Curable resin film, roll body, laminated structure, and multilayer printed wiring board
The curable resin film with a peak intensity ratio of 0.95 or less addresses flexibility and thermal stability issues, enhancing curl resistance and adhesion, resulting in improved multilayer printed wiring boards.
Patent Information
- Application Number
- JP2020154030
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-14
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-09-14
AI Technical Summary
Conventional curable resin films exhibit low flexibility and poor thermal dimensional stability, leading to issues such as curling marks and difficulty in forming fine wiring due to low adhesion with metal layers.
A curable resin film with a peak intensity ratio of 0.95 or less, achieved by optimizing the composition to include specific thermosetting compounds, inorganic fillers, and curing agents, which enhances flexibility and thermal dimensional stability.
The optimized curable resin film demonstrates improved flexibility, reduced curling, and enhanced thermal stability, allowing for finer wiring and better adhesion with metal layers, thereby improving the performance of multilayer printed wiring boards.
Smart Images

Figure 0007579093000004 
Figure 0007579093000005 
Figure 0007579093000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin film that can be cured. The present invention also relates to a roll body, a laminated structure, and a multilayer printed wiring board that use the curable resin film. [Background technology]
[0002] Conventionally, various resin materials have been used to obtain electronic components such as semiconductor devices, laminates, and printed wiring boards. For example, in a multilayer printed wiring board, a resin material is used to form an insulating layer for insulating between internal layers, or to form an insulating layer located on a surface layer. Wiring, which is generally metal, is laminated on the surface of the insulating layer. In addition, a resin film obtained by filming the resin material may be used to form the insulating layer. The resin material and the resin film are used as insulating materials for multilayer printed wiring boards, including build-up films.
[0003] The following Patent Document 1 discloses a resin composition containing an epoxy resin (A) and a salt (B) of an imidazole compound (b1) and a carboxylic anhydride (b2). Patent Document 1 also describes that a cured product of this resin composition can be used as an insulating layer for a multilayer printed wiring board or the like. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-62570 A Summary of the Invention [Problem to be solved by the invention]
[0005] As a material for an insulating layer in electronic components such as a printed wiring board, a curable resin film such as a B-stage film is used. The curable resin film is used, for example, by disposing the curable resin film on the surface of a wiring circuit layer and then curing the curable resin film. The insulating layer is formed by curing the curable resin film.
[0006] Incidentally, a curable resin film may be stored in a roll state by being wound around the outer periphery of a core. However, if the curable resin film has low flexibility, a winding mark may be generated.
[0007] Furthermore, conventional curable resin films often have poor thermal dimensional stability when cured.
[0008] With conventional curable resin films, it is difficult to increase the flexibility of the curable resin film while at the same time increasing the thermal dimensional stability of the cured product.
[0009] The object of the present invention is to provide a curable resin film capable of increasing the flexibility of the curable resin film and increasing the thermal dimensional stability of the cured product of the curable resin film. Another object of the present invention is to provide a roll body, a laminated structure, and a multilayer printed wiring board using the curable resin. [Means for solving the problem]
[0010] According to a broad aspect of the present invention, there is provided a curable resin film, in which a peak intensity ratio represented by the following formula (X) is 0.95 or less.
[0011] Peak intensity ratio = P2 / P1 (X) P1: the maximum peak intensity in the range of 0 ppm to 50 ppm in the solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity in the range of 100 ppm to 200 ppm P2: the maximum peak intensity in the range of 0 ppm to 50 ppm in the solid-state NMR spectrum of the cured product of the curable resin film normalized by the maximum peak intensity in the range of 100 ppm to 200 ppm
[0012] In a specific aspect of the curable resin film according to the present invention, the peak intensity ratio represented by the formula (X) is less than 0.7.
[0013] In a specific aspect of the curable resin film according to the present invention, P1 is 0.5 or more.
[0014] In a specific aspect of the curable resin film according to the present invention, P2 is 0.5 or less.
[0015] In a specific aspect of the curable resin film according to the present invention, in a solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity in the range from 100 ppm to 200 ppm, there are two or more peaks having a peak intensity of 1.5 times or more the average intensity of the spectrum in the range from 0 ppm to 50 ppm.
[0016] In a specific aspect of the curable resin film according to the present invention, in a solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity in the range from 100 ppm to 200 ppm, there are two or more peaks having a peak intensity three or more times the average intensity of the spectrum in the range from 0 ppm to 50 ppm.
[0017] In a specific aspect of the curable resin film according to the present invention, in a solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity from 100 ppm to 200 ppm, a peak derived from a cyclic hydrocarbon skeleton is present at 0 ppm to 50 ppm, and a peak derived from a linear hydrocarbon skeleton is present at 0 ppm to 50 ppm, and each of the peak derived from the cyclic hydrocarbon skeleton and the peak derived from the linear hydrocarbon skeleton has a peak intensity that is 1.5 times or more the average intensity of the spectrum from 0 ppm to 50 ppm.
[0018] In a specific aspect of the curable resin film according to the present invention, the curable resin film includes a thermosetting compound, and the thermosetting compound includes a thermosetting compound having an imide skeleton.
[0019] In a specific aspect of the curable resin film according to the present invention, the curable resin film contains a thermosetting compound, and the thermosetting compound contains a bismaleimide compound.
[0020] In a specific aspect of the curable resin film according to the present invention, the thermosetting compound includes an epoxy compound.
[0021] In a specific aspect of the curable resin film according to the present invention, the curable resin film contains a curing agent, and the curing agent contains an active ester compound.
[0022] In a specific aspect of the curable resin film according to the present invention, the curable resin film contains an inorganic filler, and the content of the inorganic filler is 50% by weight or more based on 100% by weight of the components excluding the solvent in the curable resin film.
[0023] In a specific aspect of the curable resin film according to the present invention, the cured product of the curable resin film has an average linear expansion coefficient of less than 35 ppm / °C at 25°C or higher and 150°C or lower.
[0024] According to a broad aspect of the present invention, there is provided a roll body including a winding core and the above-mentioned curable resin film, the curable resin film being wound around an outer periphery of the winding core.
[0025] According to a broad aspect of the present invention, there is provided a laminated structure comprising a laminate target component having a metal layer on a surface thereof and the above-mentioned curable resin film, the curable resin film being laminated on the surface of the metal layer.
[0026] In a specific aspect of the laminated structure according to the present invention, the material of the metal layer is copper.
[0027] According to a broad aspect of the present invention, there is provided a multilayer printed wiring board comprising a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, wherein at least one of the plurality of insulating layers is a cured product of the above-mentioned curable resin film. Effect of the Invention
[0028] The curable resin film according to the present invention has a peak intensity ratio represented by the above formula (X) of 0.95 or less. Since the curable resin film according to the present invention has the above configuration, the flexibility of the curable resin film can be increased, and the thermal dimensional stability of the cured product of the curable resin film can be increased. [Brief description of the drawings]
[0029] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a multilayer printed wiring board using a curable resin film according to one embodiment of the present invention. [Diagram 2] FIG. 2(a) is a solid-state NMR spectrum of the curable resin film obtained in Example 1, and FIG. 2(b) is a solid-state NMR spectrum of the cured product of the curable resin film obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The present invention will be described in detail below.
[0031] The curable resin film according to the present invention is a curable resin film, which has a peak intensity ratio represented by the following formula (X) of 0.95 or less.
[0032] Peak intensity ratio = P2 / P1 (X) P1: the maximum peak intensity in the range of 0 ppm to 50 ppm in the solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity in the range of 100 ppm to 200 ppm P2: the maximum peak intensity in the range of 0 ppm to 50 ppm in the solid-state NMR spectrum of the cured product of the curable resin film normalized by the maximum peak intensity in the range of 100 ppm to 200 ppm
[0033] Since the curable resin film according to the present invention has the above-mentioned configuration, it is possible to increase the flexibility of the curable resin film and to increase the thermal dimensional stability of the cured product of the curable resin film. Since the curable resin film according to the present invention has high flexibility, for example, even when it is made into a roll, it is unlikely to leave a rolling mark. Furthermore, since the curable resin film according to the present invention has high flexibility, for example, when the curable resin film is cut to a predetermined size, chipping is unlikely to occur.
[0034] The curable resin film is preferably a curable resin film that can be cured by heating.The curable resin film is preferably a curable resin film that is used by heating.The curable resin film is preferably a thermosetting resin film.
[0035] In the present invention, the curable resin film and the cured product of the curable resin film are each measured by solid-state NMR.
[0036] Specifically, the above solid-state NMR spectrum is measured under the following conditions and obtained by functional processing under the following conditions.
[0037] <Solid-state NMR measurement conditions> Nuclear magnetic resonance device: JEOL "ECZ-400R" Temperature: room temperature Observed nucleus: 13C Observation frequency: 100.5253MHz Probe: 8mm CPMAS probe Reference substance: Adamantane (external standard: 28.46ppm) Pulse width: 6.64μsec Capture time: 40.63msec Pulse repetition time: 60sec Magic angle rotation speed: 5kHz Accumulation count: 2048 times Measurement mode: Single pulse (DD / MAS) method Sample size: approx. 400mg
[0038] <Function processing conditions> Function processing software: JEOL Delta Processing 1: exp 50Hz Treatment 2: trapezoid P3 30% Treatment 3: Trapezoid P4 40% Process 4: zerofill multiple 4 Step 5: Fourier transform
[0039] <Phase correction> Phase 0 correction First-order phase correction
[0040] The cured product of the curable resin film used to obtain a solid-state NMR spectrum is a cured product obtained by heating the curable resin film at 130°C for 60 minutes and then at 190°C for 90 minutes. However, the heating conditions of the curable resin film when actually using the curable resin film are not particularly limited. When actually using the curable resin film, the curable resin film may be heated under heating conditions other than the conditions of heating at 130°C for 60 minutes and then at 190°C for 90 minutes.
[0041] In this specification, the above "solid-state NMR spectrum of the curable resin film normalized by the maximum value of the peak intensity in the range from 100 ppm to 200 ppm" may be referred to as "solid-state NMR spectrum (1)". Also, in this specification, the above "solid-state NMR spectrum of the cured product of the curable resin film normalized by the maximum value of the peak intensity in the range from 100 ppm to 200 ppm" may be referred to as "solid-state NMR spectrum (2)".
[0042] Therefore, the above P1 is the maximum value of the peak intensity in the range from 0 ppm to 50 ppm in the solid-state NMR spectrum (1), and the above P2 is the maximum value of the peak intensity in the range from 0 ppm to 50 ppm in the solid-state NMR spectrum (2).
[0043] In order to exert the effects of the present invention, in the curable resin film, the peak intensity ratio represented by the above formula (X) (the ratio of P2 to P1 (P2 / P1)) is 0.95 or less.
[0044] In the curable resin film, the peak intensity ratio (the ratio of P2 to P1 (P2 / P1)) represented by the formula (X) is preferably 0.1 or more, more preferably 0.2 or more, preferably less than 0.7, more preferably 0.5 or less, and even more preferably 0.4 or less. When the peak intensity ratio is equal to or more than the lower limit and less than the upper limit or equal to or less than the upper limit, the effects of the present invention can be more effectively exhibited.
[0045] The above P1 is preferably at least 0.5, more preferably at least 0.7, and even more preferably at least 0.8. When the above P1 is at least the above lower limit, the flexibility of the curable resin film can be further increased.
[0046] The P2 is preferably not more than 0.5, more preferably not more than 0.45, and even more preferably not more than 0.35. When the P2 is not more than the upper limit, the thermal dimensional stability of the cured product of the curable resin film can be further improved.
[0047] The maximum value of the peak intensity at 100 ppm or more and 200 ppm or less used to obtain the solid-state NMR spectrum (1) is preferably the maximum value of the peak intensity derived from the aromatic skeleton. The maximum value of the peak intensity at 100 ppm or more and 200 ppm or less used to obtain the solid-state NMR spectrum (2) is preferably the maximum value of the peak intensity derived from the aromatic skeleton. Therefore, the solid-state NMR spectrum (1) is preferably the solid-state NMR spectrum of the curable resin film normalized by the maximum value of the peak intensity derived from the aromatic skeleton at 100 ppm or more and 200 ppm or less. The solid-state NMR spectrum (2) is preferably the solid-state NMR spectrum of the cured product of the curable resin film normalized by the maximum value of the peak intensity derived from the aromatic skeleton at 100 ppm or more and 200 ppm or less.
[0048] In the above P1, the maximum value of the peak intensity at 0 ppm or more and 50 ppm or less is preferably the maximum value of the peak intensity attributable to an aliphatic skeleton, and more preferably the maximum value of the peak intensity attributable to an aliphatic hydrocarbon skeleton. In the above P2, the maximum value of the peak intensity at 0 ppm or more and 50 ppm or less is preferably the maximum value of the peak intensity attributable to an aliphatic skeleton, and more preferably the maximum value of the peak intensity attributable to an aliphatic hydrocarbon skeleton.
[0049] In the solid-state NMR spectrum (1), it is preferable that the peak derived from the cyclic hydrocarbon skeleton is present at 0 ppm to 50 ppm, or the peak derived from the linear hydrocarbon skeleton is present at 0 ppm to 50 ppm. It is more preferable that the peak derived from the cyclic hydrocarbon skeleton is present at 0 ppm to 50 ppm, and the peak derived from the linear hydrocarbon skeleton is present at 0 ppm to 50 ppm. In this case, the effect of the present invention can be more effectively exhibited.
[0050] Examples of the cyclic hydrocarbon skeleton include a cyclohexane ring skeleton, a cyclopentane ring skeleton, a cyclohexene ring skeleton, a norbornane skeleton, a dicyclopentadiene skeleton, and an adamantane skeleton. The cyclic hydrocarbon skeleton is preferably a cyclohexane ring skeleton.
[0051] Examples of the linear hydrocarbon skeleton include a skeleton having an alkyl group, a skeleton having an alkenyl group, and a skeleton having an alkanediyl group. The alkyl group may be branched. The linear hydrocarbon skeleton is preferably a skeleton having an alkyl group or a skeleton having an alkanediyl group, and more preferably a skeleton having an alkyl group.
[0052] In the solid-state NMR spectrum (1), it is preferable that there are two or more peaks having a peak intensity of 1.5 times or more than the average intensity of the spectrum from 0 ppm to 50 ppm. In the solid-state NMR spectrum (1), it is more preferable that there are two or more peaks having a peak intensity of 2 times or more than the average intensity of the spectrum from 0 ppm to 50 ppm, and it is even more preferable that there are two or more peaks having a peak intensity of 3 times or more. In the solid-state NMR spectrum (1), it is preferable that there are two or more peaks having a peak intensity of 15 times or less than the average intensity of the spectrum from 0 ppm to 50 ppm, and it is even more preferable that there are two or more peaks having a peak intensity of 10 times or less. In this case, the flexibility of the curable resin film can be further increased.
[0053] In the solid-state NMR spectrum (1), the peak derived from the cyclic hydrocarbon skeleton and the peak derived from the linear hydrocarbon skeleton are preferably peaks having a peak intensity of 1.5 times or more of the average intensity of the spectrum from 0 ppm to 50 ppm. In the solid-state NMR spectrum (1), the peak derived from the cyclic hydrocarbon skeleton and the peak derived from the linear hydrocarbon skeleton are more preferably peaks having a peak intensity of 2 times or more, and even more preferably peaks having a peak intensity of 3 times or more, of the average intensity of the spectrum from 0 ppm to 50 ppm. In the solid-state NMR spectrum (1), the peak derived from the cyclic hydrocarbon skeleton and the peak derived from the linear hydrocarbon skeleton are preferably peaks having a peak intensity of 15 times or less, and more preferably peaks having a peak intensity of 10 times or less, of the average intensity of the spectrum from 0 ppm to 50 ppm. In this case, the flexibility of the curable resin film can be further increased.
[0054] The average intensity of the spectrum from 0 ppm to 50 ppm is the average intensity including the part where no peak exists (part where no peak is detected) and the part where a peak exists. The average intensity of the spectrum from 0 ppm to 50 ppm is calculated by shifting the baseline in parallel so that the minimum value becomes zero when there is a negative value in the peak intensity at 1 ppm intervals in the range from 0 ppm to 50 ppm after baseline correction, and then plotting them and averaging the intensities. The ratio (peak intensity / average intensity of the spectrum from 0 ppm to 50 ppm) is calculated for the peak intensity after the baseline shift.
[0055] The curable resin film can be obtained, for example, by forming a resin composition containing a thermosetting compound into a film shape.
[0056] Hereinafter, details of each component used in the curable resin film and resin composition according to the present invention, as well as applications of the curable resin film according to the present invention will be described.
[0057] From the viewpoint of reducing the linear thermal expansion coefficient and dielectric loss tangent of the cured product and from the viewpoint of well controlling the peak intensity ratio represented by the formula (X), the curable resin film and the resin composition preferably contain a compound having a non-aromatic cyclic skeleton. The atoms constituting the non-aromatic cyclic skeleton are preferably carbon atoms, oxygen atoms, sulfur atoms, or silicon atoms, and are most preferably carbon atoms. The non-aromatic cyclic skeleton composed of carbon atoms is preferably a cyclohexane ring skeleton, a dicyclopentadiene ring skeleton, or a norbornene ring skeleton. The compound having the non-aromatic cyclic skeleton is preferably a compound having a skeleton derived from norbornanediamine, a skeleton derived from cyclohexanediamine, a skeleton derived from tricyclodecanediamine, a skeleton derived from dimer diamine, or a skeleton derived from trimer triamine.
[0058] From the viewpoint of well controlling the peak intensity ratio represented by the formula (X), the curable resin film and the resin composition preferably contain a compound having a cyclic hydrocarbon skeleton, preferably contain a compound having a linear hydrocarbon skeleton, and more preferably contain a compound having a cyclic hydrocarbon skeleton and a linear hydrocarbon skeleton. The compound having a cyclic hydrocarbon skeleton may be a thermosetting compound having a cyclic hydrocarbon skeleton, or may be a thermoplastic compound having a cyclic hydrocarbon skeleton. The compound having a linear hydrocarbon skeleton may be a thermosetting compound having a linear hydrocarbon skeleton, or may be a thermoplastic compound having a linear hydrocarbon skeleton. The compound having a cyclic hydrocarbon skeleton and a linear hydrocarbon skeleton may be a thermosetting compound having a cyclic hydrocarbon skeleton and a linear hydrocarbon skeleton, or may be a thermoplastic compound having a cyclic hydrocarbon skeleton and a linear hydrocarbon skeleton.
[0059] Examples of the cyclic hydrocarbon skeleton include a cyclohexane ring skeleton, a cyclopentane ring skeleton, a cyclohexene ring skeleton, a norbornane skeleton, a dicyclopentadiene skeleton, and an adamantane skeleton. The cyclic hydrocarbon skeleton is preferably a cyclohexane ring skeleton.
[0060] Examples of the linear hydrocarbon skeleton include a skeleton having an alkyl group, a skeleton having an alkenyl group, and a skeleton having an alkanediyl group. The linear hydrocarbon skeleton is preferably a skeleton having an alkyl group or a skeleton having an alkanediyl group, and more preferably a skeleton having an alkyl group. The alkyl group may have a branch.
[0061] From the viewpoint of well controlling the peak intensity ratio represented by the above formula (X), the content of the compound having a cyclic hydrocarbon skeleton in 100% by weight of the above curable resin film or in 100% by weight of the above resin composition is preferably 2.5% by weight or more, more preferably 5% by weight or more, and is preferably 25% by weight or less, more preferably 15% by weight or less.
[0062] In 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, the content of the compound having a cyclic hydrocarbon skeleton is preferably 5% by weight or more, more preferably 10% by weight or more, preferably 50% by weight or less, more preferably 30% by weight or less. When the content of the compound having a cyclic hydrocarbon skeleton is the lower limit or more and the upper limit or less, the peak intensity ratio represented by the formula (X) can be well controlled.
[0063] From the viewpoint of well controlling the peak intensity ratio represented by the formula (X) and from the viewpoint of improving the elongation property of the curable resin film, the curable resin film and the resin composition preferably contain a compound having a group having a straight chain. The group having a straight chain is preferably a group in which 6 or more atoms are connected in a straight chain. The group having a straight chain may have an unsaturated bond. Examples of the group having a straight chain include an alkyl group and an alkanediyl group. The atoms constituting the straight chain are preferably carbon atoms, oxygen atoms, sulfur atoms, or silicon atoms, and are most preferably carbon atoms. The group having a straight chain composed of carbon atoms is preferably an alkyl group or an alkanediyl group. The alkyl group may be an alkyl group having an ether group by inserting an oxygen atom in the middle of the alkyl group. The compound having a group having a straight chain is preferably a compound having a skeleton derived from 1,6-diaminohexane, a skeleton derived from 1,4-butanediol bis(3-aminopropyl) ether, a skeleton derived from 1,1,12-diaminododecane, a skeleton derived from a monomer monoamine, or a skeleton derived from a dimer diamine or a skeleton derived from a trimer triamine.
[0064] From the viewpoint of well controlling the peak intensity ratio represented by the above formula (X), the content of the compound having a linear group in 100% by weight of the above curable resin film or in 100% by weight of the above resin composition is preferably 1% by weight or more, more preferably 3% by weight or more, and is preferably 30% by weight or less, more preferably 15% by weight or less.
[0065] In 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, the content of the compound having a linear group is preferably 2.5% by weight or more, more preferably 7.5% by weight or more, preferably 60% by weight or less, more preferably 30% by weight or less. When the content of the compound having a linear group is the lower limit or more and the upper limit or less, the peak intensity ratio represented by the formula (X) can be well controlled.
[0066] [Thermosetting compound] The curable resin film preferably contains a thermosetting compound. The resin composition preferably contains a thermosetting compound. The thermosetting compound may be used alone or in combination of two or more kinds.
[0067] Examples of the thermosetting compound include epoxy compounds, maleimide compounds, benzoxazine compounds, vinyl compounds, phenoxy compounds, oxetane compounds, polyarylate compounds, diallyl phthalate compounds, episulfide compounds, (meth)acrylic compounds, amino compounds, unsaturated polyester compounds, polyurethane compounds, and silicone compounds.
[0068] The thermosetting compound preferably contains an epoxy compound, a maleimide compound or a vinyl compound, more preferably contains an epoxy compound or a maleimide compound, and even more preferably contains an epoxy compound. In this case, the flexibility and embeddability into uneven surfaces of the curable resin film can be improved, the film can be cured well at 200° C. or less, and the thermal dimensional stability of the cured product can be further improved.
[0069] The thermosetting compound preferably contains a thermosetting compound having an imide skeleton or an amide skeleton, more preferably contains a thermosetting compound having an imide skeleton, and further preferably contains a bismaleimide compound, which can further increase the thermal dimensional stability of the cured product and further reduce the dielectric tangent of the cured product.
[0070] From the viewpoint of well controlling the peak intensity ratio represented by the above formula (X) and from the viewpoint of enhancing the flame retardancy and thermal dimensional stability of the curable resin film, it is preferable that the above thermosetting compound contains a thermosetting compound having an aromatic skeleton.
[0071] Examples of the aromatic skeleton include a phenyl skeleton, a naphthalene skeleton, and a fluorene skeleton.
[0072] In 100% by weight of the curable resin film or in 100% by weight of the components in the resin composition excluding the solvent, the content of the thermosetting compound having an aromatic skeleton is preferably 10% by weight or more, more preferably 20% by weight or more, preferably 30% by weight or less, more preferably 25% by weight or less. When the content of the thermosetting compound having an aromatic skeleton is the lower limit or more and the upper limit or less, the peak intensity ratio represented by the formula (X) can be well controlled.
[0073] The content of the thermosetting compound having an aromatic skeleton in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 25% by weight or more, more preferably 40% by weight or more, preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the thermosetting compound having an aromatic skeleton is the lower limit or more and the upper limit or less, the peak intensity ratio represented by the formula (X) can be well controlled.
[0074] <Epoxy compounds> As the epoxy compound, a conventionally known epoxy compound can be used. The epoxy compound may be used alone or in combination of two or more kinds.
[0075] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.
[0076] The epoxy compound preferably contains an epoxy compound having an aromatic skeleton, more preferably contains an epoxy compound having a naphthalene skeleton or a phenyl skeleton, further preferably is an epoxy compound having an aromatic skeleton, and particularly preferably is an epoxy compound having a naphthalene skeleton. In this case, the dielectric tangent of the cured product can be further lowered, and the heat resistance, flame retardancy, and thermal dimensional stability can be improved.
[0077] From the viewpoint of further lowering the dielectric tangent of the cured product and improving the coefficient of linear thermal expansion (CTE), it is preferable that the epoxy compound contains an epoxy compound that is liquid at 25°C and an epoxy compound that is solid at 25°C.
[0078] The viscosity at 25°C of the epoxy compound that is liquid at 25°C is preferably 1000 mPa·s or less, and more preferably 500 mPa·s or less.
[0079] When measuring the viscosity of the epoxy compound, for example, a dynamic viscoelasticity measuring device ("VAR-100" manufactured by Rheologica Instruments) is used.
[0080] It is more preferable that the molecular weight of the epoxy compound is 1000 or less. In this case, even if the components other than the solvent in the curable resin film are 100% by weight and the content of the inorganic filler is 50% by weight or more, a resin film with high fluidity can be obtained when forming an insulating layer. Therefore, when the curable resin film is laminated on a circuit board, the inorganic filler can be uniformly present.
[0081] The molecular weight of the epoxy compound means a molecular weight that can be calculated from the structural formula when the epoxy compound is not a polymer and when the structural formula of the epoxy compound can be specified, and means a weight average molecular weight when the epoxy compound is a polymer.
[0082] The content of the epoxy compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 15% by weight or more, more preferably 25% by weight or more, preferably 50% by weight or less, more preferably 40% by weight or less. When the content of the epoxy compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0083] <Maleimide compounds> As the maleimide compound, a conventionally known maleimide compound can be used. The maleimide compound may be used alone or in combination of two or more kinds.
[0084] The maleimide compound may be a bismaleimide compound. The maleimide compound may be an aliphatic maleimide compound or an aromatic maleimide compound.
[0085] Examples of the maleimide compound include N-phenylmaleimide and N-alkylbismaleimide.
[0086] From the viewpoint of further increasing the thermal dimensional stability of the cured product and further decreasing the dielectric tangent of the cured product, the maleimide compound preferably includes a bismaleimide compound, and is more preferably a bismaleimide compound.
[0087] The bismaleimide compound preferably has a structural unit having an imide bond. The bismaleimide compound more preferably has a structural unit having an imide bond as a repeating structural unit. In this case, the dielectric tangent of the cured product of the curable resin film can be further reduced, and the thermal dimensional stability of the cured product can be improved.
[0088] The maleimide compound may or may not have a skeleton derived from dimer diamine. From the viewpoint of well controlling the peak intensity ratio represented by the formula (X), the maleimide compound is preferably a maleimide compound having a skeleton derived from dimer diamine, and more preferably a bismaleimide compound having a skeleton derived from dimer diamine.
[0089] The maleimide compound may or may not have an aromatic ring. The maleimide compound preferably has an aromatic ring.
[0090] In the maleimide compound, it is preferable that a nitrogen atom in the maleimide skeleton is bonded to an aromatic ring.
[0091] From the viewpoint of effectively exerting the effects of the present invention, the molecular weight of the maleimide compound is preferably 100 or more, more preferably 1000 or more, even more preferably 3000 or more, particularly preferably 3500 or more, and preferably less than 30,000, more preferably less than 20,000, even more preferably less than 15,000, and particularly preferably less than 12,000.
[0092] The molecular weight of the maleimide compound means a molecular weight that can be calculated from the structural formula when the maleimide compound is not a polymer and when the structural formula of the maleimide compound can be specified. When the maleimide compound is a polymer, the molecular weight of the maleimide compound means a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0093] Commercially available products of the above aliphatic maleimide compounds include, for example, "BMI-3000" and "BMI-1700" manufactured by Designer Molecules Inc.
[0094] Commercially available examples of the aromatic maleimide compound include "BMI-4000" and "BMI-5100" manufactured by Daiwa Kasei Kogyo Co., Ltd., and "MIR-3000" manufactured by Nippon Kayaku Co., Ltd.
[0095] The content of the maleimide compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 2.5% by weight or more, more preferably 5% by weight or more, even more preferably 7.5% by weight or more, preferably 50% by weight or less, and more preferably 35% by weight or less. When the content of the maleimide compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0096] <Vinyl compounds> As the vinyl compound, a conventionally known vinyl compound can be used. The vinyl compound is an organic compound having at least one vinyl group. The vinyl compound may be used alone or in combination of two or more kinds.
[0097] Examples of the vinyl compound include a styrene compound, an acrylate compound, and a divinyl compound. Examples of the divinyl compound include a divinyl benzyl ether compound. The vinyl compound may be a divinyl compound having an aliphatic skeleton or a divinyl ether compound.
[0098] The content of the vinyl compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 2.5% by weight or more, more preferably 5% by weight or more, and even more preferably 7.5% by weight or more, and is preferably 70% by weight or less, more preferably 50% by weight or less. When the content of the vinyl compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0099] [Filling material] The curable resin film preferably contains a filler. The resin composition preferably contains a filler. Examples of the filler include organic fillers and inorganic fillers. The filler is preferably an insulating filler. Only one type of the filler may be used, or two or more types may be used in combination.
[0100] The organic filler may be a particulate material made of benzoxazine resin, benzoxazole resin, fluororesin, acrylic resin, styrene resin, etc. The fluororesin may be polytetrafluoroethylene (PTFE), etc. By using fluororesin particles as the organic filler, the dielectric constant of the cured product of the curable resin film can be further reduced.
[0101] Examples of the inorganic filler include silica, talc, clay, mica, hydrotalcite, alumina, magnesium oxide, aluminum hydroxide, aluminum nitride, boron nitride, and diamond.
[0102] The filler is preferably an inorganic filler, in which case the dielectric tangent of the cured product of the curable resin film can be further reduced, and the thermal dimensional stability of the cured product can be further improved.
[0103] The inorganic filler is preferably an inorganic filler having a thermal conductivity of 10 W / mK or more, such as alumina or boron nitride, which can enhance heat dissipation.
[0104] From the viewpoint of improving embedding properties into uneven surfaces and increasing thermal dimensional stability, the inorganic filler is preferably an anisotropic inorganic filler.
[0105] The inorganic filler is preferably silica or alumina, more preferably silica, and even more preferably fused silica. In this case, the surface roughness of the surface of the cured product of the curable resin film can be reduced, the adhesive strength between the cured product and the metal layer can be further increased, finer wiring can be formed on the surface of the cured product, and the cured product can be given better insulation reliability. In particular, by using silica as the inorganic filler, the thermal expansion coefficient of the cured product can be further reduced, and the dielectric loss tangent of the cured product can be further reduced. In addition, the dielectric constant of the cured product can be improved. The shape of the silica is preferably spherical.
[0106] From the viewpoint of increasing the thermal conductivity and the insulating property, the inorganic filler is preferably alumina.
[0107] The inorganic filler is preferably spherical, more preferably spherical silica. In this case, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. When the inorganic filler is spherical, the aspect ratio of the inorganic filler is preferably 2 or less, more preferably 1.5 or less.
[0108] The inorganic filler is preferably surface-treated, more preferably surface-treated with a coupling agent, and even more preferably surface-treated with a silane coupling agent.By surface-treating the inorganic filler, the surface roughness of the roughened cured product is further reduced, and the adhesive strength between the cured product and the metal layer is further increased.In addition, by surface-treating the inorganic filler, finer wiring can be formed on the surface of the cured product, and better inter-wiring insulation reliability and inter-layer insulation reliability can be imparted to the cured product.
[0109] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a methacrylsilane, an acrylsilane, an aminosilane, an imidazole silane, a vinylsilane, an epoxysilane, etc.
[0110] The organic filler preferably has an average particle size of 1 μm or less. If the average particle size of the organic filler is equal to or less than the upper limit, the surface roughness after etching can be reduced, the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further increased. The average particle size of the organic filler may be 50 nm or more.
[0111] The inorganic filler has an average particle size of preferably 50 nm or more, more preferably 100 nm or more, and even more preferably 500 nm or more, and is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. When the average particle size of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further increased.
[0112] The median diameter (d50) at 50% is used as the average particle diameter of the filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method.
[0113] The content of the filler in 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition is preferably 50% by weight or more, more preferably 55% by weight or more, even more preferably 60% by weight or more, and particularly preferably 70% by weight or more. The content of the filler in 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition is preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, and particularly preferably 75% by weight or less. When the content of the filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the filler is equal to or less than the upper limit, the thermal dimensional stability is improved and the warping of the cured product can be effectively suppressed. When the content of the filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product.
[0114] The content of the organic filler in 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition is preferably 5% by weight or more, more preferably 10% by weight or more, even more preferably 15% by weight or more, and particularly preferably 20% by weight or more. The content of the organic filler in 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition is preferably 75% by weight or less, more preferably 60% by weight or less, even more preferably 50% by weight or less, and particularly preferably 40% by weight or less. When the content of the organic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the organic filler is equal to or less than the upper limit, the thermal dimensional stability is improved and the warping of the cured product can be effectively suppressed. When the content of the organic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product.
[0115] The content of the inorganic filler in 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 65% by weight or more, and particularly preferably 68% by weight or more. In 100% by weight of the components excluding the solvent in the curable resin film or in 100% by weight of the components excluding the solvent in the resin composition, the content is preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, and particularly preferably 75% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the inorganic filler is equal to or less than the upper limit, the thermal dimensional stability is improved and the warping of the cured product can be effectively suppressed. When the content of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product. Furthermore, with this content of inorganic filler, it is possible to reduce the thermal expansion coefficient of the cured product and at the same time improve the smear removal properties.
[0116] [Hardening agent] The curable resin film preferably contains a curing agent. The resin composition preferably contains a curing agent. The curing agent is not particularly limited. As the curing agent, a conventionally known curing agent can be used. The curing agent may be used alone or in combination of two or more kinds.
[0117] Examples of the curing agent include a phenol compound (phenol curing agent), an active ester compound, a cyanate ester compound (cyanate ester curing agent), a benzoxazine compound (benzoxazine curing agent), a carbodiimide compound (carbodiimide curing agent), an amine compound (amine curing agent), a thiol compound (thiol curing agent), a phosphine compound, a dicyandiamide, and an acid anhydride. The curing agent preferably has a functional group capable of reacting with the epoxy group of the epoxy compound.
[0118] The curing agent preferably contains at least one component selected from the group consisting of phenolic compounds, active ester compounds, cyanate ester compounds, benzoxazine compounds, carbodiimide compounds, and acid anhydrides. The curing agent more preferably contains at least one component selected from the group consisting of phenolic compounds, active ester compounds, cyanate ester compounds, benzoxazine compounds, and carbodiimide compounds, and further preferably contains an active ester compound. In this case, the dielectric tangent of the cured product of the curable resin film can be further reduced.
[0119] From the viewpoint of further lowering the dielectric tangent, when the curable resin film contains an epoxy compound, the curing agent preferably contains a phenol compound and an active ester compound.
[0120] Examples of the phenol compound include novolak type phenols, biphenol type phenols, naphthalene type phenols, dicyclopentadiene type phenols, aralkyl type phenols, and dicyclopentadiene type phenols.
[0121] Commercially available phenol compounds include novolac phenols ("TD-2091" manufactured by DIC Corporation), biphenyl novolac phenols ("MEH-7851" manufactured by Meiwa Kasei Co., Ltd.), aralkyl phenol compounds ("MEH-7800" manufactured by Meiwa Kasei Co., Ltd.), and phenols having an aminotriazine skeleton ("LA-1356" and "LA-3018-50P" manufactured by DIC Corporation).
[0122] The above-mentioned active ester compound refers to a compound that contains at least one ester bond in the structure and has an aliphatic chain, an aliphatic ring, or an aromatic ring bonded to both sides of the ester bond. The active ester compound is obtained, for example, by a condensation reaction between a carboxylic acid compound or a thiocarboxylic acid compound and a hydroxy compound or a thiol compound. An example of the active ester compound is a compound represented by the following formula (1).
[0123] [ka]
[0124] In the above formula (1), X1 represents a group containing an aliphatic chain, a group containing an aliphatic ring, or a group containing an aromatic ring, and X2 represents a group containing an aromatic ring. Preferred examples of the group containing an aromatic ring include a benzene ring which may have a substituent, and a naphthalene ring which may have a substituent. Examples of the substituent include a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably 12 or less, more preferably 6 or less, and even more preferably 4 or less.
[0125] In the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted benzene ring and an optionally substituted benzene ring, and a combination of an optionally substituted benzene ring and an optionally substituted naphthalene ring. Furthermore, in the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted naphthalene ring and an optionally substituted naphthalene ring.
[0126] The active ester compound is not particularly limited. From the viewpoint of further improving thermal dimensional stability and flame retardancy, the active ester compound is preferably an active ester compound having two or more aromatic skeletons. From the viewpoint of lowering the dielectric tangent of the cured product and improving the thermal dimensional stability of the cured product, it is more preferable that the active ester compound has a naphthalene ring in the main chain skeleton.
[0127] Commercially available products of the above active ester compound include "HPC-8000L", "HPC-8000-65T", "EXB-9416-70BK", "EXB8100-65T", "HPC-8150-62T", and "EXB-8" manufactured by DIC Corporation.
[0128] Examples of the cyanate ester compound include novolac-type cyanate ester resins, bisphenol-type cyanate ester resins, and prepolymers obtained by partially trimerizing these. Examples of the novolac-type cyanate ester resins include phenol novolac-type cyanate ester resins and alkylphenol-type cyanate ester resins. Examples of the bisphenol-type cyanate ester resins include bisphenol A-type cyanate ester resins, bisphenol E-type cyanate ester resins, and tetramethylbisphenol F-type cyanate ester resins.
[0129] Commercially available products of the cyanate ester compound include phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan) and prepolymers in which bisphenol type cyanate ester resins are trimerized ("BA-230S", "BA-3000S", "BTP-1000S" and "BTP-6020S" manufactured by Lonza Japan).
[0130] The content of the cyanate ester compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 10% by weight or more, more preferably 15% by weight or more, and even more preferably 20% by weight or more. The content of the cyanate ester compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 85% by weight or less, more preferably 75% by weight or less. When the content of the cyanate ester compound is the above lower limit or more and the above upper limit or less, the thermal dimensional stability of the cured product can be further improved.
[0131] Examples of the benzoxazine compound include Pd-type benzoxazine and Fa-type benzoxazine.
[0132] Commercially available products of the above benzoxazine compounds include "Pd type" manufactured by Shikoku Chemical Industry Co., Ltd.
[0133] The content of the benzoxazine compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 1% by weight or more, more preferably 5% by weight or more, and even more preferably 10% by weight or more. The content of the benzoxazine compound in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the benzoxazine compound is the above lower limit or more and the above upper limit or less, the thermal dimensional stability of the cured product can be further improved.
[0134] The carbodiimide compound is a compound having a structural unit represented by the following formula (2). In the following formula (2), the right end and the left end are bonding sites with other groups. The above carbodiimide compounds may be used alone or in combination of two or more kinds.
[0135] [ka]
[0136] In the above formula (2), X represents an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, a group in which a substituent is bonded to a cycloalkylene group, an arylene group, or a group in which a substituent is bonded to an arylene group, and p represents an integer of 1 to 5. When a plurality of Xs are present, the plurality of Xs may be the same or different.
[0137] In one preferred embodiment, at least one X is an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, or a group in which a substituent is bonded to a cycloalkylene group.
[0138] Commercially available examples of the carbodiimide compound include "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", "Carbodilite V-09", "Carbodilite 10M-SP", and "Carbodilite 10M-SP (modified)" manufactured by Nisshinbo Chemical Inc., as well as "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.
[0139] Examples of the acid anhydride include tetrahydrophthalic anhydride and alkylstyrene-maleic anhydride copolymer.
[0140] Commercially available products of the above acid anhydrides include "Rikacid TDA-100" manufactured by New Japan Chemical Co., Ltd.
[0141] The content of the curing agent relative to 100 parts by weight of the epoxy compound is preferably 70 parts by weight or more, more preferably 85 parts by weight or more, and preferably 150 parts by weight or less, more preferably 120 parts by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the curing property is more excellent, the thermal dimensional stability is more improved, and the volatilization of the remaining unreacted components can be more suppressed.
[0142] The total content of the thermosetting compound and the curing agent in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 30% by weight or more, more preferably 50% by weight or more, and preferably 98% by weight or less, more preferably 95% by weight or less. When the total content is equal to or more than the lower limit and equal to or less than the upper limit, the curability is more excellent and the thermal dimensional stability can be further improved.
[0143] [Cure accelerator] The curable resin film preferably contains a curing accelerator. The resin composition preferably contains a curing accelerator. The use of the curing accelerator further accelerates the curing speed. By quickly curing the resin composition or quickly curing the curable resin film, the crosslinked structure in the cured product becomes uniform and the number of unreacted functional groups decreases, resulting in a high crosslink density. The curing accelerator is not particularly limited, and a conventionally known curing accelerator can be used. The curing accelerator may be used alone or in combination of two or more.
[0144] Examples of the curing accelerator include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides.
[0145] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylolate. remellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.
[0146] Examples of the amine compound include diethylamine, triethylamine, diethylenetetramine, triethylenetetramine, and 4,4-dimethylaminopyridine.
[0147] When the curing agent contains the active ester compound, the curing accelerator preferably contains dimethylaminopyridine.
[0148] The phosphorus compound includes a triphenylphosphine compound.
[0149] Examples of the organometallic compound include zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, cobalt bisacetylacetonate (II), and cobalt trisacetylacetonate (III).
[0150] The peroxides include dicumyl peroxide and Perhexyl 25B.
[0151] From the viewpoint of further reducing the curing temperature and effectively suppressing warping of the cured product, the curing accelerator preferably contains the anionic curing accelerator, and more preferably contains the imidazole compound.
[0152] A peroxide curing accelerator may be used in combination with an anionic curing accelerator. In particular, when a vinyl compound and an epoxy compound are used in combination, the use of the above two types of curing accelerators may result in a better cured product.
[0153] From the viewpoint of further suppressing the curing temperature and effectively suppressing warping of the cured product, the content of the anionic curing accelerator in 100% by weight of the curing accelerator is preferably 20% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and most preferably 100% by weight (total amount). Therefore, it is most preferable that the curing accelerator is the anionic curing accelerator.
[0154] When the vinyl compound is used as the thermosetting compound, radical curing proceeds, so the curing accelerator preferably contains the radical curing accelerator, and more preferably is dicumyl peroxide or 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3. When the curable resin film is to be efficiently cured after precuring, a radical curing accelerator having a one-minute half-life temperature of 170°C or more and 200°C or less is more preferable. Commercially available radical curing accelerators having a one-minute half-life temperature of 170°C or more and 200°C or less include "Perhexyne 25B" manufactured by NOF Corporation.
[0155] The content of the curing accelerator in 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, and preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the curing accelerator is equal to or more than the lower limit and equal to or less than the upper limit, the resin composition and the curable resin film are cured efficiently. When the content of the curing accelerator is in a more preferred range, the storage stability of the curable resin film is further increased, and a better cured product is obtained.
[0156] [Thermoplastic resin] The curable resin film preferably contains a thermoplastic resin. The resin composition preferably contains a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl acetal resin, polyimide resin, and phenoxy resin. The thermoplastic resin may be used alone or in combination of two or more.
[0157] From the viewpoint of effectively lowering the dielectric tangent and effectively increasing the adhesion of the metal wiring regardless of the curing environment, the thermoplastic resin is preferably a phenoxy resin. By using the phenoxy resin, the deterioration of the embedding ability of the resin film in the holes or irregularities of the circuit board and the non-uniformity of the inorganic filler are suppressed. In addition, by using the phenoxy resin, the melt viscosity can be adjusted, so that the dispersibility of the inorganic filler is improved, and the resin composition or the B-stage product is less likely to wet and spread to unintended areas during the curing process.
[0158] The phenoxy resin contained in the curable resin film is not particularly limited. As the phenoxy resin, a conventionally known phenoxy resin can be used. The phenoxy resin may be used alone or in combination of two or more kinds.
[0159] Examples of the phenoxy resin include phenoxy resins having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a biphenyl skeleton, a novolac skeleton, a naphthalene skeleton, and an imide skeleton.
[0160] Commercially available examples of the phenoxy resin include "YP50", "YP55", and "YP70" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "1256B40", "4250", "4256H40", "4275", "YX6954BH30", and "YX8100BH30" manufactured by Mitsubishi Chemical Corporation.
[0161] From the viewpoints of improving handleability, plating peel strength at low roughness, and adhesion between the insulating layer and the metal layer, the thermoplastic resin is preferably a polyimide resin (polyimide compound).
[0162] From the viewpoint of obtaining a curable resin film having even better storage stability, the weight average molecular weight of the thermoplastic resin, the polyimide resin and the phenoxy resin is preferably 5,000 or more, more preferably 10,000 or more, and is preferably 100,000 or less, more preferably 50,000 or less.
[0163] The weight average molecular weights of the thermoplastic resin, the polyimide resin and the phenoxy resin indicate weight average molecular weights in terms of polystyrene measured by gel permeation chromatography (GPC).
[0164] The contents of the thermoplastic resin, the polyimide resin and the phenoxy resin are not particularly limited. In 100% by weight of the components in the curable resin film excluding the filler and the solvent, or in 100% by weight of the components in the resin composition excluding the filler and the solvent, the content of the thermoplastic resin is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less. When the content of the thermoplastic resin is equal to or more than the lower limit and equal to or less than the upper limit, the embedding property of the curable resin film in the hole or unevenness of the circuit board is improved. When the content of the thermoplastic resin is equal to or more than the lower limit, the formation of the curable resin film becomes easier, and a better insulating layer is obtained. When the content of the thermoplastic resin is equal to or less than the upper limit, the thermal expansion coefficient of the cured product becomes even lower. When the content of the thermoplastic resin is equal to or less than the upper limit, the surface roughness of the surface of the cured product becomes even smaller, and the adhesive strength between the cured product and the metal layer becomes even higher.
[0165] [solvent] The curable resin film does not contain or contains a solvent. The resin composition does not contain or contains a solvent. By using the solvent, the viscosity of the resin composition can be controlled within a suitable range, the coatability of the resin composition can be improved, and the curable resin film can be suitably obtained. The solvent may also be used to obtain a slurry containing the inorganic filler. Only one type of the solvent may be used, or two or more types may be used in combination.
[0166] Examples of the solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and naphtha, which is a mixture.
[0167] Most of the solvent is preferably removed when the resin composition is molded into a film. Therefore, the boiling point of the solvent is preferably 200°C or less, more preferably 180°C or less. The content of the solvent in the resin composition is not particularly limited. The content of the solvent can be appropriately changed in consideration of the coatability of the resin composition.
[0168] The content of the solvent in 100% by weight of the curable resin film is preferably 1% by weight or more, more preferably 2% by weight or more, and is preferably 10% by weight or less, more preferably 5% by weight or less.
[0169] When the curable resin film is a B-stage film, the content of the solvent in 100% by weight of the B-stage film is preferably 1% by weight or more, more preferably 2% by weight or more, and preferably 10% by weight or less, more preferably 5% by weight or less.
[0170] [Other ingredients] For the purpose of improving impact resistance, heat resistance, resin compatibility, workability, and the like, the curable resin film may contain a leveling agent, a flame retardant, a coupling agent, a colorant, an antioxidant, an ultraviolet degradation inhibitor, a defoaming agent, a thickener, a thixotropy imparting agent, and the like.
[0171] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a vinyl silane, an amino silane, an imidazole silane, an epoxy silane, etc.
[0172] (Other details of the curable resin film) The resin composition is molded into a film to obtain a curable resin film. The curable resin film is preferably a B-stage film (B-stage product).
[0173] Examples of a method for forming a resin composition into a film to obtain a curable resin film include the following methods: An extrusion molding method in which a resin composition is melt-kneaded and extruded using an extruder, and then molded into a film using a T-die or a circular die, etc. A casting molding method in which a resin composition containing a solvent is cast into a film. Other conventionally known film molding methods. The extrusion molding method and the casting molding method are preferred because they can be made thinner. The film includes a sheet.
[0174] The resin composition is molded into a film and dried by heating at, for example, 50° C. to 150° C. for 1 minute to 10 minutes to the extent that curing by heat does not proceed too much, to obtain a curable resin film that is a B-stage film.
[0175] The film-like resin composition obtained by the drying process as described above is called a B-stage film. The B-stage film is in a semi-cured state. The semi-cured product is not completely cured and can be further cured.
[0176] The curable resin film does not have to be a prepreg. When the curable resin film is not a prepreg, migration does not occur along the glass cloth or the like. In addition, when the curable resin film is laminated or precured, unevenness due to the glass cloth does not occur on the surface.
[0177] The curable resin film can be used in the form of a laminated film including a metal foil or a base film and a curable resin film laminated on the surface of the metal foil or the base film. The metal foil is preferably a copper foil.
[0178] Examples of the base film of the laminated film include polyester resin films such as polyethylene terephthalate film and polybutylene terephthalate film, olefin resin films such as polyethylene film and polypropylene film, and polyimide resin films. The surface of the base film may be subjected to a release treatment as necessary.
[0179] From the viewpoint of controlling the degree of curing of the curable resin film more uniformly, the thickness of the curable resin film is preferably 5 μm or more and preferably 200 μm or less. When the curable resin film is used as an insulating layer of a circuit, the thickness of the insulating layer formed by the curable resin film is preferably equal to or more than the thickness of the conductor layer (metal layer) forming the circuit. The thickness of the insulating layer is preferably 5 μm or more and preferably 200 μm or less.
[0180] The curable resin film may be wound into a roll of the curable resin film. The roll includes a winding core and the curable resin film. In the roll, the curable resin film is wound around the outer periphery of the winding core.
[0181] The dielectric loss tangent (Df) of the cured product of the curable resin film at 23° C. and a frequency of 5.8 GHz is preferably 3.00×10 -3 Less than or equal to 2.75×10 -3 Less than 2.50×10, more preferably -3 The following is particularly preferably 2.30×10 -3 Below, most preferably 2.10 x 10 -3 The dielectric loss tangent (Df) is 2.10×10 -3 or more, 2.30 x 10 -3 It may be more than that.
[0182] Specifically, the dielectric loss tangent (Df) of the cured product is measured as follows.
[0183] The curable resin film is heated to obtain a cured product of the curable resin film. The cured product of the curable resin film used to measure the dielectric loss tangent (Df) is preferably a cured product obtained by heating the curable resin film at 130°C for 60 minutes to provisionally cure it, and then heating it at 190°C for 90 minutes. The obtained cured product is cut into a size of 2 mm wide and 80 mm long, and 10 sheets are stacked together. The dielectric loss tangent is measured at room temperature (23°C) and a frequency of 5.8 GHz by the cavity resonance method using a "Cavity Resonance Perturbation Method Dielectric Constant Measurement Device CP521" manufactured by Kanto Electronics Application Development Co., Ltd. and a "Network Analyzer N5224A PNA" manufactured by Keysight Technologies, Inc.
[0184] The average coefficient of linear expansion (CTE) of the cured product of the curable resin film at 25° C. or more and 150° C. or less is preferably less than 50 ppm / ° C., more preferably 40 ppm / ° C. or less, even more preferably 35 ppm / ° C. or less, still more preferably 30 ppm / ° C. or less, particularly preferably 25 ppm / ° C. or less, and most preferably 22 ppm / ° C. or less. The average coefficient of linear expansion (CTE) may be 17 ppm / ° C. or more, or may be 19 ppm / ° C. or more.
[0185] More specifically, the average coefficient of linear expansion (CTE) of the cured product is measured as follows.
[0186] The curable resin film is heated to obtain a cured product of the curable resin film. The cured product of the curable resin film used to measure the average linear expansion coefficient (CTE) is preferably a cured product obtained by heating the curable resin film at 130°C for 60 minutes to provisionally cure it, and then heating it at 190°C for 90 minutes. The obtained cured product is cut into a size of 3 mm x 25 mm. Using a thermomechanical analyzer (for example, "EXSTAR TMA / SS6100" manufactured by SII NanoTechnology Co., Ltd.), the average linear expansion coefficient (ppm / °C) of the cut cured product from 25°C to 150°C is calculated under conditions of a tensile load of 33 mN and a heating rate of 5°C / min.
[0187] (Semiconductor devices, printed wiring boards, copper-clad laminates and multi-layer printed wiring boards) The above-mentioned curable resin film is suitably used for forming a molding resin in which a semiconductor chip is embedded in a semiconductor device.
[0188] The curable resin film is preferably used for replacing liquid crystal polymers (LCPs), millimeter wave antennas, rewiring layers, and low dielectric substrates. The curable resin film is not limited to the above applications and is preferably used for wiring formation applications in general.
[0189] The curable resin film is preferably used as an insulating material, and is preferably used for forming an insulating layer in a printed wiring board.
[0190] The printed wiring board can be obtained, for example, by hot-press molding the curable resin film.
[0191] A laminated target member having a metal layer on one or both sides can be laminated on the curable resin film. A laminated structure can be obtained by laminating a laminated target member having a metal layer on one or both sides on the curable resin film. The laminated structure includes a laminated target member having a metal layer on the surface and the curable resin film described above, and the curable resin film is laminated on the surface of the metal layer. The method of laminating the curable resin film and the laminated target member having the metal layer on the surface is not particularly limited, and a known method can be used. For example, the curable resin film can be laminated on a laminated target member having a metal layer on the surface while applying pressure with or without heating using a device such as a parallel plate press or a roll laminator.
[0192] The material of the metal layer is preferably copper.
[0193] The lamination target member having the metal layer on the surface thereof may be a metal foil such as a copper foil.
[0194] The curable resin film is preferably used to obtain a copper-clad laminate. An example of the copper-clad laminate is a copper-clad laminate including a copper foil and a curable resin film laminated on one surface of the copper foil.
[0195] The thickness of the copper foil of the copper-clad laminate is not particularly limited. The thickness of the copper foil is preferably within a range of 1 μm to 50 μm. In addition, in order to increase the adhesive strength between the cured product of the curable resin film and the copper foil, the copper foil preferably has fine irregularities on its surface. The method of forming the irregularities is not particularly limited. Examples of the method of forming the irregularities include a forming method by treatment using a known chemical solution.
[0196] The above-mentioned curable resin film is suitably used for obtaining a multilayer substrate.
[0197] An example of the multilayer board is a multilayer board including a circuit board and an insulating layer laminated on the circuit board. The insulating layer of the multilayer board is formed by the curable resin film. The insulating layer of the multilayer board may be formed by using a laminated film and the curable resin film of the laminated film. The insulating layer is preferably laminated on the surface of the circuit board on which the circuit is provided. A part of the insulating layer is preferably embedded between the circuits.
[0198] In the multilayer board, the surface of the insulating layer opposite to the surface on which the circuit board is laminated is preferably roughened.
[0199] The roughening treatment method is not particularly limited and may be any conventionally known roughening treatment method. The surface of the insulating layer may be subjected to a swelling treatment before the roughening treatment.
[0200] Preferably, the multilayer substrate further comprises a copper plating layer laminated on the roughened surface of the insulating layer.
[0201] Another example of the multilayer board is a multilayer board comprising a circuit board, an insulating layer laminated on the surface of the circuit board, and a copper foil laminated on the surface of the insulating layer opposite to the surface on which the circuit board is laminated. The insulating layer is preferably formed by using a copper-clad laminate comprising copper foil and a curable resin film laminated on one surface of the copper foil, and curing the curable resin film. Furthermore, the copper foil is preferably etched to form a copper circuit.
[0202] Another example of the multilayer board is a multilayer board including a circuit board and a plurality of insulating layers laminated on a surface of the circuit board. At least one of the insulating layers arranged on the circuit board is formed using the curable resin film. The multilayer board preferably further includes a circuit laminated on at least one surface of the insulating layer formed using the curable resin film.
[0203] The curable resin film according to the present invention is suitably used for forming an insulating layer in a printed wiring board, and is more suitably used for forming an insulating layer in a multilayer printed wiring board.
[0204] The multilayer printed wiring board includes, for example, a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, at least one of which is a cured product of the curable resin film.
[0205] FIG. 1 is a cross-sectional view that illustrates a multilayer printed wiring board using a curable resin film according to one embodiment of the present invention.
[0206] In the multilayer printed wiring board 11 shown in FIG. 1, a plurality of insulating layers 13-16 are laminated on the upper surface 12a of the circuit board 12. The insulating layers 13-16 are cured layers. A metal layer 17 is formed on a partial region of the upper surface 12a of the circuit board 12. Of the plurality of insulating layers 13-16, the insulating layers 13-15 other than the insulating layer 16 located on the outer surface opposite to the circuit board 12 side have the metal layer 17 formed on a partial region of the upper surface. The metal layer 17 is a circuit. The metal layer 17 is disposed between the circuit board 12 and the insulating layer 13, and between each of the laminated insulating layers 13-16. The lower metal layer 17 and the upper metal layer 17 are connected to each other by at least one of a via hole connection and a through hole connection not shown.
[0207] In the multilayer printed wiring board 11, the insulating layers 13-16 are formed of a cured product of the curable resin film. In this embodiment, the surfaces of the insulating layers 13-16 are roughened, so that fine holes (not shown) are formed on the surfaces of the insulating layers 13-16. The metal layer 17 reaches the inside of the fine holes. In the multilayer printed wiring board 11, the width dimension (L) of the metal layer 17 and the width dimension (S) of the portion where the metal layer 17 is not formed can be reduced. In the multilayer printed wiring board 11, good insulation reliability is provided between the upper metal layer and the lower metal layer that are not connected by via hole connection and through hole connection (not shown).
[0208] (Roughening treatment and swelling treatment) The curable resin film is preferably used to obtain a cured product to be subjected to roughening treatment or desmear treatment. The cured product also includes a pre-cured product which can be further cured.
[0209] In order to form fine irregularities on the surface of the cured product obtained by pre-curing the curable resin film, the cured product is preferably subjected to a roughening treatment. The cured product is preferably subjected to a swelling treatment before the roughening treatment. The cured product is preferably subjected to a swelling treatment after the pre-curing and before the roughening treatment, and is further preferably cured after the roughening treatment. However, the cured product does not necessarily have to be subjected to a swelling treatment.
[0210] As a method of the swelling treatment, for example, a method of treating the cured product with an aqueous solution or an organic solvent dispersion solution of a compound mainly composed of ethylene glycol or the like is used. The swelling liquid used in the swelling treatment generally contains an alkali as a pH adjuster or the like. The swelling liquid preferably contains sodium hydroxide. Specifically, for example, the swelling treatment is performed by treating the cured product with a 40 wt% ethylene glycol aqueous solution or the like at a treatment temperature of 30°C to 85°C for 1 minute to 30 minutes. The temperature of the swelling treatment is preferably within the range of 50°C to 85°C. If the temperature of the swelling treatment is too low, the swelling treatment takes a long time, and the adhesive strength between the cured product and the metal layer tends to be lowered.
[0211] In the roughening treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The roughening solution used in the roughening treatment generally contains an alkali as a pH adjuster. The roughening solution preferably contains sodium hydroxide.
[0212] The manganese compounds include potassium permanganate and sodium permanganate. The chromium compounds include potassium dichromate and potassium chromate anhydride. The persulfate compounds include sodium persulfate, potassium persulfate, and ammonium persulfate.
[0213] The arithmetic mean roughness Ra of the surface of the cured product is preferably 10 nm or more, preferably 300 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less. In this case, the adhesive strength between the cured product and the metal layer is increased, and finer wiring is formed on the surface of the insulating layer. Furthermore, conductor loss can be suppressed, and signal loss can be suppressed. The arithmetic mean roughness Ra is measured in accordance with JIS B0601:1994.
[0214] (Desmear processing) Through holes may be formed in the cured product obtained by pre-curing the curable resin film. In the multilayer board, etc., vias or through holes are formed as through holes. For example, vias can be formed by irradiating a laser such as a CO2 laser. The diameter of the via is not particularly limited, but is about 60 μm to 80 μm. Due to the formation of the through holes, smears, which are resin residues derived from the resin components contained in the cured product, are often formed at the bottom of the via.
[0215] In order to remove the smears, the surface of the cured product is preferably subjected to a desmear treatment. The desmear treatment may also serve as a roughening treatment.
[0216] In the desmear treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used, as in the roughening treatment. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The desmear treatment liquid used in the desmear treatment generally contains an alkali. The desmear treatment liquid preferably contains sodium hydroxide.
[0217] By using the above-mentioned curable resin film, the surface roughness of the surface of the desmeared cured product is sufficiently reduced.
[0218] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.
[0219] The following materials were prepared:
[0220] (thermosetting compound) Biphenyl-type epoxy compound ("NC-3000L" manufactured by Nippon Kayaku Co., Ltd.) Glycidylamine type epoxy compound (Mitsubishi Chemical Corporation "630") Resorcinol diglycidyl ether (Nagase Chemtex Corporation "EX-201") Naphthol aralkyl type epoxy compound ("ESN-475V" manufactured by Nippon Steel Chemical Co., Ltd.) Polybutadiene type epoxy compound (Daicel Corporation "PB-3600") Bismaleimide compound (synthesized according to Synthesis Example 1 below)
[0221] <Synthesis Example 1> In a 500 mL eggplant flask, 100 g of toluene, 36 g of N-methyl-2-pyrrolidone (NMP), and 6 g of methanesulfonic acid were placed. Then, 6.6 g (16 mmol) of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) and 12.5 g (64 mmol) of tricyclodecane diamine were added. Then, 17.7 g (60 mmol) of biphenyl dianhydride was added little by little. The eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having amines at both ends and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated and reacted. In this way, a compound having maleimide skeletons at both ends was obtained. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed to obtain a toluene solution. Next, the toluene solution was added to methanol to re-precipitate the product. Then, it was dried in a vacuum oven to obtain a bismaleimide compound having a cyclohexane ring.
[0222] (Inorganic filler) Silica-containing slurry (75% silica by weight: Admatechs "SC4050-HOA", average particle size 1.0 μm, aminosilane treatment, cyclohexanone 25% by weight)
[0223] (hardening agent) Active ester compound 1-containing liquid (DIC "HPC-8000L", solid content 65% by weight) Active ester compound 2-containing liquid (DIC Corporation "HPC-8150-62T", solid content 62% by weight) Active ester compound 3 (DIC "EXB-8", solid content 100% by weight, low molecular weight active ester compound) Phenol compound-containing liquid (DIC "LA-1356", solid content 60% by weight) Carbodiimide compound ("Carbodilite V-03" manufactured by Nisshinbo Chemical Co., Ltd., abbreviated as "V-03" in the table) Benzoxazine compound ("JBZ-BP100N" manufactured by JFE Chemical Corporation)
[0224] (Cure accelerator) Dimethylaminopyridine ("DMAP" manufactured by Wako Pure Chemical Industries, Ltd., anionic curing accelerator) 2-Phenyl-4-methylimidazole ("2P4MZ" manufactured by Shikoku Chemical Industry Co., Ltd., anionic curing accelerator)
[0225] (thermoplastic resin) Phenoxy resin (Mitsubishi Chemical Corporation "YX4000") Polyimide compound (polyimide resin, synthesized according to Synthesis Example 2 below, molecular weight 20,000)
[0226] <Synthesis Example 2> 600g of cyclohexanone was placed in a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube. Then, 30.1g of 1,12-dodecanediamine (manufactured by Tokyo Chemical Industry Co., Ltd.), 21.3g of 1,3-bisaminomethylcyclohexane (manufactured by Tokyo Chemical Industry Co., Ltd.), 61.5g of dimer diamine ("PRIAMINE1075" manufactured by Croda Japan Co., Ltd.), and 35.8g of bis(4-amino-3-methylcyclohexyl)methane (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed in the reaction vessel. After stirring these components, the solution in the reaction vessel was heated to 60°C. Next, 136.1g of pyromellitic dianhydride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added little by little. Then, 500g of anisole was added, and the mixture was stirred while performing an imidization reaction at 150°C for 6 hours to obtain a polyimide compound-containing solution. The molecular weight (weight average molecular weight) of the obtained polyimide compound was 20,000. The molar ratio of acid component / amine component was 1.04.
[0227] (Measurement of molecular weight) The molecular weights of the maleimide compound and the polyimide compound were determined as follows.
[0228] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.
[0229] Example 1 Preparation of resin composition: In a container, the silica-containing slurry, the thermosetting compound, and the curing agent in the amounts shown in Table 1 were placed, and the mixture was stirred with a disper at 33°C for 2 hours. After the mixture was uniformly mixed, the curing accelerator in the amount shown in Table 1 was placed, and the mixture was stirred with a disper for 1 hour. The temperature during the stirring was raised from 25°C and set to a final temperature of 33°C. Next, the thermoplastic resin in the amount shown in Table 1 was placed, and the mixture was stirred with a disper at 33°C for 30 minutes. The obtained varnish was left to stand at 25°C for 24 hours to cure, and a resin composition was obtained.
[0230] Preparation of curable resin film: The obtained resin composition was applied to the release-treated surface of a release-treated PET film (Toray Industries, Inc., "XG284", thickness 25 μm) using an applicator, and then dried for 2 minutes and 30 seconds in a gear oven at 100° C. to volatilize the solvent. In this way, a laminated film (a laminated film of a PET film and a curable resin film) was obtained in which a curable resin film (B-stage film) having a thickness of 40 μm was laminated on the PET film.
[0231] Example 2 Preparation of resin composition: In a container, the silica-containing slurry in the amounts shown in Table 1, the thermosetting compound other than the bismaleimide compound, and the curing agent were placed, and the mixture was stirred with a disper for 2 hours at 33°C. After the mixture was uniformly mixed, the curing accelerator in the amount shown in Table 1 was placed, and the mixture was stirred with a disper for 1 hour. The temperature during the stirring was raised from 25°C and set to 33°C. Next, the bismaleimide compound and the thermoplastic resin in the amounts shown in Table 1 were placed, and the mixture was stirred with a disper for 30 minutes at 33°C. The obtained varnish was left to stand at 25°C for 24 hours to cure, and a resin composition was obtained.
[0232] Preparation of curable resin film: In the same manner as in Example 1, a laminated film (a laminated film of a PET film and a curable resin film) was obtained.
[0233] Example 3 Preparation of resin composition: A resin composition was obtained in the same manner as in Example 1, except that the blending composition shown in Table 1 was used.
[0234] Preparation of curable resin film: In the same manner as in Example 1, a laminated film (a laminated film of a PET film and a curable resin film) was obtained.
[0235] Comparative Example 1 In a container, the thermosetting compound, the curing agent, the thermoplastic resin, and the solvent (cyclohexanone) in the amounts shown in Table 1 were placed, and the mixture was stirred for 2 hours at 33°C with a disper. Next, the silica-containing slurry in the amount shown in Table 1 was placed, and the mixture was stirred for 30 minutes with a disper. After the mixture was mixed uniformly, the curing accelerator in the amount shown in Table 1 was placed, and the mixture was stirred for 1 hour with a disper. The temperature during the stirring was raised from 25°C and set to 33°C at the end. Next, the thermoplastic resin in the amount shown in Table 1 was placed, and the mixture was stirred for 30 minutes at 33°C with a disper. The obtained varnish was left to stand at 25°C for 24 hours, and cured to obtain a resin composition.
[0236] Preparation of curable resin film: In the same manner as in Example 1, a laminated film (a laminated film of a PET film and a curable resin film) was obtained.
[0237] (evaluation) (1) Solid-state NMR spectroscopy The obtained curable resin film was temporarily cured by heating at 130°C for 60 minutes, and then heated at 190°C for 90 minutes to obtain a cured product of the curable resin film. The curable resin film and the cured product of the curable resin film were each measured and analyzed using a nuclear magnetic resonance apparatus ("ECZ-400R" manufactured by JEOL) under the above-mentioned solid-state NMR measurement conditions, function processing conditions, and baseline correction conditions, and the following were obtained.
[0238] 1) P1: The maximum peak intensity between 0 ppm and 50 ppm in the solid-state NMR spectrum (1). 2) P2: The maximum peak intensity between 0 ppm and 50 ppm in the solid-state NMR spectrum (2) 3) Peak intensity ratio: Ratio of P2 to P1 (P2 / P1) 4) In the solid-state NMR spectrum (1), the number of peaks having a peak intensity of 1.5 times or more the average intensity of the spectrum in the range from 0 ppm to 50 ppm.
[0239] Fig. 2 shows the solid-state NMR spectrum (normalized by the maximum peak intensity between 100 ppm and 200 ppm) obtained in Example 1. Fig. 2(a) shows the solid-state NMR spectrum of the curable resin film obtained in Example 1. Fig. 2(b) shows the solid-state NMR spectrum of the cured product of the curable resin film obtained in Example 1.
[0240] In addition, in the solid-state NMR spectrum (1), the peak detected at 41.47 ppm was assigned to the chemical shift value of cyclohexyl, and the peaks detected at 26.64 ppm and 24.76 ppm were assigned to the chemical shift values of linear alkyl chains.
[0241] (2) Flexibility of the curable resin film A winding core (diameter: 3 inches) was prepared. 10 m of a 500 mm wide curable resin film was wound around the outer circumference of the winding core to prepare a roll. The obtained roll was stored at room temperature for 3 hours and then stored in a freezer for 48 hours. After storage, the curable resin film was unwound from the winding core. The unwound curable resin film was left to stand for 2 hours, and the length of the winding mark was observed.
[0242] [Criteria for determining flexibility of curable resin film] ○: The length of the roll mark is less than 3m △: The length of the rolling marks is 3m or more and less than 6m ×: The length of the roll mark is 6m or more
[0243] (3) Chipping of hardening resin film A 5 cm cut was made in the curable resin film with a cutter knife, the cut area was observed with a metallurgical microscope (Olympus "STM6"), and the number of film fragments was counted.
[0244] [Criteria for determining chipping of curable resin film] ○: 5 or less pieces of film △: More than 5 pieces of film but less than 20 pieces ×: More than 20 pieces of film
[0245] (4) Thermal dimensional stability of the cured resin film (average coefficient of linear expansion (CTE)) The obtained 40 μm thick curable resin film (B-stage film) was heated at 190°C for 90 minutes to obtain a cured product. The obtained cured product was cut into pieces of 3 mm x 25 mm. Using a thermomechanical analyzer (SII NanoTechnology's "EXSTAR TMA / SS6100"), the average linear expansion coefficient (ppm / °C) of the cut cured product from 25°C to 150°C was calculated under conditions of a tensile load of 33 mN and a heating rate of 5°C / min.
[0246] [Criteria for determining thermal dimensional stability of cured resin film] ○○: Average linear expansion coefficient is 25ppm / ℃ or less ○: Average linear expansion coefficient is more than 25 ppm / ℃ and less than 27 ppm / ℃ ×: Average linear expansion coefficient exceeds 27 ppm / ℃
[0247] (5) Dielectric tangent (Df) of the cured resin film The obtained 40 μm thick curable resin film (B-stage film) was heated at 190° C. for 90 minutes to obtain a cured product. The obtained cured product was cut into a size of 2 mm wide and 80 mm long, and 10 sheets were stacked together. The dielectric tangent was measured at room temperature (23° C.) and a frequency of 5.8 GHz by the cavity resonance method using a "Cavity Resonance Perturbation Method Dielectric Constant Measurement Device CP521" manufactured by Kanto Electronics Application Development Co., Ltd. and a "Network Analyzer N5224A PNA" manufactured by Keysight Technologies, Inc.
[0248] [Criteria for determining the dielectric tangent of cured resin film] 〇: Dielectric tangent is 4.0×10 -3 less than △: Dielectric tangent is 4.0×10 -3 Above 6.0×10 -3 less than ×: Dielectric tangent is 6.0×10 -3 End
[0249] The compositions and results are shown in Table 1 below.
[0250] [Table 1] [Explanation of symbols]
[0251] 11...Multilayer printed wiring board 12...Circuit board 12a…Top surface 13~16…Insulating layer 17...Metal layer
Claims
1. A curable resin film, The composition includes a compound having a linear group, an epoxy compound having an aromatic skeleton, an inorganic filler, and a curing agent, the linear group has an unsaturated bond, The content of the inorganic filler is 50% by weight or more based on 100% by weight of components excluding the solvent in the curable resin film; the curing agent comprises an active ester compound, A curable resin film having a peak intensity ratio represented by the following formula (X) of 0.95 or less. Peak intensity ratio=P2 / P1 (X) P1: the maximum value of the peak intensity at 0 ppm or more and 50 ppm or less in the solid-state NMR spectrum of the curable resin film normalized by the maximum value of the peak intensity at 100 ppm or more and 200 ppm or less P2: the maximum value of the peak intensity at 0 ppm or more and 50 ppm or less in the solid-state NMR spectrum of the cured product of the curable resin film normalized by the maximum value of the peak intensity at 100 ppm or more and 200 ppm or less.
2. The curable resin film according to claim 1 , wherein the peak intensity ratio represented by the formula (X) is less than 0.
7.
3. The curable resin film according to claim 1 or 2, wherein P1 is 0.5 or more.
4. The curable resin film according to any one of claims 1 to 3, wherein the P2 is 0.5 or less.
5. The solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity at 100 ppm or more and 200 ppm or less has two or more peaks having a peak intensity of 1.5 times or more the average intensity of the spectrum at 0 ppm or more and 50 ppm or less. The curable resin film according to any one of claims 1 to 4.
6. In the solid-state NMR spectrum of the curable resin film normalized by the maximum peak intensity at 100 ppm or more and 200 ppm or less, there are two or more peaks having a peak intensity three times or more the average intensity of the spectrum at 0 ppm or more and 50 ppm or less. The curable resin film according to any one of claims 1 to 4.
7. in a solid-state NMR spectrum of the curable resin film normalized by the maximum value of peak intensity at 100 ppm or more and 200 ppm or less, a peak derived from a cyclic hydrocarbon skeleton is present at 0 ppm or more and 50 ppm or less, and a peak derived from a linear hydrocarbon skeleton is present at 0 ppm or more and 50 ppm or less, The curable resin film according to any one of claims 1 to 6, wherein the peak derived from the cyclic hydrocarbon skeleton and the peak derived from the linear hydrocarbon skeleton each have a peak intensity that is 1.5 times or more the average intensity of a spectrum from 0 ppm to 50 ppm.
8. A curable resin film described in any one of claims 1 to 7, comprising a thermosetting compound having an imide skeleton.
9. A curable resin film described in any one of claims 1 to 8, which contains a bismaleimide compound.
10. The curable resin film according to any one of claims 1 to 9, wherein the average linear expansion coefficient of the cured product of the curable resin film at 25°C or higher and 150°C or lower is less than 35 ppm / °C.
11. A winding core and The curable resin film according to any one of claims 1 to 10, The curable resin film is wound around the outer periphery of the winding core.
12. A lamination target member having a metal layer on a surface thereof; The curable resin film according to any one of claims 1 to 10, A laminated structure, wherein the curable resin film is laminated on a surface of the metal layer.
13. The laminate structure according to claim 12, wherein the material of the metal layer is copper.
14. A circuit board; a plurality of insulating layers disposed on a surface of the circuit board; a metal layer disposed between a plurality of the insulating layers; A multilayer printed wiring board, wherein at least one of the insulating layers is a cured product of the curable resin film according to any one of claims 1 to 10.
Citation Information
Patent Citations
Resin composition, resin sheet, printed wiring board, and semiconductor device
JP2018062570A
Resin material and multilayer printed wiring board
JP2020094213A
Resin material and multilayer printed wiring board
JP2020132881A
Interlayer insulating material and multilayer printed wiring board
WO2018062404A1