Magnetic recording medium, magnetic tape cartridge, and magnetic recording / reproducing device

By controlling the intensity ratio of diffraction intensities in the magnetic layer of magnetic recording media with ε-iron oxide powder, the friction and sticking issues are mitigated, ensuring smoother operation with magnetic heads.

JP7580300B2Active Publication Date: 2024-11-11FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021030918
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-26
Publication Date
2024-11-11
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Magnetic recording media with a magnetic layer containing ε-iron oxide powder experience high friction during sliding with a magnetic head, leading to sticking issues.

Method used

A magnetic recording medium with a magnetic layer containing ε-iron oxide powder, where the intensity ratio (Int1/Int2) of diffraction intensities determined by X-ray diffraction analysis is controlled between 1.0 and 6.5, optimizing the orientation of crystal planes to enhance lubrication and reduce friction.

Benefits of technology

The solution effectively suppresses friction between the magnetic layer and the magnetic head, improving the sliding performance and reducing sticking, thereby enhancing the operational reliability of magnetic recording media.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580300000001
    Figure 0007580300000001
  • Figure 0007580300000002
    Figure 0007580300000002
  • Figure 0007580300000003
    Figure 0007580300000003
Patent Text Reader

Abstract

To provide a magnetic recording medium which comprises a magnetic layer containing ε-iron oxide powder as a ferromagnetic powder and inhibits friction.SOLUTION: There is provided a magnetic recording medium comprising a non-magnetic support and a magnetic layer containing ferromagnetic powder. The ferromagnetic powder is ε-iron oxide powder. An intensity ratio (Int1 / Int2) of diffraction intensities is in a range of 1.0 to 6.5, inclusive, as derived from an X-ray diffraction analysis of the magnetic layer using an In-Plane method. There are also provided a magnetic tape cartridge comprising the magnetic recording medium and a magnetic recording / reproduction device.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic recording medium, a magnetic tape cartridge, and a magnetic recording / reproducing device. [Background technology]

[0002] 2. Description of the Related Art Magnetic recording media are widely used as data storage recording media for recording and storing various types of data (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-130208 A Summary of the Invention [Problem to be solved by the invention]

[0004] In magnetic recording media, a magnetic layer containing ferromagnetic powder is usually provided on a non-magnetic support. As for the ferromagnetic powder, ε-iron oxide powder has been attracting attention in recent years, as described in Patent Document 1, for example.

[0005] In general, data is recorded on a magnetic recording medium and the recorded data is reproduced by running the magnetic recording medium in a magnetic recording and reproducing device (usually called a "drive") and bringing the magnetic layer surface into contact with a magnetic head and sliding it against each other. If a large amount of friction occurs between the magnetic layer surface and the magnetic head during such sliding, this can cause the magnetic layer surface to stick to the magnetic head. Therefore, it is desirable for the magnetic recording medium to have small friction when sliding against the magnetic head. However, the inventors' investigations revealed that, although the reason is not clear, magnetic recording media having a magnetic layer containing ε-iron oxide powder as a ferromagnetic powder tend to generate large friction (hereinafter also simply referred to as "friction") when sliding against the magnetic head, which makes it easy for the magnetic layer surface to stick to the magnetic head.

[0006] In view of the above, an object of one aspect of the present invention is to provide a magnetic recording medium having a magnetic layer containing ε-iron oxide powder as a ferromagnetic powder, the magnetic recording medium having reduced friction. [Means for solving the problem]

[0007] One aspect of the present invention is A magnetic recording medium having a non-magnetic support and a magnetic layer containing ferromagnetic powder, The ferromagnetic powder is ε-iron oxide powder, a magnetic recording medium in which the intensity ratio (Int1 / Int2) of diffraction intensities determined by X-ray diffraction analysis of the magnetic layer using an in-plane method is 1.0 or more and 6.5 or less; Regarding.

[0008] The Int1 is the maximum value of the diffraction intensity when the diffraction angle 2θχ is in the range of 29.0° to 31.0°, and the Int2 is the maximum value of the diffraction intensity when the diffraction angle 2θχ is in the range of 36.3° to 37.5°. "Int" is used as an abbreviation for Intensity.

[0009] In one embodiment, the intensity ratio (Int1 / Int2) can be 1.5 or more and 6.0 or less.

[0010] In one embodiment, the intensity ratio (Int1 / Int2) can be 3.0 or more and 5.5 or less.

[0011] In one embodiment, the ε-iron oxide powder can include elemental cobalt.

[0012] In one embodiment, the ε-iron oxide powder can further contain an element selected from the group consisting of gallium element and aluminum element.

[0013] In one embodiment, the ε-iron oxide powder can further include elemental titanium.

[0014] In one embodiment, the magnetic recording medium can further include a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

[0015] In one embodiment, the magnetic recording medium can further have a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.

[0016] In one embodiment, the magnetic recording medium can be a magnetic tape.

[0017] One aspect of the present invention relates to a magnetic tape cartridge including the above-mentioned magnetic tape.

[0018] One aspect of the present invention relates to a magnetic recording and reproducing device including the above magnetic recording medium. Effect of the Invention

[0019] According to one aspect of the present invention, there is provided a magnetic recording medium having a magnetic layer containing ε-iron oxide powder as a ferromagnetic powder, the magnetic recording medium having reduced friction, and a magnetic tape cartridge and a magnetic recording and reproducing device including the magnetic recording medium. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] [Magnetic recording media] One aspect of the present invention relates to a magnetic recording medium having a non-magnetic support and a magnetic layer containing ferromagnetic powder. The ferromagnetic powder is ε-iron oxide powder, and the intensity ratio (Int1 / Int2) of the diffraction intensity determined by X-ray diffraction analysis of the magnetic layer using an in-plane method is 1.0 to 6.5. The Int1 is the maximum value of the diffraction intensity in the range of the diffraction angle 2θχ of 29.0° to 31.0°, and the Int2 is the maximum value of the diffraction intensity in the range of the diffraction angle 2θχ of 36.3° to 37.5°.

[0021] <Intensity ratio (Int1 / Int2)> In the present invention and this specification, the intensity ratio (Int1 / Int2) is a value determined by the following method. The intensity ratio (Int1 / Int2) is determined by X-ray diffraction analysis of the magnetic layer containing ε-iron oxide powder using the in-plane method. Hereinafter, X-ray diffraction analysis performed using the in-plane method will also be referred to as "in-plane XRD." "XRD" is an abbreviation for X-ray diffraction. In-plane XRD is performed by irradiating the magnetic layer surface with X-rays using a thin-film X-ray diffraction device under the following conditions. The measurement direction is perpendicular to the longitudinal direction for magnetic tapes, and perpendicular to the radial direction for magnetic disks. Using Cu radiation source (output 45kV, 200mA) Scan conditions: 20-40° (degrees) range, 0.05° / step, 0.1° / min Optical system used: Parallel optical system Measurement method: 2θχ scan (X-ray incidence angle 0.25°) The above conditions are the set values ​​in a thin film X-ray diffraction apparatus. A known apparatus can be used as the thin film X-ray diffraction apparatus. An example of the thin film X-ray diffraction apparatus is SmartLab manufactured by Rigaku Corporation. The sample to be subjected to the In-Plane XRD analysis is a sample cut out from the magnetic recording medium to be measured, and the size and shape of the sample are not limited as long as the X-ray diffraction spectrum described later can be confirmed. X-ray diffraction analysis techniques include thin film X-ray diffraction and powder X-ray diffraction. Powder X-ray diffraction measures the X-ray diffraction of a powder sample, whereas thin film X-ray diffraction can measure the X-ray diffraction of a layer formed on a substrate. Thin film X-ray diffraction is classified into an in-plane method and an out-of-plane method. The X-ray incident angle during measurement is usually in the range of 5.00 to 90.00° in the out-of-plane method, whereas it is usually in the range of 0.20 to 0.50° in the in-plane method. In the in-plane XRD of the present invention and this specification, the X-ray incident angle is 0.25° as described above. The in-plane method has a smaller X-ray incident angle than the out-of-plane method, so the penetration depth of the X-ray is shallow. Therefore, X-ray diffraction analysis using the in-plane method (in-plane XRD) can be performed on the surface layer of the sample to be measured. In-Plane XRD allows X-ray diffraction analysis of the magnetic layer of a sample cut out from a magnetic recording medium. In the X-ray diffraction spectrum (vertical axis: diffraction intensity, horizontal axis: diffraction angle 2θχ(°)) obtained by In-Plane XRD, the maximum value of the diffraction intensity in the range of 29.0°≦2θχ≦31.0° is defined as "Int1", and the maximum value of the diffraction intensity in the range of 36.3°≦2θχ≦37.5° is defined as "Int2". The intensity ratio (Int1 / Int2) is calculated as the ratio of Int1 and Int2 thus obtained.

[0022] The inventors believe that the above-mentioned intensity ratio (Int1 / Int2) determined for the magnetic layer containing ε-iron oxide powder can be a value that can be an index of the state of existence of the ε-iron oxide powder in the magnetic layer. More specifically, the inventors speculate as follows. An example of a component that can contribute to suppressing friction when the magnetic layer surface slides against the magnetic head is a lubricant, which will be described later. The present inventor believes that the intensity ratio (Int1 / Int2) is greater when the ε-iron oxide powder particles are present in the surface layer of the magnetic layer with a specific crystal plane that has a stronger binding force with the lubricant oriented more parallel to the magnetic layer surface. The present inventor believes that the more parallel the crystal plane is oriented to the magnetic layer surface, the more functional groups that can exert the lubricating function of the lubricant can be exposed on the magnetic layer surface, which makes it possible to suppress friction when the magnetic layer surface slides against the magnetic head. However, the present invention is not limited to the speculation described in this specification.

[0023] From the viewpoint of friction suppression of the magnetic recording medium having a magnetic layer containing ε-iron oxide powder, the intensity ratio (Int1 / Int2) is 1.0 or more, preferably 1.5 or more, more preferably 2.0 or more, even more preferably 2.5 or more, even more preferably 3.0 or more, and even more preferably 3.5 or more. It is presumed that if the intensity ratio (Int1 / Int2) is 6.5 or less, the amount of functional groups capable of exerting the lubricating function of the lubricant exposed on the magnetic layer surface can be maintained at an appropriate amount. The present inventor believes that this can also contribute to friction suppression of the magnetic recording medium having a magnetic layer containing ε-iron oxide powder. From this viewpoint, the intensity ratio (Int1 / Int2) of the magnetic recording medium is 6.5 or less, preferably 6.0 or less, and more preferably 5.5 or less. A method for controlling the intensity ratio (Int1 / Int2) will be described later.

[0024] The above magnetic recording medium will now be described in more detail.

[0025] <Magnetic layer> <<ε-iron oxide powder>> The magnetic recording medium contains ε-iron oxide powder as a ferromagnetic powder in the magnetic layer. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which the ε-iron oxide crystal structure (ε phase) is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to the ε-iron oxide crystal structure (ε phase), it is determined that the ε-iron oxide crystal structure is detected as the main phase. In addition to the ε phase as the main phase, the α phase and / or γ phase may or may not be included. The ε-iron oxide powder in the present invention and this specification includes so-called non-substituted ε-iron oxide powder composed of iron and oxygen, and so-called substituted ε-iron oxide powder containing one or more substitution elements that substitute for iron.

[0026] (Method of manufacturing ε-iron oxide powder) Known methods for producing ε-iron oxide powder include a method of producing it from goethite, a reverse micelle method, and the like. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a portion of iron is substituted with a substitution element, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp. 5200-5206, and the like.

[0027] For example, the ε-iron oxide powder contained in the magnetic layer of the magnetic recording medium is Preparing a precursor of ε-iron oxide (hereinafter also referred to as a “precursor preparation step”); subjecting the precursor to a coating film forming treatment (hereinafter also referred to as a "coating film forming step"); converting the precursor into ε-iron oxide by subjecting the precursor after the coating formation treatment to a heat treatment (hereinafter also referred to as a "heat treatment step"); and subjecting the ε-iron oxide to a coating removal treatment (hereinafter also referred to as a “coating removal step”); The ε-iron oxide powder can be obtained by a production method in which the ε-iron oxide powder is obtained through the steps of: (1) obtaining the ε-iron oxide powder by subjecting the ε-iron oxide powder to a temperature of 100° C. to 100° C.; and (2) obtaining the ε-iron oxide powder by subjecting the ε-iron oxide powder to a temperature of 100° C. to 100° C.; and (3) obtaining the ε-iron oxide powder by subjecting the ε-iron oxide powder to a temperature of 100° C. to 100° C.;

[0028] Precursor preparation process The precursor of ε-iron oxide refers to a substance that contains the crystal structure of ε-iron oxide as a main phase when heated. The precursor can be, for example, a hydroxide, an oxyhydroxide (oxide hydroxide), or the like that contains iron and an element that can replace a part of the iron in the crystal structure. The precursor preparation step can be carried out by utilizing a coprecipitation method, a reverse micelle method, or the like. Such a method for preparing a precursor is publicly known, and the precursor preparation step in the above-mentioned production method can be carried out by a publicly known method. For example, the method for preparing a precursor can be referred to publicly known techniques such as paragraphs 0017 to 0021 and examples of JP2008-174405A1, paragraphs 0025 to 0046 and examples of WO2016 / 047559A1, and paragraphs 0038 to 0040, 0042, 0044, and 0045 and examples of WO2008 / 149785A1.

[0029] ε-iron oxide that does not contain a substituting element that partially substitutes iron (Fe) can be represented by the composition formula: Fe2O3. On the other hand, ε-iron oxide in which a portion of iron is substituted, for example, by one or more elements, can be represented by the composition formula: A 1 x A 2 y A 3 z Fe (2-x-y-z) It can be expressed by A 1 、 A 2 and A 3Each independently represents one or more substitution elements that substitute for iron, and x, y, and z each independently represent 0 or more and less than 2, with the proviso that at least one of them is greater than 0, and x+y+z is less than 2. The above-mentioned ε-iron oxide powder may not contain a substitution element that substitutes for iron, or may contain, and preferably contains, one or more substitution elements. The type of the substitution element may be one or two or more, and may also be one to three, one to four, one to five, or one to six. The magnetic properties of the ε-iron oxide powder can be adjusted by the type and substitution amount of the substitution element. When a substitution element is contained, the substitution element may be one or more of Ga, Al, In, Rh, Mn, Co, Ni, Zn, Ti, Sn, etc. For example, in the above composition formula, A 1 can be one or more selected from the group consisting of Ga, Al, In and Rh, and A 2 can be one or more selected from the group consisting of Co, Mn, Ni and Zn, and A 3 can be one or more elements selected from the group consisting of Ti and Sn. In one embodiment, the ε-iron oxide powder can contain cobalt (Co), for example, cobalt, one or more elements selected from the group consisting of gallium (Ga), aluminum (Al), indium (In) and rhodium (Rh), and one or more elements selected from the group consisting of titanium (Ti) and tin (Sn). In one embodiment, the ε-iron oxide powder can contain cobalt, gallium and / or aluminum, and titanium. When producing ε-iron oxide powder containing a substituting element that substitutes iron, a part of a compound that serves as an iron supply source in ε-iron oxide may be replaced with a compound of the substituting element. The composition of the obtained ε-iron oxide powder can be controlled by the amount of substitution. Examples of compounds that serve as sources of iron and various substitution elements include inorganic salts (which may be hydrates) such as nitrates, sulfates, and chlorides, organic salts (which may be hydrates) such as pentakis (hydrogen oxalate) salts, hydroxides, and oxyhydroxides.

[0030] Film formation process When the precursor is heated after the coating treatment, the reaction of converting the precursor to ε-iron oxide can proceed under the coating. It is also believed that the coating can play a role in preventing sintering during heating. From the viewpoint of ease of coating formation, the coating treatment is preferably performed in a solution, and more preferably performed by adding a coating agent (a compound for coating formation) to a solution containing the precursor. For example, when the coating treatment is performed in the same solution subsequent to the preparation of the precursor, a coating can be formed on the precursor by adding a coating agent to the solution after the preparation of the precursor and stirring it. A silicon-containing coating can be cited as a preferred coating in terms of ease of forming a coating on the precursor in a solution. A silane compound such as an alkoxysilane can be cited as an example of a coating agent for forming a silicon-containing coating. A silicon-containing coating can be formed on the precursor by hydrolysis of the silane compound, preferably by utilizing a sol-gel method. Specific examples of the silane compound include tetraethoxysilane (TEOS; Tetraethyl orthosilicate), tetramethoxysilane, and various silane coupling agents. For the coating treatment, reference can be made to known techniques such as paragraph 0022 of JP 2008-174405 A and examples therein, paragraphs 0047-0049 of WO2016 / 047559A1 and examples therein, and paragraphs 0041 and 0043 of WO2008 / 149785A1 and examples therein. For example, the coating treatment can be performed by stirring a solution containing the precursor and the coating agent at a liquid temperature of 50 to 90°C. The stirring time can be, for example, 5 to 36 hours. The coating may cover the entire surface of the precursor, or a part of the precursor surface may be uncovered by the coating.

[0031] Heat Treatment Process The precursor after the coating treatment can be converted into ε-iron oxide by subjecting it to a heat treatment. The heat treatment can be performed, for example, on a powder (a precursor powder having a coating) collected from the solution after the coating treatment. For the heat treatment process, reference can be made to known techniques such as paragraph 0023 and examples of JP2008-174405A1, paragraph 0050 and examples of WO2016 / 047559A1, and paragraphs 0041 and 0043 and examples of WO2008 / 149785A1. The heat treatment process can be performed, for example, for about 3 to 6 hours in a heat treatment furnace with an inner temperature of 900 to 1200°C. The higher the temperature at which the heat treatment process is performed and / or the longer the heat treatment time, the larger the average particle size of the obtained ε-iron oxide powder tends to be.

[0032] Film removal process By carrying out the heat treatment step, the precursor having the coating can be converted into ε-iron oxide. Since the coating remains on the ε-iron oxide obtained in this manner, a coating removal process is preferably carried out. For the coating removal process, reference can be made to known techniques such as paragraph 0025 of JP 2008-174405 A and the Examples therein, and paragraph 0053 of WO2008 / 149785A1 and the Examples therein. The coating removal process can be carried out, for example, by stirring the ε-iron oxide having the coating in an aqueous sodium hydroxide solution having a concentration of about 1 to 5 mol / L and a liquid temperature of about 60 to 90° C. for about 5 to 36 hours. However, the ε-iron oxide powder contained in the magnetic layer of the magnetic recording medium may be one produced without undergoing the coating removal process, or one in which the coating is not completely removed in the coating removal process and some of the coating remains.

[0033] Crushing process One or more steps may be optionally performed before and / or after the various steps described above. Examples of such steps include various known steps such as classification, filtration, washing, and drying. Furthermore, for example, the ε-iron oxide powder obtained after drying may be subjected to a pulverization treatment. The pulverization treatment may contribute to breaking down the agglomeration of the ε-iron oxide powder particles. From the viewpoint of improving the dispersibility of the ε-iron oxide powder, it is preferable to subject the ε-iron oxide powder to a dispersion treatment described later after breaking down the agglomeration of the particles. The present inventors speculate that by increasing the dispersibility of the ε-iron oxide powder, a specific crystal plane of the ε-iron oxide powder particles that has a strong binding force with the lubricant can be oriented more parallel to the magnetic layer surface by the electric field application treatment described later. The pulverization treatment may be performed, for example, by a pulverization treatment using a mill pulverizer (mill pulverization). The mill pulverization treatment conditions may be set according to the mill pulverizer used, and are not particularly limited. As an example, the rotation speed of the mill grinder can be 1000 to 20000 rpm (revolutions per minute), the processing time for one mill grinding can be 0.5 to 10 minutes, and the number of times mill grinding is performed can be 1 to 4 times.

[0034] (Average particle size) From the viewpoint of magnetization stability, the average particle size of the ε-iron oxide powder contained in the magnetic layer of the magnetic recording medium is preferably 5.0 nm or more, more preferably 6.0 nm or more, even more preferably 7.0 nm or more, even more preferably 8.0 nm or more, and even more preferably 9.0 nm or more. From the viewpoint of high-density recording, the average particle size of the ε-iron oxide powder is preferably 20.0 nm or less, more preferably 19.0 nm or less, even more preferably 18.0 nm or less, even more preferably 17.0 nm or less, even more preferably 16.0 nm or less, and even more preferably 15.0 nm or less.

[0035] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as the ε-iron oxide powder is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and a photograph of the particles that make up the powder is obtained by printing it on photographic paper or displaying it on a display so that the total magnification is 500,000 times. From the obtained particle photograph, the target particle is selected, and the particle outline is traced with a digitizer to measure the particle (primary particle) size. Primary particles are independent particles that are not aggregated. The above measurements are carried out on 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is taken as the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.

[0036] As a method for collecting a sample powder from a magnetic recording medium for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.

[0037] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or amorphous shape, and in which the major axis of the particle cannot be identified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.

[0038] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values ​​obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).

[0039] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass %, and more preferably in the range of 60 to 90 mass %, relative to the mass of the magnetic layer. A high content of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.

[0040] <<Binding agent>> The magnetic recording medium may be a coating type magnetic recording medium, and may contain a binder in the magnetic layer. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coating type magnetic recording media may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination of a plurality of resins. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the non-magnetic layer and / or backcoat layer described below. For the above binders, refer to paragraphs 0028 to 0031 of JP-A-2010-24113. The binder may also be a radiation-curable resin such as an electron beam curable resin. For the radiation-curable resin, refer to paragraphs 0044 to 0045 of JP-A-2011-048878. The average molecular weight of the resin used as the binder may be, for example, 10,000 to 200,000 in weight average molecular weight. The weight average molecular weight in the present invention and this specification is a value obtained by converting a value measured by gel permeation chromatography (GPC) under the following measurement conditions into a polystyrene equivalent. The weight average molecular weight of the binder shown in the examples described later is a value obtained by converting a value measured under the following measurement conditions into a polystyrene equivalent. The binder can be used in an amount of, for example, 1.0 to 30.0 parts by mass relative to 100.0 parts by mass of the ferromagnetic powder. GPC equipment: HLC-8120 (Tosoh Corporation) Column: TSK gel Multipore HXL-M (Tosoh Corporation, 7.8 mm ID (inner diameter) × 30.0 cm) Eluent: tetrahydrofuran (THF)

[0041] A curing agent can also be used together with the resin usable as a binder. In one form, the curing agent can be a thermosetting compound, which is a compound in which a curing reaction (crosslinking reaction) proceeds by heating, and in another form, it can be a photocuring compound in which a curing reaction (crosslinking reaction) proceeds by light irradiation. As the curing reaction proceeds in the magnetic layer forming process, at least a part of the curing agent can be contained in the magnetic layer in a state of reacting (crosslinking) with other components such as the binder. This point is also true for a layer formed using a composition used to form another layer when the composition contains a curing agent. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details of polyisocyanate, refer to paragraphs 0124 to 0125 of JP 2011-216149 A. The curing agent can be used in the magnetic layer forming composition in an amount of, for example, 0 to 80.0 parts by mass per 100.0 parts by mass of the binder, and from the viewpoint of improving the strength of the magnetic layer, preferably 10.0 to 80.0 parts by mass, and more preferably 50.0 to 80.0 parts by mass.

[0042] The above descriptions regarding the binder and hardener can also be applied to the nonmagnetic layer and / or backcoat layer, in which case the above descriptions regarding the contents can be applied by replacing the ferromagnetic powder with the nonmagnetic powder.

[0043] <<Additives>> The magnetic layer may contain one or more additives as necessary. The additives may be selected from commercially available products or produced by known methods according to the desired properties and used in any amount. An example of the additive is the above-mentioned curing agent. Examples of additives contained in the magnetic layer include non-magnetic powder, lubricant, dispersant, dispersion aid, antifungal agent, antistatic agent, antioxidant, etc. For the dispersant, refer to paragraphs 0061 and 0071 of JP-A-2012-133837. The dispersant may be added to the composition for forming the non-magnetic layer. For the dispersant that can be added to the composition for forming the non-magnetic layer, refer to paragraph 0061 of JP-A-2012-133837.

[0044] Non-magnetic powders that can be included in the magnetic layer include non-magnetic powders that can function as abrasives. The content of the abrasive in the magnetic layer is preferably 1.0 to 20.0 parts by mass, more preferably 3.0 to 15.0 parts by mass, and even more preferably 4.0 to 10.0 parts by mass, relative to 100.0 parts by mass of the ferromagnetic powder. An example of an additive that can be used to improve the dispersibility of the abrasive in the magnetic layer containing the abrasive is the dispersant described in paragraphs 0012 to 0022 of JP 2013-131285 A.

[0045] Examples of non-magnetic powders that can be contained in the magnetic layer include non-magnetic powders (e.g., non-magnetic colloidal particles, carbon black, etc.) that can function as protrusion-forming agents that form protrusions that protrude appropriately on the magnetic layer surface. For example, protrusion-forming agents having an average particle size of 5 to 300 nm can be used. The average particle size of colloidal silica (silica colloidal particles) shown in the examples described below is a value determined by the method described as a method for measuring average particle size in paragraph 0015 of JP-A-2011-048878. The content of the protrusion-forming agent in the magnetic layer is, for example, preferably 0.1 to 3.5 parts by mass, more preferably 0.1 to 3.0 parts by mass, per 100.0 parts by mass of ferromagnetic powder.

[0046] (Lubricant) The magnetic recording medium may contain one or more lubricants in the portion on the non-magnetic support on the magnetic layer side. In the present invention and this specification, the "portion on the non-magnetic support on the magnetic layer side" refers to the magnetic layer in the case of a magnetic recording medium having a magnetic layer directly on the non-magnetic support, and refers to the magnetic layer and / or the non-magnetic layer in the case of a magnetic recording medium having a non-magnetic layer between the non-magnetic support and the magnetic layer, which will be described in detail later. The lubricant may be one or more selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides. As described above, the lubricant may contribute to friction suppression in a magnetic recording medium having a magnetic layer containing ε-iron oxide powder.

[0047] Examples of fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc., with stearic acid, myristic acid, and palmitic acid being preferred, and stearic acid being more preferred. The fatty acid may be contained in the magnetic layer in the form of a salt such as a metal salt. Examples of fatty acid esters include esters of various fatty acids exemplified above with respect to fatty acids, etc. Specific examples include butyl myristate, butyl palmitate, butyl stearate (butyl stearate), neopentyl glycol dioleate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, oleyl oleate, isocetyl stearate, isotridecyl stearate, octyl stearate, isooctyl stearate, amyl stearate, butoxyethyl stearate, etc. Examples of the fatty acid amide include amides of the various fatty acids exemplified above, specifically, for example, lauric acid amide, myristic acid amide, palmitic acid amide, stearic acid amide, and the like. As for fatty acids and fatty acid derivatives (amides, esters, etc.), it is preferable that the fatty acid-derived portion of the fatty acid derivative has the same or similar structure as the fatty acid used in combination. For example, when stearic acid is used as the fatty acid, it is preferable to use stearic acid amide and / or stearic acid ester in combination.

[0048] Regarding the fatty acid content, the fatty acid content of the magnetic layer forming composition is, for example, 0.1 to 10.0 parts by mass, preferably 1.0 to 7.0 parts by mass, per 100.0 parts by mass of ferromagnetic powder. When two or more different fatty acids are added to the magnetic layer forming composition, the content refers to the total content of the two or more different fatty acids. This also applies to other components. In the present invention and this specification, unless otherwise specified, a certain component may be used in one type or in two or more types. Regarding the fatty acid ester content, the fatty acid ester content of the magnetic layer forming composition is, for example, 0 to 10.0 parts by mass, and preferably 1.0 to 7.0 parts by mass per 100.0 parts by mass of the ferromagnetic powder. The fatty acid amide content in the magnetic layer-forming composition is, for example, 0.1 to 3.0 parts by mass, and preferably 0.1 to 1.0 part by mass, per 100.0 parts by mass of the ferromagnetic powder.

[0049] On the other hand, the fatty acid content of the nonmagnetic layer forming composition is, for example, 1.0 to 10.0 parts by mass, preferably 1.0 to 7.0 parts by mass, per 100.0 parts by mass of nonmagnetic powder. The fatty acid ester content of the nonmagnetic layer forming composition is, for example, 0 to 10.0 parts by mass, preferably 1.0 to 7.0 parts by mass, per 100.0 parts by mass of nonmagnetic powder. The fatty acid amide content of the nonmagnetic layer forming composition is, for example, 0.1 to 3.0 parts by mass, preferably 0.1 to 1.0 parts by mass, per 100.0 parts by mass of nonmagnetic powder. The nonmagnetic layer can play a role of retaining a lubricant and supplying it to the magnetic layer. The lubricant contained in the nonmagnetic layer can migrate to the magnetic layer and be present in the magnetic layer.

[0050] The magnetic layer described above can be provided directly on the surface of the non-magnetic support, or indirectly via a non-magnetic layer.

[0051] <Nonmagnetic layer> The nonmagnetic powder used in the nonmagnetic layer may be a powder of an inorganic substance or a powder of an organic substance. Carbon black or the like can also be used. Examples of inorganic substances include metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, and metal sulfides. These nonmagnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black usable in the nonmagnetic layer, refer to paragraphs 0040 to 0041 of JP-A-2010-24113. The content (filling rate) of the nonmagnetic powder in the nonmagnetic layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass, based on the mass of the nonmagnetic layer.

[0052] The non-magnetic layer may contain a binder and may also contain an additive. For other details of the binder, additive, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additive, known techniques related to magnetic layers can also be applied.

[0053] In the present invention and this specification, the nonmagnetic layer also includes a substantially nonmagnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, together with the nonmagnetic powder. Here, the substantially nonmagnetic layer refers to a layer having a residual magnetic flux density of 10 mT or less, a coercive force of 7.96 kA / m (100 Oe) or less, or a layer having a residual magnetic flux density of 10 mT or less and a coercive force of 7.96 kA / m (100 Oe) or less. It is preferable that the nonmagnetic layer has no residual magnetic flux density or coercive force.

[0054] <Nonmagnetic support> Next, the non-magnetic support will be described. Examples of the non-magnetic support (hereinafter, simply referred to as "support") include known biaxially stretched polyethylene terephthalate, polyethylene naphthalate, polyamides such as aromatic polyamides, polyamideimides, and the like. Among these, polyethylene terephthalate, polyethylene naphthalate, and polyamides are preferred. These supports may be subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, and the like in advance.

[0055] <Backcoat layer> In one embodiment, the magnetic recording medium may have a backcoat layer containing a nonmagnetic powder on the surface side opposite to the surface side having the magnetic layer of the nonmagnetic support, and in another embodiment, may not have a backcoat layer. The backcoat layer preferably contains one or both of carbon black and inorganic powder. The backcoat layer may contain a binder and may also contain additives. For the binder and additive of the backcoat layer, known techniques related to the backcoat layer may be applied, and known techniques related to the formulation of the magnetic layer and / or the nonmagnetic layer may also be applied. For example, the descriptions of paragraphs 0018 to 0020 of JP-A-2006-331625 and US Pat. No. 7,029,774, column 4, line 65 to column 5, line 38, may be referred to for the backcoat layer.

[0056] <Various thicknesses> The thickness of the non-magnetic support is preferably 3.0 to 6.0 μm.

[0057] From the viewpoint of high density recording, which has been demanded in recent years, the thickness of the magnetic layer is preferably 200 nm or less, more preferably in the range of 8 to 200 nm, and even more preferably in the range of 10 to 200 nm. At least one magnetic layer is sufficient, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers.

[0058] The thickness of the nonmagnetic layer is, for example, 0.1 to 1.5 μm, and preferably 0.1 to 1.0 μm.

[0059] The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably in the range of 0.1 to 0.7 μm.

[0060] The thickness of each layer of the magnetic recording medium and the non-magnetic support can be determined by a known film thickness measurement method. For example, the cross section of the magnetic recording medium in the thickness direction is exposed by a known method such as ion beam or microtome, and then the exposed cross section is observed using a transmission electron microscope or a scanning electron microscope. Various thicknesses can be determined as the thickness determined at one location in the cross section observation, or the arithmetic average of the thicknesses determined at two or more randomly selected locations. Alternatively, the thickness of each layer may be determined as a design thickness calculated from the manufacturing conditions.

[0061] <Manufacturing process> The process of preparing a composition for forming a magnetic layer, a non-magnetic layer, or a backcoat layer can usually include at least a kneading process, a dispersing process, and a mixing process provided before or after these processes as necessary. Each process may be divided into two or more stages. The components used in the preparation of each layer-forming composition may be added at the beginning or during any process. As the solvent, one or more of various solvents usually used in the manufacture of coating-type magnetic recording media can be used. For the solvent, see, for example, paragraph 0153 of JP-A-2011-216149. Also, each component can be added in two or more steps in separate steps. In order to manufacture the magnetic recording medium, conventional known manufacturing techniques can be used in various processes. In the kneading process, it is preferable to use a device with strong kneading power, such as an open kneader, a continuous kneader, a pressure kneader, or an extruder. For details of these kneading processes, see JP-A-1-106338 and JP-A-1-79274. Known dispersing machines can be used. As the dispersion media, one or more types of dispersion beads selected from the group consisting of various dispersion beads can be used. As such dispersion beads, zirconia beads, titania beads, and steel beads, which are dispersion beads with high specific gravity, are suitable. The present inventors speculate that strengthening the dispersion process to increase the dispersibility of the ε-iron oxide powder in the preparation of the magnetic layer forming composition can contribute to orienting a specific crystal face of the ε-iron oxide powder particles, which has a strong binding force with the lubricant, more parallel to the magnetic layer surface by the electric field application process described below. Specific examples of strengthening the dispersion process include extending the dispersion process time, reducing the diameter of the dispersion beads used for dispersion, and increasing the number of dispersion processes. Various dispersion conditions can be set according to the dispersing machine used. As an example, the bead diameter of the dispersion beads can be 0.1 to 1.0 mm, the processing time of one dispersion process can be 0.5 to 10 hours, and the number of dispersion processes can be two or more. Each layer forming composition may be filtered by a known method before being subjected to the coating process. Filtration can be performed, for example, by filter filtration.The filter used for filtration may be, for example, a filter with a pore size of 0.01 to 3 μm (eg, a glass fiber filter, a polypropylene filter, etc.).

[0062] The magnetic layer can be formed by directly applying the magnetic layer-forming composition onto the non-magnetic support, or by sequentially or simultaneously applying the magnetic layer-forming composition and the non-magnetic layer-forming composition in a multilayer manner. For details on the coating for forming each layer, see paragraph 0066 of JP2010-231843A.

[0063] After the coating step, various treatments such as drying, orientation of the magnetic layer, and surface smoothing (calendering) can be performed. For various treatments, known techniques such as paragraphs 0052 to 0057 of JP-A-2010-24113 can be referred to. For example, the coating layer of the magnetic layer-forming composition can be subjected to orientation treatment while the coating layer is in a wet state. For the orientation treatment, various known techniques including those described in paragraph 0067 of JP-A-2010-231843 can be applied. For example, the vertical orientation treatment can be performed by known methods such as a method using magnets with different poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the transport speed of the non-magnetic support on which the coating layer is formed in the orientation zone. In addition, the coating layer may be pre-dried before being transported to the orientation zone.

[0064] Preferably, the electric field application treatment can be performed while the coating layer of the composition for forming a magnetic layer is in a wet state. The electric field application treatment can be performed, for example, after the orientation treatment. The non-magnetic support on which the coating layer of the composition for forming a magnetic layer is formed is transported between a pair of opposing electrodes, so that an electric field can be applied perpendicularly to the surface of the coating layer. The electrodes can be arranged, for example, with a positive electrode on the magnetic layer side and a negative electrode on the other side (for example, the backcoat layer side). The applied electric field strength can be, for example, 0.2 to 2.5 kV / mm, and the greater the applied electric field strength, the greater the value of the intensity ratio (Int1 / Int2) tends to be. The present inventors speculate that the electric field application treatment can be performed to orient the functional groups of the lubricant bonded to a specific crystal plane of the ε-iron oxide powder particles by the electric field. The present inventors believe that this can contribute to orienting the specific crystal plane of the ε-iron oxide powder particles bonded to the lubricant more parallel to the magnetic layer surface.

[0065] The magnetic recording medium according to one embodiment of the present invention may be a tape-shaped magnetic recording medium (magnetic tape) or a disk-shaped magnetic recording medium (magnetic disk). For example, a magnetic tape is usually housed in a magnetic tape cartridge, and the magnetic tape cartridge is mounted in a magnetic recording and reproducing device. A servo pattern may be formed on the magnetic recording medium by a known method to enable head tracking in the magnetic recording and reproducing device. "Formation of a servo pattern" may also be referred to as "recording of a servo signal." Formation of a servo pattern will be described below using a magnetic tape as an example.

[0066] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Control methods that use servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.

[0067] As shown in ECMA (European Computer Manufacturers Association)-319 (June 2001), magnetic tapes (commonly called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard use a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. As described above, the reason why the servo pattern is formed by a pair of non-parallel magnetic stripes is to inform the servo signal reading element passing over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this purpose, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.

[0068] A servo band is made up of a series of servo signals along the length of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is called a data band. A data band is made up of multiple data tracks, and each data track corresponds to one servo track.

[0069] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.

[0070] As a method for uniquely identifying servo bands, there is also a method using the staggered method as shown in ECMA-319 (June 2001). In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. The combination of the shift between adjacent servo bands is unique across the entire magnetic tape, so when the servo pattern is read by two servo signal reading elements, it is possible to uniquely identify the servo bands.

[0071] Also, as specified in ECMA-319 (June 2001), information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.

[0072] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.

[0073] The head for forming a servo pattern is called a servo write head. The servo write head has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.

[0074] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.

[0075] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This makes it possible to increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.

[0076] The magnetic tape is usually contained in a magnetic tape cartridge, and the magnetic tape cartridge is loaded into a magnetic recording and reproducing device.

[0077] [Magnetic tape cartridge] One aspect of the present invention relates to a magnetic tape cartridge including the above-mentioned magnetic recording medium in tape form (that is, a magnetic tape).

[0078] The details of the magnetic tape contained in the magnetic tape cartridge are as described above.

[0079] In a magnetic tape cartridge, the magnetic tape is generally accommodated inside the cartridge body in a state where it is wound around a reel. The reel is provided rotatably inside the cartridge body. As the magnetic tape cartridge, a single-reel type magnetic tape cartridge having one reel inside the cartridge body and a twin-reel type magnetic tape cartridge having two reels inside the cartridge body are widely used. When a single-reel type magnetic tape cartridge is loaded into a magnetic recording and reproducing device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound around the reel on the magnetic recording and reproducing device side. A magnetic head is disposed on the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape is fed and wound between the reel (supply reel) on the magnetic tape cartridge side and the reel (take-up reel) on the magnetic recording and reproducing device side. During this time, the magnetic head comes into contact with and slides on the surface of the magnetic layer side of the magnetic tape, thereby recording and / or reproducing data. In contrast, a twin-reel magnetic tape cartridge has both a supply reel and a take-up reel inside the magnetic tape cartridge. The magnetic tape cartridge may be either a single-reel type or a twin-reel type. The magnetic tape cartridge may include the magnetic tape according to one aspect of the present invention, and other aspects may be based on known techniques. The total length of the magnetic tape contained in the magnetic tape cartridge may be, for example, 800 m or more, and may be in the range of about 800 m to 2000 m. A long total length of the tape contained in the magnetic tape cartridge is preferable from the viewpoint of increasing the capacity of the magnetic tape cartridge.

[0080] [Magnetic recording and playback device] One aspect of the present invention relates to a magnetic recording and reproducing device including the above magnetic recording medium.

[0081] In the present invention and this specification, the term "magnetic recording and reproducing device" refers to a device that can perform at least one of recording data to a magnetic recording medium and reproducing data recorded on the magnetic recording medium. Such a device is generally called a drive. In one embodiment of the magnetic recording and reproducing device, the magnetic recording medium is treated as a removable medium (so-called exchangeable medium). In such a embodiment, for example, a magnetic tape cartridge containing a magnetic tape is inserted into the magnetic recording and reproducing device and removed. That is, in one embodiment, the magnetic recording and reproducing device can include the magnetic tape cartridge in a removably manner. In another embodiment, the magnetic recording medium is not treated as an exchangeable medium, and the magnetic head and the magnetic recording medium are housed in the magnetic recording and reproducing device. In such a embodiment, for example, the magnetic tape is wound around a reel in the magnetic recording and reproducing device equipped with the magnetic head and housed therein. The magnetic recording and reproducing device may be, for example, a sliding type magnetic recording and reproducing device, which refers to a device in which a magnetic head comes into contact with and slides against the surface of the magnetic layer when recording data on the magnetic recording medium and / or reproducing the recorded data.

[0082] The magnetic recording and reproducing device may include a magnetic head. The magnetic head may be a recording head capable of recording data on a magnetic recording medium, or may be a reproducing head capable of reproducing data recorded on the magnetic recording medium. In one embodiment, the magnetic recording and reproducing device may include both a recording head and a reproducing head as separate magnetic heads. In another embodiment, the magnetic head included in the magnetic recording and reproducing device may have a configuration in which both an element for recording data (recording element) and an element for reproducing data (reproducing element) are provided in one magnetic head. Hereinafter, the element for recording data and the element for reproducing data are collectively referred to as "data element". As the reproducing head, a magnetic head (MR head) including a magnetoresistive (MR) element capable of reading data recorded on a magnetic tape with good sensitivity as a reproducing element is preferable. As the MR head, various known MR heads such as an anisotropic magnetoresistive (AMR) head, a giant magnetoresistive (GMR) head, and a tunnel magnetoresistive (TMR) head may be used. Also, the magnetic head that records and / or reproduces data may include a servo signal read element. Alternatively, the magnetic recording and reproducing device may include a magnetic head (servo head) equipped with a servo signal read element as a head separate from the magnetic head that records and / or reproduces data. For example, the magnetic head that records and / or reproduces recorded data (hereinafter also referred to as a "recording and reproducing head") may include two servo signal read elements, and each of the two servo signal read elements can simultaneously read two adjacent servo bands. One or more data elements may be disposed between the two servo signal read elements.

[0083] In the magnetic recording and reproducing device, the recording of data on the magnetic recording medium and / or the reproduction of data recorded on the magnetic recording medium can be performed, for example, by contacting and sliding the magnetic head against the surface of the magnetic recording medium on the magnetic layer side. The magnetic recording and reproducing device may include the magnetic recording medium according to one embodiment of the present invention, and other known techniques may be applied.

[0084] For example, when recording data and / or reproducing recorded data, tracking using servo signals is first performed. That is, the servo signal reading element is made to follow a specific servo track, so that the data element passes over the target data track. The data track is moved by changing the servo track read by the servo signal reading element in the tape width direction. The recording / reproducing head can also record and / or reproduce data on other data bands by using the UDIM information described above to move the servo signal reading element to a specific servo band and start tracking on that servo band. EXAMPLES

[0085] The present invention will be described below based on examples. However, the present invention is not limited to the embodiments shown in the examples. "Parts" and "%" described below mean "parts by mass" and "% by mass" unless otherwise specified. "eq" is an equivalent, and is a unit that cannot be converted to SI units. In addition, the steps and evaluations described below were performed in an environment with an atmospheric temperature of 23°C ± 1°C unless otherwise specified.

[0086] [Example 1] <Preparation of ferromagnetic powder No. 1> In 90 g of pure water, iron (III) nitrate nonahydrate (amount added: "Fe nitrate amount" in Table 1), gallium (III) nitrate octahydrate (amount added: "Ga nitrate amount" in Table 1), cobalt (II) nitrate hexahydrate (amount added: "Co nitrate amount" in Table 1), titanium (IV) sulfate (amount added: "Ti sulfate amount" in Table 1), and polyvinylpyrrolidone (PVP) 16.7 g were dissolved, and 44.0 g of ammonia solution with a concentration of 25% was added under the condition of an atmospheric temperature of 25 ° C. while stirring with a magnetic stirrer in the air atmosphere, and the mixture was stirred for 2 hours at an atmospheric temperature of 25 ° C. To the obtained solution, an aqueous citric acid solution obtained by dissolving 11 g of citric acid in 100 g of pure water was added, and the mixture was stirred for 1 hour. The powder precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace with an internal temperature of 80 ° C. The dried powder was added with 8900g of pure water, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to 50°C, and 440g of 25% ammonia aqueous solution was added dropwise while stirring. After stirring for 1 hour while maintaining the temperature at 50°C, 160mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 500g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried for 24 hours in a heating furnace with an internal temperature of 80°C to obtain a precursor of ferromagnetic powder. The obtained precursor of the ferromagnetic powder was placed in a heating furnace at the furnace temperature shown in Table 1 under an air atmosphere, and subjected to a heat treatment for 4 hours. The heat-treated powder was placed in a 4 mol / L aqueous solution of sodium hydroxide (NaOH), and the liquid temperature was maintained at 75° C. while stirring for 24 hours to carry out the coating removal step. Thereafter, the ferromagnetic powder after the coating removal process was collected by centrifugation, washed with pure water, and dried in a heating furnace at an internal temperature of 95° C. After drying, a milling process was carried out using an absolute mill (ABS-W manufactured by Osaka Chemical Co., Ltd.) under the conditions shown in Table 1. The composition of the ferromagnetic powder No. 1 obtained through the above steps was confirmed by inductively coupled plasma-optical emission spectrometry (ICP-OES), and it was confirmed to be a substituted ε-iron oxide having the composition shown in Table 1. The values ​​shown in Table 1 for the composition are those of the composition formula: A 1 x A 2 y A 3 z Fe (2-x-y-z) The numbers of each element in O3 are ((2-xyz), x, y, z). In addition, the CuKα ray was scanned at a voltage of 45 kV and an intensity of 40 mA to measure the X-ray diffraction pattern under the conditions below (X-ray diffraction analysis). From the peaks in the X-ray diffraction pattern, it was confirmed that the obtained ferromagnetic powder has a single-phase ε-phase crystal structure (ε-iron oxide crystal structure) without containing α-phase and γ-phase crystal structures. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees

[0087] <Magnetic tape production> <<Composition for forming magnetic layer>> (Magnetic liquid) ε-iron oxide powder (ferromagnetic powder listed in Table 1): 100.0 parts Sulfonic acid group-containing polyurethane resin: 15.0 parts Cyclohexanone: 150.0 parts Methyl ethyl ketone: 150.0 parts (abrasive liquid) α-alumina (average particle size: 110 nm): 9.0 parts Vinyl chloride copolymer (Kaneka MR110): 0.7 parts Cyclohexanone: 20.0 parts (Protrusion forming agent liquid) Colloidal silica (average particle size 100 nm): 1.3 parts Methyl ethyl ketone: 9.0 parts Cyclohexanone: 6.0 parts (Other Ingredients) Lubricant: See Table 1 for type and amount Polyisocyanate (Tosoh Coronate): 2.5 parts (Finishing solvent) Cyclohexanone: 180.0 parts Methyl ethyl ketone: 180.0 parts

[0088] <<Composition for forming non-magnetic layer>> Non-magnetic inorganic powder (α-iron oxide): 80.0 parts (Average particle size: 0.15 μm, average acicular ratio: 7, BET (Brunauer-Emmett-Teller) specific surface area: 52 m 2 / g) Carbon black (average particle size: 20 nm): 20.0 parts Electron beam curable vinyl chloride copolymer: 13.0 parts Electron beam curing polyurethane resin: 6.0 parts Phenylphosphonic acid: 3.0 parts Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Butyl stearate: 4.0 parts Stearic acid: 1.0 parts

[0089] <Composition for forming backcoat layer> Non-magnetic inorganic powder (α-iron oxide): 80.0 parts (Average particle size: 0.15 μm, average acicular ratio: 7, BET specific surface area: 52 m 2 / g) Carbon black (average particle size: 20 nm): 20.0 parts Carbon black (average particle size: 100 nm): 3.0 parts Vinyl chloride copolymer: 13.0 parts Sulfonic acid group-containing polyurethane resin: 6.0 parts Phenylphosphonic acid: 3.0 parts Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Stearic acid: 3.0 parts Polyisocyanate (Tosoh Coronate): 5.0 parts Methyl ethyl ketone: 400.0 parts

[0090] <<Preparation of compositions for forming each layer>> The magnetic layer forming composition was prepared by the following method. The magnetic liquid was prepared by dispersing the various components of the magnetic liquid. Dispersion was performed using a batch-type vertical sand mill under the dispersion treatment conditions for the first and second passes as shown in Table 1. Zirconia beads were used as dispersion beads. After mixing the various components of the above abrasive liquid, they were placed in a vertical sand mill disperser together with zirconia beads having a bead diameter of 1 mm, and the ratio of the bead volume to the total volume of the abrasive liquid and the bead volume was adjusted to 60%, and a sand mill dispersion process was carried out for 180 minutes. The liquid after the sand mill dispersion process was taken out and subjected to ultrasonic dispersion filtration process using a flow-type ultrasonic dispersion filtration device, to prepare the abrasive liquid. The magnetic liquid, abrasive liquid, protrusion-forming agent liquid, other components, and finishing additive solvent were introduced into a dissolver stirrer and stirred for 30 minutes at a peripheral speed of 10 m / sec. After that, the mixture was treated with a flow-type ultrasonic disperser at a flow rate of 7.5 kg / min with two passes, and then filtered once with a filter having a pore size of 1.0 μm to prepare a magnetic layer-forming composition.

[0091] The composition for forming the nonmagnetic layer was prepared by the following method. The above components, except for the lubricants (butyl stearate and stearic acid), were kneaded and diluted using an open kneader, and then dispersed using a horizontal bead mill disperser.Then, the lubricants (butyl stearate and stearic acid) were added, and the mixture was stirred and mixed using a dissolver stirrer to prepare a composition for forming a nonmagnetic layer.

[0092] The composition for forming the backcoat layer was prepared by the following method. The above components except lubricant (stearic acid), polyisocyanate and methyl ethyl ketone (400.0 parts) were kneaded and diluted by an open kneader, and then dispersed by a horizontal bead mill disperser. Then, lubricant (stearic acid), polyisocyanate and methyl ethyl ketone (400.0 parts) were added, and the mixture was stirred and mixed by a dissolver stirrer to prepare a backcoat layer forming composition.

[0093] <<Magnetic tape production>> A non-magnetic layer forming composition was applied to the surface of a 5.0 μm thick biaxially oriented polyethylene naphthalate support so that the thickness after drying was 1.0 μm, and then the support was dried and irradiated with an electron beam at an acceleration voltage of 125 kV and an energy of 40 kGy. A magnetic layer forming composition was applied thereon so that the thickness after drying was 50 nm to form a coating layer. While the coating layer was in a wet state, a magnetic field with a magnetic field strength of 0.6 T was applied perpendicularly to the surface of the coating layer in the orientation zone to perform a vertical orientation treatment. Immediately after that, an electric field with the electric field strength shown in Table 1 was applied perpendicularly to the surface of the coating layer by a positive electrode arranged on the coating layer side and a negative electrode arranged on the opposite side, and then the magnetic layer was dried to form a magnetic layer. Thereafter, a backcoat layer forming composition was applied to the surface of the support opposite to the surface on which the non-magnetic layer and magnetic layer were formed so that the thickness after drying was 0.5 μm, and then dried to form a backcoat layer. Thereafter, the surface was smoothed (calendered) using a calender roll consisting only of a metal roll at a calendering speed of 80 m / min, a linear pressure of 300 kg / cm (294 kN / m), and a surface temperature of 110°C. Then, the tape was heat-treated for 36 hours in an environment with an atmospheric temperature of 70°C. After the heat treatment, the tape was slit into a width of 1 / 2 inch (0.0127 meters), and the surface of the magnetic layer was cleaned with a tape cleaning device attached to a device having a device for feeding and winding the slit product so that a nonwoven fabric and a razor blade were pressed against the surface of the magnetic layer. After that, with the magnetic layer of the magnetic tape in a demagnetized state, a servo pattern was formed on the magnetic layer with an arrangement and shape according to the LTO (Linear Tape-Open) Ultrium format by a servo write head mounted on a servo writer. In this way, a magnetic tape was obtained in which the magnetic layer had a data band, a servo band, and a guide band in an arrangement according to the LTO Ultrium format, and the servo band had a servo pattern on it with an arrangement and shape according to the LTO Ultrium format.

[0094] [Examples 2 to 12, Comparative Examples 1 to 6] Ferromagnetic powders and magnetic tapes were prepared in the same manner as in Example 1, except that the items shown in Table 1 were changed as shown in Table 1. For ferromagnetic powder No. 8, the "amount of Al nitrate" in Table 1 indicates the amount of aluminum (III) nitrate nonahydrate. For the comparative examples in Table 1 with "0.0" written in the electric field strength column, no electric field application process was performed when the magnetic tape was prepared. ICP-OES was also performed on ferromagnetic powders No. 2 to 12 in Table 1 to confirm their compositions, and it was confirmed that Nos. 2 to 8 and 10 to 12 were substituted ε-iron oxides having the compositions shown in Table 1, while No. 9 was unsubstituted ε-iron oxide. In addition, CuKα radiation was scanned at a voltage of 45 kV and an intensity of 40 mA to measure the X-ray diffraction patterns (X-ray diffraction analysis) under the conditions described above, and it was confirmed from the peaks in the X-ray diffraction pattern that all of the obtained ferromagnetic powders had a single-phase ε-phase crystal structure (ε-iron oxide crystal structure) without containing α-phase or γ-phase crystal structures.

[0095] The average particle size of the ferromagnetic powder was determined by the method described above using a Hitachi H-9000 transmission electron microscope as the transmission electron microscope and Carl Zeiss KS-400 image analysis software as the image analysis software. The determined average particle size is shown in Table 1 as the ferromagnetic powder size.

[0096] [Evaluation method] <Intensity ratio (Int1 / Int2)> A tape sample was cut out from the prepared magnetic tape. For the cut-out tape samples, X-rays were irradiated onto the magnetic layer surface using a thin-film X-ray diffractometer (Rigaku SmartLab) and in-plane XRD was performed as described above. From the X-ray diffraction spectrum obtained by in-plane XRD, Int1 and Int2 were obtained, and the intensity ratio (Int1 / Int2) was calculated from the obtained values.

[0097] <Friction evaluation> A 50 m long tape sample was cut out from the prepared magnetic tape. In an environment where the ambient temperature was 32°C ± 1°C and the relative humidity was 80%, a magnetic recording and reproducing head (hereinafter simply referred to as "head") removed from an IBM LTO (registered trademark) G6 (Linear Tape-Open Generation 6) drive was attached to a tape running system. In this tape running system, the above-mentioned tape sample was sent out from a sending roll while applying a tension of 0.6 N (Newton) in the tape longitudinal direction, run at 10 m / sec, and wound up on a take-up roll, and run for 10,000 cycles. A strain gauge was attached to the above-mentioned head, and the voltage value obtained when the magnetic layer surface and the head slid together was monitored, and if the voltage value exceeded a predetermined value, it was determined that the tape had stuck. Here, the direction toward the other end of the magnetic tape based on one end is called the inside, and the 5 m long region from the position 5 m to the position 10 m from the end of the magnetic tape toward the inside is defined as the acceleration region. The number of times the tape stuck was counted for a total of 10 m long regions including the acceleration region on one end side of the magnetic tape and the acceleration region on the other end side. If sticking occurs less than five times during 10,000 cycles, the performance can be evaluated as being capable of meeting the stringent needs of the future.

[0098] The above results are shown in Table 1 (Table 1-1 to Table 1-3).

[0099] [Table 1-1]

[0100] [Table 1-2]

[0101] [Table 1-3]

[0102] From the results shown in Table 1, it can be confirmed that in the magnetic tapes of the Examples, friction during sliding between the magnetic layer surface and the magnetic head is suppressed compared to the magnetic tapes of the Comparative Examples. [Industrial Applicability]

[0103] One aspect of the present invention is useful in data storage applications.

Claims

1. A magnetic recording medium having a non-magnetic support and a magnetic layer containing ferromagnetic powder, the ferromagnetic powder is ε-iron oxide powder, the intensity ratio Int1 / Int2 of the diffraction intensities determined by X-ray diffraction analysis of the magnetic layer using an in-plane method is 1.0 or more and 6.5 or less; The Int1 is the maximum value of the diffraction intensity in the range where the diffraction angle 2θχ is 29.0° or more and 31.0° or less, The magnetic recording medium, wherein Int2 is the maximum value of the diffraction intensity in the range of the diffraction angle 2θχ of 36.3° or more and 37.5° or less.

2. 2. The magnetic recording medium according to claim 1, wherein the intensity ratio is equal to or greater than 1.5 and equal to or less than 6.

0.

3. 3. The magnetic recording medium according to claim 1, wherein the intensity ratio is equal to or greater than 3.0 and equal to or less than 5.

5.

4. 4. The magnetic recording medium according to claim 1, wherein the ε-iron oxide powder contains elemental cobalt.

5. 5. The magnetic recording medium according to claim 4, wherein the ε-iron oxide powder further contains an element selected from the group consisting of gallium and aluminum.

6. 6. The magnetic recording medium according to claim 4, wherein the ε-iron oxide powder further contains titanium element.

7. 7. The magnetic recording medium according to claim 1, further comprising a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer.

8. 8. The magnetic recording medium according to claim 1, further comprising a backcoat layer containing a nonmagnetic powder on the surface of the nonmagnetic support opposite to the surface having the magnetic layer.

9. 9. The magnetic recording medium according to claim 1, which is a magnetic tape.

10. A magnetic tape cartridge comprising the magnetic tape of claim 9.

11. A magnetic recording and reproducing device comprising the magnetic recording medium according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Ferrous oxide magnetic particle powder, method for manufacturing the same, coating material, and magnetic recording medium

    JP2016130208A

  • Magnetic particle and method of producing the same

    JP2018110168A

  • Magnetic recording medium, method for manufacturing epsilon-type iron oxide particles, and method for manufacturing magnetic recording medium

    JP2020140748A

  • Oriented body, method for manufacturing same, device for manufacturing same, and magnetic recording medium

    WO2017094752A1