Solder alloy, solder paste, solder ball, solder preform, solder joint, in-vehicle electronic circuit, ECU electronic circuit, in-vehicle electronic circuit device, and ECU electronic circuit device
The solder alloy composition with controlled Ag, Cu, In, Sb, Fe, and Co content addresses shear strength and heat cycle resistance issues, providing reliable automotive electronic circuit connections.
Patent Information
- Application Number
- JP2024015315
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2044-02-04
AI Technical Summary
Existing solder alloys used in automotive electronic circuits fail to provide sufficient shear strength, appropriate failure mode, and consistent heat cycle resistance, especially under varying temperature conditions, leading to potential breakage and safety concerns.
A solder alloy composition comprising specific ranges of Ag, Cu, In, Sb, Fe, and Co, with optional additives, optimized to maintain a low melting point, high shear strength, and appropriate failure mode, evaluated by standard deviation in heat cycle resistance tests.
The optimized solder alloy exhibits uniform performance with minimal breakage under harsh automotive conditions, ensuring reliable electrical connections and improved durability.
Smart Images

Figure 0007578897000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a solder alloy, a solder paste, a solder ball, a solder preform, a solder joint, an on-vehicle electronic circuit, an ECU electronic circuit, an on-vehicle electronic circuit device, and an ECU electronic circuit device. [Background technology]
[0002] Automobiles are equipped with electronic circuits (hereinafter referred to as "on-vehicle electronic circuits") that have electronic components soldered to a printed circuit board. On-vehicle electronic circuits are used in devices that electrically control the engine, power steering, brakes, etc., and are extremely important safety components for the operation of an automobile. In particular, on-vehicle electronic circuits called ECUs (Engine Control Units), which are electronic circuits that control the vehicle via computer to improve fuel efficiency, must be able to operate stably without failure for long periods of time. As the range of on-vehicle electronic circuits expands, they are now installed in locations that are subject to various external loads such as temperature changes, shocks, and vibrations.
[0003] For example, automotive electronic circuits mounted in the engine compartment can be exposed to high temperatures of over 125°C when the engine is running. On the other hand, when the engine is stopped, they can be exposed to low temperatures of under -40°C in cold regions. Highly reliable solder alloys are used for automotive electronic circuits that are used in such harsh environments.
[0004] Conventionally, Sn-Ag-Cu solder alloys have been used as versatile solder alloys. However, as mentioned above, in harsh environments that were not previously expected, the intermetallic compound layer formed at the joint interface of Sn-Ag-Cu solder alloys may become thick, and there is a concern that peeling may occur at the joint interface between the electrode and the solder alloy due to shear stress. For this reason, there is a demand for solder alloys that can maintain their joint strength even in harsh operating environments, and various studies have been conducted in the past.
[0005] Patent Document 1 discloses a Sn-Ag-Cu-In-Sb-Co-Ge solder alloy, which contains In, Sb, and Co in a Sn-Ag-Cu solder alloy, as a solder alloy with high heat cycle resistance. This solder alloy is said to be able to suppress lift-off in addition to being heat cycle resistant. In order to achieve this effect, the document describes that, although Bi has been added conventionally to suppress the rise in melting point caused by Sb, In is added instead of Bi to improve lift-off.
[0006] Patent Document 2 discloses a Sn-Ag-Cu-In-Sb-Ni-Co solder alloy as a solder alloy with high heat cycle resistance. It is said that this solder alloy can suppress the occurrence of voids and lift-off in addition to heat cycle resistance. The document describes that by balancing the Sb and In contents, the occurrence of lift-off and voids can be suppressed in addition to improving heat cycle resistance. The document also describes that Fe and the like may be further contained from the viewpoint of heat cycle resistance and suppressing void occurrence. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6349615 [Patent Document 2] Patent No. 6420936 Summary of the Invention [Problem to be solved by the invention]
[0008] As mentioned above, in the inventions described in Patent Documents 1 and 2, evaluations were conducted on heat cycle resistance and lift-off. Patent Document 2 further evaluated the occurrence of voids. Also, in order to suppress an increase in reflow temperature, evaluations were conducted on the melting point.
[0009] However, these evaluations alone are not sufficient for solder alloys used in automotive electronic circuits. For example, when a vehicle equipped with electronic circuits runs on rough roads, the electronic circuits are subjected to external stress. For this reason, it is very important for solder joints to exhibit high shear strength.
[0010] Even if a solder joint that is difficult to break is formed, if stress is continuously applied to the solder joint, it will eventually break. Such continuous stress is thought to be continuously applied by exposure to an environment with large temperature differences. This is due to the difference in thermal expansion coefficients of the electrodes, the intermetallic compounds formed at the joint interface, and the bulk. In particular, even if the load on the solder joint becomes large, the fracture mode should not be such that the fractured part is the joint interface. Since the joint interface is joined to the electrodes, it is not easy to relieve stress at the joint interface. However, physical and electrical loads are mainly applied to the joint interface of the solder joint. For this reason, it is thought that it is better to suppress fracture by relieving stress in the bulk, which is relatively easy to deform.
[0011] However, Patent Documents 1 and 2 do not consider shear strength and fracture mode at all, and it is difficult to say that they reflect the actual situation when using solder joints. Since solder joints electrically connect substrates and electronic components, fracture at the joint interface should be avoided as much as possible.
[0012] On the other hand, as mentioned above, the study of the environment where stress is continuously applied to the solder joint is evaluated by a heat cycle test. In this regard, the inventions described in Patent Documents 1 and 2 study heat cycle resistance. However, in Patent Document 1, the total length of the crack at 2000 cycles is evaluated as the average value of four samples. Also, in Patent Document 2, it seems that the occurrence of cracks at 3000 cycles is observed in 10 samples, and the occurrence of cracks crossing the solder joint is evaluated.
[0013] As described in Patent Document 1, when evaluation is based only on the average value, if there are samples with short crack lengths and samples with long crack lengths, the sample with the smaller average value will be treated as having a superior evaluation. In reality, if a sample with a long crack length is included, the problem of heat cycle resistance as a solder joint will be overlooked, even though it remains.
[0014] The evaluation described in Patent Document 2 seems to be able to grasp cracks that completely break the solder joint. However, even if there are samples that do not cross the solder joint but are close to crossing it, the sample is treated as having an excellent evaluation. If there are many samples out of 10 samples that have cracks that are close to crossing the solder joint, it is inevitable to think that there are some issues, but such a group of samples is also treated as having an excellent evaluation. Furthermore, in the invention described in Patent Document 2, cracks are evaluated at 3000 cycles by chance, but if there is a concern that several more cycles would cause multiple cracks to cross the solder joint, it must be considered that there is still an issue with heat cycle resistance.
[0015] In particular, for solder joints mounted on electronic circuits for vehicles, fracture of the solder joints must be prevented as much as possible from the viewpoint of safety. In the evaluation of heat cycle resistance in Patent Documents 1 and 2, there is a possibility that some of the solder joints may fracture in an extremely short cycle. In other words, if there is a large variation in the evaluation results, even samples that are thought to be problem-free may include ones that fracture immediately.
[0016] Thus, Patent Documents 1 and 2 do not consider the shear strength and fracture mode, which are important characteristics of solder joints. In addition, since the electrification of automobiles in recent years is progressing and the number of circuit boards mounted on them is expected to continue to increase, there is an urgent need to develop solder alloys that can guarantee high heat cycle resistance. Furthermore, in consideration of the heat resistance of electronic components, it is also desired that they have a melting point at the same level as conventional solder alloys.
[0017] Therefore, an object of the present invention is to provide a solder alloy, a solder paste, a solder ball, a solder preform, a solder joint, an on-vehicle electronic circuit, an ECU electronic circuit, an on-vehicle electronic circuit device, and an ECU electronic circuit device, which have a low melting point, high shear strength, an appropriate fracture mode, and excellent heat cycle resistance. [Means for solving the problem]
[0018] The present inventors have reexamined the solder alloys disclosed in Patent Documents 1 and 2. Among the solder alloys disclosed in both documents, the Sn-Ag-Cu-In-Sb-Co-Ge solder alloy in Example 12 of Patent Document 1 and the Sn-Ag-Cu-In-Sb-Ni-Co-Fe solder alloy in Example 15 of Patent Document 2 have the same shear strength as conventional solder alloys, and have found that there is room for improvement.
[0019] These solder alloys do not have alloy compositions designed for the purpose of improving shear strength. For each solder alloy, if the content of even one of the compositional components differs, the overall characteristics will usually differ, and it should be understood that the entire combination of alloy elements with a specified content is technically evaluated as a single entity.
[0020] Therefore, the present inventors conducted detailed research into the improvement of shear strength and the fracture mode while suppressing the rise in melting point. As a result, it was found that adding a certain amount of Fe to Example 12 of Patent Document 1 lowers the melting point by about 8 to 10 degrees. This is presumably because adding a certain amount of Fe to a Sn-Ag-Cu-In-Sb-Co-Ge solder alloy further refines the structure of the solder alloy due to a synergistic effect with Co, suppressing the precipitation of coarse compounds.
[0021] In addition, it was found that adding Fe to Sn-Ag-Cu-In-Sb-Co-Ge solder alloys results in the same melting point, shear strength, and fracture mode regardless of whether Ge is present or not. As a result, it was found that Ge can be treated as an optional element in Sn-Ag-Cu-In-Sb-Co-Fe solder alloys.
[0022] It was found that the melting point of Example 15 of Patent Document 2 is slightly higher. It is presumed that this is because when Ni is contained in the Sn-Ag-Cu-In-Sb-Co-Fe solder alloy, the solid phase due to Ni begins to precipitate at a higher temperature during the solidification process. It is also considered that the melting point is increased by the small Cu content, which is slightly deviated from the eutectic composition of Sn-Ag-Cu. Therefore, it was found that by removing Ni from Example 15 of Patent Document 2 and increasing the Cu content by 0.1 to 0.4%, the melting point is lowered and the shear strength is significantly improved.
[0023] Furthermore, it was found that compositions containing enough Co and Fe to make the alloy structure fine exhibited an appropriate fracture mode, since fracture occurred in the bulk. However, it was also found that even if the Co and Fe contents were adjusted, fracture occurred at the bonding interface when the Ag and Sb contents were too high. This is presumably because the bulk strength increased due to the precipitation of compounds, and the same result would occur if the Co and Fe contents were too high. It was also found that when there was a large amount of Cu, the shear strength deteriorated and the fracture mode became the bonding interface. This is presumably because hypereutectic formation occurred and coarse Cu6Sn5 precipitated at the bonding interface.
[0024] In addition to the above findings, Patent Documents 1 and 2 show that heat cycle resistance can be exhibited, but the present inventors confirmed that even in the examples of each patent document, some of the solder alloys broke in an extremely short cycle. In other words, this shows that there is a large variation in the evaluation results. Therefore, even in solder alloys that have been considered to have high heat cycle resistance in the conventional evaluation method, some of them have low heat cycle resistance, so it is necessary to perform a more accurate evaluation. Therefore, the present inventors have come to the conclusion that it is most effective to evaluate the number of cycles to break in the evaluation of heat cycle resistance using the standard deviation. By evaluating using the standard deviation, it is possible to extract solder alloys with low heat cycle resistance that have been overlooked so far, and to evaluate heat cycle resistance with higher accuracy.
[0025] Therefore, the inventors have evaluated the heat cycle resistance by calculating the standard deviation of the number of cycles to fracture. As a result, it has been found that a solder alloy in which each constituent element is within a predetermined range has a low melting point, high shear strength, and an appropriate fracture mode as described above, and further, the standard deviation of the number of cycles to fracture is equal to or less than a predetermined value, and thus the present invention has been completed. The present invention, which was made based on these findings, is as follows.
[0026] (0) A solder alloy comprising, by mass%, 2.0-3.6% Ag, 0.6-0.9% Cu, 1.0-5.0% In, 3.0-5.0% Sb, 0.0010-0.0300% Fe, 0.0010-0.0500% Co, and the remainder being Sn. (1) A solder alloy having an alloy composition, in mass%, of 2.0-3.6% Ag, 0.6-0.9% Cu, 1.0-5.0% In, 3.0-5.0% Sb, 0.0010-0.0300% Fe, 0.0010-0.0500% Co, and the remainder being Sn.
[0027] (2) The solder alloy according to (0) or (1) above, further comprising, by mass%, at least one of Zr, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mo, Pt, Pd, Au, Al, and Si in a total amount of 0.1% or less.
[0028] (3) The solder alloy according to any one of (0) to (2) above, wherein the alloy composition (solder alloy) satisfies the following formulae (1) and (2): 0.0020≦Ag×Cu×In×Sb×Fe×Co≦0.0090 (1) 445≦In / (Ag×Cu×Sb×Fe×Co)≦3560 (2) In the above formulas (1) and (2), Ag, Cu, In, Sb, Fe, and Co each represent the content in mass % of the solder alloy.
[0029] (4) A solder paste comprising a solder powder made of the solder alloy according to any one of (0) to (2) above.
[0030] (5) A solder ball made of the solder alloy according to any one of (0) to (2) above.
[0031] (6) A solder preform made of the solder alloy according to any one of (0) to (2) above.
[0032] (7) A solder joint comprising the solder alloy according to any one of (0) to (2) above.
[0033] (8) An on-vehicle electronic circuit comprising the solder alloy according to any one of (0) to (2) above.
[0034] (9) An ECU electronic circuit comprising the solder alloy according to any one of (0) to (2) above.
[0035] (10) An on-vehicle electronic circuit device comprising the on-vehicle electronic circuit according to (8) above.
[0036] (11) An ECU electronic circuit device comprising the ECU electronic circuit described in (9) above. [Brief description of the drawings]
[0037] [Figure 1] FIG. 1 shows optical microscope photographs of the samples after measuring the shear strength, where FIG. 1(a) is Example 4, FIG. 1(b) is Comparative Example 19, and FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] The present invention will be described in more detail below. In this specification, "%" relating to the solder alloy composition is "mass %" unless otherwise specified.
[0039] 1. Solder Alloy (1) Ag: 2.0-3.6% Ag contributes to improving the shear strength, optimizing the fracture mode by precipitation of Ag3Sn, lowering the melting point, and improving the heat cycle resistance. If the Ag content is less than 2.0%, the amount of compound precipitated is small and the shear strength is reduced. The lower limit of the Ag content is 2.0% or more, preferably 2.5% or more, more preferably 2.7% or more, and even more preferably 3.0% or more.
[0040] On the other hand, when the Ag content exceeds 3.6%, a large amount of Ag3Sn precipitates due to hypereutectic, and the strength of the bulk increases, so that the fracture mode becomes the bonding interface. In addition, the shear strength decreases, and the melting point may increase due to the precipitation of a large amount of compounds. Furthermore, because the strength of the bulk increases, cracks occur during the heat cycle test, the standard deviation increases, and the heat cycle resistance is poor. The upper limit of the Ag content is 3.6% or less, preferably 3.4% or less, and more preferably 3.2% or less.
[0041] (2) Cu: 0.6-0.9% Cu contributes to improving the shear strength, optimizing the fracture mode by controlling the amount of intermetallic compounds formed at the bonding interface, lowering the melting point, and improving the heat cycle resistance. In addition, if the content is appropriate, it is possible to suppress the precipitation of coarse Cu6Sn5. If the Cu content is less than 0.6%, Cu6Sn5 does not precipitate sufficiently, resulting in poor shear strength. In addition, the melting point increases. The lower limit of the Cu content is 0.6% or more, preferably 0.7% or more.
[0042] On the other hand, if the Cu content exceeds 0.9%, the shear strength deteriorates due to the hypereutectic structure and the precipitation of coarse Cu6Sn5 at the bonding interface. Also, the fracture mode becomes the bonding interface. Furthermore, the shear strength deteriorates, so that cracks occur during the heat cycle test, the standard deviation increases, and the heat cycle resistance deteriorates. The upper limit of the Cu content is 0.9% or less, and preferably 0.8% or less.
[0043] (3) In: 1.0-5.0% In contributes to improving the shear strength, optimizing the fracture mode, and improving the heat cycle resistance. If the In content is less than 1.0%, the shear strength is poor, and the wettability is reduced, resulting in insufficient wet spread and insufficient effect of solid solution strengthening, resulting in an inappropriate fracture mode and poor heat cycle resistance. The lower limit of the In content is 1.0% or more, preferably 1.5% or more, more preferably 2.0% or more, even more preferably 2.5% or more, and particularly preferably 3.0% or more.
[0044] On the other hand, if the In content exceeds 5.0%, a large amount of compounds are precipitated, causing the melting point to rise. Furthermore, the bulk strength is excessively increased, causing the shear strength to decrease. In addition, there is a concern that the joint interface or parts may break. Furthermore, because the bulk strength increases, cracks may occur during the heat cycle test, the standard deviation value increases, and the heat cycle resistance is poor. The upper limit of the In content is 5.0% or less, preferably 4.5% or less, more preferably 4.0% or less, and even more preferably 3.5% or less.
[0045] (4) Sb: 3.0-5.0% Sb contributes to suppressing the melting point rise, improving the shear strength, optimizing the fracture mode, and improving the heat cycle resistance. If the Sb content is less than 3.0%, the shear strength is inferior because the solid solution strengthening with respect to Sn and the precipitation strengthening of the Sn-Sb compound are insufficient. The lower limit of the Sb content is 3.0% or more, preferably 3.5% or more, more preferably 3.6% or more, even more preferably 3.8% or more, particularly preferably 3.9% or more, and most preferably 4.0% or more.
[0046] On the other hand, if the Sb content exceeds 5.0%, coarse SnSb compounds are formed, resulting in poor shear strength. Furthermore, wettability is deteriorated, and the fracture mode becomes the joint interface or component fracture, which is inappropriate. In addition, the bulk strength increases, so cracks occur during the heat cycle test, the standard deviation increases, and the heat cycle resistance is poor. The upper limit of the Sb content is 5.0% or less, preferably 4.8 or less, more preferably 4.6% or less, even more preferably 4.5% or less, particularly preferably 4.3% or less, and most preferably 4.1% or less.
[0047] (5) Fe: 0.0010~0.0300% Fe contributes to improving the shear strength, optimizing the fracture mode, and improving the heat cycle resistance. If the Fe content is less than 0.0010%, the effect of strengthening the interface by modifying the intermetallic compound layer formed at the interface is insufficient, so the shear strength is poor. The lower limit of the Fe content is 0.0010% or more, preferably 0.0050% or more, more preferably 0.0100% or more, even more preferably 0.0150% or more, and particularly preferably 0.0200% or more.
[0048] On the other hand, if the Fe content exceeds 0.0300%, a compound of Sn and Fe is precipitated, and the bulk strength is excessively increased, so that the shear strength is deteriorated and there is a concern of fracture at the bonding interface. The upper limit of the Fe content is 0.0300% or less, preferably 0.0270% or less, and more preferably 0.0250% or less.
[0049] (6) Co: 0.0010-0.0500% Co contributes to suppressing the melting point rise, improving the shear strength, optimizing the fracture mode, and improving the heat cycle resistance. If the Co content is less than 0.0010%, the bulk refinement effect is insufficient, and the shear strength decreases. The lower limit of the Co content is 0.0010% or more, preferably 0.0030% or more, more preferably 0.0060% or more, and even more preferably 0.0080% or more.
[0050] On the other hand, when the Co content exceeds 0.0500%, a compound of Sn and Co precipitates, and the strength of the bulk increases, so that the fracture mode becomes the bonding interface. In addition, the melting point increases significantly due to the precipitation of a large amount of the compound, and the wettability deteriorates, so that the shear strength decreases. Furthermore, because the strength of the bulk increases, cracks occur during the heat cycle test, the standard deviation increases, and the heat cycle resistance deteriorates. The upper limit of the Co content is 0.0500% or less, preferably 0.0300% or less, and more preferably 0.0100% or less.
[0051] (7) Remainder: Sn The balance of the solder alloy according to the present invention is Sn. In addition to the above elements, unavoidable impurities may be contained. Even if unavoidable impurities are contained, the above-mentioned effects are not affected. In the present invention, Ni is not contained because the melting point rises sharply with the addition of a small amount when the contents of each element are within the above-mentioned range in the Sn-Ag-Cu-In-Sb-Fe-Co solder alloy. In addition, Mn is not contained because the melting point rises, the wettability deteriorates, and an appropriate compound cannot be formed, resulting in a decrease in shear strength. Furthermore, when Bi coexists with In, it forms a Sn-In-Bi low melting point phase. In view of creep deformation, the low melting point phase is prone to creep deformation and strength decreases because the room temperature environment is a very high temperature environment relative to the melting point. For this reason, in the present invention, it is preferable not to contain Bi.
[0052] (8) At least one of Zr, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mo, Pt, Pd, Au, Al, and Si, total content not exceeding 0.1% The solder alloy according to the present invention may contain at least one of Zr, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mo, Pt, Pd, Au, Al, and Si as an optional element in a total amount of 0.1% or less to the extent that the effect of the present invention is not impaired. Preferably, the total amount is 0.08% or less. The lower limit of the content is not particularly limited, but may be 0.0001% or more, and may be 0.001% or more.
[0053] (9) Equations (1) and (2) 0.0020≦Ag×Cu×In×Sb×Fe×Co≦0.0090 (1) 445≦In / (Ag×Cu×Sb×Fe×Co)≦3560 (2) In the above formulas (1) and (2), Ag, Cu, In, Sb, Fe, and Co each represent the content in mass % of the solder alloy.
[0054] Formula (1) is a formula that takes into consideration the balance of the additive elements of the solder alloy according to the present invention. The solder alloy according to the present invention can exhibit a low melting point, high shear strength, appropriate fracture mode, and high heat cycle resistance due to the synergistic effect of each constituent element. Therefore, the balance of all constituent elements except Sn can further improve all the effects of the present invention. In formula (1), the contents of Ag, Cu, In, and Sb are about 10 to 100 times the contents of Fe and Co. However, it is considered that the contribution to the solder alloy is about the same. Therefore, in the present invention, in order to further improve a low melting point, high shear strength, appropriate fracture mode, and high heat cycle resistance simultaneously with one composition, it is preferable to make the contents balanced.
[0055] Formula (2) is a formula that takes into consideration the balance between In and other elements among the additive elements of the solder alloy according to the present invention. Compared with other additive elements, if In is less than the lower limit or exceeds the upper limit of the content range, the shear strength is inferior and the fracture mode becomes inappropriate. This is a phenomenon unique to the Sn-Ag-Cu-In-Sb-Co-Fe solder alloy according to the present invention. The reason for this is unclear, but it is presumed that the wettability is reduced, the wetting spread is insufficient, and the effect of solid solution strengthening is insufficient.
[0056] In the calculation of formulas (1) and (2), the numerical values themselves shown in the measured values of the alloy composition shown in Tables 1 and 2 below are used. That is, in the calculation of formulas (1) and (2), all digits smaller than the number of significant figures in the measured values shown in Tables 1 and 2 below are treated as 0. For example, if the measured value of the Co content is "0.008" mass%, the Co content used in the calculation of formulas (1) and (2) is not in the range of 0.0075 to 0.0084%, but is treated as "0.008000···". In formula (1), the calculation is made up to the fifth decimal place, and the fifth decimal place is rounded off to the fourth decimal place, while in formula (2), the calculation is made up to the first decimal place, and the first decimal place is rounded off to the first decimal place. The same procedure is applied when calculating the formulas (1) and (2) from alloy compositions specifically disclosed in patent documents or other documents mentioned in this specification.
[0057] As mentioned above, in an alloy, all the constituent elements do not function individually, but all the constituent elements form one entity as a whole, so it is rare that one element alone can simultaneously exhibit all the excellent effects. Therefore, as mentioned above, in order to exhibit even more excellent properties within the optimum content range of each constituent element, it is necessary to consider the constituent elements as a whole. In the solder alloy of the present invention, in order to achieve a low melting point, high shear strength, appropriate fracture mode, and high heat cycle resistance at an even higher level with one composition, it is preferable to satisfy formulas (1) and (2).
[0058] The lower limit of formula (1) is preferably 0.0020 or more, more preferably 0.0021 or more, even more preferably 0.0022 or more, even more preferably 0.0023 or more, particularly preferably 0.0024 or more, and most preferably 0.0028 or more, and may be 0.0029 or more, 0.0033 or more, 0.0034 or more, 0.0035 or more, 0.0036 or more, 0.0038 or more, 0.0042 or more, 0.0043 or more, 0.0045 or more, 0.0046 or more, 0.0048 or more, 0.0049 or more, 0.0050 or more, or 0.0057 or more. The upper limit of formula (1) is preferably 0.0090 or less, more preferably 0.0086 or less, even more preferably 0.085 or less, even more preferably 0.0083 or less, particularly preferably 0.0076 or less, and most preferably 0.0073 or less, and may be 0.0071 or less, 0.0069 or less, 0.0068 or less, 0.0067 or less, 0.0066 or less, 0.0065 or less, 0.0064 or less, 0.0061 or less, or 0.0060 or less.
[0059] The lower limit of formula (2) is preferably 445 or more, more preferably 525 or more, even more preferably 630 or more, even more preferably 700 or more, particularly preferably 787 or more, and most preferably 788 or more, and may be 840 or more, 1050 or more, 1225 or more, 1260 or more, 1261 or more, 1313 or more, 1378 or more, 1379 or more, 1400 or more, 1401 or more, 1470 or more, 1471 or more, or 1488 or more. The upper limit of formula (2) is preferably 3560 or less, more preferably 3501 or less, even more preferably 3151 or less, even more preferably 2801 or less, particularly preferably 2679 or less, and most preferably 2678 or less, and may be 2626 or less, 2450 or less, 2451 or less, 2363 or less, 2143 or less, 2142 or less, 2101 or less, 2100 or less, 1970 or less, 1969 or less, 1891 or less, 1890 or less, 1838 or less, 1786 or less, 1785 or less, 1751 or less, 1750 or less, 1681 or less, 1680 or less, 1576 or less, or 1575 or less.
[0060] In the examples described below, the evaluation result of "◎" indicates that the result is particularly preferable in practical use compared to "◯". Since "◯" is a more preferable result than the conventional example, if other evaluation results are also excellent, the result falls within the scope of the present invention and is treated as an example. Since "×" is an insufficient result in the present invention, the result falls outside the scope of the present invention and is treated as a comparative example.
[0061] The heat cycle resistance in the present invention takes into consideration the variation in each sample after the heat cycle test, and the smaller the deviation from the average value, the higher the evaluation. Therefore, the meaning is significantly different from the evaluation of heat cycle resistance that has been conventionally considered, which is simply a comparison of average values.
[0062] 2. Solder paste The solder paste according to the present invention is a mixture of solder powder having the above-mentioned alloy composition and flux. The flux used in the present invention is not particularly limited as long as it allows soldering by a normal method. Therefore, a suitable mixture of commonly used rosin, organic acid, activator, thixotropic agent, and solvent may be used. The blending ratio of the metal powder component and the flux component in the present invention is not particularly limited, but is preferably 70 to 90 mass % of the metal powder component and 10 to 30 mass % of the flux component.
[0063] 3. Solder balls The solder alloy according to the present invention can be used as a solder ball. When used as a solder ball, the solder alloy according to the present invention can be manufactured into a solder ball by a dropping method, which is a common method in the industry. Also, a solder joint can be manufactured by processing the solder ball by a common method in the industry, such as mounting one solder ball on one electrode coated with flux and joining the solder ball. The particle size of the solder ball is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 20 μm or more, and particularly preferably 30 μm or more. The upper limit of the particle size of the solder ball is preferably 3000 μm or less, more preferably 1000 μm or less, even more preferably 800 μm or less, and particularly preferably 600 μm or less.
[0064] 4. Solder preform The solder alloy according to the present invention can be used as a preform, which may be in the form of a washer, ring, pellet, disk, ribbon, wire, or the like.
[0065] 5. Solder joints The solder joint according to the present invention is suitable for use in joining at least two or more members to be joined. The members to be joined are not particularly limited as long as they are electrically connected using the solder alloy according to the present invention, and include, for example, elements, substrates, electronic components, printed circuit boards, insulating substrates, heat sinks, lead frames, semiconductors using electrode terminals, power modules, inverter products, and the like.
[0066] The bonding method using the solder alloy according to the present invention may be performed according to a conventional method, for example, using a reflow method. The melting temperature of the solder alloy when performing reflow soldering may be a temperature approximately 20°C higher than the liquidus temperature. Furthermore, when bonding using the solder alloy according to the present invention, the alloy structure can be made finer by taking into consideration the cooling rate during solidification. For example, the solder joint is cooled at a cooling rate of 2 to 3°C / s or more. Other bonding conditions can be appropriately adjusted depending on the alloy composition of the solder alloy.
[0067] 6. In-vehicle electronic circuit, ECU electronic circuit, in-vehicle electronic circuit device, ECU electronic circuit device As is clear from the above description, the solder alloy according to the present invention has a suppressed increase in melting point, excellent shear strength, an appropriate fracture mode, and excellent heat cycle resistance. Therefore, even when used for automobiles exposed to harsh environments, that is, for in-vehicle use, the fracture of the solder joint is suppressed without variation. Therefore, since the solder alloy according to the present invention has such particularly remarkable properties, it is found to be particularly suitable for soldering electronic circuits mounted on automobiles.
[0068] In this specification, "excellent heat cycle resistance" means that, as shown in the examples described below, a heat cycle test is performed in which the temperature is held at -40°C and +125°C for 10 minutes each, and the standard deviation of the number of cycles until the electrical resistance of the solder joint increases by 20% from before the heat cycle test is 1000 or less. Such characteristics mean that even when used under extremely harsh conditions such as the heat cycle test, the possibility of breakage of the on-board electronic circuit is reduced to a minimum, and no unusable or malfunction occurs.
[0069] Thus, the solder alloy according to the present invention is used, more particularly, for soldering in-vehicle electronic circuits or for soldering ECU electronic circuits, and exhibits excellent heat cycle resistance.
[0070] An "electronic circuit" is a system that performs a desired function as a whole through the electronic engineering combination of multiple electronic components, each of which has its own function.
[0071] Examples of electronic components that make up such electronic circuits include chip resistor components, multiple resistor components, QFP, QFN, power transistors, diodes, capacitors, etc. Electronic circuits incorporating these electronic components are mounted on a substrate to form an electronic circuit device.
[0072] In the present invention, the substrate constituting such an electronic circuit device, for example, a printed wiring board, is not particularly limited. The material is also not particularly limited, but a heat-resistant plastic substrate (e.g., FR-4 with high Tg and low CTE) is an example. The printed wiring board is preferably a printed circuit board in which the surface of the Cu land is treated with an organic substance (OSP: Organic Surface Protection) such as amine or imidazole.
[0073] 7. Other The solder alloy according to the present invention can be manufactured by using a low alpha radiation material as its raw material, and when such a low alpha radiation alloy is used to form solder bumps around a memory, it is possible to suppress soft errors. EXAMPLES
[0074] The present invention will be described with reference to the following examples, but the present invention is not limited to the following examples. In order to verify the effects of the present invention, (1) melting point, (2) shear strength, (3) fracture mode, and (4) thermal cycle test (TCT) were evaluated using the solder alloys shown in Table 1. As for (4), Example 4 and Comparative Example 19 were selected from the following Examples and Comparative Examples, and their evaluation results are shown.
[0075] (1) Melting point For the solder alloys shown in Tables 1 and 2, the respective temperatures were obtained from the DSC curves. The DSC curves were obtained by raising the temperature at 5°C / min in air using a Seiko Instruments DSC (model number: 6200). The liquidus temperature was obtained from the obtained DSC curve and was taken as the melting point. If the melting point is 232°C or lower, reflow soldering can be performed at approximately the same temperature as conventional. If the melting point is above 232°C, conventional reflow soldering cannot be performed due to the high melting point.
[0076] (2) Share strength (2-1) Preparation of samples The solder alloys shown in Tables 1 and 2 were cast to prepare solder sheets (diameter: 1 mm, thickness: 0.15 mm). A reflow furnace (SNR-615: manufactured by Senju Metal Industry Co., Ltd.) was used to solder chip resistors to the Cu-OSP electrodes of the FR-4 board. The chip resistors used were 3216CR (CR32-114JV: manufactured by Hokuriku Electric Industry Co., Ltd.). The reflow profile was to hold 220°C or higher for 40 seconds in a nitrogen atmosphere, with a peak temperature of 245°C. (2-2) Evaluation of share strength The shear strength of the samples thus prepared was measured using a shear tester (STR-1000: manufactured by RHESCA) at a shear speed of 6 mm / min. If the shear strength was 84.0 N or more, it was evaluated as "◎". If the shear strength was 70.0 N or more but less than 84.0 N, it was evaluated as "◯". If the shear strength was less than 70.0 N, it was evaluated as "×".
[0077] (3) Destruction mode The fracture mode of the samples evaluated in "(2) Shear strength" above was observed using an optical microscope (VHX-5000: manufactured by KEYENCE). If the sample fractured in the bulk, it was rated as "◎". If the sample fractured in the bulk and in the intermetallic compound (IMC) at the bonding interface, it was rated as "〇". If the sample fractured in the intermetallic compound, it was rated as "×".
[0078] (4) Thermal cycle test (TCT) Example 4 was selected from Table 1, and Comparative Example 19 was selected from Table 2. Each solder alloy was atomized to prepare solder powder. The solder paste was prepared by mixing with a soldering flux ("GLV" manufactured by Senju Metal Industry Co., Ltd.) consisting of rosin, solvent, activator, thixotropic agent, organic acid, etc. The alloy powder of the solder paste was 88 mass % and the flux was 12 mass %. The solder paste was printed on a 0.8 mm thick printed circuit board (material: FR-4) with a metal mask having a thickness of 100 μm, and then a 12 mm×12 mm LGA (Land Grid Array) component was mounted with a mounter and reflow soldered with the same reflow profile as in "(2)(2-1)" above to prepare samples. 15 samples were prepared for Example 4, and 14 samples were prepared for Comparative Example 18.
[0079] The prepared samples were placed in a heat cycle tester (TSA-101L-A: manufactured by Espec Corp.) set to low temperature -40℃, high temperature +125℃, and a holding time of 10 minutes, and the resistance value was measured during the test. Breakage was considered to have occurred when the resistance value increased by 20% from the initial resistance value, and the average number of cycles at which breakage occurred and the standard deviation were calculated. When the standard deviation was 1000 or less, it was evaluated that the variation was not a problem in practical use. On the other hand, when the standard deviation was more than 1000, it was evaluated that the variation was not practical because there were samples that were far from the average value. The evaluation results of (1) to (3) above are shown in Tables 1 and 2. The evaluation result of (4) is shown in Table 3.
[0080] [Table 1]
[0081] [Table 2]
[0082] [Table 3]
[0083] As shown in Tables 1 and 2, in Examples 1 to 62, the contents of each constituent element were appropriate, and all evaluations were acceptable for practical use. In addition, it was found that Examples 1 to 8, 10 to 17, 19 to 24, 27 to 31, 38, 39, 42, 43, and 46 to 62, which satisfy the formulas (1) and (2), showed extremely excellent results in all evaluations. These were excellent results with a significant difference among the results acceptable for practical use.
[0084] On the other hand, as shown in Table 2, Comparative Example 1 did not contain In, Sb, Fe, and Co, and therefore had poor shear strength and an inappropriate fracture mode. Comparative Example 2 had poor shear strength because of the low Ag content. Comparative Examples 3 and 4 had poor shear strength and an inappropriate fracture mode because of the high Ag content.
[0085] In Comparative Examples 5 and 6, the Cu content was low, so the shear strength was poor. In particular, in Comparative Example 6, the fracture mode was inappropriate because of the Ni content. In Comparative Example 7, the Cu content was high, so the shear strength was poor and the fracture mode was inappropriate.
[0086] In Comparative Examples 8 and 9, the In content was not appropriate, so the shear strength was poor and the fracture mode was inappropriate. In Comparative Example 10, the Sb content was low, so the shear strength was poor. In Comparative Example 11, the Sb content was high, so the shear strength was poor and the fracture mode was inappropriate.
[0087] Comparative Examples 12 to 14 had poor shear strength due to the low Fe content, and Comparative Example 15 had poor shear strength and an inappropriate fracture mode due to the high Fe content.
[0088] Comparative Example 16 had poor shear strength due to a low Co content, and Comparative Example 17 had poor shear strength and an inappropriate fracture mode due to a high Co content.
[0089] Comparative Examples 18 and 20 contained Ni or Mn, respectively, and therefore the melting point was significantly increased, the shear strength was poor, and the fracture mode was inappropriate. Comparative Example 19 contained Bi, and therefore the shear strength was poor.
[0090] Also, as is clear from Table 3, the difference in the average number of cycles between Example 4 and Comparative Example 19 was about 300 cycles. However, the standard deviation of the number of cycles in Example 4 was less than 1000, whereas the standard deviation of the number of cycles in Comparative Example 19 was significantly more than 1000.
[0091] Therefore, in Example 4, there were only samples with small variations in the heat cycle test and small differences from the average value. It was found that similar results were shown in other Examples. On the other hand, in Comparative Example 19, it was found that there were samples with large variations in the heat cycle test and extremely large differences from the average value.
[0092] FIG. 1 shows optical microscope photographs of samples after measuring the shear strength, where FIG. 1(a) is Example 4, FIG. 1(b) is Comparative Example 19, and FIG. 1(c) is Comparative Example 3. As is clear from FIG. 1, it was found that in Example 4, the solder joint broke due to bulk fracture. On the other hand, in Comparative Example 19, it was found that the solder joint broke due to fracture in the intermetallic compound at the bonding interface as well as bulk fracture. Furthermore, it was found that in Comparative Example 3, the solder joint broke at the intermetallic compound at the bonding interface. Therefore, it was found that the fracture mode was appropriate in this Example 4. This result was similar in the other Examples. [Industrial Applicability]
[0093] The solder according to the present invention can be used in on-board electronic circuits such as ECUs, which are electronic circuits that control automobiles using computers to improve fuel efficiency, but it can also be used in consumer electronic devices such as personal computers with excellent effect.
Claims
1. A solder alloy having an alloy composition, in mass%, of 2.0 to 3.6% Ag, 0.6 to 0.9% Cu, 1.0 to 5.0% In, 3.0 to 5.0% Sb, 0.0010 to 0.0300% Fe, 0.0010 to 0.0500% Co, and the balance being Sn, wherein the alloy composition satisfies the following formulas (1) and (2): 0.0020≦Ag×Cu×In×Sb×Fe×Co≦0.0090 (1) 445≦In / (Ag×Cu×Sb×Fe×Co)≦3560 (2) In the above formulas (1) and (2), Ag, Cu, In, Sb, Fe, and Co are each the content in mass % of the solder alloy.
2. 2. The solder alloy according to claim 1, wherein the alloy composition further contains, in mass%, 0.1% or less in total of at least one of Zr, Ge, Ga, P, As, Pb, Zn, Mg, Cr, Ti, Mo, Pt, Pd, Au, Al, and Si.
3. A solder paste comprising a solder powder made of the solder alloy according to claim 1 or 2.
4. A solder ball made of the solder alloy according to claim 1 or 2.
5. A solder preform comprising the solder alloy according to claim 1 or 2.
6. A solder joint comprising the solder alloy according to claim 1 or 2.
7. An in-vehicle electronic circuit comprising the solder alloy according to claim 1 or 2.
8. 3. An ECU electronic circuit comprising the solder alloy according to claim 1 or 2.
9. An on-vehicle electronic circuit device comprising the on-vehicle electronic circuit according to claim 7.
10. An ECU electronic circuit device comprising the ECU electronic circuit according to claim 8.
Citation Information
Patent Citations
Intermixing type atomizer
JP1988049615A
Method and device for fitting o-ring
JP1989020936A
Solder paste for joining micro component
JP2013252548A
Solder alloy, solder junction material, and electronic circuit substrate
JP2019063830A
JPP7376842B