Gallium powder, mixed powder, and method for producing gallium powder dispersion, method for producing gallium powder, gallium powder dispersion, and conductive paste

JP7578740B2Active Publication Date: 2024-11-06DOWA ELECTRONICS MATERIALS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023033206
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-03
Publication Date
2024-11-06
Estimated Expiration
2043-03-03

AI Technical Summary

Benefits of technology

【0021】 本発明によれば、小さい粒径のガリウム粉が得られると共に、低抵抗な電極が得られる導電性ペーストとすることが可能な当該ガリウム粉を含む混合粉を提供できる。また、製造が容易なガリウム粉分散液およびガリウム粉の製造方法を提供すると共に、ガリウム粉分散液、および低抵抗な電極が得られる導電性ペーストを提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578740000003
    Figure 0007578740000003
  • Figure 0007578740000001
    Figure 0007578740000001
  • Figure 0007578740000002
    Figure 0007578740000002
Patent Text Reader

Abstract

To provide gallium powder of a small particle size, and a mixed powder containing the gallium powder, enabling the production of a conductive paste that yields a low-resistance electrode.SOLUTION: Gallium powder according to the present invention has an SEM average diameter of 0.2 μm to 2 μm and includes a surfactant adhered to its surface, the surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, and salts thereof or anhydrides.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a gallium powder, a mixed powder, and a gallium powder dispersion, a method for producing a gallium powder, a gallium powder dispersion, and a conductive paste. [Background technology]

[0002] In recent years, gallium particles have been studied as a semiconductor material. For example, Patent Document 1 describes the production of fine particles of metal gallium or a gallium alloy by spraying molten metal from a nozzle. In addition, Patent Document 2 describes a method for producing fine particles of a gallium-indium alloy using polyvinylpyrrolidone, sodium alkylbenzenesulfonate, and alkylthiol as surfactants. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Special Publication No. 8-924 [Patent Document 2] China Patent Application Publication No. 110223798 Summary of the Invention [Problem to be solved by the invention]

[0004] Solar cells, which are an example of semiconductors, include a type in which a p-type emitter layer is formed by adding a p-type dopant to the surface of an n-type silicon substrate (n-type solar cells), and a type in which an n-type emitter layer is formed by adding an n-type dopant to the surface of a p-type silicon substrate (p-type solar cells). In recent years, due to the increase in energy demand, the demand for solar cells with high power generation efficiency has been increasing, and electrode materials have been attracting attention. In particular, there is a demand for low resistance electrodes for solar cells. When forming an electrode by applying a conductive paste to a p-type semiconductor layer (the above-mentioned p-type emitter layer or p-type substrate), attempts have been made to reduce the resistance by including Al powder, which is a p-type impurity, together with silver powder. Therefore, the present inventors tried a test of adding gallium powder to the conductive paste instead of adding Al powder to the conductive paste. However, the particle size of the conventionally known gallium powder is not easy to reduce by the method of the particle size of the silver powder used in the conductive paste, and the manufacturing cost was also high. In the method of Patent Document 2, there was a risk that sulfur and phosphorus contained in the surfactant would have an adverse effect on the conductive paste.

[0005] Therefore, the present invention provides a gallium powder having a small particle size, and a mixed powder containing the gallium powder capable of providing a conductive paste that can provide a low-resistance electrode. The present invention also aims to provide a gallium powder dispersion that is easy to manufacture, a method for manufacturing the gallium powder, and a conductive paste that can provide a gallium powder dispersion and a low-resistance electrode. [Means for solving the problem]

[0006] As a result of extensive research by the present inventors to achieve the above object, the present inventors have completed the present invention described below.

[0007] That is, the gist of the present invention for achieving the above-mentioned object is as follows.

[0008] (1) A gallium powder having an SEM average diameter of 0.2 μm or more and 2 μm or less, and having a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof attached to the surface.

[0009] (2) A gallium powder having an SEM average diameter of 0.2 μm or more and 2 μm or less, and having a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof attached to the surface; A mixed powder made by mixing silver powder with a SEM average diameter of 0.2 μm or more and 5 μm or less.

[0010] (3) The mixed powder described in (2), in which some or all of the components of the surface treatment agent adhering to the silver powder are the same as some or all of the components of the surfactant adhering to the gallium powder.

[0011] (4) The mixed powder according to (2) or (3), in which the gallium content is 0.01 wt% or more and 4 wt% or less relative to the silver.

[0012] (5) a first step of forming an emulsion by stirring a gallium melt, a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt or an anhydride thereof, and a solvent; A second step of cooling the emulsion; A method for producing a gallium powder dispersion liquid, comprising:

[0013] (6) The method for producing a gallium powder dispersion liquid according to (5), wherein in the first step, the stirring is performed by ultrasonic vibration.

[0014] (7) The method for producing a gallium powder dispersion liquid according to (5) or (6), wherein the surfactant is a fatty acid or an aliphatic amine having a carbon chain length of 10 or more.

[0015] (8) The method for producing a gallium powder dispersion liquid according to any one of (5) to (7), wherein the solvent is methanol, ethanol, isopropyl alcohol, 1-propanol, water, or a mixture thereof.

[0016] (9) The method includes a step of drying the gallium powder dispersion obtained by the method for producing a gallium powder dispersion according to (5) to obtain gallium powder, The gallium powder has an SEM average diameter of 0.2 to 2 μm, and a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof is attached to the surface of the gallium powder. A method for producing gallium powder.

[0017] (10) A gallium powder according to (1) and a solvent, A gallium powder dispersion liquid, characterized in that the gallium powder is dispersed in the solvent.

[0018] (11) A ceramic ceramic material comprising gallium powder, silver powder, a solvent, and a glass frit; The gallium powder has an SEM average diameter of 0.2 μm or more and 2 μm or less, and a surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts thereof or anhydrides thereof is attached to the surface of the gallium powder. A conductive paste.

[0019] (12) The conductive paste according to (11), wherein some or all of the components of the surface treatment agent adhering to the silver powder are the same as some or all of the components of the surfactant adhering to the gallium powder.

[0020] (13) The conductive paste according to (11) or (12), wherein the conductive paste contains 0.01 wt % or more and 4 wt % or less of the gallium relative to the silver. Effect of the Invention

[0021] According to the present invention, it is possible to provide a mixed powder containing the gallium powder, which can be made into a conductive paste that can obtain a gallium powder with a small particle size and a low resistance electrode. In addition, it is possible to provide a gallium powder dispersion liquid that is easy to manufacture and a method for manufacturing the gallium powder, and to provide a gallium powder dispersion liquid and a conductive paste that can obtain a low resistance electrode. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is an SEM image of the gallium powder in Example 1 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The gallium powder according to the present invention is obtained by drying the gallium powder dispersion obtained by the method for producing the gallium powder dispersion according to the present invention. A surfactant is attached to the surface of the gallium powder. The mixed powder contains the gallium powder according to the present invention. The conductive paste according to the present invention can be obtained by using the gallium powder according to the present invention. First, prior to the description of the embodiments, the terms used in this specification will be described.

[0024] -SEM average diameter- The SEM average diameter is determined by measuring the SEM particle diameter (Heywood diameter) of 100 or more particles. In an SEM image magnified at 5,000 times, the Heywood diameter is measured for 100 or more particles whose outer shapes can be clearly recognized using image processing software Mac-View (Ver. 4) manufactured by MOUNTECH, and the average value can be calculated. This measurement method is adopted in this specification.

[0025] - Adhered surfactant - The surfactant attached to the surface of the gallium powder is identified by qualitative analysis using GC / MS. Specifically, the gallium powder is heated in a pyrolyzer in a helium gas flow to thermally desorb the surfactant attached to the surface of the gallium powder, and the desorbed surfactant is then qualitatively analyzed using GC / MS. In addition, the molecular weight and carbon chain length of the surfactant can also be identified by qualitative analysis using GC / MS.

[0026] The method for producing a gallium powder dispersion according to the present invention will be described in detail below.

[0027] (Method of manufacturing gallium powder dispersion) The method for producing a gallium powder dispersion according to the present invention includes at least a first step of stirring a gallium melt, a surfactant, and a solvent to form an emulsion, and a second step of cooling the emulsion. In the first step, the gallium is in a molten state and not solidified, so it is liquid-liquid dispersed with the solvent and is in an emulsion state. Metallic gallium has a melting point of about 30°C, and when cooled to room temperature, it is easily solidified and becomes solid gallium powder. In the second step, the gallium powder is dispersed in a solvent such as alcohol, and a gallium powder dispersion is obtained. Details of each step are described below.

[0028] <First step> In the first step of forming an emulsion, first, high-purity gallium (4N or more) is heated to a temperature above the melting point to obtain a gallium melt. Then, this gallium melt is placed in a solvent, preferably containing a fatty acid. Furthermore, it is preferable to perform stirring using an ultrasonic vibrator such as a homogenizer, and it is preferable to make the metallic gallium into droplets with a small particle size and to attach a surfactant to the surface of the gallium droplets to form an emulsion dispersed in the liquid. By stirring using ultrasonic vibration, it is easier to make the particle size sufficiently small compared to other stirring methods such as stirring blades. However, if the liquid temperature becomes too high, the dispersed metallic gallium droplets tend to gather, and in order to avoid this phenomenon, it is preferable to keep the liquid temperature within the range of the melting point of the solvent to 70°C during stirring.

[0029] <<Gallium melt>> The main component element of the metallic gallium droplets obtained from the gallium melt and the gallium powder obtained by solidifying the same is gallium, and the gallium is 50% or more, preferably 80% or more, in terms of element concentration ratio. It is sufficient that the gallium is liquid at or below the boiling point of the surfactant or solvent used (for example, 70°C or less, preferably 60°C or less). In addition to unavoidable impurities, the gallium melt may contain elements that can be p-type impurities (for example, B, Al, In, Zn, etc.) or elements for fire-through (for example, Te), or may contain alloys of gallium and these elements, and the gallium powder may also contain these impurities and alloy forms.

[0030] <<Surfactants>> The surfactant (also called dispersant) used in this step is selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts or anhydrides thereof. A plurality of surfactants may be used. A reagent containing a selected component as a main component may be used as the surfactant, and the reagent may contain other components. Examples of such surfactants include, for example, stearic acid, palmitic acid, oleic acid, hydroxystearic acid, ricinoleic acid, benzotriazole, dodecenylsuccinic anhydride, pentadecenylsuccinic anhydride, stearylamine, and the like. In particular, as a surfactant that is unlikely to remain after firing, it is preferable to use a surfactant having a carboxy group or an amino group, and it is also preferable to use a known fatty acid or aliphatic amine used in silver powder. The surfactant is preferably a fatty acid or aliphatic amine. It is more preferable that the surfactant has a carbon chain length of 10 or more.

[0031] Here, when the gallium powder dispersion or gallium powder is used in the conductive paste, the surfactant attached to the surface of gallium is also included in the conductive paste. In consideration of this, it is preferable that the surfactant component is one that is unlikely to remain as an impurity in the conductive film after the conductive paste is applied and fired, and it is preferable that the surfactant contains little or no phosphorus and sulfur components. Phosphate-based, sulfonic acid-based, and thiol-based surfactants are very effective for dispersing gallium, but they remain in the form of phosphates or sulfates after firing, so that when they are used as a conductive paste for solar cell electrodes, they may not only deteriorate the characteristics but also the reliability. In addition, it is preferable that the molecular weight of the surfactant used in this process is 100 to 1000. In firing the conductive film in solar cells, etc., the firing time is very short, only a few tens of seconds, so depending on the type of surfactant, especially in the case of polymers with a molecular weight of more than 1000, the debinding may not be completely completed.

[0032] <<Solvent>> The solvent used in this step is not particularly limited as long as it is a solvent capable of dissolving the above-mentioned surfactant. For example, it is preferable to use methanol, ethanol, isopropyl alcohol, 1-propanol, water, or a mixture thereof.

[0033] <Second process> In the second step following the first step, the emulsion is cooled. This cooling solidifies the gallium, and a gallium powder dispersion in which the gallium powder is dispersed in the solvent can be obtained. In order to cool the emulsion, it is preferable to leave it to cool to room temperature after stirring in the first step, or to put the emulsion in a refrigerator and cool it to solidify the droplets to obtain a gallium powder dispersion. After obtaining the gallium powder dispersion, it is preferable to store it in the state of a gallium powder dispersion. Gallium powder can be obtained from this gallium powder dispersion.

[0034] (Method of manufacturing gallium powder) That is, the method for producing gallium powder according to the present invention includes a step of drying the gallium powder dispersion obtained by the above-mentioned method for producing gallium powder dispersion to obtain gallium powder. The gallium powder dispersion is dried at a temperature below the melting point of the gallium powder to obtain gallium powder. Prior to drying, the gallium powder dispersion may be filtered. In addition, after drying, the obtained powder may be subjected to a crushing step and a classification step. The obtained gallium powder has an SEM average diameter of 0.2 μm or more and 2 μm or less, and in particular, it is preferable that a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof is attached to the surface of the gallium powder. It is more preferable that a fatty acid or an aliphatic amine is attached, and it is even more preferable that the fatty acid or the aliphatic amine has a carbon chain length of 10 or more. It is even more preferable that the surfactant on the surface of the gallium powder has a low or no content of sulfur and phosphorus, and is even more preferable that the surfactant has a molecular weight of 100 to 1000.

[0035] (Gallium powder) The gallium powder obtained by the above-mentioned method for producing gallium powder has an SEM average diameter of 0.2 to 2 μm, and a surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts or anhydrides thereof is attached to the surface. The surfactant may contain other components than those mentioned above. It is preferable that the content of sulfur and phosphorus is low or absent, and the surfactant has a molecular weight of 100 to 1000. It is more preferable that the fatty acid or aliphatic amine used as the surfactant has a carbon chain length of 10 or more. This gallium powder can also be dispersed in a solvent to form a gallium powder dispersion.

[0036] (Gallium powder dispersion) That is, the gallium powder dispersion according to the present invention has the above-mentioned gallium powder and a solvent, and the gallium powder is dispersed in the above-mentioned solvent. The solvent can be, for example, methanol, ethanol, isopropyl alcohol, 1-propanol, water, or a mixture thereof, as described above. The solvent of the gallium powder dispersion can be qualitatively analyzed by putting the solvent in a sealed container, heating and vaporizing the components by headspace gas chromatography mass spectrometry (HS-GC / MS). In addition, if a certain amount of organic solvent is put into water and HS-GC / MS is performed in the same manner, it is possible to quantitate by vaporizing only the organic solvent while leaving gallium in the water. The average diameter of the gallium powder in the gallium powder dispersion can be the same as the value measured by SEM average diameter as described above for the gallium powder obtained by drying the gallium powder dispersion with cold air, and is preferably 0.2 to 2 μm.

[0037] (mixed powder) The mixed powder according to the present invention is a mixture of gallium powder and silver powder. The gallium powder is as described above, and has an SEM average diameter of 0.2 μm or more and 2 μm or less, and a surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts or anhydrides thereof is attached to the surface. The silver powder has an SEM average diameter of 0.2 μm or more and 5 μm or less. It is more preferable that the SEM average diameter of the silver powder is 2 μm or less. The SEM average diameter of each of the gallium powder and the silver powder in the mixed powder state can be measured by measuring the SEM particle size (Heywood diameter) while distinguishing the silver particles from the gallium particles by mapping of the SEM-EDS measurement. The silver powder may be a silver powder having a volume-based median diameter (D50) of 0.2 μm or more and 5 μm or less by the laser diffraction method.

[0038] It is preferable that a part or all of the components of the surface treatment agent attached to the silver powder are the same as a part or all of the components of the surfactant attached to the gallium powder. By making the components of the surface treatment agent and the surfactant the same in part or in whole, when the mixed powder is used as a filler in a conductive paste, there is no risk of contamination with components that have adverse effects.

[0039] In addition, the mixed powder preferably contains 0.01 wt% to 4 wt% gallium relative to the silver, and more preferably contains 0.2 wt% to 2 wt% gallium relative to the silver. If the mixed ratio of gallium exceeds 4 wt%, the resistance value may deteriorate. The amount of gallium relative to silver can be determined by quantitatively analyzing gallium and silver by subjecting the mixed powder to ICP analysis.

[0040] (Conductive paste) Next, a conductive paste using the gallium-containing silver powder according to the present invention will be described. The conductive paste according to the present invention contains at least gallium powder, silver powder, a solvent, and glass frit. The gallium powder is the gallium powder according to the present invention described above, and has an SEM average diameter of 0.2 μm or more and 2 μm or less, and a surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts or anhydrides thereof is attached. It is more preferable that the surface treatment agent attached to the silver powder is partially or entirely the same as the surfactant attached to the gallium powder. This conductive paste is suitable for use as a conductive paste for forming electrodes for solar cells. And, in the conductive paste, gallium is preferably contained in an amount of 0.01 wt% to 4 wt% relative to silver, and more preferably 0.2 wt% to 2 wt%. If the mixing ratio of gallium is more than 4 wt%, the resistance value may deteriorate. A method for confirming that the conductive paste "contains gallium" can be performed by ICP analysis. However, since the conductive paste also contains organic solvents and resins, it is preferable to perform pretreatment to remove these before performing ICP analysis. For example, the conductive paste is dispersed and dissolved in a large amount of organic solvent such as acetone, and the solid matter collected by filtering and washing is dissolved in nitric acid and hydrochloric acid, so that ICP analysis can be performed. Since silver and gallium components do not dissolve in organic solvents, the amount of gallium and silver can be quantitatively analyzed by ICP analysis of the solution of the collected solid matter, and the amount of gallium relative to silver can be measured.

[0041] <Filler> The filler may be composed of gallium powder and silver powder. The filler may contain other metal powders such as aluminum powder. The content of the filler in the conductive paste is preferably 65% ​​by mass or more and 95% by mass or less.

[0042] <Solvent> The solvent is not particularly limited, and examples thereof include terpineol, butyl carbitol, butyl carbitol acetate, texanol, etc. Two or more kinds of solvents may be used at the same time. The content of the solvent in the conductive paste is preferably 1% by mass or more and 40% by mass or less.

[0043] <Glass frit> The glass frit is not particularly limited, and preferably has a softening point of 550° C. or less. The shape of the glass frit is not particularly limited, and may be spherical or irregularly spherical. The content of the glass frit in the conductive paste is preferably 0.1% by mass or more and 10% by mass or less.

[0044] <Optional inclusions> The conductive paste may further contain a resin, a dispersant, a surfactant, and a viscosity modifier.

[0045] The conductive paste described above can be manufactured by a general method, except that the gallium-containing silver powder according to the present invention is used as a filler. For example, a paste composition containing at least a filler, a solvent, and a glass frit is appropriately adjusted. Then, the paste composition is mixed, pre-mixed with a stirrer, and then kneaded with a three-roll mill or the like to obtain a conductive paste. When performing dispersion and kneading, ultrasonic dispersion, a disperser, a three-roll mill, a ball mill, a bead mill, a two-axis kneader, a self-revolving stirrer, or the like may be used. If the obtained conductive paste is printed on a substrate by, for example, screen printing, offset printing, photolithography, inkjet printing, or the like, a conductive film of a desired shape can be formed. EXAMPLES

[0046] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples. Not limited to this.

[0047] Example 1 First, solid-state metallic gallium (manufactured by DOWA Electronics) with a purity of 99.99% was liquefied by heating it in a hot bath at 60°C. In addition, 20 g (room temperature) of an isopropyl alcohol (manufactured by FUJIFILM; Wako Grade 1) solution in which 1% by weight of stearic acid (used as a surfactant, manufactured by FUJIFILM; special grade reagent) was dissolved was prepared. 1 g of liquefied gallium was added to this isopropyl alcohol solution to obtain a gallium-containing liquid. This gallium-containing liquid was subjected to ultrasonic dispersion treatment using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho, model number: US-600AT). At that time, the gallium-containing liquid was cooled in a water bath and intermittently subjected to ultrasonic dispersion treatment for a total of 5 minutes while taking cooling time in between so that the temperature of the gallium-containing liquid would not exceed 70°C due to heat generated by ultrasonic irradiation, and an emulsion liquid in which metallic gallium droplets were dispersed was obtained. The liquid temperature was about 40°C, and ultrasonic dispersion was performed until gallium was no longer accumulated at the bottom of the beaker. After that, the dispersion process was stopped and the mixture was left to stand at room temperature, so that the gallium droplets were solidified while remaining dispersed, and a gallium powder dispersion liquid was obtained. Note that the output of the device during ultrasonic dispersion was not constant because it was affected by the dispersion state and the liquid temperature, and varied between 150W and 250W.

[0048] In order to evaluate the obtained gallium powder dispersion, the emulsion liquid in which metal gallium droplets were dispersed was separated, cooled in a refrigerator, and the obtained gallium powder dispersion was dried with cold air to obtain gallium powder. Figure 1 shows an SEM photograph of the gallium powder observed at a magnification of 5000 times using an SEM. In addition, the Heywood diameter of 100 or more particles with clear particle contours was measured using image processing software (Mac-View Ver.4 manufactured by MOUNTECH Co., Ltd.) for the obtained SEM observation image, and the average value was taken as the SEM average diameter. The SEM average diameter of the gallium powder was 0.9 μm.

[0049] (Preparation of conductive paste) Spherical silver powder (AG4-8FD, SEM average diameter 1.3 μm, manufactured by DOWA Electronics) and gallium powder (SEM average diameter 0.9 μm) obtained by pressure filtering the gallium powder dispersion in Example 1 above with a 0.2 μm membrane filter and vacuum drying at room temperature for 30 minutes were mixed so that the ratio of gallium powder in the filler was 1 wt%, and a mixed powder was obtained and used as a filler. Using this filler, a conductive paste was prepared with the paste composition shown in Table 1 below. The gallium content ratio to silver in the conductive paste was 1.01 wt%. The main component of the surface treatment agent attached to the surface of the spherical silver powder used was stearic acid, which is the same as the component of the surfactant attached to the surface of the gallium powder. In addition, the particle size distribution of the spherical silver powder used was measured by laser diffraction wet sample measurement using a Microtrack particle size distribution measuring device (manufactured by Microtrack Bell Co., Ltd., device name: MT-3300EXII). The volume-based median diameter (D50) measured by the laser diffraction method was 1.89 μm.

[0050] [Table 1]

[0051] These were mixed and pre-kneaded under the condition of a rotary stirrer (revolution 1000 rpm). After pre-kneading, the mixture was kneaded with a three-roll mill (manufactured by Exact) to obtain a conductive paste.

[0052] (Resistance measurement) The conductive paste was used to print a straight line shape by screen printing. The design line width of the straight line was 10, 12, 14, 16, 18, and 20 μm, respectively, and the length of the straight line was 150 mm. A Microtec printer was used for printing, and printing was performed at a squeegee speed of 350 mm / s. A silicon substrate with a thickness of about 170 μm (for solar cells, texture formation and SiNx film formation) was used for printing. After printing, the sample was dried for 5 minutes in a dryer set at a temperature of 200°C. A solar cell baking furnace (NGK) was used to bake the sample, and the furnace was set so that the peak temperature of the upper surface of the wafer was 400°C and 700°C, respectively. The resistance value of the printed electrode after baking was measured with a digital multimeter (ADC Corporation) by placing measuring terminals on both ends of the printed electrode.

[0053] (Comparative Example) The filler used in the conductive paste was spherical silver powder AG4-8FD manufactured by DOWA Electronics and Al powder (average particle size 5 μm). The Al powder was mixed so that the ratio of the filler was 1 wt%. The other conditions were the same as in Example 1, and the conductive paste was prepared, printed, and the resistance value of the printed electrode after firing was measured. The aluminum content ratio to silver in the conductive paste was 1.01 wt%.

[0054] The resistance values ​​when the line width was 18 μm in the above examples and comparative examples are shown in Table 2 below.

[0055] [Table 2]

[0056] In the low-temperature firing at 400° C., the resistance could be reduced by using the gallium powder of Example 1 compared to the comparative example.

[0057] The high-temperature firing at 700°C is a temperature at which Al can easily reach the interface with the p-type semiconductor layer of the solar cell because the melting point of Al is 660°C. It was found that when Al powder is mixed with silver powder as in the comparative example, the resistance value increases significantly. However, it was found that such a significant increase in resistance was not observed in Example 1 in which gallium powder was added according to Example 1. [Industrial Applicability]

[0058] According to the present invention, it is possible to provide a mixed powder containing the gallium powder, which can be made into a conductive paste that can obtain a gallium powder with a small particle size and a low resistance electrode. In addition, it is possible to provide a gallium powder dispersion liquid that is easy to manufacture and a method for manufacturing the gallium powder, and to provide a gallium powder dispersion liquid and a conductive paste that can obtain a low resistance electrode.

Claims

1. A gallium powder having an SEM average diameter of 0.2 μm or more and 2 μm or less, and having a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt or an anhydride thereof attached to the surface.

2. A gallium powder having an SEM average diameter of 0.2 μm or more and 2 μm or less, and having a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof attached to the surface; A mixed powder obtained by mixing with silver powder having an SEM average diameter of 0.2 μm or more and 5 μm or less.

3. The mixed powder according to claim 2 , wherein a part or all of the components of the surface treatment agent adhering to the silver powder are the same as a part or all of the components of the surfactant adhering to the gallium powder.

4. The mixed powder according to claim 2 , wherein the gallium content is 0.01 wt % or more and 4 wt % or less relative to the silver.

5. A first step of forming an emulsion by stirring a gallium melt, a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt or an anhydride thereof, and a solvent; A second step of cooling the emulsion; Including, In the first step, the stirring is performed by ultrasonic vibration, The method for producing a gallium powder dispersion liquid, wherein the solvent is methanol, ethanol, isopropyl alcohol, 1-propanol, water, or a mixture thereof.

6. The method for producing a gallium powder dispersion liquid according to claim 5, wherein the surfactant is a fatty acid or an aliphatic amine having a carbon chain length of 10 or more.

7. The method includes a step of drying the gallium powder dispersion obtained by the method for producing the gallium powder dispersion according to claim 5 to obtain gallium powder, The gallium powder has an SEM average diameter of 0.2 to 2 μm, and a surfactant selected from a fatty acid, an azole compound, an alkenylsuccinic acid, an aliphatic amine, or a salt thereof or an anhydride thereof is attached to the surface of the gallium powder. A method for producing gallium powder.

8. A method for producing a gallium powder according to claim 1, comprising: A gallium powder dispersion liquid, characterized in that the gallium powder is dispersed in the solvent.

9. Contains gallium powder, silver powder, a solvent, and glass frit; The gallium powder has an SEM average diameter of 0.2 μm or more and 2 μm or less, and a surfactant selected from fatty acids, azole compounds, alkenylsuccinic acids, aliphatic amines, or salts thereof or anhydrides thereof is attached to the surface of the gallium powder. A conductive paste.

10. The conductive paste according to claim 9, wherein some or all of the components of the surface treatment agent adhering to the silver powder are the same as some or all of the components of the surfactant adhering to the gallium powder.

11. The conductive paste according to claim 9 , wherein the conductive paste contains 0.01 wt % or more and 4 wt % or less of the gallium relative to the silver.

Citation Information

Patent Citations

  • Preparation method of shell-core structure functional conductive particle

    CN110223798A

  • Positive silver paste suitable for positive aluminum oxide-silicon nitride laminated passivation crystalline silicon solar cell and preparation method of positive silver paste

    CN111128436A

  • Production of fine particle of gallium-containing metal

    JP1990285006A

  • Purifier of circulating bath

    JP1996000924A

  • Thermal hardening type low resistance conductive paste

    JP2002008443A