Piston for internal combustion engine and manufacturing method thereof
A softened anodized film on the piston ring groove, achieved through lithium-ion sealed pores, addresses unevenness issues, improving sealing and reducing emissions in internal combustion engines.
Patent Information
- Application Number
- JP2020184383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-04
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-11-04
AI Technical Summary
The anodized film on the inner surface of the piston ring groove of an aluminum alloy piston for internal combustion engines is uneven due to silicon crystallization, leading to gaps and reduced sealing performance, which increases blow-by gas flow and oil leakage, affecting fuel efficiency and compliance with environmental regulations.
Forming a softened anodized film on the inner surface of the piston ring groove using a sealing solution containing lithium ions to seal pores and reduce the Vickers hardness to less than 320, ensuring even adhesion with the piston ring.
The softened anodized film improves sealing performance, reducing blow-by gas flow and oil leakage, enhancing fuel efficiency, and meeting environmental regulations by minimizing PM and PN emissions.
Smart Images

Figure 0007578902000001 
Figure 0007578902000002 
Figure 0007578902000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a piston for an internal combustion engine and a manufacturing method thereof, and more particularly to a piston for an internal combustion engine having an anodized coating on the inner surface of a piston ring groove and a manufacturing method thereof. [Background technology]
[0002] In recent years, the internal combustion engines of automobiles have become more powerful, and the thermal load of the pistons tends to increase. Piston rings are attached to the outer circumferential surface of the pistons to maintain the airtightness of the combustion chamber. The piston rings are fitted into ring grooves formed on the outer circumferential surface of the pistons. The inner surface of the ring groove is easily worn by being struck by the piston ring, and the sealing performance is easily impaired. Therefore, in order to improve the wear resistance of the inner surface of the ring groove, the inner surface of the ring groove is subjected to anodizing treatment.
[0003] However, aluminum alloys used as piston materials contain silicon to improve castability and wear resistance, and the silicon crystallizes into the metal structure. Since silicon is partially exposed on the inner surface of the ring groove, the anodized film that is formed by oxidizing aluminum during anodizing is partially inhibited, resulting in an uneven film with an uneven surface. With such an anodized film, gaps are formed between the piston ring and the piston, which reduces the sealing performance and increases the flow rate of blow-by gas and oil leakage, which leads to poor fuel economy and causes the generation of substances subject to European environmental regulations such as PM (Particulate Matter) and an increase in the number of PN (Particle Number).
[0004] On the other hand, Patent Document 1 describes a method for improving the corrosion resistance of an anodized film formed on the surface of an aluminum alloy and capable of treating the surface of the anodized film formed on the surface of the aluminum alloy in a short time by sealing the surface of the anodized film with a sealing treatment solution containing 0.02 to 20 g / L of lithium ions, having a pH value of 10.5 or higher, and having a temperature of 65° C. or lower. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-77532 A Summary of the Invention [Problem to be solved by the invention]
[0006] It is difficult to mechanically smooth the surface of the anodized film formed on the inner surface of the piston ring groove of an aluminum alloy piston for an internal combustion engine by post-processing, because the width of the piston ring groove is only a few millimeters.
[0007] In view of the above problems, the present invention aims to provide a piston for an internal combustion engine having an anodized coating on the inner surface of a piston ring groove, which can improve wear resistance and also provide good adhesion to the piston ring, and a manufacturing method thereof. [Means for solving the problem]
[0008] In order to achieve the above-mentioned object, one aspect of the present invention is a method for manufacturing a piston for an internal combustion engine, the method comprising the steps of: forming an anodized film on an inner surface of a piston ring groove of an aluminum alloy piston for an internal combustion engine; and sealing the anodized film with a sealing solution containing lithium ions, so that the Vickers hardness HV of the surface of the anodized film after the sealing treatment is less than 320.
[0009] In another aspect, the present invention provides a piston for an internal combustion engine having a piston ring groove on its outer peripheral surface, the piston for an internal combustion engine having an anodized coating on an inner surface of the piston ring groove, pores in a surface portion of the anodized coating are blocked, compounds of lithium, aluminum, and oxygen are present in the surface portion where the pores are blocked, and the Vickers hardness HV of the surface of the anodized coating is less than 320. Effect of the Invention
[0010] Thus, according to the present invention, an anodized film formed on the inner surface of a piston ring groove of an aluminum alloy internal combustion engine piston is sealed with a sealing solution containing lithium ions, and the Vickers hardness HV of the surface of the anodized film after sealing is made less than 320. Even if the surface of the anodized film after sealing is uneven and non-uniform, the unevenness is smoothed out by the vertical pressure of the piston ring at engine start, and adhesion to the piston ring is improved. Thus, the improved sealing of the piston ring groove of the internal combustion engine piston can reduce the flow rate of blow-by gas and suppress oil rising, thereby contributing to improved fuel efficiency and compliance with environmental regulations on PM and PN. [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional view showing an embodiment of a piston for an internal combustion engine according to the present invention, which is a schematic view of the periphery of a first piston ring groove. [Diagram 2] 2 is a cross-sectional view that typically shows the periphery of a lower surface of a first piston ring groove of the piston for the internal combustion engine shown in FIG. 1. [Diagram 3] 1 is a graph showing the measurement results of the hardness of the anodized film in Test Example 1. [Figure 4] 1 is a graph showing the results of measuring the hardness of the anodized film in Test Example 2. [Diagram 5] 1 is a graph showing the results of measuring the hardness of the anodized film in Test Example 3. [Figure 6] 13 is a graph showing the results of measuring the hardness of the anodized film in Test Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of a piston for an internal combustion engine and a manufacturing method thereof according to the present invention will be described with reference to the accompanying drawings. Note that the drawings are drawn with priority given to ease of understanding and are not drawn to scale.
[0013] 1, a piston 10 for an internal combustion engine according to this embodiment has a first piston ring groove 13 formed in its outer circumferential surface 12. The piston ring grooves include three ring grooves, namely, a first piston ring groove 13, a second piston ring groove (not shown), and an oil ring groove (not shown), which are formed in this order from the piston crown surface 11 side. A first piston ring 30 is fitted into the first piston ring groove 13, a second piston ring (not shown) is fitted into the second piston ring groove, and an oil ring (not shown) is fitted into the oil ring groove.
[0014] The piston 10 for an internal combustion engine is made of an aluminum alloy. The aluminum alloy generally contains silicon (Si) as a component that contributes to wear resistance and aluminum adhesion resistance. Examples of such aluminum alloys include AC materials such as AC4, AC8, AC8A, and AC9, ADC materials such as ADC10 to ADC14, and A4000 for pistons. On the other hand, rings such as the first piston ring 30 are made of, for example, high carbon steel or martensitic stainless steel. Rings such as the first piston ring 30 have a substantially C-shape with one circumferential opening, and are inserted into a ring groove such as the first piston ring groove 13 of the piston 10 in an elastically expanded state, and then contract in diameter due to elastic restoring force to be fitted inside the ring groove.
[0015] The outer peripheral surface 33 of the first piston ring 30 protrudes outward from the outer peripheral surface 12 of the piston 10 for an internal combustion engine. In the outer peripheral surface 12 of the piston 10, a portion between the piston crown surface 11 and the first piston ring groove 13 is called a first land 12a, a portion between the first piston ring groove 13 and a second piston ring groove (not shown) is called a second land 12b, and a portion between the second piston ring groove and an oil ring groove (not shown) is called a third land (not shown). Since the outer peripheral surfaces of the rings such as the first piston ring 30 protrude outward from the outer peripheral surface 12 of the piston 10 for an internal combustion engine, when the piston 10 for an internal combustion engine equipped with the rings such as the first piston ring 30 is inserted into the cylinder 40, the rings such as the first piston ring 30 are inserted into the cylinder 40 in a state in which they are elastically contracted in diameter. Therefore, when the internal combustion engine piston 10 is inserted into the cylinder 40, each ring, such as the first piston ring 30, is pressed against the inner wall surface 41 of the cylinder 40 by its elastic force, and the first piston ring 30 and the second ring function to maintain the airtightness of the combustion chamber, and the oil ring functions to scrape off any oil remaining on the inner wall surface 41 of the cylinder 40.
[0016] Of the inner surfaces of the first piston ring groove 13 formed in the outer peripheral surface 12 of the piston 10 for an internal combustion engine, the inner surface on the piston crown surface 11 side is called the upper surface 13a, the inner surface on the second ring groove (not shown) side is called the lower surface 13c, and the inner surface on the bottom side of the groove between them is called the side surface 13b. In this embodiment, an anodized film 20 (hereinafter referred to as a "soft anodized film") whose hardness has been reduced by the sealing treatment according to the present invention is formed on the upper surface 13a, the side surface 13b, and the lower surface 13c of the first piston ring groove 13. Note that the soft anodized film 20 may be provided only on the lower surface 13c of the inner surface of the first piston ring groove 13.
[0017] The soft anodized coating 20 is formed on the lower surface 13c of the first piston ring groove 13 in this manner because, as shown in FIG. 1, the internal combustion engine piston 10 has a high pressure in the combustion chamber on the piston crown surface 11 side during the compression stroke and expansion stroke, and the lower surface 32 of the first piston ring 30 tightly adheres to the lower surface 13c of the first piston ring groove 13. On the other hand, although not shown, the internal combustion engine piston 10 has an upper surface 31 of the first piston ring 30 tightly adheres to the upper surface 13a of the first piston ring groove 13 during the intake stroke, and the internal combustion engine piston 10 moves between the upper surface 13a and the lower surface 13c of the first piston ring groove 13 each time these strokes are repeated. Therefore, the lower surface 13c of the first piston ring groove 13 is prone to wear between the first piston ring 30, and therefore it is necessary to form the soft anodized coating 20 in order to improve wear resistance and sealing properties.
[0018] Of course, the soft anodized film 20 may also be formed on the upper surface 13a of the first piston ring groove 13. In addition, the first piston ring 30 is also in close contact with the cylinder 40 due to its tension, and therefore does not come into contact with the side surface 13b of the first piston ring groove 13. Therefore, it is not essential to form the soft anodized film 20 on the side surface 13b of the first piston ring groove 13, but of course the soft anodized film 20 may be formed on the side surface 13b of the first piston ring groove 13.
[0019] As shown in FIG. 2, the soft anodized film 20 of this embodiment has a structure including a porous portion 21 of the anodized film produced by anodizing the aluminum alloy 15 on the underside 13c of the first piston ring groove 13, and a sealing treatment portion 22 in which the pores on the surface portion of the anodized film are sealed by sealing the anodized film with a sealing treatment liquid containing lithium ions.
[0020] The anodic oxide film formed by anodizing usually grows in a direction perpendicular to the surface of the aluminum alloy 15 that is the target of the anodizing, and therefore the growth of the anodic oxide film is hindered in areas where silicon 16 or the like is crystallized on the surface layer of the aluminum alloy 15, resulting in numerous irregularities on the surface. The irregularities on the surface of the anodic oxide film cannot be smoothed out by a sealing treatment. The present invention is based on the new finding that the surface hardness of the anodic oxide film can be softened while maintaining the excellent wear resistance of the anodic oxide film by performing a sealing treatment with a sealing treatment solution containing lithium ions.
[0021] The sealing treatment 22, in which the pores in the surface portion of the anodized coating are sealed by the sealing treatment, is less hard than the anodized coating, and has excellent initial compatibility with the piston ring 30. That is, even if the surface of the softened anodized coating 20 after the sealing treatment is uneven and irregular, the unevenness is smoothed out by the vertical pressure of the piston ring 30 when the engine is started, and the surface becomes smooth as shown in FIG. 2. This improves the adhesion between the lower surface 13c of the piston ring groove and the piston ring 30, reducing the flow rate of blow-by gas and improving fuel efficiency. In addition, the sealing performance is improved, and oil leakage can be suppressed, thereby suppressing PM and PN within the required values.
[0022] If the hardness of the sealing treatment portion 22, i.e., the surface hardness of the soft anodized coating 20, is less than 320 in Vickers hardness HV, the surface irregularities can be smoothed to an extent that the adhesion with the piston ring is good due to the vertical pressure of the piston ring 30 at the time of starting the engine. The preferred surface hardness of the soft anodized coating 20 is preferably 130 or more and less than 320, more preferably 150 or more and less than 320, in Vickers hardness HV. The lower limit of the surface hardness of the soft anodized coating 20 is preferably 130 or more, which is the hardness of an aluminum alloy, in Vickers hardness HV. If it is less than 130, it may affect the wear resistance, which is the purpose of forming the anodized coating.
[0023] A method for manufacturing an internal combustion engine piston having such a soft anodized coating includes an anodized coating formed on the inner surface of a piston ring groove of an aluminum alloy internal combustion engine piston, and then a sealing treatment step of sealing the anodized coating with a sealing solution containing lithium ions. Each step is described below.
[0024] In the anodizing process, a conventional anodizing treatment capable of forming an anodized film on the surface of an aluminum alloy can be widely adopted. For example, an electrode plate such as titanium or carbon as a cathode and an internal combustion engine piston as an anode are immersed in an acidic treatment bath such as sulfuric acid, oxalic acid, phosphoric acid, or chromic acid, or a basic treatment bath such as sodium hydroxide, sodium phosphate, or sodium fluoride, and electrolysis is performed to oxidize the aluminum alloy on the inner surface of the piston ring groove of the internal combustion engine piston, thereby forming an anodized film. Any of direct current electrolysis, alternating current electrolysis, and alternating current / direct current superimposed electrolysis may be used as the electrolysis method. The anodized film to be the target of the sealing treatment of the present invention is not limited to a specific anodizing treatment.
[0025] The thickness of the anodized film formed in the anodizing treatment step is not particularly limited, but is preferably, for example, 5 to 20 μm, and more preferably 5 to 10 μm.
[0026] In the sealing process, a sealing solution containing lithium ions is applied or sprayed onto an internal combustion engine piston having an anodized film formed thereon, or the piston is immersed in the sealing solution to seal the pores in the surface of the anodized film. More specifically, the surface of the anodized film is dissolved by the sealing solution, and then re-precipitated to form a sealing treatment portion in which the pores are sealed on the surface of the anodized film. In addition to aluminum oxide, this sealing treatment portion contains compounds of lithium, aluminum, and oxygen. This sealing treatment portion will not decompose and lose its sealing state even in the high-temperature environment to which the internal combustion engine piston is exposed.
[0027] The sealing treatment liquid is an aqueous solution containing lithium ions, and the compounds that can be used as the lithium ion source include lithium sulfate, lithium chloride, lithium silicate, lithium nitrate, lithium carbonate, lithium phosphate, and lithium hydroxide. Among these, lithium hydroxide, lithium carbonate, and lithium silicate are preferred because their aqueous solutions are basic. However, lithium silicate is highly toxic and difficult to dissolve in water, making it impractical. Therefore, lithium carbonate and lithium hydroxide are more preferred.
[0028] The lithium ion concentration of the sealing solution is preferably 1 to 15 g / L, more preferably 1 to 12 g / L. With a lithium ion concentration of 1 g / L or more, the sealing reaction is promoted, and a sealing treatment part with sufficiently reduced hardness can be obtained. The upper limit of the lithium ion concentration is not particularly limited, but it is preferably 15 g / L or less. If the lithium ion concentration exceeds 15 g / L, the reaction proceeds too rapidly, which is not preferable.
[0029] The temperature of the sealing solution is preferably 10 to 70° C., more preferably 10 to 60° C. When the sealing treatment is performed at a high temperature of 10° C. or more, the activity and reactivity are high, and a sealing treatment part with sufficiently reduced hardness can be obtained even in a short time. On the other hand, a temperature exceeding 70° C. is not preferable because dissolution of the film from the surface of the anodized film proceeds rapidly.
[0030] The treatment time for the sealing treatment is preferably 0.5 to 4 minutes, and more preferably 0.5 to 2 minutes. By setting the treatment time to 0.5 minutes or more, the surface of the anodized film is dissolved, and the sealing treatment part with sufficiently reduced hardness can be re-precipitated. On the other hand, a treatment time of more than 4 minutes is not preferable because the film dissolves rapidly from the surface of the anodized film.
[0031] In the sealing treatment step, it is preferable to perform the sealing treatment with a sealing treatment solution, followed by rinsing with water and drying.
[0032] Although the soft anodized film 20 is formed on the first piston ring groove 13, the present invention is not limited to the first piston ring groove 13, and the soft anodized film 20 may be formed on other piston ring grooves such as the second piston ring groove. By improving the adhesion with the piston ring, the flow rate of blow-by gas and oil rising can be reduced, which contributes to improving fuel efficiency and complying with environmental regulations. In addition, by improving the wear resistance, it is possible to maintain good sealing with the piston ring. Furthermore, by forming the soft anodized film 20 on the first piston ring groove 13 among the piston ring grooves, fuel efficiency is improved by suppressing heat escape below the first piston ring groove 13. This can also be said to reduce cooling loss. EXAMPLES
[0033] Examples and comparative examples of the present invention will be described below.
[0034] [Test Example 1] A test piece of aluminum material A1050 simulating an aluminum alloy piston for an internal combustion engine was subjected to an anodizing treatment in a sulfuric acid bath (electrolysis conditions: 0.5 A, 10 min) to form an anodized film of about 20 μm on the surface. The test piece was immersed in a sealing treatment liquid with a lithium ion concentration of 10 g / L to perform a sealing treatment of the anodized film. The temperature of the sealing treatment liquid was 30° C., and the treatment time was 1 minute. The hardness of the anodized film after the sealing treatment was measured with a dynamic ultra-microhardness tester DUH-211 manufactured by Shimadzu Corporation. The measurement condition was a load of 100 mN. The hardness was evaluated by Vickers hardness HV. The hardness of the anodized film after the sealing treatment of five test pieces was measured, and the average value is shown in FIG. 3 (Example). As a comparative example, the hardness of the anodized film before the sealing treatment was also measured in the same manner as above. The result is shown in FIG. 3.
[0035] 3, the hardness of the anodized film that was not subjected to a sealing treatment (Comparative Example) was 320 in Vickers hardness HV, whereas the hardness of the anodized film that was subjected to a sealing treatment (Example) was significantly reduced to a Vickers hardness HV of 270. By softening the hardness of the anodized film to a significantly low value of 270 in Vickers hardness HV in this way, even if the surface of the anodized film is uneven, the unevenness can be leveled and smoothed by the vertical pressure of the piston ring when the engine is started.
[0036] [Test Example 2] Except for changing the lithium ion concentration of the sealing solution from 10 g / L to 1, 20, and 30 g / L, the test pieces were subjected to anodizing and sealing in the same manner as in Test Example 1, and the hardness of the anodized film after sealing was measured. The results are shown in Figure 4.
[0037] As shown in Fig. 4, the hardness of the anodized film (Example) after the sealing treatment was significantly lowered than that of the anodized film (Comparative Example) without the sealing treatment, regardless of the lithium ion concentration of the sealing solution. In particular, when the lithium ion concentration was 1 g / L and 10 g / L, the hardness of the anodized film after the sealing treatment was only reduced to about 200 in Vickers hardness HV, but when the lithium ion concentration was 20 g / L and 30 g / L, the hardness of the anodized film after the sealing treatment was reduced to 100 or less in Vickers hardness HV. Therefore, since the lower limit of the preferred range of Vickers hardness HV, 130, is between the lithium ion concentration of 10 to 20 g / L, it can be seen that the preferred range of lithium ion concentration is 1 to 15 g / L, and the more preferred range of lithium ion concentration is 1 to 12 g / L.
[0038] [Test Example 3] The test pieces were subjected to anodizing and sealing treatment in the same manner as in Test Example 1, except that the temperature of the sealing solution was changed from 30° C. to 10, 50, and 70° C., and the hardness of the anodized film after sealing treatment was measured. The results are shown in FIG.
[0039] 5, the hardness of the anodized film after sealing treatment (Example) could be significantly reduced compared to the hardness of the anodized film that was not sealed (Comparative Example) regardless of the temperature of the sealing treatment solution. Therefore, it is clear that the treatment temperature is preferably 10 to 70°C, and more preferably 10 to 60°C.
[0040] [Test Example 4] The test pieces were anodized and sealed in the same manner as in Test Example 1, except that the sealing treatment time was changed from 1 minute to 0.5, 5, and 10 minutes, and the hardness of the anodized film after sealing was measured. The results are shown in Figure 6.
[0041] As shown in Fig. 6, regardless of the treatment time of the sealing treatment, the hardness of the anodized film after the sealing treatment (Example) was significantly lower than the hardness of the anodized film without the sealing treatment (Comparative Example). In particular, when the treatment time was 1 minute, the hardness of the anodized film after the sealing treatment only decreased to about 180 in Vickers hardness HV, but when the treatment time was 4 minutes or more, the hardness of the anodized film after the sealing treatment decreased to 100 or less in Vickers hardness HV. Therefore, it is found that the treatment time of the sealing treatment is preferably 0.5 to 4 minutes, and more preferably 0.5 to 2 minutes. [Explanation of symbols]
[0042] 10. Pistons for internal combustion engines 11 Piston crown surface 12a Land 1 12b 2nd Land 13 No. 1 piston ring groove 13c Bottom surface of first piston ring groove 15 Aluminum alloy 16 Silicon 20 Anodized film after sealing treatment (softened anodized film) 21 Porous part 22 Sealing treatment section 30 Top Ring 40 Cylinder
Claims
1. forming an anodized coating on an inner surface of a piston ring groove of an aluminum alloy piston for an internal combustion engine; a step of sealing the anodized film with a sealing solution containing lithium ions, thereby manufacturing a piston for an internal combustion engine having a surface of the anodized film after the sealing treatment with a Vickers hardness of HV of 130 to 270; A method for manufacturing a piston for an internal combustion engine, comprising:
2. 2. The method for manufacturing a piston for an internal combustion engine according to claim 1, wherein the sealing treatment solution has a lithium ion concentration in the range of 1 to 15 g / L, and the sealing treatment solution has a temperature in the range of 10 to 70° C.
3. 2. The method for manufacturing a piston for an internal combustion engine according to claim 1, wherein the sealing treatment solution has a lithium ion concentration in the range of 1 to 12 g / L, and the sealing treatment solution has a temperature in the range of 10 to 70° C.
4. The method for manufacturing a piston for an internal combustion engine according to any one of claims 1 to 3, wherein the treatment time for the sealing treatment is in the range of 0.5 to 4 minutes.
5. The method for manufacturing a piston for an internal combustion engine according to any one of claims 1 to 3, wherein the treatment time for the sealing treatment is in the range of 0.5 to 2 minutes.
6. A piston for an internal combustion engine having a piston ring groove on an outer peripheral surface, The piston ring groove has an inner surface provided with an anodized coating, The piston for an internal combustion engine has pores in a surface portion of the anodized film that are sealed, and a compound of lithium, aluminum, and oxygen is present in a sealing treatment portion that seals the pores, and the Vickers hardness HV of the surface of the anodized film is 130 to 270.
Citation Information
Patent Citations
Anodic oxide film and methods for manufacturing same
CN103938250A
Member made of al alloy and its manufacture
JP1993017899A
Piston for internal combustion engine and manufacture thereof
JP1997159022A
Sealing method for anodic oxide film
JP2010077532A
Sealing treatment method for anodic oxide film
JP2012246512A