Piston for internal combustion engine and manufacturing method thereof

By eluting copper from the top ring groove of aluminum alloy pistons and forming a heat-insulating anodic oxide film, the method addresses the heat insulation and smoothness issues, ensuring effective sealing and compliance with environmental regulations.

JP7578912B2Active Publication Date: 2024-11-07SUZUKI MOTOR CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021044604
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-18
Publication Date
2024-11-07
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

Conventional aluminum alloys used in internal combustion engine pistons with higher copper content for improved mechanical properties suffer from reduced heat insulation and impaired smoothness of the top ring groove, leading to poor sealing performance and increased oil upflow, which violates environmental regulations.

Method used

A method involving a mixed acid immersion treatment to elute copper from the top ring groove of an aluminum alloy piston, followed by anodization to form a heat-insulating anodic oxide film with reduced copper content, enhancing the heat insulation and smoothness of the groove.

Benefits of technology

The method improves heat insulation and maintains smoothness of the top ring groove, ensuring good sealing performance and compliance with environmental regulations by preventing oil upflow and reducing PM and PN emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578912000003
    Figure 0007578912000003
  • Figure 0007578912000004
    Figure 0007578912000004
  • Figure 0007578912000005
    Figure 0007578912000005
Patent Text Reader

Abstract

To provide a piston for an internal combustion engine which can improve the heat insulation performance of a top ring groove even if using an aluminum alloy largely containing Cu more than before as a raw material, and can maintain seal performance with a piston ring by maintaining the smoothness of an inner face of the top ring groove, and its manufacturing method.SOLUTION: A manufacturing method of a piston for an internal combustion engine according to this invention applies masking to a piston main body which is formed with an aluminum alloy containing 5.0 to 20.0% of Si, and Cu exceeding 1.3% and equal to or lower than 5.0% as a raw material 10 so that an inner face of a top ring groove is exposed. The piston main body is immersed into an acid-mixed aqueous solution, and after Cu in a region 27a is eluted up to a depth corresponding to more than half of a film thickness of a formation-scheduled anodic oxidation membrane from a surface, the anodic oxidation membrane is formed at the an inner face of the top ring groove. By this constitution, the piston for the internal combustion engine can be obtained having a heat insulation layer 27b having the content of Cu smaller than that of the raw material between the raw material 10 and the anodic oxidation membrane 20.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piston for an internal combustion engine and a manufacturing method thereof, and more particularly to a piston for an internal combustion engine having an anodized coating on the inner surface of a top ring groove and a manufacturing method thereof. [Background technology]

[0002] In recent years, in response to environmental regulations, there has been an increasing demand for higher efficiency and higher compression ratios in internal combustion engines such as automobile engines, as well as for supercharged engines, and the maximum combustion pressure of internal combustion engines is rising. In response to this background, the temperatures of the piston ring groove (particularly the top ring groove) and land portions (particularly the first and second lands) of pistons for internal combustion engines are becoming higher than those of conventional internal combustion engines of the same displacement. An anodized film is sometimes formed on the top ring groove of the piston to impart wear resistance. This is because the anodized film has a hardness more than twice that of the aluminum alloy, which is the base material of the piston, and has excellent wear resistance properties.

[0003] As such an anodized coating, for example, Patent Document 1 describes an anodized coating having a uniform thickness and density and high impact resistance for a piston whose base material is an aluminum alloy that has excellent corrosion resistance and a large amount of precipitation of impurities and / or additives (such as silicon (Si)). The anodized coating has a structure in which the cells of the anodized coating grow in random directions on the surface of the aluminum alloy and have no orientation, and the cells surround the impurities and / or additives to form spherical or elliptical shapes, and the cells gather together to form a bunch of grapes. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2006-83467 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, aluminum alloys with improved mechanical properties (fatigue strength, tensile strength, etc.) up to high temperatures, which are called high-strength materials and have been increasingly adopted in recent years, may contain more added elements such as copper (Cu) and nickel (Ni) than aluminum alloys such as the conventional JIS (Japanese Industrial Standards)-AC8A (Al-Si-Cu-Ni-Mg system) alloys. Copper in particular has a thermal conductivity 1.5 times higher than aluminum (Al), so if a piston is formed using such a high-strength aluminum alloy with a large amount of copper as the base material, there is a risk that the insulation properties will be reduced.

[0006] Heat generated in the combustion chamber of an internal combustion engine is transmitted through the gap between the piston and the cylinder bore, and further from the piston ring to the base material on the cylinder bore side and the base material on the top ring groove side. If the base material on the top ring groove side becomes too hot, it will soften and the smoothness of the top ring groove may be impaired. If the smoothness is impaired, the sealing performance between the piston ring and the top ring groove will decrease, causing the phenomenon of oil used for lubrication of the internal combustion engine flowing into the combustion chamber (oil rise), which may cause the oil to burn in the combustion chamber and lead to the generation of substances subject to European environmental regulations, such as particulate matter (PM), and an increase in the number of such substances, such as the particle number (PN).

[0007] In view of the above problems, the present invention has an object to provide a piston for an internal combustion engine, and a manufacturing method thereof, which can improve the heat insulation in the top ring groove and maintain the smoothness of the inner surface of the top ring groove to maintain good sealing performance with the piston ring, even when an aluminum alloy containing more Cu than conventional aluminum alloys is used as the base material. [Means for solving the problem]

[0008] In order to achieve the above object, one aspect of the present invention is a method for manufacturing a piston for an internal combustion engine, the method comprising the steps of: a masking step of masking an internal combustion engine piston body formed from an aluminum alloy containing 5.0 to 20.0% by mass of Si and more than 1.3% by mass and not more than 5.0% by mass of Cu so as to expose at least an inner surface of a top ring groove; a mixed acid immersion step of immersing the masked piston body in an aqueous solution of mixed acid to elute Cu from a region of the exposed inner surface of the top ring groove from the surface to a depth equivalent to more than half the film thickness of an anodized film to be formed; and an anodizing step of forming an anodized film with the intended film thickness on the inner surface of the top ring groove of the piston body removed from the aqueous solution of mixed acid.

[0009] In another aspect, the present invention provides a piston for an internal combustion engine having a top ring groove, the piston comprising an aluminum alloy containing 5.0 to 20.0 mass% Si and more than 1.3 mass% but not more than 5.0 mass% Cu as a base material, a thermal insulation layer located on the inner surface of the top ring groove and made of an aluminum alloy composition having a lower Cu content than the base material, and an anodized coating located on the surface of the thermal insulation layer. Effect of the Invention

[0010] Thus, according to the present invention, even if the base material is an aluminum alloy containing more Cu than in the past, the anodized coating is formed in the top ring groove via a heat insulating layer made of an aluminum alloy composition with a lower Cu content than the base material, improving the heat insulation of the top ring groove to the base material. This prevents the base material in the top ring groove from softening, maintains its smoothness, and maintains good sealing performance with the piston ring. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing an embodiment of a piston for an internal combustion engine according to the present invention, which is a schematic view of the periphery of a top ring groove. FIG. [Diagram 2]FIG. 2 is an enlarged cross-sectional view illustrating a schematic view of the vicinity of an inner surface of a top ring groove in one embodiment of a piston for an internal combustion engine and a manufacturing method thereof according to the present invention. [Diagram 3] FIG. 1 is a flow chart showing an embodiment of a method for manufacturing a piston for an internal combustion engine according to the present invention. [Figure 4] FIG. 4 is a flow chart showing in more detail the mixed acid immersion treatment step in the method for producing a piston for an internal combustion engine shown in FIG. 3. [Diagram 5] 1 is a graph showing the relationship between the mixed acid immersion time and the surface roughness of a top ring groove in Example 1 and Comparative Example 1. [Figure 6] 6 is a photograph showing the surface of a top ring groove before and after immersion in mixed acid in Example 1. [Figure 7] 5 is a cross-sectional photograph showing the surface of a top ring groove before and after immersion in mixed acid in Comparative Example 1. [Figure 8] 3 is a photograph showing the surface of the anodized film of Example 2. [Figure 9] 3 is a photograph showing the surface of an anodized film of Comparative Example 2. [Figure 10] 1 is a cross-sectional photograph of a top ring groove on which an anodized film is formed in Example 2. [Figure 11] 1 is a cross-sectional photograph of a top ring groove on which an anodized film is formed in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of a piston for an internal combustion engine and a manufacturing method thereof according to the present invention will be described with reference to the accompanying drawings. Note that the drawings are drawn with priority given to ease of understanding and are not drawn to scale.

[0013] As shown in FIG. 1, the piston 1 for an internal combustion engine according to this embodiment is formed from a base material 10 which is an aluminum alloy with improved mechanical properties containing 5.0 to 20.0 mass % Si and more than 1.3 mass % but not more than 5.0 mass % Cu, and an anodized coating 20 is formed on the surface of the base material in the top ring groove 13 via a heat insulating layer (not shown).

[0014] In the aluminum alloy of the base material 10, Si is a component that crystallizes as primary crystal silicon or eutectic silicon and improves heat resistance and wear resistance. Si also reduces the thermal expansion coefficient. If the Si content is 5.0 mass% or more, the thermal expansion coefficient is low, and wear resistance and strength at high temperatures can be improved, and if it is 20.0 mass% or less, primary crystal silicon becomes small, and the elongation of the alloy can be improved. The Si content is more preferably 10.0 to 13.0 mass%.

[0015] Cu is a component that improves mechanical strength and wear resistance at room temperature and high temperatures. If the Cu content exceeds 1.3 mass%, the effect of improving strength and wear resistance can be exhibited, and if it is 5.0 mass% or less, there is no significant decrease in elongation of the alloy and the specific gravity of the alloy is small. On the other hand, if it exceeds 5.0 mass%, the elongation is significantly decreased and the specific gravity of the alloy becomes large. The Cu content is more preferably 2.5 to 5.0 mass%.

[0016] In addition, three ring grooves are formed on the outer peripheral surface 12 of the piston 1, in order from the piston crown surface 11 side, as piston ring grooves, namely, a top ring groove (first ring groove) 13, a second ring groove (not shown), and an oil ring groove (not shown). A top ring (first ring) 30 is fitted into the top ring groove 13, a second ring (not shown) is fitted into the second ring groove, and an oil ring (not shown) is fitted into the oil ring groove. In addition, along the outer peripheral surface 12 of the piston 1, a space between the piston crown surface 11 and the top ring groove 13 is called a first land 12a, a space between the top ring groove 13 and the second ring groove (not shown) is called a second land 12b, and a space between the second ring groove and the oil ring groove (not shown) is called a third land (not shown).

[0017] The rings such as the top ring 30 are formed of, for example, high carbon steel or martensitic stainless steel. The rings such as the top ring 30 have a substantially C-shape with one opening in the circumferential direction, and are inserted into a ring groove such as the top ring groove 13 in an elastically expanded state, and then contract in diameter due to their elastic restoring force to be fitted inside the ring groove. The outer peripheral surface 33 of the top ring 30 protrudes outward from the outer peripheral surface 12 of the piston 1, and the outer peripheral surfaces of the other rings (not shown) also protrude outward from the outer peripheral surface 12. Therefore, when the piston 1 with the rings attached thereto is inserted into the cylinder 40, the rings are inserted into the cylinder 40 in an elastically contracted state. When the piston 1 is inserted into the cylinder 40, the rings are pressed against the inner wall surface 41 of the cylinder 40 by their elastic force, and the top ring 30 and the second ring perform the function of maintaining the airtightness of the combustion chamber, and the oil ring performs the function of scraping off the oil remaining on the inner wall surface 41 of the cylinder 40.

[0018] The inner surface of the top ring groove 13 on the piston crown surface 11 side is called the upper surface 13a, the inner surface on the second ring groove (not shown) side is called the lower surface 13c, and the inner surface on the bottom side of the groove between them is called the side surface 13b. An anodic oxide coating 20 is formed on the upper surface 13a, the side surface 13b, and the lower surface 13c of the top ring groove 13. The lower surface 32 of the top ring 30 tightly adheres to the lower surface 13c of the top ring groove 13 because the inside of the combustion chamber on the piston crown surface 11 side becomes high pressure due to the compression stroke and expansion stroke of the piston 1. On the other hand, although not shown, the upper surface 31 of the top ring 30 adheres to the upper surface 13a of the top ring groove 13 during the intake stroke. Since the top ring 30 moves between the upper surface 13a and the lower surface 13c of the top ring groove 13 every time these steps are repeated, wear is likely to occur between the inner surface of the top ring groove 13 and the top ring 30. Therefore, the anodic oxide film 20 is formed on the inner surface of the top ring groove 13 of the piston 1, including the upper surface 13a and the lower surface 13c. The anodic oxide film 20 may be formed on the piston crown surface 11 in addition to the inner surface of the top ring groove 13, and in that case, it may also be formed on the first land 12a therebetween. Furthermore, the anodic oxide film 20 may also be formed on the second ring groove (not shown). In that case, it may be formed on the second land 12b.

[0019] The structure of the top ring groove having an anodized film formed on the base material surface with a heat insulating layer therebetween will be described in more detail with reference to FIG.

[0020] As shown in FIG. 2(a), the piston for an internal combustion engine is formed of an aluminum alloy containing more Cu than conventional aluminum alloys as the base material 10, and the base material 10 has primary crystal silicon 15 and acicular silicon 16 crystallized in an α phase 14. The α phase 14 is a phase in which other elements such as Cu are dissolved in aluminum (Al). The primary crystal silicon 15 is a relatively large lump of Si crystallized during the manufacturing process of the piston body. The particle size of the primary crystal silicon 15 is, for example, about 30 to 40 μm. The acicular silicon 16 is also Si crystallized during the manufacturing process of the piston body, but also contains a copper component.

[0021] 2(b), the inner surface 13s of the top ring groove is immersed in a mixed acid, which will be described later in detail, to dissolve the Cu-containing acicular silicon 16 in the surface portion of the base material 10, and also dissolve the Cu component from the α-phase 14. As a result, a heat insulating layer 27a is formed having an aluminum alloy composition in which the Cu concentration is reduced compared to the base material. Note that although the primary crystal silicon 15 is also dissolved in the heat insulating layer 27a, a part of the primary crystal silicon 15 remains without being dissolved.

[0022] As shown in FIG. 2(c), the heat insulating layer 27a is anodized to form an anodized film 20 on the surface of the heat insulating layer 27b, as will be described in detail later. The anodized film 20 is a film formed by oxidizing aluminum in the heat insulating layer 27b, and is made of amorphous aluminum oxide (Al 2 O 3 ) as a main component and has excellent wear resistance. The state of the cells of the anodic oxide film 20 can have various structures that differ depending on the electrolysis conditions, but a structure in which the cells are branched in random directions and surround the primary crystal silicon in the film is preferable. This structure is the structure of a film (AC-DC superimposed electrolytic film) formed by AC-DC superimposed electrolysis, which will be described in detail later. This results in a film with improved surface smoothness compared to a film formed by DC electrolysis, for example. The good surface smoothness of the anodic oxide film 20 improves the sealing performance with the piston ring. In addition, the anodic oxide film 20 has many fine pores on its surface by forming it on the surface of the above-mentioned heat insulating layer 27. The air in these fine pores allows the anodic oxide film 20 to further improve the heat insulating performance in the top ring groove.

[0023] The thickness of the anodic oxide coating 20 is preferably 5.0 μm or more, and more preferably 10 μm or more, since it is reduced by wear with the piston ring 30 during engine operation. There is no particular upper limit to the thickness of the anodic oxide coating 20, but it is preferably 40 μm or less, and more preferably 30 μm or less.

[0024] The heat insulating layer 27 is a layer in the top ring groove that contains less Cu than the base material 10. For example, it is preferable that the heat insulating layer 27 contains substantially no Cu component in the α phase 14 and is substantially free of acicular silicon 16. It is preferable that the primary crystal silicon 15 is present in an amount less than that of the base material.

[0025] As shown in Table 1, Cu has a high thermal conductivity among the constituent materials of pistons for internal combustion engines, for example, a thermal conductivity 1.5 times or more that of Al. Therefore, the Cu content of the heat insulating layer 27 and the base material 10 has a large effect on the heat insulating performance of the top ring groove. The heat insulating layer 27 has a lower Cu content than the base material 10, and therefore has a low thermal conductivity, which results in excellent heat insulating properties. The thickness of the heat insulating layer 27b after the anodizing treatment is preferably 1.0 μm or more, more preferably 5.0 μm or more, and even more preferably 10 μm or more, in order to exhibit sufficient heat insulating properties against the base material 10. The upper limit of the thickness of the heat insulating layer 27b is not particularly limited, but since the longer the immersion time of the mixed acid immersion treatment for forming the heat insulating layer, the greater the impact on the surface smoothness of the top ring groove, the more preferably the thickness is 30 μm or less, and more preferably 20 μm or less.

[0026] [Table 1]

[0027] By improving the heat insulation in the top ring groove, softening of the base material 10 can be suppressed, so that the smoothness of the surface of the top ring groove can be maintained, and the sealing performance with respect to the top ring can be maintained. This prevents oil from flowing into the combustion chamber through the gap between the top ring groove and the top ring, which is known as oil rising, and prevents the oil from burning in the combustion chamber, so that the generation of substances subject to European environmental regulations such as PM and PN and an increase in the number of these substances can be suppressed.

[0028] Next, one embodiment of a method for manufacturing a piston for an internal combustion engine according to the present invention will be described with reference to Figures 3 and 4. As shown in Figure 3, the manufacturing method according to the present invention includes at least a step 31 of casting a piston body using an aluminum alloy as a base material, a step 32 of heat treating the cast piston body, a step 33 of further processing the heat-treated piston to form piston ring grooves including a top ring groove, a step 34 of immersing the top ring groove of the piston body in mixed acid, and a step 35 of anodizing the top ring groove.

[0029] The above-mentioned casting, heat treatment and machining steps 31, 32 and 33 are similar to the steps used in manufacturing a general piston for an internal combustion engine, and therefore a detailed explanation thereof will be omitted here.

[0030] As shown in FIG. 4, step 34 of performing mixed acid immersion treatment further includes step 41 of masking the piston body, step 42 of degreasing the areas exposed by the masking, step 43 of rinsing the areas with water, step 44 of drying the areas, step 45 of immersing the areas in mixed acid, step 46 of rinsing the piston after the mixed acid treatment with water, and step 47 of removing the masking.

[0031] In the masking step 41, the periphery of the target portion is covered with a masking member so that the heat insulating layer is not formed in any portion other than the portion where the heat insulating layer is to be formed. For example, in FIG. 1, when the heat insulating layer is formed only on the inner surface of the top ring groove 13, the positions of the first land 12a and the second land 12b of the piston 1 are covered with a masking member to expose the inner surface of the top ring groove 13. The material of the masking member can be a rubber material that is resistant to chemicals such as mixed acids, such as natural rubber, butadiene rubber, styrene rubber, acrylic rubber, urethane rubber, nitrile rubber, and silicone rubber, and nitrile rubber or silicone rubber is more preferable. Nitrile rubber or silicone rubber has sufficient resistance to chemicals such as sulfuric acid, which is the treatment liquid used in the anodizing treatment step 35, so that the anodizing treatment step 35 can be performed with the masking member attached.

[0032] After the masking step 41, a degreasing step 42, a water washing step 43, and a drying step 44 are carried out in this order. These are similar to the processes generally carried out to remove impurities from the processing target area, and therefore a detailed description thereof will be omitted here.

[0033] In the mixed acid immersion process 45, the top ring groove exposed from the masking member is immersed in a mixed acid treatment solution to dissolve Cu components from the region from the processed surface of the top ring groove to a predetermined treatment depth. The mixed acid treatment solution may be any solution capable of dissolving Cu components from the aluminum alloy, and may be, for example, an aqueous solution of mixed acid in which at least two types of acids such as nitric acid, hydrofluoric acid, and sulfuric acid are mixed. In particular, an aqueous solution of mixed acid of nitric acid and hydrofluoric acid, which has good dissolution properties of copper and silicon components, is preferred. The concentration of nitric acid in the mixed acid treatment solution is preferably 40 to 60 mass %, and the concentration of hydrofluoric acid is preferably 5 to 15 mass %. The mixture ratio of nitric acid to hydrofluoric acid is preferably nitric acid:hydrofluoric acid=3:1 to 10:1 by mass.

[0034] In the mixed acid immersion process 45, by immersing in the mixed acid treatment solution, the Cu component in the α phase 14 is dissolved at a predetermined treatment depth as shown in FIG. 2(b), and the acicular silicon 16 is also dissolved. The primary silicon 15 is also dissolved, but not all of it, and some of the primary silicon 15 remains on the surface 13s of the top ring groove. In this way, the primary silicon 15 and the acicular silicon 16 are dissolved, and the surface 17 having unevenness is formed in the insulating layer 27a. Since the primary silicon 15 is a large lump, the occurrence of large recesses can be reduced and a significant increase in the surface roughness of the insulating layer 27a can be prevented by the primary silicon and acicular silicon on the surface of the top ring groove. On the other hand, the presence of the primary silicon and acicular silicon on the surface of the top ring groove prevents the formation of an anodic oxide film with a smooth surface, so the reduction of the primary silicon and acicular silicon on the surface of the insulating layer 27a can improve the smoothness of the surface of the anodic oxide film.

[0035] Such improvement in the surface smoothness of the anodized film can greatly contribute to suppressing the generation of the above-mentioned PM and PN, which are substances subject to European environmental regulations, and to suppressing an increase in the number of these substances. Furthermore, the improvement in the surface smoothness of the anodized film further improves the sealing performance in the top ring groove, which can contribute to improving fuel efficiency by reducing the amount of blow-by gas.

[0036] In the mixed acid immersion treatment that can leave a part of the primary crystal silicon 15, the treatment depth of the base material by the mixed acid immersion treatment, which will be described in detail later, is preferably set to 30 μm or less. This is because, according to the knowledge of the present inventors, the treatment depth of the base material by the mixed acid immersion treatment is proportional to the amount of primary crystal silicon 15 on the surface of the insulating layer 27a formed by the mixed acid immersion treatment. The treatment depth of the base material by the mixed acid immersion treatment is more preferably set to 20 μm or less, and even more preferably set to 15 μm or less.

[0037] The treatment depth of the base material in the mixed acid immersion treatment step 45 is a depth exceeding 1 / 2 of the thickness of the anodized film planned for the anodized film treatment step 35. This is because the anodized film is an aluminum oxide film, and as shown in Figs. 2(b) and (c), the surface of the anodized film 20 after the surface treatment rises in size by about 1 / 2 the thickness of the anodized film 20 compared to the heat insulating layer 27a before the anodized treatment. That is, the surface of the heat insulating layer 27b after the surface treatment (the interface with the anodized film 20) drops by about 1 / 2 the thickness of the anodized film 20. Therefore, in order to leave the heat insulating layer 27 after the anodized treatment, the treatment depth of the base material is set to a depth exceeding 1 / 2 the thickness of the planned anodized film 20. Specifically, the treatment depth of the base material is preferably more than 2.5 μm, more preferably more than 5.0 μm, and even more preferably more than 7.5 μm. The treatment depth of the base material is preferably the sum of half the thickness of the planned anodized film and the thickness of the heat insulating layer 27b to be left after the anodizing treatment. In this case, the upper limit of the treatment depth of the base material is preferably 30 μm or less, more preferably 20 μm or less, and even more preferably 15 μm or less.

[0038] The processing depth of the base material by the mixed acid immersion treatment can be controlled by the immersion time in the mixed acid treatment solution. Although it depends on the concentration of the mixed acid treatment solution and the composition of the aluminum alloy of the base material, the processing depth of the base material can be made to exceed 2.5 μm by making the immersion time 10 seconds or more, and the processing depth of the base material can be made to exceed 7.5 μm by making the immersion time 30 seconds or more. In addition, the processing depth of the base material can be made to be 30 μm or less by making the immersion time 120 seconds or less, the processing depth of the base material can be made to be 20 μm or less by making the immersion time 80 seconds or less, and the processing depth of the base material can be made to be 15 μm or less by making the immersion time 60 seconds or less.

[0039] The degree of the mixed acid treatment in the mixed acid immersion treatment step 45 can be expressed by the surface roughness (particularly the surface roughness Ra) of the surface 17 of the heat insulating layer 27a after the mixed acid immersion treatment. The surface roughness Ra represents the arithmetic mean roughness of the contour curve as specified by JIS B0601. The deeper the treatment depth of the base material in the mixed acid treatment, the larger the value of the surface roughness Ra of the heat insulating layer after the mixed acid immersion treatment tends to be. The lower limit of the surface roughness Ra is, for example, preferably 0.3 μm or more, more preferably 0.5 μm or more, and even more preferably 0.8 μm or more. The upper limit of the surface depth Ra is, for example, preferably 3.2 μm or less, more preferably 2.4 μm or less, and even more preferably 1.6 μm or less.

[0040] After the mixed acid immersion treatment step 45, a water washing step 46 is performed, followed by a masking member removal step 47. Then, as shown in Fig. 3, an anodizing treatment step 35 is performed. As described above, when a predetermined masking member is used, an anodizing film is formed in the anodizing treatment step 35 while the mask is still on, and then the masking member is removed.

[0041] In the anodizing process 35, an electrode plate such as titanium or carbon as a cathode and an internal combustion engine piston as an anode are immersed in an electrolytic solution such as sulfuric acid or oxalic acid in an electrolytic cell (not shown), and electricity is passed from a power source to perform electrolysis and oxidize the inner surface of the top ring groove of the internal combustion engine piston. After the electrolysis, as shown in FIG. 2(c), an anodized film 20 is formed on the surface of the insulating layer 27b. The thickness of the insulating layer 27b after the anodizing process is the thickness of the insulating layer 27a before the anodizing process reduced by half the thickness of the anodized film 20.

[0042] The anodizing process 45 can be a conventional electrolytic process for forming an anodized film on the inner surface of the top ring groove. 2 SO 4 ), oxalic acid (H 2 C 2 O 4 ), phosphoric acid (H 3 PO 4 ), Chromic acid (H 2 CrO 4 ), sodium hydroxide (NaOH), sodium phosphate (Na 3 PO 4 A basic treatment solution such as sodium fluoride (NaF) or sodium chloride (NaF) can be used, and sulfuric acid is preferred from a practical point of view. The cathode plate can be a titanium plate, a carbon plate, an aluminum plate, a stainless steel plate, or the like. The electrolysis method can be a direct current electrolysis method, an AC-DC superimposed electrolysis method in which an AC current is superimposed on a direct current, or the like, and the AC-DC superimposed electrolysis method is preferred. In the AC-DC superimposed electrolysis method, the application of a positive voltage to form a film and the application of a negative voltage to remove the charge accumulated in the film are alternately repeated, thereby preventing electricity from concentrating and flowing at a specific location, and as a result, a film with a uniform thickness and small surface roughness can be obtained. The good smoothness of the surface of the anodic oxide film improves the sealing between the piston ring groove and the piston ring.

[0043] In addition, in this embodiment, the aluminum alloy as the base material may be an alloy containing at least one element selected from the group consisting of nickel (Ni), chromium (Cr), titanium (Ti), zirconium (Zr), phosphorus (P), iron (Fe), manganese (Mn) and magnesium (Mg) in addition to the above-mentioned Si and Cu, with the balance being substantially composed of Al and unavoidable impurities. Preferably, the aluminum alloy base material contains, in addition to the above-mentioned ranges of the respective contents of Si and Cu, 1.5 to 3.5 mass% Ni, 0.05 to 0.15 mass% Cr, 0.05 to 0.20 mass% Ti, 0.05 to 0.30 mass% Zr, 0.10 to 0.31 mass% Fe, 0.05 mass% or less Mn and 0.5 to 1.1 mass% Mg, with the balance being substantially composed of Al and unavoidable impurities. Since Si and Cu have already been described, the other components and their contents will be described.

[0044] Ni is a component that mainly improves strength and wear resistance in high temperature ranges and reduces the thermal expansion coefficient. If the Ni content is 1.5 mass% or more, these effects are suitably exhibited, and if it is 3.5 mass% or less, good elongation is obtained.

[0045] Cr is a component that strengthens the grain boundaries between crystal grains such as intermetallic compounds, primary crystal silicon, and acicular silicon crystallized in the alloy, thereby improving strength at high temperatures. A Cr content of 0.05% by mass or more favorably strengthens the grain boundaries and improves strength at high temperatures, while a Cr content of 0.15% by mass or less provides good toughness and machinability.

[0046] Ti is a component that mainly refines crystal grains to improve heat resistance, castability, and strength, and this effect is suitably exhibited if the Ti content is in the range of 0.05 to 0.20 mass %, and the Ti content is preferably 0.05 to 0.15 wt %.

[0047] Zr is a component that mainly has the effect of refining crystal grains in the alloy and contributes to improving heat resistance, castability, and strength, and if the Zr content is in the range of 0.05 to 0.30 mass%, the effect is suitably exhibited. The Zr content is preferably 0.05 to 0.15 wt%.

[0048] Fe is a component that mainly crystallizes intermetallic compounds and improves wear resistance and strength at high temperatures. If the size of these intermetallic compounds is coarse, strength decreases. If the Fe content is in the range of 0.10 to 0.31 mass%, the size of the Fe-Mn intermetallic compounds can be reduced.

[0049] Mn is a component that mainly crystallizes intermetallic compounds and improves wear resistance and strength at high temperatures. If the size of the intermetallic compounds is coarse, the strength decreases. If the Mn content is 0.05 mass% or less, the size of the Fe-Mn intermetallic compounds can be made small. The lower limit of the Mn content may be zero or may be contained in a very small amount similar to that of an impurity, for example, 0.001 mass%.

[0050] Mg is a component that mainly improves strength and toughness. If the Mg content is 0.5% by mass or more, the effect of improving strength is exerted, and if it is 1.1% by mass or less, good toughness is obtained.

[0051] In the present embodiment, the masking is performed at the positions of the first land and the second land, and the heat insulating layer and the anodic oxide film are formed on the inner surface of the top ring groove, but the present invention is not limited to this. For example, the heat insulating layer and the anodic oxide film may be formed on the inner surface of the top ring groove and the piston crown surface by masking at the position of the second land in the masking process, or on the inner surfaces of the top ring groove and the second ring groove by masking at the positions of the first land and the third land, or on the inner surfaces of the top ring groove and the second ring groove and the piston crown surface by masking at the position of the third land. In any case, an excellent heat insulating effect is obtained, so that the cooling loss of the piston can be reduced.

[0052] In addition, in the present embodiment, the piston for an internal combustion engine has been described assuming a piston for a port injection type spark ignition combustion engine, but the present invention is not limited to this, and the piston for an internal combustion engine according to the present invention can also be suitably applied to a piston for a direct injection type spark ignition combustion engine, a piston for a diesel engine, a piston for a homogenous charge compression ignition combustion engine, a piston for a CNG (Compressed Natural Gas) engine, a piston for a general-purpose engine, etc. EXAMPLES

[0053] EXAMPLES Hereinafter, examples and comparative examples according to the present invention will be described. Note that the piston for an internal combustion engine and the manufacturing method thereof according to the present invention are not limited to the following examples and comparative examples.

[0054] [Example 1] An Al-Si aluminum alloy casting material was used, with the composition shown in Table 2. This casting material was subjected to a heat treatment called T6 treatment, which is widely used for aluminum alloys for pistons, and then processed to produce a test piece simulating an internal combustion engine piston (hereinafter, also referred to as high-strength material). The inner surface of the top ring groove was finished by cutting, and had a very smooth surface with a surface roughness Ra of 0.07 μm.

[0055] [Table 2]

[0056] [Comparative Example 1] A test piece simulating a piston for an internal combustion engine was produced in the same manner as in Example 1 using a conventional AC8A aluminum alloy (hereinafter, also referred to as a normal material).

[0057] (Measurement of surface roughness versus mixed acid immersion time) The surface roughness of each test piece of Example 1 and Comparative Example 1 was measured at predetermined time intervals while immersed in the mixed acid treatment solution at room temperature, and the change in surface roughness with respect to the mixed acid immersion time was evaluated. Regarding the surface roughness, the arithmetic mean roughness (surface roughness Ra) of the test piece surface was measured by a method conforming to JIS B 0601-2001, with a measurement length of 4 mm and a cutoff of 0.8 mm. The mixed acid treatment solution used was a mixture of nitric acid, hydrofluoric acid, and water in a predetermined ratio (50:6:44 by mass%). The results are shown in FIG. 5.

[0058] As shown in FIG. 5, it was confirmed that the surface roughness Ra of the high-strength material (Example 1) with respect to the mixed acid immersion time tends to increase more than that of the normal material (Comparative Example 1). This can be assumed to be because the content of metals that are easily eluted, such as copper, in the high-strength material is greater than that of the normal material. It was also confirmed that the surface roughness Ra increases in proportion to the immersion time in both Example 1 and Comparative Example 1. This can be assumed to be because the longer the immersion time, the more acicular silicon (which also contains Cu) on the treated surface is eluted, and the more primary crystal silicon, which is less likely to be eluted than acicular silicon, is eluted. When the immersion time was 10 seconds or more, the surface roughness Ra was 0.4 μm or more, when the immersion time was 30 seconds or more, the surface roughness Ra was 0.8 μm or more, and when the immersion time was 60 seconds, the surface roughness Ra was 1.6 μm. Furthermore, the treatment depth when the immersion time was 10 seconds was 2.5 μm, the treatment depth when the immersion time was 30 seconds was 7.5 μm, and the treatment depth when the immersion time was 60 seconds was 15 μm.

[0059] (Observation of the machined surface of the top ring groove before and after mixed acid immersion treatment) For the test piece of Example 1, the above mixed acid treatment solution was used to observe the machined surface of the top ring groove before mixed acid immersion treatment, the machined surface of the top ring groove after mixed acid immersion treatment with a mixed acid immersion time of 30 seconds, and the cross-sections of these machined surfaces, and the change in the machined surface of the top ring groove before and after mixed acid immersion treatment was evaluated. The surface observation was performed using a scanning electron microscope (SEM), and the cross-section observation of the machined surface of the top ring groove was performed by cutting the test piece. The surface roughness Ra was measured in the same manner as the measurement of surface roughness described above. Figure 6(a) shows a surface photograph of the machined surface before mixed acid immersion treatment, and Figure 6(b) shows a surface photograph of the machined surface after mixed acid immersion treatment. Also, Figure 7(a) shows a cross-sectional photograph of the machined surface before mixed acid immersion treatment, and Figure 7(b) shows a cross-sectional photograph of the machined surface after mixed acid immersion treatment.

[0060] As shown in FIG. 6(a), the machined surface of the top ring groove before the mixed acid immersion treatment was very smooth, while as shown in FIG. 6(b), the machined surface of the top ring groove after the mixed acid immersion treatment had irregularities. This is because many parts 14a where Cu in the α phase was presumed to have been dissolved were observed, and many parts 16a where acicular silicon containing Cu components was presumed to have been dissolved were also observed. The remaining primary crystal silicon 15 was confirmed. As shown in FIG. 7(a), the cross section of the machined surface of the top ring groove before the mixed acid immersion treatment was very smooth, with a surface roughness Ra of 0.07 μm. On the other hand, as shown in FIG. 7(b), many recesses were observed on the cross section of the machined surface of the top ring groove after the mixed acid immersion treatment due to the dissolution of Cu in the α phase, the dissolution of acicular silicon (including Cu), and the dissolution of some primary crystal silicon due to the mixed acid immersion treatment. The surface roughness Ra was 0.85.

[0061] [Example 2] For the test piece of Example 1, the processed surface of the top ring groove was immersed in the mixed acid at room temperature for 30 seconds using the mixed acid treatment solution. Next, the top ring groove after the mixed acid immersion treatment was anodized. The anodization treatment was performed using sulfuric acid at 5°C as the electrolyte, titanium that had been surface-treated to improve chemical resistance as the cathode plate, the test piece was attached to the anode plate, and a jig was used in which the electrolyte flows only in the top ring groove. The anodization treatment was performed for 40 seconds using constant voltage electrolysis with a positive voltage of 65V, a negative voltage of -2V, and a frequency of 12kHz using AC / DC superimposed electrolysis as the electrolysis method.

[0062] [Comparative Example 2] The test piece of Example 1 was subjected to anodizing treatment in the same manner as in Example 2, except that the mixed acid immersion treatment was not performed.

[0063] (Evaluation of top ring grooves with anodized film) For Example 2 and Comparative Example 2, the surface of the top ring groove on which the anodized film was formed was observed, and the thickness and surface roughness of the anodized film were measured to evaluate the difference in the anodized film depending on whether or not the anodized film was immersed in mixed acid. The surface observation and surface roughness measurement were performed in the same manner as described above. The thickness of the anodized film was calculated by cutting the test piece, measuring 10 equally spaced points on the cross section of the anodized film using an optical microscope, and averaging the obtained values. FIG. 8 shows a surface photograph of the anodized film of Example 2, and FIG. 9 shows a surface photograph of the anodized film of Comparative Example 2. FIG. 10 shows a cross-sectional photograph of the top ring groove on which the anodized film of Example 2 was formed, and FIG. 11 shows a cross-sectional photograph of the top ring groove on which the anodized film of Comparative Example 2 was formed.

[0064] As shown in Fig. 8, numerous micropores were found on the surface of the anodized film of Example 2. On the other hand, as shown in Fig. 9, although micropores were found on the surface of the anodized film of Comparative Example 2, the number of micropores was fewer than in Example 2. These results confirmed that the mixed acid immersion treatment forms numerous micropores on the surface of the anodized film that improve heat insulation.

[0065] In addition, as shown in FIG. 10, a heat insulating layer 27 having a thickness of several μm was confirmed between the anodized film 20 and the base material 10 in the cross section of the top ring groove of Example 2, in which primary crystal silicon or acicular silicon was not confirmed. On the other hand, as shown in FIG. 11, primary crystal silicon 15 and acicular silicon 16 were observed under the anodized film 20 in the cross section of the top ring groove of Comparative Example 2, and no layer different from the base material 10 as in Example 2 was confirmed. The surface roughness Ra of the anodized film of Example 2 was 0.77 μm, and the film thickness was 12.0 μm. The surface roughness Ra of the anodized film of Comparative Example 2 was 1.75 μm, and the film thickness was 14.1 μm. From these results, while there is no significant difference in film thickness depending on whether or not the mixed acid immersion treatment is performed, the surface roughness is reduced by nearly half. From this, it can be inferred that the mixed acid immersion treatment greatly contributes to the surface smoothness of the anodized film. This is presumably due to the mixed acid immersion treatment dissolving primary crystal silicon and acicular silicon (which also contains Cu), which are the causes of the generation of irregularities in the anodized film. [Explanation of symbols]

[0066] 1. Pistons for internal combustion engines 10 Piston base material 11 Piston crown surface 12 Piston outer surface 12a Land 1 12b 2nd Land 13 Top ring groove 13a Top surface of top ring groove 13b Side of top ring groove 13c Underside of top ring groove 14 α phase 15 Primary silicon 16 Needle-shaped silicon 17 Surface of insulation layer after mixed acid immersion treatment 20 Anodized film 27 Insulation Layer 30 Top Ring 40 Cylinder

Claims

1. a masking step of masking an internal combustion engine piston body formed from an aluminum alloy containing 5.0 to 20.0% by mass of Si and more than 1.3% by mass and not more than 5.0% by mass of Cu as a base material so as to expose an inner surface of a top ring groove; a mixed acid immersion treatment process in which the masked piston body is immersed in an aqueous solution of a mixed acid to dissolve Cu from a region of the exposed inner surface of the top ring groove to a depth equivalent to more than half the thickness of the anodized coating to be formed and not more than 20 μm from the surface; an anodizing process for forming an anodized coating film having the expected thickness on the inner surface of the top ring groove of the piston body taken out of the aqueous solution of the mixed acid; A method for manufacturing a piston for an internal combustion engine, comprising:

2. A piston body for an internal combustion engine formed from an aluminum alloy containing 5.0 to 20.0% by mass of Si and more than 1.3% by mass and not more than 5.0% by mass of Cu as a base material, comprising: a masking step of masking an inner surface of a top ring groove to expose the inner surface; a mixed acid immersion treatment process in which the masked piston body is immersed in an aqueous solution of a mixed acid to dissolve Cu from a region of the exposed inner surface of the top ring groove to a depth corresponding to more than half the thickness of the anodized film to be formed; an anodizing process for forming an anodized coating film having the expected thickness on the inner surface of the top ring groove of the piston body taken out of the aqueous solution of the mixed acid; A method for manufacturing a piston for an internal combustion engine, comprising: In the mixed acid immersion treatment step, acicular silicon is dissolved in the region, Cu is dissolved from the α phase of the aluminum alloy, and a part of primary crystal silicon is left.

3. 3. The method for manufacturing a piston for an internal combustion engine according to claim 1, wherein the top ring groove from which Cu has been eluted in the mixed acid immersion treatment step has a surface roughness Ra of 0.4 to 3.2 μm.

4. The method for manufacturing a piston for an internal combustion engine according to any one of claims 1 to 3, wherein in the anodizing treatment step, the anodized film is formed by AC / DC superimposed electrolysis.

5. A piston for an internal combustion engine having a top ring groove, The aluminum alloy contains 5.0 to 20.0% by mass of Si and more than 1.3% by mass and not more than 5.0% by mass of Cu as a base material, a heat insulating layer located on an inner surface of the top ring groove, the heat insulating layer having an aluminum alloy composition with a lower Cu content than the base material, the heat insulating layer having a thickness of 1.0 μm or more and 20 μm or less; an anodized coating located on the surface of the thermal insulation layer; A piston for an internal combustion engine.

6. 6. The piston for an internal combustion engine according to claim 5, wherein cells of the anodized coating extend in random directions relative to the inner surface of the top ring groove, and the cells surround the silicon in the anodized coating in a state where they are branched in random directions.

Citation Information

Patent Citations

  • Manufacture of aluminum alloy piston

    JP1991100198A

  • Piston for internal combustion engine

    JP1994081711A

  • Anodized film and anodizing method

    JP2006083467A

  • Forming method of heat insulation film

    JP2018035688A

  • Surface structure and surface treatment method of aluminum member

    JP2019218587A