Manufacturing method of carbon nanotube composite member

By employing an adhesive with a lower thermal expansion coefficient and a support member, the method addresses solvent-induced wrinkling in carbon nanotube heaters, enhancing the reliability and appearance of carbon nanotube composite members.

JP7578569B2Active Publication Date: 2024-11-06CANADEVIA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021152917
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-01
Filing Date
2021-09-21
Publication Date
2024-11-06
Estimated Expiration
2041-09-21

AI Technical Summary

Technical Problem

The issue of solvent evaporation causing substrate swelling and adhesive wrinkling in carbon nanotube heaters due to thermal expansion during baking, leading to potential malfunction and appearance deterioration.

Method used

A manufacturing method involving the use of an adhesive with a lower thermal expansion coefficient than the substrate, combined with a support member having an even lower expansion coefficient, to stabilize the substrate during solvent removal and sealing, thereby preventing adhesive wrinkling.

Benefits of technology

The method effectively suppresses adhesive wrinkling and improves the appearance and sealing performance of carbon nanotube composite members by controlling thermal expansion, ensuring reliable operation and enhanced durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578569000002
    Figure 0007578569000002
  • Figure 0007578569000003
    Figure 0007578569000003
  • Figure 0007578569000004
    Figure 0007578569000004
Patent Text Reader

Abstract

To suppress the generation of wrinkles in a pressure-sensitive adhesive.SOLUTION: A manufacturing method of a CNT composite member comprises: a step (a step S11) of adhering a pressure-sensitive adhesive having a thermal expansion coefficient smaller than that of a first sheet portion to at least a circumference region of one main surface of the first sheet portion; a step (a step S12) of arranging a pair of electrodes and a CNT formation body connecting the pair of electrodes onto an upper surface of the first sheet portion; a step (a step S13) of fixing a support member having the thermal expansion coefficient smaller than that of the first sheet portion to the first sheet portion; a step (a step S14) of evaporating a solvent immersed into a connection sheet portion thereby removing the same by heating the connection sheet portion; and a step (a step S16) of nipping and laminating the first and second sheet portions between the connection sheet portion and the pressure-sensitive adhesive, fixing the second sheet portion with the pressure-sensitive adhesive to the first sheet portion, and sealing the connection sheet portion. Thus, the generation of wrinkles in the pressure-sensitive adhesive can be suppressed.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a carbon nanotube composite member. [Background technology]

[0002] In recent years, it has been proposed to mold multiple carbon nanotubes into various shapes and use them in various products such as heaters, sensors, etc. For example, Patent Document 1 proposes a heater in which a carbon nanotube film, which is a heating element, is sandwiched between two substrates, and the two substrates and the carbon nanotube film are bonded together with hot melt glue. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 5721995 Summary of the Invention [Problem to be solved by the invention]

[0004] Incidentally, when manufacturing a carbon nanotube film, a solvent such as ethanol may be applied to the carbon nanotube film in order to aggregate a large number of carbon nanotubes. The solvent is removed to some extent by a drying process after the aggregation, but remains adsorbed between the many carbon nanotubes. Therefore, when the carbon nanotube film is sealed between substrates to form a heater, the heat generated when the heater is used may evaporate the solvent between the substrates, causing the substrates to bulge outward, resulting in abnormal heating.

[0005] Therefore, it is considered to fix the carbon nanotube film and the electrodes to the main surface of one of the substrates via an adhesive such as double-sided adhesive tape, and then perform a heating treatment such as baking to remove the solvent adsorbed on the carbon nanotube film. In this case, after baking, the other substrate is laminated on the one substrate, and the substrates are joined to each other via the above-mentioned adhesive around the periphery of the carbon nanotube film, but wrinkles may occur in the adhesive during baking, which may cause sealing problems or deterioration of the appearance. It is believed that the wrinkles are caused by the adhesive being irreversibly stretched due to the relatively large thermal expansion of the substrate during baking.

[0006] The present invention has been made in consideration of the above problems, and has an object to suppress the occurrence of wrinkles in an adhesive material. [Means for solving the problem]

[0007] The invention described in claim 1 is a method for manufacturing a carbon nanotube composite member, comprising the steps of: a) attaching an adhesive having a smaller thermal expansion coefficient than the first sheet portion to at least a peripheral region of one main surface of a first sheet portion; b) arranging a pair of electrodes and a carbon nanotube molding connecting the pair of electrodes on the one main surface of the first sheet portion; c) fixing a support member having a smaller thermal expansion coefficient than the first sheet portion to the first sheet portion; d) after steps a) to c), heating the carbon nanotube molding to evaporate and remove the solvent impregnated in the carbon nanotube molding; and e) after step d), stacking the first sheet portion and the second sheet portion with the carbon nanotube molding and the adhesive sandwiched between them, and fixing the second sheet portion to the first sheet portion with the adhesive to seal the carbon nanotube molding.

[0008] A second aspect of the present invention provides the method for producing a carbon nanotube composite member according to the first aspect, further comprising, after the step d), a step of removing the support member from the first sheet portion.

[0009] The invention recited in claim 3 is the method for producing a carbon nanotube composite member recited in claim 1 or 2, wherein in the step c), the support member is fixed onto the other main surface of the first sheet portion.

[0010] The invention described in claim 4 is a method for manufacturing a carbon nanotube composite material described in any one of claims 1 to 3, wherein in step c), the support member is fixed at a position on the peripheral region overlapping the adhesive material.

[0011] The invention described in claim 5 is a method for manufacturing a carbon nanotube composite material described in claim 4, wherein in step c), the support member is fixed to the peripheral region along a direction from one of the pair of electrodes to the other.

[0012] The invention described in claim 6 is a method for manufacturing a carbon nanotube composite material described in any one of claims 1 to 5, wherein in step a), the adhesive is applied over the entire surface of one of the main surfaces of the first sheet portion.

[0013] The invention described in claim 7 is a method for manufacturing a carbon nanotube composite material described in any one of claims 1 to 6, wherein the carbon nanotube molding is an electric heating part that generates heat by electricity supplied between the pair of electrodes and heats an object.

[0014] The invention described in claim 8 is a method for manufacturing a carbon nanotube composite material described in any one of claims 1 to 7, wherein the adhesive material is a double-sided adhesive tape having adhesive layers on both sides of a sheet-shaped substrate.

[0015] The invention described in claim 9 is a method for manufacturing a carbon nanotube composite material described in any one of claims 1 to 8, further comprising: f) a step of attaching another adhesive material to a main surface of the second sheet portion prior to step e), and step e) comprises: g) a step of stacking the second sheet portion on the first sheet portion, the adhesive material and the carbon nanotube molding while facing the carbon nanotube molding and the other adhesive material; h) a step of pressing the first sheet portion and the second sheet portion stacked in step g) against each other to fix them; and i) a step of heating the other adhesive material to a predetermined post-treatment temperature after step h).

[0016] A tenth aspect of the present invention provides the method for producing a carbon nanotube composite material according to the ninth aspect, wherein the Arrhenius parameter during heating in the step i) is 1.05 or more. Effect of the Invention

[0017] In the present invention, the occurrence of wrinkles in the adhesive material can be suppressed. [Brief description of the drawings]

[0018] [Figure 1] 1 is a plan view of a CNT composite material according to a first embodiment. [Diagram 2] FIG. 2 is a cross-sectional view of a CNT composite member. [Diagram 3] FIG. 2 is a cross-sectional view of a CNT composite member. [Figure 4] FIG. 1 is a diagram showing a manufacturing flow of a CNT composite material. [Diagram 5] FIG. 2 is a plan view of a CNT composite member in the process of being manufactured. [Figure 6] FIG. 2 is a plan view of a CNT composite member in the process of being manufactured. [Figure 7] FIG. 2 is a plan view of a CNT composite member in the process of being manufactured. [Figure 8] FIG. 2 is a bottom view of a CNT composite member in the process of being manufactured. [Figure 9] FIG. 2 is a side view showing a laminator used in manufacturing a CNT composite member. [Figure 10] FIG. [Figure 11] FIG. 11 is a cross-sectional view of a CNT composite material according to a second embodiment. [Figure 12] FIG. 1 is a diagram showing a part of the manufacturing flow of a CNT composite material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] FIG. 1 is a plan view showing a carbon nanotube composite member 1 (hereinafter also referred to as "CNT composite member 1") according to a first embodiment of the present invention. FIG. 2 is a cross-sectional view of the CNT composite member 1 cut at the position II-II in FIG. 1. FIG. 3 is a cross-sectional view of the CNT composite member 1 cut at the position III-III in FIG. 1. In the following description, the left-right direction in FIG. 1 is also referred to as the "longitudinal direction", and the up-down direction in FIG. 1 is also referred to as the "width direction". Furthermore, the direction perpendicular to the paper surface in FIG. 1 is also referred to as the "up-down direction". The up-down direction may or may not coincide with the actual direction of gravity.

[0020] In this embodiment, the CNT composite material 1 is a relatively thin carbon nanotube heater (hereinafter, also referred to as a "CNT heater") that generates heat when supplied with electric power and is used to heat an object. In the example shown in FIG. 1, the CNT composite material 1 is a sheet-like member that is substantially rectangular in plan view. In this specification, the term "sheet-like" refers to a shape that is thin relative to its length and width, and may or may not be flexible. In addition, in this specification, the term "sheet-like" is a concept that also includes a shape called a film-like shape.

[0021] The CNT composite member 1 includes a connecting sheet portion 21, a pair of electrodes 22, a first sheet portion 31, and a second sheet portion 32. In the following description, the connecting sheet portion 21 and the pair of electrodes 22 are collectively referred to as the CNT device 2. The CNT device 2 is sandwiched and sealed between the first sheet portion 31 and the second sheet portion 32. That is, the first sheet portion 31 and the second sheet portion 32 are exterior members that house (i.e., cover) and fix the CNT device 2. In the example shown in FIG. 1, the entire CNT device 2 is sealed between the first sheet portion 31 and the second sheet portion 32.

[0022] In addition, as for sealing of the CNT device 2 by the first sheet portion 31 and the second sheet portion 32, as long as the entire connecting sheet portion 21 is sealed, the pair of electrodes 22 may be partially sealed. That is, the entire connecting sheet portion 21 and a part of each electrode 22 may be sealed between the first sheet portion 31 and the second sheet portion 32, and the other part of each electrode 22 may protrude outward from between the first sheet portion 31 and the second sheet portion 32. Alternatively, the pair of electrodes 22 may be exposed in its entirety without being covered by the first sheet portion 31 and the second sheet portion 32.

[0023] The first sheet portion 31 and the second sheet portion 32 are each a substantially sheet-like member that extends in the longitudinal direction and the width direction. In the example shown in FIG. 1, the first sheet portion 31 and the second sheet portion 32 are each a substantially rectangular shape in a plan view having sides that are substantially parallel to the longitudinal direction and the width direction. The first sheet portion 31 and the second sheet portion 32 are each a flexible insulating sheet-like member. The first sheet portion 31 and the second sheet portion 32 are made of, for example, a resin or an elastic polymer material, and in this embodiment, are made of silicone rubber. The first sheet portion 31 and the second sheet portion 32 are, for example, a transparent or semi-transparent member. The first sheet portion 31 and the second sheet portion 32 may be opaque. The first sheet portion 31 and the second sheet portion 32 do not necessarily have to be flexible and may be a hard member. Furthermore, the first sheet portion 31 and the second sheet portion 32 may be made of different materials, colors, etc.

[0024] In the example shown in FIG. 1 to FIG. 3, the first sheet portion 31 and the second sheet portion 32 are fixed by a sheet-like adhesive material 33 over substantially the entire circumference around the CNT device 2. In FIG. 1, the adhesive material 33 is omitted from the illustration in order to facilitate understanding of the figure. In this embodiment, the adhesive material 33 is a double-sided adhesive tape in which an adhesive layer is provided on both sides of a sheet-like base material. The base material of the adhesive material 33 is made of, for example, resin, and in this embodiment, is PET (polyethylene terephthalate). In a temperature range of 0°C to 200°C, the thermal expansion coefficient (i.e., linear expansion modulus) of the adhesive material 33 is smaller than the thermal expansion coefficient of the first sheet portion 31. In detail, the thermal expansion coefficient of the base material of the adhesive material 33 in the above temperature range is smaller than the thermal expansion coefficient of the first sheet portion 31 in the above temperature range. In the following description, the thermal expansion coefficient in a temperature range of 0°C to 200°C is simply called the "thermal expansion coefficient". The thermal expansion coefficient of the above-mentioned PET is 65 ppm / °C (ie, ppm / K), and the thermal expansion coefficient of silicone rubber is 250 to 400 ppm / °C.

[0025] The pair of electrodes 22 are disposed facing each other with a space therebetween in the longitudinal direction. Each of the pair of electrodes 22 is a sheet-like (e.g., thin plate-like) member having a substantially rectangular band shape extending substantially linearly along the width direction. In the example shown in FIG. 1, the longitudinal distance between the pair of electrodes 22 is substantially the same at any position in the width direction. In other words, the pair of electrodes 22 extend substantially parallel to each other in the width direction. Each electrode 22 is an electric conductor, and is, for example, a metal foil made of copper (Cu) or the like. The thickness of each electrode 22 is, for example, 20 μm to 300 μm, and preferably 40 μm to 100 μm. The thermal expansion coefficient of Cu forming the electrode 22 and the support member 41 described later is 17.7 ppm / °C.

[0026] The connection sheet portion 21 extends in the longitudinal direction from one electrode 22 to the other electrode 22, and electrically connects the pair of electrodes 22. The connection sheet portion 21 is a conductive sheet member. Both longitudinal ends of the connection sheet portion 21 are fixed to the pair of electrodes 22. The connection sheet portion 21 and the electrode 22 are fixed, for example, by sandwiching the longitudinal end of the connection sheet portion 21 between two stacked sheets of metal foil and soldering the two sheets of metal foil. In this case, the two stacked sheets of metal foil become one electrode 22. Alternatively, the connection sheet portion 21 and the electrode 22 may be fixed by folding and pressing the metal foil that becomes the electrode 22 with the longitudinal end of the connection sheet portion 21 sandwiched therebetween. The connection sheet portion 21 may be fixed to the electrode 22 by a fixing method other than the above.

[0027] The connecting sheet portion 21 is a flexible sheet-like carbon nanotube molded body (hereinafter also referred to as a "CNT molded body") formed from a large number of carbon nanotubes. The connecting sheet portion 21 is, for example, a laminated sheet-like member in which a plurality of carbon nanotube sheets (hereinafter also referred to as "CNT sheets") are laminated in the thickness direction (i.e., the up-down direction). The number of stacked CNT sheets in the connecting sheet portion 21 may be changed in various ways. Alternatively, the connecting sheet portion 21 may be a single layer of a CNT sheet.

[0028] The shape of the connecting sheet portion 21 in a plan view is generally rectangular with sides generally parallel to the longitudinal direction and width direction, similar to the first sheet portion 31 and the second sheet portion 32. The connecting sheet portion 21 is smaller than the first sheet portion 31 and the second sheet portion 32. In a plan view, the connecting sheet portion 21 entirely overlaps with the first sheet portion 31 and the second sheet portion 32. In the example shown in FIG. 1, the pair of electrodes 22 also entirely overlap with the first sheet portion 31 and the second sheet portion 32 in a plan view.

[0029] The orientation of the carbon nanotubes in the connecting sheet portion 21 (i.e., the direction in which the carbon nanotubes extend) is approximately parallel to the longitudinal direction. In other words, in the multiple CNT sheets that constitute the connecting sheet portion 21, the numerous carbon nanotubes that constitute each CNT sheet extend approximately parallel to the longitudinal direction. Note that the orientation of the carbon nanotubes in the connecting sheet portion 21 may be changed in various ways, and may be, for example, approximately parallel to the width direction.

[0030] The size of the connecting sheet portion 21 varies depending on the performance required for the CNT heater 1. The length of the connecting sheet portion 21 in the longitudinal direction is, for example, 20 mm to 500 mm, and preferably 20 mm to 200 mm. The width of the connecting sheet portion 21 in the width direction is, for example, 10 mm to 500 mm, and preferably 60 mm to 150 mm.

[0031] The CNT composite material 1 further includes a pair of terminals (not shown). The pair of terminals are electrically connected to the pair of electrodes 22, respectively. Power is supplied between the pair of electrodes 22 of the CNT device 2 from a power supply source via the pair of terminals. This causes the connection sheet portion 21 of the CNT device 2 to generate heat and heat the target object. The connection sheet portion 21 is an electric heating portion that heats the target object.

[0032] Next, a method for producing the CNT composite material 1 will be described with reference to Fig. 4 to Fig. 8. Fig. 4 is a diagram showing the flow of producing the CNT composite material 1. Figs. 5 to 8 are diagrams showing the CNT composite material 1 in the process of being produced.

[0033] When the CNT composite member 1 is manufactured, first, as shown in Fig. 5, an adhesive material 33, which is a double-sided adhesive tape having a substantially rectangular strip shape, is attached to one main surface 311 (hereinafter also referred to as "upper surface 311") of the first sheet portion 31 (step S11). In Fig. 5, the adhesive material 33 is indicated with parallel diagonal lines to facilitate understanding of the figure (the same applies to Figs. 6 and 7). In the example shown in Fig. 5, the adhesive material 33 extends substantially parallel to the longitudinal direction and is arranged in the width direction, and is attached to substantially the entire upper surface 311 of the first sheet portion 31.

[0034] Next, as shown in FIG. 6, the lower layer portion of each electrode 22 having a laminated structure is placed on the upper surface 311 of the first sheet portion 31. The lower layer portion is fixed on the first sheet portion 31 by an adhesive 33. Next, as shown in FIG. 7, the connecting sheet portion 21 is placed on the upper surface 311 of the first sheet portion 31 with both ends in the longitudinal direction overlapping the lower layer portions of the pair of electrodes 22. A solvent such as ethanol is applied to the CNT sheet constituting the connecting sheet portion 21 in the manufacturing stage for the purpose of agglomerating a large number of carbon nanotubes. The solvent is removed to some extent in a drying process during the manufacturing of the CNT sheet, but remains adsorbed between the large number of carbon nanotubes. Therefore, in the state shown in FIG. 7, the connecting sheet portion 21 is impregnated with the solvent.

[0035] When the connecting sheet portion 21 is placed on the first sheet portion 31, the upper layer portion of each electrode 22 is laminated on the above-mentioned lower layer portion and soldered. As a result, a pair of electrodes 22 is formed, and both longitudinal ends of the connecting sheet portion 21 are joined to the pair of electrodes 22. Furthermore, a portion of the connecting sheet portion 21 located between the pair of electrodes 22 in the longitudinal direction is fixed onto the first sheet portion 31 by an adhesive material 33. As a result, the connecting sheet portion 21 and the pair of electrodes 22 (i.e., the CNT device 2) are placed on the upper surface 311 of the first sheet portion 31 (step S12).

[0036] When the arrangement of the CNT device 2 is completed, the support member 41 is fixed onto the other main surface 312 (hereinafter also referred to as the "lower surface 312") of the first sheet portion 31 (step S13), as shown in Fig. 8. Fig. 8 is a bottom view showing the lower surface 312 of the first sheet portion 31 (i.e., a bottom view of the CNT composite member 1 in the process of being manufactured). In the example shown in Fig. 8, the support member 41 is a sheet-like (e.g., thin plate-like) member having a substantially rectangular band shape extending in a substantially linear manner.

[0037] The support member 41 is, for example, a metal foil made of copper (Cu) or the like. The thermal expansion coefficient of the support member 41 is smaller than that of the first sheet portion 31. Preferably, the thermal expansion coefficient of the support member 41 is smaller than that of the adhesive material 33 (in the above example, the thermal expansion coefficient of the base material of the adhesive material 33). The support member 41 is fixed to the first sheet portion 31 by a removable adhesive material (for example, a double-sided adhesive tape or an adhesive layer, etc.). The material of the support member 41 is not limited to metal, and may be variously changed to ceramics, resin, etc.

[0038] The support member 41 is fixed to the peripheral region 313 of the first sheet portion 31 along the longitudinal direction (i.e., the direction from one of the pair of electrodes 22 to the other) over substantially the entire longitudinal length of the first sheet portion 31. The peripheral region 313 of the first sheet portion 31 is a frame-shaped region along the outer periphery of the first sheet portion 31, and in the example shown in FIG. 8, is a substantially rectangular frame-shaped region indicated by a two-dot chain line. The peripheral region 313 is, for example, a region of the entire first sheet portion 31 excluding the smallest rectangular region circumscribing the CNT device 2 (i.e., the arrangement region of the CNT device 2). The support member 41 overlaps with the adhesive material 33 (see FIG. 7) attached on the peripheral region 313 on the upper surface 311 of the first sheet portion 31 in a plan view. The support member 41 may be fixed to the upper surface 311 of the first sheet portion 31. In this case, the support member 41 is fixed to the upper surface 311 of the first sheet portion 31 via an adhesive material 33, for example.

[0039] After steps S11 to S13 are completed, the CNT device 2 is heated together with the first sheet portion 31 and the support member 41. As a result, the solvent impregnated in the connecting sheet portion 21 of the CNT device 2 is vaporized and removed from the connecting sheet portion 21 (step S14). The heating in step S14 is performed, for example, in a baking furnace. The baking process of the CNT device 2 is performed, for example, at 100° C. to 200° C. for 0.5 hours to 5 hours. As a result, the solvent remaining in the connecting sheet portion 21 is almost completely removed from the connecting sheet portion 21. The heating method of the CNT device 2, the first sheet portion 31, and the support member 41 may be variously changed in terms of the heating apparatus, heating temperature, heating time, etc.

[0040] As described above, since the support member 41, which has a smaller thermal expansion coefficient than the first sheet portion 31, is fixed to the first sheet portion 31, the thermal expansion of the first sheet portion 31 is suppressed in the heat treatment of step S14. After the baking treatment is completed, the temperatures of the CNT device 2, the first sheet portion 31, and the support member 41 are lowered to room temperature (e.g., 25°C).

[0041] If the support member 41 is not fixed to the first sheet portion 31, the peripheral region 313 of the first sheet portion 31 to which the CNT device 2 is not fixed will experience relatively large thermal expansion since there is no restriction such as thermal expansion suppression by the CNT device 2. In particular, in a region of the peripheral region 313 away from the electrode 22, which has a smaller thermal expansion coefficient than the first sheet portion 31 (i.e., a region of the peripheral region 313 extending in a direction from one electrode 22 to the other electrode 22), the thermal expansion of the first sheet portion 31 will be large.

[0042] However, in the manufacture of the CNT composite member 1 according to the present embodiment, since the support member 41 is fixed on the peripheral region 313 along the direction from one electrode 22 to the other electrode 22, the thermal expansion of the first sheet portion 31 can be suitably suppressed even in the peripheral region 313. This makes it possible to suppress the adhesive material 33 attached to the first sheet portion 31 from being pulled by the thermally expanding first sheet portion 31 and expanding more than its own thermal expansion (i.e., the thermal expansion when the adhesive material 33 is heated in a state independent of the first sheet portion 31). In addition, as described above, since the thermal expansion coefficient of the support member 41 is smaller than the thermal expansion coefficient of the adhesive material 33, the thermal expansion of the first sheet portion 31 can be made closer to the thermal expansion of the adhesive material 33 itself. Therefore, it is possible to further suppress the adhesive material 33 from expanding more than its own thermal expansion. Therefore, it is possible to suppress or prevent the occurrence of wrinkles due to irreversible expansion in the adhesive material 33 after the temperature is lowered. It is preferable that wrinkles in the adhesive material 33 are suppressed to an extent that they are not visible in a visual appearance inspection.

[0043] When the temperature drop of the CNT device 2, the first sheet portion 31, and the support member 41 is completed, the support member 41 is peeled off and removed from the first sheet portion 31 (step S15). Then, the second sheet portion 32 is laminated on the upper surface 311 of the first sheet portion 31. In other words, the first sheet portion 31 and the second sheet portion 32 are laminated with the CNT device 2 (i.e., the connection sheet portion 21 and the pair of electrodes 22) and the adhesive material 33 sandwiched therebetween. Then, the second sheet portion 32 is fixed to the first sheet portion 31 by the adhesive material 33 around the CNT device 2 (i.e., in the peripheral region 313). As a result, the CNT device 2 is sealed between the first sheet portion 31 and the second sheet portion 32, and the manufacture of the CNT composite member 1 is completed (step S16).

[0044] The first sheet portion 31 and the second sheet portion 32 may be fixed to each other by, for example, a laminator in step S16. FIGS. 9 and 10 are a side view and a plan view, respectively, showing how the first sheet portion 31 and the second sheet portion 32 are fixed to each other by the laminator 5. In FIG. 9, the first sheet portion 31 and the second sheet portion 32 are shown in cross section. The laminator 5 includes two rolls 51 and 52 arranged adjacent to each other in the vertical direction in FIG. 9. In the laminator 5, the first sheet portion 31 and the second sheet portion 32, which have the CNT device 2 sandwiched therebetween, are fixed to each other by passing between the two rolls 51 and 52 while being pressed from the right side to the left side in FIG. 9 and FIG. 10.

[0045] In the laminator 5, at least one of the rolls 51, 52 may be heated to heat the first sheet portion 31 and the second sheet portion 32. In this case, the temperature of the first sheet portion 31 and the second sheet portion 32 while passing through the laminator 5 is, for example, 50° C. to 60° C. In addition, the time required for the first sheet portion 31 and the second sheet portion 32 to pass through the laminator 5 is, for example, about 1 second.

[0046] As shown in FIG. 10, when the first sheet part 31 and the second sheet part 32 sandwiching the CNT device 2 pass between the two rolls 51 and 52, the moving direction of the first sheet part 31 and the second sheet part 32 is preferably approximately parallel to the extending direction of the pair of electrodes 22 (i.e., the longitudinal direction of the pair of electrodes 22). This makes it possible to suppress the first sheet part 31 and the second sheet part 32 from wrinkling along the moving direction due to the force, heat, etc. applied from the rolls 51 and 52 and causing wrinkles. The suppression of the wrinkles is due to the rigidity of the pair of electrodes 22 suppressing partial deformation (for example, partial elongation due to the force or heat from the rolls 51 and 52) of the first sheet part 31 and the second sheet part 32 in the moving direction. In particular, the first sheet part 31 may be relatively easily deformed since it is heated in a baking furnace or the like in step S14 as described above. Therefore, when the first sheet portion 31 and the second sheet portion 32 are fixed by the laminator 5, it is preferable to use the pair of electrodes 22 to suppress deformation.

[0047] In the above-described method for producing the CNT composite member 1, in step S11, it is sufficient that the adhesive material 33 is attached to at least the peripheral region 313 of the upper surface 311 of the first sheet portion 31. Even in this case, in step S16, the second sheet portion 32 is fixed to the first sheet portion 31 via the adhesive material 33. In addition, in step S12, the CNT device 2 is placed on the upper surface 311 of the first sheet portion 31 without the adhesive material 33, and is fixed to the first sheet portion 31 by, for example, an adhesive or the like.

[0048] As described above, the method for producing the CNT composite material 1 includes a step of attaching an adhesive 33 having a smaller thermal expansion coefficient than that of the first sheet portion 31 to at least the peripheral region 313 of one main surface (i.e., the upper surface 311) of the first sheet portion 31 (step S11), a step of arranging a pair of electrodes 22 and a CNT molded body (i.e., the connecting sheet portion 21) connecting the pair of electrodes 22 on the upper surface 311 of the first sheet portion 31 (step S12), and a step of attaching a support member 41 having a smaller thermal expansion coefficient than that of the first sheet portion 31 to the first sheet portion 31. The method includes a step of fixing the connecting sheet portion 21 to the connecting sheet portion 21 (step S13), a step of heating the connecting sheet portion 21 to evaporate and remove the solvent impregnated in the connecting sheet portion 21 (step S14), and a step of laminating the first sheet portion 31 and the second sheet portion 32 with the connecting sheet portion 21 and the adhesive material 33 sandwiched therebetween and fixing the second sheet portion 32 to the first sheet portion 31 with the adhesive material 33 to seal the connecting sheet portion 21 (step S16).

[0049] In this manufacturing method, the support member 41 suppresses the thermal expansion of the first sheet portion 31, thereby suppressing the occurrence of wrinkles in the adhesive material 33 due to irreversible elongation of the adhesive material 33. As a result, the appearance of the CNT composite material 1 can be improved, and the sealing performance of the connecting sheet portion 21 can be improved.

[0050] As described above, it is preferable that the method for producing the CNT composite material 1 further includes, after step S14, a step (step S15) of removing the support member 41 from the first sheet portion 31. This can simplify the structure of the CNT composite material 1. It can also make the CNT composite material 1 smaller and lighter.

[0051] As described above, in step S13, it is preferable that the support member 41 is fixed onto the other main surface (i.e., the lower surface 312) of the first sheet portion 31. This allows the support member 41 to be arranged without considering interference between the connection sheet portion 21 and the electrodes 22 and the support member 41. This allows the degree of freedom in arranging the support member 41 on the first sheet portion 31 to be improved.

[0052] As described above, in step S13, the support member 41 is preferably fixed to a position overlapping the adhesive material 33 on the peripheral region 313. This makes it possible to suppress the elongation of the adhesive material 33 in the peripheral region 313 where the first sheet portion 31 is prone to thermal expansion (i.e., the adhesive material 33 is prone to elongation) due to no restriction by the CNT device 2.

[0053] As described above, in step S13, the support member 41 is preferably fixed to the peripheral region 313 along the direction from one of the pair of electrodes 22 to the other. This makes it possible to suppress elongation of the adhesive material 33 in a region of the peripheral region 313 that is away from the electrodes 22 and therefore where the first sheet portion 31 is likely to thermally expand (i.e., a region where the adhesive material 33 is likely to be stretched).

[0054] As described above, in step S11, the adhesive material 33 is preferably applied over the entire surface of the upper surface 311 of the first sheet portion 31. This allows both the first sheet portion 31 and the second sheet portion 32 to be fixed, and the CNT device 2 to the first sheet portion 31 to be fixed, by the adhesive material 33. As a result, the structure of the CNT composite material 1 can be simplified, and the manufacture of the CNT composite material 1 can be facilitated.

[0055] As described above, the connecting sheet portion 21 is preferably an electric heating portion that heats an object by generating heat due to power supplied between the pair of electrodes 22. In the manufacturing method of the CNT composite material 1 described above, the solvent impregnated in the connecting sheet portion 21 can be vaporized and removed while improving the appearance of the CNT composite material 1 and the sealing property of the connecting sheet portion 21, and therefore the manufacturing method is particularly suitable for the above structure in which the solvent is easily vaporized by the heat generated by the connecting sheet portion 21.

[0056] As described above, the adhesive material 33 is preferably a double-sided adhesive tape having adhesive layers provided on both sides of a sheet-like substrate. Since the above-mentioned method for producing the CNT composite material 1 can suppress the occurrence of wrinkles in the adhesive material 33, the method is particularly suitable for the case where the adhesive material 33 is a double-sided adhesive tape that is easily wrinkled when stretched by a relatively small force.

[0057] Next, a CNT composite member 1a according to a second embodiment of the present invention will be described. Fig. 11 is a cross-sectional view showing the CNT composite member 1a, and corresponds to Fig. 2 described above. In the CNT composite member 1a, in addition to the above-mentioned adhesive material 33, another adhesive material 34 is provided between the first sheet portion 31 and the second sheet portion 32. The other structures of the CNT composite member 1a are substantially similar to those of the above-mentioned CNT composite member 1. In the following description, the same reference numerals as the corresponding components of the CNT composite member 1 will be used for the components of the CNT composite member 1a.

[0058] The adhesive material 34 is, for example, a double-sided adhesive tape having adhesive layers provided on both sides of a sheet-like base material, similar to the adhesive material 33. The adhesive material 34 is, for example, a double-sided adhesive tape of the same type (i.e., having the same properties) as the adhesive material 33. Note that the adhesive material 34 may be a double-sided adhesive tape having properties different from those of the adhesive material 33.

[0059] The adhesive material 34 is attached to the lower surface of the second sheet portion 32 (i.e., the lower main surface in FIG. 11). The adhesive material 34 faces the CNT device 2 in the thickness direction and is bonded to at least the connecting sheet portion 21 of the CNT device 2. In the example shown in FIG. 11, the adhesive material 34 is provided over substantially the entire surface of the lower surface of the second sheet portion 32 and is bonded to substantially the entire CNT device 2 and the adhesive material 33 on the first sheet portion 31.

[0060] Next, a method for producing the CNT composite material 1a will be described with reference to Fig. 4 and Fig. 12. Fig. 12 is a diagram showing part of the flow of producing the CNT composite material 1a. When the CNT composite material 1a is produced, first, the above-mentioned steps S11 to S15 (see Fig. 4) are carried out in the same manner as in the production of the CNT composite material 1. Then, step S21 shown in Fig. 12 is carried out, and steps S22 to S24 are carried out. Steps S22 to S24 show the detailed flow of the above-mentioned step S16.

[0061] Specifically, first, the adhesive 33 is attached to the upper surface 311 (see FIG. 8) of the first sheet portion 31 (step S11), and the connecting sheet portion 21 and the pair of electrodes 22 (i.e., the CNT device 2) are arranged on the upper surface 311 of the first sheet portion 31 (step S12). Then, the support member 41 (see FIG. 8) is fixed on the lower surface 312 of the first sheet portion 31 (step S13), and the CNT device 2 is heated together with the first sheet portion 31 and the support member 41. As a result, the solvent impregnated in the connecting sheet portion 21 of the CNT device 2 is vaporized and removed from the connecting sheet portion 21 (step S14). The heating in step S14 is performed, for example, in a baking furnace at 100° C. to 200° C. for 0.5 to 5 hours. Thereafter, the support member 41 is peeled off and removed from the first sheet portion 31 (step S15).

[0062] After steps S11 to S15 are completed, the adhesive material 34 is attached to one main surface of the second sheet portion 32 (step S21). In this embodiment, the adhesive material 34 is attached over substantially the entire surface of the main surface of the second sheet portion 32. Next, the second sheet portion 32 is laminated on the first sheet portion 31 so as to cover the adhesive material 33 attached to the first sheet portion 31 and the CNT device 2 fixed on the adhesive material 33 (step S22). At this time, the adhesive material 34 attached to the second sheet portion 32 faces the CNT device 2 and the adhesive material 33 in the thickness direction and comes into contact with the CNT device 2 and the adhesive material 33.

[0063] Note that the above-mentioned step S21 may be performed at any timing before step S22. For example, step S21 may be performed in parallel with any of steps S11 to S15, may be performed between any of steps S11 to S15, or may be performed before step S11.

[0064] The first sheet portion 31 and the second sheet portion 32 laminated in step S22 are pressed against each other and fixed (step S23). The pressing in step S23 is performed, for example, by the above-mentioned laminator 5 (see Figs. 9 and 10). In the laminator 5, the first sheet portion 31 and the second sheet portion 32 sandwiching the CNT device 2 therebetween are passed between two rolls 51, 52 while being pressed against each other, as described above, and thereby fixed to each other.

[0065] As described above, in the laminator 5, the first sheet portion 31 and the second sheet portion 32 may be heated by heating at least one of the rolls 51, 52. In this case, the temperature of the first sheet portion 31 and the second sheet portion 32 while passing through the laminator 5 is, for example, 50° C. to 60° C. In addition, the time required for the first sheet portion 31 and the second sheet portion 32 to pass through the laminator 5 is, for example, about 1 second.

[0066] As described above, when the first sheet part 31 and the second sheet part 32 sandwiching the CNT device 2 therebetween pass between the two rolls 51, 52, the moving direction of the first sheet part 31 and the second sheet part 32 is preferably approximately parallel to the extending direction of the pair of electrodes 22 (i.e., the longitudinal direction of the pair of electrodes 22). This makes it possible to prevent the first sheet part 31 and the second sheet part 32 from undulating along the moving direction and generating wrinkles due to the force, heat, etc. applied from the rolls 51, 52.

[0067] In step S23, the second sheet portion 32 is pressed against the first sheet portion 31, so that the adhesive material 34 attached to the second sheet portion 32 is bonded to the adhesive material 34 on the first sheet portion 31, the connection sheet portion 21, and the pair of electrodes 22. The connection sheet portion 21 is composed of a large number of carbon nanotubes, and therefore has minute irregularities on its surface. Therefore, even after step S23 is completed, a minute space may remain between the adhesive material 34 bonded to the connection sheet portion 21 and the surface of the connection sheet portion 21. At the position where the minute space exists, the bonding strength between the adhesive material 34 and the connection sheet portion 21 is reduced, so that when the CNT composite member 1a is used as a CNT heater, the connection sheet portion 21 and the adhesive material 34 may easily peel off in a high-temperature environment.

[0068] Therefore, when step S23 is completed, an aging process is performed in which the adhesive 34 is heated to a predetermined post-treatment temperature to soften the adhesive 34 and make it conform to the surface of the connecting sheet portion 21 (step S24). As a result, even if a small space remains between the connecting sheet portion 21 and the adhesive 34 at the end of step S23, the space is reduced, improving the adhesion between the connecting sheet portion 21 and the adhesive 34. Also, if the first sheet portion 31 and the second sheet portion 32 are deformed (for example, curved) by passing through the laminator 5, the deformation is eliminated or reduced. When step S24 is completed and the first sheet portion 31, the second sheet portion 32, etc. are cooled to near room temperature, the production of the CNT composite member 1a is completed. The temperature reduction may be performed by natural cooling or by controlled cooling in which the temperature reduction rate is controlled.

[0069] Step S24 is performed, for example, by placing the first sheet portion 31 and the second sheet portion 32 fixed to each other with the CNT device 2, the adhesive material 33, and the adhesive material 34 sandwiched therebetween in a baking furnace and heating them at the above-mentioned post-treatment temperature for a predetermined time. The post-treatment temperature is equal to or lower than the heat-resistant temperature of the adhesive material 34 and equal to or higher than the softening temperature of the adhesive layer of the adhesive material 34. The post-treatment temperature is, for example, 60°C to 100°C, and is 80°C in this embodiment. The heating time in step S24 is, for example, 0.5 hours to 8 hours, and is 4 hours in this embodiment. The Arrhenius parameter E during heating in step S24 is preferably 1.05 or more. The Arrhenius parameter E is calculated by the following formula 1.

[0070] E=k B ×T×ln(vt) (Formula 1)

[0071] k in Eq. B is the Boltzmann constant (eV / K), T is the heating temperature (K), v is the frequency factor (1 / s), and t is the heating time (s).

[0072] The following Table 1 shows experimental results showing the relationship between the Arrhenius parameter E and the bonding state of the first sheet portion 31 and the second sheet portion 32. In Experimental Examples 1 to 6, the Arrhenius parameter E was changed by changing the heating temperature T and the heating time t. The Arrhenius parameter E is also expressed by k B is 0.0000861 (eV / K), and v is 1×10 11 It was calculated as (1 / s).

[0073] [Table 1]

[0074] The evaluation in Table 1 indicates whether the bonding state of the adhesive 34 to the connecting sheet portion 21 is good or bad. The evaluation was performed by supplying power to the CNT composite member 1a manufactured by steps S11 to S15 and S21 to S24 and visually observing the bonding state between the adhesive 34 and the connecting sheet portion 21 when used as a CNT heater. "△" in the evaluation column indicates that peeling has occurred between the adhesive 34 and the connecting sheet portion 21, and the ratio of the peeled area to the area of ​​the connecting sheet portion 21 is 10% or more. "○" in the evaluation column indicates that peeling has occurred between the adhesive 34 and the connecting sheet portion 21, and the ratio of the peeled area to the area of ​​the connecting sheet portion 21 is less than 5%. "◎" in the evaluation column indicates that substantially no peeling has occurred between the adhesive 34 and the connecting sheet portion 21.

[0075] In Experimental Examples 1 to 3, the heating temperature was 27°C (i.e., 300K), and the heating times were 3600 seconds, 57600 seconds, and 230400 seconds, respectively. The Arrhenius parameters E of Experimental Examples 1 to 3 were 0.87, 0.94, and 0.97, respectively, and all were evaluated as "△". In Experimental Examples 4 to 6, the heating temperature was 80°C (i.e., 353K), and the heating times were 3600 seconds, 7200 seconds, and 14400 seconds, respectively. The Arrhenius parameters E of Experimental Examples 4 to 6 were 1.02, 1.04, and 1.06, respectively. Experimental Examples 4 and 5 were evaluated as "○", and Experimental Example 6 was evaluated as "◎". From Experimental Examples 1 to 6, it is preferable that the Arrhenius parameter E is 1.05 or more.

[0076] As described above, the method for manufacturing the CNT composite material 1a includes a step of attaching an adhesive 33 having a smaller thermal expansion coefficient than that of the first sheet portion 31 to at least the peripheral region 313 of one main surface (i.e., the upper surface 311) of the first sheet portion 31 (step S11), a step of arranging a pair of electrodes 22 and a CNT molded body (i.e., the connecting sheet portion 21) connecting the pair of electrodes 22 on the upper surface 311 of the first sheet portion 31 (step S12), and a step of attaching a support member 41 having a smaller thermal expansion coefficient than that of the first sheet portion 31 to the first sheet portion 31. The method includes a step of fixing the connecting sheet portion 21 to the connecting sheet portion 21 (step S13), a step of heating the connecting sheet portion 21 to evaporate and remove the solvent impregnated in the connecting sheet portion 21 (step S14), and a step of laminating the first sheet portion 31 and the second sheet portion 32 with the connecting sheet portion 21 and the adhesive material 33 sandwiched therebetween and fixing the second sheet portion 32 to the first sheet portion 31 with the adhesive material 33 to seal the connecting sheet portion 21 (step S16).

[0077] The manufacturing method of the CNT composite member 1a further includes a step (step S21) of attaching another adhesive material 34 to the main surface of the second sheet portion 32 prior to step S16. Step S16 further includes a step (step S22) of stacking the second sheet portion 32 on the first sheet portion 31, the adhesive material 33, and the CNT device 2 while the CNT device 2 and the adhesive material 34 face each other, a step (step S23) of pressing the first sheet portion 31 and the second sheet portion 32 stacked in step S22 against each other to fix them, and a step (step S24) of heating the adhesive material 34 to a predetermined post-treatment temperature after step S23.

[0078] In this manufacturing method, similarly to the above, the thermal expansion of the first sheet portion 31 is suppressed by the support member 41, thereby making it possible to suppress the occurrence of wrinkles in the adhesive material 33 due to irreversible elongation of the adhesive material 33. Furthermore, the aging treatment in step S24 makes it possible to improve the adhesion between the connecting sheet portion 21 and the adhesive material 34. As a result, it is possible to suppress the adhesive material 34 from partially peeling off from the connecting sheet portion 21 and swelling in a high-temperature environment, which would result in a decrease in the sealing ability of the connecting sheet portion 21 and a decrease in the appearance of the CNT composite member 1.

[0079] As described above, the Arrhenius parameter E during heating in step S24 is preferably 1.05 or more, which can further improve the adhesion between the connecting sheet portion 21 and the adhesive material 34.

[0080] The above-mentioned method for producing the CNT composite materials 1 and 1a can be modified in various ways.

[0081] For example, the shape of the CNT composite members 1, 1a in a plan view is not limited to a substantially rectangular shape and may be modified in various ways. The shapes and arrangements of the connecting sheet portion 21 and the electrodes 22 may also be modified in various ways. The shapes of the first sheet portion 31 and the second sheet portion 32 may also be modified in various ways. For example, the second sheet portion 32 does not necessarily have to have the same shape as the first sheet portion 31, and may be smaller than the first sheet portion 31. The shape of the support member 41 may also be modified in various ways.

[0082] The CNT composite member 1, 1a may be provided with a film-like or thin-plate-like heat dissipation portion fixed to the outer surface of the first sheet portion 31 and / or the second sheet portion 32 by an adhesive or the like. The heat dissipation portion is, for example, a metal foil or a sheet-like member made of metal. The heat dissipation portion may be a thin metal film formed by deposition or the like on the outer surface of the first sheet portion 31 and / or the second sheet portion 32. The heat dissipation portion is a heat dissipation surface that equalizes and dissipates heat from the connecting sheet portion 21.

[0083] The adhesive material 33 does not necessarily have to be a double-sided adhesive tape, and may be modified in various ways. For example, the adhesive material 33 may be a thin film layer formed of an adhesive. The same applies to the adhesive material 34.

[0084] The support member 41 does not necessarily have to be fixed over substantially the entire length of the first sheet portion 31 in the longitudinal direction, and may be fixed to only a portion of the first sheet portion 31 in the longitudinal direction. Moreover, the support member 41 does not necessarily have to be fixed to the peripheral region 313 along the longitudinal direction, and may be fixed to the peripheral region 313 along a direction other than the longitudinal direction. The support member 41 does not necessarily have to be fixed to a position overlapping the adhesive material 33 in a plan view. The support member 41 does not necessarily have to be fixed to the peripheral region 313, and may be fixed to various positions on the first sheet portion 31 as long as the positions are positions that can suppress the elongation of the adhesive material 33 due to thermal expansion of the first sheet portion 31.

[0085] As described above, the support member 41 may be fixed to the upper surface 311 of the first sheet portion 31. Also, the support member 41 may be fixed to both the upper surface 311 and the lower surface 312 of the first sheet portion 31. In this case, the support member 41 fixed to the upper surface 311 of the first sheet portion 31 and the support member 41 fixed to the lower surface 312 may or may not overlap in a plan view.

[0086] In the above-described manufacturing method of the CNT composite material 1, 1a, the step of removing the support member 41 (step S15) may be performed after the step of fixing the second sheet portion 32 to the first sheet portion 31 (step S16), or in parallel with step S16. Furthermore, in this manufacturing method, step S15 is not necessarily required, and the CNT composite material 1 in a state in which the support member 41 is fixed to the first sheet portion 31 may be used as a product. For example, the support member 41 may be provided over substantially the entire surface of the lower surface 312 of the first sheet portion 31, and used as the above-described heat dissipation portion.

[0087] In the above-mentioned method for producing the CNT composite member 1a, deformation such as bending of the first sheet portion 31 and the second sheet portion 32 is reduced in step S24, but this is not necessarily limited to this. For example, in step S24, it is also possible to intentionally deform the CNT composite member 1a by fitting the first sheet portion 31 and the second sheet portion 32 to a jig of a predetermined shape. Also, in step S24, only a portion of the adhesive material 34 facing the connecting sheet portion 21 may be heated via the second sheet portion 32 or the first sheet portion 31. In this case, for example, light is irradiated to only a portion of the adhesive material 34 facing the connecting sheet portion 21, or heated air or the like is applied thereto.

[0088] In the CNT device 2, for example, a large number of carbon nanotubes constituting the connection sheet portion 21 may be bonded to each other by an adhesive mainly composed of a polyvinyl alcohol (PVA) aqueous solution or the like. The connection sheet portion 21 may also be bonded to the first sheet portion 31 by the adhesive. The adhesive may be an epoxy-based, acrylic-based, or silicone rubber-based adhesive. The adhesive may contain a conductive additive. The conductive additive is, for example, metal fine particles such as silver (Ag), graphene (specifically, powder obtained by pulverizing sheet-like graphene), milled fiber, or powder of carbon nanotubes. The diameter of the conductive additive is preferably 10 μm or less, and more preferably less than 1 μm. The adhesive may not contain a conductive additive.

[0089] The CNT composite members 1 and 1a do not necessarily have to be CNT heaters, and the connecting sheet portion 21 does not necessarily have to be a heat generating portion. For example, the CNT composite members 1 and 1a may be a sensor such as a strain sensor, and the connecting sheet portion 21 may be a conductive portion of the sensor.

[0090] In the CNT composite members 1, 1a, it is not necessary to provide a sheet-shaped CNT body such as the connecting sheet portion 21; for example, a thread-shaped (i.e., twisted or untwisted thread-shaped) CNT body may be provided between a pair of electrodes 22.

[0091] The configurations in the above-described embodiment and each of the modified examples may be combined as appropriate as long as they are not mutually inconsistent. [Explanation of symbols]

[0092] 1,1a CNT composite material 21 Connection sheet section 22 electrodes 31 First seat section 32 Second seat section 33 Adhesive material 41 Support member 311 (First sheet part) upper surface 312 (First sheet part) underside 313 (First seat part) peripheral area S11~S16 steps

Claims

1. A method for producing a carbon nanotube composite member, comprising the steps of: a) attaching an adhesive material having a smaller thermal expansion coefficient than that of the first sheet portion to at least a peripheral region of one main surface of the first sheet portion; b) arranging a pair of electrodes and a carbon nanotube molding connecting the pair of electrodes on the one main surface of the first sheet portion; c) fixing a support member having a thermal expansion coefficient smaller than that of the first sheet portion to the first sheet portion; d) a step of heating the carbon nanotube molded body after the steps a) to c) to vaporize and remove the solvent impregnated in the carbon nanotube molded body; e) after the step d), stacking the first sheet portion and the second sheet portion with the carbon nanotube molding and the adhesive material sandwiched therebetween, and fixing the second sheet portion to the first sheet portion with the adhesive material to seal the carbon nanotube molding; A method for producing a carbon nanotube composite member, comprising:

2. A method for producing a carbon nanotube composite member according to claim 1, comprising the steps of: A method for producing a carbon nanotube composite member, further comprising the step of removing the support member from the first sheet portion after the step d).

3. 3. A method for producing a carbon nanotube composite member according to claim 1 or 2, comprising the steps of: The method for producing a carbon nanotube composite member, wherein in the step c), the support member is fixed onto the other main surface of the first sheet portion.

4. A method for producing a carbon nanotube composite member according to any one of claims 1 to 3, comprising the steps of: The method for producing a carbon nanotube composite member, wherein in the step c), the support member is fixed at a position on the peripheral region where the support member overlaps with the adhesive material.

5. A method for producing a carbon nanotube composite member according to claim 4, comprising the steps of: A method for producing a carbon nanotube composite member, wherein in the step c), the support member is fixed to the peripheral region along a direction from one of the pair of electrodes to the other.

6. A method for producing a carbon nanotube composite member according to any one of claims 1 to 5, comprising the steps of: The method for producing a carbon nanotube composite member, wherein in the step a), the adhesive material is applied over the entire surface of the one main surface of the first sheet portion.

7. A method for producing a carbon nanotube composite member according to any one of claims 1 to 6, comprising the steps of: The carbon nanotube molding is an electric heating part that generates heat by electric power supplied between the pair of electrodes to heat an object, according to the method for producing a carbon nanotube composite member.

8. A method for producing a carbon nanotube composite member according to any one of claims 1 to 7, comprising the steps of: The method for producing a carbon nanotube composite member device is characterized in that the adhesive material is a double-sided adhesive tape having adhesive layers provided on both sides of a sheet-like substrate.

9. A method for producing a carbon nanotube composite member according to any one of claims 1 to 8, comprising the steps of: f) before the e) step, a step of attaching another adhesive material to a main surface of the second sheet portion, The step e) comprises: g) laminating the second sheet portion on the first sheet portion, the adhesive material, and the carbon nanotube molded body while the carbon nanotube molded body and the other adhesive material face each other; h) pressing the first sheet portion and the second sheet portion laminated in the g) step against each other to fix them; i) a step of heating the other adhesive material to a predetermined post-treatment temperature after the step h); A method for producing a carbon nanotube composite member, comprising:

10. A method for producing a carbon nanotube composite member according to claim 9, comprising the steps of: A method for producing a carbon nanotube composite member, wherein the Arrhenius parameter during heating in the step i) is 1.05 or more.

Citation Information

Patent Citations

  • High-efficiency aerating method

    JP1982021995A

  • Manufacturing method of surface heating body

    JP2001357966A

  • Planar heat source

    JP2010034056A

  • Heater and method of manufacturing the same

    JP2011103293A

  • Carbon nanotube device manufacturing method, carbon nanotube device, and carbon nanotube heater