Section repair material and section repair mortar
A cross-sectional repair material with cement, fly ash, and silica fume, optimized for flow and strength, addresses pumping challenges and ensures uniformity and durability in concrete repairs.
Patent Information
- Application Number
- JP2021040104
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-12
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2041-03-12
AI Technical Summary
Conventional mortars for cross-section repair face issues with high fluidity leading to difficulty in pumping under pressure and non-uniform composition due to separation of solid content from water, and require improved compressive strength of the cured mortar product.
A cross-sectional repair material comprising cement, fly ash, fine aggregate, and silica fume, with specific ratios and ranges of these components, ensuring a flow value of 120-200 mm and inclusion of admixtures like expanding agents and water reducers, to enhance compressive strength and maintain fluidity for effective pumping.
The solution allows for high compressive strength, reduced drying shrinkage, and minimized material separation, enabling efficient pumping and uniform composition, thus improving the quality and durability of the repaired concrete structures.
Smart Images

Figure 0007579184000001 
Figure 0007579184000002 
Figure 0007579184000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cross-section repair material and a cross-section repair mortar. [Background technology]
[0002] The cross-section repair method is widely known as a method for repairing concrete structures deteriorated due to various causes. In the cross-section repair method, the deteriorated parts of the concrete are removed by chipping or the like, and the removed cross-section parts are repaired with cross-section repair mortar or grout material. The cross-section repair mortar is a mixture prepared by mixing a cross-section repair material containing cement, fine aggregate, etc. with water. Methods for covering the removed parts of the concrete with cross-section repair mortar include the filling method, the spraying method, and the plastering method. The filling method is a method in which a formwork is attached around the removed parts of the concrete, and the space between the removed parts of the concrete and the formwork is filled with cross-section repair mortar to repair the concrete. The spraying method is a method in which the removed parts of the concrete are repaired by spraying cross-section repair mortar. The plastering method is a method in which the removed parts of the concrete are repaired by manually applying cross-section repair mortar to them using a metal trowel, a wooden trowel, or the like.
[0003] In places where the cross-sectional area of the removed portion of deteriorated concrete is large, the filling method is widely used for repairing it. For the cross-sectional repair mortar used in the filling method, studies are being conducted to improve the fluidity of the mortar for cross-sectional repair in order to improve the filling ability of the mortar between the removed portion of concrete and the formwork.
[0004] Patent Document 1 describes a grout material that has the same or higher fluidity as conventional cement-based grout materials, but can prevent material separation and suppress or prevent cracks due to temperature stress or drying shrinkage in the cross section after repair. The grout material has a specific surface area of 5000 cm2 and is made of cement and blaine. 2 The document describes a grout material composition containing classified fly ash with a molecular weight of 1000 to 15000 kcal / g or more, a calcium sulfoaluminate-based expansion agent, a drying shrinkage reducing agent, and fine aggregate.
[0005] Furthermore, Patent Document 2 describes a cross-section repair material that contains Portland cement, fine aggregate, fly ash, an antifoaming agent, and a water-reducing agent as a mortar for repairing concrete structures that has excellent pumpability, fluidity, and self-filling properties. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5812836 [Patent Document 2] JP 2019-178035 A Summary of the Invention [Problem to be solved by the invention]
[0007] In the filling method, the mortar for repairing the cross section may be pumped to the construction site using a pump. However, with conventional mortar (grout material), pumping may not be possible if the fluidity becomes too high, and the solid content of the mortar may separate from the water after pumping, resulting in a non-uniform composition. The mortar described in Patent Document 2 has improved pumpability. However, it is desired that the compressive strength of the hardened mortar obtained by hardening the mortar described in Patent Document 2 is further improved.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a cross-section repair mortar that can be pumped and that can give a hardened mortar product with high compressive strength, and a cross-section repair material that can be advantageously used as a raw material for the cross-section repair mortar. [Means for solving the problem]
[0009] In order to solve the above problems, the cross-section repair material of the present invention contains cement, fly ash, fine aggregate and silica fume, and is characterized in that the content of the fine aggregate per 100 parts by mass of the total amount of the cement and the fly ash is in the range of 130 parts by mass or more and 170 parts by mass or less, the content of the silica fume per 100 parts by mass of the total amount of the cement and the fly ash is in the range of 6 parts by mass or more and 10 parts by mass or less, and the flow value measured by the method described below is in the range of 120 mm or more and 200 mm or less. (Method of measuring flow value) 32 parts by mass of water is added to 100 parts by mass of the total amount of the cement and the fly ash, and the mixture is kneaded to prepare a mortar. The flow value of the obtained mortar is measured in accordance with the Architectural Institute of Japan standard JASS 15M-103 (quality standard for self-leveling materials).
[0010] The cross-section repair material of the present invention thus constituted contains fine aggregate in the above range together with cement and fly ash, and therefore improves the compressive strength when made into a hardened mortar. Also, the mortar obtained by adding 32 parts by mass of water to 100 parts by mass of the total amount of cement and fly ash and kneading the mixture and containing silica fume in the above range has a flow value within the above range, so that it has high fluidity, can be pumped, and is unlikely to separate from the water and become non-uniform in composition after pumping.
[0011] In the cross-section repair material of the present invention, the fly ash has a Blaine specific surface area of 2500 cm 2 / g or more 5000cm 2 It is preferable that the molecular weight is in the range of less than 1 / g. In this case, since the Blaine specific surface area of the fly ash is within the above range, the compressive strength of the hardened mortar is high.
[0012] In the cross-section repair material of the present invention, the content of the fly ash relative to 100 parts by mass of the total amount of the cement and the fly ash is preferably within the range of 35 parts by mass or more and 50 parts by mass or less. In this case, since the fly ash content is within the above range, the fluidity of the mortar is improved, and the solids are less likely to separate from the water after pumping, resulting in an uneven composition. In addition, the amount of heat generated when the mortar hardens is reduced. Furthermore, the drying shrinkage rate of the hardened mortar is also reduced.
[0013] In addition, the cross-section repair material of the present invention preferably contains an expansive material in the range of 2.5 parts by mass to 4.5 parts by mass per 100 parts by mass of the total amount of the cement and the fly ash. In this case, since the expansive material is contained within the above range, drying shrinkage and the like can be suppressed when the mortar is hardened.
[0014] In addition, the cross-section repair material of the present invention preferably contains a water-reducing agent in the range of 0.1 part by mass to 0.5 part by mass per 100 parts by mass of the total amount of the cement and the fly ash. In this case, since the water reducing agent is contained within the above range, it becomes easier to maintain the flow value of the mortar within the above range.
[0015] In addition, the cross-section repair material of the present invention preferably contains a foaming agent in a range of 0.002 parts by mass or more and 0.020 parts by mass or less per 100 parts by mass of the total amount of the cement and the fly ash. In this case, since the foaming agent is contained within the above range, shrinkage during the initial stage of hardening can be suppressed by introducing gas into the hardened mortar to cause expansion.
[0016] The mortar for repairing cross sections of the present invention comprises cement, fly ash, fine aggregate, silica fume and water, and is characterized in that the content of the fine aggregate per 100 parts by mass of the total amount of the cement and the fly ash is within the range of 130 parts by mass or more and 170 parts by mass or less, the content of the silica fume per 100 parts by mass of the total amount of the cement and the fly ash is within the range of 6 parts by mass or more and 10 parts by mass or less, the content of the water per 100 parts by mass of the total amount of the cement and the fly ash is within the range of 26 parts by mass or more and 35 parts by mass or less, and the flow value measured in accordance with JASS 15M-103 (quality standard for self-leveling materials) of the Architectural Institute of Japan standard is within the range of 120 mm or more and 200 mm or less.
[0017] The cross-section repair mortar of the present invention thus constructed contains fine aggregate in the above-mentioned ranges together with cement and fly ash, improving the compressive strength of the hardened mortar. Also, since it contains silica fume and water in the above-mentioned ranges and has a flow value in the above-mentioned ranges, it has high fluidity, can be pumped, and is unlikely to separate from the water after pumping, resulting in a non-uniform composition.
[0018] Here, in the mortar for repairing a cross section of the present invention, the compressive strength at one day of age at an environmental temperature of 20°C is 15 N / mm 2 The compressive strength at 3 days at an environmental temperature of 5°C is 15N / mm 2 More preferably, it is equal to or greater than this. In this case, the construction period can be shortened because the compressive strength at one day is the above value at an environmental temperature of 20°C. Also, the compressive strength at three days is the above value at an environmental temperature of 5°C, so the construction period can also be shortened in winter.
[0019] Furthermore, in the mortar for repairing cross sections of the present invention, a test specimen having a dimension of 4 x 4 x 16 cm is used in accordance with Japanese Industrial Standard JIS A 1129-3:2010 (Method for measuring change in length of mortar and concrete - Part 3: Dial gauge method), and the specimen is demolded one day after molding, the base length is measured, and it is preferable that the length change rate when stored for 91 days in a constant temperature and humidity chamber at a temperature of 20°C and a relative humidity of 60% is 0.05% or less. In this case, the shape of the hardened mortar is unlikely to change, so that concrete structures repaired using this material are unlikely to develop cracks or chips over the long term.
[0020] In addition, it is preferable that the cross-section repair mortar of the present invention has a temperature rise of 33°C or less when it is poured into a cylindrical formwork having a diameter of 10 cm and a height of 20 cm in an environment of 20°C and the temperature is measured in an insulated state. In this case, the amount of heat generated when the mortar hardens is small, so that the hardened mortar is less likely to crack or chip due to stress accompanying an increase in temperature. Effect of the Invention
[0021] According to the present invention, it is possible to provide a cross-section repair mortar that can be pumped and that can produce a hardened mortar product with high compressive strength, and a cross-section repair material that can be advantageously used as a raw material for the cross-section repair mortar. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, a cross-section repair material and a cross-section repair mortar according to one embodiment of the present invention will be described.
[0023] [Cross-section repair material] The cross-section repair material according to an embodiment of the present invention is a cement composition containing cement, fly ash, fine aggregate, and silica fume. The cross-section repair material may contain admixtures such as an expansive agent, a water-reducing agent, a foaming agent, and a defoaming agent. The cross-section repair material is used as a raw material for preparing a cross-section repair mortar by kneading with water.
[0024] The flow value of the cross-section repair material, measured by the following method, is set to be within the range of 120 mm to 200 mm. Note that, if the cross-section repair material is a composition containing admixtures other than cement, fly ash, fine aggregate, and silica fume, the flow value is a value measured in the state of the composition containing the admixture.
[0025] (Method of measuring flow value) A predetermined amount of water is added to 100 parts by mass of the total amount of the cement and the fly ash, and the mixture is kneaded to prepare mortar. The flow value of the obtained mortar is measured in accordance with the Architectural Institute of Japan standard JASS 15M-103 (quality standard for self-leveling materials). 15M-103 is, for example, published in "Standard Specifications for Building Construction and Commentary 15 Plastering Work 2019 Edition, published by the Architectural Institute of Japan." The flow value is measured at 20°C.
[0026] If the flow value is too low, it may be difficult to pump the mixture by pumping. On the other hand, if the flow value is too high, the solids may separate from the water after pumping, resulting in a non-uniform composition. The flow value is preferably in the range of 130 mm to 190 mm.
[0027] (cement) As the cement, various cements that are used as raw materials for cross-sectional repair materials, such as ordinary Portland cement, early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, blast-furnace cement, etc., can be used. The cement is preferably ordinary Portland cement.
[0028] (Fly ash) Fly ash is a granular material formed by the aggregation of coal ash particles produced by the combustion of coal in the boilers of coal-fired power plants. Fly ash is generally spherical in shape, and the ball-bearing effect of the spherical particles improves the fluidity and self-compacting properties of mortar, as well as improving pumpability. For example, fly ash has a Blaine specific surface area of 2500 cm.2 / g or more 5000cm 2 / g, and may be in the range of less than 2500 cm 2 / g or more 4800cm 2 / g or less. If the Blaine specific surface area is too small, the fly ash particles become coarse, which may reduce the pozzolanic activity and reduce the strength development of the mortar. In addition, the ball bearing effect of the spherical particles of the fly ash may be weakened, which may reduce the fluidity of the mortar and reduce the self-filling ability. On the other hand, if the Blaine specific surface area is too large, that is, if the fly ash particles become too fine, it may easily form agglomerated particles and reduce the fluidity.
[0029] The content of the fly ash may be within the range of 35 parts by mass to 50 parts by mass based on 100 parts by mass of the total amount of the cement and the fly ash. If the content of the fly ash is too low, the effect of adding the fly ash may not be obtained. On the other hand, if the content of the fly ash is too high, the fluidity of the mortar may decrease, the pumpability may decrease, and the strength and resistance to carbonation of the hardened product of the mortar may decrease.
[0030] There is no particular limitation on the fine aggregate, and any known fine aggregate used as a fine aggregate for cross-section repair materials can be used. Examples of fine aggregate that can be used include mountain sand, river sand, land sand, crushed sand, sea sand, and silica sand No. 3 to 8.
[0031] The content of fine aggregate is set to be within the range of 130 to 170 parts by mass per 100 parts by mass of the total amount of cement and fly ash. If the content of fine aggregate is too low, there will be too little fine aggregate to serve as a dispersion medium when adding water and mixing to make mortar, and it may not be possible to mix well. In addition, drying shrinkage and autogenous shrinkage will increase when the mortar is hardened, and cracks may occur in the repaired area. On the other hand, if the content of fine aggregate is too high, the fine aggregate may settle and separate in the mortar, and the strength of the hardened mortar may decrease.
[0032] (Silica fume) Silica fume is a fine silicon oxide powder with a particle size of 1 μm or less. Silica fume improves the fluidity of mortar and also inhibits the separation of materials in the mortar.
[0033] The content of silica fume is set to be within the range of 6 to 10 parts by mass per 100 parts by mass of the total amount of cement and fly ash. If the content of silica fume is too low, the flow value of the mortar may become too high, and the materials in the mortar may become more likely to separate. On the other hand, if the content of silica fume is too high, the flow value of the mortar may become too low, and the mortar may become difficult to pump. The content of silica fume is preferably within the range of 7 to 9 parts by mass per 100 parts by mass of the total amount of cement and fly ash.
[0034] (Expansion material) Expansive agents have the effect of compensating for drying shrinkage and the like when the mortar is hardened by its expansion action, and suppressing the occurrence of cracks when the mortar is hardened. As the expansive agent, known materials used as expansive agents for cross-section repair materials such as ettringite-based, lime-based, and ettringite-lime composite-based materials can be used.
[0035] The content of the expansive agent is preferably in the range of 2.5 to 4.5 parts by mass per 100 parts by mass of the total amount of cement and fly ash. If the content of the expansive agent is too low, the above-mentioned effects of the expansive agent may not be fully exhibited. On the other hand, if the content of the expansive agent is too high, the mortar may undergo expansion cracks due to excessive expansion when hardened, resulting in a decrease in strength.
[0036] (Antifoaming agent) The defoaming agent has the effect of suppressing the generation of coarse bubbles when made into mortar and improving the fluidity. As the defoaming agent, for example, known materials used as defoaming agents for cross-section repair materials, such as ethers, fatty acid esters, fatty acid amides, higher alcohols, highly polymerized glycols, silicones, etc., can be used.
[0037] The content of the defoaming agent is preferably in the range of 0.03 parts by mass to 2.0 parts by mass to 100 parts by mass of the total amount of cement and fly ash, and more preferably in the range of 0.05 parts by mass to 1.5 parts by mass. If the content of the defoaming agent is too small, the above-mentioned effects of the defoaming agent may not be fully exhibited. On the other hand, if the content of the defoaming agent is too large, not only will the defoaming effect not be increased, but there is also a risk of delayed hardening and reduced strength development when made into mortar. In addition, material costs will increase.
[0038] (foaming agent) The foaming agent has the effect of generating fine bubbles when made into mortar, thereby introducing bubbles into the hardened mortar, causing it to expand and suppressing shrinkage in the early stage of hardening. As the foaming agent, for example, a known material used as a foaming agent for non-shrink mortar, such as aluminum powder, can be used.
[0039] The content of the foaming agent is preferably in the range of 0.002 parts by mass or more and 0.020 parts by mass or less per 100 parts by mass of the total amount of cement and fly ash. If the content of the foaming agent is too low, the above-mentioned effects of the foaming agent may not be fully exhibited. On the other hand, if the content of the foaming agent is too high, the amount of bubbles in the hardened mortar may be too large, causing excessive expansion and reducing the strength.
[0040] (Water reducing agent) The water-reducing agent has the effect of increasing the dispersibility of cement and admixtures when made into mortar, and improving the fluidity of the mortar. As the water-reducing agent, a water-reducing agent, a high-performance water-reducing agent, an air-entraining water-reducing agent, and a high-performance air-entraining water-reducing agent can be used. As the material of the water-reducing agent, for example, a known material used as a water-reducing agent for a cross-section repair material, such as lignin sulfonate, oxyorganic acid salt, β-naphthalene sulfonate, polycarboxylate, melamine resin sulfonate, and creosote oil sulfonic acid condensate salt, can be used.
[0041] The content of the water reducing agent varies depending on the type of the water reducing agent, but is preferably in the range of 0.1 to 5.0 parts by mass relative to 100 parts by mass of the total amount of cement and fly ash, and more preferably in the range of 0.20 to 3.0 parts by mass. If the content of the water reducing agent is too low, the above-mentioned effect of the water reducing agent may not be fully exhibited, and the viscosity of the mortar may increase and the fluidity may not be improved. In addition, the flow value of the mortar may be too low, making it difficult to pump the mortar. On the other hand, if the content of the water reducing agent is too high, material separation may occur when the mortar is made, and there may be adverse effects such as delayed hardening of the mortar and reduced strength development.
[0042] (Other Ingredients) The cross-section repair material may further contain other admixtures and reinforcing fibers. Examples of the other admixtures include thickeners, air entraining agents, rust inhibitors, fast-hardening admixtures, setting regulators, organic short fibers, inorganic short fibers, re-emulsified powdered resins, and salt adsorbents.
[0043] (Manufacturing method) The cross-section repair material of this embodiment can be manufactured by mixing the above-mentioned materials. As a mixer, a typical powder mixer such as a rocking mixer, a V-type mixer, a vertical mixer, a universal mixer, or a proshare mixer can be used.
[0044] According to the cross-section repair material of the present embodiment, the content of fine aggregate is in the range of 130 parts by mass to 170 parts by mass to 100 parts by mass of the total amount of cement and fly ash, so that the compressive strength of the hardened mortar is improved. In addition, the content of silica fume is in the range of 6 parts by mass to 10 parts by mass to 100 parts by mass of the total amount of cement and fly ash, and the mortar obtained by adding 32 parts by mass of water to 100 parts by mass of the total amount of cement and fly ash and kneading has a flow value in the range of 120 mm to 200 mm, so that the mortar has high fluidity, can be pumped, and is unlikely to separate from the water after pumping, resulting in an uneven composition. Therefore, the cross-section repair material of the present embodiment can be advantageously used for cross-section repair by filling method.
[0045] In the cross-section repair material of this embodiment, the fly ash has a Blaine specific surface area of 2500 cm 2 / g or more 5000cm 2 If the content is within the range of less than 1 / g, the simplified adiabatic temperature rise (heat generation) when the mortar is hardened will be small.
[0046] In the cross-section repair material of this embodiment, when the content of fly ash is within the range of 35 parts by mass to 50 parts by mass relative to 100 parts by mass of the total amount of cement and fly ash, the fluidity of the mortar is improved, and the solid content is less likely to separate from the water after pumping, resulting in a non-uniform composition. In addition, the amount of heat generated when the mortar hardens is reduced. Furthermore, the drying shrinkage rate of the hardened mortar is reduced.
[0047] In the cross-section repair material of this embodiment, if the water-reducing agent is contained in a range of 0.1 to 0.5 parts by mass per 100 parts by mass of the total amount of cement and fly ash, the flow value when made into mortar is more easily maintained within the above range.
[0048] In the cross-section repair material of this embodiment, when the foaming agent is contained in a range of 0.002 parts by mass or more and 0.020 parts by mass or less per 100 parts by mass of the total amount of cement and fly ash, shrinkage during the initial hardening period can be suppressed by introducing gas into the hardened mortar to cause it to expand.
[0049] [Mortar for repairing sections] The mortar for repairing a cross section of this embodiment includes cement, fly ash, fine aggregate, silica fume, and water. The cross section repair material may include admixtures such as an expansion agent, a water reducing agent, a foaming agent, and a water reducing agent. The admixtures such as cement, fly ash, fine aggregate, silica fume, an expansion agent, a water reducing agent, a foaming agent, and a water reducing agent are the same as those in the case of the above-mentioned cross section repair. In addition, the mortar for repairing a cross section has a flow value measured in accordance with the Architectural Institute of Japan standard JASS 15M-103 (quality standard for self-leveling materials) when a predetermined amount of water is added and mixed, within a range of 120 mm or more and 200 mm or less.
[0050] The water content is set to be within the range of 26 to 35 parts by mass per 100 parts by mass of the total amount of cement and fly ash. If the water content is too low, the fluidity of the mortar will decrease significantly, and it may become impossible to pump it using a pressure pump. On the other hand, if the water content is too high, the fluidity will be too high and material separation may occur.
[0051] The mortar for repairing the cross section has a compressive strength of 15N / mm2 at 1 day of age at an ambient temperature of 20℃. 2 The compressive strength at 3 days at an environmental temperature of 5°C is 15N / mm 2 The compressive strength of the hardened mortar may be 15N / mm 2If the concrete is more than this, even if the formwork is removed from the hardened mortar, problems such as the repaired part falling off or the hardened mortar cracking are unlikely to occur. Therefore, the compressive strength at one day at an environmental temperature of 20°C is 15N / mm 2 This means that the construction period can be shortened. In addition, the compressive strength at 3 days at an environmental temperature of 5°C is 15N / mm 2 The above means that the form can be removed relatively quickly even in winter, and the construction period can be shortened in the same way as at 20°C.
[0052] The mortar for repairing the cross section may be a specimen with dimensions of 4×4×16 cm, which is measured by demolding the specimen one day after molding and measuring the base length. The length change rate (hereinafter also referred to as drying shrinkage rate) when stored for 91 days in a constant temperature and humidity room at a temperature of 20°C and a relative humidity of 60% may be 0.05% or less. The drying shrinkage rate is an index of the ease of change in shape due to drying when the mortar is hardened. In the "Structure Construction Management Guidelines" published by the Expressway Research Institute Co., Ltd., drying shrinkage is listed as a performance inspection item for repairing the cross section by the pouring method, and the drying shrinkage rate after a storage period of three months is specified as 0.05% or less as a standard value. Therefore, if the drying shrinkage rate is 0.05% or less, it is considered that cracks due to drying shrinkage of the mortar are unlikely to occur.
[0053] The mortar for repairing the cross section may have a temperature rise of 33°C or less when it is poured into a cylindrical formwork with a diameter of 10 cm and a height of 20 cm in an environment of 20°C and the temperature is measured in an adiabatic state (hereinafter, also referred to as a simplified adiabatic temperature rise). The temperature of the mortar for repairing the cross section poured into the cylindrical formwork rises due to heat generated by the hardening reaction. The simplified adiabatic temperature rise is the maximum temperature reached by the mortar minus the environmental temperature (20°C). If the simplified adiabatic temperature rise becomes too high, the shape of the mortar filled in the formwork may change due to internal stress caused by the temperature rise, and cracks or defects may occur in the obtained hardened mortar. For this reason, the "Pier Deterioration Investigation and Repair Manual" published by Tokyo Port Terminal Corporation specifies the heat of hydration as the quality standard value for the cross section repair material, and the manual states that "the heat of hydration should be as small as possible," and it is preferable that the temperature rise is as small as possible.
[0054] (Method of preparing mortar for cross-section repair) The mortar for repairing the cross section can be prepared by mixing the cross section repair material with water. The cross section repair material and water can be mixed by adding the cross section repair material to a container or mixer that already contains a predetermined amount of water while stirring, but this method is not limited to this. As a mixing device, a mortar mixer, grout mixer, hand mixer, etc. can be used.
[0055] According to the mortar for repairing a cross section of the present embodiment, the content of the fine aggregate is in the range of 130 parts by mass to 170 parts by mass relative to 100 parts by mass of the total amount of cement and fly ash, so that the compressive strength of the hardened mortar is improved. In addition, the content of silica fume is in the range of 6 parts by mass to 10 parts by mass, the content of water is in the range of 26 parts by mass to 35 parts by mass, and the flow value is in the range of 120 mm to 200 mm relative to 100 parts by mass of the total amount of cement and fly ash, so that the mortar has high fluidity, can be pumped, and is unlikely to separate from the water after pumping, resulting in an uneven composition. Therefore, the mortar for repairing a cross section of the present embodiment can be advantageously used for repairing a cross section by filling method.
[0056] In the mortar for repairing sections of this embodiment, the compressive strength at one day of age at an environmental temperature of 20°C is 15 N / mm 2 If the compressive strength is 15N / mm2 or more at 3 days old at an environmental temperature of 5℃, the construction period can be shortened. 2 If this is the case, the construction period can be shortened even in winter.
[0057] In the case of the mortar for cross-section repair of this embodiment, if the drying shrinkage rate is 0.05% or less, the shape of the hardened mortar is unlikely to change, and concrete structures repaired using this are unlikely to develop cracks or defects over the long term.
[0058] In the case of the mortar for cross-section repair of this embodiment, when it is poured into a cylindrical formwork having a diameter of 10 cm and a height of 20 cm in an environment of 20°C and the temperature is measured in an insulated state, if the amount of temperature rise is 33°C or less, the amount of heat generated when the mortar hardens is small, so that the hardened mortar is less likely to crack or chip due to internal stress accompanying the rise in temperature of the mortar. EXAMPLES
[0059] The effects of the present invention will now be described in more detail with reference to examples. The types, names, manufacturers and abbreviations of the materials used in this example are shown in Table 1 below.
[0060] [Table 1]
[0061] The mortar obtained in this example was evaluated for the following items. (1) Flow value Measurements were performed in accordance with the Architectural Institute of Japan standard JASS 15M-103 (quality standards for self-leveling materials) published in "Standard Specifications for Construction Works, Commentary 15, Plastering Works 2019 Edition, published by the Architectural Institute of Japan." The measurement temperature was 20°C.
[0062] (2) Visual Observation The mortar was visually observed. When no separation of the mortar material was observed, it was rated as "good", and when separation of the mortar material was observed, it was rated as "separated".
[0063] (3) Compressive strength Measurements were performed in accordance with the compressive strength test method for mortar or cement paste using cylindrical specimens (JSCE-G 505-1999) published in the "2018 Standard Specifications for Concrete, Criteria Edition, edited by the Japan Society of Civil Engineers, Concrete Committee, Criteria-related Subcommittee." The size of the cylindrical specimen was 5cm in diameter and 10cm in height. The curing temperature was 20°C or 5°C. When the curing temperature was 20°C, compressive strength was measured at material ages of 1 day, 3 days, and 28 days. When the curing temperature was 5°C, compressive strength was measured at material ages of 3 days.
[0064] (4) Drying shrinkage rate (storage for 91 days) The dimensions of the specimen for drying shrinkage were 4 x 4 x 16 cm. Drying shrinkage was measured in accordance with the Japanese Industrial Standard JIS A 1129-3:2010 (Method for measuring change in length of mortar and concrete - Part 3: Dial gauge method). After 1 day of age, the specimen was demolded and the base length was measured. The specimen was then stored in a constant temperature and humidity room at a temperature of 20°C and a relative humidity of 60%, and the rate of change in length after 91 days of storage was measured as the drying shrinkage.
[0065] (5) Simplified adiabatic temperature rise In an environment of 20°C, the mortar was poured into a cylindrical formwork with a diameter of 10 cm and a height of 20 cm, and then the cylindrical formwork was placed in a polystyrene foam container (30 cm long x 30 cm wide x 40 cm high) and covered with a lid to create an insulated state. The maximum temperature reached at the center of the mortar was measured with a thermocouple, and the value obtained by subtracting 20°C from the maximum temperature reached was determined as the simplified adiabatic temperature rise. The time from preparation of the mortar to pouring it into the cylindrical formwork was within 30 minutes.
[0066] [Examples 1 to 5 of the present invention, Comparative Examples 1 to 12] A cement composition was produced by mixing cement, fly ash, aggregate, silica fume, expansive agent, antifoaming agent, foaming agent, and water reducing agent using a V-type mixer in the amounts of raw materials shown in Tables 2 to 4 below. The resulting cement composition and water were mixed using a mortar mixer in a ratio of 32 parts by mass of water per 100 parts by mass of the total amount of cement and fly ash in the cement composition, to produce mortar.
[0067] The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The mortar was pumped using a mortar pump OKP-50M (manufactured by Okasan Kiko Co., Ltd.: motor output: 3.7 kW, discharge capacity: 1 to 5 m 3 The mortar was pumped using a pumping speed of 1000 / h over a pumping distance of 50 m. The flow value and compressive strength of the mortar after pumping were measured. The results are shown in Tables 2 to 4.
[0068] In Tables 2 to 4, SF / (N+FA) is the silica fume content when the total amount of cement and fly ash is 100 parts by mass, S / (N+FA) is the aggregate content when the total amount of cement and fly ash is 100 parts by mass, and Water / (N+FA) is the water content when the total amount of cement and fly ash is 100 parts by mass.
[0069] In Tables 2 to 4, the rate of change in flow value after pumping is a value calculated from the following formula. Rate of change after pumping (%) = {(Flow value after pumping - Flow value before pumping) / Flow value before pumping} x 100 The pumpability was evaluated as follows: mortar flow value after pumping within ±20% was rated as "good", and others were rated as "poor".
[0070] In Tables 2 to 4, the rate of change in compressive strength after pumping is a value calculated from the following formula. Rate of change after pumping (%) = {(compressive strength after pumping - compressive strength before pumping) / compressive strength before pumping} x 100
[0071] [Table 2]
[0072] [Table 3]
[0073] [Table 4]
[0074] As shown in Table 2, the mortars of Examples 1 to 4 of the present invention, which have a silica fume content (SF / (N+FA)) in the range of 6 parts by mass or more and 10 parts by mass per 100 parts by mass of the total amount of cement and fly ash, and have flow values of 120 mm or more and 200 mm or less, have small rates of change in flow value after pumping and in compressive strength after pumping, and show little change in physical properties due to pumping.
[0075] In contrast, as shown in Table 3, the mortar of Comparative Example 1, in which both the silica fume content and flow value were lower than the range of the present invention, could not be pumped. The mortars of Comparative Examples 2 and 3, in which the silica fume content was lower than the range of the present invention and the flow value was within the range of the present invention, could be pumped, but the rate of change in the flow value after pumping of the mortar was large. The mortar of Comparative Example 4, in which the silica fume content was lower than the range of the present invention and the flow value was higher than the range of the present invention, could be pumped, but separation of materials occurred in the mortar after pumping. The mortars of Comparative Examples 5 and 6, in which the silica fume content (SF / (N+FA)) was within the range of the present invention and the flow value was lower than the range of the present invention, could not be pumped.
[0076] As shown in Table 4, the mortars of Comparative Examples 7 and 8, in which the silica fume content was within the range of the present invention and the flow value was higher than the range of the present invention, could be pumped, but the mortar after pumping experienced separation of materials. The mortar of Comparative Example 9, in which the silica fume content (SF / (N+FA)) was higher than the range of the present invention and the flow value was lower than the range of the present invention, could not be pumped. The mortars of Comparative Examples 10 and 11, in which the silica fume content (SF / (N+FA)) was higher than the range of the present invention and the flow value was within the range of the present invention, could be pumped, but the rate of change in the flow value after pumping of the mortar was large. In addition, the mortar of Comparative Example 12, in which both the silica fume content and flow value were higher than the range of the present invention, could be pumped, but the mortar after pumping experienced separation of materials.
[0077] From the above results, it was confirmed that in order to enable pumping, it is effective to set both the silica fume content and flow value of the mortar within the ranges of the present invention.
[0078] [Examples 6 to 9 of the present invention] A cement composition was produced in the same manner as in Example 3 of the present invention, except that the blending amounts of cement and fly ash were set to the amounts shown in Table 5 below. Then, water was added to the obtained cement composition so that the water / (N+FA) ratio was 32 to produce a mortar. The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The results are shown in Table 5 below, together with the results of Example 3 of the present invention.
[0079] [Table 5]
[0080] As shown in Table 5, as the cement content in the total amount of cement and fly ash increases, the compressive strength increases and the drying shrinkage rate and simple adiabatic temperature rise tend to increase.
[0081] [Examples 11 to 14] A cement composition was produced in the same manner as in Example 3 of the present invention, except that the amount of the expansive agent was set to the amount shown in Table 6 below. Then, water was added to the obtained cement composition so that the water / (N+FA) ratio was 32 to produce a mortar. The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The results are shown in Table 6 below, together with the results of Example 3 of the present invention.
[0082] [Table 6]
[0083] The results in Table 6 show that the drying shrinkage rate tends to decrease as the amount of expansive agent increases.
[0084] [Examples 15-16 of the present invention, Comparative Examples 13-14] A cement composition was produced in the same manner as in Example 3 of the present invention, except that the amount of fine aggregate was set to the amount shown in Table 7 below. Then, water was added to the obtained cement composition so that the water / (N+FA) ratio was 32 to produce a mortar. The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The results are shown in Table 7 below, together with the results of Example 3 of the present invention.
[0085] [Table 7]
[0086] From the results in Table 7, it can be seen that the mortars of Examples 3 and 15 to 16 of the present invention, in which the amount of fine aggregate is within the range of 130 to 170 parts by mass, have higher compressive strength than the mortars of Comparative Examples 13 to 14, in which the amount of fine aggregate is outside this range. It can also be seen that the drying shrinkage rate and simplified adiabatic temperature rise tend to decrease as the amount of fine aggregate increases.
[0087] [Examples 17 to 20] A cement composition was produced in the same manner as in Example 3 of the present invention, except that the amount of the water reducing agent was set to the amount shown in Table 8 below. Then, water was added to the obtained cement composition so that the water / (N+FA) ratio was the amount shown in Table 8 below, to produce a mortar. The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The results are shown in Table 8 below, together with the results of Example 3 of the present invention.
[0088] [Table 8]
[0089] In Examples 17 to 20 of the present invention, the amount of water reducing agent and water was adjusted so that the mortar flow value was within the range of 157 to 164 mm. The results in Table 8 show that when the amount of water mixed is within the range of 26 to 35 (water / (N+FA)), the compressive strength tends to be high and the drying shrinkage rate tends to be low.
[0090] [Examples 21 and 22] Fly ash FA1 (Blaine specific surface area: 3670 cm 2 / g), FA2 (Blaene specific surface area: 4740 cm 2 / g), FA3 (Blaine specific surface area: 5450 cm 2 A cement composition was produced in the same manner as in Example 3 of the present invention, except that 100% N / g of FA was used. Then, water was added to the obtained cement composition so that the water / (N+FA) ratio was 32%, to produce a mortar. The flow value, visual observation, compressive strength, drying shrinkage rate, and simplified adiabatic temperature rise of the obtained mortar were measured using the above-mentioned methods. The results are shown in Table 9 below, together with the results of Example 3 of the present invention.
[0091] [Table 9]
[0092] From the results in Table 9, it can be seen that as the Blaine specific surface area of fly ash increases, the drying shrinkage rate decreases and the simplified adiabatic temperature rise increases (the temperature becomes higher).
Claims
1. Contains cement, fly ash, fine aggregate and silica fume. the content of the fine aggregate is within a range of 130 parts by mass or more and 170 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, the content of the silica fume is within a range of 6 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, and the content of the fly ash is within a range of 20 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, A cross-section repair material characterized in that the flow value measured by the following method is in the range of 120 mm or more and 200 mm or less. (Method of measuring flow value) 32 parts by mass of water is added to 100 parts by mass of the total amount of the cement and the fly ash, and the mixture is kneaded to prepare a mortar. The flow value of the obtained mortar is measured in accordance with the Architectural Institute of Japan standard JASS 15M-103 (quality standard for self-leveling materials).
2. The fly ash has a Blaine specific surface area of 2500 cm 2 / g or more 5000cm 2 2. The cross section repair material according to claim 1, wherein the cross section repair material has a viscosity of less than 1000 MPa.
3. 3. The cross-section repair material according to claim 1, wherein the content of the fly ash is in the range of 35 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash.
4. The cross-section repair material according to any one of claims 1 to 3, characterized in that it contains an expansive material in a range of 2.5 parts by mass or more and 4.5 parts by mass or less per 100 parts by mass of the total amount of the cement and the fly ash.
5. The cross-section repair material according to any one of claims 1 to 4, characterized in that it contains a water reducing agent in a range of 0.1 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the total amount of the cement and the fly ash.
6. The cross-section repair material according to any one of claims 1 to 5, characterized in that it contains a foaming agent in a range of 0.002 parts by mass or more and 0.020 parts by mass or less per 100 parts by mass of the total amount of the cement and the fly ash.
7. Contains cement, fly ash, fine aggregate, silica fume and water. the content of the fine aggregate is within a range of 130 parts by mass or more and 170 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, the content of the silica fume is within a range of 6 parts by mass or more and 10 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, the content of the water is within a range of 26 parts by mass or more and 35 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, and the content of the fly ash is within a range of 20 parts by mass or more and 50 parts by mass or less relative to 100 parts by mass of the total amount of the cement and the fly ash, A mortar for repairing cross sections, characterized in that a flow value measured in accordance with JASS 15M-103 (quality standard for self-leveling materials) is within the range of 120 mm or more and 200 mm or less.
8. Compressive strength at 1 day at an environmental temperature of 20°C is 15 N / mm 2 The compressive strength at 3 days at an environmental temperature of 5°C is 15 N / mm 2 8. The cross section repair mortar according to claim 7, characterized in that:
9. The mortar for repairing cross sections according to claim 7 or 8, characterized in that a test specimen having a dimension of 4 x 4 x 16 cm is used in accordance with Japanese Industrial Standard JIS A 1129-3:2010 (Method for measuring change in length of mortar and concrete - Part 3: Dial gauge method), the specimen is demolded one day after molding, the base length is measured, and the mortar is stored for 91 days in a constant temperature and humidity room at a temperature of 20°C and a relative humidity of 60%, and the length change rate is 0.05% or less.
10. A mortar for repairing cross sections as described in any one of claims 7 to 9, characterized in that when poured into a cylindrical formwork having a diameter of 10 cm and a height of 20 cm in an environment of 20°C and the temperature is measured in an insulated state, the temperature rise is 33°C or less.
Citation Information
Patent Citations
Vehicle travel control unit
JP1983012836A
High-strength glass fiber reinforced concrete composition
JP1993078154A
Plasticizing additive for mortar and method of producing mortar using the same
JP2006069854A
Highly flowable non-shrinkage mortar
JP2006248831A
Wear-resistant concrete product and its manufacturing method
JP2007076956A