Glass-ceramic articles
A zirconium silicon nitride layer on glass-ceramic surfaces addresses scratches and stains, enhancing durability and appearance while maintaining mechanical properties for cooktops and furniture applications.
Patent Information
- Application Number
- JP2021556996
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-22
- Filing Date
- 2020-03-19
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-03-19
AI Technical Summary
Glass-ceramic plates face issues with scratches and stains due to friction with utensils and cleaning products, compromising their appearance and mechanical properties, especially when used as cooktops or furniture surfaces.
A zirconium silicon nitride layer is applied on the glass-ceramic surface, with a specific atomic ratio of zirconium to silicon, enhancing durability and reducing scratches and stains through improved hardness and adhesion, while maintaining thermal stability and compatibility with heating elements.
The zirconium silicon nitride layer significantly reduces scratches and stains, maintaining the mechanical strength and aesthetic appeal of glass-ceramic surfaces, making them suitable for high-temperature and high-friction applications without delamination or degradation.
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of glass ceramics. More specifically, the present invention relates to articles or products made of glass ceramics, in particular glass ceramic plates intended to act as furniture surfaces and / or as cooking surfaces. The term "glass ceramic article" or "article made of glass ceramic" is understood to mean an article based on a substrate (such as a plate) made of glass ceramic material, which substrate can, if appropriate, be equipped with additional accessories or elements, decorative or functional, required for its final use, and the article can refer either to the substrate alone or to the substrate equipped with additional fittings (for example a cooktop with a control panel, its heating elements, etc.). [Background technology]
[0002] Glass-ceramics start out as glasses, called precursor or matrix glasses or green glasses, whose specific chemical composition allows controlled crystallization to occur by a suitable heat treatment, called ceramization. This specific partial crystal structure gives glass-ceramics their unique properties.
[0003] Considering that currently there are various types of glass-ceramic plates and that it is a major problem to modify these plates and / or the manufacturing methods for these plates without the risk of adversely affecting the desired properties, each variant is the result of major research and numerous tests. In particular, to be able to be used as a cooktop, glass-ceramic plates must generally exhibit a transmittance of wavelengths in the visible range that is low enough to hide at least a part of the underlying heating element when it is switched off, and depending on the situation (radiative heating, inductive heating, etc.) high enough to allow the user to visually detect the heating element in the operating state for safety. Glass-ceramic plates must also exhibit a high transmittance of wavelengths in the infrared range, especially in the case of plates with radiative heating elements. Glass-ceramic plates must also exhibit sufficient mechanical strength as required in their field of use. In particular, to be used as a cooktop in the household appliance field or as a surface for furniture, glass-ceramic plates must exhibit good resistance to pressure, impacts (support of appliances and drops, etc.).
[0004] Traditionally, glass-ceramic plates are used as cooktops or they can also be associated with heating elements in other applications, for example to form fireplace inserts. Recently, their use has been extended to other areas of daily life, and glass-ceramic plates can be used as furniture surfaces, in particular to form worktops, central islands, consoles, etc., and the surface area that they occupy in these new applications is larger than in the past.
[0005] Due to the repeated use of utensils on their surfaces (such as saucepans for cooktops or various household items for work surfaces), glass-ceramic plates can become scuffed under the effect of friction with these utensils with use, and can even become stained under the effect of friction with metals. The use of cleaning products such as more abrasive scouring sponges can also be an additional source of scuffing, as food can stick to the surface of the plates or these plates can show fingerprint problems.
[0006] The plates can furthermore present different coatings with functional and / or decorative purpose, the most common being enamels based on glass frits and pigments, as well as certain paints resistant to high temperatures, for example based on silicone resins. Other coatings also exist, in particular layers based on layers or stacks of layers, such as reflective layers, to obtain contrast effects, but these coatings are generally more expensive and their production is often more problematic. Adding coatings can also complicate the maintenance of the plates, since they can be adversely altered during cleaning or can adversely alter the optical or mechanical properties of the glass ceramic. Summary of the Invention [Problem to be solved by the invention]
[0007] Whether the glass-ceramic is coated or not, an ongoing concern in the field of glass-ceramics remains the ability to provide products that are easy to maintain and that retain their appearance and their properties over time.
[0008] The present invention seeks to overcome the above-mentioned drawbacks of glass-ceramic plates with regard to damage related to utensil friction (abrasion, staining due to metal friction). The overcoming of this drawback is by providing an improved glass-ceramic plate, in particular a new glass-ceramic plate intended to be used with one or more heating elements such as a cooktop or intended to act as a furniture surface. This plate makes it possible to suppress the appearance of scratches on its surface in its daily use, and also to suppress the appearance of staining due to friction with metal utensils, without compromising other properties desired for its use or without compromising its aesthetic appearance.
[0009] This object is achieved by the glass-ceramic product developed according to the invention, in which the appearance of scratches or staining is suppressed by the application of a specific coating, which is selected according to precise criteria to obtain the desired effect. This is because the inventors have demonstrated that the addition of zirconium in a layer of hard material (for example silicon nitride and / or aluminum nitride type material) deposited on the surface of the glass-ceramic, and in particular the deposition or presence on the surface of the glass-ceramic (in particular on the surface intended to come into contact with the instrument, generally the upper surface of the plate) of a layer comprising zirconium silicon nitride with a specific atomic ratio of zirconium, has a very favorable effect on the reduction of scratches and the reduction of staining effects due to frictional action with metals. [Means for solving the problem]
[0010] According to this, the invention comprises at least one substrate, for example a plate, made of glass ceramic, said substrate being made of zirconium silicon nitride Si x Zr y N zand the atomic ratio y / (x+y) of Zr to the total Si+Zr is between 10% and 90% (or in other words within a range between 10% and 90%, the limit being included or extending from 10% to 90%), preferably between 15% and 50%, in particular between 28% and 33%. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The layer deposited according to the invention increases the durability of the plate by making it possible both to significantly reduce the appearance of scratches and to reduce the appearance of stains due to the rubbing action of metal utensils (such as saucepans).
[0012] The products according to the invention also show good adhesion of said layers to the glass-ceramic substrate or to any adjacent layers that may be present on the substrate (without the need for pretreatment of the support and / or the use of adhesion promoters, tie layers or primers). The layers / coatings in particular do not show delamination after thermal shock (e.g. near 600° C.) and withstand high temperatures. The coated substrates show good thermal stability and can be used with different heating sources (inductive heat sources, radiative heat sources, etc.). Furthermore, the layers / coatings do not mechanically weaken the glass-ceramic substrate.
[0013] The above-mentioned layer is advantageously made essentially (up to at least 85% by weight) of silicon, zirconium and nitrogen, in fact only of silicon, zirconium and nitrogen (with the exception of impurities present in this case not exceeding 5% of the layer), which layer is then more simply called "zirconium silicon nitride layer". The name "zirconium silicon nitride layer" does not exclude the presence, if appropriate, of other chemical elements, nor does it prejudge the actual stoichiometry of the layer. The zirconium silicon nitride layer may in particular be doped with or contain small amounts of one or more chemical elements, typically aluminum or boron, which are added as dopants in the targets used in order to increase their electronic conductivity and thereby facilitate deposition by magnetron cathode sputtering techniques. The layer selected according to the invention is in particular zirconium silicon nitride Si x Zr y N z or a layer of zirconium silicon nitride doped with aluminum, x Zr y N z :Al. However, the content of dopants (especially aluminum) is less than 15% by weight (in the target and in the layer), preferably less than 10% by weight, and even practically zero. More generally, the content of components other than silicon, zirconium and nitrogen in the layer is less than 15% by weight, preferably less than 10% by weight, and even practically zero.
[0014] In the zirconium silicon nitride layer selected according to the invention, the atomic ratio y / (x+y) of Zr to the total Si+Zr is, as mentioned above, 10% to 90%, preferably 15% to 50%, in particular 28% to 33%. Such a layer can in particular be deposited with a target containing, for example, 15% to 40% Zr and 85% to 60% Si, which target is sputtered in a nitrogen-containing atmosphere.
[0015] The layer selected according to the invention may furthermore exhibit a nitrogen number z in particular ranging from 4 / 3(x+y) to 5 / 3(x+y).
[0016] The zirconium silicon nitride layer (or each zirconium silicon nitride layer, in the case of a plurality of zirconium silicon nitride layers, as specified below) used to coat the glass ceramic with the aim of improving its durability is advantageously a thick layer, in particular thicker than the thin layers usually deposited by magnetron (whose (physical) thickness does not exceed about 100 nm), the (physical) thickness of said layer being in particular in the range from 200 to 5000 nm, in particular from 700 to 2500 nm, preferably from 1000 to 1500 nm.
[0017] Advantageously, the zirconium silicon nitride layer according to the invention exhibits a hardness H of more than 14 GPa, in particular more than 20 GPa, in practice more than 30 GPa. This layer also exhibits an elastic modulus E of more than 140 GPa, in particular more than 150 GPa, in practice even more than 200 GPa. The hardness H and the elastic modulus E are measured on a layer deposited as a solid shade (with 100% coverage) on a glass ceramic, using a nanoindenter of the type DCMII-400 sold by the company CSM Instruments, using a pyramidal diamond tip of the three-sided Berkovich type according to standard NF EN ISO 14577.
[0018] In the present invention, one zirconium silicon nitride layer is particularly sufficient to obtain the improvement according to the invention. The term "layer" is understood to mean a homogeneous layer of one and the same material, even if said layer is obtained by several passes starting from one and the same target, for example. Accordingly, a coating comprising a layer selected according to the present invention can advantageously contain only one layer comprising zirconium silicon nitride, and in fact can even contain only said layer.
[0019] However, for the purposes of obtaining an improved product according to the invention, it is not excluded to use several zirconium silicon nitride layers in the same coating, or to use a stack of layers comprising the aforementioned layer and one or more other layers (or in other words one or more other layers above or below the aforementioned zirconium silicon nitride layer), the coating (or stack) made by these layers increasing the durability of the plate due to the presence of the zirconium silicon nitride layer according to the invention.
[0020] A coating comprising at least one zirconium silicon nitride layer according to the invention can, for example, comprise at least one layer, or a stack of layers, between the substrate and the above-mentioned layer. These layers or stacks of layers can, for example, affect the reflective appearance of the plate, or can be used to block possible ion migration, or act as an adhesive layer, etc. This coating can, for example, comprise a layer of silicon oxynitride or silicon nitride, or a layer of silica or SiO x and the (physical) thickness of this or these layers is preferably in the range ranging from 1 to 30 nm.
[0021] The coating may comprise multiple zirconium silicon nitride layers (i.e., zirconium silicon nitride Si x Zr y N z In the case where the layers include a layer containing zirconium silicon nitride, the atomic ratio y / (x+y) of Zr to the total Si+Zr for each of these layers is preferably 10% to 90%, but does not necessarily have to be the same for all of these layers containing zirconium silicon nitride (according to this, the ratio y / (x+y) is the ratio of the zirconium silicon nitride Si x Zr y N z (which may be different for the two layers present, including
[0022] In an advantageous embodiment, the zirconium silicon nitride layer or at least one zirconium silicon nitride layer according to the invention is deposited in direct contact with a substrate made of glass ceramic (or in other words, in the product, in (direct) contact with said glass ceramic) on at least one of its faces (preferably that face intended to be directed towards the user in the position of use, or the upper or outer face, the other faces (lower or inner faces) being generally hidden in the position of use) without other underlying coating layers.
[0023] In another alternative or cumulative embodiment, the zirconium silicon nitride layer or at least one layer incorporating zirconium silicon nitride according to the invention constitutes the outer layer (or outer layer, i.e. the layer of the coating located on the atmospheric side or the layer furthest from the glass ceramic or the visible layer) of the coating present on the glass ceramic.
[0024] Alternatively, the above-mentioned layers can be coated with one or more other layers (air side). In a particularly advantageous embodiment, the coating deposited on the glass-ceramic substrate according to the invention comprises, in addition to the zirconium silicon nitride layer according to the invention, at least one layer (in particular an outer layer) having a low coefficient of friction (less than 0.25), such as titanium oxide TiO x or TiZrO x or BN or ZrO x(one or the other of these layers can also be doped) or layers based on these. This layer exhibits lubricating properties and the presence of this layer makes it possible to further reduce the susceptibility of the stack to scuffing and staining. The thickness of this layer is preferably less than 20 nm, in particular less than or equal to 10 nm, preferably between 2 and 10 nm, in particular of the order of 4 to 8 nm. In particular, the coating on the glass-ceramic substrate according to the invention can consist of only a combination of two layers: a zirconium silicon nitride layer defined according to the invention in contact with the glass-ceramic and a layer on the air side with a coefficient of friction of less than 0.25, this layer with a low coefficient of friction coating the zirconium silicon nitride layer according to the invention. The coefficient of friction is measured using a CSM microscratch device sold by CSM Instruments. In this device, a constant force of 1 N is applied to a stainless steel ball with a diameter of 1 cm moving at a constant speed over a distance of 2 cm, performing a total of 30 passes (15 back and forth movements). The coefficient of friction is the ratio of the tangential force to the normal force measured by the sensor.
[0025] Of course, the different embodiments described above can be combined with each other.Preferably, the coating deposited with the aim of obtaining the improved properties according to the invention consists of only one zirconium silicon nitride layer defined according to the invention, or, starting from the substrate in succession, consists of said zirconium silicon nitride layer and a layer with a low coefficient of friction (less than 0.25), as described above, for example TiO2.
[0026] The total thickness of the coating (including the zirconium silicon nitride layer and any other optional layers) is preferably between 200 and 5000 nm.
[0027] The zirconium silicon nitride layer or a coating (or stack) incorporating this layer can cover only a part of the substrate or the entire surface (particularly the main surface), for example the upper surface at the point of use, which surface is particularly susceptible to cleaning. In particular, substrates made of glass ceramics are provided on their upper or outer surface with said zirconium silicon nitride layer according to the invention, either alone or forming part of a stack of layers.
[0028] The glass-ceramic article (or product) according to the invention is in particular a cooktop, or a cooking device or installation, or any furniture article incorporating (or containing or made from) at least one substrate made of glass-ceramic (material) (the substrate is most commonly in the form of a plate, which is to be incorporated or assembled into or combined with other elements to form part of the furniture), said substrate being capable of presenting, where appropriate, areas with display properties (for example in combination with a light-emitting source) or areas with decorative areas, or of being combined with a heating element. In its most common application, the article according to the invention is intended to act as a cooktop, this plate being generally intended to be incorporated into a kitchen range or cooking surface, which also includes a heating element, for example a radiant or halogen heat source or an induction heating element. In another advantageous application, the article according to the invention is a worktop, or a central island, made of glass-ceramic, where appropriate, with different display devices, not necessarily having a cooking area, and even in fact a console type of furniture (the substrate forms, for example, the upper part), etc.
[0029] The substrate (or the article according to the invention itself, if it is formed only from the substrate) is generally (in the form of) a plate, intended in particular to be used with, in particular to cover or receive, at least one light source and / or one heating element, or to act as a furniture surface. This substrate (or each of these plates) is generally of a geometric shape, in particular rectangular, indeed square, indeed circular or elliptical, etc., and generally presents a face (or visible face or outer face, generally the upper face in the use position) that is directed towards the user in the use position, another face (or inner face, generally the lower face in the use position) that is generally hidden in the use position, for example in the framework or casing of the furniture, and an edge face (or edge or thickness). The upper or outer face is generally flat and smooth, but may locally present at least one protruding area and / or at least one recessed area and / or at least one opening and / or beveled edge, etc., these variations in shape in particular constituting a continuous variation of the plate. The lower or inner face may also be flat and smooth or may be provided with pins.
[0030] The thickness of the glass-ceramic substrate is generally at least 2 mm, in particular at least 2.5 mm, advantageously less than 15 mm, in particular in the order of 3 to 15 mm, in particular in the order of 3 to 8 mm or in the order of 3 to 6 mm. The substrate is preferably a flat or substantially flat plate (in particular having a deflection of less than 0.1% from the diagonal of the plate, preferably zero).
[0031] The substrate may be based on any glass ceramic, but it preferably has a zero or substantially zero CTE, in particular a CTE of 30·10 between 20 and 700° C. -7 K -1 Less than (absolute value), especially 15·10 -7 K -1 Less than 5-10°C between 20 and 700°C -7 K -1 It advantageously exhibits a CTE of less than 0.05.
[0032] The invention is particularly advantageous for substrates with a dark appearance, where scratches are more easily found, which have low transmittance and weak scattering, in particular essentially based on any glass ceramic with a light transmittance TL of less than 40%, in particular less than 5%, in particular 0.2% to 2% for glass ceramics up to 6 mm thick, and an optical transmittance (determined in a known manner by taking the ratio of the transmitted light intensity to the incident light intensity at a given wavelength) of 0.5% to 3% for a wavelength of 625 nm in the visible range. The term "essentially" is understood to mean that the substrate has such a transmittance by itself, without the presence of any one coating. The optical measurements are carried out according to the standard EN 410. In particular, the light transmittance TL is measured using illuminant D65 in accordance with standard EN 410 and is the total transmittance (in particular integrated over the visible range and weighted by the sensitivity curve of the human eye) and takes into account both the direct transmittance and a possible diffuse transmittance, the measurement being carried out, for example, using a spectrophotometer equipped with an integrating sphere (in particular the spectrophotometer sold under the reference Lambda 950 by Perkin-Elmer).
[0033] In particular, the substrate is a substrate with a black or brown appearance, which, in combination with a light source arranged underneath, makes it possible to display light areas or decorations while masking possible underlying elements. The substrate can in particular be based on a black glass-ceramic comprising crystals of β-quartz structure in a residual glass phase, the absolute value of whose coefficient of expansion is advantageously 15·10 -7 K -1 The following is actually 5·10 -7 K -1This substrate is, for example, a glass ceramic of the type sold by Eurokera under the name KeraBlack+. It may in particular be a glass ceramic having a composition as described in EP 0 437 228 A or US 5 070 045 A or FR 2 657 079 A, or a tin-refined glass ceramic exhibiting a content of arsenic oxide preferentially less than 0.1%, as described, for example, in WO 2012 / 156444, or a sulfide-refined glass ceramic as described in WO 2008 / 053110, etc.
[0034] The invention can also be applied when the substrate is lighter, for example in the case of transparent substrates and, where appropriate, in the case of substrates coated on their underside with an opacifying coating, generally made of paint, such as the plates sold under the name Keralite® by Eurokera.
[0035] According to the invention, the glass-ceramic substrate under consideration is coated in one or more areas (or at least one area of said substrate is coated), more particularly on the surface, on at least a part of the face, advantageously on the face facing the user in the position of use and / or on at least a part of the face requiring reduced visibility of scratches and staining, generally on the upper or outer face in the position of use, in particular over the entirety of said face. The glass-ceramic substrate is coated with at least one layer defined according to the invention or with a coating comprising said layer.
[0036] The substrate according to the invention can be coated, if appropriate, with other coatings or layers having functional and / or decorative effects (anti-spill layers, opacifying layers, etc.), in particular with localized coatings or layers, such as, for example, regular patterns based on enamel (for example on the upper surface to form a logo or a simple pattern) or a layer of opacifying paint on the lower surface of the substrate. In particular, the substrate can be coated at least partially or entirely above (in particular on the air side) or below (in particular in contact with the substrate) the layer defined according to the invention, or above or below (at least partially or entirely) a stack comprising said layer according to the invention, with at least one layer of enamel and / or paint, in particular of gloss type, localized or not, and said layer of enamel or paint / gloss can be in contact with the layer according to the invention. The term "gloss type paint" is understood in particular to mean a paint made from metal oxides and not containing pigments, this paint or gloss exhibiting in particular a refractive index of more than 1.54. The thickness of such a paint layer can in particular be between 10 and 100 nm.
[0037] The article according to the invention may further comprise, associated with or in combination with the substrate, one or more light sources and / or one or more heating elements (such as one or more radiant or halogen elements and / or one or more atmospheric gas burners and / or one or more induction heating means), generally arranged on the underside of the substrate. The one or more light sources may be integrated into or combined with one or more display type structures, touch-sensitive digital displays, electronic control panels, etc. The one or more light sources are advantageously made by more or less divergent light-emitting diodes, optionally associated with one or more light guides.
[0038] The article may also include (or have associated therewith) additional functional elements (frames, connectors, cables, control elements, etc.).
[0039] According to this, the invention has made it possible to develop glass-ceramic products with a surface more resistant to scratching and staining in desired locations (for example over the entire surface or in only a few areas, for example areas exposed to handling operations or scratching, such as heating areas), while the product retains the mechanical strength required for various applications (in particular for use as a cooktop). According to this, the solution according to the invention makes it possible to obtain areas of greater resistance to scratching and staining in any desired area of the product in a simple and economical way, without complex operations (it is possible to deposit layers by deposition techniques under reduced pressure, such as cathode sputtering, as will be described below), in a durable way and with high adaptability, even if these areas are intended to be exposed to high temperatures. The articles according to the invention in particular exhibit good heat resistance, which makes them compatible with the use of various types of heating procedures, and do not present maintenance problems. The products according to the invention in particular do not undergo thermal decomposition at temperatures above 400 ° C, which can be achieved in particular in applications such as use as a cooktop.
[0040] The present invention also relates to a method for producing a glass-ceramic article according to the invention, starting from a substrate made of glass ceramic, in which at least one layer selected according to the invention is deposited (or applied) onto at least one region of said substrate.
[0041] The application or deposition of the layer (or each layer, if appropriate) of zirconium silicon nitride according to the invention can be carried out by any suitable and rapid technique that allows to produce a uniform layer or a solid shade of this type of layer, in particular by a method for deposition under reduced pressure, such as cathode sputtering, in particular magnetron enhanced cathode sputtering, or chemical vapor deposition (CVD), if appropriate plasma enhanced chemical vapor deposition (PECVD), this application is preferably carried out by cathode sputtering, in particular magnetron enhanced cathode sputtering. This deposition is carried out with good yield and good deposition rate. Any other layers of oxide or nitride of the same coating can also be deposited, if appropriate, by the same deposition method (deposition is in particular continuous), other layers (enamel, glaze) optionally present on the substrate are deposited independently by any conventional technique (such as screen printing or inkjet printing for enamel).
[0042] The cathode sputtering used preferentially is of the AC (alternating current) type or of the DC (direct current) type, or in a particularly preferred manner of the pulsed DC type, according to the type of generator employed to polarize the cathode. The target is, for example, planar.
[0043] The deposition of the layer (or layers) of silicon zirconium nitride is in particular carried out in an atmosphere consisting of plasma generating gas (generally argon) and nitrogen, using a silicon zirconium target with an atomic ratio y / (x+y) of 10% to 90% Zr relative to the total Si+Zr, in particular in an atmosphere consisting of argon and nitrogen, doped with aluminium or boron, if appropriate, to increase the electronic conductivity.
[0044] The active components of the plasma bombard the target and thereby strip off the elements described above that are to be deposited on the substrate to form the desired layer, and / or react with gases contained in the plasma to form said layer.
[0045] Advantageously, the atmosphere during deposition in the chamber in which the deposition in question is taking place (made up of the plasma generating gas) contains less than 1% by volume of oxygen (which may remain in the chamber or may be optionally supplied) and is practically oxygen-free. Preferably, the oxygen flow rate during deposition of the layer is zero, in other words no oxygen is intentionally introduced into the sputtering atmosphere of said target.
[0046] The pressure of (or during) the deposition of the layer according to the invention is in particular at most 2.5 μbar, preferably in the range of 1.5 μbar to 2.3 μbar. The term "deposition pressure" is understood to mean the pressure prevailing in the chamber in which the deposition of this layer takes place. The application of a selected pressure in the relevant deposition chamber contributes to obtaining a layer exhibiting good mechanical and abrasion resistance.
[0047] Also, the power of the deposition of the layer is preferably within 1 cm of the target during the deposition of said layer. 2 2~10W / cm 2 and the advance speed of the substrate beneath the various targets is preferably in the range ranging from 0.1 to 3 m / min.
[0048] The deposition is in particular carried out on a preceramized and unheated substrate. According to a particularly preferred embodiment, the coated substrate is then subjected to a heat treatment, in particular a strengthening treatment or slow cooling, for example at a temperature of the order of 750° C. to 900° C. for about 10 minutes. This treatment makes it possible to relieve stresses and to further increase the hardness of the layer according to the invention.
[0049] Just to be clear, the manufacture of glass-ceramic plates is generally carried out as follows: a glass having a composition selected to form the glass-ceramic is melted in a melting furnace, then the molten glass is rolled to give a standard ribbon or sheet by passing the molten glass between rolling rolls, and the glass ribbon is cut to the desired dimensions. The plates thus cut are then cerammed in a manner known per se. Ceramming consists in firing the plates according to a thermal profile selected to transform the glass into a polycrystalline material known as "glass-ceramic". The coefficient of expansion of glass-ceramics is zero or practically zero, and glass-ceramics are particularly resistant to thermal shocks that may range up to 700°C. Ceramming generally involves gradually increasing the temperature to the nucleation range, passing through a nucleation interval (e.g., 650°C-830°C) for several minutes (e.g., 5-60 minutes), further increasing the temperature to allow crystal growth and maintaining the temperature of the ceramming stationary phase for several minutes (e.g., 5-30 minutes) (e.g., ceramming for an interval in the range of 850°C-1000°C), and then rapidly cooling to ambient temperature.
[0050] Where appropriate, the method also includes a cutting operation (generally before ceramming), e.g. using a jet of water, mechanical marking using a cutting wheel, etc., followed by a shaping operation (grinding, chamfering, etc.).
[0051] The following examples are illustrative of the present invention but are not intended to be limiting thereof. EXAMPLES
[0052] In these examples, small 20 cm x 20 cm plates of the same substrate were used, made from a translucent black glass ceramic sold by Eurokera under the name KeraBlack+. These small plates presented a smooth upper surface and a lower surface with pins and were 4 mm thick.
[0053] 1200nm thick Six Zr y N z A thick layer of 6 W / cm was deposited by pulsed DC magnetron enhanced cathode sputtering at a pressure as low as 2 μbar. 2 Deposition was performed on these small plates at a power density per unit area of the target of less than 10 ... x Zr y N z In the present study, the atomic ratio y / (x+y) of Zr to the total Si+Zr was 32%.
[0054] The hardness H and the elastic modulus E of the bare glass ceramic and then of the glass ceramic provided with said zirconium silicon nitride layer were then measured using a nanoindenter of the DCMII-400 type with a pyramidal diamond tip of the Berkovich type (3 sided) according to standard NF EN ISO 14577.
[0055] It was observed that the bare glass ceramic had a hardness of 7.5 GPa, and that the deposition of a thick layer of zirconium silicon nitride allowed an increase in hardness to about 14.5 GPa. The elastic modulus (or modulus of elasticity) E of the layer was 140 GPa.
[0056] Afterwards, slow cooling (or tempering) at 850°C for 10 min was performed on the coated glass-ceramic, resulting in higher values of hardness of the coated substrate and elastic modulus of the layer E, i.e. H=15.5-20.5 GPa and E=155 GPa.
[0057] The abrasion resistance of these samples was also evaluated using abrasive paper of the P800 type sold by Norton, incorporating silicon carbide particles with an average equivalent diameter of 20 μm, with 15 double strokes per minute and a load of 5 N / cm on the surface of glass ceramics (bare or coated). 2The abrasion resistance was measured by moving the paper back and forth over a distance of 3.81 cm with an applied pressure of 1.0 MPa. The number of scratches was measured from a photograph taken by illuminating the sample with a three-color light-emitting diode in a light box. Image processing (binarization to black and white, making scratches visible as black pixels and unabraded white pixels visible as white pixels) allowed the photograph to be analyzed. The "abrasion index" was evaluated, giving an index x corresponding to the number y of black pixels recorded in an image of 132000 pixels divided by 10000 (x=y / 10,000, where x is, for example, 1 for 10000 black pixels, 2 for 20000 black pixels, etc.). The bare glass-ceramic had an index of 4, whereas the glass-ceramic coated according to the invention had an index of 2 before annealing and 1 after annealing at a temperature of the order of 850° C. for about 10 minutes. This indicates a significant reduction in the number of scratches compared to the bare glass-ceramic.
[0058] The coefficient of friction was also measured using a CSM microscratch device sold by CSM Instruments. A constant force of 1 N was applied to a stainless steel ball with a diameter of 1 cm moving at a constant speed over a distance of 2 cm, a total of 30 passes were performed. The measured coefficient of friction is the ratio of the applied tangential force to the applied normal force, these forces being measured by a sensor. The coefficient of friction measured for the bare glass ceramic (glass ceramic / metal contact) was 0.3, while that of the coated glass ceramic was reduced to 0.2. In comparison, the one obtained by using as a coating a hard coating of the same thickness based on SiN (zirconium-free) instead of the layer according to the invention obtained a higher coefficient equal to 0.4.
[0059] These same samples were subjected to a metal friction test in a linear abrasion tester, model 5750 (sold by Taber), equipped with a flat stainless steel wiper. The arm of this tester holds said wiper, which travels 3.81 cm at a speed of 60 cycles per minute, applying a force of 2 MPa. The test consists in performing a reciprocating motion and determining the number of cycles at which a metal deposit is observed on the surface. This test makes it possible to simulate the movement of a saucepan on the surface of the glass ceramic, which generates two types of damage: scratches in the form of metal deposits resulting from the saucepan, and plastic deformation or cracks or wear of the glass ceramic.
[0060] On bare glass ceramic, the wiper is x or TiZrO x As in the case of the sample having only a deposit of SiN (of the same thickness as the layer according to the invention tested), the surface was scratched in less than about 20 cycles, and the sample carried a layer of SiN resulting in a metal deposit after about 30 cycles.
[0061] The sample according to the invention (with the above-mentioned layer of SiZrN) was only rubbed from about 60 cycles, ie twice as many as the best cycles of the preceding comparative sample.
[0062] TiO with a thickness of 5 nm, which have friction coefficients of 0.17 and 0.15, respectively. x or TiZrO x By adding a layer of SiZrN to the layer of SiZrN mentioned above, these results could be further improved, even exceeding about 100 periods.
[0063] Various cleaning tests on surfaces bearing traces of coffee, milk, vinegar, burnt tomato sauce under low and high temperature conditions with various household products (such as VitroClen brand products from Reckitt Benckiser, or derived and glass-ceramic cleaning products from Kiraviv) also demonstrated that the glass-ceramics coated with the layer selected according to the invention are easy to clean and that the layer does not chemically decompose. Likewise, the layer did not delaminate after a thermal shock at 620°C and showed no degradation after 100 hours at 580°C.
[0064] The article according to the invention can in particular be advantageously used to manufacture a new range of cooktops for kitchen ranges or cooking surfaces, or a new range of worktops, consoles, credenzas, central islands and the like. Some of the embodiments of the present invention are described in items 1 to 15 below. <Item 1> At least one substrate, for example a plate, made of glass ceramic, the substrate being made of zirconium silicon nitride Si x Zr y N z wherein the atomic ratio y / (x+y) of Zr to the total Si+Zr is 10% to 90%, preferably 15% to 50%, in particular 28% to 33%. Item 2: The glass-ceramic article according to item 1, characterized in that the layer is essentially (up to at least 85% by weight) made of silicon, zirconium, and nitrogen, and in fact is made only of silicon, zirconium, and nitrogen, excluding impurities that may be present, in which case the impurities do not exceed 5% of the layer, being a zirconium silicon nitride layer. <Item 3> The glass-ceramic article according to item 1 or 2, characterized in that the layer has a thickness in the range of 200 to 5000 nm, particularly 700 to 2500 nm, and preferably 1000 to 1500 nm. <Item 4> The layer has a hardness H of more than 15 GPa, particularly more than 20 GPa, in practice more than 30 GPa, and an elastic modulus E of more than 140 GPa, particularly more than 150 GPa. The glass-ceramic article according to any one of items 1 to 3. <Item 5> The coating comprising the layer comprises only one layer comprising zirconium silicon nitride, and in fact comprises only the layer. A glass ceramic article according to any one of items 1 to 4. <Item 6> The substrate is coated with at least one layer of enamel and / or paint, particularly gloss type enamel and / or paint, on or under the layer containing zirconium silicon nitride. The glass ceramic article according to any one of items 1 to 5. <Item 7> The glass ceramic article according to any one of Items 1 to 6, characterized in that the layer is in direct contact with the glass ceramic substrate without any other underlying coating layer. <Item 8> The glass-ceramic article according to any one of items 1 to 7, characterized in that the layer or at least one layer incorporating zirconium silicon nitride constitutes an outer layer of a coating comprising zirconium silicon nitride present on the glass ceramic. <Item 9> The glass ceramic article according to any one of items 1 to 8, characterized in that the layer is coated with at least one layer having a friction coefficient of less than 0.25. <Item 10> The glass-ceramic article according to any one of Items 1 to 9, characterized in that the layer exhibits a nitrogen number z in the range of 4 / 3(x+y) to 5 / 3(x+y). <Item 11> The target used, as well as the content of dopants in the layer, in particular the content of aluminum, or the content of other components in the layer, is less than 15% by weight, preferably less than 10% by weight, or even practically zero. The glass-ceramic article according to any one of items 1 to 10. <Item 12> The glass ceramic article according to any one of Items 1 to 11, further comprising one or more heating elements. <Item 13> A method for producing a glass ceramic article according to any one of items 1 to 12, wherein the article comprises at least one substrate, such as a plate, made of glass ceramic; Zirconium silicon nitride Si, in which the atomic ratio y / (x+y) of Zr to the total Si+Zr is 10% to 90%, preferably 15% to 50%, particularly preferably 28% to 33%. x Zr y N z depositing at least one layer comprising: <Item 14> The method according to Item 13, characterized in that the substrate thus coated is subjected to a strengthening treatment or slow cooling at a temperature of 750°C to 900°C. Item 15: A method according to item 13 or 14, characterized in that the deposition of the layer is carried out by cathode sputtering, in particular magnetron-enhanced cathode sputtering, the cathode sputtering being preferably of the pulsed DC type.
Claims
1. At least one substrate, for example a plate, made of glass ceramic, said substrate being made of zirconium silicon nitride Si x Zr y N z wherein the atomic ratio y / (x+y) of Zr to the total Si+Zr is 10% to 90%, preferably 15% to 50%, in particular 28% to 33%, and wherein the thickness of said layer is in the range of 200 to 5000 nm.
2. 2. The glass-ceramic article according to claim 1, characterized in that the layer is a zirconium silicon nitride layer made essentially (up to at least 85% by weight) of silicon, zirconium and nitrogen, in particular made only of silicon, zirconium and nitrogen, with the exception of possible impurities, in which case said impurities do not exceed 5% of the layer.
3. 3. The glass-ceramic article according to claim 1 or 2, characterized in that the thickness of said layer is in the range of 700 to 2500 nm, preferably 1000 to 1500 nm.
4. 4. The glass-ceramic article according to claim 1 , wherein the layer exhibits a hardness H of more than 15 GPa, in particular more than 20 GPa, in particular more than 30 GPa, and an elastic modulus E of more than 140 GPa, in particular more than 150 GPa.
5. 5. A glass-ceramic article according to claim 1, characterized in that the coating comprising said layers comprises only one layer comprising zirconium silicon nitride, in particular only said layer.
6. 6. The glass-ceramic article according to claim 1, wherein the substrate is coated with at least one layer of enamel and / or paint, in particular gloss type enamel and / or paint, above or below the layer comprising zirconium silicon nitride.
7. 7. The glass-ceramic article according to claim 1, wherein the layer is in direct contact with the substrate made of glass-ceramic, without other underlying coating layers.
8. 8. The glass-ceramic article according to claim 1, wherein the layer, or at least one layer incorporating zirconium silicon nitride, constitutes the outer layer of a coating comprising zirconium silicon nitride present on the glass ceramic.
9. 9. The glass-ceramic article according to claim 1, wherein said layer is coated with at least one layer having a coefficient of friction of less than 0.
25.
10. 10. A glass-ceramic article according to claim 1, characterized in that the layer exhibits a nitrogen number z, in particular in the range from 4 / 3(x+y) to 5 / 3(x+y).
11. 11. The glass-ceramic article according to claim 1, characterized in that the target used and the content of dopants in the layer, in particular the content of aluminum, or the content of other components in the layer, is less than 15% by weight, preferably less than 10% by weight, in particular even zero.
12. The glass-ceramic article according to any one of claims 1 to 11, characterized in that it is a cooking device further comprising one or more heating elements.
13. A method for producing an article made of glass ceramic according to any one of claims 1 to 12, said article comprising at least one substrate, for example a plate, made of glass ceramic, Zirconium silicon nitride Si, in which the atomic ratio y / (x+y) of Zr to the total Si+Zr is 10% to 90%, preferably 15% to 50%, in particular 28% to 33%. x Zr y N z depositing at least one layer comprising:
14. A method according to claim 13, characterized in that the substrate thus coated is subjected to a tempering treatment or slow cooling at a temperature between 750°C and 900°C.
15. 15. Method according to claim 13 or 14, characterized in that the deposition of the layer is carried out by cathodic sputtering, in particular magnetron enhanced cathodic sputtering, said cathodic sputtering being preferably of the pulsed DC type.
Citation Information
Patent Citations
Durable thin-film coating for controlling low- emissivity insolation
JP1994003523A
glass ceramic
JP2016507451A
Materials with laminates that have thermal properties
JP2018520982A
Material comprising a stack with thermal properties
WO2019015917A1