Composite nonwoven fabric and its manufacturing method

The composite nonwoven fabric balances liquid absorption, strength, and comfort by optimizing fabric properties through a specific design and manufacturing process, ensuring suitability for medical and nursing care uses.

JP7578430B2Active Publication Date: 2024-11-06NIPPON PAPER CRECIA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020130232
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-31
Publication Date
2024-11-06
Estimated Expiration
2040-07-31

AI Technical Summary

Technical Problem

Existing composite nonwoven fabrics used in medical and nursing care settings face challenges in balancing liquid absorption performance, strength, and wiping comfort, as increasing pulp content for better absorption can compromise sheet strength and comfort.

Method used

A composite nonwoven fabric design with specific ranges for basis weight, drip water absorption, water retention, tensile strength, softness, smoothness, and stiffness, achieved through hydroentangling a pulp fiber web with a spunbond nonwoven fabric using an air-laid method, air-through drying, and calender treatment.

Benefits of technology

The fabric achieves excellent liquid absorption, strength, and wiping comfort, making it suitable for medical and nursing care applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578430000003
    Figure 0007578430000003
  • Figure 0007578430000001
    Figure 0007578430000001
  • Figure 0007578430000002
    Figure 0007578430000002
Patent Text Reader

Abstract

To provide a composite nonwoven fabric that is excellent all in liquid absorbability, strength, and feeling of wiping and suitable for use in medical settings and at the point of care.SOLUTION: A composite nonwoven fabric is formed by laminating a pulp fiber web PFW on a spun-bonded nonwoven fabric SW so as to integrate them. The composite nonwoven fabric has 50.0 to 80.0 g / m2 of basis weight, 0.5 to 2.0 seconds of drop water absorbency that is an indicator of liquid absorbability, 300 to 490 g / m2 of water capacity (T.W.A.) that is an indicator of liquid-holding capacity. The spun-bonded nonwoven fabric SW has 9.8 to 29.4 N / 25 mm of longitudinal tensile strength and 3.9 to 9.8 N / 25 mm of traverse tensile strength. The pulp fiber web PFW has 10.0 to 15.0 dBV2rms of TS7 value that is an indicator of softness of the pulp fiber web PFW and 25.0 to 50.0 dBV2rms of TS750 value that is an indicator of smoothness, and 1.6 to 2.5 mm / N of TSA (D value) that is an indicator of rigidity.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite nonwoven fabric obtained by hydroentangling a pulp fiber web and a spunbond nonwoven fabric, and more particularly to a composite nonwoven fabric suitable for use in medical and nursing care settings. [Background technology]

[0002] A composite nonwoven fabric made of a pulp fiber web and a spunbond nonwoven fabric has both the liquid absorption performance derived from the pulp fibers and the strength derived from the spunbond nonwoven fabric, and therefore has traditionally been widely used as hand towels, towels, and other personal wipers, but in recent years there has been increasing demand for it in medical and nursing care settings.

[0003] For example, as disclosed in Patent Document 1, a pulp fiber web and a spunbond nonwoven fabric are layered and then integrated by a hydroentanglement process in which a high-pressure water jet (water flow) is sprayed onto them. Here, the spunbond nonwoven fabric has excellent strength and functions as a backing layer for the composite nonwoven fabric produced. Meanwhile, the pulp fiber web has excellent liquid absorption performance. Therefore, such a composite nonwoven fabric can be provided to medical and nursing care sites as an excellent composite nonwoven fabric that combines the advantages of a pulp fiber web that has good absorbency for both aqueous and oil-based liquids and a spunbond nonwoven fabric that has excellent strength. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 2533260 Summary of the Invention [Problem to be solved by the invention]

[0005] In medical and nursing care settings, composite nonwoven fabrics are used when wiping the body of a patient or the like in a dry or moderately wet state. For this reason, it is important that such composite nonwoven fabrics have not only the above-mentioned liquid-absorbing performance, but also strength and a good wiping comfort. The above-mentioned liquid-absorbing performance can be evaluated by liquid-absorbing ability, which is the ability to quickly absorb liquid, and liquid-retentiveness, which is the ability to retain the absorbed liquid. However, for example, if the relative amount of pulp is increased to improve the liquid absorbency, the sheet strength and thickness of the composite nonwoven fabric increase, making the fabric harder to the touch and worsening the wiping comfort. In other words, simply increasing the amount of pulp to improve the liquid absorption performance can have a negative effect on the strength and wiping comfort, and it has not been easy to design a composite nonwoven fabric that is excellent in all of the liquid absorption performance, strength, and wiping comfort.

[0006] SUMMARY OF THE PRESENT DISCLOSURE An object of the present invention is to provide a composite nonwoven fabric which is excellent in all respects of liquid absorption performance, strength and wiping comfort and is suitable for use in medical and nursing care settings. [Means for solving the problem]

[0007] The above object is to provide a composite nonwoven fabric in which a pulp fiber web is laminated and integrated onto a spunbond nonwoven fabric, Basis weight: 50.0~80.0g / m 2 The drop absorbency, which is an index of liquid absorption, is 0.5 to 2.0 seconds, and the total water amount (TWA), which is an index of liquid retention, is 300 to 490 g / m 2 and the spunbonded nonwoven fabric has a longitudinal tensile strength of 9.8 to 29.4 N / 25 mm and a transverse tensile strength of 3.9 to 9.8 N / 25 mm; Furthermore, the TS7 value, which is an index showing the softness of the pulp fiber web, is 10.0 to 15.0 dBV. 2 rms, TS750 value which is an index of smoothness is 25.0-50.0dBV 2 This can be achieved by a composite nonwoven fabric characterized in that the rms and TSA (D value), which is an index of stiffness, are 1.6 to 2.5 mm / N.

[0008] And, it is preferable that the wet Taber value is 5 or more. The pulp fiber web has a basis weight of 30.0 to 70.0 g / m 2 At the same time, it is desirable that the weight composition ratio of the spunbond nonwoven fabric to the pulp fiber web is 30 / 70 to 10 / 90 (wt %).

[0009] The basis weight of the spunbond nonwoven fabric is 10.0 to 30.0 g / m 2 The spunbond nonwoven fabric is formed to include a plurality of fusion points that bond the spun resin fibers, and the area of ​​each fusion point is 0.10 to 0.50 mm 2 The area ratio of the fusion points per unit area is 7 to 20%, and the number of the fusion points is 10 to 150 / cm 2 It is desirable that:

[0010] The spunbond nonwoven fabric is preferably formed from one or a mixture of two or more materials selected from the group consisting of nylon, vinylon, polyester, acrylic, polyethylene, polypropylene, and polystyrene.

[0011] The pulp fiber web is preferably comprised of bleached kraft pulp fibers from a softwood selected from the group consisting of radiata pine, slash pine, southern pine, lodgepole pine, spruce, and Douglas fir.

[0012] The object of the present invention is to provide a method for producing any one of the composite nonwoven fabrics described above, The method includes at least a lamination step of supplying the pulp fiber web onto the spunbonded nonwoven fabric to form a laminate, a hydroentanglement step of promoting integration of the pulp fiber web and the spunbonded nonwoven fabric to obtain a laminate, and a drying step of drying the laminate after the hydroentanglement step, The object can be achieved by a method for producing a composite nonwoven fabric, which is characterized in that an air-laid method is adopted in the lamination step, and an air-through dryer is adopted in the drying step. It is more preferable to carry out a calendar treatment after the drying step. Effect of the Invention

[0013] According to the present invention, a composite nonwoven fabric that is excellent in all respects of liquid absorption performance, strength, and wiping comfort and is suitable for use in medical and nursing care settings can be provided. Moreover, according to the manufacturing method of the present invention, the composite nonwoven fabric can be manufactured. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram showing a manufacturing apparatus for a composite nonwoven fabric. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, a composite nonwoven fabric according to one embodiment of the present invention will be described. The inventors of the present application have conducted extensive research into composite nonwoven fabrics suitable for use in medical and nursing care settings, and have developed a method for determining the basis weight (g / m 2 ), drop absorbency (sec), which is an index of liquid absorption, and water retention capacity (g / m 2 ), the tensile strength (N / 25mm) of the spunbond nonwoven fabric in both the vertical and horizontal directions, and the softness (TS7 value (dBV 2 rms), smoothness (TS750 value (dBV 2 The present invention was arrived at by confirming that a composite nonwoven fabric designed so that the TSA (rms) and stiffness (TSA (D value) (mm / N)) are within a specified range is excellent in all respects of liquid absorption performance, strength, and wiping comfort. It is preferable to manufacture such a composite nonwoven fabric by using an air-laid method in the lamination process in which a pulp fiber web is supplied onto a spunbond nonwoven fabric to form a laminate, and by using an air-through dryer in the drying process. It is more preferable to manufacture the composite nonwoven fabric by carrying out a calendar treatment after the drying process. The composite nonwoven fabric of the present invention can be excellent in all respects of absorbency, strength, and wiping comfort by designing each of the above-mentioned components to fall within a specified range, even when the relative amount of the pulp fiber web is increased to enhance absorbency, for example.

[0016] The basis weight of the composite nonwoven fabric according to the present invention is 50.0 to 80.0 g / m 2 , preferably 60.0 to 70.0 g / m 2 is set to. The drop absorbency is 0.5 to 2.0 seconds and the water retention capacity (TWA: Total Water Absorbency) is 300 to 490 g / m 2 The drop water absorbency is set at 100%. The drop water absorbency is based on the water absorption rate test specified in JIS L 1907, and can be obtained by measuring the time (seconds) from when a 0.1 ml water drop reaches the surface of the test piece until the mirror reflection of the test piece disappears. The TWA can be obtained as follows. First, the nonwoven fabric is cut into a 75 x 75 mm square to prepare a test piece, and the dry weight is measured. Next, the test piece is immersed in distilled water for 2 minutes, and then the test piece is hung in a container saturated with water vapor so that one corner of the test piece becomes the top, and this top and the two adjacent corners are supported and hung in a stretched state (100% RH), and the test piece is left for 30 minutes and the weight after draining is measured. A paper towel cut to 3 x 38 mm is used for draining. The measured value is then measured for 1 m of the test piece. 2 Water retention per unit (g / m 2 ) can be obtained by converting

[0017] The longitudinal tensile strength of the spunbond nonwoven fabric is set to 9.8 to 29.4 N / 25 mm, and the transverse tensile strength is set to 3.9 to 9.8 N / 25 mm. Here, the composite nonwoven fabric is cut into strips with a width of 25 mm, and the strength is measured in the longitudinal direction (MD: the feed direction during production) and the transverse direction (CD: the width direction perpendicular to the MD) using a tensile tester.

[0018] Furthermore, the TS7 value, which indicates the softness of the pulp fiber web side, which are important factors for composite nonwoven fabrics, is set to 10.0 to 15.0, the TS750 value, which indicates smoothness, is set to 25.0 to 50.0, and the TSA (D value), which indicates rigidity, is set to 1.6 to 2.5.

[0019] The above TS7 value, TS750 value, and TSA (D value) were measured using a tissue softness analyzer (TSA). The TSA tissue softness analyzer quantitatively evaluates the softness (hand feel) of nonwoven fabrics and the like by pressing a bladed rotor, for example, with a pressing pressure of 100 mN against a composite nonwoven fabric (sample) placed on a sample stage with the pulp side facing up and rotating at 2.0 / sec. Vibration data detected by various sensors is analyzed and parameterized (TS value), and the softness (hand feel) of nonwoven fabrics and the like is evaluated. This is the product name of Emtec Electronic GmbH of Germany (Japan distributor is Nippon Luft Co., Ltd.). In measurements using the above-mentioned tissue softness measuring device TSA, for example, the vibration of the sample stage is measured by a vibration sensor installed inside the sample stage, and the vibration frequency is analyzed and parameterized (TS value). The vibration frequency depends on the structural dimensions of creep processing, embossing processing, etc., and the rotation speed of the blade. The induction of horizontal vibration of the blade itself (resonant frequency: for example, 6500 Hz) occurs when the blade advances over the surface of the sample, due to momentary interruption by a convex part of the sample and the vibration of the blade. The intensity of the first maximum peak in the spectrum from the low frequency side is expressed as the TS750 value (dBV 2 rms), and the intensity of the maximum peak in the spectrum including the resonance frequency of 6500 Hz (around 6500 Hz) is the TS7 value (dBV 2 rms). Furthermore, without rotating the bladed rotor, the sample is deformed, for example, with a pressing pressure of 100 mN and 600 mN, and the amount of deformation (mm / N) in the vertical direction is measured as the TSA (D value).

[0020] The software for analyzing vibration and parameterizing (TS value) can be the emtec measurement system. This software is equipped with various algorithms (e.g., Base Tissue, Facial, TP, etc.), and the above TS7 value, TS750 value, and TSA (D value) are automatically obtained on the software, and the HF (hand feel) value is calculated from these TS7 value, TS750 value, and TSA (D value) or basis weight, thickness, number of plies, etc., depending on the type of algorithm. In the present invention, the TS7 value, TS750 value, and TSA (D value) are specified instead of the HF value, and any algorithm can be used as long as the measurement conditions are met, and the TS7 value, TS750 value, and TSA (D value) do not change depending on the type of algorithm.

[0021] As shown above, the basis weight (g / m 2 ), drip water absorption (sec), water retention amount (g / m 2 ), the tensile strength (N / 25mm) of the spunbond nonwoven fabric in both the vertical and horizontal directions, and the softness (TS7 value (dBV 2 rms), smoothness (TS750 value (dBV 2 The composite nonwoven fabric of the present invention is designed so that the linearity (TSA (D value) (mm / N)) and stiffness (TSA (D value) (mm / N)) are within predetermined preferred ranges, and is excellent in all respects of liquid absorption performance, strength and wiping comfort, making it a suitable composite nonwoven fabric for use in medical and nursing care settings. Furthermore, it is preferable that the abrasive is designed so that the wet Taber value, which is an index of durability, is 5 times or more. Using a Taber tester specified by JIS, a sample moistened with water is attached to a rotating horizontal disk, and a pair of friction wheels formed of abrasive grain combination is applied under a specified load, and it is preferable that the abrasion resistance is such that the wet Taber value is at least 5 times.

[0022] The basis weight of the pulp fiber web is 30.0 to 70.0 g / m 2and the weight composition ratio of the spunbond nonwoven fabric to the pulp fiber web is preferably 30 / 70 to 10 / 90 (wt%). A material within this range has excellent water absorption performance and a good feel in the hand, and also contributes to the shape stability of the composite nonwoven fabric. In the composite nonwoven fabric of the present invention, the pulp fiber web has a relatively large basis weight, but by adjusting the basis weight of the spunbond nonwoven fabric, the strength of the composite nonwoven fabric required in medical and nursing care sites is ensured. The basis weight of the spunbond nonwoven fabric is 10.0 to 30.0 g / m 2 In addition, the spunbond nonwoven fabric is formed to include a plurality of fusion points that bond the spun resin fibers, and the area of ​​each of the fusion points is preferably 0.10 to 0.50 mm. 2 The area ratio of fusion points per unit area is 7-20%, and the number of fusion points is 10-150 / cm 2 Such a spunbonded nonwoven fabric has an appropriate rigidity and is suitable for use as a spunbonded nonwoven fabric to be combined with a pulp fiber web to form a composite nonwoven fabric. The shape of the fusion points is not particularly limited and may be circular, elliptical, polygonal, etc.

[0023] The spunbond nonwoven fabric is preferably made of one or a mixture of two or more materials selected from the group consisting of nylon, vinylon, polyester, acrylic, polyethylene, polypropylene, and polystyrene. Among these, polypropylene is preferably used. Furthermore, it is preferable to use the pulp fiber web formed from bleached kraft pulp fibers of a softwood selected from the group consisting of radiata pine, slash pine, southern pine, lodgepole pine, spruce and Douglas fir.

[0024] The steps of producing the composite nonwoven fabric of the present invention described above are described below. The composite nonwoven fabric of the present invention is preferably produced by adopting an air-laid method in the lamination step and an air-through dryer in the drying step. Furthermore, it is preferable to perform a calendaring process after the drying step. The production apparatus for producing the composite nonwoven fabric WP of the present invention is described in detail below.

[0025] 1, a composite nonwoven fabric manufacturing apparatus 1 is provided with an airlaid device 2 on the upstream side, a spunbond supplying device 3 that supplies a spunbond nonwoven fabric, and a suction device 4. The suction device 4 is disposed below the airlaid device 2 so as to face it. In the web transport direction TD, downstream of these devices 2, 3, and 4, there are arranged, in this order from the upstream side, a hydroentanglement device 5 that sprays water jets for hydroentanglement treatment, a suction device 6, and a drying device 7. Downstream of the drying device 7, there is further provided a winding device 8 for winding up the composite nonwoven fabric WP that is continuously produced.

[0026] The airlaid apparatus 2 includes a defibrator 21 that defibrates raw pulp RP, which is a sheet-like material in which fibers are densely packed together, into pulp fibers, and a duct 22 that is equipped with a blower (not shown) and transports the defibrated pulp fibers PF to an airlaid hopper 23.

[0027] Additionally, an airlaid hopper 23 is disposed downstream of the duct 22. Inside this airlaid hopper 23, the pulp fibers in a defibrated state drop while being dispersed, and are designed to gradually pile up at a stacking position 24 set on the lower surface to form a pulp fiber web PFW. In the manufacture of the composite nonwoven fabric according to the present invention, it is preferable to supply the pulp fiber web by the airlaid method as described above. Manufacturing in this manner ensures the bulk that contributes to liquid absorption and liquid retention. A suction device 4 is disposed facing the lower side of the stacking position 24. More specifically, the suction device 4 has a suction section 42 on the upper surface of an apparatus main body 41, and the suction section 42 is set with respect to the stacking position 24 so as to apply a suction force (negative pressure) to the pulp fiber web PFW. 1 shows an example in which the pulp fiber web PFW is formed by arranging the airlaid hopper 23 and the suction device main body 41 in a single stage. However, the present invention is not limited to this, and the airlaid hopper 23 and the suction device main body 41 may be arranged in two or more stages depending on the basis weight (basis weight) and production speed of the pulp fiber web PFW.

[0028] A transport wire 43 for transporting the web is disposed around the suction device 4. The transport wire 43 is disposed so that the pulp fiber web PFW on which the pulp fibers PF are accumulated at the stacking position 24 can be placed and transports the web downstream. However, the pulp fiber web PFW is not placed directly on the transport wire 43. This will become clear from the explanation given later. The conveying wire 43 is formed in an open mesh shape so that the suction force of the suction portion 42 extends to the opposite side (upper side).

[0029] A spunbond supplying device 3 is disposed below the airlaid device 2 and upstream of the suction device 4. A roll of spunbond nonwoven fabric SW that has been prepared in advance is set in this spunbond supplying device 3. The spunbond nonwoven fabric SW is pulled out from the spunbond supplying device 3 and transported to the layering position 24 on the transport wire 43 described above. As the spunbond nonwoven fabric SW, it is preferable to use a web of continuous filaments of a synthetic resin formed by a spunbonding method.

[0030] The above-mentioned pulp fiber web PFW is placed on the spunbond nonwoven fabric SW located at the stacking position 24 (stacking step). At this time, the suction force by the suction section 42 of the suction device 4 passes through the conveying wire 43 at the stacking position 24 and acts on the spunbond nonwoven fabric SW and the pulp fiber web PFW thereon. Thus, the preliminary laminate PWeb in which the spunbond nonwoven fabric SW and the pulp fiber web PFW are stacked is conveyed downstream.

[0031] The above-mentioned preliminary laminate PWeb is maintained in a laminated state by being suction-compressed by the suction force of the suction device 4. At this time, the fibers of the upper pulp fiber web PFW are in a dense state. However, if the preliminary laminate PWeb is transported and fed into the downstream hydroentangling device 5 in this state, there is a risk that a part of the pulp fibers PF will be blown up by the water jet (high-pressure water flow). Therefore, in the present manufacturing apparatus 1, there are provided clamping rollers 28 for sandwiching the preliminary laminate PWeb from above and below to stabilize the placement state of the pulp fiber web PFW on the spunbond nonwoven fabric SW, and a pre-wetting device 30 for applying moisture to prevent the fibers from scattering upstream of the hydroentangling device 5. The pre-wetting device 30 preferably includes a spray nozzle 31 for spraying water mist from above the preliminary laminate PWeb, and a suction device 32 for applying suction force from the underside of the preliminary laminate PWeb (i.e., the underside of the pulp fiber web PFW). 1 shows an example in which the pre-wetting device 30 is provided as a new device before the hydroentanglement device 5 as described above, but the present invention is not limited to this. The design of the hydroentanglement device 5 may be modified so that the first set of a plurality of sets each consisting of a water jet head 51 and a suction device 52 (described later) is used as the pre-wetting device 30. In this case, adjustments may be made so that low-pressure water mist is sprayed from the first water jet head 51. In the case of a hydroentanglement device 5 that has a sufficient number of sets of water jet heads 51 and suction devices 52 to perform the hydroentanglement treatment, using the leading water jet head 51 and suction device 52 as a pre-wetting device as described above is effective in reducing equipment costs.

[0032] Then, in the hydroentangling device 5, entangling of the pulp fibers is promoted by spraying a high-pressure water jet onto the preliminary laminate PWeb that has been treated by the clamping rollers 28 and the pre-wetting device 30, which are the pre-treatment section. This promotes integration of the pulp fiber web PFW layer located on the upper side with the spunbond nonwoven fabric SW layer located on the lower side. The hydroentangling device 5 exemplarily shown in FIG. 1 has water jet heads 51 arranged in multiple stages (four stages are shown in FIG. 1) along the conveyance direction TD. 1 does not show the nozzles provided on the water jet head 51 extending in the direction perpendicular to the conveying direction TD (the width direction of the web), but multiple water jet nozzles are arranged at appropriate positions in the width direction. The hole diameter φ of the water jet nozzle is preferably 0.06 to 0.15 mm. The interval between the water jet nozzles is preferably 0.4 to 1.0 mm.

[0033] The water pressure during the hydroentanglement treatment is desirably set in consideration of the basis weights of the pulp fiber web PFW and the spunbond web SW, and is preferably selected within the range of, for example, 1 to 30 MPa.

[0034] A suction device 52 is disposed opposite the water jet head 51. A high-pressure water jet from the water jet head 51 is sprayed onto the pulp fiber web PFW located on the upper side, while the suction force of the suction device 52 is applied to the lower side of the spunbond nonwoven fabric SW located on the lower side. It is presumed that the cooperative action of the water jet head 51 and the suction device 52 creates a state in which the pulp fibers on the pulp fiber web PFW side penetrate into the spunbond nonwoven fabric SW on the lower side, or penetrate through the spunbond nonwoven fabric SW to reach the opposite side. This action promotes integration of the two layers.

[0035] The hydroentangling device 5 is also provided with a conveying wire 55. The conveying wire 55 receives the preliminary laminate PWeb downstream of the pre-treatment units 28 and 30, and conveys it into the hydroentangling device 5. The conveying wire 55 is provided so as to pass between the water jet head 51 and the suction device 52 of the hydroentangling device 5 from the upstream side to the downstream side. Therefore, the preliminary laminate PWeb transported on the transport wire 55 undergoes more hydroentanglement treatment as it moves downstream in the transport direction TD, and by the time it leaves the hydroentanglement device 5, sufficient entanglement treatment is achieved between the upper pulp fiber web PFW layer and the lower spunbond nonwoven fabric SW layer. Immediately after leaving the hydroentangling device 5, the nonwoven fabric is in a wet state, and the bonds between the pulp fibers etc. are not yet sufficiently established.

[0036] 1, a suction device 6 and a dryer 7 are provided downstream of the hydroentanglement device 5 to remove residual moisture from the web by suction and then dry the web to complete the production of the composite nonwoven fabric WP. By performing dehydration and drying using the suction device 6 and the dryer 7 in this manner at the latter stage of the production of the composite nonwoven fabric WP, the nonwoven fabric can be produced efficiently, and the nonwoven fabric can be dried without applying a large external pressure to the hydroentangled nonwoven fabric, resulting in a finished product with a sense of bulk. The suction device 6 is, for example, a vacuum type, and dehydrates the nonwoven fabric after hydroentanglement. The drying device 7 is preferably a non-compression type dryer, preferably an air-through dryer. In Fig. 1, the rotatable dryer body 71 of the air-through dryer is a cylindrical body, and a number of through holes are provided on its peripheral surface, and it is preferable that hot air heated by a heat source (not shown) is sucked from the outer periphery of the dryer body toward the center. In the production of the composite nonwoven fabric according to the present invention, as described above, it is preferable to use an air through dryer as the drying device 7. By producing the composite nonwoven fabric in this manner, it is possible to further ensure the bulk that contributes to the liquid absorption and retention properties.

[0037] The composite nonwoven fabric WP continuously produced as described above is generally wound onto a roll 81 of a winding device 8 after drying, but in the manufacturing apparatus shown in FIG. 1, a calender device CA is disposed between the drying device 7 and the winding device 8 as a post-processing device. A pair of plain calendar rolls (not shown) are disposed within the calender device CA, and the composite nonwoven fabric WP is conveyed between them while being clamped with a linear pressure (clamping pressure) within a predetermined range. The plain calender roll that can be used here is not particularly limited in material, so long as it has a flat outer peripheral surface and can apply a stable and uniform linear pressure to the nonwoven fabric WP after the composite treatment. For example, a pair of calender rolls can be preferably used, in which one is a plain metal roll and the other is a metal-rubber plain roll in which a rubber material is provided on the outside of a metal core material. The metal roll and the metal core material can be, for example, a steel roll, and the rubber material can be, for example, a special hard rubber.

[0038] In the calendering device CA, the calendering is performed, for example, by setting the roll temperature at 40 to 100° C., the gap between the rolls at 0 to 0.3 mm, preferably 0.1 to 0.3 mm, and a linear pressure of 1 to 30 kg / cm on the composite nonwoven fabric WP passing between the rolls. Calendering under such conditions can provide a composite nonwoven fabric having a smooth surface and satisfactory usability and abrasion resistance, even if the ratio of the pulp fiber web is relatively high. If necessary, the pair of plain calender rolls may be arranged in multiple stages in the calender device CA so that the calendering process can be carried out in multiple stages.

[0039] FIG. 1 shows an example in which a calendering device CA is preferably added online. It is preferable to provide the calendering device CA integrally with the nonwoven fabric wiper manufacturing apparatus in this manner. However, it is also possible to first take up the nonwoven fabric wiper WP around a roller 81 and then perform calendering offline using a separately provided calendering device CA.

[0040] (Example) The composite nonwoven fabrics of the examples produced by the embossing process using the above-mentioned production apparatus will be described below. The composite nonwoven fabrics of Examples 1 to 7 and Comparative Examples 1 to 4 were manufactured so as to have the basis weight, water drop absorbency, water retention (TWA), tensile strength in the machine direction (DMD) and cross direction (DCD) of the spunbond nonwoven fabric (SB), TS7 value indicating softness, TS750 value indicating smoothness, and TSA (D value) indicating stiffness as shown in Table 1. The softness and smoothness were evaluated sensorily according to the following criteria as indicators for judging the wiping comfort when the composite nonwoven fabric is used for body wiping according to the following criteria. 1) Softness: Evaluate the softness when wiping the body Moderate flexibility and stiffness make it easy to wipe (Excellent ◎), No problem with ease of wiping (Good 〇), Too soft and lacking stiffness, difficult to wipe (Poor × 1), Too hard and lacking flexibility, difficult to wipe (Poor × 2) 2) Dryness: Evaluate the dryness of the skin surface when wiping the body. The skin surface after wiping is particularly smooth and excellent (Excellent ◎), the skin surface after wiping remains smooth (Good 〇), the skin surface after wiping is sticky (Not Good ×)

[0041] [Table 1]

[0042] [Table 2]

[0043] As shown in Table 1 above, Examples 1 to 7 can be provided as products, but as shown in Table 2 above, Comparative Examples 1 to 4 are out of the specified range in any one of the following: basis weight, drop absorbency, water retention (TWA), tensile strength in the machine direction (DMD) and cross direction (DCD) of the spunbond nonwoven fabric (SB), TS7 value indicating softness, TS750 value indicating smoothness, and TSA (D value) indicating stiffness.

[0044] The above Examples 1 to 7 have a basis weight of 50.0 to 80.0 g / m 2, drop water absorption is 0.5 to 2.0 seconds and water retention (TWA) is 300 to 490g / m 2 The tensile strength of the spunbond nonwoven fabric is 9.8-29.4N / 25mm and the tensile strength of the cross section is 3.9-9.8N / 25mm, and the TS7 value indicating softness is 12.0-20.0dBV. 2 rms, TS750 value indicating smoothness is 33.0-71.0dBV 2 The rms and TSA (D value) are within the preferred range of 1.6 to 2.5 mm / N.

[0045] In Comparative Example 1, the softness was evaluated as ◯, but the dryness was evaluated as ×, and the wiping comfort was poor. The basis weight of this composite nonwoven fabric was 40 g / m 2 and 50.0 g / m 2 It has a drop water absorption of 5.6 seconds and a water retention capacity (TWA) of 262g / m 2 This composite nonwoven fabric is relatively light and has low liquid absorption performance, making it unsuitable for use in medical or nursing care settings. In addition, the TS7 value of Comparative Example 2 exceeds the preferred range, and the fabric is hard and lacks flexibility, making wiping difficult. The TS7 value of Comparative Example 4 exceeds the preferred range, and the fabric is hard and lacks flexibility, and also has low drip absorbency, making wiping difficult and poor in liquid wiping performance. Therefore, the fabric is not suitable as a composite nonwoven fabric for use in medical or nursing care settings. In addition, in Comparative Example 3, the strength of the spunbond nonwoven fabric (SB) used was weak, resulting in a composite nonwoven fabric that was too soft and lacked stiffness. This composite nonwoven fabric was too soft and difficult to wipe off. Therefore, it was not suitable for use in medical or nursing care settings.

[0046] This concludes the description of the embodiment, but it goes without saying that the present invention is not limited to the above embodiment, and can be implemented with various modifications without departing from the spirit of the present invention. [Explanation of symbols]

[0047] 1. Composite nonwoven fabric manufacturing equipment 2 Air Raid Equipment 3 Spunbond nonwoven fabric supply device 4 Suction device 5 Hydro-entangling device 6 Suction device 7 Drying equipment 8 Winding device 21 Fiberizer 22 Duct 23 Air Raid Hopper 24 Stacking position 28 Clamping roller 30 Pre-wetting device 31 Spray nozzle 32 Suction device 41 Suction device main body 42 Suction section 43 Transport Wire 51 Water Jet Head 52 Suction device 55 Transport Wire SW spunbond nonwoven fabric PF pulp fiber PFW Pulp Fiber Web PWeb Pre-Laminate (Laminate Web) WP composite nonwoven fabric TD Transport direction CA Calendar Device

Claims

1. A method for producing a composite nonwoven fabric comprising integrating a pulp fiber web, which is formed by laminating pulp fibers on a spunbond nonwoven fabric, the method comprising the steps of: a lamination step of supplying pulp fibers onto the spunbond nonwoven fabric to form the pulp fiber web; a hydroentanglement step for promoting integration of the pulp fiber web and the spunbonded nonwoven fabric to obtain a laminate; a drying step of drying the laminate after the hydroentanglement step; a step of subjecting the laminate to a calendar treatment after the drying step; At least The lamination step employs an air-laid method, and the drying step employs an air-through dryer; The calendering is performed by setting the temperature of rolls in a calender device to 40 to 100° C., the gap between rolls to 0.1 mm to 0.3 mm, and a linear pressure of 1 to 30 kg / cm applied to the laminate passing through the gap between rolls, The composite nonwoven fabric is Basis weight: 50.0 to 80.0 g / m 2 The drop absorbency, which is an index of liquid absorbency, is 0.5 to 2.0 seconds, and the water retention amount (T.W.A.), which is an index of liquid retention, is 300 to 490 g / m 2 and the spunbond nonwoven fabric has a longitudinal tensile strength of 9.8 to 29.4 N / 25 mm and a transverse tensile strength of 3.9 to 9.8 N / 25 mm; Furthermore, the TS7 value, which is an index showing the softness of the pulp fiber web, is 10.0 to 15.0 dBV. 2 TS750 value, which is an index of rms and smoothness, is 25.0 to 50.0 dBV 2 A method for producing a composite nonwoven fabric, characterized in that the rms and TSA (D value), which is an index of stiffness, are 1.6 to 2.5 mm / N.

2. 2. The method for producing a composite nonwoven fabric according to claim 1, wherein the wet Taber value is 5 or more.

3. The pulp fiber web has a basis weight of 30.0 to 70.0 g / m 2 3. The method for producing a composite nonwoven fabric according to claim 1, wherein the weight ratio of the spunbond nonwoven fabric to the pulp fiber web is 30 / 70 to 10 / 90 (wt %).

4. The spunbond nonwoven fabric has a basis weight of 10.0 to 30.0 g / m 2 The spunbond nonwoven fabric is formed to include a plurality of fusion points that bond the spun resin fibers, and the area of ​​each fusion point is 0.10 to 0.50 mm 2 The area ratio of the fusion points per unit area is 7 to 20%, and the number of the fusion points is 10 to 150 / cm 2 The method for producing a composite nonwoven fabric according to any one of claims 1 to 3, characterized in that

5. The method for producing a composite nonwoven fabric according to any one of claims 1 to 4, characterized in that the spunbond nonwoven fabric is formed of one type or a mixture of two or more types selected from the group consisting of nylon, vinylon, polyester, acrylic, polyethylene, polypropylene and polystyrene.

6. The method for producing a composite nonwoven fabric according to any one of claims 1 to 5, characterized in that the pulp fiber web is made of fibers of bleached kraft pulp from a softwood selected from the group consisting of radiata pine, slash pine, southern pine, lodgepole pine, spruce and Douglas fir.

Citation Information

Patent Citations

  • Nonwoven fabric sheet for wiping human

    JP2016089277A

  • Conjugate type nonwoven fabric and method for producing the same

    JP2020105656A

  • Nonwoven composite fabric with high pulp content

    JP2533260B2