Gallium-containing silver powder, method for producing the same, and conductive paste
The gallium-containing silver powder addresses resistance issues in solar cell electrodes by utilizing controlled gallium attachment on silver particles, achieving lower resistance through optimized production methods and interface doping.
Patent Information
- Application Number
- JP2023033204
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-03
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2043-03-03
AI Technical Summary
Conductive pastes containing aluminum or indium-coated silver powders for solar cells face issues with increased resistance and contamination risks, as aluminum can form oxides and indium's atomic radius is too large for effective doping, leading to inefficiencies in resistance reduction.
Development of gallium-containing silver powder with controlled particle size and surface attachment of gallium, produced through a method involving dispersion and adhesion of metallic gallium droplets onto silver powder, using specific surfactants to enhance dispersion and reduce resistance.
The gallium-containing silver powder effectively lowers electrical resistance during both low-temperature and high-temperature firing by ensuring gallium reaches the semiconductor interface, outperforming traditional methods in reducing electrode resistance.
Smart Images

Figure 0007578739000007 
Figure 0007578739000008 
Figure 0007578739000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a gallium-containing silver powder, a method for producing the gallium-containing silver powder, and a conductive paste. [Background technology]
[0002] Silver powder is used as a bonding material for various electrodes. For example, there are solar cells that have a p-type emitter layer formed by adding a p-type dopant to the surface of an n-type silicon substrate (n-type solar cells), and solar cells that have an n-type emitter layer formed by adding an n-type dopant to the surface of a p-type silicon substrate (p-type solar cells). In recent years, due to rising energy demand, there has been an increasing demand for solar cells with high power generation efficiency, and electrode materials have attracted attention.
[0003] Conventionally, when forming an electrode by applying a conductive paste to a semiconductor layer that has been made p-type by a p-type dopant (the above-mentioned p-type emitter layer or p-type substrate), attempts have been made to include in the conductive paste an element that acts as a p-type impurity for the Si substrate.
[0004] For example, Patent Document 1 discloses the use of a silver-aluminum paste containing a combination of Ag (silver) and Al (aluminum) as a conductive filler in the formation of an electrode on the light-receiving surface of an n-type solar cell. In Patent Document 1, the conductive paste contains Al, which additionally dopes the semiconductor layer with a p-type dopant, thereby reducing the resistance at the interface between the p-type semiconductor layer and the electrode.
[0005] Furthermore, Patent Document 2 discloses silver powder coated with In (indium), which is an element of the same group as Al, a method for producing the same, and a conductive paste containing the silver powder. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2016-519839 [Patent Document 2] JP 2015-132002 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, it was found that when Al is contained in the conductive paste as in Patent Document 1, even if the element that becomes a p-type impurity for silicon (Si) can be contained and the element can be supplied to the interface with the p-type semiconductor layer, the resistance value of the formed electrode may increase. In addition, the indium-coated silver powder disclosed in Patent Document 2 is not generally used as a coating material for silver powder because the atomic radius of indium is too large to be used as a dopant for silicon. Therefore, it is desired to develop a powder that can contribute to lowering the resistance more than aluminum. In addition, the method of adding a reducing agent to a slurry containing silver powder and metal ions disclosed in Patent Document 2 is likely to produce gallium oxide because the redox potential of gallium is lower than the redox potential of hydrogen, and when trying to obtain gallium-coated silver powder using this method, gallium must be reduced using a very strong reducing agent such as metallic aluminum, and the oxidized aluminum may remain in the form of oxide or hydroxide and become a contamination.
[0008] The present inventors came up with the idea of incorporating gallium into silver powder instead of aluminum, and attempted to realize this idea. Therefore, the present invention aims to provide a gallium-containing silver powder and a manufacturing method thereof, which can supply gallium, which is a p-type impurity, in an appropriate form so as to reach the interface with the p-type semiconductor layer of a solar cell, and can reduce the resistance during low-temperature firing and can reduce the electrical resistance during high-temperature firing compared to the case where aluminum is added, as well as a conductive paste using the same. [Means for solving the problem]
[0009] As a result of extensive research by the present inventors to achieve the above-mentioned object, the present inventors have completed the present invention described below.
[0010] That is, the gist of the present invention for achieving the above-mentioned object is as follows.
[0011] (1) A gallium-containing silver powder containing gallium, The gallium-containing silver powder is characterized in that the volume-based median diameter D50 of the gallium-containing silver powder measured by a laser diffraction method is 0.2 μm or more and 5.0 μm or less.
[0012] (2) The gallium-containing silver powder according to (1), in which gallium is attached to the surface of the silver particles constituting the gallium-containing silver powder.
[0013] (3) A gallium-containing silver powder according to (1) or (2), wherein the gallium is metallic gallium.
[0014] (4) A gallium-containing silver powder according to any one of (1) to (3), in which the gallium is contained in an amount of 0.01 wt% or more and 10 wt% or less relative to the silver.
[0015] (5) A gallium-containing silver powder according to any one of (1) to (4), in which a surfactant is attached to the surface of the gallium-containing silver powder, and the amount of organic matter contained in the gallium-containing silver powder is 0.01 wt% or more and 4 wt% or less.
[0016] (6) a dispersing step of forming an emulsion liquid having metallic gallium droplets dispersed therein; In a liquid containing silver powder, (a) the emulsion liquid, or (b) A gallium powder dispersion obtained by cooling the emulsion. A method for producing gallium-containing silver powder, comprising the step of adhering gallium to the silver powder by adding
[0017] (7) A method for producing gallium-containing silver powder according to (6), wherein in the dispersion step, a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt or anhydride thereof is used.
[0018] (8) A method for producing gallium-containing silver powder according to (6) or (7), in which the liquid temperature in the adhesion step is 70°C or lower.
[0019] (9) A conductive paste including a filler, a solvent, and a glass frit, A conductive paste, characterized in that the filler contains the gallium-containing silver powder according to any one of (1) to (5).
[0020] (10) The conductive paste according to (9), wherein the filler further contains silver powder.
[0021] (11) The conductive paste according to (9) or (10), wherein the conductive paste contains 0.01 to 4 wt % of the gallium relative to the silver. Effect of the Invention
[0022] According to the present invention, it is possible to provide a gallium-containing silver powder and a method for producing the same, which can supply gallium as a p-type impurity in an appropriate form, particularly so that it reaches the interface with the p-type semiconductor layer of a solar cell, and can reduce the resistance during low-temperature firing and can reduce the electrical resistance more than when aluminum is added during high-temperature firing. It is also possible to provide a conductive paste using the same. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is an SEM image of the gallium powder in Example 1 of the present invention. [Diagram 2] FIG. 2 is an SEM image of the gallium-containing silver powder in Example 1 of the present invention. [Diagram 3] FIG. 3 is a diagram showing element mapping by SEM-EDS of the gallium-containing silver powder in Example 1 of the present invention. [Figure 4] FIG. 4 is a diagram showing an SEM image of the gallium-containing silver powder in Example 1 of the present invention by SEM-EDS and element mapping of each element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] The silver powder of the present invention is a gallium-containing silver powder containing gallium. In this specification, the term "gallium" refers not only to the gallium element alone, but also to a form in which a part of the surface of metal gallium is oxidized. First, prior to the description of the embodiment, the gallium of the present specification will be described.
[0025] -Metal gallium (Ga)- First, the electrical resistivities of simple substances such as gallium (Ga) and the related Group III metal elements are as shown in Table 1 below.
[0026] [Table 1]
[0027] Ga is a group III element like B, Al, and In, but the electrical resistivity of Ga is larger than that of Al and In. Therefore, it has been thought that Ga does not contribute to lowering the resistance of electrodes made of Ag. However, the present inventors have found that silver powder containing gallium has the effect of lowering the electrical resistance, especially when used to form an FF50 type electrode for a solar cell.
[0028] Furthermore, while metallic gallium has a high resistivity, it also has an extremely low melting point.
[0029] [Table 2]
[0030] It is believed that Ga, which has a low melting point, melts at the start of initial sintering or below the glass softening temperature, and moves to the substrate first. When firing a conductive paste containing silver powder, if the silver powder contains Al at the temperature at which the Ag particles start to neck together, Al may remain between the Ag particles. On the other hand, if the silver powder contains Ga, gallium is no longer present between the Ag particles at that temperature, and it is expected that gallium has already moved to the vicinity of the interface with the semiconductor layer. This contributes to lowering the resistance of the silver powder compared to when Al is used, and is particularly likely to contribute to lowering the resistance during low-temperature firing at peak temperatures below 500°C (e.g., 400°C).
[0031] -Gallium included- Here, the fact that the gallium-containing silver powder "contains gallium" can be confirmed when gallium is detected by ICP analysis using a sample solution in which the gallium-containing silver powder is completely dissolved using nitric acid and hydrochloric acid. When the silver powder is subjected to ICP analysis, the element detected other than silver is mainly gallium, which is the gallium-containing silver powder, and the gallium-containing silver powder includes a form in which silver and gallium are alloyed in part of the silver powder.
[0032] -Gallium adhesion- A state in which gallium is attached to the surface of silver powder is also one aspect of gallium-containing silver powder. The fact that gallium is attached to the surface of silver powder can be confirmed by gallium mapping, which is performed by observing the surface of silver particles using SEM-EDS and performing elemental mapping. If gallium is attached to even a part of the surface of the silver particles, gallium can be detected. When the particle size of the gallium-containing silver powder is small, elemental analysis of the surface may be performed using a measurement method with a small detection depth, such as Auger electron spectroscopy (AES) or X-ray photoelectron spectroscopy (XPS).
[0033] -Volumetric median diameter- The median diameter of the gallium-containing silver powder is the cumulative 50% diameter (D50) based on the volume by the laser diffraction method. The measurement by the laser diffraction method can be performed using a Microtrack particle size distribution measuring device (manufactured by Microtrack Bell Co., Ltd., device name: MT-3300EXII), and this device was used in this specification.
[0034] The gallium-containing silver powder according to the present invention will be described in detail below.
[0035] (Gallium-containing silver powder) The gallium-containing silver powder according to the present invention contains gallium, and the volume-based median diameter D50 of the gallium-containing silver powder measured by a laser diffraction method is 0.2 μm or more and 5.0 μm or less. The median diameter D50 is preferably 1 μm or more and 3 μm or less. The BET specific surface area of the gallium-containing silver powder is 0.15 m2 or less as measured by a BET single point method. 2 / g or more 4m 2 / g or less, and 0.25m 2 / g or more 1m 2 It is more preferable that the molecular weight is not more than 1 / g.
[0036] As elements other than silver and gallium in the gallium-containing silver powder, in addition to unavoidable impurities, elements that can be p-type impurities (e.g., B, Al, In, Zn, etc.) and elements for fire-through (e.g., Te) may be included, and alloys of gallium and these elements may be included, within the scope of obtaining the effects of the present invention. Also, alloys of silver and gallium may be included. Here, the gallium contained in the gallium-containing silver powder can be 50% or more, preferably 80% or more, in terms of element concentration ratio, of all elements other than silver.
[0037] In the silver particles constituting the gallium-containing silver powder, it is preferable that gallium is attached to the surface of at least a part of the silver particles. Also, it is more preferable that the gallium-containing silver powder is one in which metallic gallium is attached to the surface of at least a part of the silver particles. In the gallium-containing silver powder, the ratio of the number of silver particles in which gallium is observed at least in part in the mapping of SEM-EDS is preferably 5% or more, more preferably 10% or more, relative to the number of all particles. Gallium or metallic gallium may be attached to the entire surface of the silver particles, or may be attached to a part of the silver particles. Note that metallic gallium particles used in the manufacturing process of the gallium-containing silver powder of the present invention may be partially mixed. When gallium is attached to the surface of the silver particles, it is considered that the movement of gallium is easy when a conductive paste containing gallium-containing silver powder is applied to a semiconductor layer and then heated. In addition, it is considered that gallium has a low melting point, and in order to function as a dopant, particularly for the semiconductor layer of a solar cell, it is preferable that gallium exists in the state of metallic gallium rather than in the state of an oxide.
[0038] In the gallium-containing silver powder according to the present invention, it is preferable that the gallium content is 0.01 wt% or more and 10 wt% or less relative to the silver, and it is more preferable that the gallium content is 2 wt% or less relative to the silver. If the gallium content in the paste is too high, it is disadvantageous because the electrical resistance value increases, but it is also possible to adjust the amount of gallium relative to the silver in the paste to an appropriate range by mixing a gallium-containing silver powder with a high gallium content with a silver powder that does not contain gallium. If we must say, since the particle ratio of gallium-containing particles that serve as a gallium source decreases in a gallium-containing silver powder with a high gallium content, in order to improve the uniformity of the electrode fired film, it is preferable that the gallium content is not extremely high. The gallium content can be determined by quantitatively determining the amount of gallium by ICP analysis using a sample solution in which the gallium-containing silver powder is completely dissolved using nitric acid and hydrochloric acid.
[0039] It is preferable that the surfactant is attached to the surface of the gallium-containing silver powder, and the amount of organic matter contained in the gallium-containing silver powder is 0.01 to 4 wt%. The amount of organic matter can be measured by dissolving the gallium-containing silver powder in an acid, extracting it with an organic solvent such as hexane, and performing GC / MS or carbon analysis on the extraction solvent layer. In addition, since highly polar organic matter such as having a hydroxyl group may have a low extractability (distribution coefficient) into an organic solvent, for example, a quantitative analysis may be performed after mixing an acid and an alcohol as a pretreatment and heating the mixture to esterify the carboxyl group to increase the solvent extractability. The type of organic matter attached to the surface is preferably a surfactant that does not contain sulfur or phosphorus and has a molecular weight of 100 to 1000, and is also preferably a fatty acid or aliphatic amine with a carbon chain length of 10 or more. The type of organic matter attached to the surface can be identified by heating it in a pyrolyzer in a He gas flow to thermally desorb it, and performing a qualitative analysis with GC / MS. The ignition weight change of the gallium-containing silver powder is preferably 0.6 wt% or less. The ignition weight change is the total amount of impurities such as moisture and organic matter contained in the gallium-containing silver powder, and is the value obtained by dividing the difference between the initial mass and the mass after heating (e.g., 800°C for 30 minutes) sufficient to eliminate the weight change and reach a constant mass, by the initial mass.
[0040] Next, the manufacturing method for obtaining the above-mentioned gallium-containing silver powder according to the present invention will be described in detail.
[0041] (Method of manufacturing gallium-containing silver powder) The method for producing gallium-containing silver powder according to the present invention includes at least a dispersion step of forming an emulsion liquid in which metallic gallium droplets are dispersed, and an attachment step of adding (a) the emulsion liquid or (b) a gallium powder dispersion liquid obtained by cooling the emulsion liquid to a liquid containing silver powder and adhering gallium to the silver powder while mixing. Hereinafter, each step and optional step of the production method according to the present invention will be described in order.
[0042] <Dispersion process> In the dispersion process, an emulsion liquid in which metallic gallium droplets are dispersed is formed. The molten gallium liquid, which is obtained by heating high-purity gallium (4N or higher) to a temperature above its melting point, is placed in a solvent containing a surfactant (sometimes called a dispersant), and is stirred using an ultrasonic vibrator such as a homogenizer to turn the metallic gallium into droplets with small particle sizes, while the surfactant is attached to the surface of the gallium droplets to form an emulsion liquid (liquid-liquid dispersion state) in which the metallic gallium is dispersed in the liquid.
[0043] -Surfactants- Here, when the gallium-containing silver powder is used in the conductive paste, the surfactant that adheres to the surface of gallium is also included in the conductive paste. In consideration of this, it is preferable that the surfactant is one that is unlikely to remain as an impurity in the conductive film after the conductive paste is applied and fired, and is preferably a surfactant selected from, for example, fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts or anhydrides thereof. A plurality of surfactants may be used. A reagent containing a selected component as the main component can be used as the surfactant, and the reagent may contain other components. It is more preferable that the surfactant is a fatty acid or an aliphatic amine. It is more preferable that the surfactant has a carbon chain length of 10 or more. It is preferable that the surfactant contains little or no phosphorus and sulfur components. Phosphate-based, sulfonic acid-based, and thiol-based surfactants are very effective in dispersing gallium, but there is a risk that they will remain in the conductive film in the form of phosphates or sulfates after firing, which may not only reduce the characteristics but also deteriorate the reliability. In particular, it is preferable to use a surfactant that does not contain sulfur or phosphorus and has a molecular weight of 100 to 1000, and it is preferable to use a fatty acid or aliphatic amine with a carbon chain length of 10 or more. In the firing of conductive films in solar cells and the like, the firing time is very short, on the order of several tens of seconds, and therefore, depending on the type of surfactant, in the case of polymers with a molecular weight exceeding 1000, it is considered that debinding may not be completed completely.
[0044] When considering using the gallium-containing silver powder obtained by this manufacturing method in a conductive paste, it is also preferable to use a known surface treatment agent used for silver powder as a surfactant that is unlikely to remain after firing the conductive paste, such as stearic acid, palmitic acid, oleic acid, hydroxystearic acid, ricinoleic acid, benzotriazole, dodecenylsuccinic anhydride, pentadecenylsuccinic anhydride, stearylamine, etc. In addition, it is also preferable that the surfactant has the same components as the surface treatment agent attached to the surface of the silver powder used in the adhesion process described below, or that the entire surfactant has the same components as the surface treatment agent attached to the surface of the silver powder used in the adhesion process described below.
[0045] -solvent- The solvent to be used is not particularly limited, and is preferably a solvent capable of dissolving the above-mentioned surfactant, for example, alcohol such as ethanol or isopropyl alcohol, or water.
[0046] <Attachment process> In the adhesion step performed after the dispersion step, gallium is adhered to the silver powder by adding (a) an emulsion liquid or (b) a gallium powder dispersion liquid obtained by cooling the emulsion liquid to a liquid containing silver powder. Here, since the melting point of metallic gallium is about 30°C as described above, the gallium in the emulsion liquid is solidified by simply cooling the emulsion liquid to room temperature, for example, and a gallium powder dispersion liquid in which solid gallium powder is dispersed is obtained. In this step, the emulsion liquid obtained in the previous step may be added in the emulsion state, or the gallium powder dispersion liquid obtained by cooling the emulsion liquid may be added. It is preferable that the liquid containing silver powder is stirred before addition.
[0047] In the adhesion step, silver powder is dispersed in a solvent, and the emulsion liquid or gallium powder dispersion liquid in which the metallic gallium droplets obtained in the previous step are dispersed is dropped into the solvent. Gallium is adhered to the silver powder surface while mixing these, thereby obtaining a dispersion liquid of gallium-containing silver powder. In this step, the method of adhering metallic gallium to the silver powder while mixing the liquid containing silver powder with the emulsion liquid or the gallium powder dispersion liquid obtained by cooling it is arbitrary, but it is preferable to use ultrasonic vibration.
[0048] <<Liquid temperature>> In addition, the liquid temperature in the adhesion step is preferably 70°C or less, the liquid temperature is preferably equal to or higher than the melting point of the solvent, and the liquid temperature is more preferably 20°C or more and 60°C or less, and it is preferable that the liquid temperature is within a range not exceeding 70°C during stirring. If the liquid temperature becomes too high, the dispersed metallic gallium droplets may gather. Although it is not possible to measure the actual local temperature, it is considered ideal that only the local parts where the gallium droplets or the gallium particles and the silver particles collide after the mixing process have a temperature above the melting point of gallium (30°C or more). Although it depends on the amount of kinetic energy such as ultrasonic vibration added in the mixing process, if the liquid temperature is less than 20°C, it is difficult to raise the local temperature to 30°C or more even if kinetic energy such as ultrasonic vibration is added, while on the other hand, if it exceeds 70°C, gallium alone is likely to aggregate. In addition, after the adhesion step, it is preferable to cool it to room temperature or use a refrigerator to solidify the droplets and store it as a gallium powder dispersion liquid.
[0049] <<Gallium powder dispersion liquid obtained by cooling the emulsion liquid>> -SEM average diameter- The SEM average diameter of the metallic gallium particles obtained by cooling and drying the emulsion liquid and the SEM average diameter of the metallic gallium particles obtained by drying the gallium dispersion liquid are preferably 0.01 to 10 μm, more preferably 0.2 to 2 μm. The method for measuring the SEM average diameter is to measure the Heywood diameter of 100 or more particles whose outer shape can be clearly recognized in a 5,000x SEM image using image processing software Mac-View Ver.4 manufactured by MOUNTECH, and calculate the average value.
[0050] <Optional process> The resulting dispersion of gallium-containing silver powder is filtered and dried to obtain gallium-containing silver powder, which may be further subjected to a crushing step and a classification step.
[0051] The above-mentioned manufacturing method of gallium-containing silver powder is an example, and a method of directly stirring and mixing the emulsion liquid or gallium powder dispersion liquid in which the above-mentioned metallic gallium droplets are dispersed with the dried silver powder while heating is also considered. Also, during the wet manufacturing process of silver powder (from the time of adding the reducing agent to the silver complex solution until filtration), the emulsion liquid or gallium powder dispersion liquid in which the above-mentioned metallic gallium droplets are dispersed may be mixed and stirred.
[0052] (Conductive paste) Next, a conductive paste using the gallium-containing silver powder according to the present invention will be described. The conductive paste according to the present invention contains at least a filler, a solvent, and a glass frit. The filler contains the above-mentioned gallium-containing silver powder according to the present invention. This conductive paste is suitable for use as a conductive paste for forming a p-type electrode of a solar cell. In the conductive paste, gallium is preferably contained in an amount of 0.01 wt% to 4 wt% relative to silver, and more preferably in an amount of 0.2 wt% to 2 wt% relative to silver. A method for confirming that the conductive paste "contains gallium" can be performed by ICP analysis. However, since the conductive paste also contains organic solvents and resins, it is preferable to perform a pretreatment to remove these before performing ICP analysis. For example, the conductive paste is dispersed and dissolved in a large amount of organic solvent such as acetone, and the solid content collected by filtering and washing is dissolved in nitric acid and hydrochloric acid, whereby ICP analysis can be performed. Silver and gallium components are not dissolved in organic solvents, so that the amount of gallium and the amount of silver can be quantitatively analyzed by ICP analysis of the solution of the collected solid content, and the amount of gallium relative to silver can be measured.
[0053] <Filler> The filler may further contain silver powder (silver powder not containing gallium) in addition to the gallium-containing silver powder. It may further contain metal powder such as aluminum powder. The content of the filler in the conductive paste is preferably 65 wt% or more and 95 wt% or less.
[0054] <Solvent> The solvent is not particularly limited, and examples thereof include terpineol, butyl carbitol, butyl carbitol acetate, and texanol. Two or more kinds of solvents may be used at the same time. The content of the solvent in the conductive paste is preferably 1 wt% or more and 40 wt% or less.
[0055] <Glass frit> The glass frit is not particularly limited, and preferably has a softening point of 550° C. or less. The shape of the glass frit is not particularly limited, and may be spherical or irregularly spherical. The content of the glass frit in the conductive paste is preferably 0.1 wt % or more and 10 wt % or less.
[0056] <Optional inclusions> The conductive paste may further contain a resin, a dispersant, a surfactant, and a viscosity modifier.
[0057] The conductive paste described above can be manufactured by a general method, except that the gallium-containing silver powder according to the present invention is used as a filler. For example, a paste composition containing at least a filler, a solvent, and a glass frit is appropriately adjusted. Then, the paste composition is mixed, pre-mixed with a stirrer, and then kneaded with a three-roll mill or the like to obtain a conductive paste. When performing dispersion and kneading, ultrasonic dispersion, a disperser, a three-roll mill, a ball mill, a bead mill, a two-axis kneader, a self-revolving stirrer, or the like may be used. If the obtained conductive paste is printed on a substrate by, for example, screen printing, offset printing, photolithography, inkjet printing, or the like, a conductive film of a desired shape can be formed. EXAMPLES
[0058] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. Not limited to this.
[0059] Example 1 First, solid-state metallic gallium (manufactured by DOWA Electronics) with a purity of 99.99% was liquefied by heating it in a hot bath at 60 ° C. In addition, 20 g (room temperature) of an isopropyl alcohol (manufactured by FUJIFILM; Wako Grade 1) solution in which stearic acid (used as a surfactant, manufactured by FUJIFILM; special grade reagent) was dissolved at 1 wt% was prepared. 1 g of liquefied gallium was added to this isopropyl alcohol solution to obtain a gallium-containing liquid. This gallium-containing liquid was subjected to ultrasonic dispersion treatment using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho, model number: US-600AT). At that time, the gallium-containing liquid was cooled in a water bath and intermittently subjected to ultrasonic dispersion treatment for a total of 5 minutes while taking cooling time in between so that the temperature of the gallium-containing liquid would not exceed 70 ° C. due to heat generation caused by ultrasonic irradiation, and an emulsion liquid in which metallic gallium droplets were dispersed was obtained. The liquid temperature was about 40°C, and ultrasonic dispersion was performed using an ultrasonic homogenizer until gallium was no longer accumulated at the bottom of the beaker. After that, the dispersion process was stopped and the mixture was left to stand at room temperature, so that the gallium droplets were solidified while still dispersed, and a gallium powder dispersion was obtained. Note that the output of the device during ultrasonic dispersion was not constant because it was affected by the dispersion state and the liquid temperature, and varied between 150W and 250W.
[0060] In order to evaluate the obtained gallium powder dispersion, the emulsion liquid in which metal gallium droplets were dispersed was separated, cooled in a refrigerator, and the obtained gallium powder dispersion was dried with cold air to obtain gallium powder. Figure 1 shows an SEM photograph of the gallium powder observed at a magnification of 5000 times using an SEM. In addition, the Heywood diameter of 100 or more particles with clear particle contours was measured using image processing software (Mac-View Ver.4 manufactured by MOUNTECH Co., Ltd.) for the obtained SEM observation image, and the average value was taken as the SEM average diameter. The SEM average diameter of the gallium powder was 0.9 μm.
[0061] Next, 100 g of spherical silver powder (DOWA Electronics; AG4-8FD, SEM average diameter 1.3 μm) was added to 20 g of isopropyl alcohol (FUJIFILM; Wako First Grade), and ultrasonic dispersion treatment was performed for 5 minutes at an output of 100 W using an ultrasonic homogenizer (Nippon Seiki Seisakusho, device name: US-600AT). The main component of the surface treatment agent for the spherical silver powder used is stearic acid.
[0062] After the above-mentioned 5-minute dispersion treatment of the spherical silver powder, the ultrasonic dispersion treatment was continued, and the previously prepared gallium powder dispersion liquid (total amount of 21 g) was dropped with a dropper over 1 minute, and ultrasonic dispersion treatment was performed for another 5 minutes to prepare a dispersion liquid containing gallium-containing silver powder. During the dispersion treatment, the liquid temperature rose to 60°C. After the dispersion treatment was stopped, it was cooled to room temperature.
[0063] The dispersion liquid containing this gallium-containing silver powder was then pressure filtered through a membrane filter with an opening of 0.2 μm, and the resulting cake was dried at room temperature in the air for 12 hours to obtain the gallium-containing silver powder according to Example 1. A photograph of the obtained gallium-containing silver powder observed at 5000 times by SEM is shown in FIG.
[0064] (SEM-EDS measurement) The obtained gallium-containing silver powder was observed at 10,000 times by SEM-EDS, and the images of element mapping by qualitative analysis are shown in Figures 3 and 4. Figure 3 shows the overlapping of C (carbon)-KO (oxygen)-K, Ga (gallium)-L, and Ag (silver)-L mappings (K means K line, L means L line), and Figure 4 shows the SEM image and mapping of each element. IMG1 (1st) in Figure 4 is a secondary electron image before EDS measurement, and IMG1 is a secondary electron image after EDS measurement. As can be seen from Figures 3 and 4, silver particles with gallium attached to part of the silver surface (dark gray area in Ag (silver)-L in Figure 4 and dark gray area in Ga (gallium)-L) were observed, and it was confirmed that gallium particles not attached to silver particles (black area in Ag (silver)-L in Figure 4 and gray area in Ga (gallium)-L) were mixed. Considering the manufacturing method of the present invention, it is not easy for Ga to be mixed into the inside of silver particles, so it can be assumed that Ga is present on the surface of the silver particles. It is considered that the amount of gallium particles remaining without adhering to the silver particles can be reduced by adjusting the manufacturing conditions, and the entire amount can be made to be in an attached state.
[0065] (Particle size distribution measurement) In addition, the particle size distribution of the obtained gallium-containing silver powder was measured by laser diffraction wet sample measurement using a Microtrack particle size distribution measuring device (Microtrack Bell Co., Ltd., device name: MT-3300EXII). The measurement sample was prepared by adding 0.1 g of gallium-containing silver powder to 40 mL of isopropyl alcohol (IPA) and dispersing it. The dispersion was performed using an ultrasonic homogenizer (Nihon Seiki Seisakusho, device name: US-150T) with a tip diameter of 18 mm at a frequency of 19.5 kHz, and the dispersion time was set to 2 minutes. The dispersed sample was subjected to the above-mentioned device, and the particle size distribution was measured using the attached analysis software. The measurement results obtained are shown in Table 3. As can be seen from the results in Table 3, there was almost no difference in the particle size distribution before and after the attachment of gallium, compared to the particle size distribution of the silver powder (DOWA Electronics; AG4-8FD) before the addition of gallium.
[0066] [Table 3]
[0067] (BET specific surface area measurement) The BET specific surface area of the gallium-containing silver powder was determined using a fully automatic specific surface area measuring device (Mountec Co., Ltd., device name: Macsorb HM-model 1210). Specifically, the gallium-containing silver powder was placed in the device, degassed by flowing a He-N2 mixed gas (30% nitrogen) at 60°C for 10 minutes, and then measured by the BET single-point method, and the specific surface area was found to be 0.49 m. 2 The specific surface area of the base powder used, spherical silver powder AG4-8FD manufactured by DOWA Electronics, was confirmed to be 0.43 m 2 / g, it was confirmed that the BET specific surface area of the gallium-coated silver powder to which gallium was attached was slightly higher.
[0068] (Gallium content measurement) The amount of gallium in the gallium-containing silver powder was quantified, and it was confirmed that the gallium content in the gallium-containing silver powder was 0.95 wt%, and that the gallium content in the silver was 0.96 wt%. The theoretical value in manufacturing is 1 wt% gallium relative to the silver powder, so almost all of the added gallium was attached to the silver. The gallium content was quantified using the following analytical method. 1) 1 g of sample was precisely weighed, 15 mL of pure water and 10 mL of nitric acid (for precision analysis) were added, and the sample was heated at 200°C for 30 minutes. 2) 15 mL of pure water and 10 mL of hydrochloric acid (for precision analysis) were added and heated at 150°C for 30 minutes. 3) After heating, the sample was adjusted to a volume of 100 mL, and 5 mL was then taken and adjusted to a volume of 100 mL again to prepare a sample for ICP analysis. 4) ICP quantification was performed using an Aglent 5800 ICP-OES from Agilent Technologies.
[0069] (Organic substance analysis) 0.5g of gallium-containing silver powder was dissolved in nitric acid, then extracted with hexane. The extraction solvent layer was qualitatively analyzed with GC / MS (7890A / 5975C, Agilent Technologies), and it was confirmed that the organic matter contained in the gallium-containing silver powder was stearic acid. After evaporating the hexane extraction solvent, the carbon content of the residue was measured using a carbon-sulfur analyzer (EMIA-810W, Horiba, Ltd.). The organic matter contained in the gallium-containing silver powder was determined to be all stearic acid, and the stearic acid content was calculated from the carbon content to be 0.18wt%.
[0070] (Ignition weight change measurement) The ignition weight change was measured by weighing 3 g of gallium-containing silver powder and placing it in a magnetic crucible, gradually increasing the temperature from room temperature, and igniting the powder at 800°C for 30 minutes, sufficient heating to reach a constant weight, and then cooling and weighing the sample to determine the mass (w) after heating. The ignition weight change (wt%) was calculated using the following formula (1), and it was confirmed that the ignition weight change was 0.37 wt%. Ignition weight change (wt%) = (3-w) / 3 x 100 (1)
[0071] (Preparation of conductive paste) A conductive paste was prepared according to the paste composition shown in Table 4 below.
[0072] [Table 4]
[0073] These were mixed and pre-mixed under the condition of a rotary mixer (revolution 1000 rpm). After pre-mixing, it was mixed with a three-roll mill (manufactured by Exact) to obtain a conductive paste. The gallium content ratio to silver in the conductive paste was 0.96 wt%.
[0074] (Resistance measurement) The conductive paste was used to print a straight line shape by screen printing. The design line width of the straight line was 10, 12, 14, 16, 18, and 20 μm, respectively, and the length of the straight line was 150 mm. A Microtec printer was used for printing, and printing was performed at a squeegee speed of 350 mm / s. A silicon substrate with a thickness of about 170 μm (for solar cells, texture formation and SiNx film formation) was used for printing. After printing, the sample was dried for 5 minutes in a dryer set at a temperature of 200°C. A solar cell baking furnace (NGK) was used to bake the sample, and the furnace was set so that the peak temperature of the upper surface of the wafer was 400°C and 700°C, respectively. The resistance value of the printed electrode after baking was measured with a digital multimeter (ADC Corporation) by placing measuring terminals on both ends of the printed electrode.
[0075] Example 2 A gallium-containing silver powder was prepared in the same manner as in Example 1, except that the spherical silver powder was replaced with spherical silver powder (AG4-54F manufactured by DOWA Electronics) and the adhesion process was carried out. The main component of the surface treatment agent for the spherical silver powder was stearic acid.
[0076] The particle size distribution of the gallium-containing silver powder was measured by laser diffraction in the same manner as in Example 1. The measurement results are shown in Table 5. As can be seen from the results in Table 5, there was almost no difference in the particle size distribution before and after the attachment of gallium. The specific surface area was also measured in the same manner as in Example 1, and was found to be 0.43 m 2 It was confirmed that the specific surface area of the spherical silver powder (AG4-54F, manufactured by DOWA Electronics) used was 0.37 m 2 / g, it was confirmed that the BET specific surface area of the gallium-coated silver powder to which gallium was attached was slightly higher. When the amount of gallium in the gallium-containing silver powder was quantified, it was confirmed that the gallium-containing silver powder contained 0.75 wt% gallium, and 0.76 wt% gallium relative to silver. Since the theoretical value in the production is 1 wt% gallium relative to the silver powder, it is assumed that some loss occurred due to liquid splashing during ultrasonic dispersion processing in the process, adhesion to the container wall during mixing and addition, and handling. As a result of organic matter analysis performed in the same manner as in Example 1, the organic matter contained in the gallium-containing silver powder was stearic acid, and the amount of organic matter in the gallium-containing silver powder was 0.14 wt%. In the ignition weight change, the increase in the amount of gallium due to oxidation was greater than the amount of impurities such as moisture and organic matter contained in the silver powder, resulting in -0.12 wt%. In addition, a conductive paste was prepared using the gallium-containing silver powder of Example 2, printed, and the resistance value of the printed electrode after firing was measured in the same manner as in Example 1. The gallium content ratio to silver in the conductive paste was 0.76 wt%.
[0077] [Table 5]
[0078] (Reference example) The filler used in the conductive paste was a spherical silver powder AG4-8FD manufactured by DOWA Electronics that does not have gallium attached, and a gallium powder (SEM average diameter 0.9 μm) that was pressure filtered through a 0.2 μm membrane filter and vacuum dried at room temperature for 30 minutes in the above example. The proportion of gallium powder in the filler was 1 wt%, and the filler was mixed with 0.89 wt% Ga powder and 87.84 wt% silver powder. The conductive paste was prepared in the same manner as in Example 1, the conductive paste was printed, and the resistance value of the printed electrode after firing was measured. The gallium content ratio to silver in the conductive paste was 1.01 wt%.
[0079] (Comparative Example) Spherical silver powder AG4-8FD (manufactured by DOWA Electronics) without gallium attached and Al powder (average particle size 5 μm) were used as the filler for the conductive paste. The Al powder was mixed so that the ratio of the filler was 1 wt%. The other conditions were the same as in Example 1 to prepare a conductive paste, which was printed and fired, and the resistance value of the printed electrode was measured. The aluminum content ratio to silver in the conductive paste was 1.01 wt%.
[0080] The resistance values when the line width is 18 μm in the above-mentioned Examples, Reference Examples, Conventional Examples, and Comparative Examples are shown in Table 6 below.
[0081] [Table 6]
[0082] In the low-temperature firing at 400° C., the resistance was reduced in Examples 1 and 2 and the Reference Example, compared to the Comparative Example. In addition, it was found that the gallium-containing silver powder of the present invention has a superior effect of reducing resistance compared to the Reference Example.
[0083] The high-temperature firing at 700°C is a temperature at which Al can easily reach the interface with the p-type semiconductor layer of the solar cell because the melting point of Al is 660°C. It was found that when Al powder is mixed with silver powder as in the comparative example, the resistance value increases significantly. However, it was found that such a significant increase in resistance was not observed in Examples 1 and 2 and the reference example in which gallium was added. [Industrial Applicability]
[0084] According to the present invention, it is possible to provide a gallium-containing silver powder and a method for producing the same, which can supply gallium as a p-type impurity in an appropriate form, particularly so that it reaches the interface with the p-type semiconductor layer of a solar cell, and can reduce the resistance during low-temperature firing and can reduce the electrical resistance more than when aluminum is added during high-temperature firing. It is also possible to provide a conductive paste using the same.
Claims
1. A gallium-containing silver powder containing gallium, The volume-based median diameter D50 of the gallium-containing silver powder measured by a laser diffraction method is 0.2 μm or more and 5.0 μm or less; Gallium is attached to the surface of the silver particles constituting the gallium-containing silver powder, and A surfactant is attached to the surface of the gallium-containing silver powder, and the amount of organic matter contained in the gallium-containing silver powder is 0.01 wt % or more and 4 wt % or less. Gallium-containing silver powder characterized by:
2. The gallium-containing silver powder according to claim 1 , wherein said gallium is metallic gallium.
3. The gallium-containing silver powder according to claim 1, wherein the gallium is contained in an amount of 0.01 wt % or more and 10 wt % or less relative to the silver.
4. A dispersing step of forming an emulsion liquid in which metallic gallium droplets are dispersed; In a liquid containing silver powder, (a) the emulsion liquid, or (b) The emulsion is cooled to obtain a gallium powder dispersion. a step of adhering gallium to the silver powder by adding A step of obtaining gallium-containing silver powder by filtering and drying the obtained dispersion of gallium-containing silver powder; A method for producing gallium-containing silver powder, comprising the steps of:
5. The method for producing gallium-containing silver powder according to claim 4, wherein a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof is used in the dispersion step.
6. The method for producing gallium-containing silver powder according to claim 5, wherein the liquid temperature in the adhesion step is 70°C or lower.
7. A conductive paste including a filler, a solvent, and a glass frit, A conductive paste comprising the filler containing the gallium-containing silver powder according to claim 1.
8. The conductive paste of claim 7 , wherein the filler further comprises silver powder.
9. The conductive paste according to claim 7 or 8, wherein the conductive paste contains 0.01 to 4 wt % of gallium relative to silver.
Citation Information
Patent Citations
Electric conduction slurry and application of electric conduction slurry in N type silicon wafer solar cells
CN104795127A
Positive silver paste suitable for positive aluminum oxide-silicon nitride laminated passivation crystalline silicon solar cell and preparation method of positive silver paste
CN111128436A
N-type solar cell silver paste doped with organic gallium and preparation method thereof
CN112786232A
P-type emitter region ohmic contact silver electrode slurry
CN113096846A