Fluoride-free waterproof moisture-permeable nanofiber membrane and preparation method thereof
By introducing three-dimensional interoperable pore structures and hydrophobic microbeads into the nanofiber membrane, the problems of high production cost and low hydrostatic pressure resistance of nanofiber membranes are solved, and the effects of fluorine-free environmental protection and excellent waterproof and moisture-permeable performance are achieved.
Patent Information
- Application Number
- CN202410899009.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
Smart Images

Figure CN118880550A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrostatic spinning nanofiber membranes, and specifically relates to a fluorine-free waterproof and moisture-permeable nanofiber membrane and a preparation method thereof. Background Art
[0002] Waterproof and breathable membrane is a high-performance film that integrates excellent waterproof, breathable and breathable functions. According to the breathability mechanism, waterproof and breathable membranes can be divided into non-porous membranes and microporous membranes. The waterproof and breathable mechanism of hydrophilic non-porous membranes is a non-porous diffusion mechanism. The more common one is thermoplastic polyurethane (TPU) membrane. The non-porous membrane is cheap, but the air permeability is extremely poor. Microporous membranes achieve selective permeation of water droplets / water molecules through the pore size screening effect. Common microporous films include polytetrafluoroethylene (PTFE) membranes, nanofiber membranes, etc. The preparation technology of PTFE microporous membranes is mature and has a high market share, but the film has poor elasticity, and PTFE is not easy to degrade and has the characteristics of long-distance migration, which will have adverse effects on the human body and the environment. The nanofiber membrane prepared by electrospinning technology has the advantages of small pore size, high pore size ratio and large specific surface area. The raw material selection is flexible, which is convenient for giving the membrane functionality and easy to construct a multi-faceted surface structure. In recent years, it has been gradually applied to wearable waterproof and breathable membranes. However, nanofiber membranes have the disadvantages of easy sliding and average water resistance. The common solution is to add fluorine-containing compounds to improve the hydrophobicity and water resistance of the membrane material, but this also brings environmental problems. Therefore, it is particularly important to develop a new type of environmentally friendly waterproof and breathable membrane.
[0003] Patent CN 110438659 A discloses a method for preparing a waterproof and breathable nanofiber composite membrane. Polyacrylonitrile is used as the main raw material, polyvinylidene fluoride and polyurethane are added, and a hydrophobic waterproof and breathable membrane is obtained by solution blending and spinning. Polypropylene gives the membrane the characteristics of high porosity, fine fiber diameter, and small pore size. The hydrophobic groups of polyvinylidene fluoride and polyurethane give the membrane a certain hydrophobicity, but its resistance to hydrostatic pressure is generally low.
[0004] Patent CN 104562444 A provides a method for preparing an electrostatically sprayed nano spider web waterproof and breathable membrane. In the electrostatic spraying, the droplets are sprayed in a reverse airflow parallel to the spray direction of the polymer emulsion droplets, causing the droplets to deform under force when flying in the electric field to form a liquid film, and then phase separation to form a two-dimensional mesh material with a stable hexagonal mesh structure. The nano spider web waterproof and breathable membrane has a spider web coverage area of 100%, good structural integrity, an average pore size of 10 to 200 nm, and a porosity of ≥80%. This method has low production efficiency, poor fiber strength, and is easy to stratify and rupture.
[0005] Patent CN 117587577 A provides a waterproof and breathable membrane and its preparation method and application. It uses a nanofiber membrane as a substrate, and uses a blocked solvent-based isocyanate crosslinker to crosslink with the active groups in the waterproofing agent after unblocking, so that the hydrophobic segments are stably coated on the fiber surface, thereby improving the durability of the waterproofing agent coating. After 50 wear cycles, the contact angle did not change significantly, and the hydrostatic pressure resistance and moisture permeability flux remained basically unchanged after 30 washes, but the use of the crosslinker greatly increased the production cost.
[0006] In order to meet the needs of production and practical applications, providing a fluorine-free waterproof and breathable membrane with low cost and good waterproof and breathable properties has become a current research hotspot. Summary of the invention
[0007] The nanofiber membranes prepared by the prior art have the problems of high production cost, low efficiency, low hydrostatic pressure resistance, etc. In view of the problems existing in the prior art, the purpose of the present invention is to provide a fluorine-free waterproof and breathable nanofiber membrane with low cost and good waterproof and breathable properties and a preparation method thereof.
[0008] The method for preparing the fluorine-free waterproof and breathable nanofiber membrane provided by the present invention comprises the following steps:
[0009] 1) Using N,N-dimethylformamide (DMF) and tetrahydrofuran (THF) as solvents and thermoplastic polyurethane (TPU) as solute, magnetic stirring is performed to obtain solution A;
[0010] 2) using THF as solvent and polydimethylsiloxane (PDMS) (the ratio of main agent to curing agent is 10:1) as solute, and ultrasonically dispersing to obtain solution B;
[0011] 3) mixing the above solution A and solution B, adding DMF and THF, and magnetically stirring to obtain spinning solution C;
[0012] 4) placing the spinning solution C into a needle tube, and performing high-voltage electrospinning to obtain a nanofiber membrane D, and forming hydrophobic microbeads by introducing a three-dimensional interconnected pore structure into the nanofiber membrane to construct a Wenzel model;
[0013] 5) The nanofiber membrane D is subjected to heat pressing to obtain a nanofiber membrane E.
[0014] In step 1) of the above method, the mass ratio of DMF to THF is 7:3 to 3:7, specifically 7:3, 6:4, 5:5, 4:6 and 3:7, etc. In the solution A, the mass concentration of TPU can be 10wt% to 50wt%, and the magnetic stirring time can be 6 to 8h, specifically 6h or 8h.
[0015] In step 2), the mass concentration of PDMS may be 30 wt% to 60 wt%;
[0016] In step 3) of the above method, in the spinning solution C, the total mass concentration of TPU and PDMS is 15wt% to 25wt% (specifically 20%, 16%, 24%, etc.), wherein the mass ratio of TPU to PDMS is 2:3 to 3:2; the mass ratio of DMF to THF can be 7:3 to 3:7;
[0017] In step 4) of the above method, the voltage of the electrospinning is 16-20 kV, the distance between the needle and the receiving device is 10-20 cm, the propulsion speed is 0.5-1.5 mL / h; and the time of the electrospinning is 1-3 h.
[0018] In step 5) of the above method, the temperature of the hot pressing treatment is 60 to 90° C. and the time is 0.5 to 1.5 min.
[0019] The fluorine-free waterproof and breathable nanofiber membrane prepared by the above method also belongs to the protection scope of the present invention.
[0020] The beneficial effects of adopting the above technical solution are:
[0021] (1) The present invention introduces an appropriate amount of hydrophobic microbeads into the three-dimensional interconnected pore structure of the nanofiber membrane to construct a Wenzel model, thereby effectively improving the hydrophobicity of the film.
[0022] (2) The present invention adopts a one-step molding method to simultaneously spin out nanofibers and microbeads, thereby achieving real-time and uniform mixing of nanofibers and microbeads. The process is simple, the production efficiency is high, and the application range is wide.
[0023] (3) The nanofiber membrane provided by the present invention is fluorine-free and environmentally friendly, and has excellent waterproof and moisture permeability. The hot pressing treatment significantly improves the hydrostatic pressure resistance of the film. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The present invention is a flow chart for preparing the fluorine-free waterproof and breathable nanofiber membrane;
[0025] Figure 2 Surface SEM images of the fluorine-free waterproof and breathable nanofiber membranes prepared in Example 2, Example 4, and Comparative Example 2 of the present invention;
[0026] Figure 3 The water contact angle comparison results of the fluorine-free waterproof and breathable nanofiber membranes prepared in Examples 2, 4 and 6 of the present invention and the nanofiber membranes prepared in Comparative Examples 1 and 2;
[0027] Figure 4The waterproof and moisture permeability properties of the fluorine-free waterproof and moisture permeable nanofiber membranes prepared in Examples 2, 4 and 6 of the present invention are compared with those of the nanofiber membranes prepared in Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0028] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0029] The experimental methods in the following examples, unless otherwise specified, are all conventional methods, and are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0030] according to Figure 1 The preparation flow chart is used to prepare the fluorine-free waterproof and breathable nanofiber membrane of the present invention.
[0031] Example 1
[0032] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0033] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a solution B with a mass concentration of 50 wt%;
[0034] (3) 4 g of solution A and 1.6 g of solution B were mixed, 1.96 g of DMF and 2.44 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 16 wt %; TPU:PDMS=1:1; DMF:THF=1:1;
[0035] (4) adding the electrospinning solution into the needle tube, and obtaining the nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0036] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0037] The water contact angle of the prepared moisture-permeable nanofiber membrane is 134.9° and the moisture permeability is 13400 g / m 2 ·d, hydrostatic pressure resistance is 70kPa.
[0038] Example 2
[0039] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0040] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0041] (3) 5 g of solution A and 2 g of solution B were mixed, 1.2 g of DMF and 1.8 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=1:1, DMF:THF=1:1;
[0042] (4) adding the electrospinning solution into the needle tube, and obtaining the nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0043] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0044] The water contact angle of the waterproof and breathable nanofiber membrane is 132.8° and the moisture permeability is 12700 g / m 2 ·d, hydrostatic pressure resistance is 75.6kPa.
[0045] Example 3
[0046] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0047] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50% solution B;
[0048] (3) 6 g of solution A and 2.4 g of solution B were mixed, 0.44 g of DMF and 1.16 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 24 wt%, TPU:PDMS=1:1, DMF:THF=1:1;
[0049] (4) placing the electrospinning solution into a needle tube and obtaining a nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0050] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0051] The water contact angle of the waterproof and breathable nanofiber membrane is 128.9° and the moisture permeability is 12400 g / m 2 d, hydrostatic pressure resistance is 72.4 kPa.
[0052] Example 4
[0053] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0054] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0055] (3) 5 g of solution A and 2 g of solution B were mixed, 2.8 g of DMF and 0.2 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=1:1, DMF:THF=7:3;
[0056] (4) adding the electrospinning solution into the needle tube, and obtaining the nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0057] (5) The nanofiber membrane is subjected to a heat press treatment at 90° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0058] The water contact angle of the waterproof and breathable nanofiber membrane is 128.6° and the moisture permeability is 10800 g / m 2 ·d, hydrostatic pressure resistance is 68.8kPa.
[0059] Example 5
[0060] (1) 8.4 g DMF and 3.6 g THF were used as solvents, 8 g TPU was used as solute, and magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 40 wt%;
[0061] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0062] (3) 2.5 g of solution A and 2 g of solution B were mixed, 1.35 g of DMF and 4.15 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=1:1, DMF:THF=3:7;
[0063] (4) placing the electrospinning solution into a needle tube and obtaining a nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0064] (5) The nanofiber membrane is subjected to a heat press treatment at 60° C. for 1 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0065] The water contact angle of the waterproof and breathable nanofiber membrane is 119.6° and the moisture permeability is 12100 g / m 2 ·d, hydrostatic pressure resistance is 64.7kPa.
[0066] Example 6
[0067] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0068] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0069] (3) 6 g of solution A and 1.6 g of solution B were mixed, 0.64 g of DMF and 1.76 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=3:2, DMF:THF=1:1;
[0070] (4) adding the electrospinning solution into the needle tube, and obtaining the nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0071] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0072] The water contact angle of the waterproof and breathable nanofiber membrane was 135.6° and the moisture permeability was 13200 g / m 2 ·d, hydrostatic pressure resistance is 72.2kPa.
[0073] Example 7
[0074] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0075] (2) Using 10 g of THF as a solvent and 10 g of PDMS (the ratio of the main agent to the curing agent is 10:1) as a solute, ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0076] (3) 4 g of solution A and 2.4 g of solution B were mixed, 1.76 g of DMF and 1.84 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=2:3, DMF:THF=1:1;
[0077] (4) adding the electrospinning solution into the needle tube, and obtaining the nanofiber membrane by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h;
[0078] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0079] The water contact angle of the waterproof and breathable nanofiber membrane is 119.6° and the moisture permeability is 11900 g / m 2 ·d, hydrostatic pressure resistance is 74.5kPa.
[0080] Comparative Example 1
[0081] (1) Using 11.2 g DMF and 4.8 g THF as solvents and 4 g TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0082] (2) Using 10 g of THF as a solvent and 10 g of PDMS as a solute (the ratio of the main agent to the curing agent is 10:1), ultrasonic dispersion was performed for 0.5 h to obtain a 50 wt% solution B;
[0083] (3) 5 g of solution A and 2 g of solution B were mixed, 1.2 g of DMF and 1.8 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20 wt%, TPU:PDMS=1:1, DMF:THF=1:1;
[0084] (4) The electrospinning liquid is added into the needle tube, and a nanofiber membrane is obtained by high-voltage electrospinning, wherein the electrospinning voltage is 18 kV, the distance between the needle and the receiving device is 15 cm, the propulsion speed is 1 mL / h, and the spinning time is 2 h to obtain a moisture-permeable nanofiber membrane.
[0085] The water contact angle of the waterproof and breathable nanofiber membrane was 131.2° and the moisture permeability was 13300 g / m 2 ·d, hydrostatic pressure resistance is 48.8kPa.
[0086] Comparative Example 2
[0087] (1) Using 11.2 g of DMF and 4.8 g of THF as solvents and 4 g of TPU as solute, magnetic stirring was performed for 8 h to obtain a solution A with a mass concentration of 20 wt%;
[0088] (2) Using 15 g of THF as a solvent and 5 g of PDMS as a solute (the ratio of the main agent to the curing agent is 10:1), ultrasonic dispersion was performed for 0.5 h to obtain a 25% solution B;
[0089] (3) 7 g of solution A and 2.4 g of solution B were mixed, 0.08 g of DMF and 0.52 g of THF were added, and the mixture was stirred magnetically to obtain an electrospinning solution; the total mass concentration of TPU and PDMS in the spinning solution was 20%, TPU:PDMS=7:3, DMF:THF=1:1
[0090] (4) The electrospinning solution was placed in a needle tube and a nanofiber membrane was obtained by high-voltage electrospinning, wherein the electrospinning voltage was 18 kV, the distance between the needle and the receiving device was 15 cm, the propulsion speed was 1 mL / h, and the spinning time was 2 h to obtain a moisture-permeable nanofiber membrane.
[0091] (5) The nanofiber membrane is subjected to hot pressing at 70° C. for 0.5 min to obtain a waterproof and moisture-permeable nanofiber membrane.
[0092] The water contact angle of the waterproof and breathable nanofiber membrane is 96.8° and the moisture permeability is 12800 g / m 2 ·d, hydrostatic pressure resistance is 50.3kPa.
[0093] Comparative Example 1 was not heat treated relative to Example 2, and the fibers were easy to slide. From the hydrostatic pressure resistance data, it can be seen that the hydrostatic pressure resistance of the fiber membrane without heat pressing treatment is much lower than that of the fiber membrane with heat pressing treatment.
[0094] Figure 2 The surface SEM images of the fluorine-free waterproof and breathable nanofiber membranes prepared in Example 2, Example 6, and Comparative Example 2 (from left to right: Example 2, Example 6, Comparative Example 2). Figure 2 It can be seen that the fluorine-free waterproof and breathable nanofiber membrane prepared in Example contains uniform hydrophobic microbeads inside, while there is no microbead structure in Comparative Example 2, indicating that the ratio of TPU and PDMS concentration is an important factor affecting the three-dimensional microstructure of the nanofiber membrane.
[0095] Figure 3 The water contact angles of Example 2, Example 4, Example 6 and Comparative Example 1 and Comparative Example 2 are compared. Figure 3 It can be seen that the presence of the microbead structure can further improve the hydrophobicity of the film. The water contact angle test step is: place the sample on the sample table of the contact angle instrument, ensure that the sample is placed flat, add 4μL of water droplets on the sample surface through a needle, and then test the contact angle after standing for 5s. Conduct contact angle tests on at least 3 locations of each sample and calculate the average contact angle.
[0096] Figure 4 The hydrostatic pressure resistance and water vapor permeability of Example 2, Example 4, Example 6 are compared with those of Comparative Example 1 and Comparative Example 2. The hydrostatic pressure resistance test is based on GB / T 4744-2013 "Testing of Waterproof Performance of Textiles and Average Hydrostatic Pressure Method":
[0097] (1) Randomly cut 5 specimens with a test area of approximately 180*180 mm. Place the specimens face down in contact with the water surface on the instrument to ensure that the surface of the specimens is flat and wrinkle-free. Press the specimens tightly.
[0098] (2) Apply a continuously increasing water pressure to the sample at a water pressure increase rate of 6 kPa / min, and observe the water seepage phenomenon on the sample surface. Record the hydrostatic pressure value when the third water drop just appears on the sample.
[0099] The moisture permeability test is based on GB / T 12704.1-2009 "Test method for moisture permeability of textile fabrics Part 1: Moisture absorption method":
[0100] (1) Place about 35g of desiccant into a dry permeable cup so that the desiccant forms a flat surface. Place the test surface of the sample on the permeable cup with the test surface facing upward, install the gasket and pressure ring, screw on the nut, and then use vinyl adhesive tape to seal the pressure ring, gasket and permeable cup from the side to form a test assembly.
[0101] (2) Quickly place the test assembly horizontally in the test chamber and take it out after 1 hour of equilibration. Quickly cover the corresponding cup lid, place it in a silica gel desiccator at about 20°C for equilibration for 30 minutes, and weigh it.
[0102] (3) Remove the cup cover and place the test assembly back into the test chamber. Take it out after 1 hour of testing and weigh it again.
[0103] (4) The formula for calculating moisture permeability is: Where: Δm is the difference between two weighings of the same test assembly, Δm' is the difference between two weighings of the same test assembly of the blank sample, A is the effective test area, and t is the test time.
[0104] The present invention has been described in detail above. For those skilled in the art, without departing from the purpose and scope of the present invention, and without the need to carry out unnecessary experimental conditions, the present invention can be implemented in a wide range under equivalent parameters, concentrations and conditions. Although the present invention provides specific embodiments, it should be understood that the present invention can be further improved. In a word, according to the principles of the present invention, the application is intended to include any changes, uses or improvements to the present invention, including departure from the disclosed scope in the application, and changes made with conventional techniques known in the art.
Claims
1. A method for preparing a fluorine-free waterproof and breathable nanofiber membrane, comprising the following steps: 1) Using N,N-dimethylformamide (DMF) and tetrahydrofuran (THF) as solvents and thermoplastic polyurethane (TPU) as solute, magnetic stirring is performed to obtain solution A; 2) mixing polydimethylsiloxane (PDMS) as a main agent and a curing agent in a ratio of 10:1, using THF as a solvent, and performing ultrasonic dispersion to obtain a solution B; 3) mixing the above solution A and solution B, adding DMF and THF, and magnetically stirring to obtain spinning solution C; 4) Adding the spinning solution C into the needle tube, and performing high-voltage electrospinning to obtain the nanofiber membrane D; 5) The nanofiber membrane D is subjected to heat pressing to obtain a nanofiber membrane E.
2. The method according to claim 1, characterized in that In step 1), the mass ratio of DMF to THF is 7:3 to 3:7; in the solution A, the mass concentration of TPU is 10wt% to 50wt%.
3. The method according to claim 1, characterized in that In step 2), in the solution B, the mass concentration of PDMS is 30wt% to 60wt%.
4. The method according to claim 1, characterized in that: In step 3), in the spinning solution C, the total mass concentration of TPU and PDMS is 15wt% to 25wt%, wherein the mass ratio of PDMS to TPU is 2:3 to 3:
2.
5. The method according to claim 1, characterized in that In step 4), the voltage of the electrospinning is 16-20 kV, the distance between the needle and the receiving device is 10-20 cm, the propulsion speed is 0.5-1.5 mL / h; and the time of the electrospinning is 1-3 h.
6. The method according to claim 1, characterized in that In step 5), the temperature of the hot pressing treatment is 60-90° C. and the time is 0.5-1.5 min.
7. A fluorine-free waterproof and breathable nanofiber membrane prepared by the method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method of waterproof and breathable fast-food box
CN111086247A
Preparation method of PDMS surface modified multi-component waterproof and moisture-permeable film
CN111235761A
Super-elastic waterproof and breathable skin dressing with wrinkled structure, and preparation method thereof
CN111575904A
Preparation method of cobweb-structured blended waterproof moisture-permeable film
CN114541040A
Polyurethane nanofiber waterproof moisture-permeable film as well as preparation method and application thereof
CN117779345A
Cited By
High-temperature-resistant fluoride-free waterproof breathable nanofiber membrane and preparation method thereof
CN119777071A
Fluoride-free waterproof sound-transmitting film and preparation method thereof
CN119956564A
Nanofiber fluorine film composite fabric and preparation process thereof
CN121572702A
A nanofiber fluorine membrane composite fabric and its preparation process
CN121572702B