a manufacturing method using a build-up method in which insulating layers and conductor layers are alternately stacked is known. In the manufacturing method using the build-up method, the insulating layer is generally formed by curing a resin composition. For example, Patent Document 1 describes that an insulating layer is formed by curing a resin composition containing an epoxy resin, an active ester compound, a carbodiimide compound, a thermoplastic resin, and an inorganic filler. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2016-27097 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors further studied the resin composition and obtained the following findings. When a large amount of inorganic filler is contained in the resin composition, the surface area of the inorganic filler increases, and the interface area of the inorganic filler also increases. As a result, it was found that the cured product of the resin composition becomes brittle, and the rough surface after roughening treatment becomes rough. In addition, from the viewpoint of thinning, etc., when an inorganic filler having a small average particle size or a large specific surface area is contained in the resin composition, the cured product of the resin composition becomes more brittle because the surface area of the inorganic filler is large.
[0005] The object of the present invention is to provide a resin composition which can give a cured product having a low ten-point average roughness (Rz) and linear thermal expansion coefficient and high peel strength even when an inorganic filler having a small average particle size or a large specific surface area is used; a resin sheet containing the resin composition; and a printed wiring board and a semiconductor device which have an insulating layer formed using the resin composition. [Means for solving the problem]
[0006] In order to achieve the object of the present invention, the present inventors have conducted intensive research and found that thermoplastic resins containing phenoxy resins and aliphatic resins have excellent flexibility, but are prone to produce highly polar components such as alcohols during curing, which results in poor desmear resistance, and as a result, when roughening treatment is performed, the ten-point average roughness (Rz) may become high. Based on this knowledge, the present inventors have conducted further intensive research and found that when a resin composition contains a (C) component having a rigid and highly hydrophobic polycyclic aromatic hydrocarbon skeleton, it is possible to obtain a resin composition that can obtain a cured product with low ten-point average roughness (Rz) and linear thermal expansion coefficient, high peel strength, and improved brittleness, even when an inorganic filler with a small average particle size or a large specific surface area is used, and have completed the present invention.
[0007] That is, the present invention includes the following. [1] (A) epoxy resin, (B) an active ester curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler; A resin composition, wherein the average particle size of component (D) is 100 nm or less. [2] (A) epoxy resin, (B) an active ester curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler; (D) Component has a specific surface area of 15m 2 / g or more. [3] The resin composition according to [1] or [2], wherein the polycyclic aromatic hydrocarbon skeleton is an aromatic hydrocarbon skeleton in which a five-membered ring compound and an aromatic ring are condensed. [4] The resin composition according to any one of [1] to [3], wherein the polycyclic aromatic hydrocarbon skeleton is at least one of an indane skeleton and a fluorene skeleton. [5] The resin composition according to any one of [1] to [4], wherein the weight average molecular weight of the component (C) is 5,000 or more. [6] The resin composition according to any one of [1] to [5], wherein the component (C) has a repeating unit having a polycyclic aromatic hydrocarbon skeleton and a repeating unit having an imide structure. [7] The resin composition according to [6], in which a mass ratio of the repeating units having a polycyclic aromatic hydrocarbon skeleton to the repeating units having an imide structure (mass of repeating units having a polycyclic aromatic hydrocarbon skeleton / mass of repeating units having an imide structure) is 0.5 or more and 2 or less. [8] The resin composition according to any one of [1] to [7], wherein the content of component (C) is 0.1% by mass or more and 3% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass. [9] The resin composition according to any one of [1] to [8], wherein the content of component (B) is 1% by mass or more and 25% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.
[10] The resin composition according to any one of [1] to [9], wherein the content of the (D) component is 30% by mass or more and 80% by mass or less, when the total amount of non-volatile components in the resin composition is 100% by mass.
[11] The resin composition according to any one of [1] to
[10] , further comprising (E) a curing agent.
[12] The resin composition according to
[11] , wherein the (E) curing agent is a phenol-based curing agent.
[13] The resin composition according to any one of [1] to
[12] , which is for forming an insulating layer for forming a conductor layer.
[14] The resin composition according to any one of [1] to
[13] , which is for forming an insulating layer of a printed wiring board.
[15] The resin composition according to any one of [1] to
[14] , which is for forming an interlayer insulating layer of a printed wiring board.
[16] A resin sheet comprising a support and a layer of the resin composition according to any one of [1] to
[15] provided on the support.
[17] A printed wiring board including a first conductor layer, a second conductor layer, and an insulating layer formed between the first conductor layer and the second conductor layer, The printed wiring board, wherein the insulating layer is a cured product of the resin composition according to any one of [1] to
[15] .
[18] A semiconductor device comprising the printed wiring board according to
[17] . Effect of the Invention
[0008] According to the present invention, it is possible to provide a resin composition which can give a cured product having a low ten-point average roughness (Rz) and linear thermal expansion coefficient, high peel strength, and improved brittleness even when an inorganic filler having a small average particle size or a large specific surface area is used; a resin sheet containing the resin composition; and a printed wiring board and a semiconductor device which have an insulating layer formed using the resin composition. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a partial cross-sectional view that illustrates an example of a printed wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The resin composition, resin sheet, printed wiring board, and semiconductor device of the present invention will be described in detail below.
[0011] [Resin composition] The resin composition according to the first embodiment of the present invention contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, and the average particle size of the (D) component is 100 nm or less. The resin composition according to the second embodiment of the present invention contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, and the specific surface area of the (D) component is 15 m. 2 / g or more. The resin composition of the first embodiment contains (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and thus can provide a resin composition that can give a cured product with low ten-point average roughness (Rz) and linear thermal expansion coefficient, high peel strength, and improved brittleness, even when (D) an inorganic filler having an average particle size of 100 nm or less is contained. Similarly, the resin composition of the second embodiment contains (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and thus can provide a cured product with (D) a specific surface area of 15 m 2 Even when an inorganic filler of 0.1 g or more is contained, it is possible to obtain a resin composition which gives a cured product having a low ten-point average roughness (Rz) and linear thermal expansion coefficient, high peel strength, and improved brittleness.
[0012] The resin composition may further contain components such as (E) a curing agent (excluding active ester curing agents), (F) a curing accelerator, (G) a thermoplastic resin, and (H) other additives, as necessary. Each component contained in the resin composition of the first and second embodiments of the present invention will be described in detail below. Here, the resin composition of the first embodiment and the resin composition of the second embodiment may be collectively referred to as the "resin composition."
[0013] <(A) Epoxy resin> The resin composition includes an epoxy resin (A). Examples of the epoxy resin include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, and tetraphenylethane type epoxy resin. The epoxy resins may be used alone or in combination of two or more.
[0014] The epoxy resin preferably contains an epoxy resin having two or more epoxy groups in one molecule. When the non-volatile component of the epoxy resin is 100 mass%, it is preferable that at least 50 mass% is an epoxy resin having two or more epoxy groups in one molecule. Among them, the resin composition preferably contains a combination of an epoxy resin that is liquid at a temperature of 20°C (hereinafter referred to as "liquid epoxy resin") and an epoxy resin that is solid at a temperature of 20°C (hereinafter also referred to as "solid epoxy resin"). As the liquid epoxy resin, a liquid epoxy resin having two or more epoxy groups in one molecule is preferable, and an aromatic liquid epoxy resin having two or more epoxy groups in one molecule is more preferable. As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable. In the present invention, an aromatic epoxy resin means an epoxy resin having an aromatic ring in its molecule.
[0015] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, glycidyl amine type epoxy resin, and epoxy resin having a butadiene structure are preferred, bisphenol A type epoxy resin, bisphenol F type epoxy resin, and cyclohexane type epoxy resin are more preferred, and bisphenol A type epoxy resin is even more preferred. Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation, "828US", "jER828EL", "825", "Epikote 828EL" (bisphenol A type epoxy resin), "jER807", "1750" (bisphenol F type epoxy resin), "jER152" (phenol novolac type epoxy resin), "630", and "630LSD" (glycidylamine type epoxy resin) manufactured by Mitsubishi Chemical Corporation, and "ZX1059" (bisphenol A type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. Examples of epoxy resins include a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin, Nagase ChemteX's "EX-721" (glycidyl ester type epoxy resin), Daicel's "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton), "PB-3600" (epoxy resin having a butadiene structure), Nippon Steel & Sumikin Chemical's "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin), and Mitsubishi Chemical's "630LSD" (glycidylamine type epoxy resin). These may be used alone or in combination of two or more.
[0016] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, bixylenol type epoxy resin, naphthalene type epoxy resin, bisphenol AF type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, and naphthylene ether type epoxy resin are more preferred, and bixylenol type epoxy resin, naphthol type epoxy resin, and biphenyl type epoxy resin are even more preferred.Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200" (dicyclopentadiene type epoxy resin), "HP-7200HH", "HP-7200H", "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin), and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), "NC3000H", and "NC3000" manufactured by DIC Corporation. , "NC3000L", "NC3100" (biphenyl type epoxy resin), "ESN475V" (naphthalene type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., "YX4000H", "YX4000", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd., "YL7760" (bisphenol AF type epoxy resin) and "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "jER1010" (solid bisphenol A type epoxy resin), "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., and the like. These may be used alone or in combination of two or more types.
[0017] When a liquid epoxy resin and a solid epoxy resin are used in combination as the (A) component, the ratio of the amounts thereof (liquid epoxy resin: solid epoxy resin) is preferably in the range of 1:0.1 to 1:20 by mass. By setting the ratio of the liquid epoxy resin to the solid epoxy resin in this range, the following effects can be obtained: i) when used in the form of a resin sheet, appropriate adhesion is provided; ii) when used in the form of a resin sheet, sufficient flexibility is obtained and handling is improved; and iii) a cured product having sufficient breaking strength can be obtained. From the viewpoint of the above effects i) to iii), the ratio of the liquid epoxy resin to the solid epoxy resin (liquid epoxy resin: solid epoxy resin) is more preferably in the range of 1:0.3 to 1:10 by mass, and even more preferably in the range of 1:0.5 to 1:1.5.
[0018] From the viewpoint of obtaining an insulating layer exhibiting good mechanical strength and insulating reliability, the content of the (A) component in the resin composition is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit of the epoxy resin content is not particularly limited as long as the effects of the present invention are achieved, but is preferably 60% by mass or less, more preferably 45% by mass or less, 40% by mass or less, or 35% by mass or less.
[0019] The epoxy equivalent of the (A) component is preferably 50 to 5000, more preferably 50 to 3000, even more preferably 80 to 2000, and even more preferably 110 to 1000. Within this range, the crosslink density of the cured product is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent can be measured according to JIS K7236, and is the mass of a resin containing one equivalent of an epoxy group.
[0020] The weight average molecular weight of the component (A) is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. Here, the weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0021] <(B) Active ester curing agent> The resin composition includes (B) an active ester curing agent. The active ester curing agent is an active ester compound having one or more active ester groups in one molecule. As the active ester curing agent, an active ester curing agent having two or more active ester groups in one molecule is preferred, and for example, an active ester curing agent having two or more ester groups with high reactivity in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferably used. The active ester curing agent may be used alone or in combination of two or more.
[0022] From the viewpoint of improving heat resistance, an active ester-based curing agent obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound is preferred. Among them, an active ester-based curing agent obtained by reacting a carboxylic acid compound with one or more selected from a phenolic compound, a naphthol compound and a thiol compound is more preferred, an aromatic compound having two or more active ester groups in one molecule obtained by reacting a carboxylic acid compound with an aromatic compound having a phenolic hydroxyl group is even more preferred, and an aromatic compound having two or more active ester groups in one molecule obtained by reacting a carboxylic acid compound having at least two or more carboxy groups in one molecule with an aromatic compound having a phenolic hydroxyl group is even more preferred. The active ester-based curing agent may be linear or branched. In addition, if the carboxylic acid compound having at least two or more carboxy groups in one molecule is a compound containing an aliphatic chain, it can increase the compatibility with the resin composition, and if it is a compound having an aromatic ring, it can increase the heat resistance.
[0023] Examples of the carboxylic acid compound include aliphatic carboxylic acids having 1 to 20 carbon atoms and aromatic carboxylic acids having 7 to 20 carbon atoms. The aliphatic carboxylic acids preferably have 1 to 20 carbon atoms, more preferably have 2 to 10 carbon atoms, and even more preferably have 2 to 8 carbon atoms, and specifically include acetic acid, malonic acid, succinic acid, maleic acid, and itaconic acid. The aromatic carboxylic acids preferably have 1 to 20 carbon atoms, more preferably have 7 to 10 carbon atoms, and specifically include benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Among them, from the viewpoint of heat resistance, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, and terephthalic acid are preferred, and isophthalic acid and terephthalic acid are more preferred.
[0024] The thiocarboxylic acid compound is not particularly limited, but examples thereof include thioacetic acid and thiobenzoic acid.
[0025] The phenol compound preferably has 6 to 40 carbon atoms, more preferably 6 to 30 carbon atoms, even more preferably 6 to 23 carbon atoms, and even more preferably 6 to 22 carbon atoms. Specific examples of suitable phenol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, and dicyclopentadiene-type diphenol. As the phenol compound, phenol novolac and phosphorus atom-containing oligomers having phenolic hydroxyl groups described in JP-A-2013-40270 may also be used.
[0026] The naphthol compound preferably has 10 to 40 carbon atoms, more preferably 10 to 30 carbon atoms, and even more preferably 10 to 20 carbon atoms. Specific examples of suitable naphthol compounds include α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, and 2,6-dihydroxynaphthalene. As the naphthol compound, naphthol novolak may also be used.
[0027] Among these, bisphenol A, bisphenol F, bisphenol S, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenols, phenol novolac, and phosphorus atom-containing oligomers having phenolic hydroxyl groups are preferred, and catechol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenols, phenol novolac, and phenolic hydroxyl groups are preferred. More preferred are phosphorus atom-containing oligomers having an acid group, and still more preferred are 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, dicyclopentadiene-type diphenols, phenol novolac, and phosphorus atom-containing oligomers having a phenolic hydroxyl group, and still more preferred are 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dicyclopentadiene-type diphenols, phenol novolac, and phosphorus atom-containing oligomers having a phenolic hydroxyl group, and particularly preferred are 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dicyclopentadiene-type diphenols, and phosphorus atom-containing oligomers having a phenolic hydroxyl group, and particularly preferred are dicyclopentadiene-type diphenols.
[0028] The thiol compound is not particularly limited, but examples thereof include benzenedithiol and triazinedithiol.
[0029] Suitable specific examples of the active ester curing agent include active ester curing agents containing a dicyclopentadiene-type diphenol structure, active ester curing agents containing a naphthalene structure, active ester curing agents containing an acetylated product of phenol novolac, active ester curing agents containing a benzoylated product of phenol novolac, and active ester curing agents obtained by reacting an aromatic carboxylic acid with a phosphorus-containing oligomer having a phenolic hydroxyl group, among which active ester curing agents containing a dicyclopentadiene-type diphenol structure, active ester curing agents containing a naphthalene structure, and active ester curing agents obtained by reacting an aromatic carboxylic acid with a phosphorus-containing oligomer having a phenolic hydroxyl group are more preferred. In the present invention, the term "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.
[0030] As the active ester curing agent, the active ester curing agents disclosed in JP-A-2004-277460 and JP-A-2013-40270 may be used, and commercially available active ester curing agents may also be used. Examples of commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", and "HPC-8000L-65M" (active ester curing agents containing a dicyclopentadiene-type diphenol structure) manufactured by DIC Corporation, "EXB9416-70BK" (active ester curing agent containing a naphthalene structure) manufactured by DIC Corporation, "DC808" (active ester curing agent containing an acetylated product of phenol novolac) manufactured by Mitsubishi Chemical Corporation, "YLH1026" (active ester curing agent containing a benzoylated product of phenol novolac) manufactured by Mitsubishi Chemical Corporation, and "EXB9050L-62M" (active ester curing agent containing a phosphorus atom) manufactured by DIC Corporation.
[0031] From the viewpoint of lowering the linear thermal expansion coefficient and increasing the peel strength, the content of the active ester curing agent is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, when the non-volatile components in the resin composition are 100% by mass. The upper limit of the content of the active ester curing agent is not particularly limited, but is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less.
[0032] In addition, when the number of epoxy groups in the epoxy resin (A) is 1, from the viewpoint of obtaining an insulating layer with good mechanical strength, the number of reactive groups in the active ester curing agent (B) is preferably 0.1 to 10, more preferably 0.1 to 5, and even more preferably 0.1 to 1. Here, the "number of epoxy groups in the epoxy resin" refers to the total value of the solid content mass of each epoxy resin present in the resin composition divided by the epoxy equivalent for all epoxy resins. In addition, the "reactive group" refers to a functional group that can react with an epoxy group, and the "number of reactive groups in the active ester curing agent" refers to the total value of all values obtained by dividing the solid content mass of the active ester curing agent present in the resin composition by the reactive group equivalent.
[0033] <(C) Polyimide resin having a polycyclic aromatic hydrocarbon skeleton> The resin composition includes a polyimide resin having a polycyclic aromatic hydrocarbon skeleton (C). By having a polycyclic aromatic hydrocarbon skeleton, which is a rigid skeleton, it is possible to obtain a cured product having a low ten-point average roughness (Rz) and a low linear thermal expansion coefficient, and a high peel strength, even when an inorganic filler having a small average particle size or a large specific surface area is used. As described above, thermoplastic resins containing phenoxy resins and aliphatic resins have poor desmear resistance due to their high polarity, and as a result, the ten-point average roughness (Rz) may be high. The (C) component has a polycyclic aromatic hydrocarbon skeleton, which is a rigid skeleton with excellent hydrophobicity, in addition to a rigid imide resin. The cured product of the resin composition containing such a (C) component has a lower polarity than when a thermoplastic resin such as a phenoxy resin is contained, and as a result, the roughness after the roughening treatment can be reduced, and the ten-point average roughness (Rz) can be reduced. In addition, since the (C) component has a rigid skeleton, the resin is less likely to break, and therefore the peel strength is high. Furthermore, since component (C) has a rigid skeleton, it is difficult to expand, and therefore it is believed that the linear thermal expansion coefficient is low.
[0034] A polycyclic aromatic hydrocarbon refers to a hydrocarbon that contains two or more ring structures in one molecule, at least one of which is an aromatic ring, and the two or more ring structures may or may not be condensed.
[0035] The polycyclic aromatic hydrocarbon skeleton may or may not have a substituent. The substituent is not particularly limited, and examples of the substituent include a halogen atom, -OH, -OC 1-6 Alkyl group, -N(C 1-6 Alkyl group) 2, C 1-6 Alkyl group, C 6-10 Aryl groups, -NH2, -CN, -C(O)OC 1-6 Alkyl groups, -COOH, -C(O)H, -NO2, etc. are included. 1-6 An alkyl group is preferable, and a methyl group is more preferable. The substituent may be one kind or a plurality of kinds.
[0036] Here, "C p-qThe term "」(where p and q are positive integers and p < q)" indicates that the number of carbon atoms in the organic group described immediately after this term is p to q. For example, " 1-6 the expression "alkyl group" indicates an alkyl group having 1 to 6 carbon atoms.
[0037] Examples of the polycyclic aromatic hydrocarbon skeleton include an indane skeleton including an indane skeleton such as 1,1,3-trimethylindane skeleton, and an aromatic hydrocarbon skeleton in which a 5-membered ring compound and an aromatic ring are condensed such as a fluorene skeleton; an aromatic hydrocarbon skeleton in which aromatics such as a naphthalene skeleton and an anthracene skeleton are condensed; an aromatic hydrocarbon skeleton (non-condensed aromatic hydrocarbon skeleton) having two or more aromatics such as a biphenyl skeleton without condensation, etc. From the viewpoint of making the ten-point average roughness (Rz) lower, an aromatic hydrocarbon skeleton in which a 5-membered ring compound and an aromatic ring are condensed is preferable. Among them, from the viewpoints of lowering the linear thermal expansion coefficient of the cured product of the resin composition and increasing the glass transition temperature and peel strength, the polycyclic aromatic hydrocarbon skeleton is preferably at least one of an indane skeleton and a fluorene skeleton.
[0038] (C) component is not particularly limited as long as it is an imide resin having a polycyclic aromatic hydrocarbon skeleton, but from the viewpoints of lowering the linear thermal expansion coefficient of the cured product of the resin composition and increasing the glass transition temperature and peel strength, it is preferably a polyimide resin having a cyclic imide structure.
[0039] Examples of the cyclic imide structure include phthalimide, succinimide, glutarimide, 3-methylglutarimide, maleimide, dimethylmaleimide, trimellitimide, pyromellitimide, preferably phthalimide and succinimide. Among them, a polyimide resin having an aromatic imide structure is preferable, and phthalimide is more preferable.
[0040] (C) component preferably has a repeating unit having a polycyclic aromatic hydrocarbon skeleton and a repeating unit having an imide structure from the viewpoints of lowering the linear thermal expansion coefficient of the cured product of the resin composition and increasing the glass transition temperature and peel strength.
[0041] As a repeating unit having a polycyclic aromatic hydrocarbon skeleton, for example, a repeating unit represented by the following general formula (1) is preferable. [ka] (In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton, and D represents a single bond or a divalent linking group.)
[0042] In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton, and the details of the polycyclic aromatic hydrocarbon skeleton are as described above.
[0043] D in formula (1) represents a single bond or a divalent linking group, preferably a divalent linking group. Examples of the divalent linking group include an oxygen atom, a sulfur atom, an alkylene group, an arylene group, -NH-, -C(=O)-, -SO-, or a group consisting of a combination of two or more of these.
[0044] The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and even more preferably an alkylene group having 1 to 3 carbon atoms. The alkylene group may be linear, branched, or cyclic. Examples of such alkylene groups include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group, and the methylene group is preferred.
[0045] The arylene group is preferably an arylene group having 6 to 14 carbon atoms, and more preferably an arylene group having 6 to 10 carbon atoms. Examples of the arylene group include a phenylene group, a naphthylene group, and an anthracenylene group, and the phenylene group is preferable.
[0046] The alkylene group and the arylene group may or may not have a substituent. The substituent is the same as the substituent that the polycyclic aromatic hydrocarbon skeleton may have.
[0047] As the group consisting of two or more of these combinations, a group consisting of two or more of oxygen atoms, arylene groups, and alkylene groups is preferred. Examples of such groups include a group in which one or more arylene groups and one or more alkylene groups are bonded (a group consisting of a combination of an arylene group and an alkylene group), a group in which one or more oxygen atoms and one or more arylene groups are bonded (a group consisting of a combination of an oxygen atom and an arylene group), and the like. Examples of the group in which one or more arylene groups and one or more alkylene groups are bonded include a divalent group consisting of phenylene-methylene, a divalent group consisting of phenylene-dimethylmethylene, and the like. Examples of the group in which one or more oxygen atoms and one or more arylene groups are bonded include a divalent group consisting of phenylene-oxygen atom-phenylene, a divalent group consisting of oxygen atom-phenylene, and a divalent group consisting of oxygen atom-naphthalene, and the like.
[0048] Suitable examples of the repeating unit having a polycyclic aromatic hydrocarbon skeleton include the following. [ka]
[0049] The repeating unit having an imide structure is not particularly limited as long as it has an imide structure, but from the viewpoint of lowering the linear thermal expansion coefficient and increasing the glass transition temperature and peel strength of the cured product of the resin composition, it is preferable that the repeating unit have a cyclic imide structure.
[0050] Examples of the cyclic imide structure include phthalimide, succinimide, glutarimide, 3-methylglutarimide, maleimide, dimethylmaleimide, trimellitimide, and pyromellitimide, and preferably phthalimide and succinimide. Among them, aromatic imide structures are preferred, and phthalimide is more preferred. The repeating unit having an imide structure may be an embodiment in which the imide structure is bonded to a divalent linking group. The divalent linking group is the same as the divalent linking group represented by D in general formula (1).
[0051] Suitable examples of the repeating unit having an imide structure include the following. [ka]
[0052] The mass ratio of the repeating unit having a polycyclic aromatic hydrocarbon skeleton to the repeating unit having an imide structure (mass of repeating unit having a polycyclic aromatic hydrocarbon skeleton / mass of repeating unit having an imide structure) is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.8 or more, and is preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.5 or less. By setting the mass ratio within this range, it is possible to lower the linear thermal expansion coefficient of the cured product of the resin composition and to increase the glass transition temperature and peel strength.
[0053] The method for producing the component (C) is not particularly limited, and it can be produced according to various methods. In a preferred embodiment, it can be obtained by polymerizing a monomer that becomes a repeating unit having an imide structure and a monomer that becomes a repeating unit having a polycyclic aromatic hydrocarbon skeleton. When carrying out the polymerization, a polymerization initiator or the like may be used as necessary.
[0054] From the viewpoint of obtaining a cured product having a low ten-point average roughness (Rz) and linear thermal expansion coefficient and high peel strength, the weight average molecular weight of component (C) is preferably at least 5000, more preferably at least 10000, and even more preferably at least 11000, and is preferably at most 100000, more preferably at most 50000, and even more preferably at most 30000. Here, the weight average molecular weight of component (C) is the polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0055] From the viewpoint of obtaining a cured product having a low ten-point average roughness (Rz) and a low coefficient of linear thermal expansion and a high peel strength, the content of the (C) component is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1.5% by mass or less.
[0056] <(D) Inorganic filler> The resin composition of the first embodiment contains (D) an inorganic filler having an average particle size of 100 nm or less. The resin composition of the second embodiment contains (D) an inorganic filler having a specific surface area of 15 m 2 / g or more of inorganic filler. The material of component (D) is not particularly limited, but examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. As the silica, spherical silica is preferred. The inorganic filler may be used alone or in combination of two or more.
[0057] The average particle size of the inorganic filler in the first embodiment is 100 nm or less, preferably 90 nm or less, more preferably 80 nm or less, from the viewpoint of thinning and reducing the ten-point average roughness (Rz). The lower limit of the average particle size is not particularly limited, but it can be preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. In addition, the average particle size of the inorganic filler in the second embodiment is preferably 100 nm or less, more preferably 90 nm or less, and even more preferably 80 nm or less, from the viewpoint of thinning and reducing the ten-point average roughness (Rz). The lower limit of the average particle size is not particularly limited, but it can be preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. An example of a commercially available inorganic filler having such an average particle size is "UFP-30" manufactured by Denki Kagaku Kogyo Co., Ltd.
[0058] The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample is preferably an inorganic filler dispersed in methyl ethyl ketone using ultrasonic waves. Examples of laser diffraction / scattering particle size distribution measuring devices that can be used include the LA-500 manufactured by Horiba, Ltd. and the SALD-2200 manufactured by Shimadzu Corporation.
[0059] The specific surface area of the inorganic filler in the second embodiment is set to 15 m from the viewpoint of thinning and reducing the ten-point average roughness (Rz). 2 / g or more, more preferably 20m 2 / g or more, more preferably 30m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, more preferably 50m 2 / g or less, more preferably 40m 2 / g or less. In addition, the specific surface area of the inorganic filler in the first embodiment is preferably 15 m2 from the viewpoint of thinning and reducing the ten-point average roughness (Rz). 2 / g or more, more preferably 20m 2 / g or more, more preferably 30m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, more preferably 50m2 / g or less, more preferably 40m 2 / g or less. The specific surface area can be obtained according to the BET method by adsorbing nitrogen gas onto the surface of the sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountec Co., Ltd.) and calculating the specific surface area using the BET multipoint method.
[0060] From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler is preferably treated with one or more surface treatment agents such as a fluorine-containing silane coupling agent, an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an alkoxysilane, an organosilazane compound, a titanate coupling agent, etc., and more preferably treated with an aminosilane silane coupling agent. Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).
[0061] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably 0.2 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, and even more preferably 0.3 to 3 parts by mass, per 100 parts by mass of component (D). The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0062] The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.
[0063] The content of the (D) component is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of reducing the linear thermal expansion coefficient. The upper limit is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 65% by mass or less, from the viewpoint of improving the insulating performance.
[0064] <(E) Hardener> In one embodiment, the resin composition may contain a curing agent (E). However, the curing agent (E) does not include an active ester-based curing agent (B). The component (E) is not particularly limited as long as it has a function of curing the component (A), and examples thereof include phenol-based curing agents, naphthol-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. Among them, the component (E) is preferably a phenol-based curing agent. The curing agent may be used alone or in combination of two or more types.
[0065] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.
[0066] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Chemical Industry Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA-3018-50P", and "EXB-9500" manufactured by DIC Corporation.
[0067] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.
[0068] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.
[0069] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.
[0070] When the resin composition contains the (E) component, the ratio of the amount of the (A) component to the (E) component is preferably 1:0.01 to 1:2, more preferably 1:0.05 to 1:1.5, and even more preferably 1:0.08 to 1:1, in terms of the ratio of [total number of epoxy groups in the (A) component]:[total number of reactive groups in the (E) component]. Here, the reactive groups in the (E) component are active hydroxyl groups and the like, and vary depending on the type of the (E) component. The total number of epoxy groups in the (A) component is the total value of the solid content mass of each (A) component divided by the epoxy equivalent, and the total number of reactive groups in the (E) component is the total value of the solid content mass of each (E) component divided by the reactive group equivalent, and the total value of the solid content mass of each (E) component divided by the reactive group equivalent, and the total value of the (E) component. By setting the ratio of the (A) component to the (E) component in this range, the linear thermal expansion coefficient of the cured product of the resin composition can be lowered, and the peel strength can be improved.
[0071] Furthermore, when the resin composition contains component (E), the quantitative ratio of the epoxy resin (A) to the components (B) and (E) is preferably in the range of 1:0.01 to 1:3, more preferably 1:0.005 to 1:2, and even more preferably 1:0.1 to 1:1.5, in terms of the ratio of [total number of epoxy groups in component (A)]:[total number of reactive groups in component (B) and component (E)].
[0072] When the resin composition contains the (E) component, from the viewpoint of lowering the linear thermal expansion coefficient of the cured product of the resin composition and increasing the peel strength, the content of the (E) component is preferably 15% by mass or less, more preferably 10% by mass or less, and even more preferably 5% by mass or less, based on 100% by mass of the non-volatile components in the resin composition. There is no particular lower limit, but the content is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more.
[0073] <(F) Curing accelerator> In one embodiment, the resin composition may contain (F) a curing accelerator. Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators. Phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, and amine-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more.
[0074] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0075] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.
[0076] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.
[0077] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.
[0078] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.
[0079] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0080] When the resin composition contains a curing accelerator, the content of the curing accelerator is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 3% by mass or less, more preferably 2% by mass or less, and even more preferably 1% by mass or less. By setting the content of the curing accelerator within this range, a cured product of the resin composition having a low linear thermal expansion coefficient and high peel strength can be obtained.
[0081] <(G)Thermoplastic resin> In one embodiment, the resin composition may contain (G) a thermoplastic resin. However, the (G) thermoplastic resin does not include (C) a polyimide resin having a polycyclic aromatic hydrocarbon.
[0082] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin (excluding polyimide resin corresponding to component (C)), polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, polyester resin, etc., and phenoxy resin is preferable. The thermoplastic resin may be used alone or in combination of two or more.
[0083] The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is preferably 8,000 or more, more preferably 10,000 or more, even more preferably 20,000 or more, and particularly preferably 40,000 or more. The upper limit is not particularly limited, but is preferably 70,000 or less, more preferably 60,000 or less. The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured by gel permeation chromatography (GPC). Specifically, the polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured at a column temperature of 40° C. using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K., chloroform or the like as a mobile phase, and can be calculated using a calibration curve of standard polystyrene.
[0084] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton) manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "YL7500BH30", "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.
[0085] Examples of polyvinyl acetal resin include polyvinyl formal resin and polyvinyl butyral resin, and polyvinyl butyral resin is preferred.Specific examples of polyvinyl acetal resin include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.
[0086] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).
[0087] A specific example of a polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd. A specific example of a polyphenylene ether resin is "OPE-2St 1200", an oligophenylene ether-styrene resin having a vinyl group manufactured by Mitsubishi Gas Chemical Co., Ltd.
[0088] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers.
[0089] When the resin composition contains a thermoplastic resin, the content of the thermoplastic resin is preferably 0.1% by mass or more, more preferably 0.3% by mass or more, and even more preferably 0.5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition. The upper limit is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass.
[0090] <(H) Other Additives> In one embodiment, the resin composition may further contain other additives as necessary. Examples of such other additives include flame retardants such as organic phosphorus compounds, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone compounds, and metal hydroxides; organic fillers such as rubber particles; organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds; and resin additives such as thickeners, defoamers, leveling agents, adhesion promoters, and colorants.
[0091] <Physical properties and applications of resin compositions> The resin composition of the present invention provides an insulating layer (cured product of the resin composition layer) having a low ten-point average roughness (Rz) and a low linear thermal expansion coefficient after roughening treatment, and a high peel strength. Therefore, the resin composition of the present invention can be suitably used as a resin composition layer for insulating purposes. Specifically, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for insulating layer of printed wiring board), and can be more suitably used as a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for interlayer insulating layer of printed wiring board). In addition, since the resin composition of the present invention provides an insulating layer with good component embedding properties, it can also be suitably used when the printed wiring board is a component-embedded circuit board. In addition, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) on an insulating layer.
[0092] The resin composition is thermally cured at 100°C for 30 minutes, and then at 180°C for 30 minutes to produce a cured product that exhibits a low ten-point average roughness (Rz) after roughening treatment. That is, an insulating layer with a low ten-point average roughness is obtained. The ten-point average roughness (Rz) is preferably 1500 nm or less, more preferably 1000 nm or less, and even more preferably 600 nm or less. The lower limit is not particularly limited, but may be 1 nm or more. The ten-point average roughness (Rz) can be measured according to the method described in <Measurement of peel strength and ten-point average roughness (Rz value)> described later.
[0093] The resin composition is thermally cured at 100°C for 30 minutes and then at 180°C for 30 minutes to produce a cured product that exhibits high peel strength (plating peel strength). That is, an insulating layer with high peel strength is obtained. The peel strength is preferably 145 kgf / cm or more, more preferably 148 kgf / cm or more, and even more preferably 150 kgf / cm or more. The upper limit is not particularly limited, but may be 300 kgf / cm or less. The peel strength can be measured according to the method described in <Measurement of peel strength and ten-point average roughness (Rz value)> described later.
[0094] The cured product obtained by thermally curing the resin composition at 200°C for 90 minutes exhibits the characteristic of a high glass transition temperature. Therefore, an insulating layer with improved brittleness is obtained. The glass transition temperature is preferably 145°C or higher, more preferably 148°C or higher, and even more preferably 150°C or higher. The upper limit is not particularly limited, but may be 300°C or lower. The glass transition temperature can be measured according to the method described in <Measurement of glass transition temperature and linear thermal expansion coefficient> described later.
[0095] The resin composition is thermally cured at 200°C for 90 minutes to produce a cured product with a low linear thermal expansion coefficient. That is, an insulating layer with a low linear thermal expansion coefficient is obtained. The linear thermal expansion coefficient is preferably 45 ppm or less, more preferably 44 ppm or less, and even more preferably 43 ppm or less. The lower limit is not particularly limited, but may be 1 ppm or more. The linear thermal expansion coefficient can be measured according to the method described in <Measurement of glass transition temperature and linear thermal expansion coefficient> described later.
[0096] [Resin sheet] The resin sheet of the present invention includes a support and a resin composition layer formed from the resin composition of the present invention provided on the support.
[0097] From the viewpoint of thinning the printed wiring board, the thickness of the resin composition layer is preferably 200 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, even more preferably 20 μm or less, 15 μm or less, or 10 μm or less. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 1 μm or more, 3 μm or more, etc.
[0098] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0099] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0100] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0101] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0102] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0103] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0104] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.
[0105] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving a resin composition in an organic solvent, applying this resin varnish onto a support using a die coater or the like, and then drying the same to form a resin composition layer.
[0106] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone (MEK) and cyclohexanone, acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, amide solvents such as dimethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone, etc. The organic solvents may be used alone or in combination of two or more.
[0107] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0108] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0109] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer formed from a cured product of the resin composition of the present invention, a first conductor layer, and a second conductor layer. The insulating layer is provided between the first conductor layer and the second conductor layer, and insulates the first conductor layer from the second conductor layer (the conductor layer may be referred to as a wiring layer).
[0110] The thickness of the insulating layer between the first and second conductor layers is preferably 6 μm or less, more preferably 5.5 μm or less, and even more preferably 5 μm or less. The lower limit is not particularly limited, but may be 0.1 μm or more. The distance between the first conductor layer and the second conductor layer (the thickness of the insulating layer between the first and second conductor layers) refers to the thickness t1 of the insulating layer 3 between the main surface 11 of the first conductor layer 1 and the main surface 21 of the second conductor layer 2, as shown in FIG. 1 as an example. The first and second conductor layers are adjacent conductor layers with an insulating layer interposed between them, and the main surface 11 and the main surface 21 face each other.
[0111] The thickness t2 of the entire insulating layer is preferably 15 μm or less, more preferably 13 μm or less, and further preferably 10 μm or less. There is no particular lower limit, but it can usually be 1 μm or more, 1.5 μm or more, 2 μm or more, etc.
[0112] The printed wiring board can be produced by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate so that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of thermally curing the resin composition layer to form an insulating layer
[0113] The "inner layer substrate" used in step (I) is a member that becomes the substrate of a printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be further formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.
[0114] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.
[0115] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 26.7hPa or less.
[0116] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.
[0117] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.
[0118] The support may be removed between step (I) and step (II) or after step (II).
[0119] In step (II), the resin composition layer is thermally cured to form an insulating layer.
[0120] The conditions for thermally curing the resin composition layer are not particularly limited, and conditions that are usually employed when forming an insulating layer for a printed wiring board may be used.
[0121] For example, the thermal curing conditions for the resin composition layer will vary depending on the type of resin composition, etc., but the curing temperature can be in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time can be in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).
[0122] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C. (preferably 60° C. or more and 115° C. or less, more preferably 70° C. or more and 110° C. or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes).
[0123] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). If necessary, the steps (II) to (V) of forming the insulating layer and the conductor layer may be repeated to form a multilayer wiring board. In this case, the thickness of the insulating layer between each conductor layer (t1 in FIG. 1) is preferably within the above range.
[0124] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.
[0125] Step (IV) is a step of roughening the insulating layer. The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid used for the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution and a potassium hydroxide solution are more preferable. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment with a swelling liquid is not particularly limited, but can be performed, for example, by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 minute to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes. The oxidizing agent used in the roughening treatment is not particularly limited, but for example, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide can be mentioned. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. In addition, the concentration of the permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan. The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product is, for example, "Reduction Solution Securigant P" manufactured by Atotech Japan. Treatment with a neutralizing solution can be performed by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30°C to 80°C for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40°C to 70°C for 5 to 20 minutes is preferred.
[0126] In one embodiment, the arithmetic mean roughness (Ra) of the insulating layer surface after the roughening treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but it may be preferably 0.5 nm or more, more preferably 1 nm or more, etc. In addition, the root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 400 nm or less, more preferably 350 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, but it may be preferably 0.5 nm or more, more preferably 1 nm or more, etc. The arithmetic mean roughness (Ra) and root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.
[0127] Step (V) is a step of forming a conductor layer. When no conductor layer is formed on the inner layer substrate, step (V) is a step of forming a first conductor layer, and when a conductor layer is formed on the inner layer substrate, the conductor layer is the first conductor layer and step (V) is a step of forming a second conductor layer.
[0128] The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of the conductor layer formation, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.
[0129] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.
[0130] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.
[0131] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.
[0132] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.
[0133] The resin sheet of the present invention provides an insulating layer with good component embedding properties, and can therefore be suitably used when the printed wiring board is a circuit board with built-in components. The circuit board with built-in components can be produced by a known production method.
[0134] A printed wiring board produced using the resin sheet of the present invention may be in an embodiment including an insulating layer that is a cured product of the resin composition layer of the resin sheet, and an embedded wiring layer embedded in the insulating layer.
[0135] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.
[0136] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).
[0137] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.
[0138] The method of mounting a semiconductor chip when manufacturing a semiconductor device is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a bumpless buildup layer (BBUL) mounting method, an anisotropic conductive film (ACF) mounting method, a non-conductive film (NCF) mounting method, etc. Here, the "bumpless buildup layer (BBUL) mounting method" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES
[0139] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0140] First, the various measurement and evaluation methods will be explained.
[0141] <Peel strength and ten-point average roughness (Rz value) measurement> (Preparation of samples for measuring peel strength and ten-point average roughness (Rz value)) (1) Surface preparation for inner layer circuit boards A glass cloth-based epoxy resin double-sided copper-clad laminate (copper foil thickness 18 μm, substrate thickness 0.8 mm, Panasonic "R1766") with an inner layer circuit formed was prepared as an inner layer circuit board, and both sides of the board were immersed in a microetching agent (Mec "CZ8101") to roughen the copper surface (copper etching amount: 1.0 μm).
[0142] (2) Lamination of resin sheets The resin sheets with a resin composition layer thickness of 10 μm prepared in the examples and comparative examples were laminated on both sides of the inner layer circuit board using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd., 2-stage build-up laminator, CVP700) so that the resin composition layer was bonded to the inner layer circuit board. The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 100°C and a pressure of 0.74 MPa for 30 seconds. Next, a heat press was performed at 100°C and a pressure of 0.5 MPa for 60 seconds.
[0143] (3) Curing of the resin composition After laminating a resin sheet having a resin composition layer of 10 μm in thickness, the resin composition layer was thermally cured at 100° C. for 30 minutes and then at 180° C. for 30 minutes to form an insulating layer. Thereafter, the support was peeled off to expose the insulating layer.
[0144] (4) Roughening treatment The substrate with the exposed insulating layer was immersed in a swelling solution (Atotech Japan's "Swelling Dip Securigant P", an aqueous solution of sodium hydroxide containing diethylene glycol monobutyl ether) at 60°C for 10 minutes, then in an oxidizing agent (Atotech Japan's "Concentrate Compact CP", an aqueous solution of potassium permanganate at about 6% by mass and sodium hydroxide at about 4% by mass) at 80°C for 20 minutes, and finally in a neutralizing solution (Atotech Japan's "Reduction Solution Securigant P", an aqueous solution of hydroxylamine sulfate) at 40°C for 5 minutes. It was then dried at 80°C for 15 minutes. The obtained substrate is called "evaluation substrate a".
[0145] (5) Formation of the conductor layer A conductor layer was formed on the roughened surface of the insulating layer by a semi-additive method, that is, by carrying out a plating process (copper plating process using a chemical solution manufactured by Atotech Japan) including the following steps 1 to 6.
[0146] 1. Alkaline cleaning (cleaning the surface of the insulating layer with via holes and adjusting the charge) The surface of the evaluation substrate a was cleaned with Cleaning Cleaner Securiganth 902 (trade name) at 60° C. for 5 minutes. 2. Soft etching (cleaning inside the via hole) The surface of the evaluation substrate a was treated with an aqueous solution of sodium peroxodisulfate acidified with sulfuric acid at 30° C. for 1 minute. 3. Pre-dip (adjusting the charge on the surface of the insulating layer for Pd deposition) The surface of the evaluation substrate a was treated with Pre. Dip Neoganth B (trade name) at room temperature for 1 minute. 4. Adding an activator (adding Pd to the surface of the insulating layer) The surface of the evaluation substrate a was treated with Activator Neoganth 834 (trade name) at 35° C. for 5 minutes. 5. Reduction (reducing Pd added to the insulating layer) The surface of the evaluation substrate a was treated with a mixed solution of Reducer Neoganth WA (trade name) and Reducer Accelerator 810 mod. (trade name) at 30° C. for 5 minutes. 6. Electroless copper plating process (Cu is deposited on the surface of the insulating layer (Pd surface)) The surface of evaluation substrate a was treated with a mixture of Basic Solution Printganth MSK-DK (trade name), Copper solution Printganth MSK (trade name), Stabilizer Printganth MSK-DK (trade name), and Reducer Cu (trade name) at 35° C. for 30 minutes. The thickness of the electroless copper plating layer formed was 1 μm.
[0147] Next, the substrate was heated at 150°C for 30 minutes for annealing, after which an etching resist was formed and a pattern was formed by etching. After that, copper sulfate electrolytic plating was performed using a chemical solution manufactured by Atotech Japan to form a conductor layer with a thickness of 25 μm, and an annealing treatment was performed at 200°C for 60 minutes. The obtained substrate is referred to as "evaluation substrate b".
[0148] (Measurement of ten-point average roughness (Rz)) For evaluation substrate a before the formation of the conductor layer, the maximum height roughness (Rz) as specified in the Japanese Industrial Standards (JIS B0601-2001) was determined using a non-contact surface roughness meter (Beeco Instruments' "WYKO NT3300") in VSI contact mode with a 50x lens to obtain a measurement range of 121 μm x 92 μm.
[0149] (Measurement of peel strength of plated conductor layer) The peel strength of the plated conductor layer was measured for evaluation board b in accordance with the Japanese Industrial Standards (JIS C6481). Specifically, a 10 mm wide and 100 mm long cut was made in the conductor layer of evaluation board b, one end of which was peeled off and held with a gripper, and the load (kgf / cm) was measured when 35 mm was peeled off vertically at a speed of 50 mm / min at room temperature to determine the peel strength. A tensile tester (TSE's "AC-50C-SL") was used for the measurement.
[0150] <Measurement of glass transition temperature and linear thermal expansion coefficient> (Preparation of cured product for evaluation) The resin sheets having a resin composition layer thickness of 25 μm produced in the examples and comparative examples were heated at 200° C. for 90 minutes to thermally cure the resin composition layer, and then the support was peeled off. The obtained cured product is referred to as “evaluation cured product c”.
[0151] (Measurement of glass transition temperature and linear thermal expansion coefficient) The cured product c for evaluation was cut into a test piece having a width of 5 mm and a length of 15 mm. The test piece was subjected to a thermomechanical analysis by a tensile load method using a thermomechanical analyzer (Rigaku Corporation, "Thermo Plus TMA8310"). In detail, the test piece was mounted on the thermomechanical analyzer, and then measured twice consecutively under the measurement conditions of a load of 1 g and a heating rate of 5°C / min. In the two measurements, the glass transition temperature (°C) and the linear thermal expansion coefficient (ppm / °C) in the planar direction in the range from 25°C to 150°C were calculated, and the average value was calculated.
[0152] <Synthesis Example 1: Synthesis of polyimide resin 1 having a polycyclic aromatic hydrocarbon skeleton> A 500 mL separable flask equipped with a water content receiver connected to a reflux condenser, a nitrogen inlet tube, and a stirrer was prepared. 20.3 g of 4,4'-oxydiphthalic anhydride (ODPA), 200 g of γ-butyrolactone, 20 g of toluene, and 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane were added to the flask, and the mixture was stirred at 45°C for 2 hours under a nitrogen stream to carry out the reaction, thereby obtaining a reaction solution.
[0153] Next, the reaction solution was heated and maintained at about 160°C, while the condensed water was azeotropically removed with toluene under a nitrogen stream. It was confirmed that a predetermined amount of water had accumulated in the water content receiver and that no water was flowing out. After confirmation, the reaction solution was further heated and stirred at 200°C for 1 hour. It was then cooled to obtain a varnish containing 20 mass% of a polyimide resin having a 1,1,3-trimethylindane skeleton (hereinafter sometimes referred to as "polyimide resin 1"). The obtained polyimide resin 1 had a repeating unit represented by the following formula (X1) and a repeating unit represented by (X2). The weight average molecular weight of polyimide resin 1 was 12,000.
[0154] [ka] [ka]
[0155] <Synthesis Example 2: Synthesis of polyimide resin 2 having a polycyclic aromatic hydrocarbon skeleton> In Synthesis Example 1, 29.6 g of 5-(4-aminophenoxy)-3-[4-(4-aminophenoxy)phenyl]-1,1,3-trimethylindane was changed to 22.9 g of 9,9-bis(4-aminophenyl)fluorene. A varnish containing 20 mass% of a polyimide resin having a fluorene skeleton (hereinafter, sometimes referred to as "polyimide resin 2") was obtained in the same manner as in Synthesis Example 1 except for the above. The obtained polyimide resin 2 had a repeating unit represented by the following formula (X3) and a repeating unit represented by the formula (X2). The weight average molecular weight of polyimide resin 2 was 14,000.
[0156] [ka]
[0157] <Synthesis Example 3: Synthesis of polyimide resin 3 having no polycyclic aromatic hydrocarbon skeleton> In a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube, 65.0 g of aromatic tetracarboxylic dianhydride (SABIC Japan "BisDA-1000"), 266.5 g of cyclohexanone, and 44.4 g of methylcyclohexane were charged, and the solution was heated to 60°C. Next, 43.7 g of dimer diamine (Croda Japan "PRIAMINE 1075") and 5.4 g of 1,3-bisaminomethylcyclohexane were dropped, and then imidization reaction was carried out at 140°C for 1 hour. As a result, a varnish containing a dimer diamine polyimide resin (non-volatile content 30% by mass) was obtained (hereinafter, sometimes referred to as "polyimide resin 3"). The weight average molecular weight of polyimide resin 3 was 25,000.
[0158] <Example 1> Thirty parts of bisphenol A type epoxy resin ("828US" manufactured by Mitsubishi Chemical Corporation, epoxy equivalent approximately 180) and 30 parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent approximately 269) were dissolved in a mixed solvent of 40 parts of solvent naphtha and 15 parts of cyclohexanone with stirring, and then cooled to room temperature. The mixed solution was added with spherical silica (average particle size 0.078 μm, specific surface area 30.7 m) that had been surface-treated with an aminosilane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.). 2 / g, Denki Kagaku Kogyo Co., Ltd. "UFP-30") 100 parts, triazine skeleton-containing phenolic curing agent (DIC Corporation "LA-3018-50P", hydroxyl equivalent of about 151, 2-methoxypropanol solution with solid content of 50%) 14 parts, active ester curing agent (DIC Corporation "HPC-8000-65T", active group equivalent of about 223, toluene solution with non-volatile components of 65% by mass) 40 parts, varnish containing polyimide resin 1 synthesized in Synthesis Example 1 (γ-butyrolactone solution with solid content of 20% by mass), and curing accelerator (DMAP, 4-dimethylaminopyridine, methyl ethyl ketone (hereinafter abbreviated as "MEK") solution with solid content of 5% by mass) were mixed and uniformly dispersed in a high-speed rotating mixer to prepare resin varnish 1.
[0159] Two PET films with an alkyd resin-based release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) were prepared as supports. Resin varnish 1 was uniformly applied onto the release layer of each support so that the thickness of the resin composition layer after drying was 10 μm and 25 μm, and the resin sheet 1 was produced by drying at 70 to 95° C. for 2 minutes.
[0160] <Example 2> In Example 1, 30 parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269) was changed to 30 parts of naphthol type epoxy resin ("ESN475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., epoxy equivalent of 332). A resin varnish 2 and a resin sheet 2 were produced in the same manner as in Example 1 except for the above points.
[0161] <Example 3> In Example 1, 30 parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent of about 269) was changed to 30 parts of bixylenol type epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent of about 185). A resin varnish 3 and a resin sheet 3 were produced in the same manner as in Example 1 except for the above points.
[0162] <Example 4> In Example 1, the amount of the varnish (γ-butyrolactone solution with a solid content of 20% by mass) containing the polyimide resin 1 synthesized in Synthesis Example 1 was changed from 20 parts to 10 parts, and 7 parts of a phenoxy resin (YX6954BH30 manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30% by mass) was added. Resin varnish 4 and resin sheet 4 were produced in the same manner as in Example 1 except for the above.
[0163] <Example 5> In Example 1, 20 parts of the varnish (γ-butyrolactone solution with a solid content of 20% by mass) containing the polyimide resin 1 synthesized in Synthesis Example 1 was changed to 20 parts of the varnish (γ-butyrolactone solution with a solid content of 20% by mass) containing the polyimide resin 2 synthesized in Synthesis Example 2. A resin varnish 5 and a resin sheet 5 were produced in the same manner as in Example 1 except for the above points.
[0164] <Comparative Example 1> In Example 1, 20 parts of the varnish (γ-butyrolactone solution with a solid content of 20% by mass) containing the polyimide resin synthesized in Synthesis Example 1 was changed to 13 parts of a phenoxy resin ("YX6954BH30" manufactured by Mitsubishi Chemical Corporation, a 1:1 solution of MEK and cyclohexanone with a solid content of 30% by mass). A resin varnish 6 and a resin sheet 6 were produced in the same manner as in Example 1 except for the above points.
[0165] <Comparative Example 2> In Example 1, 20 parts of the varnish (γ-butyrolactone solution with a solid content of 20 mass %) containing the polyimide resin synthesized in Synthesis Example 1 was changed to 13 parts of the varnish (a mixed solution of cyclohexanone and methylcyclohexane with a solid content of 30 mass %) containing the polyimide resin 3 synthesized in Synthesis Example 3. Resin varnish 7 and resin sheet 7 were produced in the same manner as in Example 1 except for the above points.
[0166] The following table shows the components and their amounts (in terms of nonvolatile content) used in the preparation of resin compositions 1 to 7. In the table, "content of component (D) (mass%)" indicates the content of component (D) when the nonvolatile content in the resin composition is taken as 100 mass%.
[0167] [Table 1]
[0168] In Examples 1 to 5, it was confirmed that even when components (E) to (G) were not contained, the results were similar to those of the above Examples, although to a different extent. [Explanation of symbols]
[0169] 1 First Conductor Layer 11: Main surface of first conductor layer 2 Second conductor layer 21 Main surface of second conductor layer 3. Insulation layer t1: Distance between the first and second conductor layers (thickness of the insulating layer between the first and second conductor layers) t2 Total thickness of the insulating layer
Claims
1. A resin sheet comprising a support and a resin composition layer formed of a resin composition on the support, The resin composition contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, The average particle size of the (D) component is 100 nm or less, The component (C) is selected from the group consisting of polyimide resins having a fluorene skeleton and polyimide resins having a repeating unit represented by the following formula (1): A resin sheet (excluding those having a first resin composition layer made of a first resin composition provided on a support, and a second resin composition layer made of a second resin composition provided on the first resin composition layer) in which the content of component (C) is 0.1 mass % or more, when the non-volatile components in the resin composition are taken as 100 mass %. [Formula 1] (In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton in which a five-membered ring compound and an aromatic ring are condensed, and D represents a divalent linking group consisting of a combination of two or more of an oxygen atom, an unsubstituted arylene group, and an unsubstituted alkylene group.)
2. A resin sheet comprising a support and a resin composition layer formed of a resin composition on the support, The resin composition contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, (D) The specific surface area of the component is 15 m 2 / g or more, The component (C) is selected from the group consisting of polyimide resins having a fluorene skeleton and polyimide resins having a repeating unit represented by the following formula (1): A resin sheet (excluding those having a first resin composition layer made of a first resin composition provided on a support, and a second resin composition layer made of a second resin composition provided on the first resin composition layer) in which the content of component (C) is 0.1 mass % or more, when the non-volatile components in the resin composition are taken as 100 mass %. [Case 2] (In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton in which a five-membered ring compound and an aromatic ring are condensed, and D represents a divalent linking group consisting of a combination of two or more of an oxygen atom, an unsubstituted arylene group, and an unsubstituted alkylene group.)
3. The resin sheet according to claim 1 or 2, wherein the component (C) has a weight average molecular weight of 5,000 or more.
4. A resin sheet comprising a support and a resin composition layer formed of a resin composition on the support, The resin composition contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, The average particle size of the (D) component is 100 nm or less, The component (C) has a weight average molecular weight of 5,000 or more and 14,000 or less, The component (C) is selected from the group consisting of polyimide resins having a fluorene skeleton and polyimide resins having a repeating unit represented by the following formula (1): A resin sheet (excluding those having a first resin composition layer made of a first resin composition provided on a support, and a second resin composition layer made of a second resin composition provided on the first resin composition layer) in which the content of component (C) is 0.1 mass % or more, when the non-volatile components in the resin composition are taken as 100 mass %. [C3] (In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton in which a five-membered ring compound and an aromatic ring are condensed, and D represents a divalent linking group consisting of a combination of two or more of an oxygen atom, an unsubstituted arylene group, and an unsubstituted alkylene group.)
5. A resin sheet comprising a support and a resin composition layer formed of a resin composition on the support, The resin composition contains (A) an epoxy resin, (B) an active ester-based curing agent, (C) a polyimide resin having a polycyclic aromatic hydrocarbon skeleton, and (D) an inorganic filler, (D) The specific surface area of the component is 15 m 2 / g or more, The component (C) has a weight average molecular weight of 5,000 or more and 14,000 or less, The component (C) is selected from the group consisting of polyimide resins having a fluorene skeleton and polyimide resins having a repeating unit represented by the following formula (1): A resin sheet (excluding those having a first resin composition layer made of a first resin composition provided on a support, and a second resin composition layer made of a second resin composition provided on the first resin composition layer) in which the content of component (C) is 0.1 mass % or more, when the non-volatile components in the resin composition are taken as 100 mass %. [C4] (In formula (1), A represents a polycyclic aromatic hydrocarbon skeleton in which a five-membered ring compound and an aromatic ring are condensed, and D represents a divalent linking group consisting of a combination of two or more of an oxygen atom, an unsubstituted arylene group, and an unsubstituted alkylene group.)
6. The resin sheet according to any one of claims 1 to 5, wherein the polycyclic aromatic hydrocarbon skeleton is at least one of an indane skeleton and a fluorene skeleton.
7. The resin sheet according to any one of claims 1 to 6, wherein the component (C) has a repeating unit having a polycyclic aromatic hydrocarbon skeleton and a repeating unit having an imide structure.
8. 8. The resin sheet according to claim 7, wherein a mass ratio of the repeating unit having a polycyclic aromatic hydrocarbon skeleton to the repeating unit having an imide structure (mass of the repeating unit having a polycyclic aromatic hydrocarbon skeleton / mass of the repeating unit having an imide structure) is 0.5 or more and 2 or less.
9. The resin sheet according to any one of claims 1 to 8, wherein the content of the component (C) is 3% by mass or less, when the content of the non-volatile components in the resin composition is 100% by mass.
10. The resin sheet according to any one of claims 1 to 9, wherein the content of the component (B) is 1 mass% or more and 25 mass% or less, when the non-volatile components in the resin composition are 100 mass%.
11. The resin sheet according to any one of claims 1 to 10, wherein the content of the component (D) is 30% by mass or more and 80% by mass or less, when the content of the non-volatile components in the resin composition is 100% by mass.
12. The resin sheet according to any one of claims 1 to 11, further comprising (E) a curing agent other than the (B) active ester-based curing agent.
13. The resin sheet according to claim 12, wherein the curing agent (E) is a phenol-based curing agent.
14. The resin sheet according to any one of claims 1 to 13, which is for forming an insulating layer for forming a conductor layer.
15. The resin sheet according to any one of claims 1 to 14, which is for forming an insulating layer of a printed wiring board.
16. The resin sheet according to any one of claims 1 to 15, which is for forming an interlayer insulating layer of a printed wiring board.
Citation Information
Patent Citations
Thermosetting resin composition, resin film, and film-attached product
JP2006328214A
Method for producing laminate
JP2015085637A
Resin composition
JP2016027097A