LCD panel
The liquid crystal panel design with a polarizing film and anti-reflective film, directly contacting alkali-free glass, addresses light reflection and coloration issues, improving visibility in displays by ensuring neutral reflected light and reduced reflection.
Patent Information
- Application Number
- JP2019225876
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-13
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2039-12-13
AI Technical Summary
Existing liquid crystal display devices face issues with light reflection and unwanted coloration of reflected light, particularly in applications requiring good visibility like in-vehicle displays, when an anti-reflection film is used without a conductive layer between the polarizing film and the liquid crystal cell.
A liquid crystal panel design with a polarizing film having an anti-reflective film, where the polarizing film is laminated with an alkali-free glass, and an adhesive layer directly contacts the glass, ensuring the reflected light meets specific colorimetric criteria to achieve a neutral hue and reduced reflection.
The solution effectively suppresses light reflection and maintains a neutral hue of reflected light, enhancing visibility in applications such as in-vehicle displays.
Smart Images

Figure 0007579055000006 
Figure 0007579055000007 
Figure 0007579055000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal panel. [Background technology]
[0002] A liquid crystal display device includes, for example, a liquid crystal panel having a structure in which a polarizing film is arranged on the viewing side of a liquid crystal cell, and an illumination system that irradiates the liquid crystal panel with light. The liquid crystal display device displays an image by applying a voltage to the liquid crystal cell and adjusting the orientation of the liquid crystal molecules contained in the liquid crystal cell.
[0003] In the field of liquid crystal panels, it is known that, for example, an ITO (indium tin oxide) layer is disposed on the surface of the liquid crystal cell on the polarizing film side in order to prevent static electricity in liquid crystal display devices. However, from the viewpoint of cost, etc., the above-mentioned ITO layer is sometimes omitted. For example, Patent Documents 1 and 2 disclose liquid crystal panels in which an ITO layer is not disposed on the surface of the liquid crystal cell on the polarizing film side, and a polarizing film with an adhesive layer is in direct contact with the liquid crystal cell. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2018 / 181477 [Patent Document 2] Patent No. 5679337 Summary of the Invention [Problem to be solved by the invention]
[0005] According to the study by the present inventors, when a liquid crystal display device is required to have good visibility, for example, when the liquid crystal display device is used as an in-vehicle display, it is found that it is necessary to sufficiently suppress the reflection of light on the liquid crystal panel. Based on this knowledge, the present inventors have conducted further studies and found that when an anti-reflection film is used for the purpose of suppressing the reflection of light on the liquid crystal panel, the hue of the reflected light from the liquid crystal panel changes significantly, resulting in unwanted coloration.
[0006] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a liquid crystal panel that sufficiently suppresses light reflection and produces reflected light with a neutral hue. [Means for solving the problem]
[0007] The present invention relates to a polarizing film with an anti-reflection film, the polarizing film and the pressure-sensitive adhesive layer being arranged in this order in the lamination direction; A liquid crystal cell; Equipped with no conductive layer is provided between the anti-reflection coated polarizing film and the liquid crystal cell; The anti-reflection coated polarizing film is laminated on the non-alkali glass so that the pressure-sensitive adhesive layer is in direct contact with the non-alkali glass, and when light from a CIE standard illuminant D65 is incident on the surface opposite to the pressure-sensitive adhesive layer, the anti-reflection coated polarizing film has a reflectance of L * a * b * a in color system * value and b * The present invention provides a liquid crystal panel that produces reflected light whose values satisfy the following relational expressions (1) and (2): -10≦a * <= 10 (1) -18≦b * <=5 (2) Effect of the Invention
[0008] According to the present invention, it is possible to provide a liquid crystal panel that sufficiently suppresses light reflection and provides reflected light with a neutral hue. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view of a liquid crystal panel according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of an anti-reflection film. [Diagram 3] FIG. 11 is a cross-sectional view showing another example of an antireflection film. [Figure 4] FIG. 11 is a cross-sectional view showing a modified example of the liquid crystal panel. [Diagram 5] FIG. 11 is a cross-sectional view showing another modified example of the liquid crystal panel. [Figure 6] FIG. 11 is a cross-sectional view showing still another modified example of the liquid crystal panel. [Figure 7] 1 is a graph showing the relationship between the a* value and the b* value of reflected light from antireflection coated polarizing films of Examples, Reference Examples, and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will now be described in detail, but the following description is not intended to limit the present invention to a specific embodiment.
[0011] (Embodiment of Liquid Crystal Panel) As shown in FIG. 1, the liquid crystal panel 100 of the present embodiment includes a polarizing film 15 with an anti-reflection film and a liquid crystal cell 25. No conductive layer, such as an ITO layer, is provided between the polarizing film 15 with an anti-reflection film and the liquid crystal cell 25, and the polarizing film 15 with an anti-reflection film is in direct or indirect contact with the liquid crystal cell 25. A layer other than the conductive layer may be disposed between the polarizing film 15 with an anti-reflection film and the liquid crystal cell 25 as long as it does not impede the effects of the present invention. The polarizing film 15 with an anti-reflection film has an anti-reflection film 10, a polarizing film 20, and a pressure-sensitive adhesive layer 30 in this order in the lamination direction. The polarizing film 20 is in contact with, for example, each of the anti-reflection film 10 and the pressure-sensitive adhesive layer 30.
[0012] In the polarizing film with anti-reflection coating 15, when the adhesive layer 30 is laminated with non-alkali glass so that the adhesive layer 30 is in direct contact with the non-alkali glass, light from a CIE standard illuminant D65 is incident on the surface opposite to the adhesive layer 30 (typically, the surface of the anti-reflection coating 10), L * a * b * a in the color space (CIE1976) * value and b * The anti-reflection coated polarizing film 15 produces reflected light whose values satisfy the following relational expressions (1) and (2). The anti-reflection coated polarizing film 15 which produces such reflected light can adjust the reflected light of the liquid crystal panel 100 to a neutral hue. -10≦a * <= 10 (1) -18≦b * <=5 (2)
[0013] For details, see above a * value and b * The value can be specified by the following method. First, the anti-reflection coated polarizing film 15 is attached to the alkali-free glass by the adhesive layer 30. The alkali-free glass is glass that does not substantially contain an alkali component (alkali metal oxide), and in detail, the weight ratio of the alkali component in the glass is, for example, 1000 ppm or less, and further 500 ppm or less. The alkali-free glass is, for example, in a plate shape and has a thickness of 0.5 mm or more. Next, a black film is attached to the surface of the alkali-free glass opposite to the surface attached to the anti-reflection coated polarizing film 15. Next, light from the CIE standard illuminant D65 is made to enter the surface of the anti-reflection coated polarizing film 15 on the anti-reflection coating 10 side at an incident angle of 5°. The specular reflectance in the wavelength range of 360 nm to 740 nm generated at this time is specified, and the tristimulus values (X, Y, and Z) in the XYZ color system (CIE1931) are specified from the spectral reflectance. The tristimulus values are specified in detail in JIS Z8701:1999. Using the obtained tristimulus values, a is calculated by the following formulas (i) and (ii) specified in JIS Z8781-4:2013. * value and b * Identify the value.
number
[0014] The above a * The value is preferably -6 or more and 6 or less, more preferably -3 or more and 3 or less. * The value is preferably -15 or more and 3 or less, more preferably -10 or more and 2 or less, further preferably -6 or more and 2 or less, and particularly preferably -5 or more and 2 or less. * value and b * The value may satisfy the following relations (3) and (4). b * ≧-1.5a * -15 (3) b * ≦-1.5a * +7.5 (4)
[0015] In addition, * value and b * The value may satisfy the following relations (5) and (6). b * ≧-1.5a * -5 (5) b * ≦-1.5a * +4.5 (6)
[0016] The reflected light L * The value is, for example, 12 or less, preferably 10 or less, more preferably 8 or less, and even more preferably 7 or less. * The lower limit of the value is not particularly limited, and is, for example, 3. * The value can be determined by the following formula (iii) defined in JIS Z8781-4:2013 using the above tristimulus values.
number
[0017] L * Value=0,a * Value = 0 and b* The color difference ΔE between light that satisfies the value = 0 (light with a completely neutral hue) and the above reflected light is, for example, 22 or less, preferably 18 or less, more preferably 15 or less, even more preferably 10 or less, and particularly preferably 8 or less. The lower limit of the color difference ΔE is not particularly limited, and is, for example, 3. The color difference ΔE is determined by the L * Value, a * value and b * Using the values, it can be calculated based on the following formula (iv). ΔE * ={(L * ) 2 +(a * ) 2 +(b * ) 2} 1 / 2 (iv)
[0018] The luminous reflectance Y of the reflected light (Y value of the tristimulus values) is, for example, 1.1% or less, preferably 1.0% or less, more preferably 0.9% or less, even more preferably 0.8% or less, and particularly preferably 0.7% or less. The lower limit of the luminous reflectance Y is not particularly limited, and is, for example, 0.1%. A liquid crystal panel 100 including a polarizing film with an antireflection film 15 having a luminous reflectance Y of reflected light of 1.1% or less is suitable for applications requiring good visibility, such as an in-vehicle display.
[0019] [Anti-reflective film] 2, the antireflection film 10 has a first high refractive index layer 1, a first low refractive index layer 2, a second high refractive index layer 3, and a second low refractive index layer 4 in this order in the stacking direction. The first high refractive index layer 1 is in contact with, for example, a polarizing film 20. The second low refractive index layer 4 is, for example, located closest to the viewing side among these layers.
[0020] The high refractive index layers 1 and 3 have a higher refractive index than the low refractive index layers 2 and 4, and the refractive index is, for example, in the range of 1.6 to 3.2. The refractive index of the first high refractive index layer 1 may be the same as or different from that of the second high refractive index layer 3. In this specification, unless otherwise specified, the "refractive index" refers to a value measured in accordance with the provisions of JIS K0062:1992 at a temperature of 25°C using light with a wavelength λ of 550 nm.
[0021] In a preferred embodiment of the present invention, the high refractive index layers 1 and 3 contain, for example, a binder resin and inorganic fine particles dispersed in the binder resin. The binder resin is typically a cured product of an ionizing radiation curable resin, more specifically, a cured product of an ultraviolet curable resin. The ultraviolet curable resin may be a resin containing a polymer or oligomer having a radically polymerizable substituent, such as a (meth)acrylate resin. The (meth)acrylate resin as the ultraviolet curable resin may contain, for example, a polymer or oligomer such as epoxy (meth)acrylate, polyester (meth)acrylate, acrylic (meth)acrylate, or ether (meth)acrylate. The (meth)acrylate resin may further contain a radically polymerizable monomer (precursor) in addition to the above polymer or oligomer. The molecular weight of this monomer is, for example, 200 to 700. Specific examples of this monomer include pentaerythritol triacrylate (PETA: molecular weight 298), neopentyl glycol diacrylate (NPGDA: molecular weight 212), dipentaerythritol hexaacrylate (DPHA: molecular weight 632), dipentaerythritol pentaacrylate (DPPA: molecular weight 578), and trimethylolpropane triacrylate (TMPTA: molecular weight 296). The ionizing radiation curable resin may contain an initiator as necessary. Examples of the initiator include UV radical generators (Irgacure 907, 127, 192, etc., manufactured by Ciba Specialty Chemicals) and benzoyl peroxide. The binder resin may contain other resins in addition to the cured product of the ionizing radiation curable resin. The other resins may be thermosetting resins or thermoplastic resins. Examples of the other resins include aliphatic resins (e.g., polyolefins), urethane resins, and the like.
[0022] The refractive index of the binder resin is, for example, 1.40 to 1.60. The blending amount of the binder resin is, for example, 10 parts by weight to 80 parts by weight, and preferably 20 parts by weight to 70 parts by weight, with respect to 100 parts by weight of the high refractive index layer to be formed.
[0023] The material of the inorganic fine particles is, for example, a metal oxide. Specific examples of metal oxides include zirconium oxide (zirconia) (refractive index: 2.19), aluminum oxide (refractive index: 1.56 to 2.62), titanium oxide (refractive index: 2.49 to 2.74), and silicon oxide (refractive index: 1.25 to 1.46). These metal oxides not only have low light absorption but also have a higher refractive index than organic materials such as ionizing radiation curable resins and thermoplastic resins, and are therefore suitable for adjusting the refractive index of the high refractive index layers 1 and 3. The inorganic fine particles preferably contain zirconium oxide or titanium oxide.
[0024] The refractive index of the inorganic fine particles is, for example, 1.60 or more, preferably 1.70 to 2.80, and more preferably 2.00 to 2.80. Inorganic fine particles having a refractive index of 1.60 or more are suitable for adjusting the refractive index of the high refractive index layers 1 and 3. The average particle size of the inorganic fine particles is, for example, 1 nm to 100 nm, preferably 10 nm to 80 nm, and more preferably 20 nm to 70 nm. The average particle size of the inorganic fine particles means a particle size (d50) corresponding to a volume cumulative 50% in a particle size distribution measured by, for example, a laser diffraction particle sizer.
[0025] The inorganic fine particles may not be surface-modified, but are preferably surface-modified. Surface-modified inorganic fine particles tend to disperse well in the binder resin. The surface modification is performed, for example, by applying a surface modifier to the surface of the inorganic fine particles to form a surface modifier layer. Examples of the surface modifier include coupling agents such as silane coupling agents and titanate coupling agents; and surfactants such as fatty acid surfactants. When such a surface modifier is used, the wettability between the binder resin and the inorganic fine particles is improved, and the interface between the binder resin and the inorganic fine particles tends to be stabilized.
[0026] The blending amount of the inorganic fine particles is, for example, 10 parts by weight to 90 parts by weight, more preferably 20 parts by weight to 80 parts by weight, relative to 100 parts by weight of the high refractive index layer to be formed. If the blending amount of the inorganic fine particles is within the above range, the antireflection film has sufficient mechanical properties and tends to be able to sufficiently reduce the luminous reflectance Y of reflected light.
[0027] The refractive index of the high refractive index layers 1 and 3 containing a binder resin and inorganic fine particles is, for example, 1.6 to 2.6, and preferably 1.7 to 2.2.
[0028] In another preferred embodiment of the present invention, the high refractive index layers 1 and 3 include a metal oxide or a metal nitride, and preferably consist essentially of a metal oxide or a metal nitride. Specific examples of metal oxides include titanium oxide (TiO2), indium / tin oxide (ITO), niobium oxide (Nb2O5), yttrium oxide (Y2O3), indium oxide (In2O3), tin oxide (SnO2), zirconium oxide (ZrO2), hafnium oxide (HfO2), antimony oxide (Sb2O3), tantalum oxide (Ta2O5), zinc oxide (ZnO), and tungsten oxide (WO3). Specific examples of metal nitrides include silicon nitride (Si3N4). The high refractive index layers 1 and 3 preferably include niobium oxide (Nb2O5) or titanium oxide (TiO2). The refractive index of the high refractive index layer made of a metal oxide or a metal nitride is, for example, 2.00 to 2.60, and preferably 2.10 to 2.45.
[0029] The material of the first high refractive index layer 1 may be the same as that of the second high refractive index layer 3, or may be different.
[0030] The physical thickness of the first high refractive index layer 1 is, for example, 9 nm to 15 nm, and preferably 11 nm to 13 nm. The optical thickness of the first high refractive index layer 1 is, for example, 20 nm to 35 nm, and preferably 25 nm to 30 nm. In this specification, the optical thickness is a value represented by the product of the refractive index of light with a wavelength of 550 nm and the physical thickness.
[0031] The second high refractive index layer 3 has a physical thickness of, for example, 98 nm to 124 nm, and preferably 111 nm to 120 nm. The second high refractive index layer 3 has an optical thickness of, for example, 230 nm to 290 nm, and preferably 260 nm to 280 nm.
[0032] The low refractive index layers 2 and 4 are layers having a lower refractive index than the high refractive index layers 1 and 3, and the refractive index is, for example, 1.35 to 1.55, and preferably 1.40 to 1.50. There is a tendency that light reflection can be suppressed by appropriately adjusting the difference in refractive index between the low refractive index layers 2 and 4 and the high refractive index layers 1 and 3. The refractive index of the first low refractive index layer 2 may be the same as or different from that of the second low refractive index layer 4.
[0033] Examples of materials for the low refractive index layers 2 and 4 include metal oxides and metal fluorides. A specific example of a metal oxide is silicon oxide (SiO2). Specific examples of metal fluorides are magnesium fluoride and fluorosilicic acid. From the viewpoint of refractive index, the materials for the low refractive index layers 2 and 4 are preferably magnesium fluoride and fluorosilicic acid, and from the viewpoints of ease of manufacture, mechanical strength, moisture resistance, and the like, silicon oxide is preferred, and taking various properties into consideration overall, silicon oxide is preferred. The material for the first low refractive index layer 2 may be the same as that for the second low refractive index layer 4, or may be different.
[0034] The material of the low refractive index layers 2 and 4 may be a cured product of a curable fluorine-containing resin. The curable fluorine-containing resin has, for example, a structural unit derived from a fluorine-containing monomer and a structural unit derived from a crosslinkable monomer. Specific examples of the fluorine-containing monomer include fluoroolefins (fluoroethylene, vinylidene fluoride, tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoro-2,2-dimethyl-1,3-dioxole, etc.), (meth)acrylic acid ester derivatives having a partially or completely fluorinated alkyl group (Viscoat 6FM (manufactured by Osaka Organic Chemical Industry Co., Ltd.), M-2020 (manufactured by Daikin Industries, Ltd.), etc.), and completely or partially fluorinated vinyl ethers. Examples of the crosslinkable monomer include (meth)acrylate monomers having a crosslinkable functional group in the molecule, such as glycidyl methacrylate, and (meth)acrylate monomers having a functional group, such as a carboxyl group, a hydroxyl group, an amino group, or a sulfonic acid group ((meth)acrylic acid, methylol (meth)acrylate, hydroxyalkyl (meth)acrylate, allyl (meth)acrylate, etc.). The fluorine-containing resin may have a constituent unit derived from a monomer other than the above-mentioned compounds (for example, an olefin-based monomer, a (meth)acrylate-based monomer, or a styrene-based monomer).
[0035] The first low refractive index layer 2 has a physical thickness of, for example, 26 nm to 34 nm, and preferably 27 nm to 31 nm. The first low refractive index layer 2 has an optical thickness of, for example, 38 nm to 50 nm, and preferably 40 nm to 45 nm.
[0036] The second low refractive index layer 4 has a physical thickness of, for example, 68 nm to 88 nm, and preferably 72 nm to 79 nm. The second low refractive index layer 4 has an optical thickness of, for example, 100 nm to 128 nm, and preferably 105 nm to 115 nm.
[0037] The method for producing the high refractive index layer and the low refractive index layer is not particularly limited. When these layers contain resin, they can be formed by a so-called wet process (curing after applying a resin composition). When these layers are composed of metal oxides, metal fluorides, metal nitrides, etc., they can be formed by a so-called dry process. Specific examples of the dry process include a PVD (Physical Vapor Deposition) method and a CVD (Chemical Vapor Deposition) method. Examples of the PVD method include a vacuum deposition method, a reactive deposition method, an ion beam assisted method, a sputtering method, and an ion plating method. Examples of the CVD method include a plasma CVD method. From the viewpoint of reducing the variation in the hue of the reflected light, the sputtering method is preferable as the dry process.
[0038] The antireflection film 10 in Fig. 2 may further include other members in addition to the high refractive index layer and the low refractive index layer. Fig. 3 shows another example of the antireflection film. The antireflection film 11 in Fig. 3 further includes a substrate 5 and an adhesive layer 6. The substrate 5 is disposed, for example, between the first high refractive index layer 1 and the polarizing film 20, and is in contact with the first high refractive index layer 1. The adhesive layer 6 is disposed, for example, between the substrate 5 and the polarizing film 20, and is in contact with both the substrate 5 and the polarizing film 20.
[0039] The substrate 5 includes, for example, a resin film having transparency. Examples of materials for such resin films include cellulose-based resins (triacetyl cellulose, diacetyl cellulose, propionyl cellulose, butyryl cellulose, acetylpropionyl cellulose, nitrocellulose, etc.), polyamide-based resins (nylon-6, nylon-66, etc.), polyimide-based resins, polycarbonate-based resins, polyester-based resins (polyethylene terephthalate, polyethylene naphthalate, poly-1,4-cyclohexanedimethylene terephthalate, polyethylene-1,2-diphenoxyethane-4,4'-dicarboxylate, polybutylene terephthalate, etc.), polyolefin-based resins (polyethylene, polypropylene, polymethylpentene, etc.), polysulfone-based resins, polyethersulfone-based resins, polyarylate-based resins, polyetherimide-based resins, polymethylmethacrylate-based resins, polyetherketone-based resins, polystyrene resins, polyvinyl chloride resins, polyvinyl alcohol resins, ethylene vinyl alcohol resins, (meth)acrylic resins, and (meth)acrylonitrile resins. The substrate 5 may be a single resin film layer, a laminate of a plurality of resin films, or a laminate of a resin film and a hard coat layer described later. The substrate 5 may contain an additive. Specific examples of the additive include an antistatic agent, an ultraviolet absorbing agent, a plasticizer, a lubricant, a colorant, an antioxidant, and a flame retardant.
[0040] In a preferred embodiment of the present invention, the substrate 5 is a triacetyl cellulose (TAC) film. The triacetyl cellulose film can also function as a protective film for the polarizer. Therefore, by using the antireflection film 11 having the substrate 5 made of a triacetyl cellulose film, the transparent protective film that the polarizing film 20 has on the viewing side can be omitted in some cases.
[0041] In another preferred embodiment of the present invention, the substrate 5 includes a hard coat layer. The substrate 5 may be composed of a hard coat layer, or may be a laminate of a resin film and a hard coat layer. The hard coat layer is, for example, a cured layer of an ionizing radiation curable resin. Examples of the ionizing radiation include ultraviolet light, visible light, infrared light, and electron beams, and preferably ultraviolet light. That is, the ionizing radiation curable resin is preferably an ultraviolet radiation curable resin. Examples of the ultraviolet radiation curable resin include (meth)acrylic resins, silicone resins, polyester resins, urethane resins, amide resins, and epoxy resins. Examples of the (meth)acrylic resin include a cured product (polymerization product) obtained by curing a polyfunctional monomer containing a (meth)acryloyloxy group with ultraviolet light. The polyfunctional monomer is used, for example, one type or a combination of two or more types. The polyfunctional monomer is used, for example, by mixing with a photopolymerization initiator.
[0042] Inorganic or organic fine particles may be dispersed in the hard coat layer. The average particle size (d50) of the fine particles is, for example, 0.01 μm to 3 μm. As the fine particles dispersed in the hard coat layer, silicon oxide (SiO2) is preferable from the viewpoints of refractive index, stability, heat resistance, etc. The hard coat layer may contain additives. Specific examples of the additives include leveling agents, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antioxidants, and thixotropic agents. Furthermore, the surface of the hard coat layer may be formed with an uneven shape. A hard coat layer having an uneven surface has a light diffusion function (anti-glare).
[0043] There is no particular limitation on the physical thickness of the substrate 5. When the substrate 5 is a single resin film layer or a laminate of multiple resin films, the physical thickness of the substrate 5 is, for example, in the range of 10 μm to 200 μm. When the substrate 5 includes a hard coat layer, the physical thickness of the hard coat layer is, for example, in the range of 1 μm to 50 μm.
[0044] The refractive index of the substrate 5 (when the substrate 5 has a laminated structure, the refractive index of the layer closest to the first high refractive index layer 1) is, for example, 1.3 to 1.8, and preferably 1.4 to 1.7.
[0045] The adhesive layer 6 is a layer containing an adhesive. The adhesive contained in the adhesive layer 6 may be, for example, a resin having adhesive properties. Examples of such resins include acrylic resins, acrylic urethane resins, urethane resins, and silicone resins. The adhesive layer 6 preferably contains an acrylic adhesive made of an acrylic resin.
[0046] The adhesive layer 6 may further contain additives as necessary. Examples of additives include crosslinking agents, tackifiers, plasticizers, pigments, dyes, fillers, antioxidants, conductive materials, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, and antioxidants. Examples of crosslinking agents include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, peroxide-based crosslinking agents, melamine-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, and amine-based crosslinking agents.
[0047] The physical thickness of the pressure-sensitive adhesive layer 6 is, for example, 5 μm to 100 μm, and preferably 10 μm to 50 μm.
[0048] The anti-reflection film 11 may further include other members in addition to the substrate 5 and the adhesive layer 6. The anti-reflection film 11 may further include an anti-glare layer disposed between the substrate 5 and the first high refractive index layer 1, for example. The anti-reflection film 11 may further include an adhesion layer disposed between specific members (for example, between the substrate 5 and the first high refractive index layer 1, or between the anti-glare layer and the first high refractive index layer 1). The adhesion layer is a layer that improves adhesion between members, and is made of, for example, silicon or SiO x (x<2) The physical thickness of the adhesive layer is, for example, 1 nm to 10 nm, and preferably 2 nm to 5 nm. The refractive index of the adhesive layer is, for example, 1 to 2.5.
[0049] The antireflection films 10 and 11 are disposed on the viewing side of the second low refractive index layer 4, and may further include an antifouling layer in contact with the second low refractive index layer 4. The antifouling layer is a layer having an antifouling effect, and contains at least one selected from, for example, a fluorine-based resin and a silicone-based resin. The physical film thickness of the antifouling layer is, for example, 5 nm to 13 nm, and preferably 5 nm to 10 nm. The refractive index of the antifouling layer is, for example, 1 to 2.
[0050] The reflected light generated when light from the CIE standard illuminant D65 is incident on the anti-reflection coatings 10 and 11 is L * a * b * A1 in color system * Value and b1 * It is preferable that the absolute value of a1 is small. * The value is, for example, −6 or more and 6 or less, more preferably −3 or more and 3 or less. * The value is, for example, from −15 to 3, preferably from −10 to 2, and more preferably from −5 to 2. * Value and b1 * The value can be specified by the following method. First, the first high refractive index layer 1, the first low refractive index layer 2, the second high refractive index layer 3, and the second low refractive index layer 4 of the antireflection film 10 are laminated in this order on a black film, or the antireflection film 11 is attached to the black film by the adhesive layer 6 of the antireflection film 11. Next, light from a CIE standard illuminant D65 is made to be incident on the surface of the antireflection film 10 or 11 on the second low refractive index layer side at an incident angle of 5°. The specular reflectance in the wavelength range of 360 nm to 740 nm generated at this time is specified, and the tristimulus values in the XYZ color system are specified from the spectral reflectance. Using the obtained tristimulus values, the a1 is calculated by the above-mentioned formulas (i) and (ii). * Value and b1 * Identify the value.
[0051] The luminous reflectance Y1 of the reflected light is, for example, 0.3% or less, and preferably 0.2% or less.
[0052] [Polarizing film] The polarizing film 20 is a laminate including a polarizer and a transparent protective film. The transparent protective film is disposed, for example, in contact with the main surface (the surface having the widest area) of the layered polarizer. The polarizer may be disposed between two transparent protective films. The polarizer is not particularly limited, and examples thereof include a hydrophilic polymer film such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or an ethylene-vinyl acetate copolymer partially saponified film, which is uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye; a polyene-based oriented film such as a dehydrated product of polyvinyl alcohol or a dehydrochlorinated product of polyvinyl chloride; and the like. The polarizer is preferably made of a polyvinyl alcohol film and a dichroic substance such as iodine.
[0053] The thickness of the polarizer is not particularly limited and is, for example, 80 μm or less. The thickness of the polarizer may be 10 μm or less, preferably 1 to 7 μm. Such a thin polarizer has less thickness unevenness and is excellent in visibility. The thin polarizer is suppressed in dimensional change and is excellent in durability. The thin polarizer allows the polarizing film 20 to be made thinner.
[0054] As the material of the transparent protective film, for example, a thermoplastic resin excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc. is used. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The material of the transparent protective film may be a thermosetting resin or an ultraviolet-curing resin such as a (meth)acrylic, urethane, acrylic urethane, epoxy, or silicone-based resin. When the polarizing film 20 has two transparent protective films, the materials of the two transparent protective films may be the same as or different from each other. For example, a transparent protective film made of a thermoplastic resin may be attached to one main surface of the polarizer via an adhesive, and a transparent protective film made of a thermosetting resin or an ultraviolet-curing resin may be attached to the other main surface of the polarizer. The transparent protective film may contain one or more optional additives.
[0055] The transparent protective film may have optical properties such as anti-glare properties and anti-reflection properties. The transparent protective film may be a film that functions as a retardation film. In this specification, the retardation film means a film having birefringence in the in-plane direction or the thickness direction. Examples of films that function as retardation films include those obtained by stretching a polymer film and those obtained by aligning and fixing a liquid crystal material.
[0056] The adhesive for bonding the polarizer and the transparent protective film is not particularly limited as long as it is optically transparent, and examples thereof include aqueous, solvent-based, hot-melt, radical-curing, and cationic-curing adhesives, preferably aqueous adhesives and radical-curing adhesives.
[0057] The thickness of the polarizing film 20 is, for example, 10 μm to 500 μm. The total light transmittance of the polarizing film 20 is not particularly limited, and is, for example, 30% to 50%. In this specification, "total light transmittance" means the transmittance of light having a wavelength in the range of 380 nm to 700 nm. The total light transmittance can be measured in accordance with the provisions of JIS K7361-1:1997. The CIE standard illuminant D65 is used to measure the total light transmittance.
[0058] When light from a CIE standard illuminant D65 is incident on the polarizing film 20, the a value of the transmitted light in the Hunter Lab color system is preferably -6.0 to 0, more preferably -3.0 to -0.5, and particularly preferably -1.8 to -1.2. The b value of the transmitted light in the Hunter Lab color system is preferably 1.0 to 10, more preferably 1.5 to 5.0, and particularly preferably 2.2 to 4.0. The a value and b value of the transmitted light in the Hunter Lab color system can be determined by the following method. First, the transmittance of the light from a CIE standard illuminant D65 in the polarizing film 20 is measured using an integrating sphere of a spectrophotometer. The obtained transmittance is subjected to luminosity correction (780 to 380 nm: every 5 nm) using the 2-degree visual field XYZ system specified in JIS Z8701:1999, so that the a value and b value of the transmitted light in the Hunter Lab color system can be determined.
[0059] [Adhesive layer] The adhesive layer 30 is a layer containing an adhesive. Examples of the adhesive contained in the adhesive layer 30 include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. The adhesive contained in the adhesive layer 30 is preferably an acrylic-based adhesive, since it has excellent optical transparency, appropriate adhesive properties such as wettability, cohesiveness, and adhesion, and excellent weather resistance, heat resistance, and the like.
[0060] The acrylic pressure-sensitive adhesive contains a (meth)acrylic polymer as a base polymer. The (meth)acrylic polymer contains, for example, a structural unit derived from a (meth)acrylic acid ester as a main component. In this specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid. "Main component" means a structural unit contained in the polymer in the largest amount by weight.
[0061] The number of carbon atoms in the ester moiety (other than the (meth)acrylic acid group) contained in the (meth)acrylic acid ester for forming the main skeleton of the (meth)acrylic polymer is not particularly limited, and is, for example, 1 to 18. The ester moiety of the (meth)acrylic acid ester may contain an aromatic ring such as a phenyl group or a phenoxy group, and may contain an alkyl group. This alkyl group may be linear or branched. The (meth)acrylic polymer may contain one or more structural units derived from a (meth)acrylic acid ester. In the (meth)acrylic polymer, the average number of carbon atoms in the ester moiety contained in the structural unit derived from the (meth)acrylic acid ester is preferably 3 to 9. From the viewpoints of adhesive properties, durability, adjustment of retardation, adjustment of refractive index, etc., the (meth)acrylic polymer preferably has a structural unit derived from a (meth)acrylic acid ester containing an aromatic ring. By adjusting the retardation of the adhesive layer 30 with the (meth)acrylic acid ester containing an aromatic ring, it is possible to suppress light leakage of a liquid crystal display device caused by thermal shrinkage of the polarizing film 20 and stretching of the adhesive layer 30. Furthermore, this (meth)acrylic acid ester is suitable for adjusting the refractive index of the adhesive layer 30 and reducing the difference in refractive index between the adhesive layer 30 and the adherend (liquid crystal cell). If the difference in refractive index is reduced, the reflection of light at the interface between the adhesive layer 30 and the adherend can be suppressed, and the visibility of the display can be improved.
[0062] Examples of the (meth)acrylic acid ester containing an aromatic ring include benzyl (meth)acrylate, phenyl (meth)acrylate, o-phenylphenol (meth)acrylate, phenoxy (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypropyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, ethylene oxide-modified cresol (meth)acrylate, phenol ethylene oxide-modified (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, and the like. Examples of the acrylic acid esters include (meth)acrylic acid esters containing a benzene ring, such as methoxybenzyl (meth)acrylate, methoxybenzyl (meth)acrylate, chlorobenzyl (meth)acrylate, cresyl (meth)acrylate, and styryl (meth)acrylate; (meth)acrylic acid esters containing a naphthalene ring, such as hydroxyethylated β-naphthol acrylate, 2-naphthoethyl (meth)acrylate, 2-naphthoxyethyl acrylate, and 2-(4-methoxy-1-naphthoxy)ethyl (meth)acrylate; and (meth)acrylic acid esters containing a biphenyl ring, such as biphenyl (meth)acrylate. Among these, benzyl (meth)acrylate and phenoxyethyl (meth)acrylate are preferred from the viewpoint of improving the adhesive properties and durability of the adhesive layer 30.
[0063] When the refractive index of the adhesive layer 30 is adjusted by the (meth)acrylic acid ester containing an aromatic ring, the content of the structural unit derived from the (meth)acrylic acid ester containing an aromatic ring in all the structural units of the (meth)acrylic polymer is preferably 3% by weight to 25% by weight. This content is more preferably 22% by weight or less, and even more preferably 20% by weight or less. This content is more preferably 8% by weight or more, and even more preferably 12% by weight or more. If the content of the structural unit derived from the (meth)acrylic acid ester containing an aromatic ring is 25% by weight or less, light leakage from the liquid crystal display device due to shrinkage of the polarizing film 20 can be suppressed, and the reworkability of the adhesive layer 30 tends to be improved. If this content is 3% by weight or more, light leakage from the liquid crystal display device tends to be sufficiently suppressed.
[0064] From the viewpoint of improving adhesiveness and heat resistance, the (meth)acrylic polymer may have at least one structural unit derived from a copolymerization monomer having a polymerizable functional group containing an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group, in addition to the structural unit derived from the (meth)acrylic acid ester containing an aromatic ring as described above. Examples of the copolymerization monomer include hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl acrylate; (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, and the like. carboxyl group-containing monomers such as acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; caprolactone adducts of acrylic acid; sulfonic acid group-containing monomers such as styrenesulfonic acid, allylsulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; and phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate.
[0065] Examples of the copolymerizable monomer include (N-substituted) amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; (meth)acrylic acid alkylaminoalkyl ester monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; (meth)acrylic acid alkoxyalkyl monomers such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate; and N-(meth)acryloyloxymethylene succinyloxymethylene ether monomers. and succinimide-based monomers such as N-(meth)acryloyl-6-oxyhexamethylenesuccinimide and N-(meth)acryloyl-8-oxyoctamethylenesuccinimide; morpholine-based monomers such as N-acryloylmorpholine; maleimide-based monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide and N-phenylmaleimide; and itaconimide-based monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide and N-laurylitaconimide.
[0066] Examples of the copolymerization monomer include vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; and acrylic ester monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, silicone (meth)acrylate, and 2-methoxyethyl acrylate. Further, examples of copolymerizable monomers include olefin monomers such as isoprene, butadiene, and isobutylene; and ether group-containing vinyl monomers such as vinyl ethers.
[0067] Examples of the copolymerizable monomer include silane-based monomers such as 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, and 10-acryloyloxydecyltriethoxysilane.
[0068] Examples of the copolymerizable monomer include tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol Also usable are esters of (meth)acrylic acid and polyhydric alcohols (polyfunctional monomers having two or more unsaturated double bonds such as (meth)acryloyl groups, vinyl groups, etc.), such as dipentaerythritol hexa(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate; and compounds in which two or more compounds having unsaturated double bonds such as (meth)acryloyl groups, vinyl groups, etc. are added to a backbone of polyester, epoxy, urethane, etc. (for example, polyester (meth)acrylate, epoxy (meth)acrylate, and urethane (meth)acrylate).
[0069] The content of the structural units derived from the above-mentioned copolymerization monomers in the (meth)acrylic polymer is not particularly limited and is, for example, 0 wt% to 20 wt%, preferably 0.1 wt% to 15 wt%, and more preferably 0.1 wt% to 10 wt%.
[0070] As the copolymerization monomer, from the viewpoint of adhesion and durability, a hydroxyl group-containing monomer and a carboxyl group-containing monomer are preferred. As the copolymerization monomer, a hydroxyl group-containing monomer and a carboxyl group-containing monomer may be used in combination. For example, when the adhesive composition for forming the adhesive layer 30 contains a crosslinking agent, the copolymerization monomer functions as a reaction site with the crosslinking agent. Hydroxyl group-containing monomers, carboxyl group-containing monomers, etc. have excellent reactivity with an intermolecular crosslinking agent, and are therefore suitable for improving the cohesiveness and heat resistance of the resulting adhesive layer 30. In particular, the hydroxyl group-containing monomer is suitable for improving the reworkability of the adhesive layer 30. The carboxyl group-containing monomer is suitable for achieving both durability and reworkability of the adhesive layer 30.
[0071] When a hydroxyl group-containing monomer is used as the copolymerization monomer, the content of the structural unit derived from the hydroxyl group-containing monomer in the (meth)acrylic polymer is preferably 0.01 wt% to 15 wt%, more preferably 0.03 wt% to 10 wt%, and even more preferably 0.05 wt% to 7 wt%. When a carboxyl group-containing monomer is used as the copolymerization monomer, the content of the structural unit derived from the carboxyl group-containing monomer in the (meth)acrylic polymer is preferably 0.05 wt% to 10 wt%, more preferably 0.1 wt% to 8 wt%, and even more preferably 0.2 wt% to 6 wt%.
[0072] The weight average molecular weight of the (meth)acrylic polymer is, for example, 500,000 to 3,000,000, and from the viewpoint of durability, particularly heat resistance, it is preferably 700,000 to 2,700,000, and more preferably 800,000 to 2,500,000. When the weight average molecular weight of the (meth)acrylic polymer is 500,000 or more, the pressure-sensitive adhesive layer 30 tends to have sufficient heat resistance for practical use. When the weight average molecular weight of the (meth)acrylic polymer is 3,000,000 or less, the viscosity of the coating liquid for producing the pressure-sensitive adhesive layer 30 tends to be easily adjustable. If the viscosity of the coating liquid can be easily adjusted, it is not necessary to add a large amount of dilution solvent to the coating liquid, so that the manufacturing cost of the pressure-sensitive adhesive layer 30 can be reduced. In this specification, the weight average molecular weight refers to a value obtained by converting the measurement result by GPC (gel permeation chromatography) into polystyrene.
[0073] The (meth)acrylic polymer can be produced by known polymerization reactions such as solution polymerization, bulk polymerization, emulsion polymerization, various radical polymerizations, etc. The (meth)acrylic polymer may be a random copolymer, a block copolymer, or a graft copolymer.
[0074] The adhesive contained in the adhesive layer 30 may have a structure in which a base polymer is crosslinked by a crosslinking agent. For example, when a (meth)acrylic polymer is used as the base polymer, an organic crosslinking agent or a polyfunctional metal chelate can be used as the crosslinking agent. Examples of organic crosslinking agents include isocyanate crosslinking agents, peroxide crosslinking agents, epoxy crosslinking agents, and imine crosslinking agents. The polyfunctional metal chelate means a compound in which a polyvalent metal is covalently bonded or coordinately bonded to an organic compound. Examples of atoms constituting a polyvalent metal include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, and Ti. The organic compound contained in the polyfunctional metal chelate includes, for example, an oxygen atom. Examples of the organic compound include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds.
[0075] In the pressure-sensitive adhesive, the amount of the crosslinking agent used is preferably 3 parts by weight or less, more preferably 0.01 to 3 parts by weight, further preferably 0.02 to 2 parts by weight, and particularly preferably 0.03 to 1 part by weight, based on 100 parts by weight of the (meth)acrylic polymer.
[0076] The adhesive layer 30 may further contain other materials besides the adhesive. Examples of the other materials include conductive materials, silane coupling agents, and other additives. The conductive material is suitable for reducing the surface resistivity of the adhesive layer 30 and preventing display defects due to charging of the liquid crystal display device. Examples of the conductive material include those used in the conductive layer described below. The conductive material contained in the adhesive layer 30 is preferably an ionic compound from the viewpoints of compatibility with the base polymer and transparency of the adhesive layer 30. In particular, when the adhesive layer 30 contains an acrylic adhesive containing a (meth)acrylic polymer as a base polymer, it is preferable to use an ionic compound as the conductive material. The ionic compound is preferably an ionic liquid from the viewpoint of antistatic performance.
[0077] The adhesive layer 30 preferably contains 0.05 to 20 parts by weight of a conductive material (e.g., an ionic compound) relative to 100 parts by weight of a base polymer of the adhesive (e.g., a (meth)acrylic polymer). When the adhesive layer 30 contains 0.05 parts by weight or more of a conductive material, the surface resistivity of the adhesive layer 30 is sufficiently reduced, and the antistatic performance of the adhesive layer 30 tends to be sufficiently improved. The adhesive layer 30 preferably contains 0.1 parts by weight or more of a conductive material relative to 100 parts by weight of a base polymer of the adhesive, and more preferably contains 0.5 parts by weight or more. From the viewpoint of imparting sufficient durability for practical use to the adhesive layer 30, the adhesive layer 30 preferably contains 20 parts by weight or less of a conductive material relative to 100 parts by weight of a base polymer of the adhesive, and more preferably contains 10 parts by weight or less.
[0078] Other additives include, for example, polyether compounds such as polyalkylene glycol (e.g., polypropylene glycol), colorants, pigments, dyes, surfactants, plasticizers, tackifiers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, inorganic fillers, organic fillers, metal powders, etc., which can be used appropriately depending on the application. The additives may be in the form of powder, particles, or foil. A redox system may be formed by using a reducing agent as an additive within a controllable range. The hue of the reflected light from the liquid crystal panel 100 may be adjusted by adding a pigment such as a colorant to the adhesive layer 30. The adhesive layer 30 preferably contains 5 parts by weight or less of other additives relative to 100 parts by weight of the base polymer (e.g., (meth)acrylic polymer) of the adhesive, more preferably 3 parts by weight or less, and even more preferably 1 part by weight or less.
[0079] The thickness of the pressure-sensitive adhesive layer 30 is not particularly limited and is, for example, 5 to 100 μm, and preferably 10 to 50 μm.
[0080] In the anti-reflection coated polarizing film 15, the surface resistivity of the pressure-sensitive adhesive layer 30 is not particularly limited, but is preferably 1.0×10 14 It may be less than 1.0×10 12 The lower limit of the surface resistivity of the pressure-sensitive adhesive layer 30 is not particularly limited, but from the viewpoint of durability, it is preferably, for example, 1.0×10 8The surface resistivity of the adhesive layer 30 is Ω / □. The surface resistivity of the adhesive layer 30 can be measured by the following method. First, a laminate in which the surface of the adhesive layer 30 is exposed to the outside is prepared. An example of such a laminate is a laminate in which the adhesive layer 30 is disposed on a separator film such as a polyethylene terephthalate film. Next, the surface resistivity of the surface of the adhesive layer 30 in the prepared laminate is measured. The surface resistivity can be measured using a Hiresta-UP MCP-HT450 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) in accordance with the method specified in JIS K6911:1995. The measured value obtained by this measurement can be regarded as the surface resistivity of the adhesive layer 30.
[0081] [Other layers] The antireflection-coated polarizing film 15 may further include layers other than the antireflection film 10, the polarizing film 20, and the pressure-sensitive adhesive layer 30. The antireflection-coated polarizing film 15 may include one or more other layers. The other layers are, for example, disposed closer to the viewing side than the antireflection film 10 and in contact with the antireflection film 10. Examples of the other layers include a surface protective film and a retardation film.
[0082] The surface protective film has, for example, a support film and an adhesive layer disposed on at least one side of the support film. The adhesive layer of the surface protective film may contain a light release agent, a conductive material, etc. When the adhesive layer of the surface protective film contains a conductive material, the surface protective film is attached to the anti-reflective film 10, and then the surface protective film is peeled off, so that the conductive material is contained in the anti-reflective film 10 and the conductive function can be imparted to the surface. Examples of the conductive material include those used in the conductive layer described below. In order to impart a conductive function to the surface of the anti-reflective film 10 by peeling off the surface protective film, it is preferable that the adhesive layer of the surface protective film contains a light release agent together with the conductive material. Examples of the light release agent include silicone resins such as polyorganosiloxane. The conductive function imparted to the surface of the anti-reflective film 10 can be appropriately adjusted by the amount of the conductive material and the light release agent used.
[0083] The other layer may include an easy-adhesion layer for improving adhesion between members. When the other layer is an easy-adhesion layer, the easy-adhesion layer may be disposed on the surface of the polarizing film 20. Instead of the easy-adhesion layer, the surface of the polarizing film 20 may be subjected to an easy-adhesion treatment such as a corona treatment or a plasma treatment.
[0084] [Liquid crystal cell] The liquid crystal cell 25 includes, for example, a liquid crystal layer 50, a first transparent substrate 60, and a second transparent substrate 70. The liquid crystal layer 50 is, for example, disposed between the first transparent substrate 60 and the second transparent substrate 70, and is in contact with each of the first transparent substrate 60 and the second transparent substrate 70. The pressure-sensitive adhesive layer 30 of the anti-reflection coated polarizing film 15 is in contact with, for example, the first transparent substrate 60 of the liquid crystal cell 25. The liquid crystal panel 100 does not have, for example, an ITO layer between the pressure-sensitive adhesive layer 30 and the first transparent substrate 60.
[0085] The liquid crystal layer 50 includes, for example, liquid crystal molecules that are homogeneously aligned in the absence of an electric field. The liquid crystal layer 50 including such liquid crystal molecules is suitable for an IPS (In-Plane-Switching) mode. However, the liquid crystal layer 50 may also be used for a TN (Twisted Nematic) type, an STN (Super Twisted Nematic) type, a π type, a VA (Vertical Alignment) type, or the like. The thickness of the liquid crystal layer 50 is, for example, 1.5 μm to 4 μm.
[0086] Examples of materials for the first transparent substrate 60 and the second transparent substrate 70 include glass and polymer. In this specification, a transparent substrate made of a polymer may be referred to as a polymer film. Examples of polymers constituting a transparent substrate include polyethylene terephthalate, polycycloolefin, and polycarbonate. A transparent substrate made of glass has a thickness of, for example, 0.1 mm to 1 mm. A transparent substrate made of a polymer has a thickness of, for example, 10 μm to 200 μm.
[0087] The liquid crystal cell 25 may further include layers other than the liquid crystal layer 50, the first transparent substrate 60, and the second transparent substrate 70. Examples of the other layers include a color filter, an easy-adhesion layer, and a hard coat layer. The color filter is, for example, disposed on the viewing side of the liquid crystal layer 50, and is preferably located between the first transparent substrate 60 and the pressure-sensitive adhesive layer 30 of the anti-reflection coated polarizing film 15. The easy-adhesion layer and the hard coat layer are, for example, disposed on the surface of the first transparent substrate 60 or the second transparent substrate 70.
[0088] [Other parts] The liquid crystal panel 100 may further include other components in addition to the anti-reflection coated polarizing film 15 and the liquid crystal cell 25. For example, the liquid crystal panel 100 may further include a conductive structure (not shown) electrically connected to the side surface of the anti-reflection coated polarizing film 15. If the conductive structure is connected to earth, it is easy to prevent the anti-reflection coated polarizing film 15 from being charged with static electricity. The conductive structure may cover the entire side surface of the anti-reflection coated polarizing film 15, or may cover only a part of the side surface of the anti-reflection coated polarizing film 15. The ratio of the area of the side surface of the anti-reflection coated polarizing film 15 covered by the conductive structure to the area of the entire side surface of the anti-reflection coated polarizing film 15 is, for example, 1% or more, and preferably 3% or more.
[0089] Examples of materials for the conductive structure include conductive pastes made of metals such as silver and gold, conductive adhesives, and other conductive materials. The conductive structure may be wiring extending from the side surface of the anti-reflection coated polarizing film 15.
[0090] The liquid crystal panel 100 may further include other optical films in addition to the polarizing film 20. Examples of the other optical films include films used in liquid crystal display devices, such as polarizing films, reflectors, anti-transmitting films, retardation films, viewing angle compensation films, and brightness enhancement films. Retardation films include, for example, ½ wavelength plates and ¼ wavelength plates. The liquid crystal panel 100 may include one or more of these other optical films.
[0091] When the other optical film is a polarizing film, the polarizing film is bonded to the second transparent substrate 70 of the liquid crystal cell 25, for example, via an adhesive layer. This polarizing film has, for example, the configuration described above for the polarizing film 20. In the polarizing film as the other optical film, the transmission axis (or absorption axis) of the polarizer is, for example, perpendicular to the transmission axis (or absorption axis) of the polarizer in the polarizing film 20. As the material of the adhesive layer for bonding the polarizing film and the second transparent substrate 70, the materials described above for the adhesive layer 30 can be used. The thickness of this adhesive layer is not particularly limited and is, for example, 1 to 100 μm, preferably 2 to 50 μm, more preferably 2 to 40 μm, and further preferably 5 to 35 μm.
[0092] The liquid crystal panel 100 of this embodiment includes the anti-reflection-coated polarizing film 15, so that the hue of the reflected light from the liquid crystal panel 100 can be adjusted to a neutral hue. Furthermore, the present inventors have newly discovered that the reflection of light in the liquid crystal panel 100 can be significantly suppressed by adopting a configuration in which no conductive layer such as an ITO layer is provided between the anti-reflection-coated polarizing film 15 and the liquid crystal cell 25. The liquid crystal panel 100 is suitable for applications requiring good visibility, particularly for in-vehicle displays. Examples of in-vehicle displays include panels for car navigation devices, cluster panels, and mirror displays. The cluster panel is a panel that displays the vehicle's running speed, engine RPM, and the like.
[0093] (Modification of liquid crystal panel) The anti-reflection coated polarizing film 15 included in the liquid crystal panel 100 may further include other members in addition to the above-mentioned members. As shown in FIG. 4, in the liquid crystal panel 110 according to this modification, the anti-reflection coated polarizing film 16 further includes a transparent substrate 40 and an adhesive layer 45 disposed between the anti-reflection film 10 and the polarizing film 20. Except for the transparent substrate 40 and the adhesive layer 45, the structure of the liquid crystal panel 110 is the same as that of the liquid crystal panel 100. Therefore, the same reference symbols are used for elements common to the liquid crystal panel 100 and the liquid crystal panel 110 of the modification, and their description may be omitted. That is, the description of each of the following embodiments is applicable to each other as long as there is no technical contradiction. The following embodiments may be combined with each other as long as there is no technical contradiction.
[0094] The transparent substrate 40 is in contact with, for example, the first high refractive index layer 1 of the antireflection coating 10. However, the antireflection coated polarizing film 16 may have the antireflection coating 11 described in FIG. 3 instead of the antireflection coating 10. In this case, the adhesive layer 6 of the antireflection coating 11 is in contact with the transparent substrate 40. The adhesive layer 45 is disposed, for example, between the transparent substrate 40 and the polarizing film 20, and is in contact with both the transparent substrate 40 and the polarizing film 20.
[0095] The transparent substrate 40 may be any of the first transparent substrate 60 and the second transparent substrate 70 described above, and is preferably made of glass. In this specification, the transparent substrate 40 made of glass may be referred to as a "cover glass."
[0096] The adhesive layer 45 may be any of those described above for the adhesive layer 30. In particular, the adhesive layer 45 preferably contains a commercially available optically clear adhesive (OCA). The adhesive layer 45 may be formed using an adhesive tape such as LUCIACS (registered trademark) CS9621T.
[0097] (Another variation of the liquid crystal panel) 5, in a liquid crystal panel 120 according to this modification, the antireflection-coated polarizing film 17 further includes a conductive layer 46 disposed between the polarizing film 20 and the adhesive layer 30. The conductive layer 46 is in contact with both the polarizing film 20 and the adhesive layer 30.
[0098] The conductive layer 46 is a layer containing a conductive material. The conductive material may be a material other than ITO, such as a conductive polymer, a complex of a conductive polymer and a dopant, an ionic surfactant, conductive fine particles, an ionic compound, or the like. The conductive layer 46 preferably contains a conductive polymer in terms of transparency, total light transmittance, appearance, antistatic effect, and stability of the antistatic effect under high temperature or humid environment. When the conductive layer 46 contains a conductive polymer as a conductive material, haze is less likely to occur even if the thickness of the conductive layer 46 is adjusted to a relatively large value, compared to when the conductive layer 46 contains conductive fine particles. Therefore, even when the conductive layer 46 is disposed between the liquid crystal cell 25 and the polarizer, the conductive layer 46 containing a conductive polymer is less likely to cause depolarization and is less likely to reduce the contrast of the image displayed by the liquid crystal display device. When the conductive layer 46 contains a conductive polymer as a conductive material, the refractive index of the conductive layer 46 tends to be lower than when the conductive fine particles are included. Therefore, the conductive layer 46 containing a conductive polymer is suitable for further reducing the light reflectance of the liquid crystal panel 120.
[0099] Examples of the conductive polymer include polythiophene, polyaniline, polypyrrole, polyquinoxaline, polyacetylene, polyphenylenevinylene, polynaphthalene, and derivatives thereof. The conductive material may contain one or more of these conductive polymers. As the conductive polymer, polythiophene, polyaniline, and derivatives thereof are preferred, and polythiophene derivatives are particularly preferred. Polythiophene, polyaniline, and derivatives thereof function as conductive polymers having water-solubility or water-dispersibility, for example. When the conductive polymer is water-soluble or water-dispersible, the conductive layer 46 can be prepared using an aqueous solution or aqueous dispersion of the conductive polymer. In this case, it is not necessary to use a non-aqueous organic solvent to prepare the conductive layer 46, so that the deterioration of the polarizing film 20 and the like due to the organic solvent can be suppressed.
[0100] The conductive polymer may have a hydrophilic functional group. Examples of the hydrophilic functional group include a sulfone group, an amino group, an amide group, an imino group, a hydroxyl group, a mercapto group, a hydrazino group, a carboxyl group, a sulfate group, a phosphate group, and salts thereof (e.g., quaternary ammonium bases). When the conductive polymer has a hydrophilic functional group, the conductive polymer tends to be easily dissolved in water, or the fine particle-shaped conductive polymer tends to be easily dispersed in water.
[0101] From the viewpoint of electrical conductivity and chemical stability, the conductive polymer is preferably poly(3,4-disubstituted thiophene). Examples of poly(3,4-disubstituted thiophene) include poly(3,4-alkylenedioxythiophene) and poly(3,4-dialkoxythiophene), and poly(3,4-alkylenedioxythiophene) is preferable. Poly(3,4-alkylenedioxythiophene) has a structural unit represented by the following formula (I), for example. [ka]
[0102] In formula (I), R 1is, for example, an alkylene group having 1 to 4 carbon atoms. The alkylene group may be linear or branched. Examples of the alkylene group include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1-methyl-1,2-ethylene group, a 1-ethyl-1,2-ethylene group, a 1-methyl-1,3-propylene group, and a 2-methyl-1,3-propylene group, and preferably a methylene group, a 1,2-ethylene group, or a 1,3-propylene group, and more preferably a 1,2-ethylene group. The conductive polymer is preferably poly(3,4-ethylenedioxythiophene) (PEDOT).
[0103] The dopant may be, for example, a polyanion. When the conductive polymer is polythiophene (or a derivative thereof), the polyanion forms an ion pair with the polythiophene (or a derivative thereof), and the polythiophene (or a derivative thereof) can be stably dispersed in water. The polyanion is not particularly limited, and may be, for example, a carboxylic acid polymer such as polyacrylic acid, polymaleic acid, or polymethacrylic acid; or a sulfonic acid polymer such as polystyrene sulfonic acid, polyvinyl sulfonic acid, or polyisoprene sulfonic acid. The polyanion may be a copolymer of vinyl carboxylic acid or vinyl sulfonic acid with other monomers. Examples of the other monomers include, for example, (meth)acrylate compounds; and aromatic vinyl compounds such as styrene and vinyl naphthalene. The polyanion is particularly preferably polystyrene sulfonic acid (PSS). Examples of the complex of the conductive polymer and the dopant include, for example, a complex of poly(3,4-ethylenedioxythiophene) and polystyrene sulfonic acid (PEDOT / PSS).
[0104] Examples of ionic surfactants include cationic surfactants such as quaternary ammonium salt type, phosphonium salt type, and sulfonium salt type; anionic surfactants such as carboxylic acid type, sulfonate type, sulfate type, phosphate type, and phosphite type; amphoteric surfactants such as sulfobetaine type, alkylbetaine type, and alkylimidazolium betaine type; and nonionic surfactants such as polyhydric alcohol derivatives, β-cyclodextrin inclusion compounds, sorbitan fatty acid monoesters, sorbitan fatty acid diesters, polyalkylene oxide derivatives, and amine oxides.
[0105] Examples of the conductive fine particles include metal oxide fine particles such as tin oxide, antimony oxide, indium oxide, and zinc oxide, and tin oxide fine particles are preferred. Examples of materials for tin oxide fine particles include tin oxide, antimony-doped tin oxide, indium-doped tin oxide, aluminum-doped tin oxide, tungsten-doped tin oxide, titanium oxide-cerium oxide-tin oxide complex, and titanium oxide-tin oxide complex. The average particle diameter of the conductive fine particles is, for example, 1 to 100 nm, and preferably 2 to 50 nm. The average particle diameter of the conductive fine particles means a particle diameter (d50) corresponding to 50% cumulative volume in a particle size distribution measured by, for example, a laser diffraction particle sizer.
[0106] Examples of the ionic compound include alkali metal salts and / or organic cation-anion salts. Examples of the alkali metal salts include organic and inorganic salts of alkali metals. In this specification, the organic cation-anion salt means an organic salt containing an organic cation. The anion contained in the organic cation-anion salt may be an organic anion or an inorganic anion. The organic cation-anion salt may be called an ionic liquid or an ionic solid.
[0107] Examples of the alkali metal ion contained in the alkali metal salt include a lithium ion, a sodium ion, and a potassium ion, with the lithium ion being preferred.
[0108] Examples of anions contained in organic salts of alkali metals include CH3COO - , CF3COO - , CH3SO3 - , CF3SO3 - , (CF3SO2)3C - , C4F9SO3 - , C3F7COO - , (CF3SO2)(CF3CO)N - , - O3S(CF2)3SO3 - , (CN)2N - and anions represented by the following general formulas (a) to (d). (a) (C n F 2n+1 SO2)2N - (where n is an integer between 1 and 10) (b) CF2(C m F 2m SO2)2N - (where m is an integer between 1 and 10) (c) - O3S(CF2) l SO3 - (where l is an integer between 1 and 10) (d) (C p F 2p+1 SO2)N - (C q F 2q+1 SO2) (wherein p and q are each independently an integer from 1 to 10)
[0109] The anion contained in the organic salt of an alkali metal preferably contains a fluorine atom. The anion containing a fluorine atom allows the organic salt of an alkali metal to function as an ionic compound with excellent ion dissociation properties.
[0110] Examples of anions contained in inorganic salts of alkali metals include Cl. - , Br - , I - , AlCl4 - , Al2Cl7 - , BF4 - , PF6 - , ClO4- , NO3 - , AsF6 - , SbF6 - , NbF6 - , TaF6 - , (FSO2)2N - , CO3 2- etc.
[0111] The anion contained in the alkali metal salt is (CF3SO2)2N - , (C2F5SO2)2N - The (perfluoroalkylsulfonyl)imides represented by the above general formula (a) are preferred, and in particular, (CF3SO2)2N - Preferred is (trifluoromethanesulfonyl)imide represented by the following formula:
[0112] Examples of organic salts of alkali metals include sodium acetate, sodium alginate, sodium ligninsulfonate, sodium toluenesulfonate, LiCF3SO3, Li(CF3SO2)2N, Li(C2F5SO2)2N, Li(C4F9SO2)2N, Li(CF3SO2)3C, KO3S(CF2)3SO3K, LiO3S(CF2)3SO3K, etc., preferably LiCF3SO3, Li(CF3SO2)2N, Li(C2F5SO2)2N, Li(C4F9SO2)2N, Li(CF3SO2)3C, more preferably Li(CF3SO2)2N, Li(C2F5SO2)2N, Li(C4F9SO2)2N. The organic salt of the alkali metal is preferably a fluorine-containing lithium imide salt, and particularly preferably a (perfluoroalkylsulfonyl)imide lithium salt.
[0113] Inorganic salts of alkali metals include, for example, lithium perchlorate and lithium iodide.
[0114] Examples of the organic cation contained in the organic cation-anion salt include a pyridinium cation, a piperidinium cation, a pyrrolidinium cation, a cation having a pyrroline skeleton, a cation having a pyrrole skeleton, an imidazolium cation, a tetrahydropyrimidinium cation, a dihydropyrimidinium cation, a pyrazolium cation, a pyrazolinium cation, a tetraalkylammonium cation, a trialkylsulfonium cation, and a tetraalkylphosphonium cation.
[0115] Examples of anions contained in organic cation-anion salts include Cl. - , Br - , I - , AlCl4 - , Al2Cl7 - , BF4 - , PF6 - , ClO4 - , NO3 - , CH3COO - , CF3COO - , CH3SO3 - , CF3SO3 - , (CF3SO2)3C - , AsF6 - , SbF6 - , NbF6 - , TaF6 - , (CN)2N - , C4F9SO3 - , C3F7COO - , (CF3SO2)(CF3CO)N - , (FSO2)2N - , - O3S(CF2)3SO3 - and the anions represented by the above-mentioned general formulas (a) to (d). The anion contained in the organic cation-anion salt preferably contains a fluorine atom. When the anion contains a fluorine atom, the organic cation-anion salt functions as an ionic compound having excellent ion dissociation properties.
[0116] The ionic compound is not limited to the above-mentioned alkali metal salts and organic cation-anion salts, but may also be, for example, inorganic salts such as ammonium chloride, aluminum chloride, copper chloride, ferrous chloride, ferric chloride, ammonium sulfate, etc. The conductive material may contain one or more of the above-mentioned ionic compounds.
[0117] The conductive material is not limited to the above-mentioned materials, and examples thereof include carbon materials such as acetylene black, ketjen black, natural graphite, and artificial graphite; titanium black; homopolymers of monomers having a cationic conductive group such as a quaternary ammonium salt, an amphoteric ionic conductive group such as a betaine compound, an anionic conductive group such as a sulfonate, or a nonionic conductive group such as glycerin, or copolymers of the monomers with other monomers (e.g., polymers having ionic conductivity such as polymers having structural units derived from acrylate or methacrylate having a quaternary ammonium base); and alloys of hydrophilic polymers such as copolymers of ethylene and methacrylate with acrylic resins or the like (permanent antistatic agents).
[0118] The conductive layer 46 may further contain other materials such as a binder in addition to the conductive material. The binder tends to improve, for example, the film-forming property of the conductive material and to improve the adhesion and adhesiveness (anchoring force) of the conductive layer 46 to the polarizing film 20. Examples of the binder include oxazoline group-containing polymers, polyurethane resins, polyester resins, acrylic resins, polyether resins, cellulose resins, polyvinyl alcohol resins, epoxy resins, polyvinylpyrrolidone, polystyrene resins, polyethylene glycol, pentaerythritol, and the like, and preferably oxazoline group-containing polymers, polyurethane resins, polyester resins, and acrylic resins, and particularly preferably polyurethane resins. The conductive layer 46 may contain one or more of these binders. The content of the binder in the conductive layer 46 is, for example, 1 wt% to 90 wt%, and preferably 10 wt% to 80 wt%.
[0119] The thickness of the conductive layer 46 is, for example, 5 nm to 180 nm, preferably 150 nm, more preferably 120 nm or less, even more preferably 100 nm or less, particularly preferably 80 nm or less, and especially preferably 50 nm or less. The thickness of the conductive layer 46 may be 10 nm or more, or may be 20 nm or more.
[0120] The anti-reflection coated polarizing film 17 having the conductive layer 46 can be produced, for example, by the following method. First, a solution or dispersion of a conductive material is prepared. The solvent of the solution or dispersion is, for example, water, and may further contain a water-soluble organic solvent. Examples of the water-soluble organic solvent include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-amyl alcohol, isoamyl alcohol, sec-amyl alcohol, tert-amyl alcohol, 1-ethyl-1-propanol, 2-methyl-1-butanol, n-hexanol, and cyclohexanol.
[0121] Next, a solution or dispersion of a conductive material is applied to the surface of the polarizing film 20. The resulting coating film is dried to form a conductive layer 46 on the polarizing film 20. In this way, a laminate L consisting of the polarizing film 20 and the conductive layer 46 is obtained.
[0122] Next, an anti-reflection film 10 (or 11) is placed on the polarizing film 20 of the laminate L to prepare a laminate L1. Next, a solution containing an adhesive is prepared. This solution is applied to the surface of a separator to obtain a coating film. The separator is not particularly limited, and for example, a polyethylene terephthalate film treated with a silicone-based release agent can be used. Next, the coating film is dried to form an adhesive layer 30 on the separator. The obtained adhesive layer 30 is transferred onto the conductive layer 46 of the laminate L1 to prepare a polarizing film 17 with an anti-reflection film.
[0123] In the anti-reflection coated polarizing film 17, the surface resistivity of the conductive layer 46 is, for example, 1.0×10 6 Ω / □ or more, preferably 1.0×10 7 The upper limit of the surface resistivity of the conductive layer 46 is not particularly limited, and is, for example, 1.0×10 14 Ω / □. 1.0×10 6 The conductive layer 46 having a surface resistivity larger than Ω / □ is suitable for suppressing charging of the liquid crystal panel 120 while maintaining the touch sensitivity of the liquid crystal panel 120 when the liquid crystal panel 120 has a touch sensing function. The surface resistivity of the conductive layer 46 can be specified by the following method. First, a laminate in which the surface of the conductive layer 46 is exposed to the outside is prepared. An example of such a laminate is a laminate L consisting of a polarizing film 20 and a conductive layer 46. Next, the surface resistivity of the surface of the conductive layer 46 in the prepared laminate is measured. The surface resistivity of the conductive layer 46 can be measured using a Hiresta-UP MCP-HT450 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) in accordance with the method specified in JIS K6911:1995. The measured value obtained by this measurement can be regarded as the surface resistivity of the conductive layer 46 in the polarizing film 17 with an anti-reflection film.
[0124] In the polarizing film 17 with anti-reflection coating, the loss A of the total light transmittance due to the conductive layer 46 is, for example, 0.9% or less, preferably 0.8% or less, more preferably 0.6% or less, even more preferably 0.5% or less, particularly preferably 0.4% or less, and particularly preferably less than 0.2%. The lower limit of the loss A is not particularly limited, and is, for example, 0.01%. The loss A can be determined by the following method. First, the total light transmittance T1 of the polarizing film 20 and the total light transmittance T2 of the laminate L consisting of the polarizing film 20 and the conductive layer 46 are measured. The total light transmittance T2 of the laminate L is a value when light is incident from the polarizing film 20 side. The difference (T1-T2) between the total light transmittance T1 and the total light transmittance T2 can be determined as the loss A.
[0125] The anchoring force between the conductive layer 46 and the polarizing film 20 is, for example, 10.0 N / 25 mm or more, preferably 12.0 N / 25 mm or more, more preferably 14.0 N / 25 mm or more, and even more preferably 18.0 N / 25 mm or more. The anchoring force can be measured by the following method. First, the polarizing film 17 with antireflection film to be evaluated is cut to a width of 25 mm x length of 150 mm to prepare a test piece. Next, the entire surface of the antireflection film 10 provided on the test piece is superimposed on a stainless steel test plate via double-sided tape, and a 2 kg roller is moved back and forth once to press the two together. Next, the adhesive layer 30 provided on the test piece is superimposed on the evaluation sheet, and a 2 kg roller is moved back and forth once to press the two together. The evaluation sheet is not particularly limited as long as it has a size of 30 mm wide x 150 mm long and does not peel off from the adhesive layer 30 during the test. As the evaluation sheet, for example, an ITO film (such as 125 Tetolite OES (manufactured by Oike Kogyo Co., Ltd.) can be used. Next, using a commercially available tensile tester, while holding the evaluation sheet, the adhesive layer 30 and the conductive layer 46 are peeled off from the polarized film 20 at a peel angle of 180° and a tensile speed of 300 mm / min. The average peel force measured is determined as the anchor force between the conductive layer 46 and the polarized film 20. The above test is performed in an atmosphere of 23°C.
[0126] (Yet another modified example of the liquid crystal panel) 6, in the liquid crystal panel 130 according to this modification, the liquid crystal cell 26 further includes a touch sensing electrode unit 80 disposed between the first transparent substrate 60 and the second transparent substrate 70. The touch sensing electrode unit 80 has a touch sensor and a touch drive function. The liquid crystal panel 130 is a so-called in-cell type liquid crystal panel, and the liquid crystal cell 26 is a so-called in-cell type liquid crystal cell.
[0127] The touch sensing electrode unit 80 has, for example, a touch sensor electrode 81 and a touch drive electrode 82. The touch sensor electrode 81 means a (receiving) electrode for touch detection. The touch sensor electrode 81 and the touch drive electrode 82 can be formed independently in various patterns. For example, when the liquid crystal cell 26 is planar, the touch sensor electrode 81 and the touch drive electrode 82 can be formed independently in the X-axis direction and the Y-axis direction, respectively, in a pattern in which they intersect at right angles. In FIG. 6, in the touch sensing electrode unit 80, the touch sensor electrode 81 is disposed closer to the viewing side than the touch drive electrode 82. However, the touch drive electrode 82 may be disposed closer to the viewing side than the touch sensor electrode 81. In the touch sensing electrode unit 80, the touch sensor electrode 81 and the touch drive electrode 82 may be integrated.
[0128] 6, the touch sensing electrode unit 80 is disposed between the liquid crystal layer 50 and the first transparent substrate 60 (on the viewing side of the liquid crystal layer 50). However, the touch sensing electrode unit 80 may also be disposed between the liquid crystal layer 50 and the second transparent substrate 70 (on the lighting system side of the liquid crystal layer 50).
[0129] In the touch sensing electrode unit 80, the touch sensor electrode 81 and the touch drive electrode 82 may not be in contact with each other. For example, the touch sensor electrode 81 may be disposed between the liquid crystal layer 50 and the first transparent substrate 60, and the touch drive electrode 82 may be disposed between the liquid crystal layer 50 and the second transparent substrate 70.
[0130] The drive electrode in the touch sensing electrode unit 80 (the touch drive electrode 82, or an electrode in which the touch sensor electrode 81 and the touch drive electrode 82 are integrated) can also serve as a common electrode that controls the liquid crystal layer 50.
[0131] The touch sensor electrode 81 (capacitive sensor) and the touch drive electrode 82 constituting the touch sensing electrode unit 80, or an electrode formed by integrating these, function as a transparent conductive layer. The material of this transparent conductive layer is not particularly limited, and examples thereof include metals such as gold, silver, copper, platinum, palladium, aluminum, nickel, chromium, titanium, iron, cobalt, tin, magnesium, and tungsten, and alloys thereof. The material of the transparent conductive layer may be an oxide of a metal such as indium, tin, zinc, gallium, antimony, zirconium, and cadmium. Specific examples of this oxide include indium oxide, tin oxide, titanium oxide, cadmium oxide, and mixtures thereof. The material of the transparent conductive layer may be a metal compound such as copper iodide. The material of the transparent conductive layer is preferably indium oxide (ITO) containing tin oxide, tin oxide containing antimony, and the like, and ITO is particularly preferable. When the material of the transparent conductive layer is ITO, it is preferable that the transparent conductive layer contains 80 to 99% by weight of indium oxide and 1 to 20% by weight of tin oxide.
[0132] The electrodes constituting the touch sensing electrode unit 80 (the touch sensor electrode 81, the touch drive electrode 82, or an electrode formed by integrating these) can be formed as a transparent electrode pattern between the first transparent substrate 60 and the second transparent substrate 70 by a conventional method. This transparent electrode pattern is electrically connected to, for example, a wiring line formed at the end of the transparent substrate. The wiring line is connected to, for example, a controller IC. The transparent electrode pattern can be in any shape depending on the application, such as a comb shape, a stripe shape, or a diamond shape. The transparent electrode pattern has a thickness of, for example, 10 nm to 100 nm. The transparent electrode pattern has a width of, for example, 0.1 mm to 5 mm.
[0133] (Embodiment of Liquid Crystal Display Device) The liquid crystal display device of this embodiment includes, for example, a liquid crystal panel 100 and an illumination system. In the liquid crystal display device, liquid crystal panels 110, 120, or 130 can be used instead of the liquid crystal panel 100. In the liquid crystal display device, the liquid crystal panel 100 is disposed, for example, on the viewing side of the illumination system. The illumination system includes, for example, a backlight or a reflector, and irradiates the liquid crystal panel 100 with light. EXAMPLES
[0134] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the examples shown below. In the following, unless otherwise specified, "%" indicates "weight %", "parts" indicates "weight parts", and "thickness" indicates "physical film thickness". Unless otherwise specified, the indoor temperature and humidity are 23°C and 65% RH.
[0135] <Weight average molecular weight of (meth)acrylic polymer> In the following examples, the weight average molecular weight (Mw) of the (meth)acrylic polymer was measured by gel permeation chromatography (GPC). The Mw / Mn of the (meth)acrylic polymer was also measured in the same manner. Analytical equipment: Tosoh HLC-8120GPC Column: Tosoh G7000H XL +GMH XL +GMH XL Column size: 7.8mmφ×30cm each, total 90cm Column temperature: 40℃ ·Flow rate: 0.8mL / min ·Injection volume: 100μL Eluent: Tetrahydrofuran Detector: Differential refractometer (RI) Standard sample: polystyrene
[0136] <Adhesive layer A> First, a monomer mixture was obtained by charging 76.9 parts of butyl acrylate, 18 parts of benzyl acrylate, 5 parts of acrylic acid, and 0.1 parts of 4-hydroxybutyl acrylate into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate for 100 parts of the monomer mixture (solid content). While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at around 55°C, and the polymerization reaction was carried out for 8 hours, to prepare a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2 million and Mw / Mn=4.1.
[0137] Next, 0.45 parts of an isocyanate crosslinking agent (Coronate L, trimethylolpropane tolylene diisocyanate, manufactured by Tosoh Corporation), 0.1 parts of a peroxide crosslinking agent (Niper BMT, manufactured by Nippon Oil & Fats Corporation), and 0.2 parts of a silane coupling agent (KBM-403, γ-glycidoxypropylmethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were further blended per 100 parts of the solid content of the acrylic polymer solution to prepare a solution of an acrylic pressure-sensitive adhesive composition.
[0138] Next, the obtained solution was applied to one side of a separator (Mitsubishi Chemical Polyester Film Corporation's MRF38). The separator was a polyethylene terephthalate film treated with a silicone-based release agent. The obtained coating film was dried at 155°C for 1 minute to form a pressure-sensitive adhesive layer A on the surface of the separator. The thickness of the pressure-sensitive adhesive layer A was 20 µm.
[0139] <Adhesive layer B> First, a monomer mixture was obtained by charging 81 parts of butyl acrylate, 18 parts of benzyl acrylate, and 1 part of 4-hydroxybutyl acrylate into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate per 100 parts of the monomer mixture (solid content). While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at around 55°C, and the polymerization reaction was carried out for 8 hours, to prepare a solution of an acrylic polymer with a weight average molecular weight (Mw) of 1.8 million and Mw / Mn=3.9.
[0140] Next, 0.3 parts of a peroxide crosslinking agent (Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), 0.1 parts of an isocyanate crosslinking agent (Takenate D110N, trimethylolpropane xylylene diisocyanate, manufactured by Mitsui Takeda Chemical Co., Ltd.), 7 parts of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, manufactured by Mitsubishi Materials Corporation), and 0.2 parts of a silane coupling agent (A-100, manufactured by Midoriken Chemical Co., Ltd.) were further blended with 100 parts of the solid content of the acrylic polymer solution to prepare a solution of an acrylic adhesive composition.
[0141] Next, the obtained solution was applied to one side of a separator (Mitsubishi Chemical Polyester Film Corporation's MRF38). The separator was a polyethylene terephthalate film treated with a silicone-based release agent. The obtained coating film was dried at 155°C for 1 minute to form an adhesive layer B on the surface of the separator. The thickness of the adhesive layer B was 20 µm.
[0142] <Adhesive layer C> Adhesive layer C was produced in the same manner as adhesive layer B, except that the blending amount of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, manufactured by Mitsubishi Materials Corporation) was changed to 1 part.
[0143] <Adhesive layer D> First, a monomer mixture was obtained by charging 94.9 parts of butyl acrylate, 5 parts of acrylic acid, and 0.1 parts of 4-hydroxybutyl acrylate into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.1 parts of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts of ethyl acetate per 100 parts of the monomer mixture (solid content). While gently stirring the mixture, nitrogen gas was introduced into the flask to replace the atmosphere with nitrogen. The liquid temperature in the flask was maintained at around 55°C, and the polymerization reaction was carried out for 8 hours, to prepare a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2.1 million and Mw / Mn=4.0.
[0144] Next, 0.45 parts of an isocyanate crosslinking agent (Coronate L, trimethylolpropane tolylene diisocyanate, manufactured by Tosoh Corporation), 0.1 parts of a peroxide crosslinking agent (Niper BMT, manufactured by Nippon Oil & Fats Corporation), and 0.2 parts of a silane coupling agent (KBM-403, γ-glycidoxypropylmethoxysilane, manufactured by Shin-Etsu Chemical Co., Ltd.) were further blended per 100 parts of the solid content of the acrylic polymer solution to prepare a solution of an acrylic pressure-sensitive adhesive composition.
[0145] Next, the obtained solution was applied to one side of a separator (Mitsubishi Chemical Polyester Film Corporation's MRF38). The separator was a polyethylene terephthalate film treated with a silicone-based release agent. The obtained coating film was dried at 155°C for 1 minute to form an adhesive layer D on the surface of the separator. The thickness of the adhesive layer D was 12 µm.
[0146] <Anti-reflection film AR1> First, 50 parts by weight of an ultraviolet-curable urethane acrylate resin (manufactured by Mitsubishi Chemical Corporation, product name "UV1700TL", solids concentration 80% by weight) and 50 parts by weight of a multifunctional acrylate whose main component is pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Ltd., product name "Viscoat #300", solids concentration 100% by weight) were prepared as resins for forming the anti-glare layer. Per 100 parts by weight of the solid content of these resins, 4 parts by weight of particles containing a copolymer of (meth)acrylic acid ester and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer SSX504TNR", weight average particle size: 3.0 μm), 1.5 parts by weight of synthetic smectite (manufactured by Kunimine Kogyo Co., Ltd., trade name "Sumecton SAN") which is an organic clay as a thixotropy imparting agent, 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907"), and 0.015 parts by weight of a leveling agent (manufactured by DIC Corporation, trade name "GRANDIC PC4100", solid content concentration 10% by weight) were mixed. This mixture was diluted with a toluene / cyclopentanone mixed solvent (weight ratio 80 / 20) so that the solid content concentration was 50% by weight, and a material (coating liquid) for forming an anti-glare layer was prepared.
[0147] Next, a triacetyl cellulose (TAC) film (manufactured by Fuji Film Corporation, product name "TD60UL") was prepared. A material (coating liquid) for forming an anti-glare layer was applied to one side of this transparent plastic film (TAC film) using a bar coater to form a coating film. Next, the transparent plastic film on which the coating film was formed was heated at 80°C for 1 minute to dry the coating film. Next, the coating film was irradiated with a high-pressure mercury lamp with an integrated light quantity of 300 mJ / cm2. 2 The film was cured by irradiating it with ultraviolet light of 1000 nm. As a result, an anti-glare layer having a thickness of 8.0 μm was formed, and a TAC film with an anti-glare layer was obtained. The haze of the TAC film with the anti-glare layer was 8%.
[0148] Next, this TAC film with an anti-glare layer was introduced into a roll-to-roll sputtering deposition device, and the surface of the anti-glare layer was bombarded (plasma treatment with Ar gas) by running the film. Next, a SiO x A layer (x<2) was formed. Next, a Nb2O5 layer (first high refractive index layer) with a physical thickness of 12 nm, a SiO2 layer (first low refractive index layer) with a physical thickness of 29 nm, a Nb2O5 layer (second high refractive index layer) with a physical thickness of 116 nm, and a SiO2 layer (second low refractive index layer) with a physical thickness of 78 nm were formed in this order on the adhesive layer to produce a laminate a. When forming these oxide thin films, the amount of oxygen introduced was adjusted by plasma emission monitoring (PEM) control while the pressure inside the device was kept constant by adjusting the amount of argon introduced and exhausted.
[0149] Next, a layer (physical thickness: 9 nm) made of a fluorine-based resin was formed as an antifouling layer on the surface of the second low refractive index layer (SiO2 layer) of the laminate a. Furthermore, an adhesive layer D was transferred to the surface of the TAC film of the laminate a to prepare an antireflection film AR1.
[0150] <Anti-reflection coating AR2~AR11> Except for changing the physical thickness of each layer to the value shown in Table 1, antireflection films AR2 to AR11 were produced in the same manner as antireflection film AR1.
[0151] [Table 1]
[0152] <Polarizing film P1> First, an acrylic film was produced by the following method. 8,000 g of methyl methacrylate (MMA), 2,000 g of 2-(hydroxymethyl)methyl acrylate (MHMA), 10,000 g of 4-methyl-2-pentanone (methyl isobutyl ketone, MIBK), and 5 g of n-dodecyl mercaptan were charged into a 30 L kettle-type reactor equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen inlet tube. While introducing nitrogen into the reactor, the mixture in the reactor was heated to 105°C and refluxed. Next, 5.0 g of t-butylperoxyisopropyl carbonate (Kayacarvon BIC-7, manufactured by Kayaku Akzo Co., Ltd.) was added as a polymerization initiator, and a solution consisting of 10.0 g of t-butylperoxyisopropyl carbonate and 230 g of MIBK was dropped over 4 hours to perform solution polymerization. The solution polymerization was performed under reflux at about 105 to 120°C. After the solution was added dropwise, the mixture was aged for an additional 4 hours.
[0153] Next, 30 g of a stearyl phosphate / distearyl phosphate mixture (Phoslex A-18, Sakai Chemical Industry Co., Ltd.) was added to the obtained polymer solution, and a cyclization condensation reaction was carried out at about 90 to 120 ° C. for 5 hours under reflux. Next, the obtained solution was introduced into a vent-type screw twin-screw extruder (φ = 29.75 mm, L / D = 30) with a barrel temperature of 260 ° C., a rotation speed of 100 rpm, a vacuum degree of 13.3 to 400 hPa (10 to 300 mmHg), one rear vent, and four fore vents at a processing rate of 2.0 kg / h in terms of resin amount. In the extruder, further cyclization condensation reaction and devolatilization proceeded. As a result, transparent pellets of a lactone ring-containing polymer were obtained.
[0154] The lactone ring-containing polymer thus obtained was subjected to dynamic TG measurement, and a mass loss of 0.17% by mass was detected. The lactone ring-containing polymer had a weight average molecular weight of 133,000, a melt flow rate of 6.5 g / 10 min, and a glass transition temperature of 131° C.
[0155] The pellets obtained were mixed and extruded with an acrylonitrile-styrene (AS) resin (Toyo AS AS20, manufactured by Toyo Styrene Co., Ltd.) in a mass ratio of 90 / 10 using a single-screw extruder (screw 30 mmφ) to obtain transparent pellets. The glass transition temperature of the pellets obtained was 127°C.
[0156] The pellets were melt-extruded from a 400 mm wide coat hanger type T-die using a 50 mmφ single screw extruder to produce a film with a thickness of 120 μm. The film was stretched 2.0 times vertically and 2.0 times horizontally at a temperature of 150° C. using a biaxial stretching device to obtain a stretched film (acrylic film) with a thickness of 30 μm. The optical properties of the stretched film were measured to find that the total light transmittance was 93%, the in-plane retardation Δnd was 0.8 nm, and the thickness direction retardation Rth was 1.5 nm.
[0157] Next, a polarizing film P1 was produced by the following method. First, a 45 μm thick polyvinyl alcohol film was stretched to a stretching ratio of 3 times while being dyed in a 0.3% iodine solution (temperature 30° C.) for 1 minute between a plurality of rolls with different speed ratios. Next, the obtained stretched film was stretched to a total stretching ratio of 6 times while being immersed in an aqueous solution (temperature 60° C.) containing 4% boric acid and 10% potassium iodide for 0.5 minutes. Next, the stretched film was washed by immersing it in an aqueous solution (temperature 30° C.) containing 1.5% potassium iodide for 10 seconds. Next, the stretched film was dried at 50° C. for 4 minutes to obtain a polarizer with a thickness of 18 μm. A 40 μm thick TAC film (manufactured by Konica Minolta, product name "KC4UY") was attached to one main surface of the obtained polarizer via a polyvinyl alcohol-based adhesive. The above-mentioned acrylic film having a thickness of 30 μm was attached to the other main surface of the polarizer via a polyvinyl alcohol-based adhesive, thereby obtaining a polarizing film P1.
[0158] <Polarizing films P2~P3> Polarizing films P2 to P3 were produced in the same manner as polarizing film P1, except that the drying conditions (drying temperature and drying time) of the stretched film for producing a polarizer were appropriately changed.
[0159] Example 1 The adhesive layer D of the antireflection film AR1 was attached to the surface of the TAC film of the polarizing film P1. Furthermore, the adhesive layer A was transferred to the surface of the acrylic film of the polarizing film P1 to prepare the polarizing film with the antireflection film of Example 1 having a structure of the antireflection film AR1 / polarizing film P1 / adhesive layer A.
[0160] (Example 2 5. Reference Examples 1 to 8 and Comparative Examples 1 to 3) Examples 2 to 4 were prepared in the same manner as in Example 1, except that the anti-reflection film, the polarizing film, and the adhesive layer were changed to the combinations shown in Table 2. 5. Reference Examples 1 to 8 And, antireflection-coated polarizing films were produced for Comparative Examples 1 to 3. The configuration of the antireflection-coated polarizing film of Comparative Example 3 was the same as that of the antireflection-coated polarizing film of Comparative Example 1.
[0161] Example 6 ) First, 8.6 parts of a solution containing a thiophene-based polymer at a solid content concentration of 10 to 50% by weight (trade name: Denatron P-580W, manufactured by Nagase ChemteX), 1 part of a solution containing an oxazoline group-containing acrylic polymer (trade name: Epocross WS-700, manufactured by Nippon Shokubai), and 90.4 parts of water were mixed to prepare a coating solution (solid content concentration 0.5% by weight) for forming a conductive layer. In the obtained coating solution, the concentration of the polythiophene-based polymer was 0.04% by weight, and the concentration of the oxazoline group-containing acrylic polymer was 0.25% by weight.
[0162] Next, the obtained coating liquid was applied to the surface of the acrylic film of the polarizing film P2. The obtained coating film was dried at 80°C for 2 minutes to obtain a conductive layer having a thickness of 0.06 μm. In the conductive layer, the content of the polythiophene-based polymer was 8 wt%, and the content of the oxazoline group-containing acrylic polymer was 50 wt%.
[0163] Next, the adhesive layer D of the anti-reflection film AR1 was attached to the surface of the TAC film of the polarizing film P2. Furthermore, the adhesive layer C was transferred to the surface of the conductive layer to form an example having a structure of the anti-reflection film AR1 / polarizing film P2 / conductive layer / adhesive layer C. 6 A polarizing film with an anti-reflection film was prepared.
[0164] <Optical properties of polarizing film with anti-reflection coating> Working Example , Reference Example Regarding the polarizing film with an anti-reflection film obtained in the comparative example, the luminous reflectances Y and L of reflected light generated when light from a CIE standard light source D65 is incident on the anti-reflection film in a state in which the pressure-sensitive adhesive layer is directly in contact with the non-alkali glass and laminated thereon are * Value, a * value and b * Value, as well as L * Value=0,a * Value = 0 and b * The color difference ΔE between the light that satisfies the value=0 and the reflected light was evaluated by the above-mentioned method. At this time, the polarizing film with anti-reflection film was cut into a 50 mm square and used. Corning EG-XG (thickness 0.7 mm) was used as the alkali-free glass. Polyethylene terephthalate (PET) was used as the black film. The spectral reflectance was measured using a spectrophotometer (Konica Minolta, product name "CM2600D"). The evaluation sample for evaluating the optical characteristics had a configuration of an anti-reflection film-attached polarizing film / alkali-free glass / black PET film. However, for the polarizing film with anti-reflection film of Comparative Example 1, the reflected light was evaluated using alkali-free glass on the surface of which an amorphous ITO layer (thickness 20 nm) was formed. That is, in Comparative Example 1, the evaluation sample had a configuration of an anti-reflection film-attached polarizing film / ITO layer / alkali-free glass / black PET film. Sputtering was used to prepare the ITO layer. The Sn ratio of ITO contained in the ITO layer was 3% by weight. The Sn ratio was calculated from the weight of Sn atoms in ITO / (weight of Sn atoms+weight of In atoms).
[0165] <Optical properties of anti-reflective coating> For the anti-reflection films AR1 to AR11, the luminous reflectances Y1 and a1 of reflected light generated when light from the CIE standard illuminant D65 is incident * Value and b1 * The values were evaluated by the method described above. The black film, spectrophotometer, etc. used were the same as those used to evaluate the optical properties of the anti-reflection coated polarizing film.
[0166] <Optical properties of polarizing film> The total light transmittance of the polarizing film was measured using a spectrophotometer (V7100 manufactured by JASCO Corporation) in accordance with the provisions of JIS K7361-1:1997. CIE standard illuminant D65 was used as the light source. Furthermore, the obtained transmittance was subjected to luminosity correction (780 to 380 nm: 5 nm intervals) using the 2-degree visual field XYZ system prescribed in JIS Z8701:1999 to determine the a and b values in the Hunter Lab color system of the transmitted light when light from the CIE standard illuminant D65 was incident on the polarizing film. Note that in the examples 6 With a conductive layer formed on polarizing film P2, the total light transmittance, and the a value and b value of the transmitted light in the Hunter Lab color system were measured.
[0167] <Surface resistivity of adhesive layer> The surface resistivity (Ω / □) of the pressure-sensitive adhesive layers A to C was measured at the stage where the pressure-sensitive adhesive layers A to C were formed on the surface of the separator. A resistivity meter (Hiresta-UP MCP-HT450 manufactured by Mitsubishi Chemical Analytech Co., Ltd.) was used to measure the surface resistivity. The measurement conditions were an applied voltage of 250 V and an application time of 10 seconds.
[0168] <Surface resistivity of conductive layer> Working Example 6 The surface resistivity (Ω / □) of the conductive layer was measured at the stage where the conductive layer was formed on the surface of the polarizing film P2. A resistivity meter (Hiresta-UP MCP-HT450 manufactured by Mitsubishi Chemical Analytech Co., Ltd.) was used to measure the surface resistivity. The measurement conditions were an applied voltage of 10 V and an application time of 10 seconds.
[0169] <ESD test> First, in the examples , Reference Example The polarizing films with antireflection films obtained in the examples and comparative examples were bonded to the surface on the visual recognition side of the in-cell type liquid crystal cell to fabricate a liquid crystal panel incorporating a touch sensing function. The liquid crystal cell had the same structure as the liquid crystal cell 26 shown in FIG. 6. However, for Comparative Example 1, a liquid crystal cell having an amorphous ITO layer (thickness: 20 nm) formed on the surface was used. That is, in Comparative Example 1, the liquid crystal panel had a configuration of antireflection film-polarizing film / ITO layer / liquid crystal cell. For the fabrication of the ITO layer, sputtering was utilized. The Sn ratio of ITO contained in the ITO layer was 3% by weight. Next, silver paste was applied with a width of 5 mm so as to cover the side surface of the polarizing film with the antireflection film. By drying the silver paste, a conductive structure composed of silver was formed. Through this conductive structure, the liquid crystal panel was electrically connected to an external ground electrode. Next, the liquid crystal panel was set on a backlight device. Next, using an electrostatic discharge (ESD) gun whose applied voltage was adjusted to 10 kV, static electricity was applied to the visual recognition side (antireflection film side) of the liquid crystal panel. As a result, a part of the liquid crystal panel became white. After applying the static electricity, the time T until the white part disappeared was measured. In Table 2, the results of the ESD test were evaluated based on the following criteria regarding the time T. The ESD test was conducted under the conditions of 23°C and 55% RH.
[0170] <Color tone> The liquid crystal panel fabricated in the above ESD test was visually observed from the visual recognition side (antireflection film side), and the color tone was evaluated. In the color tone item in Table 2, A means that no color tone was confirmed. B means that a very slight color tone was confirmed. C means that a slight color tone was confirmed. D means that a color tone was confirmed.
[0171]
Table 2
[0172] As can be seen from Table 2, a* value and b * Examples 1 to 3 which produce reflected light whose values satisfy the relational expressions (1) and (2) 6 and Reference Examples 1 to 8 In the liquid crystal panel equipped with the polarizing film with an anti-reflection film of Example 1, no color was observed, or even if a color was observed, it was not of a practical problem, compared with the liquid crystal panels equipped with the polarizing films with an anti-reflection film of Comparative Examples 2 and 3. 6 and Reference Examples 1 to 8 The reflected light from the liquid crystal panel having the anti-reflection coated polarizing film had a neutral hue. Furthermore, the luminous reflectance Y value of the reflected light was sufficiently low in Examples 1 to 5. 6 and Reference Examples 1 to 8 In the liquid crystal panel equipped with the anti-reflection coated polarizing film, light reflection was sufficiently suppressed.
[0173] From the results of the ESD tests of Comparative Examples 1 and 3, it is presumed that the charging of the liquid crystal panel is suppressed when an ITO layer is disposed between the anti-reflection coated polarizing film and the liquid crystal cell. However, in Comparative Example 1, the luminous reflectance Y is significantly increased due to the presence of the ITO layer, and the reflection of light on the liquid crystal panel could not be sufficiently suppressed.
[0174] Further, examples 5 and 6 As can be seen from the results of the ESD test, even if an ITO layer is not disposed between the polarizing film with an anti-reflection film and the liquid crystal cell, if the polarizing film with an anti-reflection film has a pressure-sensitive adhesive layer or a conductive layer with low surface resistivity, charging of the liquid crystal panel can be sufficiently suppressed. [Industrial Applicability]
[0175] The liquid crystal panel of the present invention can be suitably used in applications requiring good visibility, such as vehicle-mounted displays. [Explanation of symbols]
[0176] 1. First high refractive index layer 2. First low refractive index layer 3 Second high refractive index layer 4. Second low refractive index layer 5 Base material 6 Adhesive layer 10,11 Anti-reflection coating 15,16,17 Polarizing film with anti-reflection coating 20 Polarizing Film 25,26 Liquid crystal cell 30 Adhesive layer 40 Transparent Substrate 45 Adhesive layer 46 Conductive Layer 50 Liquid crystal layer 60 1st transparent substrate 70 Second transparent substrate 80 Touch sensing electrode 100,110,120,130 LCD panel
Claims
1. a polarizing film with an anti-reflection film, the polarizing film and the pressure-sensitive adhesive layer being arranged in this order in the lamination direction; A liquid crystal cell; Equipped with no conductive layer is provided between the anti-reflection coated polarizing film and the liquid crystal cell; The anti-reflection film-attached polarizing film is laminated on the non-alkali glass so that the pressure-sensitive adhesive layer is in direct contact with the non-alkali glass, and when light from a CIE standard illuminant D65 is incident on the surface opposite to the pressure-sensitive adhesive layer, the anti-reflection film has an L * a * b * A in color system * Value and b * A liquid crystal panel that produces reflected light whose values satisfy the following relationship expressions (1) and (2). 0.9≦a * ≦6 (1) −5≦b * ≦2 (2)
2. 2. The liquid crystal panel according to claim 1, wherein the luminous reflectance Y of the reflected light is 1.1% or less.
3. The a * 3. The liquid crystal panel according to claim 1, wherein the value is 0.9 or more and 3 or less.
4. The a * value and the b * 4. The liquid crystal panel according to claim 1, wherein the value satisfies the following relational expression (4): b * ≦-1.5a * +7.5 (4)
5. The liquid crystal panel according to any one of claims 1 to 4, wherein the anti-reflection film has a first high refractive index layer, a first low refractive index layer, a second high refractive index layer, and a second low refractive index layer in this order in a stacking direction.
6. the first high refractive index layer has an optical thickness of 20 nm to 35 nm; The first low refractive index layer has an optical thickness of 38 nm to 50 nm; the second high refractive index layer has an optical thickness of 230 nm to 290 nm; 6. The liquid crystal panel according to claim 5, wherein the second low refractive index layer has an optical thickness of 100 nm to 128 nm.
7. The anti-reflection coated polarizing film further comprises a conductive layer, The surface resistivity of the conductive layer of the anti-reflection film-attached polarizing film is 1.0×10 6 7. The liquid crystal panel according to claim 1, wherein the resistance is greater than Ω / □.
8. The liquid crystal panel according to claim 7 , wherein the conductive layer of the anti-reflection coated polarizing film is disposed between the polarizing film and the pressure-sensitive adhesive layer.
9. 9. The liquid crystal panel according to claim 1, wherein the pressure-sensitive adhesive layer contains a conductive material.
10. The liquid crystal cell is A first transparent substrate and a second transparent substrate; The liquid crystal panel according to claim 1 , further comprising: a touch sensing electrode portion disposed between the first transparent substrate and the second transparent substrate.
Citation Information
Patent Citations
Data comparator
JP1981079337A
Antireflection film
JP2019032524A
In-cell liquid crystal panel and liquid crystal display device
WO2018181477A1