Method for preparing silicon nitride ceramic material

A two-step sintering process with controlled atmospheres and specific sintering aids transforms silicon nitride ceramics into high thermal conductivity materials by minimizing defects and converting grain boundary phases, addressing the limitations of conventional silicon nitride ceramics for high-power semiconductor applications.

JP7578835B2Active Publication Date: 2024-11-06SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023543225
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-20
Filing Date
2022-01-17
Publication Date
2024-11-06
Estimated Expiration
2042-01-17

AI Technical Summary

Technical Problem

Conventional silicon nitride ceramic materials exhibit low thermal conductivity and are difficult to densify due to the presence of lattice defects and amorphous grain boundary phases, which are exacerbated by the use of sintering aids, making them unsuitable for high-power semiconductor devices.

Method used

A two-step sintering process is employed, involving low-temperature and high-temperature heat treatments under controlled atmospheres to minimize impurities and convert amorphous grain boundary phases to crystalline phases, using specific sintering aids like Y2O3 and MgO to promote densification and enhance thermal conductivity.

Benefits of technology

The resulting silicon nitride ceramic materials achieve thermal conductivity of 90 W m⁻¹·K⁻¹ and breakdown electric field strength of 30 kV/mm, suitable for high-power semiconductor devices with improved mechanical and thermal performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578835000001
    Figure 0007578835000001
  • Figure 0007578835000002
    Figure 0007578835000002
  • Figure 0007578835000003
    Figure 0007578835000003
Patent Text Reader

Abstract

The present invention relates to a method for producing a silicon nitride ceramic material, comprising the steps of: (1) using at least one of silica fume and silicon nitride powder as a raw material powder; 2 O 3 (1) mixing the raw material powder and the sintering aid in a protective atmosphere, using MgO powder as a sintering aid, and molding the mixture to obtain a raw material; (2) placing the obtained raw material in a reducing atmosphere and performing pretreatment at 500-800°C to obtain a rough body, the reducing atmosphere being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5% or less; and (3) placing the obtained rough body in a nitrogen atmosphere and performing low-temperature heat treatment at 1600-1800°C and then high-temperature heat treatment at 1800-2000°C.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for preparing silicon nitride ceramic materials and belongs to the field of silicon nitride ceramics. [Background technology]

[0002] In recent years, semiconductor devices have been rapidly developing toward higher power, higher frequency, and greater integration. The heat generated by the operation of semiconductor devices is a factor that can cause failures in semiconductor devices, and the thermal conductivity of insulating substrates is an important factor that affects the overall heat dissipation of semiconductor devices. In addition, in fields such as electric vehicles, high-speed railways, and rail traffic, semiconductor devices are constantly exposed to complex mechanical environments, including shocks and vibrations, during use, which places strict demands on the reliability of the materials used.

[0003] High thermal conductivity silicon nitride (Si3N4) ceramics is considered to be the optimal semiconductor insulating substrate material with high strength and high thermal conductivity due to its excellent mechanical and thermal performance, and has great potential in the heat dissipation application of high power insulated gate bipolar transistors (IGBTs). The theoretical thermal conductivity of silicon nitride crystal is 400 W m -1 ·K -1 With its excellent mechanical properties and potential for high thermal conductivity, silicon nitride ceramics are expected to make up for the shortcomings of existing ceramic substrate materials such as alumina and aluminum nitride, and have great potential for application to high-end semiconductor devices, especially high-power IGBT heat dissipation substrates. However, the thermal conductivity of conventional silicon nitride ceramic materials is only 20-30 W·m -1 ·K -1 This is only sufficient to completely meet the application demands of heat dissipation for high-power semiconductor device substrates.

[0004] On the other hand, silicon nitride is a strong covalent compound and is difficult to sinter densely by solid-state diffusion, so it is necessary to add an appropriate amount (the amount added is usually more than 5wt%) of rare earth oxides and / or metal oxides as sintering aids (e.g. Y2O3, La2O3, MgO, Al2O3, CaO, etc.). However, the addition of sintering aids significantly reduces the thermal conductivity of silicon nitride ceramics, and a low content of sintering aids contributes to obtaining high thermal conductivity, but a low content of sintering aids leads to problems with densification of silicon nitride ceramics sintering. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-330178 A [Patent Document 2] China Patent Application Publication No. 108585881 [Non-patent literature]

[0006] [Non-Patent Document 1] DUAN Yusen et al., “Cost effective preparation of Si3N4 ceramics with improved thermal”, Journal of the European Ceramic Society, Vol. 40, No. 2, October 2019 (2019-10-05), ISSN: 0955-2219, page 2, Experiment procedure section Summary of the Invention

[0007] In order to solve the above technical problems, the present invention provides a method for preparing a silicon nitride ceramic material, so as to obtain a dense silicon nitride ceramic material with high thermal conductivity.

[0008] In the course of previous research, the inventor discovered that silicon nitride ceramics is a phonon heat transfer mechanism, and only when the silicon nitride crystal lattice is perfect and defect-free can the phonon mean free path be large and the thermal conductivity be high. However, in the process of preparing silicon nitride ceramic materials, lattice oxygen, metal impurity ions, carbon impurities, etc. always enter the silicon nitride crystal lattice to different degrees, forming structural defects such as vacancies and dislocations, which greatly reduce the phonon mean free path, thereby reducing the thermal conductivity of the material. Therefore, how to reduce the content of lattice oxygen, metal impurity ions, carbon impurities, etc. is the key to improving the thermal conductivity of silicon nitride ceramic materials.

[0009] The inventors have found that in the process of sintering silicon nitride ceramic materials at high temperatures, the added sintering aid can form a low molten liquid phase and prevent a small amount of native oxide (SiO, SiO) on the surface of the silicon nitride powder. x It was further discovered that the formation of a low-melting-point liquid phase, which is easily reactive to metals such as fluorine, fluorine-containing oxides, etc., promotes the liquid-phase mass transfer of silicon nitride crystal grains to realize high-temperature sintering densification (i.e., liquid-phase sintering mechanism). However, as the sintering temperature decreases, these liquid phases form grain boundary phases between silicon nitride crystal grains, which are mainly composed of an amorphous glass phase, and this grain boundary phase, which is mainly composed of an amorphous glass phase, has low thermal conductivity (generally several to several tens of W·m -1 ·K -1 Therefore, how to transform the amorphous grain boundary phase into a crystallized grain boundary phase (i.e., how to increase the content of the crystalline phase in the grain boundary phase) is a key point in improving the thermal conductivity of silicon nitride ceramic materials.

[0010] Furthermore, preliminary research by the present inventors has revealed that the thermal conductivity of silicon nitride ceramics tends to decrease as the ionic radius of the rare earth element in the sintering aid increases, and that compared with the MgO sintering aid, the addition of CaO sintering aid does not contribute to the growth of columnar crystal grains of silicon nitride, resulting in generally lower thermal conductivity and strength.

[0011] As a result of the above research, the inventors have determined that how to select an appropriate type of sintering aid, how to control the content of the sintering aid, and how to control the degree of crystallinity of the grain boundary phase are important means for improving the thermal conductivity of silicon nitride ceramic materials.

[0012] In this regard, in one aspect, the present invention provides a method for producing a silicon nitride ceramic material, the method comprising the steps of: Silicon Powder and silicon nitride powder End a step of mixing at least one of the above powders as raw material powders, Y2O3 powder and MgO powder as sintering aids, and forming the raw material powders and sintering aids in a protective atmosphere to obtain a base material, wherein the molar ratio of the Y2O3 powder to the MgO powder is (1.0-1.4):(2.5-2.9), the proportion of the sintering aid is 5 wt% or less of the sum of the mass of the raw material powders and the mass of the sintering aids, and the raw material powders are Silicon Powder or Silicon Powder and silicon nitride powder End In the case of a mixed powder of silicon nitride powder and silicon nitride powder, the mass of the raw powder is the mass of the raw powder. End and in the raw powder Silicon Powder This refers to the total mass of silicon nitride produced after the nitriding process, and is calculated based on the mass of the raw powder. Silicon Powder If it contains, Silicon Powder (1) wherein the mass of the raw material powder is 75 wt% or more of the raw material powder mass, and the protective atmosphere is an inert atmosphere or a nitrogen atmosphere; (2) placing the obtained material in a reducing atmosphere and pretreating it at 500 to 800°C to obtain a rough body, the reducing atmosphere being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5 vol% or less; The rough body is subjected to a low-temperature heat treatment at 1600 to 1800°C in a nitrogen atmosphere, and then a high-temperature heat treatment at 1800 to 2000°C to obtain the silicon nitride ceramic material. Silicon Powderand (3) nitriding the rough body obtained after the pretreatment and before the low-temperature heat treatment, the nitriding parameters being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5 vol% or less, a pressure of 0.1 to 0.2 MPa, a temperature of 1350 to 1450°C, and a heat-holding time of 3 to 6 hours; The silicon nitride ceramic material thus obtained contains a silicon nitride phase and a grain boundary phase, the content of the silicon nitride phase being ≥ 95 wt%, the grain boundary phase being a mixture containing at least the three elements Y, Mg, and O, the content of the grain boundary phase being ≤ 5 wt%, and the content of the crystalline phase in the grain boundary phase being ≥ 40 vol%, and the thermal conductivity being 90 W m -1 ·K -1 and the breakdown electric field strength is 30 kV / mm or more.

[0013] In another aspect, the present invention further provides a method for producing the silicon nitride ceramic material. Another aspect of the method for producing the silicon nitride ceramic material of the present invention includes the steps of: Silicon Powder and silicon nitride powder End a step of using at least one of the above as a raw material powder, using Y2O3 powder and MgO powder as sintering aids, further adding an organic solvent and an adhesive, and mixing in a protective atmosphere to obtain a mixed slurry, wherein the molar ratio of the Y2O3 powder to the MgO powder is (1.0-1.4):(2.5-2.9), the proportion of the sintering aid is 5 wt% or less of the sum of the raw material powder mass and the sintering aid mass, and the raw material powder is Silicon Powder or Silicon Powder and silicon nitride powder End In the case of a mixed powder of silicon nitride powder and silicon nitride powder, the mass of the raw powder is the mass of the raw powder. End and in the raw powder Silicon Powder This refers to the total mass of silicon nitride produced after nitriding, and is calculated based on the raw powder. Silicon Powder If it contains, Silicon Powder Step (1), in which the mass of the adhesive is 75 wt% or more of the mass of the raw material powder, the protective atmosphere is an inert atmosphere or a nitrogen atmosphere, and the amount of the adhesive added is 5 to 9 wt% of the sum of the mass of the raw material powder and the mass of the sintering aid; (2) obtaining a dough by tape casting the obtained mixed slurry in a protective atmosphere; (3) placing the obtained material in a reducing atmosphere and pretreating it at 500 to 800°C to obtain a rough body, the reducing atmosphere being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5 vol% or less; The rough body is placed in a nitrogen atmosphere, and first, a low-temperature heat treatment is performed at 1600 to 1800°C, and then a high-temperature heat treatment is performed at 1800 to 2000°C to obtain the silicon nitride ceramic material. Silicon Powder and (4) nitriding the rough body obtained after the pretreatment and before the low-temperature heat treatment, the nitriding parameters being a hydrogen-nitrogen mixed atmosphere having a hydrogen content of 5 vol% or less, a pressure of 0.1 to 0.2 MPa, a temperature of 1350 to 1450°C, and a heat-holding time of 3 to 6 hours; The silicon nitride ceramic material thus obtained contains a silicon nitride phase and a grain boundary phase, the content of the silicon nitride phase being ≥ 95 wt%, the grain boundary phase being a mixture containing at least the three elements Y, Mg, and O, the content of the grain boundary phase being ≤ 5 wt%, and the content of the crystalline phase in the grain boundary phase being ≥ 40 vol%, and the thermal conductivity being 90 W m -1 ·K -1 and the breakdown electric field strength is 30 kV / mm or more.

[0014] In the present invention, the inventors complete the preparation of the powder and the rough body in a protective atmosphere to control the oxygen content, metal impurity ions, impurity carbon atoms and other impurities in the raw powder, and at the same time, pre-treat the rough body in a reducing atmosphere to suppress further oxidation during the preparation of the raw powder, thereby ultimately reducing the concentration of oxygen and other defects in the silicon nitride ceramic lattice. Based on this, the inventors use a two-stage sintering method (firstly perform low-temperature heat treatment at 1600-1800°C in a nitrogen atmosphere, and then perform high-temperature heat treatment at 1800-2000°C) to adjust the components and content of the grain boundary phase in the silicon nitride ceramic material, improve the content of the crystalline phase in the grain boundary phase, and finally obtain a silicon nitride ceramic material with high thermal conductivity and high breakdown field strength. Specifically, first, in the low-temperature sintering stage at 1600-1800°C, the sintering aid is promoted to generate a liquid phase, and densification is promoted. Then, in the high-temperature stage at 1800-2000°C, the remaining MgO sintering aid is partially volatilized, and the content of the grain boundary phase is controlled to be ≦5wt%. At the same time, the content of the glass phase in the grain boundary phase is further reduced, and the content of the crystalline phase in the grain boundary phase is ≧40vol%, so as to reduce the content of the grain boundary phase, increase the crystallinity of the grain boundary phase, and further achieve the purpose of improving the thermal conductivity and breakdown field strength of the silicon nitride ceramic material. The silicon nitride ceramic material obtained has a high composition content of silicon nitride phase and a volume content of the crystalline phase in the grain boundary phase of ≧40%, and this high silicon nitride crystalline phase and the grain boundary phase of the crystal are favorable for reducing the scattering of phonons, and improve the thermal conductivity and breakdown field strength of the silicon nitride ceramic material. Generally, sintering aid oxides (e.g., Y2O3, MgO, etc.) and small amounts of native oxides (SiO2, SiO x In the high-temperature sintering process of silicon nitride ceramic materials, low molten liquid phases are formed (i.e., liquid phase sintering mechanism), and with the decrease in sintering temperature, these low molten liquid phases are always transformed into solid state (i.e., grain boundary phase) in the form of amorphous glass phase and exist in the fabricated silicon nitride ceramic materials. Compared with silicon nitride crystal grains, the thermal conductivity and breakdown electric field strength of the grain boundary phase are lower, and the higher the content of amorphous glass phase in the grain boundary phase, the lower its corresponding thermal conductivity and breakdown electric field strength.

[0015] Preferably, the total amount of impurities in the resulting silicon nitride ceramic material is ≦1.0 wt%. Preferably, the resulting impurities include at least one of lattice oxygen, metal impurity ions, and impurity carbon.

[0016] In this method, the pretreatment time is preferably 1 to 3 hours.

[0017] In this method, preferably, the pressure of the nitrogen atmosphere (preferably not containing hydrogen) is 0.5 to 10 MPa, the time of the low-temperature heat treatment is 1.5 to 2.5 hours, and the time of the high-temperature heat treatment is 4 to 12 hours. Effect of the Invention

[0018] The present invention achieves the purpose of reducing the amount of structural defects such as crystal vacancies and dislocations and improving the thermal conductivity and breakdown field strength of silicon nitride ceramic materials by controlling the oxygen content during the preparation process (including avoiding the oxidation of raw materials during mixing and molding, and pre-treatment in a reducing atmosphere), controlling the content of metal impurity ions, and controlling the carbon content. At the same time, the present invention adjusts the components and content of the grain boundary phase through a two-stage sintering process, promoting the sintering aid to generate a liquid phase in the low-temperature sintering stage, promoting densification, and allowing the remaining MgO sintering aid to partially volatilize in the high-temperature stage, while further reducing the content of the glass phase in the grain boundary phase, thereby reducing the content of the grain boundary phase, increasing the crystallization degree of the grain boundary phase, and further improving the thermal conductivity of silicon nitride ceramic materials. At the same time, the high breakdown field strength of the material contributes to the application of high-power devices, and contributes to reducing the thickness of the substrate material and reducing the thermal resistance, and the copper-clad laminates made of this material embody typical properties such as thermal shock resistance, high reliability, and long life. [Brief description of the drawings]

[0019] [Figure 1] 1 is an XRD pattern of the silicon nitride ceramic material produced in Example 1. [Diagram 2]1 is a typical SEM microstructure of the silicon nitride ceramic material produced in Example 1. [Diagram 3] 1 is a typical TEM microstructure of the silicon nitride ceramic material produced in Example 1. [Figure 4] 1 is an XRD pattern of the material produced after nitridation in Example 6. [Diagram 5] 1 is an XRD pattern of the material produced in Example 6 after high temperature sintering. [Figure 6] 1 is a typical SEM microstructure of the silicon nitride ceramic material produced in Example 6. [Figure 7] Table 1 shows the composition of silicon nitride ceramic materials and their manufacturing process. [Figure 8] Table 2 shows the phase composition and performance parameters of silicon nitride ceramic materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be further described below with reference to the following embodiments. It should be understood that the following embodiments are only for illustrating the present invention, and are not intended to limit the present invention.

[0021] In the present disclosure, the silicon nitride ceramic material contains 95% or more of silicon nitride phase and grain boundary phase with a crystalline phase content of 40% or more. The silicon nitride ceramic material thus obtained has low contents of lattice oxygen, metal impurity ions, carbon impurities, etc., with the total amount being 1.0 wt% or less. Therefore, the silicon nitride ceramic material in the present invention has high thermal conductivity and breakdown electric field strength.

[0022] In one embodiment of the present invention, a cleaning and protective atmosphere preparation process is adopted to avoid contact of air or hot air with the material, and the impurity and oxygen contents in the ceramic preparation are controlled to achieve the purpose of improving the thermal conductivity and breakdown field strength of the material without reducing the bending strength of the material. The method for preparing silicon nitride ceramic material provided by the present invention is described below by way of example.

[0023] The method for preparing the silicon nitride ceramic material specifically includes the steps of mixing and green compacting in a protective atmosphere, pre-treatment in a reducing atmosphere, sintering in a nitrogen atmosphere and controlling the sintering precision.

[0024] Mixing in a Protective Atmosphere The raw material powder, sintering aid Y2O3 powder and MgO powder are mixed uniformly in a sealed container with anhydrous ethanol as a solvent, and then mixed uniformly in a protective atmosphere, and then dried to obtain a mixed powder. Alternatively, the raw material powder, sintering aid Y2O3 powder and MgO powder are placed in a sealed container, and then anhydrous ethanol is added as an organic solvent, and PVB is used as an adhesive, and then mixed uniformly in a protective atmosphere to obtain a mixed slurry. The adhesive may be 5wt% of the total mass of the raw material powder + sintering aid. The solid content of the obtained mixed slurry is 50-70wt%.

[0025] In an alternative embodiment, the protective atmosphere used for mixing is an inert atmosphere or a nitrogen atmosphere, preferably a nitrogen atmosphere. Preferably, mixing is performed using a closed container with a polyurethane or nylon lining, and the container is sparged with nitrogen to prevent air ingress.

[0026] In an alternative embodiment, the raw material powder is silicon nitride powder, Silicon Powder , or silicon nitride powder End and Silicon Powder It is a mixed powder of silicon nitride. powder and silicon powder Of the mixed powders, Silicon Powderis 75% or more, that is, the mass ratio of silicon nitride produced after the Si powder nitriding treatment to the entire silicon nitride phase is 80% or more.

[0027] In an alternative embodiment, the total mass of the sintering aid (Y2O3 powder and MgO powder) is 5 wt% or less of the total mass of the raw powder + sintering aid. If the amount of sintering aid is too much, the grain boundary phase content in the silicon nitride ceramic material produced increases, so the thermal conductivity and breakdown field strength of the material decrease. If the amount of sintering aid is too little, densification cannot be sufficiently promoted, the density of the silicon nitride ceramic material produced is relatively low, the porosity increases, and the thermal conductivity and breakdown field strength of the material decrease. More preferably, the molar ratio of Y2O3 and MgO in the sintering aid may be 1.0-1.4:2.5-2.9. If MgO is excessive, the liquid phase eutectic temperature formed by the sintering aid is relatively low, and MgO volatilizes severely at high temperatures, so the thermal conductivity and breakdown field strength of the silicon nitride ceramic material produced is relatively low. If the amount of MgO is small, the ratio of MgO in the sintering aid is relatively low, so the liquid phase eutectic temperature formed by the sintering aid is relatively high and the effect of densifying the material is relatively poor, so that the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both significantly reduced.

[0028] Dough forming in a protective atmosphere In a protective atmosphere, the mixed powder is directly press molded to obtain a dough. Here, the press molding method includes, but is not limited to, dry press molding, isostatic compression molding, etc. Alternatively, in a protective atmosphere, the mixed slurry is directly tape cast molded to obtain a dough (flake dough). Preferably, the mixed slurry is vacuum degassed before tape casting (the vacuum degree is generally -0.1 to -10 kPa, and the treatment time is 4 to 24 hours). More preferably, the scraper height of the tape casting molding is controlled to adjust the thickness of the flake dough. In an optional embodiment, the protective atmosphere used for dough molding may be an inert atmosphere or a nitrogen atmosphere, and is preferably a nitrogen atmosphere. Generally, nitrogen is directly injected during molding to provide protection.

[0029] Pretreatment of the molding material in a reducing atmosphere The pretreatment of the molding material is carried out in a reducing atmosphere at a constant temperature to remove oxygen from the raw powder and to remove organic matter from the molding material. Silicon Powder , or silicon nitride powder and silicon powder When the mixed powder is a mixture of the above, the molding material is first pretreated at a constant temperature in a reducing atmosphere, and then further nitrided in a reducing atmosphere.

[0030] In an alternative embodiment, the pretreatment may be performed in a reducing nitrogen atmosphere having a hydrogen content of 5 vol% or less, and the gas pressure of the reducing atmosphere is 0.1 to 0.2 MPa. The pretreatment temperature may be 500 to 800°C, and the heat retention time may be 1 to 3 hours.

[0031] In an alternative embodiment, the nitriding treatment may be performed in a nitrogen atmosphere having a hydrogen content of 5 vol% or less, and the atmospheric pressure is 0.1 to 0.2 MPa. The nitriding treatment temperature is 1350 to 1450° C., and the heat retention time is 3 to 6 hours.

[0032] The sintering process of the rough body includes low-temperature heat treatment and high-temperature heat treatment. Specifically, the rough body is sintered and densified in a stepwise sintering process under high nitrogen pressure, and the stepwise sintering process includes low-temperature heat treatment to suppress the volatilization of low-melting-point substances in the sintering aid, and further high-temperature sintering to densify the rough body. In the present invention, the sintering process should adopt gas pressure sintering under high nitrogen pressure conditions, and the atmospheric pressure may be 0.5-10 MPa. The rough body can be sintered in a BN crucible. Here, the temperature of the low-temperature heat treatment (low-temperature sintering) may be 1600-1800°C, and the warming time may be 1.5-2.5 hours. The temperature of the high-temperature heat treatment (high-temperature sintering) may be 1800-2000°C, and the warming time may be 4-12 hours.

[0033] In the present invention, the silicon nitride ceramics produced have low contents of lattice oxygen, metal impurity ions, impurity carbon, etc., and are characterized by high thermal conductivity and high breakdown electric field strength, with a thermal conductivity of 90 W m -1 ·K -1 At the same time, the breakdown electric field strength is 30KV / mm or more.

[0034] The present invention will be described in detail below with reference to examples. Similarly, the following examples are only used to further explain the present invention and should not be understood as limiting the scope of protection of the present invention. Any essential improvements and adjustments made by those skilled in the art based on the above content of the present invention are within the scope of protection of the present invention. The following exemplary process parameters are also examples of appropriate ranges. In other words, those skilled in the art can make selections within appropriate ranges based on the description in this specification, and are not limited to the following exemplary specific values.

[0035] Example 1 First, 95g of Si3N4 powder, 5g of sintering aid powder (Y2O3:MgO=1.2:2.5, molar ratio), 1g of castor oil, 1g of PEG, 70g of anhydrous ethanol and 200g of silicon nitride polishing balls were placed in a ball mill tank with polyurethane lining and atmospheric protection. After packaging the ball mill tank cap, the tank was vacuumed and N2 protective atmosphere was injected, and a slurry was obtained after 6 hours of ball milling mixing. 5g of PVB and 3g of DBP were further added to the above slurry, followed by 6 hours of ball milling under N2 atmosphere protection to obtain a uniform slurry. Next, the slurry was vacuum degassed for 6 hours, and the substrate was tape cast in N2 atmosphere protection. The thickness of the substrate was d±0.05mm (d=0.2~2.0). Again, the green substrate was cut into the required shape and placed into a BN crucible, which was then placed in a carbon tube furnace, and then heat-treated in the following process sequence: (1) The specimen was heated to 600°C at a rate of 5°C / min under a 0.15MPa N2 (containing 5% H2) atmosphere, and then pre-treated for 2 hours. (2) In a 2 MPa N2 atmosphere, the temperature was raised to 1650°C at a rate of 5°C / min, and then low-temperature heat treatment was performed for 2 hours. (3) In an 8MPa N2 atmosphere, the temperature was raised to 1950°C at a rate of 3°C / min, and then sintered at high temperature for 8 hours. (4) Cool in the furnace to room temperature.

[0036] The silicon nitride ceramic substrate material produced in this Example 1 has a bending strength of 810 MPa and a thermal conductivity of 106 W m -1 ·K -1The breakdown electric field strength was 45KV / mm. The XRD pattern of this material, as shown in Figure 1, only had high intensity β-Si3N4 diffraction peaks, and no obvious steamed bread-shaped peaks. This indicates that the content of β-Si3N4 phase in the fabricated material was greater than 95wt%, and the content of grain boundary phase was less than 5%. The typical SEM microstructure of the material, as shown in Figure 2, showed that the material had high density and uniform microstructure. The Si3N4 grains (gray black areas) exhibited a typical bimodal distribution, with fine and small equiaxed Si3N4 grains. i 3 N 4 grains and large long columnar S i 3 N The grains were interdigitated with each other. The content of the grain boundary phase (gray area) was low and uniformly diffused and distributed in the Si3N4 matrix. Furthermore, statistical analysis of at least 10 SEM images and reference to the total amount of sintering aids in the raw materials being ≦5 wt%, it can be obtained that the content of the grain boundary phase in the silicon nitride ceramic material prepared in this example is 5 wt%. A typical TEM microstructure of the material is shown in FIG. 3 (B in FIG. 3 is a partial enlargement of the dotted box area in A in FIG. 3), in which the grain boundary phase (gray area) is dispersedly distributed between the Si3N4 grains (gray black area), but the grain boundary phase is composed of a glass phase (light area) and a crystalline phase (dark area). Statistical analysis of at least 10 TEM images shows that the content of the crystalline phase in the grain boundary phase of the silicon nitride ceramic material prepared in this example is about 54 vol%.

[0037] Examples 2 to 5 Specific parameters such as raw material composition, sintering aid composition, pretreatment process, and sintering process are shown in Table 1 (Fig. 7). The process steps refer to Example 1, and the composition and performance of the produced material are shown in Table 2 (Fig. 8).

[0038] Example 6 First, 3g of Si3N4 powder, 55g of Si powder, 4.5g of sintering aid powder (Y2O3:MgO=1.4:2.6, molar ratio), 0.7g of castor oil, 0.6g of PEG, 50g of anhydrous ethanol and 130g of silicon nitride grinding balls were placed in a ball mill tank with polyurethane lining and atmospheric protection. After packaging the ball mill tank cap, the tank was vacuumed and N2 protective atmosphere was injected, and the slurry was obtained after 8 hours of ball milling mixing. 4g of PVB and 2.5g of DBP were further added to the above slurry, and a uniform slurry was obtained after 6 hours of ball milling under N2 atmosphere protection. Next, the slurry was vacuum degassed for 6 hours, and the substrate was tape cast in N2 atmosphere protection. Again, the molded substrate was cut into the required shape and placed in a BN crucible, which was then placed in a carbon tube furnace, and then heat treated in the following process sequence: (1) The specimen was heated to 600°C at a rate of 4°C / min under a 0.2MPa N2 (containing 5% H2) atmosphere and then pretreated for 3 hours. (2) The specimen was heated to 1450°C at a rate of 5°C / min under a 0.2MPa N2 (5% H2) atmosphere, and then nitrided for 6 hours. (3) The specimen was heated to 1700°C at a rate of 6°C / min under a 3MPa N2 atmosphere, and then subjected to low-temperature heat treatment for 2 hours. (4) In an 8MPa N2 atmosphere, the temperature was raised to 1950°C at a rate of 5°C / min, and then sintered at high temperature for 10 hours. (5) Cool in the furnace to room temperature.

[0039] The silicon nitride ceramic substrate material produced in this Example 6 has a bending strength of 710 MPa and a thermal conductivity of 110 W m -1 ·K -1The breakdown electric field strength was 48KV / mm. The XRD pattern of this material after the nitriding process (above process (2)) is shown in FIG. 4, in which the main crystal phase is α-Si3N4, and at the same time, contains a small amount of β-Si3N4 phase (5-10%). The XRD pattern of this material after the high-temperature sintering process (above process (4)) is shown in FIG. 5, in which only β-Si3N4 diffraction peaks are present, and there are no obvious steamed bread-shaped peaks. This indicates that the content of β-Si3N4 phase in the fabricated material is greater than 95wt%, and the content of grain boundary phase is less than 5wt%. Furthermore, using the same method as in Example 1, the content of the crystal phase in the grain boundary phase of the fabricated material was measured to be about 60vol%. A typical SEM microstructure of the material cross section, as shown in FIG. 6, indicates that the material has a high density, uniform microstructure, and is composed of small equiaxed Si3N4 grains and large, long columnar Si3N4 grains interdigitated with each other.

[0040] Examples 7 to 10 Specific parameters such as raw material composition, sintering aid composition, pretreatment process, nitriding process, sintering process, etc. are shown in Table 1 (Fig. 7). The process steps refer to Example 6, and the material composition and performance are shown in Table 2 (Fig. 8).

[0041] Example 11 In this Example 11, the preparation process of silicon nitride ceramic material was referred to Example 1, with the main difference being that 95g of Si3N4 powder, 5g of sintering aid powder (Y2O3:MgO=1.2:2.5, molar ratio), 1g of castor oil, 1g of PEG, 70g of anhydrous ethanol and 200g of silicon nitride grinding balls were placed in a ball mill tank with polyurethane lining and atmospheric protection function. After packaging the ball mill tank cap, the tank was vacuumed and N2 protective atmosphere was injected, and the slurry was obtained by ball milling for 6 hours. Then, the mixture was dried, sieved, dry pressed (20 MPa) and cold isostatically pressed (200 MPa) in a nitrogen atmosphere to obtain a dough.

[0042] Comparative Example 1 The specific parameters of the raw material formulation, sintering aid composition, pretreatment process, sintering process, etc. are the same as those of Example 1 (see Table 1 (Figure 7)), and the process steps refer to Example 1, with the difference being that no nitrogen atmosphere protection measures are adopted during the processes of ball mill mixing and dough molding. The composition and performance of the prepared material are shown in Table 1 (Figure 7). Since the nitrogen atmosphere protection measures described in the present invention were not adopted during the material preparation process, the silicon nitride powder in the raw material End The thermal conductivity and breakdown electric field strength of the prepared silicon nitride ceramic materials both decreased obviously, but the bending strength remained basically unchanged.

[0043] Comparative Example 2 The specific parameters such as the sintering aid composition ratio, pretreatment process, sintering process, etc. are the same as those in Example 1 (see Table 1 (FIG. 7)), with the difference being that the total amount of sintering aid is increased. The composition and performance of the prepared material are shown in Table 2 (FIG. 8). Since the content of sintering aid is relatively high, the content of grain boundary phase with low thermal conductivity characteristics formed by the sintering aid is relatively high, and the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both obviously reduced, but the bending strength is basically unchanged.

[0044] Comparative Example 3 The specific parameters such as raw material composition, sintering aid type and total amount, pretreatment process, sintering process, etc. are the same as those in Example 1 (see Table 1 (Figure 7)), except for the composition of the sintering aid (Y2O3:MgO=1.2:4.0). The composition and performance of the prepared material are shown in Table 2 (Figure 8). Because the ratio of MgO in the sintering aid is relatively high, the liquid phase eutectic temperature formed by the sintering aid is relatively low, and volatilization at high temperatures is serious, and the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both obviously reduced.

[0045] Comparative Example 4 The specific parameters such as raw material composition, sintering aid type and total amount, pretreatment process, sintering process, etc. are the same as those in Example 1 (see Table 1 (Figure 7)), except for the composition of the sintering aid (Y2O3:MgO=1.3:2.0). The composition and performance of the prepared material are shown in Table 2 (Figure 8). Because the ratio of MgO in the sintering aid is relatively low, the liquid phase eutectic temperature formed by the sintering aid is relatively high, and the effect of material densification is relatively poor, so that the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both significantly reduced.

[0046] Comparative Example 5 The specific parameters of the raw material formulation, sintering aid composition, pretreatment process, etc. are the same as those in Example 1 (see Table 1 (FIG. 7)), and the process is similar to that in Example 1, with the difference being that the sintering process is a one-step sintering process. The composition and performance of the prepared material are shown in Table 2 (FIG. 8). Since the low-temperature heat treatment process is not included, serious MgO volatilization occurs when the material is not sufficiently densified, and the densification effect of the material is relatively poor, and the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both obviously reduced.

[0047] Comparative Example 6 The specific parameters of the raw material formulation, sintering aid composition, pretreatment process, sintering process, etc. are the same as those in Example 1 (see Table 1 (FIG. 7)), and the process is the same as that in Example 1, except that the temperature of the low-temperature heat treatment is relatively low. The composition and performance of the prepared material are shown in Table 2 (FIG. 8). Because the temperature of the low-temperature heat treatment is relatively low, the densification effect of the material is relatively poor, and the thermal conductivity and breakdown field strength of the prepared silicon nitride ceramic material are both significantly reduced.

[0048] Comparative Examples 7 to 8 The specific parameters of the raw material formulation, sintering aid composition, pretreatment process, sintering process, etc. are the same as those of Example 8 (see Table 1 (FIG. 7)), and the process is the same as that of Example 8, with the difference being that the nitriding temperature is relatively low (Comparative Example 7) or relatively high (Comparative Example 8). The composition and performance of the prepared material are shown in Table 2 (FIG. 8). Because the nitriding temperature is relatively low (Comparative Example 7) or relatively high (Comparative Example 8), the Si powder nitriding process in the material is insufficient (Comparative Example 7) or some silicification phenomenon occurs (Comparative Example 8), and the mechanical, thermal and electrical performance of the prepared silicon nitride ceramic material are all obviously deteriorated.

Claims

1. At least one of silicon powder and silicon nitride powder is used as raw material powder, and Y 2 O 3 powder and MgO powder as sintering aids, and in a protective atmosphere, the raw material powder and the sintering aids are mixed and molded to obtain a raw material, 2 O 3 a molar ratio of the powder to the MgO powder is (1.0-1.4):(2.5-2.9), the proportion of the sintering aid is 5 wt% or less of the sum of the mass of the raw material powder and the mass of the sintering aid, when the raw material powder is silicon powder or a mixed powder of silicon powder and silicon nitride powder, the mass of the raw material powder refers to the sum of the mass of the silicon nitride powder in the raw material powder and the mass of the silicon nitride generated after the nitriding treatment of the silicon powder in the raw material powder, when the raw material powder contains silicon powder, the mass of the silicon powder is 75 wt% or more of the mass of the raw material powder, and the protective atmosphere is an inert atmosphere or a nitrogen atmosphere; (2) placing the obtained material in a reducing atmosphere and pretreating it at 500 to 800 ° C to obtain a rough body, the reducing atmosphere being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5 vol % or less; The rough body is first subjected to a low-temperature heat treatment at 1600 to 1800 ° C. in a nitrogen atmosphere, and then a high-temperature heat treatment at 1800 to 2000 ° C. to obtain the silicon nitride ceramic material. In the case where the raw material powder contains silicon powder, the rough body obtained is subjected to a nitriding treatment after the pretreatment and before the low-temperature heat treatment, and the parameters of the nitriding treatment are a hydrogen / nitrogen mixed atmosphere with a hydrogen content of 5 vol% or less, a pressure of 0.1 to 0.2 MPa, a temperature of 1350 to 1450 ° C., and a heat retention time of 3 to 6 hours. (3) The silicon nitride ceramic material thus obtained contains a silicon nitride phase and a grain boundary phase, the content of the silicon nitride phase being ≧95 wt %, the grain boundary phase being a mixture containing at least three elements, Y, Mg, and O, the content of the grain boundary phase being ≦5 wt %, and the content of the crystalline phase in the grain boundary phase being ≧40 vol %, and the thermal conductivity being 90 W·m -1 K -1 or more, and the breakdown electric field strength is 30 kV / mm or more; 1. A method for producing a silicon nitride ceramic material comprising the steps of:

2. At least one of silicon powder and silicon nitride powder is used as a raw material powder, and Y 2 O 3 powder and MgO powder as sintering aids, further adding organic solvent and adhesive, and mixing in a protective atmosphere to obtain a mixed slurry; 2 O 3 step (1), in which the molar ratio of the powder to the MgO powder is (1.0-1.4):(2.5-2.9), the proportion of the sintering aid is 5 wt% or less of the sum of the mass of the raw material powder and the mass of the sintering aid, when the raw material powder is silicon powder or a mixed powder of silicon powder and silicon nitride powder, the mass of the raw material powder refers to the sum of the mass of the silicon nitride powder in the raw material powder and the mass of the silicon nitride generated after the silicon powder nitriding treatment in the raw material powder, when the raw material powder contains silicon powder, the mass of the silicon powder is 75 wt% or more of the mass of the raw material powder, the protective atmosphere is an inert atmosphere or a nitrogen atmosphere, and the amount of the adhesive added is 5-9 wt% of the sum of the mass of the raw material powder and the mass of the sintering aid; (2) obtaining a dough by tape casting the obtained mixed slurry in a protective atmosphere; (3) placing the obtained material in a reducing atmosphere and pretreating it at 500 to 800 ° C to obtain a rough body, the reducing atmosphere being a hydrogen / nitrogen mixed atmosphere having a hydrogen content of 5 vol % or less; The rough body is first subjected to a low-temperature heat treatment at 1600 to 1800 ° C. in a nitrogen atmosphere, and then a high-temperature heat treatment at 1800 to 2000 ° C. to obtain the silicon nitride ceramic material. In the case where the raw material powder contains silicon powder, the rough body obtained is subjected to a nitriding treatment after the pretreatment and before the low-temperature heat treatment, and the parameters of the nitriding treatment are a hydrogen / nitrogen mixed atmosphere with a hydrogen content of 5 vol% or less, a pressure of 0.1 to 0.2 MPa, a temperature of 1350 to 1450 ° C., and a heat retention time of 3 to 6 hours. (4) The silicon nitride ceramic material thus obtained contains a silicon nitride phase and a grain boundary phase, the content of the silicon nitride phase being ≧95 wt %, the grain boundary phase being a mixture containing at least three elements, Y, Mg, and O, the content of the grain boundary phase being ≦5 wt %, and the content of the crystalline phase in the grain boundary phase being ≧40 vol %, and the thermal conductivity being 90 W·m -1 K -1 or more, and the breakdown electric field strength is 30 kV / mm or more; 1. A method for producing a silicon nitride ceramic material comprising the steps of:

3. 2. The method according to claim 1, wherein in step (3), the pressure of the nitrogen atmosphere is 0.5 to 10 MPa, the time of the low-temperature heat treatment is 1.5 to 2.5 hours, and the time of the high-temperature heat treatment is 4 to 12 hours.

4. 3. The method according to claim 2, wherein in step (4), the pressure of the nitrogen atmosphere is 0.5 to 10 MPa, the time of the low-temperature heat treatment is 1.5 to 2.5 hours, and the time of the high-temperature heat treatment is 4 to 12 hours.

5. 3. The method of claim 2, wherein the mixed slurry is vacuum degassed before tape casting, and the adhesive is polyvinyl butyral.

Citation Information

Patent Citations

  • High-heat-conductivity silicon nitride ceramic and preparation method thereof

    CN108585881A

  • Circuit board

    JP1997157054A

  • Silicon nitride heat radiating board having pressurized contact and prepared for thyristor, and thyristor using the same

    JP1999345923A

  • Highly thermoconductive silicon nitride sintered compact and its production

    JP2000034172A

  • High thermoconductivity high strength silicon nitride ceramic and manufacturing method therefor

    JP2005330178A