Catalyst for reducing nitrogen oxides

The nitrogen oxide storage catalyst with optimized washcoat layers enhances NOx storage and conversion efficiency, addressing low-temperature challenges and meeting Euro 6 standards by leveraging cerium oxide, alkaline earth metals, and noble metals for improved catalyst compatibility.

JP7579260B2Active Publication Date: 2024-11-07UMICORE AG & CO KG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021542171
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-18
Filing Date
2020-02-18
Publication Date
2024-11-07
Estimated Expiration
2040-02-18

AI Technical Summary

Technical Problem

Existing nitrogen oxide storage catalysts face challenges in achieving efficient NOx storage and conversion, especially at low exhaust temperatures, and require improved compatibility between different catalyst components to meet stringent emission standards like Euro 6d.

Method used

A nitrogen oxide storage catalyst comprising specific washcoat layers with defined compositions and arrangements, including cerium oxide, alkaline earth and alkali metal compounds, platinum, palladium, and rhodium, supported on a carrier material, optimized for spatial separation and enhanced interaction.

Benefits of technology

The catalyst achieves high NOx conversion rates across a wide temperature range, including low temperatures, without adverse effects, making it suitable for Euro 6 applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579260000002
    Figure 0007579260000002
  • Figure 0007579260000001
    Figure 0007579260000001
Patent Text Reader

Abstract

The present invention relates to a nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, wherein washcoat layer A is disposed on the support and contains cerium oxide, an alkaline earth metal compound, and / or an alkali metal compound, and platinum or platinum and palladium in a weight ratio of >5:1; washcoat layer B is disposed on washcoat layer A and contains cerium oxide, and platinum or platinum and palladium in a weight ratio of >5:1, and is free of alkali metal compounds and compounds of calcium, strontium and barium; washcoat layer C is disposed on washcoat layer B and contains cerium oxide-supported palladium or palladium and platinum, and rhodium in a weight ratio of >2:1; and washcoat layer D is disposed on washcoat layer C and contains platinum or platinum and palladium, and a method for converting NOx in exhaust gases from vehicles operated with a lean-burn engine.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for reducing nitrogen oxides contained in the exhaust gas of a lean-burn combustion engine. [Background technology]

[0002] The exhaust gas from automobiles operated with lean-burn combustion engines such as diesel engines contains carbon monoxide (CO) and nitrogen oxides (NO x ), as well as components resulting from incomplete combustion of the fuel in the combustion chambers of the cylinders. In addition to residual hydrocarbons (HC), which are usually present mainly in gas form, these also contain particulate emissions, also called "diesel soot" or "soot particles". These are complex agglomerates mainly from carbonaceous particulate matter and an adherent liquid phase, usually containing mainly long-chain hydrocarbon aggregates. The liquid phase that adheres to the solid components is also called "soluble organic fraction (SOF)" or "volatile organic fraction (VOF)".

[0003] In order to purify such exhaust gases, certain constituents must be converted as completely as possible into harmless compounds, which can only be achieved by using suitable catalysts.

[0004] To remove nitrogen oxides, so-called nitrogen oxide storage catalysts, commonly referred to as "lean NOx traps" or LNTs, are known. Their purification action is based on the fact that during lean engine operating phases, the nitrogen oxides are stored by the storage material of the storage catalyst, mainly in the form of nitrates, which are decomposed again during the subsequent rich engine operating phases, and the nitrogen oxides thus released are converted into nitrogen, carbon dioxide and water by the reducing exhaust gas components in the storage catalyst. This operating principle is described, for example, in the SAE document SAE 950809.

[0005] As storage materials, oxides, carbonates or hydroxides of magnesium, calcium, strontium, barium, alkali metals, rare earth metals or mixtures thereof are considered in particular. As a result of their alkaline properties, these compounds form nitrates with the acidic nitrogen oxides of the exhaust gas and are thus able to store the nitrogen oxides. The storage materials are deposited in the most highly dispersed form possible on suitable support materials in order to provide a large interaction surface with the exhaust gas. As a rule, nitrogen oxide storage catalysts also contain precious metals such as platinum, palladium and / or rhodium as catalytically active components. The task of these catalysts is, on the one hand, to oxidize NO to NO2 and CO and HC to CO2 under lean conditions, and, on the other hand, to reduce the released NO2 to nitrogen during rich operating phases in which the nitrogen oxide storage catalyst is regenerated.

[0006] A further well-known method for removing nitrogen oxides from exhaust gases in the presence of oxygen is selective catalytic reduction (SCR method) with ammonia over a suitable catalyst. In this method, the nitrogen oxides to be removed from the exhaust gases are converted to nitrogen and water using ammonia. The ammonia used as reducing agent can be made available by feeding ammonia precursor compounds, such as urea, ammonium carbamate or ammonium formate, into the exhaust gas stream and subsequent hydrolysis.

[0007] For example, certain metal-exchanged zeolites can be used as SCR catalysts, in particular iron-exchanged beta zeolites and copper-exchanged small-pore zeolites (e.g., chabazite), depending on the application. Also used as SCR catalysts are so-called mixed oxide catalysts. These are in particular vanadium oxide, tungsten oxide, and optionally further oxide-containing compounds, generally containing titanium dioxide as the oxide support.

[0008] To meet Euro 6d and future exhaust gas legislation, exhaust systems must be used that exhibit high CO and NOx conversion rates over a wide temperature range. Such systems may be a combination of a nitrogen oxide storage catalyst and an SCR catalyst, where the nitrogen oxide storage catalyst in particular must meet stringent requirements. Efficient NOx storage and conversion is therefore a major challenge, especially in urban driving where exhaust temperatures do not exceed 200°C. The nitrogen oxide storage catalyst must also provide sufficient NO2 for effective NOx conversion by the SCR catalyst.

[0009] For example, nitrogen oxide storage catalysts have been shown to be most active when different components or functions of the catalyst are spatially separated to avoid undesirable interactions. Thus, WO 2011 / 154913 discloses a catalyst consisting of three layers superimposed on a catalyst substrate, the bottom layer containing a nitrogen oxide storage material, the middle layer containing a material for reacting nitrogen oxides and the top layer containing a hydrocarbon storage material.

[0010] WO 2017 / 191099 describes a catalyst in which three material regions are arranged in a specific manner on a support. Further nitrogen oxide storage catalysts consisting of at least two layers are disclosed in EP 0 885 650 (A2), WO 2009 / 158453 (A1), WO 2012 / 029050 (A1), WO 2014 / 108362 (A1), WO 2017 / 134065 (A1) and WO 2017 / 144426 (A1). Summary of the Invention [Problem to be solved by the invention]

[0011] However, further developed nitrogen oxide storage catalysts, in particular with further improved NOx storage, NO2 formation and reduction capacities and further adapted to one another, may be required in the future. [Means for solving the problem]

[0012] The present invention relates to a nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, washcoat layer A is disposed on a support and contains cerium oxide, an alkaline earth metal compound, and / or an alkali metal compound, and platinum or platinum and palladium in a weight ratio of >5:1; washcoat layer B is disposed on washcoat layer A and contains cerium oxide and platinum or platinum and palladium in a weight ratio of >5:1, and is free of alkali metal compounds and compounds of calcium, strontium, and barium; washcoat layer C is disposed on washcoat layer B and comprises palladium on cerium oxide or palladium and platinum, and rhodium in a weight ratio of >2:1; Washcoat layer D is disposed on washcoat layer C and comprises platinum or platinum and palladium.

[0013] In one embodiment of the present invention, washcoat layer B is free of alkali metal compounds and alkaline earth metal compounds.

[0014] In another embodiment of the present invention, the washcoat layer B comprises magnesium oxide (MgO). In this case, the washcoat layer B preferably comprises magnesium oxide in an amount of 3 to 20 g / l relative to the volume of the support.

[0015] In a further embodiment of the nitrogen oxide storage catalyst according to the invention, washcoat layers A and B are combined to form a single layer comprising cerium oxide, an alkaline earth metal compound and / or an alkali metal compound, and platinum or platinum and palladium in a weight ratio of >5:1, this washcoat layer being referred to below as AB.

[0016] The cerium oxide used in the washcoat layers A, B and C may be of commercial quality, i.e., having a cerium oxide content of 90-100% by weight. Preferred is a cerium oxide having a cerium oxide content of at least 10 ml, even after calcination at 1150° C. for 6 hours. 2Cerium oxide having these surface properties is well known and is described, for example, in EP 1 527 018 B1.

[0017] In an embodiment of the invention, cerium oxide is used in the washcoat layer A in an amount of 110 to 160 g / l, for example 125 to 145 g / l, based on the volume of the support. In the washcoat layer B, cerium oxide is used in an amount of 22 to 120 g / l, for example 40 to 100 g / l or 45 to 65 g / l, based on the volume of the support.

[0018] In an embodiment of the nitrogen oxide storage catalyst according to the invention in which washcoat layers A and B are combined to form a single washcoat layer AB, cerium oxide is used in the washcoat layer AB in an amount of 132 to 280 g / l, for example 165 to 210 g / l, based on the volume of the support.

[0019] In the washcoat layer C, the amount of cerium oxide is in particular 20 to 120 g / l, preferably 40 to 70 g / l, relative to the volume of the support.

[0020] As the alkaline earth metal compound in the washcoat layer A, particularly preferred are oxides, carbonates and / or hydroxides of magnesium, strontium and / or barium, in particular magnesium oxide, barium oxide and strontium oxide.

[0021] The alkali metal compounds in the washcoat layer A are in particular the oxides, carbonates and / or hydroxides of lithium, potassium and / or sodium.

[0022] In an embodiment of the invention, the alkaline earth metal compound or alkali metal compound is present in the washcoat layer A in an amount of 10 to 50 g / l, in particular 15 to 20 g / l, calculated as alkaline earth metal oxide or alkali metal oxide, relative to the volume of the support.

[0023] In the embodiment of the nitrogen oxide storage catalyst according to the invention in which the washcoat layers A and B are combined to form a single washcoat layer AB, this contains an alkaline earth metal compound or an alkali metal compound, preferably in an amount of 10 to 50 g / l, in particular 15 to 20 g / l, calculated as alkaline earth metal oxide or alkali metal oxide, relative to the volume of the support.

[0024] In one embodiment of the invention, the washcoat layer C comprises an iron compound. The iron compound is preferably an iron oxide, in particular Fe2O3. The iron is especially present in the washcoat layer C in an amount of 1 to 10% by weight, preferably 2 to 7% by weight, relative to the weight of the washcoat layer C, calculated as Fe2O3.

[0025] It is preferred that iron compounds, whether iron oxide or another iron compound, are not used as support materials for any of the precious metals platinum, palladium and rhodium, or for any of the other components of the washcoat layer C.

[0026] The washcoat layer A contains platinum or platinum and palladium, preferably rhodium-free. When it contains platinum and palladium, the weight ratio Pt:Pd is >5:1, preferably ≧8:1, for example 8:1 to 20:1, for example 8:1, 10:1, 12:1, 14:1, 16:1, 18:1 or 20:1.

[0027] The washcoat layer B also contains platinum or platinum and palladium, preferably without rhodium. When it contains platinum and palladium, the weight ratio Pt:Pd is >5:1, preferably ≧8:1, for example 8:1 to 20:1, for example 8:1, 10:1, 12:1, 14:1, 16:1, 18:1 or 20:1.

[0028] The platinum or platinum and palladium contents and their weight ratios in washcoat layer A and washcoat layer B are independent of each other.

[0029] Typical platinum loadings for washcoat layers A and B range from 0.7 to 1.5 g / l and palladium loadings range from 0.035 to 0.3 g / l, relative to the volume of support, in each case.

[0030] The washcoat layer C preferably contains palladium or palladium and platinum in a weight ratio of preferably 2:1 to 8:1, preferably 4:1 to 6:1. The mass concentration of palladium or palladium and platinum relative to the amount of cerium oxide in the washcoat layer C is usually 0.2 to 1%, preferably 0.4 to 0.6%.

[0031] In addition, the washcoat layer C also contains rhodium, preferably in an amount of 0.003 to 0.35 g / l, in particular 0.18 to 0.26 g / l, in each case relative to the volume of the support.

[0032] The washcoat layer D contains platinum or platinum and palladium, preferably rhodium-free. When it contains platinum and palladium, the weight ratio Pt:Pd is >5:1, preferably ≧8:1, for example 8:1 to 18:1, for example 8:1, 10:1, 12:1, or 14:1.

[0033] The ratio of the amount of platinum and palladium in washcoat layer D to the total amount of platinum and palladium in washcoat layers A and B is usually 0.3 to 1.2, preferably 0.35 to 0.5.

[0034] In an embodiment of the present invention, the total amount of precious metals, i.e. platinum, palladium and, optionally, rhodium, in the nitrogen oxide storage catalyst according to the present invention is between 2.12 and 7.1 g / l (60 to 200 g / ft) relative to the volume of the support. 3 ).

[0035] The precious metals platinum or platinum and palladium are typically present on a suitable support material in washcoat layer A, washcoat layer B, and washcoat layer D. As such, in particular, 30 to 250 m 2 / g, preferably 100 to 200m2 Use is made of oxides having a BET surface area (determined in accordance with DIN 66132) of 1000 nm / g, such as aluminum oxide, silicon dioxide, titanium dioxide, but also mixed oxides, such as aluminum / silicon mixed oxides and cerium / zirconium mixed oxides.

[0036] In an embodiment of the invention, aluminum oxide is used as support material for the precious metals platinum or platinum and palladium, in particular such aluminum oxide is stabilized with 1 to 6% by weight, in particular 4% by weight, of lanthanum oxide.

[0037] In the washcoat layer C, the precious metals palladium and platinum are supported on cerium oxide, while rhodium is preferably present on one of the customary support materials mentioned above, ie in particular on aluminium oxide or lanthanum oxide-stabilised aluminium oxide.

[0038] The precious metals platinum or platinum and palladium, and rhodium are preferably supported only on one or more of the aforementioned support materials and therefore are not in intimate contact with all components of the respective washcoat layers. In particular, iron is preferably not used as a support for palladium, platinum, and rhodium.

[0039] In an embodiment of the invention, the total washcoat loading of the support is between 300 and 600 g / l of the support volume.

[0040] In a preferred embodiment, the present invention relates to a nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, - washcoat layer A is disposed on a support, Cerium oxide in an amount of 100 to 160 g / l relative to the volume of the support; platinum or platinum and palladium in a weight ratio of 10:1, magnesium oxide and / or barium oxide, washcoat layer B is disposed on washcoat layer A; Contains no alkali metal compounds, no calcium, strontium, or barium compounds, platinum or platinum and palladium in a weight ratio of 10:1, cerium oxide in an amount of 45 to 65 g / l relative to the volume of the support, Washcoat layer C is placed on washcoat layer B, ○Contains 40-70g / l of cerium oxide, Palladium and platinum are supported in an amount of 0.16 to 0.72 g / l based on the volume of the support, Rhodium in an amount of 0.18 to 0.26 g / l relative to the volume of the support; Fe2O3 in an amount of 2 to 7 g / l relative to the volume of the support, Washcoat layer D is disposed on washcoat layer C, Contains platinum or platinum and palladium in a weight ratio of 10:1.

[0041] The catalytically active washcoat layers A, B, C and D are applied onto the support by customary dip coating or pump and suck coating methods, followed by thermal post-treatment (calcination and reduction, if applicable, with forming gas or hydrogen), which methods are well known from the prior art.

[0042] The required coating suspension can be obtained according to methods well known to those skilled in the art. Thus, the components of the individual washcoat layers, such as cerium oxide, alkaline earth metal compounds and / or alkali metal compounds, precious metals supported on a suitable support material, and iron compounds, are mixed in a suitable mill, in particular a ball mill, with d 50 = 3-5 μm particle size and suspended in the corresponding amount.

[0043] The nitrogen oxide storage catalyst of the present invention is capable of reducing NO in exhaust gas from automobiles operated with lean-burn engines such as diesel engines. xThese catalysts achieve good NOx conversion at temperatures of approximately 200-450° C., without adversely affecting the NOx conversion at higher temperatures. The nitrogen oxide storage catalysts according to the invention are therefore suitable for Euro 6 applications.

[0044] Therefore, the present invention also relates to a method for reducing NOx in exhaust gases from automobiles operating with lean-burn engines, such as diesel engines. x The present invention also relates to a method for converting exhaust gases, characterized in that the exhaust gases are passed over a nitrogen oxide storage catalyst according to the invention.

[0045] The embodiment of the method according to the invention with respect to the nitrogen oxide storage catalyst corresponds to what is described above.

[0046] Thus, the present invention provides a) a nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, a washcoat layer A is disposed on the support and contains cerium oxide, an alkaline earth metal compound, and / or an alkali metal compound, and platinum or platinum and palladium in a weight ratio of >5:1; a washcoat layer B is disposed on the washcoat layer A and contains cerium oxide and platinum or platinum and palladium in a weight ratio of >5:1, and is free of alkali metal compounds and compounds of calcium, strontium, and barium; a washcoat layer C disposed on washcoat layer B and comprising palladium on cerium oxide or palladium and platinum, and rhodium in a weight ratio of >2:1; a washcoat layer D arranged on the washcoat layer C, the washcoat layer D comprising a nitrogen oxide storage catalyst, the nitrogen oxide storage catalyst comprising platinum or platinum and palladium; b) an SCR catalyst; and an exhaust gas system comprising the SCR catalyst.

[0047] In the exhaust gas system according to the invention, the SCR catalyst can in principle be selected from all catalysts active in the SCR reaction of nitrogen oxides with ammonia, in particular from those known to be conventional to the skilled person in the field of automotive exhaust gas catalysis, including catalysts of the mixed oxide type as well as catalysts based on zeolites, in particular transition metal exchanged zeolites, for example zeolites exchanged with copper, iron or copper and iron.

[0048] In an embodiment of the invention, a small pore zeolite with a maximum ring size of eight tetrahedral atoms and an SCR catalyst that is a transition metal, such as copper, iron, or copper and iron, is used. Such SCR catalysts are described, for example, in WO 2008 / 106519 (A1), WO 2008 / 118434 (A1), and WO 2008 / 132452 (A2).

[0049] Additionally, large and medium pore zeolites may be used, with particular consideration being given to those of the BEA structure type, thus iron-BEA and copper-BEA.

[0050] Particularly preferred zeolites belong to the BEA, AEI, CHA, KFI, ERI, LEV, MER or DDR structural type and are particularly preferably exchanged with copper, iron or copper and iron.

[0051] Within the context of the present invention, the term "zeolite" also includes molecular sieves, which are sometimes also called "zeolite-like" compounds. Molecular sieves are preferred if they belong to one of the aforementioned structural types. Examples include silica aluminum phosphate zeolites, known by the term "SAPO", and aluminum phosphate zeolites, known by the term "AlPO".

[0052] These are also preferred, especially when exchanged with copper, iron, or copper and iron.

[0053] Preferred zeolites are also those having a SAR (silica to alumina ratio) value of 2-100, in particular 5-50.

[0054] The zeolites or molecular sieves contain the transition metal, in particular in an amount of 1 to 10% by weight, in particular 2 to 5% by weight, calculated in particular as metal oxide, ie for example as Fe2O3 or CuO.

[0055] A preferred embodiment of the present invention contains as the SCR catalyst a beta type (BEA), chabazite type (CHA), or Levin type (LEV) zeolite or molecular sieve exchanged with copper, iron, or copper and iron. The corresponding zeolites or molecular sieves are known, for example, under the names ZSM-5, Beta, SSZ-13, SSZ-62, Nu-3, ZK-20, LZ-132, SAPO-34, SAPO-35, AlPO-34, and AlPO-35, see, for example, U.S. Patent Nos. 6,709,644 and 8,617,474.

[0056] In one embodiment of the exhaust gas system according to the invention, an injection device for the reducing agent is placed between the catalyst according to the invention and the SCR catalyst.

[0057] The injection device can be freely selected by the skilled person, and suitable devices can be obtained from the literature (see, for example, T. Mayer, Feststoff-SCR-System auf Basis von Ammoniumcarbamat, dissertation, TU Kaiserslautern, 2005). Ammonia can be injected into the exhaust gas stream via the injection device either as such or in the form of a compound from which ammonia is formed under ambient conditions. Examples of suitable compounds are aqueous solutions of urea or ammonium formate, and solid ammonium carbamate. Typically, the reducing agent or its precursor is available and kept in an associated container connected to the injection device.

[0058] The SCR catalyst is preferably in the form of a coating on a support, which can be, for example, a flow-through substrate or a wall-flow filter, and can be comprised of, for example, silicon carbide, aluminum titanate, or cordierite.

[0059] Alternatively, the support itself can be comprised of the SCR catalyst and matrix components described above, ie, in extruded form.

[0060] The invention also relates to a method for purifying exhaust gases from a motor vehicle operated with a lean-burn engine, such as a diesel engine, characterized in that the exhaust gases are passed through an exhaust gas system according to the invention.

[0061] The invention is explained in more detail in the following examples and figures. [Brief description of the drawings]

[0062] [Figure 1] 1 shows the NOx storage capacity at 70% NOx conversion as a function of the temperature before the catalyst for catalysts RK1, RK2, K1 and K2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0063] Comparative Example 1 a) An aqueous suspension was prepared for the washcoat layer A. Thus, 0.7 g / l platinum and 0.07 g / l palladium were added to an aqueous suspension of 34 g / l aluminum oxide as tetraethylammonium hydroxide or nitrate relative to the volume of the support. Then, 19.5 g / l cerium oxide coated with 17% BaO relative to the amount of cerium oxide and 45.5 g / l cerium oxide were added to the suspension. 3 g / l aluminum oxide was added as an alumina sol. Then, 102.5 g / l solids were applied by immersing the flow monolith, drying and calcining at 550° C. for 2 hours.

[0064] b) To prepare coating suspension B, 0.7 g / l of platinum was prepared as tetraethylammonium hydroxide and mixed with 40 g / l of aluminum oxide relative to the amount of solids of the suspension. Then, 148 g / l of cerium oxide, 0.07 g / l of palladium as Pd nitrate and 10 g / l of magnesium oxide as Mg acetate were added. An iron oxide component was used as a prefix powder. For this purpose, an aluminum oxide with 25% by weight of iron oxide was prepared by impregnating the aluminum oxide with an iron nitrate solution and subsequent calcination at 550°C. 20 g / l of this material was used in the coating suspension. In addition, 8 g / l of aluminum oxide and 0.18 g / l of rhodium as Rh nitrate were added to the suspension. 227 g / l was applied to washcoat layer A as washcoat layer B. The layer was then dried and calcined at 550°C for 2 hours.

[0065] c) Washcoat layer C was prepared by mixing 1.8 g / l platinum with respect to the weight of solids in washcoat suspension C, 0.18 g / l palladium as palladium nitrate and 70 g / l aluminium oxide as palladium nitrate. 72 g / l of this suspension was applied to washcoat layer B, dried and then calcined at 550° C. for 2 hours. The catalyst thus obtained is hereinafter referred to as RK1.

[0066] Comparative Example 2

[0067] Comparative Example 1 was repeated, differing in that in washcoat layer B, 50 g / l of cerium oxide was coated with 0.5% by weight palladium relative to the cerium oxide prior to addition to washcoat dispersion B, such that layer B contained 98 g / l of cerium oxide and 50 g / l of palladium-coated cerium oxide. The catalyst thus obtained is hereinafter referred to as RK2.

[0068] [Example 1] a) To prepare a catalyst according to the invention, a washcoat layer A was coated similarly to Comparative Examples 1 and 2.

[0069] b) To prepare coating suspension B, 0.7 g / l of platinum was prepared as tetraethylammonium hydroxide and mixed with 40 g / l of aluminum oxide relative to the amount of solids of the suspension. Then, 100 g / l of cerium oxide, 0.07 g / l of palladium as palladium nitrate and 10 g / l of magnesium oxide as magnesium acetate were added. 3 g / l of aluminum oxide was added as alumina sol. 154 g / l was applied to washcoat layer A as washcoat layer B. The layer was then dried and calcined at 550° C. for 2 hours.

[0070] c) To prepare the washcoat layer C, 0.25 g / l of palladium as palladium nitrate in aqueous suspension was adsorbed on 50 g / l of cerium oxide. To this suspension, an iron oxide component was added as a prefix powder. For this purpose, an aluminum oxide with 25% by weight of iron oxide was prepared by impregnating the aluminum oxide with an iron nitrate solution and subsequent calcination at 550°C. 20 g / l of this material was used in the coating suspension. In addition, 5 g / l of aluminum oxide and 0.18 g / l of rhodium as rhodium nitrate were added to the suspension. 75 g / l were applied to the washcoat layer B as washcoat layer C. The layer was then dried and calcined at 550°C for 2 hours.

[0071] d) Washcoat layer D corresponded to washcoat layer C in Comparative Examples 1 and 2. The catalyst thus obtained is hereinafter referred to as K1.

[0072] [Example 2] Example 2 was repeated, differing in that washcoat layer B contained 0.65 g / l platinum and washcoat layer C further contained 0.05 g / l platinum. The catalyst thus obtained is hereinafter referred to as K2.

[0073] test: To test the catalytic activity of catalysts RK1, RK2, K1 and K2, samples were first subjected to a heat pretreatment at 800° C. for 16 hours in an atmosphere of 10% oxygen, 10% water and balance nitrogen.

[0074] They were then heated to 650°C and exposed to the gas composition in Table 1 with a temperature ramp of 7.5 min-1 while a lean (oxidizing) gas atmosphere was induced over the catalyst samples for 150 seconds and a rich (reducing) gas atmosphere was induced over the catalyst samples for 30 seconds. NOx concentrations in the gas stream downstream of the catalyst were measured by FTIR.

[0075] [Table 1]

[0076] To determine the NOx conversion activity, the NOx storage mass in mg per catalyst volume was determined for each lean phase when the NOx conversion reached a value of 70%.

[0077] The NOx conversion is calculated using the following formula: NOx conversion rate [%] = 100x(c(NOx in )-c(NOx out )) / c(NOx out )

[0078] The stored mass of NOx is calculated from the difference between the mass of NOx in the gas upstream of the catalyst and the mass of NOx in the gas downstream of the catalyst from the start of the lean phase until the point at which 70% NOx conversion is achieved.

[0079] 1 shows the NOx storage values ​​at 70% NOx conversion as a function of temperature for the reference catalysts RK1 and RK2 and the catalysts K1 and K2 according to the invention. In the range of 175-250° C., a higher NOx storage is achieved with the four-layer design of the catalyst according to the invention. The use of palladium and platinum in catalyst K2 leads to a further increase in the NOx storage.

Claims

1. A nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, a washcoat layer A is disposed on the support and contains (1) cerium oxide, (2) an alkaline earth metal compound, and / or an alkali metal compound, and (3) platinum or platinum and palladium (in a weight ratio of platinum:palladium >5:1); a washcoat layer B is disposed on the washcoat layer A and also contains cerium oxide, and platinum or platinum and palladium (with a weight ratio of platinum:palladium >5:1), and is free of alkali metal compounds and compounds of calcium, strontium and barium; a washcoat layer C is disposed on the washcoat layer B and comprises cerium oxide-supported palladium or palladium and platinum (with a weight ratio of palladium:platinum >2:1) and rhodium; a washcoat layer D disposed on the washcoat layer C, the nitrogen oxide storage catalyst comprising platinum or platinum and palladium.

2. 2. The nitrogen oxide storage catalyst according to claim 1, wherein the washcoat layer B does not contain any alkali metal compounds or alkaline earth metal compounds.

3. 2. The nitrogen oxide storage catalyst according to claim 1, wherein the washcoat layer B contains magnesium oxide (MgO).

4. 4. The nitrogen oxide storage catalyst according to claim 3, wherein the washcoat layer B contains magnesium oxide in an amount of 3 to 20 g / l relative to the volume of the support.

5. 5. The nitrogen oxide storage catalyst according to claim 1, wherein the washcoat layer A contains cerium oxide in an amount of 110 to 160 g / l relative to the volume of the support.

6. 6. The nitrogen oxide storage catalyst according to claim 1, wherein the washcoat layer B contains cerium oxide in an amount of 22 to 120 g / l relative to the volume of the support.

7. 7. The nitrogen oxide storage catalyst according to claim 1, wherein the washcoat layer C contains cerium oxide in an amount of 20 to 120 g / l relative to the volume of the support.

8. 8. The nitrogen oxide storage catalyst according to claim 1, wherein the alkaline earth metal compound in the washcoat layer A is an oxide, carbonate, and / or hydroxide of magnesium, strontium, and / or barium.

9. 9. The nitrogen oxide storage catalyst according to claim 1, wherein the alkaline earth metal compound or alkali metal compound in washcoat layer A is present in an amount of 10 to 50 g / l, calculated as alkaline earth metal oxide or alkali metal oxide, relative to the volume of the support.

10. The nitrogen oxide storage catalyst according to any one of claims 1 to 9, wherein the washcoat layer C contains an iron compound.

11. 11. The nitrogen oxide storage catalyst according to claim 10, wherein the iron compound is iron oxide.

12. Iron oxide is present in the washcoat layer C in an amount of 1 to 10% by weight based on the weight of the washcoat layer C, and Fe 2 O 3 12. The nitrogen oxide storage catalyst according to claim 10 or 11, wherein the nitrogen oxide storage catalyst is calculated as follows:

13. The nitrogen oxide storage catalyst according to any one of claims 1 to 12, wherein the washcoat layer A does not contain rhodium.

14. NO in exhaust gas from automobiles operated with lean-burn engines x 14. A method for converting exhaust gases from nitrogen oxide storage catalyst according to claim 1, characterized in that the exhaust gases are directed over a nitrogen oxide storage catalyst according to claim 1.

15. 1. An exhaust gas system comprising: a) a nitrogen oxide storage catalyst comprising a support and washcoat layers A, B, C and D, a washcoat layer A is disposed on said support and also contains (1) cerium oxide, (2) an alkaline earth metal compound, and / or an alkali metal compound, and (3) platinum or platinum and palladium (in a weight ratio of platinum:palladium >5:1); a washcoat layer B is disposed on the washcoat layer A and also contains cerium oxide, and platinum or platinum and palladium (with a weight ratio of platinum:palladium >5:1), and is free of alkali metal compounds and compounds of calcium, strontium, and barium; a washcoat layer C is disposed on the washcoat layer B and comprises cerium oxide-supported palladium or palladium and platinum (with a weight ratio of palladium:platinum >2:1) and rhodium; a washcoat layer D disposed on the washcoat layer C and comprising a nitrogen oxide storage catalyst comprising platinum or platinum and palladium, and b) an SCR catalyst;

Citation Information

Patent Citations

  • Catalytic system for reducing nitrogen oxides