Hard-coated components

A DLC film with a periodically varying sp3/sp2 ratio addresses adhesion and stress issues, enhancing smoothness and wear resistance for cutting tools and sliding members.

JP7579502B2Active Publication Date: 2024-11-08MITSUBISHI MATERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2019144892
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-08-06
Publication Date
2024-11-08
Estimated Expiration
2039-08-06

AI Technical Summary

Technical Problem

DLC films face issues with poor adhesion to metal substrates due to high compressive stress and potential peeling, especially when thicker, and lack smoothness required for cutting tools and sliding members.

Method used

A DLC film with a sp3/sp2 ratio that continuously and periodically increases and decreases, providing improved adhesion and stress relief without an intermediate layer, ensuring high hardness and wear resistance.

Benefits of technology

The DLC film achieves smoothness, high adhesion, and enhanced wear resistance, leading to improved machining efficiency and tool life for cutting tools and longer life for sliding members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579502000004
    Figure 0007579502000004
  • Figure 0007579502000005
    Figure 0007579502000005
  • Figure 0007579502000001
    Figure 0007579502000001
Patent Text Reader

Abstract

To provide a member coated with a film including a DLC film that has smoothness required for cutting tools, sliding members, metal molds, motor vehicle components, and the like, as well as improved adhesion to the base materials, without the need for the inclusion of intermediate layers.SOLUTION: Provided is a coating member having a hard film coated on a base material, in which the hard film is a DLC film that is substantially free of hydrogen, a sp3 ratio defined by sp3 bond / (sp2 bond+sp3 bond) increases and decreases continuously and periodically from the substrate side to the film surface side, the average value of maximum values of the sp3 ratio is 0.7 to 0.9, the average value of minimum values of the sp3 ratio is 0.4 to 0.6, and a difference between the average value of the maximum values and the average value of the minimum values is 0.2 to 0.5.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a member coated with a hard coating including a DLC coating, which is suitable for applications such as cutting tools, sliding members, dies, and automobile parts, which require high adhesion and smoothness for the coating, and in particular for applications such as cutting tools. [Background technology]

[0002] DLC (Diamond-Like Carbon) coating has a diamond structure (sp 3 structure) and graphite structure (sp 2 It is an amorphous carbon coating that has a mixture of amorphous carbon and tantalum (structure) and has high hardness and excellent wear resistance, so it is widely used as a coating for cutting tools, sliding members, molds, automobile parts, etc.

[0003] DLC films have a problem that they have poor affinity with metal materials, and because they have very high compressive stress, they have poor adhesion to the substrate and are prone to peeling. For this reason, it has been considered to improve adhesion by providing an intermediate layer. However, when an intermediate layer is used, the manufacturing process becomes complicated because multiple raw materials are used, and even if the adhesion at the interface between the DLC film and the substrate is only strengthened by the intermediate layer, if the high compressive stress of the DLC film cannot be alleviated in the first place, the film may peel off when the film is made thicker. Therefore, in order to alleviate this compressive stress, it has been proposed to use a structure in which hard DLC films and soft DLC films are alternately laminated.

[0004] For example, Patent Document 1 describes a DLC coating in which, when a cross section is observed using a bright-field TEM image, white hard carbon layers (soft layers) shown in relative white and black hard carbon layers (hard phases) shown in black are alternately laminated in the thickness direction to a total thickness of more than 1 μm and not more than 50 μm, and the white hard carbon layers have regions that grow in a fan shape in the thickness direction.

[0005] Furthermore, for example, Patent Document 2 describes a DLC coating having a metal intermediate layer formed on the sliding surface side of a substrate, a laminated carbon film formed on the metal intermediate layer and consisting of alternately laminated first and second carbon films, and a hard carbon film formed on the laminated carbon film, wherein an image of the first carbon film in bright-field observation with a transmission electron microscope is brighter than an image of the second carbon film in bright-field observation with a transmission electron microscope, the thickness of the first carbon film is T1 and the thickness of the second carbon film is T2, T2 is more than 10 nm and 1000 nm or less, and T1 / T2 is 0.010 or more and 0.60 or less.

[0006] Furthermore, for example, Patent Document 3 describes a DLC coating which is a laminated coating in which two types of layers with different hardness are laminated in multiple layers (excluding cases where only two layers are laminated), the difference in hardness between the two types of layers is 500 to 1700 HV, the layer with the higher hardness has a thickness equal to or greater than the layer with the lower hardness, and the thickness of the entire coating is 5.0 μm or more. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 6273563 [Patent Document 2] JP 2017-53435 A [Patent Document 3] Patent No. 5977322 Summary of the Invention [Problem to be solved by the invention]

[0008] The DLC coating described in Patent Document 1 has a problem in that the film is not smooth due to the presence of fan-shaped precipitates in the film. In addition, in Patent Documents 2 and 3, there is a risk of the film peeling off at the interface between the hard DLC coating and the soft DLC coating.

[0009] Therefore, an object of the present invention is to solve the above-mentioned problems and to provide a member coated with a DLC film that does not have an intermediate layer and has the smoothness required for cutting tools, sliding members, dies, automotive parts, etc., and has improved adhesion to a substrate. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to improve the adhesion of smooth DLC coatings, which are required for cutting tools, sliding members, molds, automobile parts, and the like. As a result, the sp 3 The researchers have gained the novel discovery that by forming a DLC coating in which the ratio increases and decreases continuously and periodically, it is possible to obtain a hard coating that is smooth, relieves compressive stress, improves peeling resistance, is thick, has high hardness, and has excellent abrasion resistance.

[0011] That is, the present invention is based on this finding and is as follows. (1) On the substrate Without an intermediate layer, A coated member coated with a hard coating, The hard coating is a DLC coating that does not substantially contain hydrogen, and is leather sp toward the membrane surface 3 join / (sp 2 join+sp 3 sp defined as 3 The ratio is linear and that it increases and decreases periodically. The above sp 3 The average value of the maximum ratio is 0.7 to 0.9. The above sp 3 The average value of the minimum ratio is 0.4 to 0.6. the difference between the average value of the maximum value and the average value of the minimum value is 0.2 to 0.5; A covering member comprising: (2) The coated member according to (1) above, wherein the average value of the period is 15 to 500 nm. (3) The coated member according to (1) or (2) above, wherein the hard coating has a thickness of 350 to 2000 nm." Effect of the Invention

[0012] Since the members coated with the hard coating of the present invention are smooth and have high adhesion and wear resistance, it is possible to obtain cutting tools with higher processing efficiency and tool life, sliding members, dies, automobile parts, and the like with long life. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram showing the positions of the π* and σ* peaks of a DLC film and graphite. [Diagram 2] FIG. 2 is a schematic diagram showing that the sp3 ratio of the hard coating increases and decreases continuously and periodically (the number of periods is 2). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Next, the hard coating of the present invention will be described in more detail. In this specification and claims, when a numerical range is expressed as "X to Y", the range includes the upper and lower numerical limits (i.e., from X to Y). When no unit is specified for X and only Y, the unit of X is the same as the unit of Y.

[0015] 1. Base material The substrate is selected according to the application of the coated member and is not particularly limited, and examples thereof include steel, cemented carbide, Ti-based alloy, Al-based alloy, Cu-based alloy, ceramics, and resin materials. Examples of steel include structural carbon steel, alloy steel, tool steel, and stainless steel.

[0016] 2.Hard coating The hard coating does not substantially contain hydrogen, and the sp 3 join / (sp 2 join+sp 3bond) represented by sp 3 This is a DLC coating in which the ratio increases and decreases continuously and periodically. In the claims and the description of this specification, sp 3 The ratio "periodically increases and decreases" when 3 This refers to a change in the ratio that "decreases from the maximum value to the minimum value and then increases from the minimum value to the maximum value in each half of the cycle" or "increases from the minimum value to the maximum value and then decreases from the maximum value to the minimum value in each half of the cycle" repeated one or more times.

[0017] (1)sp 3 ratio sp 3 The ratio sp 3 join / (sp 2 join+sp 3 The bond was analyzed by line analysis from the interface between the substrate and the hard coating to the surface of the hard coating using electron energy loss spectroscopy (ELLS). 2 Integrated intensity of bond-derived peaks, sp 3 The integrated intensity of the peak resulting from the binding is measured and calculated. As shown in Figure 1, the EELS spectrum of carbon-based materials shows sp 2 The 1s→π* peak due to the bond, and the sp peak around 290-300 eV 2 Bonds and sp 3 The peaks of 1s and σ* due to the sp bond are overlapped. 3 In order to extract only the intensity of the 1s → σ* bond, sp 2 Graphite, a material composed only of bonds, is used as a reference sample. The integrated intensity of the graphite peak around 285 eV is G π* is the integrated intensity of the DLC peak, D π* The integrated intensity of the graphite peak seen in the vicinity of 290-300 eV is G σ* is the integrated intensity of the DLC peak, D σ* Then, sp 3 The ratio can be calculated using the following formula: sp 3 Ratio=1-(D π* / D σ* ) / (G π* / Gσ* )

[0018] (2)sp 3 Continuous and cyclical changes in ratios In the hard coating, sp 3 The ratio increases and decreases continuously and periodically. Here, increasing and decreasing continuously and periodically means that sp 3 This means that there are alternating regions of increasing and decreasing ratios. 3 Plot the increase or decrease in the ratio on a graph, calculate the average line of that change, and if this line is sp 3 Find the maximum and minimum values ​​for each area crossing the graph of the increase or decrease in the ratio. Here, this line is drawn so that the area surrounded by the line and the curve showing the repeated change is equal on both sides of the line. Note that sp 3 Since the ratio is a set of discontinuous measurement points measured at a specified interval, the maximum and minimum values ​​are not defined mathematically; rather, the maximum value is the value of a measurement point where an increase turns to a decrease, and the minimum value is the value of a measurement point where a decrease turns to an increase.

[0019] It is preferable that the average of the maximum values ​​is 0.7 to 0.9, and the average of the minimum values ​​is 0.4 to 0.6. The reasons for this are as follows. The reason for setting the average of the maximum values ​​to 0.7 to 0.9 is that sp 3 If the ratio is less than 0.7, the film strength will be insufficient, and there is a possibility that the film will be damaged when an external force is applied, and the resistance to welding will be poor. On the other hand, if the ratio exceeds 0.9, the stress will be high and the adhesive strength will be reduced. The reason for setting the average of the minimum values ​​to 0.4 to 0.6 is that if it is less than 0.4, the film strength is insufficient and there is a possibility that the film will be damaged when an external force is applied, whereas if it exceeds 0.6, the entire film will become hard and the stress relaxation effect and impact relaxation effect will not be obtained.

[0020] Here, the difference between the average of the maximum value and the average of the minimum value is preferably 0.2 to 0.5. The reason is that if the difference between the average of the maximum value and the average of the minimum value is less than 0.2, a sufficient stress relaxation effect cannot be obtained, and the adhesive strength decreases, while if it exceeds 0.5, sp 3 This is because there are areas with a low ratio, and therefore the membrane may be damaged when an external force is applied.

[0021] Also, sp 3 The average period of increase and decrease in the ratio is preferably 15 to 500 nm, because if it is less than 15 nm, a clear periodic structure is not formed, resulting in a hard coating with low abrasion resistance and adhesion resistance, whereas if it exceeds 500 nm, sufficient stress relaxation effect and impact relaxation effect cannot be obtained. Here, the period refers to the interval between adjacent maximum values ​​or between adjacent minimum values.

[0022] (3) Thickness of the hard coating The thickness of the hard coating depends on the application, but is preferably 350 to 2000 nm, because within this range, sufficient stress relaxation effect, impact relaxation effect, and peeling resistance effect are easily obtained.

[0023] (4) Bright field TEM image The hard film was thinned using a focused ion beam (FIB) and observed under a bright-field transmission electron microscope (TEM). 3 The lower ratio is white, and the higher ratio is black. 3 In a hard coating, the ratio of which increases and decreases continuously and periodically, the periodic presence of white and black areas can be seen in a bright-field TEM image as shown diagrammatically in Figure 2.

[0024] (5) Indentation hardness of hard coating The indentation hardness, i.e., nanoindentation hardness, of the hard coating is preferably 50 to 80 GPa. This is because, when used as a cutting tool in which hardness must be taken into consideration, if the hardness is less than 50 GPa, sufficient wear resistance and adhesion resistance cannot be obtained, whereas if the hardness exceeds 80 GPa, the coating may peel off due to high compressive stress. Nanoindentation hardness is a method of determining hardness on a nanometer scale by pressing a diamond indenter into a sample placed on a stage, obtaining a load-displacement curve, and calculating the hardness of the sample on the basis of the resistance force of the sample.

[0025] (6) Surface roughness of hard coating The surface roughness of a hard coating depends on the application. For example, the arithmetic surface roughness of the substrate surface is R a1 , the arithmetic surface roughness of the hard coating surface is R a2 Then, R a2 and R a1 Difference R a2 -R a1 It is preferable that R is 10 nm or less. a2 -R a1 If the thickness exceeds 10 nm, there is a risk that the film will be damaged when an external force is applied, and there is also a risk that adhesion of the opposing material will occur when the film is used for tools or dies.

[0026] 3. Manufacturing method The hard coating can be produced, for example, by using a PVD method (AIP: Arc Ion Plating) in such a way that the bias voltage applied to the substrate at the start of hard coating formation is -100V, the bias voltage is changed to any voltage between -500 and 0V excluding near -100V for a time corresponding to half the cycle, and then the bias voltage is returned to the -100V again for the same time, and this operation is repeated one or more times. Alternatively, the hard coating can also be produced by applying a bias voltage to the substrate at the start of hard coating formation, any voltage between -500 and 0V excluding near -100V, the bias voltage is changed to -100V for a time corresponding to half the cycle, and then the bias voltage is returned to any voltage between -500 and 0V excluding near -100V for the same time, and this operation is repeated one or more times. Note that the manner of voltage change can be linear (constant rate of change), or the like, and the like. 3 There are no restrictions as long as the ratio increases or decreases periodically. EXAMPLES

[0027] Next, the present invention will be described more specifically by giving an example in which the coated member of the present invention is used as a cutting tool, but the present invention is not limited to this example.

[0028] 1. Base material In this embodiment, a WC cemented carbide was used as the substrate.

[0029] 2. Hard coating A hard coating was formed on a carbide tip (ISO standard SNGN120408) by FAD (Filtered Arc Deposition), a type of AIP targeting graphite. The change in bias voltage is shown in Table 1. That is, the bias voltage listed on the left side of the bias range column in the table was set as the bias voltage at the start of film formation, and the bias voltage was changed to the bias voltage listed on the right side of the column at half the time of one cycle of film formation (bias rise and fall speed), and then the bias voltage was returned to the bias voltage at the start of film formation at the same time (same bias rise and fall speed), and this operation was repeated a predetermined number of times (number of times the bias was raised and lowered). The bias voltage was changed linearly (at a constant rate of change). The number of layers and the sp of the hard coating (DLC coating) of the obtained coated members of the present invention (examples of the present invention) 1 to 9 are 3 In this embodiment, the average of the minimum and maximum values ​​of the ratio, the average period, and the thickness were determined as follows. The results are shown in Table 2.

[0030] Hard coating sp 3 The averages of the minimum and maximum values ​​of the ratio were found as follows: using EELS, a line analysis was performed from the interface between the substrate and the hard coating to the surface of the hard coating with a beam spot of 1 nm in 1 nm steps, the results of this line analysis were analyzed, a graph was created in which the results of this line analysis were plotted as dots, and the average values ​​of the minimum values ​​where a decrease turns to an increase and the average values ​​of the maximum values ​​where an increase turns to a decrease were found based on each point on the graph without performing any interpolation processing. The thickness of the hard coating was determined by dividing the cross-sectional area of ​​the film in an observation field with a length of more than 1 μm in a direction horizontal to the substrate surface using a TEM (magnification: 50,000 times) by the length in the direction horizontal to the substrate surface. In addition, the periodic number was determined by EELS line analysis. 3 The maximum and minimum values ​​of the ratio were counted, and the smaller of the two was taken as the number of cycles. The average cycle was calculated by dividing the thickness of the hard coating determined by the above method by the number of cycles.

[0031] The arithmetic surface roughness of the hard coating and the substrate was determined by measuring arbitrary locations on the hard coating surface using a stylus probe under the following measurement conditions and calculating the average value of the measured values. Number of measurements: 3 Stylus radius: 2μm Measurement length: 1mm Measurement speed: 0.1mm / s

[0032] In the present examples, the nanoindentation hardness was determined by measuring arbitrary locations on the surface of the hard coating under the following measurement conditions and calculating the average value of the measured values. Measurement points: 20 points Indenter shape: Berkovich (edge ​​angle 115°) Pressing load: 0.98mN Pressing time: 10 seconds Holding time: 1 second Unloading time: 10 seconds

[0033] For comparison, the conditions for forming the hard film were adjusted to form comparative coated members (Comparative Examples) 1 to 5 that do not satisfy the requirements of the present invention. As with Inventive Examples 1 to 9, the sp of the hard film was also determined for Comparative Examples 1 to 5. 3 The average of the maximum and minimum ratios, thickness, arithmetic surface roughness, and nanoindentation hardness were determined, and the results are shown in Table 2.

[0034] [Table 1]

[0035] [Table 2]

[0036] Next, the coated members of the present invention and the comparative examples were subjected to the following cutting test using a superhard tip (ISO standard SNGN120408) to check the welded area and the presence or absence of peeling. The results are shown in Table 3.

[0037] Wet cutting test Cutting method: Turning Work material: Aluminum alloy (A6063) Cutting speed: 1000m / min Feed: 0.4mm Cutting depth: 1mm Cutting test time: 10 seconds

[0038] [Table 3]

[0039] As is clear from Table 3, the coated members of Examples 1 to 9 having hard coatings satisfying the requirements of the present invention are smooth, have excellent adhesion, and are also excellent in resistance to welding, so that they can be said to have good friction characteristics and can be used as cutting tools with higher processing efficiency and longer tool life. It is also clear that these coated members can be used as sliding members, dies, automobile parts, etc. On the other hand, it is clear that the coated members of Comparative Examples 1 to 5, which have hard coatings that do not satisfy the requirements of the present invention, are difficult to use as cutting tools having high processing efficiency and tool life, and are also difficult to use as sliding members, dies, or automobile parts. [Industrial Applicability]

[0040] The coated member of the present invention can be used for cutting tools having high processing efficiency and long tool life, sliding members, dies, and automobile parts, and has extremely high industrial applicability.

Claims

1. A coated member having a hard coating on a substrate without an intermediate layer, The hard coating is a DLC coating that does not substantially contain hydrogen, and sp 3 Combine / (sp 2 bond+sp 3 sp defined as 3 The ratio increases and decreases linearly and periodically. The sp 3 The average value of the maximum ratio is 0.7 to 0.

9. The sp 3 The average value of the minimum ratio is 0.4 to 0.

6. the difference between the average value of the maximum value and the average value of the minimum value is 0.2 to 0.5; The arithmetic surface roughness of the surface of the substrate is R a1 The arithmetic surface roughness of the hard coating surface is R a2 Then, R a2 and R a1 The difference R a2 -R a1 is 10 nm or less; A covering member comprising:

2. 2. The coated member according to claim 1, wherein the average value of the period is 15 to 500 nm.

3. 3. The coated member according to claim 1, wherein the hard coating has a thickness of 350 to 2000 nm.

Citation Information

Patent Citations

  • Modulating system for receiver of radiometer

    JP1984077322A

  • Manufacture of plate for sealed alkaline storage battery

    JP1987073563A

  • Carbon-based multi-layered thin film manufacturing method using ion beam

    JP2006037158A

  • Diamond-like carbon (DLC) film and DLC coated die

    JP2008297171A

  • Slide member and piston ring

    JP2017053435A