Decorative Sheet
The decorative sheet with a metal-neutralized ionomer resin and specific olefin polymers ensures effective low-temperature adhesion and improved scratch resistance, addressing the challenge of productivity in decorative sheet attachment.
Patent Information
- Application Number
- JP2021024053
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-18
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-02-18
AI Technical Summary
Existing decorative sheets face challenges in achieving effective adhesion at low temperatures, which affects productivity when attached to objects.
A decorative sheet comprising a decorative layer made of ionomer resin neutralized with monovalent or divalent metals and an adhesive layer containing olefin polymers with specific heat of fusion and molecular weight, along with optional hydrocarbon-based synthetic oils, to enhance adhesion and scratch resistance.
The decorative sheet exhibits excellent adhesion at low temperatures, improving productivity and providing enhanced scratch resistance and chemical resistance.
Smart Images

Figure 0007578501000003 
Figure 0007578501000004 
Figure 0007578501000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet, and more particularly to a decorative sheet that is attached to an object to be decorated. [Background technology]
[0002] 2. Description of the Related Art It is conventionally known to impart design features to the interior or exterior of a vehicle, building, or the like by adhering a decorative sheet.
[0003] As such a decorative sheet, a transfer decoration base film produced by extrusion molding a resin component containing an ionomer resin has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-160339 A Summary of the Invention [Problem to be solved by the invention]
[0005] On the other hand, when attaching such a decorative sheet to an object to be decorated, adhesiveness at low temperatures is required from the viewpoint of improving productivity.
[0006] The present invention provides a decorative sheet that has excellent adhesiveness at low temperatures. [Means for solving the problem]
[0007] The present invention [1] is a coating composition comprising a decorative layer and an adhesive layer in this order toward one side in a thickness direction, the decorative layer containing an ionomer resin neutralized with a monovalent metal and / or a divalent metal, the adhesive layer being made of an adhesive composition containing an olefin polymer, the olefin polymer having a heat of fusion of 0 J / g or more and 50 J / g or less as measured in accordance with JIS K7122, and a weight average molecular weight of 1×10 as measured by a GPC method.4 That's it, 1000 x 10 4 The following is a decorative sheet.
[0008] The present invention [2] includes the decorative sheet according to the above [1], in which the metal that neutralizes the ionomer resin includes a monovalent metal, and the monovalent metal is sodium.
[0009] The present invention [3] includes the decorative sheet according to the above [1], in which the metal that neutralizes the ionomer resin includes a divalent metal, and the divalent metal is zinc.
[0010] The present invention [4] includes the decorative sheet according to any one of the above [1] to [3], wherein the olefin polymer includes the following first olefin polymer and / or the following second olefin polymer. First olefin polymer: an olefin polymer containing structural units derived from an α-olefin having 2 to 20 carbon atoms Second olefin polymer: a polymer containing structural units derived from an α-olefin having 2 to 20 carbon atoms, a part or the whole of which is graft-modified with a polar group-containing monomer.
[0011] The present invention [5] includes the decorative sheet according to the above [4], wherein the olefin polymer comprises the second olefin polymer, and in the second olefin polymer, a structural unit derived from a polar group-containing monomer is contained in an amount of 0.1 part by mass or more and 15 parts by mass or less per 100 parts by mass of the second olefin polymer.
[0012] The present invention [6] includes the decorative sheet according to the above [4] or [5], wherein in the first olefin polymer or the second olefin polymer, the structural units derived from an α-olefin having 2 to 20 carbon atoms include structural units derived from propylene, and the content of the structural units derived from propylene is 50 mol % or more and 100 mol % or less relative to 100 mol % of the total amount of the structural units derived from propylene and the structural units derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene), and the content of the structural units derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene) is 0 mol % or more and 50 mol % or less.
[0013] The present invention [7] includes the decorative sheet according to any one of the above [4] to [6], wherein the polar group-containing monomer is an unsaturated carboxylic acid and / or an unsaturated carboxylic acid anhydride.
[0014] The present invention [8] is a method for manufacturing an adhesive composition comprising the steps of: 2 / sec or more, 500000mm 2 / sec or less, and the kinematic viscosity of the semi-solid hydrocarbon at 200°C is 1000mm 2 / second or more 100000mm 2 / sec or less. The decorative sheet according to any one of [1] to [7] above is included.
[0015] The present invention [9] includes the decorative sheet according to the above [8], in which the blending ratio of the olefin polymer is 10 parts by mass or more and 99 parts by mass or less, and the blending ratio of the hydrocarbon-based synthetic oil or the semi-solid hydrocarbon is 1 part by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the total amount of the olefin polymer and the hydrocarbon-based synthetic oil or the semi-solid hydrocarbon. Effect of the Invention
[0016] The decorative sheet of the present invention includes a decorative layer and an adhesive layer arranged in this order toward one side in a thickness direction. The decorative layer includes a predetermined ionomer resin. The adhesive layer is made of an adhesive composition including an olefin polymer having a predetermined heat of fusion and a predetermined weight average molecular weight.
[0017] This provides excellent adhesion between the decorative layer and the adhesive layer at low temperatures. Furthermore, such a decorative sheet also has excellent scratch resistance and chemical resistance. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a schematic diagram showing one embodiment of the decorative sheet of the present invention. [Diagram 2] Fig. 2 shows one embodiment of the method for producing a decorative sheet of the present invention. Fig. 2A shows a first step of preparing a decorative layer. Fig. 2B shows a second step of disposing an adhesive layer 3 on one surface of the decorative layer 2 in the thickness direction. [Diagram 3] FIG. 3 is a schematic diagram showing an embodiment in which an object to be decorated is decorated with the decorative sheet of the present invention. [Figure 4] FIG. 4 shows a cross-sectional view of a modified embodiment of the decorative sheet of the present invention (decorative sheet having a skin layer). [Diagram 5] FIG. 5 shows a cross-sectional view of a modified embodiment of the decorative sheet of the present invention (decorative sheet having a release layer). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] An embodiment of the decorative sheet of the present invention will be described with reference to FIG.
[0020] In Fig. 1, the up-down direction of the paper is the up-down direction (thickness direction), the upper side of the paper is the upper side (one side in the thickness direction), and the lower side of the paper is the lower side (the other side in the thickness direction). The left-right direction and the depth direction of the paper are surface directions perpendicular to the up-down direction. Specifically, they follow the directional arrows in each figure.
[0021] <Decorative sheet> The decorative sheet 1 has a film shape (including a sheet shape) with a predetermined thickness, as shown in Fig. 1. The decorative sheet 1 extends in a plane direction perpendicular to the thickness direction. The decorative sheet 1 has a flat upper surface and a flat lower surface.
[0022] The decorative sheet 1 includes a decorative layer 2 and an adhesive layer 3 in this order toward one side in the thickness direction. Specifically, the decorative sheet 1 includes the decorative layer 2 and the adhesive layer 3 disposed directly on the upper surface of the decorative layer 2 (one surface in the thickness direction).
[0023] <Decorative layer> The decorative layer 2 is a design layer provided for imparting design to an object to be decorated 10 (described later).
[0024] The decorative layer 2 has a film shape. The decorative layer 2 is disposed on the entire lower surface of the adhesive layer 3 so as to be in contact with the lower surface of the adhesive layer 3.
[0025] The decorative layer 2 contains an ionomer resin neutralized with a monovalent metal and / or a divalent metal. Preferably, the decorative layer 2 is formed from an ionomer resin neutralized with a monovalent metal and / or a divalent metal.
[0026] The ionomer resin neutralized with a monovalent metal and / or a divalent metal can be obtained by neutralizing a resin with a monovalent metal and / or a divalent metal.
[0027] The resin has a polymer skeleton composed of, for example, a hydrocarbon. The resin also has carboxyl groups in the side chains of the polymer skeleton. As will be described in detail later, at least a portion of the carboxyl groups is neutralized with a monovalent metal and / or a divalent metal.
[0028] Such a resin may, for example, be an ethylene-unsaturated carboxylic acid copolymer.
[0029] The ethylene-unsaturated carboxylic acid copolymer is a copolymer of polymerization components including ethylene and an unsaturated carboxylic acid.
[0030] The unsaturated carboxylic acid may, for example, be an unsaturated carboxylic acid having 3 to 8 carbon atoms. Examples of the unsaturated carboxylic acid having 3 to 8 carbon atoms include monobasic acids and dibasic acids. Examples of the monobasic acid include (meth)acrylic acid (acrylic acid and / or methacrylic acid), crotonic acid, and isocrotonic acid. Examples of the dibasic acid include maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, glutaconic acid, allylsuccinic acid, nadic acid, methylnadic acid, tetrahydrofumaric acid, and methylhexahydrophthalic acid. Examples of the unsaturated carboxylic acid having 3 to 8 carbon atoms include preferably monobasic acids, and more preferably (meth)acrylic acid, from the viewpoint of facilitating the production of an ethylene-unsaturated carboxylic acid copolymer.
[0031] The unsaturated carboxylic acids can be used alone or in combination of two or more kinds.
[0032] In the polymerization components, the blending ratio of ethylene relative to 100 parts by mass of the total amount of ethylene and unsaturated carboxylic acid is, for example, 60 parts by mass or more, preferably 75 parts by mass or more, and for example, 95 parts by mass or less, preferably 92 parts by mass or less. Also, the blending ratio of unsaturated carboxylic acid relative to 100 parts by mass of the total amount of ethylene and unsaturated carboxylic acid is, for example, 5 parts by mass or more, preferably 8 parts by mass or more, and for example, 40 parts by mass or less, preferably 25 parts by mass or less.
[0033] The mixing ratio of ethylene and unsaturated carboxylic acid relative to the polymerization components is, for example, 60 mass % or more, preferably 80 mass % or more, and more preferably 90 mass % or more.
[0034] The polymeric components may further comprise other polymeric components.
[0035] Examples of the other polymerization components include unsaturated carboxylic acid esters and vinyl esters. Examples of the unsaturated carboxylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, and isobutyl (meth)acrylate. Examples of the vinyl esters include vinyl acetate.
[0036] When the polymerization components contain other polymerization components, the blending ratio of the other polymerization components to the polymerization components is, for example, 40 mass % or less, preferably 20 mass % or less, and more preferably 10 mass % or less.
[0037] The resin can be obtained by polymerizing the polymerization components by a known polymerization method. Such a resin has a carboxyl group derived from an unsaturated carboxylic acid.
[0038] The ionomer resin neutralized with a monovalent metal and / or a divalent metal can be obtained by neutralizing the carboxyl groups of the above resin with a monovalent metal and / or a divalent metal.
[0039] Examples of the monovalent metal include sodium and potassium, and from the viewpoint of ease of production, sodium is preferred.
[0040] Examples of divalent metals include magnesium, zinc, calcium, copper, iron, and barium, and from the viewpoint of ease of production, zinc is preferred.
[0041] To neutralize the carboxyl groups of the resin with a monovalent metal and / or a divalent metal, the resin is mixed with a compound having a monovalent metal and / or a compound having a divalent metal.
[0042] Examples of the compound having a monovalent metal include hydroxides of the above monovalent metals, and preferably sodium hydroxide.
[0043] Examples of the compound having a divalent metal include oxides, hydroxides, and carbides of the above divalent metals, and preferably zinc hydroxide.
[0044] This results in an ionomer resin neutralized with a monovalent metal and / or a divalent metal.
[0045] The metal that neutralizes the ionomer resin includes a monovalent metal and / or a divalent metal, preferably includes a monovalent metal or includes a divalent metal, more preferably includes only a monovalent metal or includes only a divalent metal, more preferably includes only a monovalent metal.
[0046] As such an ionomer resin neutralized with a monovalent metal and / or a divalent metal, preferably, from the viewpoint of adhesiveness, an ionomer resin neutralized with a monovalent metal or an ionomer resin neutralized with a divalent metal, more preferably, an ionomer resin neutralized with sodium or an ionomer resin neutralized with zinc, and even more preferably, from the viewpoint of further improving adhesiveness and scratch resistance, an ionomer resin neutralized with sodium.
[0047] The decorative layer 2 is obtained by molding an ionomer resin neutralized with a monovalent metal and / or a divalent metal by a known method.
[0048] As such a decorative layer 2, a commercially available product may be used, specifically, the Himilan series (manufactured by Dow Mitsui Polychemicals Co., Ltd.).
[0049] The decorative layer 2 has a thickness of, for example, 10 μm or more, preferably 50 μm or more, and for example, 200 μm or less.
[0050] <Adhesive layer> The adhesive layer 3 is a layer for disposing (attaching) the decorative sheet 1 to an object to be decorated 10 (described later).
[0051] The adhesive layer 3 has a film shape. The adhesive layer 3 is disposed on the entire upper surface of the decorative layer 2 so as to be in contact with the upper surface of the decorative layer 2.
[0052] The adhesive layer 3 is made of an adhesive composition. More specifically, the adhesive layer 3 is formed of an adhesive composition.
[0053] The adhesive composition includes an olefin polymer.
[0054] The heat of fusion of the olefin polymer, measured according to JIS K7122, is 0 J / g or more, preferably 10 J / g or more, more preferably 20 J / g or more, and is 50 J / g or less, preferably 40 J / g or less.
[0055] When the heat of fusion is equal to or higher than the lower limit, the low-temperature adhesiveness is excellent.
[0056] In addition, if the heat of fusion is equal to or less than the above upper limit, the olefin polymer will have excellent stability when it is dissolved in a solvent to prepare a varnish.
[0057] The method for measuring the heat of fusion will be described in detail in the Examples below.
[0058] The melting point of the olefin polymer is, for example, 60°C or higher, preferably 70°C or higher, more preferably 75°C or higher, and, for example, 90°C or lower.
[0059] The method for measuring the melting point will be described in detail in the Examples below.
[0060] The weight average molecular weight of the olefin polymer measured by GPC method is 1×10 4 More than 10×10 4 Above, 1000 x 10 4 Less than or equal to 100×10 4 More preferably, from the viewpoint of adhesiveness, 50×10 4 The following is the result.
[0061] When the weight average molecular weight is equal to or higher than the above lower limit, the mechanical strength of the adhesive layer 3 can be increased.
[0062] When the weight average molecular weight is equal to or less than the above upper limit, the olefin polymer is excellent in stability when it is dissolved in a solvent to prepare a varnish.
[0063] The method for measuring the weight average molecular weight will be described in detail in the Examples below.
[0064] Such an olefin polymer includes a first olefin polymer and / or a second olefin polymer. Specifically, the olefin polymer includes the first olefin polymer and / or the second olefin polymer and has the above-mentioned predetermined heat of fusion and the above-mentioned predetermined weight average molecular weight.
[0065] The first olefin polymer is an olefin polymer containing structural units derived from an α-olefin having 2 to 20 carbon atoms. That is, the first olefin polymer is obtained by polymerizing an α-olefin having 2 to 20 carbon atoms.
[0066] Examples of α-olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.
[0067] From the viewpoint of coating film strength, the structural unit derived from an α-olefin having 2 to 20 carbon atoms preferably contains a structural unit derived from propylene.
[0068] When the structural unit derived from an α-olefin having 2 to 20 carbon atoms contains a structural unit derived from propylene, the content of the structural unit derived from propylene relative to the total amount (100 mol%) of the structural units derived from propylene and the structural units derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene) is, for example, 50 mol% or more, preferably 60 mol% or more, and, for example, 100 mol% or less, preferably 80 mol% or less. Furthermore, the content of the structural unit derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene) relative to the total amount (100 mol%) of the structural units derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene) is, for example, 0 mol% or more, preferably 20 mol% or more, and, for example, 50 mol% or less, preferably 40 mol% or less.
[0069] When the content of the structural unit derived from propylene and the content of the structural unit derived from an α-olefin having 2 to 20 carbon atoms (excluding propylene) are within the above ranges, the low-temperature adhesiveness is excellent.
[0070] The above content ratio is, for example, 13 This can be confirmed by known means such as C-NMR measurement.
[0071] Furthermore, when the structural units derived from an α-olefin having 2 to 20 carbon atoms contain structural units derived from propylene, the structural units derived from an α-olefin having 2 to 20 carbon atoms preferably contain structural units derived from 1-butene together with the structural units derived from propylene, and more preferably consist of structural units derived from propylene and structural units derived from 1-butene only. In other words, more preferably, the first olefin polymer is a propylene / 1-butene copolymer.
[0072] The first olefin polymer can be obtained by, for example, the method described in Japanese Patent No. 3939464 and International Publication WO 2004 / 87775. Specifically, the first olefin polymer can be obtained by polymerizing an α-olefin having 2 to 20 carbon atoms in the presence of a metallocene catalyst.
[0073] The first olefin polymer may be used alone or in combination of two or more kinds.
[0074] The second olefin polymer is obtained by polymerizing an α-olefin having 2 to 20 carbon atoms, a part or all of which is graft-modified with a polar group-containing monomer. That is, the second olefin polymer is an olefin polymer containing structural units derived from an α-olefin having 2 to 20 carbon atoms, a part or all of which is graft-modified with a polar group-containing monomer.
[0075] Such a second olefin polymer may be an olefin polymer in which the above-mentioned first olefin polymer (preferably a propylene / 1-butene copolymer) is partially or entirely graft-modified with a polar group-containing monomer.
[0076] Examples of the polar group-containing monomer include hydroxyl group-containing ethylenically unsaturated compounds, amino group-containing ethylenically unsaturated compounds, epoxy group-containing ethylenically unsaturated compounds, unsaturated carboxylic acids, unsaturated carboxylic anhydrides, vinyl ester compounds, and derivatives thereof (excluding unsaturated carboxylic anhydrides).
[0077] Examples of the hydroxyl group-containing ethylenically unsaturated compound include hydroxyl group-containing (meth)acrylic acid esters. Examples of the hydroxyl group-containing (meth)acrylic acid esters include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate.
[0078] Examples of the amino group-containing ethylenically unsaturated compound include aminomethyl (meth)acrylate and propylaminoethyl (meth)acrylate.
[0079] An example of the epoxy group-containing ethylenically unsaturated compound is glycidyl (meth)acrylate.
[0080] Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid.
[0081] Examples of unsaturated carboxylic acid anhydrides include maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic anhydride.
[0082] Vinyl ester compounds include, for example, vinyl acetate, vinyl propionate, and vinyl n-butyrate.
[0083] The derivatives include derivatives of unsaturated carboxylic acids. The derivatives of unsaturated carboxylic acids include, for example, maleic acid derivatives, fumaric acid derivatives, itaconic acid derivatives, citraconic acid derivatives, phthalic acid derivatives, (meth)acrylic acid derivatives, and other derivatives. The maleic acid derivatives include, for example, malenyl chloride, malenylimide, dimethyl maleate, monomethyl maleate, and diethyl maleate. The fumaric acid derivatives include, for example, diethyl fumarate. The itaconic acid derivatives include, for example, dimethyl itaconate. The citraconic acid derivatives include, for example, diethyl citraconic acid. The phthalic acid derivatives include, for example, dimethyl tetrahydrophthalate. The (meth)acrylic acid derivatives include, for example, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, glycidyl (meth)acrylate, aminoethyl methacrylate, and aminopropyl methacrylate. Other derivatives include, for example, dimethyl bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylate.
[0084] From the viewpoint of ease of production, the polar group-containing monomer preferably contains an unsaturated carboxylic acid and / or an unsaturated carboxylic acid anhydride, more preferably contains an unsaturated carboxylic acid anhydride, further preferably contains maleic anhydride, and particularly preferably consists of maleic anhydride. That is, particularly preferably, the second olefin polymer is a maleic anhydride-modified propylene / 1-butene copolymer.
[0085] The modification amount (introduced amount) of the polar group-containing monomer in the second olefin polymer, i.e., the content ratio of the structural units derived from the polar group-containing monomer in the second olefin polymer, is, for example, from the viewpoint of adhesion to polar substrates, 0.1 part by mass or more, preferably 0.5 part by mass or more, and, for example, from the viewpoint of adhesion to non-polar substrates, 15 parts by mass or less, preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 2 parts by mass or less, per 100 parts by mass of the second olefin polymer.
[0086] The above-mentioned modification amount is, for example, 1 This can be confirmed by known means such as H-NMR measurement. 1 Examples of H-NMR measurement conditions are as follows:
[0087] That is, the conditions are as follows: a JEOL ECX400 nuclear magnetic resonance apparatus is used, the solvent is deuterated orthodichlorobenzene, the sample concentration is 20 mg / 0.6 mL, the measurement temperature is 120°C, the observation nucleus is 1H (400 MHz), the sequence is single pulse, the pulse width is 5.12 μsec (45° pulse), the repetition time is 7.0 sec, and the number of accumulations is 500 or more. The reference chemical shift is set to 0 ppm for hydrogen of tetramethylsilane, but similar results can be obtained by, for example, setting the peak derived from the residual hydrogen of deuterated orthodichlorobenzene at 7.10 ppm as the reference value of the chemical shift. Peaks such as 1H derived from polar group-containing monomers can be identified by ordinary methods.
[0088] When an unsaturated carboxylic acid or an unsaturated carboxylic anhydride is used as the polar group-containing monomer, for example, it is also possible to use the acid value.
[0089] The acid value of the second olefin polymer is, for example, 0.1 mgKOH / g or more, preferably 0.5 mgKOH / g or more, and for example, 100 mgKOH / g or less, preferably 30 mgKOH / g or less, more preferably 10 mgKOH / g or less.
[0090] Here, examples of methods for measuring the acid value include the following.
[0091] That is, the basic operation is in accordance with JIS K-2501-2003. Specifically, about 10 g of the second olefin polymer is accurately measured and placed in a 200 mL tall beaker. 150 mL of a mixed solvent made by mixing xylene and dimethylformamide in a 1:1 (volume ratio) is added thereto as a titration solvent. A few drops of a 1 w / v% phenolphthalein ethanol solution (manufactured by Wako Pure Chemical Industries, Ltd.) are added as an indicator, and the liquid temperature is heated to 80°C to dissolve the sample. After the liquid temperature becomes constant at 80°C, titration is performed using a 0.1 mol / L potassium hydroxide 2-propanol solution (manufactured by Wako Pure Chemical Industries, Ltd.), and the acid value is calculated from the titration amount based on the following formula (1).
[0092] Acid value (mgKOH / g)=(EP1-BL1)×FA1×C1 / SIZE (1) It is.
[0093] In the above formula, EP1 is the titration volume (mL), BL1 is the blank value (mL), FA1 is the factor of the titrant (1.00), C1 is the concentration conversion value (5.611 mg / mL: equivalent to potassium hydroxide in 1 mL of 0.1 mo1 / L KOH), and SIZE is the sample size (g).
[0094] This measurement is repeated three times and the average value is taken as the acid value.
[0095] The second olefin polymer is obtained by polymerizing a polar group-containing monomer in the presence of the first olefin polymer. As a result, the first olefin polymer is graft-modified with the polar group-containing monomer or a polymer thereof. Specifically, the second olefin polymer can be prepared, for example, by the following methods (1) to (4).
[0096] (1) A method in which a first olefin polymer is dissolved in an organic solvent, a polar group-containing monomer and a radical polymerization initiator are added, and the mixture is heated and stirred to modify and react the first olefin polymer with the polar group-containing monomer. (2) A method in which a first olefin polymer is heated and melted, and a polar group-containing monomer and a radical polymerization initiator are added to the resulting melt and stirred to modify and react the first olefin polymer with the polar group-containing monomer. (3) A method in which a first olefin polymer, a polar group-containing monomer and a radical polymerization initiator are mixed in advance, and the resulting mixture is fed into an extruder and heated and kneaded while modifying and reacting the first olefin polymer with the polar group-containing monomer. (4) A method in which a first olefin polymer is impregnated with a solution obtained by dissolving a polar group-containing monomer and a radical polymerization initiator in an organic solvent, and then heated to the highest temperature at which the first olefin polymer does not dissolve, thereby modifying and reacting the first olefin polymer with the polar group-containing monomer.
[0097] The reaction temperature is, for example, 50° C. or more, preferably 80° C. or more, and, for example, 250° C. or less. The reaction time is, for example, 1 minute or more and 10 hours or less.
[0098] The reaction system may be a batch system or a continuous system, and in order to carry out the modification reaction uniformly, the batch system is preferred.
[0099] Examples of the radical polymerization initiator include organic peroxides and organic peresters.
[0100] Examples of organic peroxides include dicumyl peroxide, benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(peroxybenzoate)hexyne-3, 1,4-bis(tert-butylperoxyisopropyl)benzene, lauroyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, and tert-butyl peroxybenzoate. Examples of organic peresters include tert-butyl peracetate, tert-butyl perphenyl acetate, tert-butyl perisobutyrate, tert-butyl persec-octoate, tert-butyl perpivalate, cumyl perpivalate, and tert-butyl perethyl acetate. Further, the radical polymerization initiator may also include other azo compounds, such as azobis-isobutylnitrile and dimethylazoisobutylnitrile.
[0101] Of the radical polymerization initiators, preferred are organic peroxides, and more preferred is di-tert-butyl peroxide.
[0102] The mixing ratio of the radical polymerization initiator is, for example, 0.001 parts by mass or more and 10 parts by mass or less with respect to 100 parts by mass of the second olefin polymer.
[0103] The second olefin polymer is prepared by the above methods (1) to (4) in the presence of a solvent or without using a solvent.
[0104] Examples of the solvent include aromatic hydrocarbons, aliphatic hydrocarbons, alicyclic hydrocarbons, alcohols, ketones, cellosolves, esters, and halogenated hydrocarbons. Examples of the aromatic hydrocarbons include benzene, toluene, and xylene. Examples of the aliphatic hydrocarbons include hexane, heptane, octane, and decane. Examples of the alicyclic hydrocarbons include cyclohexane, cyclohexene, and methylcyclohexane. Examples of the alcohols include methanol, ethanol, isopropyl alcohol, butanol, pentanol, hexanol, propanediol, and phenol. Examples of the ketones include acetone, methyl isobutyl ketone, methyl ethyl ketone, pentanone, hexanone, isophorone, acetophenone, and cyclohexanone. Examples of the cellosolves include methyl cellosolve and ethyl cellosolve. Examples of the esters include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, and butyl formate. Halogenated hydrocarbons include, for example, trichloroethylene, dichloroethylene, and chlorobenzene.
[0105] When the above modification is carried out in the presence of a solvent, the resulting second olefin polymer is prepared as a varnish.
[0106] For the preparation of the second olefin polymer, the above method (1) is preferably selected from the viewpoint of modification efficiency.
[0107] The olefin polymer preferably contains a first olefin polymer or a second olefin polymer, and more preferably contains only the second olefin polymer from the viewpoints of adhesiveness and scratch resistance.
[0108] The adhesive composition may further include a hydrocarbon-based synthetic oil or a semi-solid hydrocarbon.
[0109] When the adhesive composition contains a hydrocarbon synthetic oil or a semi-solid hydrocarbon, the adhesive property between the decorative layer 2 and the adhesive layer 3 at low temperatures can be improved.
[0110] Although the hydrocarbon synthetic oil and the semi-solid hydrocarbon will be described in detail later, both are olefin polymers containing structural units derived from olefins having 2 to 20 carbon atoms. In other words, the hydrocarbon synthetic oil and the semi-solid hydrocarbon are obtained by polymerizing olefins having 2 to 20 carbon atoms.
[0111] On the other hand, the synthetic hydrocarbon oils and the semi-solid hydrocarbons have different kinetic viscosities, i.e., the synthetic hydrocarbon oils and the semi-solid hydrocarbons can be distinguished by their kinetic viscosities.
[0112] The kinetic viscosity of the hydrocarbon synthetic oil and the kinetic viscosity of the semi-solid hydrocarbon can be set within a predetermined range, for example, by adjusting the type of structural unit derived from an olefin having 2 to 20 carbon atoms and the content of the structural unit derived from an olefin having 2 to 20 carbon atoms.
[0113] The above-mentioned olefin polymers can be distinguished from the hydrocarbon synthetic oils and semi-solid hydrocarbons by the heat of fusion and weight average molecular weight described for the above-mentioned olefin polymers. More specifically, the hydrocarbon synthetic oils and semi-solid hydrocarbons do not have at least one of the specified heat of fusion and the specified weight average molecular weight of the above-mentioned olefin polymers.
[0114] The synthetic hydrocarbon oils and the semi-solid hydrocarbons will be described in detail below.
[0115] The hydrocarbon synthetic oil is an olefin polymer containing structural units derived from an olefin having 2 to 20 carbon atoms. In other words, the hydrocarbon synthetic oil is obtained by polymerizing olefins having 2 to 20 carbon atoms.
[0116] Examples of the olefin having 2 to 20 carbon atoms include the α-olefins having 2 to 20 carbon atoms listed in the above-mentioned first olefin polymer. Preferred examples of the olefin having 2 to 20 carbon atoms include ethylene and propylene. In other words, the hydrocarbon-based synthetic oil is preferably an ethylene / propylene copolymer.
[0117] When the structural unit derived from an olefin having 2 to 20 carbon atoms includes a structural unit derived from ethylene and a structural unit derived from propylene, the content ratio of the structural unit derived from ethylene relative to the total amount of the structural units derived from ethylene and the structural units derived from propylene is, for example, 30 mol% or more, preferably 40 mol% or more, and, for example, 70 mol% or less, preferably 60 mol% or less, relative to the total amount of the structural units derived from ethylene and the structural units derived from propylene is, for example, 30 mol% or more, preferably 40 mol% or more, and, for example, 70 mol% or less, preferably 60 mol% or less, relative to the total amount of the structural units derived from ethylene and the structural units derived from propylene.
[0118] The above content ratio is, for example, 13 This can be confirmed by known means such as C-NMR measurement.
[0119] The synthetic hydrocarbon oil is obtained by polymerizing the above-mentioned olefins having 2 to 20 carbon atoms in the presence of a known polymerization catalyst. Examples of the polymerization catalyst include vanadium oxy compounds (e.g., vanadium oxyethoxide dichloride) and organoaluminum compounds (e.g., ethylaluminum sesquichloride).
[0120] The kinematic viscosity of a synthetic hydrocarbon oil at 40°C is, for example, 30mm 2 / sec or more, preferably 300 mm 2 / sec or more, more preferably 5,000 mm 2 / sec or more, more preferably 20,000 mm 2 / sec, also, for example, 500,000 mm 2 / sec or less, preferably 400,000 mm 2 / sec or less, more preferably 300,000 mm 2 / sec or less, and more preferably 100,000 mm 2 / sec, particularly preferably 50,000 mm 2 / second.
[0121] If the kinetic viscosity at 40° C. is within the above range, the adhesion between the decorative layer 2 and the adhesive layer 3 at low temperatures can be improved.
[0122] The kinetic viscosity at 40° C. can be measured based on ASTM D 445.
[0123] The semi-solid hydrocarbon is an olefin polymer containing structural units derived from an olefin having 2 to 20 carbon atoms. In other words, the semi-solid hydrocarbon is formed by polymerizing an olefin having 2 to 20 carbon atoms.
[0124] Examples of the α-olefin having 2 to 20 carbon atoms include the α-olefins having 2 to 20 carbon atoms exemplified in the above-mentioned first olefin polymer. Preferable examples of the α-olefin having 2 to 20 carbon atoms include ethylene, propylene, and 1-butene.
[0125] The semi-solid hydrocarbons can be produced in the same manner as in the above-mentioned synthetic hydrocarbon oils.
[0126] The kinetic viscosity of a semi-solid hydrocarbon at 200°C is, for example, 1,000 mm 2 / sec or more, preferably 1,100 mm 2 / sec or more, preferably 1,200 mm 2 / sec or more, e.g., 100,000 mm 2 / sec or less, preferably 80,000 mm 2 / sec or less, more preferably 60,000 mm 2 / sec or less.
[0127] If the kinetic viscosity at 200° C. is within the above range, the adhesion between the decorative layer 2 and the adhesive layer 3 at low temperatures can be improved.
[0128] The kinetic viscosity at 200° C. can be measured based on JIS K 2283.
[0129] The blending ratio of the olefin polymer relative to 100 parts by mass of the total amount of the olefin polymer and the hydrocarbon synthetic oil or semi-solid hydrocarbon is, for example, 10 parts by mass or more, preferably 30 parts by mass or more, more preferably 60 parts by mass or more, even more preferably 70 parts by mass or more, and for example, 99 parts by mass or less. Furthermore, the blending ratio of the hydrocarbon synthetic oil or semi-solid hydrocarbon relative to 100 parts by mass of the total amount of the hydrocarbon synthetic oil or semi-solid hydrocarbon is, for example, 1 part by mass or more, and, for example, 90 parts by mass or less, preferably 70 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less.
[0130] The blending ratio of the olefin polymer to the adhesive composition is, for example, 10% by mass or more, preferably 30% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 75% by mass or more, and for example, 99% by mass or less. The blending ratio of the hydrocarbon synthetic oil or semi-solid hydrocarbon to the adhesive composition is, for example, 1% by mass or more, and, for example, 90% by mass or less, preferably 70% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably 15% by mass or less.
[0131] When the blending ratio of the olefin polymer and the blending ratio of the hydrocarbon synthetic oil or semi-solid hydrocarbon are within the above ranges, the adhesion between the decorative layer 2 and the adhesive layer 3 at low temperatures can be further improved.
[0132] The adhesive composition may further include other components.
[0133] Examples of the other components include other olefin polymers, transition metal compounds, tackifiers, pigments, thixotropic agents, thickeners, defoamers, surface conditioners, antisettling agents, antioxidants, weathering agents, heat stabilizers, light stabilizers, pigment dispersants, and antistatic agents, and preferably, tackifiers.
[0134] The other olefin polymers are olefin polymers that do not fall under the above-mentioned olefin polymers, the above-mentioned hydrocarbon-based synthetic oils, and the above-mentioned semi-solid hydrocarbons.
[0135] Examples of the transition metal compound include titanium oxide (rutile type) and zinc oxide.
[0136] Examples of tackifiers include rosin resins and terpene resins.
[0137] The blending ratio of the other components is appropriately set depending on the purpose and application. Specifically, when the other component is a tackifier, the mixing ratio of the tackifier relative to the adhesive composition is, for example, 1 mass % or more, preferably 5 mass % or more, and for example, 20 mass % or less.
[0138] The adhesive composition can be obtained by mixing the olefin polymer, the hydrocarbon synthetic oil or the semi-solid hydrocarbon, and other components that are added as necessary, and heating as necessary.
[0139] The adhesive composition can also be prepared as a varnish by dissolving it in a solvent (the above-mentioned solvent).
[0140] Next, to form the adhesive layer 3, an adhesive composition (varnish of the adhesive composition) is applied to one surface in the thickness direction of the decorative layer 2 and dried, as described in detail below. Thus, the adhesive layer 3 is formed.
[0141] The adhesive layer 3 has a thickness of, for example, 3 μm or more and, for example, 50 μm or less.
[0142] <Method of manufacturing decorative sheet> The method for producing the decorative sheet 1 includes a first step of preparing the decorative layer 2, and a second step of arranging the adhesive layer 3 on one surface of the decorative layer 2 in the thickness direction.
[0143] In the first step, as shown in FIG. 2A, a decorative layer 2 is prepared.
[0144] In the second step, as shown in FIG. 2B, an adhesive layer 3 is disposed on one surface of the decorative layer 2 in the thickness direction.
[0145] In order to dispose the adhesive layer 3 on one surface in the thickness direction of the decorative layer 2, the one surface in the thickness direction of the decorative layer 2 is subjected to a surface treatment, if necessary.
[0146] Examples of the surface treatment include corona treatment, plasma treatment, flame treatment, ozone treatment, primer treatment, glow treatment, and saponification treatment, and preferably corona treatment.
[0147] Next, the adhesive composition (varnish of the adhesive composition) is applied to one surface in the thickness direction of the decorative layer 2 and dried. In this way, the adhesive layer 3 is disposed (formed) on one surface in the thickness direction of the decorative layer 2.
[0148] In this way, the decorative sheet 1 is obtained.
[0149] <Use of decorative sheets> The decorative film 1 can be used, for example, by using the insert molding method, the in-mold molding method, and the TOM method using a "vacuum forming device" described in Patent No. 3733564, to place (attach) the decorative sheet 1 on the object to be decorated 10 via an adhesive layer 3, as shown in Figure 3, thereby decorating the object to be decorated 10.
[0150] The object 10 to be decorated is not particularly limited, but examples thereof include polyolefin materials, polyamide resins, polar resins, and inorganic materials. Examples of polyolefin materials include polypropylene (PP). Examples of polyamide resins include nylon. Examples of polar resins include acrylonitrile / butadiene / styrene copolymers (ABS), polycarbonate (PC), polyethylene terephthalate (PET), polyphenylene sulfide (PPS), and acrylic resins. Examples of inorganic materials include ED steel plates, Mg alloys, SUS (stainless steel), aluminum, aluminum alloys, and glass.
[0151] The object to be decorated 10 can be used alone or in combination of two or more kinds.
[0152] The decorative film 1 can be suitably used in, for example, automotive interior and exterior components, various front panels (e.g., AV equipment), surface decorative materials (e.g., buttons, emblems), cases (e.g., mobile phones), housings, display windows, buttons, furniture exterior materials, architectural interior materials (bathrooms, walls, ceilings, and floors), surface decorative materials (window frames, doors, handrails, thresholds, lintels, and furniture), various displays, optical components (e.g., lenses, mirrors, goggles, and window glass), various packaging containers (e.g., bottles, cosmetic containers, and trinket boxes), miscellaneous goods (e.g., prizes and small items), white goods (air conditioners, refrigerators, and washing machines), and various other applications.
[0153] <Action and effect> The decorative sheet 1 includes a decorative layer 2 and an adhesive layer 3 in this order toward one side in the thickness direction. The decorative layer 2 contains a predetermined ionomer resin. The adhesive layer 3 is made of an adhesive composition containing an olefin polymer having a predetermined heat of fusion and a predetermined weight average molecular weight.
[0154] In other words, the decorative sheet 1 is composed of a combination of a specific decorative layer 2 and a specific adhesive layer 3. This allows it to fuse and conform to the adherend at low temperatures, and also prevents the penetration of chemicals into the adherend interface. As a result, it has excellent adhesion at low temperatures. It also has excellent scratch resistance and chemical resistance.
[0155] In particular, since the decorative sheet 1 has excellent adhesiveness at low temperatures, for example, the decorative sheet 1 can be firmly placed (attached) on the object 10 to be decorated even at low temperatures (specifically, 120° C. or less, preferably 110° C. or less, and for example, 80° C. or more). Therefore, the object 10 to be decorated can be decorated using the decorative sheet 1 with reduced energy. As a result, productivity is excellent.
[0156] <Modification> In the modified example, the same components and steps as those in the first embodiment are denoted by the same reference numerals, and detailed description thereof will be omitted. In addition, the modified example can achieve the same effects as those in the first embodiment, unless otherwise specified. Furthermore, the first embodiment and its modified example can be appropriately combined.
[0157] In the above description, the decorative sheet 1 includes the decorative layer 2 and the adhesive layer 3, in that order, toward one side in the thickness direction. Meanwhile, the decorative sheet 1 may further include a skin layer 4. Specifically, as shown in Fig. 4, the decorative sheet 1 includes the skin layer 4, the decorative layer 2, and the adhesive layer 3, in that order, toward one side in the thickness direction. More specifically, the decorative sheet 1 includes the skin layer 4, the decorative layer 2 disposed directly on the upper surface (one surface in the thickness direction) of the skin layer 4, and the adhesive layer 3 disposed directly on the upper surface (one surface in the thickness direction) of the decorative layer 2.
[0158] The skin layer 4 is a design layer provided to further impart design to the object to be decorated 10 (described later).
[0159] The skin layer 4 has a film shape and is disposed over the entire lower surface of the decorative layer 2 so as to be in contact with the lower surface of the decorative layer 2.
[0160] A resin sheet is selected as the skin layer 4. Examples of such a resin sheet include ethylene vinyl acetate, acrylonitrile-butadiene-styrene copolymer, polystyrene, acrylonitrile-styrene copolymer, and polyvinyl chloride.
[0161] The thickness of the skin layer 4 is appropriately set depending on the purpose and application.
[0162] The skin layer 4 is disposed, for example, on the other side in the thickness direction of the decorative layer 2 via a known adhesive.
[0163] In the above description, the decorative sheet 1 includes a decorative layer 2 and an adhesive layer 3, which are arranged in this order toward one side in the thickness direction. Meanwhile, the decorative sheet 1 may further include a peeling layer 5. Specifically, as shown in Fig. 5, the decorative sheet 1 includes a decorative layer 2, an adhesive layer 3, and a peeling layer 5, which are arranged in this order toward one side in the thickness direction. More specifically, the decorative sheet 1 includes a decorative layer 2, an adhesive layer 3 arranged directly on the upper surface (one surface in the thickness direction) of the decorative layer 2, and a peeling layer 5 arranged directly on the upper surface (one surface in the thickness direction) of the adhesive layer 3.
[0164] The release layer 5 is a layer for protecting the adhesive layer 3 until it is used (when the decorative sheet 1 is used to decorate the object to be decorated 10).
[0165] The release layer 5 has a film shape. The release layer 5 is disposed over the entire upper surface of the adhesive layer 3 so as to be in contact with the upper surface of the adhesive layer 3.
[0166] The release layer 5 may be, for example, a polyethylene, polypropylene, polyethylene terephthalate, or polyester film.
[0167] Moreover, the release layer 5 is preferably subjected to a release treatment using a release agent (for example, silicone-based, fluorine-based, long-chain alkyl-based, and fatty acid amide-based) or a release treatment using silica powder.
[0168] The thickness of the release layer 5 is appropriately set depending on the purpose and application.
[0169] The release layer 5 is peeled off from the adhesive layer 3 during use.
[0170] Although not shown, the decorative sheet 1 may also include both the above-mentioned skin layer 4 and the above-mentioned release layer 5. In such a case, the decorative sheet 1 includes the skin layer 4, the decorative layer 2, the adhesive layer 3, and the release layer 5 in this order toward one side in the thickness direction. Specifically, the decorative sheet 1 includes the skin layer 4, the decorative layer 2 disposed directly on the upper surface (one surface in the thickness direction) of the skin layer 4, the adhesive layer 3 disposed directly on the upper surface (one surface in the thickness direction) of the decorative layer 2, and the release layer 5 disposed directly on the upper surface (one surface in the thickness direction) of the adhesive layer 3. EXAMPLES
[0171] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. In addition, the specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit value (numerical value defined as "less than or equal to" or "less than") or lower limit value (numerical value defined as "more than or equal to" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention".
[0172] 1.Details of ingredients The trade names and abbreviations of the components used in each Production Example, each Example, and each Comparative Example are described in detail below.
[0173] A-1: Product name "Himilan 1601", sodium-neutralized ionomer resin (ionomer resin obtained by neutralizing ethylene-unsaturated carboxylic acid copolymer with sodium), thickness 100 μm, Dow Mitsui Polychemicals Co., Ltd. A-2: Product name "Himilan 1650", zinc-neutralized ionomer resin (ionomer resin obtained by neutralizing ethylene-unsaturated carboxylic acid copolymer with zinc), thickness 100 μm, Mitsui Dow Polychemicals Co., Ltd. A-3: PMMA, product name "Technoloy S001G", thickness 100 μm, manufactured by Sumika Acrylic Sales Co., Ltd. A-4: Polycarbonate resin, product name "Technoloy C000", thickness 100 μm, manufactured by Sumika Acrylic Sales Co., Ltd. PP: Polypropylene, product name "Polypropylene", manufactured by Test Piece Co., Ltd. AL: Aluminum alloy, product name "Aluminum alloy A5052", manufactured by Test Piece Co., Ltd. ABS: Acrylonitrile / butadiene / styrene copolymer, product name "ABS", manufactured by Test Piece Co., Ltd. PET: Polyethylene terephthalate, product name "Polyethylene terephthalate", manufactured by Test Piece Co., Ltd. Rosin ester: Rosin ester, product name "Super Ester W-125", weight average molecular weight: 2,500, acid value (mgKOH / g): 14.3, manufactured by Arakawa Chemical Industries, Ltd.
[0174] 2. Measurement of melting point and heat of fusion The melting point and heat of fusion were determined using a differential scanning calorimeter (TA Instruments; DSC-Q1000). The temperature was raised from 30°C to 180°C at 10°C / min, then lowered to 0°C at 10°C / min, and then raised again to 150°C at 10°C / min. The melting point and heat of fusion were determined according to JIS K 7122 from the thermogram at the second temperature rise.
[0175] 3. Measurement of weight average molecular weight The weight average molecular weight was measured by GPC using a gel permeation chromatograph (Shimadzu Corporation; LC-10 series) under the following measurement conditions. Detector: Shimadzu Corporation; C-R4A Column: TSKG 6000H-TSKG 4000H-TSKG 3000H-TSKG 2000H (manufactured by Tosoh Corporation) Mobile phase: tetrahydrofuran Temperature: 40℃ Flow rate: 0.8ml / min Sample concentration: 3000ppm Injection volume: 100μl
[0176] The weight average molecular weight was calculated using a calibration curve prepared from monodisperse standard polystyrene.
[0177] 4. Propylene content and ethylene content In the production example 1 described later, the propylene content in the propylene / 1-butene copolymer is 13 This was determined using C-NMR.
[0178] In addition, in Production Example 4 described later, the ethylene content of the ethylene / propylene copolymer is 13 This was determined using C-NMR.
[0179] 5. Denaturation amount In Production Examples 2 and 3 described later, the modification amount of the polar group-containing monomer per 100 parts by mass of the copolymer is 1 H-NMR was used to determine this.
[0180] 6. Measurement of kinematic viscosity at 40℃ Measured according to ASTM D 445.
[0181] 7. Measurement of kinetic viscosity at 200℃ Measurements were performed based on JIS K 2283.
[0182] 8. Preparation of Olefin Polymers Production Example 1 (First Olefin Polymer) In a 2-liter autoclave that had been thoroughly purged with nitrogen, 900 ml of hexane as a solvent and 90 g of 1-butene were charged. Then, 1 mmol of triisobutylaluminum was added, and the temperature was raised to 70°C. Then, propylene was fed to a total pressure of 7 kg / cm. 2G, 0.30 mmol of methylaluminoxane and 0.001 mmol of rac-dimethylsilylene-bis{1-(2-methyl-4-phenylindenyl)}zirconium dichloride (calculated as Zr atom) were added, and propylene was continuously fed to maintain the total pressure at 7 kg / cm 2 The polymerization was carried out for 30 minutes while maintaining the temperature at 100°C. As a result, a propylene / 1-butene copolymer (first olefin polymer) was obtained. After that, the first olefin polymer was recovered in a large amount of methanol after degassing, and dried under reduced pressure at 110°C for 12 hours. The melting point of the propylene / 1-butene copolymer was 78.3°C. The heat of fusion of the propylene / 1-butene copolymer was 29.2 J / g. The weight average molecular weight of the propylene / 1-butene copolymer was 330,000. The propylene content of the propylene / 1-butene copolymer was 67.2 mol%. The results of the melting point, heat of fusion, and weight average molecular weight are shown in Table 1.
[0183] Production Example 2 (Second Olefin Polymer) 3 kg of the propylene / 1-butene copolymer of Production Example 1 was added to 10 L of toluene, and the temperature was raised to 145° C. under a nitrogen atmosphere, and the propylene / 1-butene copolymer of Production Example 1 was dissolved in toluene. Next, 382 g of maleic anhydride as a polar group-containing monomer and 175 g of di-tert-butyl peroxide as a radical polymerization initiator were fed under stirring over 4 hours, and the mixture was stirred at 145° C. for 2 hours. As a result, a maleic anhydride-modified propylene / 1-butene copolymer (second olefin polymer) was obtained. Then, the mixture was cooled, and a large amount of acetone was added to precipitate the maleic anhydride-modified propylene / 1-butene copolymer. Then, the mixture was filtered, washed with acetone, and vacuum dried.
[0184] The melting point of the maleic anhydride modified propylene / 1-butene copolymer was 75.8°C. The heat of fusion of the maleic anhydride modified propylene / 1-butene copolymer was 28.6 J / g. The weight average molecular weight of the maleic anhydride modified propylene / 1-butene copolymer was 110,000. The amount of modification with maleic anhydride in the maleic anhydride modified propylene / 1-butene copolymer was 1 part by mass per 100 parts by mass of the maleic anhydride modified propylene / 1-butene copolymer. The results of the melting point, heat of fusion, weight average molecular weight and modification amount are shown in Table 1.
[0185] Production Example 3 3 kg of styrene / ethylene / 1-butene / styrene copolymer (G1652M, Kraton) was added to 10 L of toluene, and the temperature was raised to 145° C. under a nitrogen atmosphere, and the styrene / ethylene / 1-butene / styrene copolymer was dissolved in toluene. Next, 382 g of maleic anhydride and 175 g of di-tert-butyl peroxide were fed under stirring over 4 hours, and the mixture was stirred at 145° C. for 2 hours. This resulted in maleic anhydride-modified styrene / ethylene / 1-butene / styrene. After that, the mixture was cooled and a large amount of acetone was added to precipitate maleic anhydride-modified styrene / ethylene / 1-butene / styrene. After that, the mixture was filtered, washed with acetone, and then vacuum dried.
[0186] The melting point and heat of fusion of the maleic anhydride-modified styrene / ethylene / 1-butene / styrene were not observed. The weight average molecular weight of the maleic anhydride-modified styrene / ethylene / 1-butene / styrene was 100,000. The modification amount of maleic anhydride in the maleic anhydride-modified styrene / ethylene / 1-butene / styrene was 2 parts by mass per 100 parts by mass of the maleic anhydride-modified styrene / ethylene / 1-butene / styrene. The results of the melting point, heat of fusion, weight average molecular weight and modification amount are shown in Table 1.
[0187] 9. Preparation of synthetic hydrocarbon oil Production Example 4 1 L of dehydrated and purified hexane was added to a continuous polymerization reactor equipped with an agitator that had been thoroughly purged with nitrogen. Then, ethylaluminum sesquichloride (Al(C)) adjusted to 96 mmol / L was added. 2 H 5 ) 1.5 ·Cl 1.5 A hexane solution of VO(OC) was continuously fed at a rate of 500 ml / h for 1 hour. Then, a 16 mmol / L solution of VO(OC) was added as a catalyst. 2 H 5 ) C l2 A hexane solution of the above was continuously fed at 500 ml / hour. Meanwhile, the polymerization liquid was continuously extracted from the top of the polymerization vessel so that the polymerization liquid in the polymerization vessel was always 1 liter. Next, ethylene gas was fed at 47 L / hour, propylene gas at 47 L / hour, and hydrogen gas at 20 L / hour using a bubbling tube. The copolymerization reaction was carried out at 35°C by circulating a coolant through a jacket attached to the outside of the polymerization vessel. The obtained polymerization solution was deashed with hydrochloric acid, then poured into a large amount of methanol to precipitate, and then dried under reduced pressure at 130°C for 24 hours. As a result, an ethylene / propylene copolymer (hydrocarbon-based synthetic oil) was obtained.
[0188] The ethylene / propylene copolymer had an ethylene content of 55.9 mol%. The ethylene / propylene copolymer had a weight average molecular weight of 14,000. The 40°C kinematic viscosity of the ethylene / propylene copolymer was 37,500 mm 2 The 200°C kinematic viscosity of the ethylene / propylene copolymer was 132 mm 2 / second.
[0189] 10. Manufacturing of decorative sheets Example 1 80 parts by mass of the propylene / 1-butene copolymer of Production Example 1 and 20 parts by mass of the hydrocarbon synthetic oil of Production Example 4 were dissolved under heating in 400 parts by mass of a mixed solvent of methylcyclohexane / ethyl acetate = 80 / 20, thereby obtaining an adhesive composition.
[0190] Next, the adhesive composition was applied to one surface in the thickness direction (corona-treated surface) of "Himilan 1601" (A-1) as a decorative layer using an applicator. As a result, an adhesive layer (15 g / m 2 ) was placed on the sheet. In this way, a decorative sheet was produced.
[0191] Next, the object to be decorated was decorated using this decorative sheet. Specifically, "polypropylene" (PP) was placed on a vertically adjustable table installed in a "double-sided vacuum molding device NGF-0404" manufactured by Fuse Vacuum Co., Ltd., which consists of an upper and lower box. Next, the decorative sheet was set in a sheet clamp frame located above the molding substrate (molded product) of the double-sided vacuum molding device. Next, the pressure in the upper and lower boxes was reduced to 99.0 kPa, and the temperature of the decorative sheet was heated to 110°C using a near-infrared heater, and the molding substrate was raised to pressure-bond the molding substrate and the painted decorative sheet, which was held for 5 seconds. After that, only the upper box was released to atmospheric pressure. This decorated the object to be decorated.
[0192] Examples 2 to 7 and Comparative Examples 1 to 3 According to Table 2, a decorative sheet was produced in the same manner as in Example 1, and an object to be decorated was decorated.
[0193] 11. Evaluation <Adhesiveness> (110℃ laminated appearance) After the object to be decorated was decorated (after the decorative sheet was pressure-bonded at 110° C.), the appearance of the decorative sheet was evaluated based on the following criteria. The results are shown in Table 1. ◯: No wrinkles were observed on the decorative sheet. ×: Wrinkles were observed on the decorative sheet.
[0194] (110℃ lamination adhesive strength) The decorated object was cut into a piece 15 mm wide to prepare a test piece. A 180° peel test was carried out on this test piece using a universal tensile tester at a crosshead speed of 200 mm / min to peel the decorative sheet from the object to be decorated and measure the peel strength. The results are shown in Table 1. The peel strength was also evaluated based on the following criteria. The results are shown in Table 1.
[0195] (Scratch resistance) The gloss (gloss before abrasion) of the surface (decorative layer) of the decorated object was measured using a gloss meter. Next, the surface (decorative layer) of the decorated object was reciprocated 10 times with #0000 steel wool under a load of 500 g (the decorative layer was rubbed). The gloss (gloss after abrasion) of the decorative layer after rubbing was measured using a gloss meter. The rate of change in gloss was then calculated based on the following formula (2). A lower rate of change in gloss indicates better scratch resistance. The results are shown in Table 2. Glossiness change rate = (glossiness before abrasion - glossiness after abrasion) / glossiness before abrasion x 100 (2)
[0196] (Xylene rubbing resistance) The surface of the decorated object (decorative layer) was measured for gloss (gloss before abrasion) using a gloss meter. Next, the surface of the decorated object (decorative layer) was rubbed 50 times with Bemcot M-1 soaked in xylene (the decorative layer was rubbed). The decorative layer after rubbing was measured for gloss (gloss after abrasion) using a gloss meter. The rate of change in gloss was then calculated based on the above formula (2). A lower rate of change in gloss indicates better resistance to xylene rubbing. The results are shown in Table 2.
[0197] (Chemical resistance) Based on ASTM D-543, a chemical resistance test was conducted using a 10% sodium hydroxide solution (manufactured by Wako Pure Chemical Industries, Ltd.). Specifically, the decorated object was immersed in a 10% sodium hydroxide solution at 23°C for 7 days. The chemical resistance was evaluated based on the following criteria. The results are shown in Table 1. ◯: The decorative layer did not peel off. ×: The decorative layer peeled off.
[0198] [Table 1]
[0199] [Table 2] [Explanation of symbols]
[0200] 1 Decorative sheet 2 Decorative layer 3 Adhesive layer
Claims
1. A decorative layer and an adhesive layer are provided in this order toward one side in a thickness direction, the decorative layer contains an ionomer resin in which an ethylene-unsaturated carboxylic acid copolymer is neutralized with a monovalent metal and / or a divalent metal, and does not contain a partially crosslinked olefin-based thermoplastic elastomer; the monovalent metal is sodium; the divalent metal is zinc; The adhesive layer is made of an adhesive composition, The adhesive composition comprises an olefin polymer, The olefin polymer has a heat of fusion of 0 J / g or more and 50 J / g or less as measured in accordance with JIS K7122, and a weight average molecular weight of 1×10 or less as measured by a GPC method. 4 That's it, 1000 x 10 4 Below is the decorative sheet.
2. The decorative sheet according to claim 1 , wherein the olefin polymer comprises the following first olefin polymer and / or the following second olefin polymer: First olefin polymer: an olefin polymer containing a structural unit derived from an α-olefin having 2 to 20 carbon atoms Second olefin polymer: a polymer containing structural units derived from an α-olefin having 2 to 20 carbon atoms, a part or the whole of which has been graft-modified with a polar group-containing monomer.
3. the olefin polymer comprises the second olefin polymer, The decorative sheet according to claim 2 , wherein the second olefin polymer contains from 0.1 parts by mass to 15 parts by mass of a constituent unit derived from a polar group-containing monomer relative to 100 parts by mass of the second olefin polymer.
4. In the first olefin polymer or the second olefin polymer, The structural unit derived from an α-olefin having 2 to 20 carbon atoms includes a structural unit derived from propylene, 4. The decorative sheet according to claim 2 or 3, wherein the content of the propylene-derived structural units is 50 mol% or more and 100 mol% or less, and the content of the carbon number 2 to 20 α-olefin (excluding propylene)-derived structural units is 0 mol% or more and 50 mol% or less, relative to 100 mol% of the total amount of the propylene-derived structural units and the carbon number 2 to 20 α-olefin (excluding propylene).
5. 5. The decorative sheet according to claim 2, wherein the polar group-containing monomer is an unsaturated carboxylic acid and / or an unsaturated carboxylic acid anhydride.
6. The adhesive composition comprises a synthetic hydrocarbon oil or a semi-solid hydrocarbon, The hydrocarbon synthetic oil has a kinetic viscosity of 30 mm at 40°C. 2 / second or more, 500000mm 2 / sec or less, The semi-solid hydrocarbon has a kinetic viscosity of 1000 mm at 200° C. 2 / sec or more 100000mm 2 The decorative sheet according to any one of claims 1 to 5, wherein the thickness of the decorative sheet is less than or equal to 1 / second.
7. per 100 parts by mass of the total amount of the olefin polymer and the hydrocarbon-based synthetic oil or the semi-solid hydrocarbon, The blending ratio of the olefin polymer is 10 parts by mass or more and 99 parts by mass or less, The decorative sheet according to claim 6 , wherein the blending ratio of the hydrocarbon synthetic oil or the semi-solid hydrocarbon is from 1 part by mass to 90 parts by mass.
Citation Information
Patent Citations
Laminate and manufacture thereof
JP1993042619A
Substrate film for transferring and decorating
JP2017160339A
Coating agent, decorative film and molded body
WO2013164976A1
Composition, coating agent, adhesive, and laminate
WO2018221331A1