Films for EUV lithography
The membrane assembly for EUV lithography, composed of silicon and transition metal layers, addresses space and contamination issues by enhancing emissivity and reducing attachment feature size, improving production efficiency and cost-effectiveness.
Patent Information
- Application Number
- JP2022195017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-04-06
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2036-12-02
AI Technical Summary
In EUV lithography, existing membrane assemblies for protecting patterning devices are bulky, require significant space for attachment features, and have low emissivity, leading to contamination issues that disrupt production and increase costs.
A membrane assembly for EUV lithography with a thickness of 200 nm or less, comprising a silicon layer and layers of silicon compounds, transition metal silicides, and capping layers made of ruthenium, along with anti-migration layers of molybdenum and titanium, to enhance emissivity and reduce contamination.
The membrane assembly reduces the space required for attachment features, enhances emissivity, and minimizes contamination, thereby reducing production disruptions and costs while maintaining high EUV transmission.
Smart Images

Figure 0007580439000005 
Figure 0007580439000006 
Figure 0007580439000007
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims priority to European Patent No. 15199845.7, filed December 14, 2015, and European Patent No. 16163962.0, filed April 6, 2016, which are incorporated herein by reference.
[0002] The present invention relates to membranes, patterning device assemblies, and dynamic gas lock assemblies for EUV lithography. [Background technology]
[0003]
[0003] A lithographic apparatus is a machine that applies a desired pattern onto a substrate, usually onto a target portion of the substrate. Lithographic apparatus can be used, for example, in the manufacture of integrated circuits (ICs). In such a case, a patterning device, alternatively called a mask or reticle, can be used to generate the circuit pattern to be formed on an individual layer of the IC. This pattern can be transferred onto a target portion (e.g. comprising part of, one, or several dies) on the substrate (e.g. a silicon wafer). Transfer of the pattern is typically by imaging onto a layer of radiation-sensitive material (resist) provided on the substrate. Generally, a single substrate will contain a network of adjacent target portions that are successively patterned.
[0004]
[0004] Lithography is widely recognized as one of the primary steps in manufacturing ICs and other devices and / or structures. However, as the dimensions of features produced using lithography become finer, lithography is becoming a more critical factor in enabling the manufacture of miniature ICs or other devices and / or structures.
[0005]
[0005] A theoretical estimate of the limit of pattern printing is given by the Rayleigh resolution criterion as shown in equation (1).
number
[0006]
[0006] To shorten the exposure wavelength and therefore the minimum printable size, it has been proposed to use extreme ultraviolet (EUV) radiation sources. EUV radiation is electromagnetic radiation having a wavelength in the range of 10-20 nm, for example in the range of 13-14 nm. It has also been proposed that EUV radiation having a wavelength less than 10 nm, for example in the range of 5-10 nm, such as 6.7 nm or 6.8 nm, may be used. Such radiation is called extreme ultraviolet radiation or soft x-ray radiation. Possible radiation sources include, for example, laser-produced plasma sources, discharge plasma sources, or radiation sources based on synchrotron radiation provided by electron storage rings.
[0007]
[0007] A lithographic apparatus includes a patterning device (e.g. a mask or a reticle). Radiation is provided through or reflected off the patterning device to form an image on a substrate. To protect the patterning device from airborne particles or other forms of contamination, a membrane assembly may be provided. A membrane assembly for protecting a patterning device is sometimes called a pellicle. Contamination on a surface of the patterning device may cause manufacturing defects for the substrate. The membrane assembly may comprise a boundary and a membrane extending transversely of the boundary.
[0008]
[0008] In use, the membrane needs to be fixed relative to the patterning device, for example by attachment features. It is desirable to reduce the amount of space taken up by the attachment features. It is also desirable for the membrane to have high emissivity and a low possibility of failing. Summary of the Invention
[0009]
[0009] According to one aspect of the present invention, there is provided a film for EUV lithography having a thickness of 200 nm or less and comprising a stack including at least one silicon layer and at least one silicon compound layer made of a compound of silicon and an element selected from the group consisting of boron, phosphorus, bromine, and sulfur.
[0010]
[0010] According to one aspect of the present invention, there is provided a film for EUV lithography having a thickness of 200 nm or less and comprising a stack including at least one silicon layer, at least one capping layer comprising ruthenium on an outer surface of the film, and at least one anti-migration layer adjacent to each capping layer comprising at least one of molybdenum and titanium.
[0011]
[0011] According to one aspect of the present invention, there is provided a film for EUV lithography having a thickness of 200 nm or less and comprising a stack including at least one silicon layer and / or at least one silicon compound layer made of a compound of silicon and an element selected from the group consisting of boron, phosphorus, bromine, and sulfur, at least one capping layer on an outer surface of the film, each capping layer comprising a material selected from the group consisting of transition metal silicide, transition metal boride, transition metal carbide, transition metal nitride, and transition metal oxide, and / or at least one transition metal layer between the capping layer and the silicon layer or silicon compound layer, each transition metal layer comprising a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, or W. [Brief description of the drawings]
[0012]
[0012] Embodiments of the present invention will now be described, by way of example only, with reference to the accompanying schematic drawings in which corresponding reference symbols indicate corresponding parts, in which:
[0013] [Figure 1] 1 depicts a lithographic apparatus according to an embodiment of the present invention; [Diagram 2]
[0014] 1 depicts a more detailed view of the lithographic apparatus; [Diagram 3]
[0015] 1 shows a schematic cross-sectional view of a portion of a membrane assembly according to one embodiment of the present invention; [Figure 4]
[0016] 1A-1D show schematic diagrams in plan view of steps for using a locking mechanism of a membrane assembly according to an embodiment of the invention; [Diagram 5]
[0016] Figure 1 shows a schematic plan view of steps for using a locking mechanism of a membrane assembly in accordance with one embodiment of the present invention; [Figure 6]
[0016] Figure 1 shows a schematic plan view of steps for using a locking mechanism of a membrane assembly in accordance with one embodiment of the present invention; [Figure 7]
[0017] 1 shows a schematic cross-sectional view of a membrane according to different embodiments of the present invention; [Figure 8]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. [Figure 9]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. [Figure 10]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. [Figure 11]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. [Figure 12]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. [Figure 13]
[0017] Membranes according to different embodiments of the present invention are illustrated diagrammatically in cross-section. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014]
[0018] 1 depicts a schematic diagram of a lithographic apparatus 100 including a source collector module SO according to an embodiment of the present invention. - an illumination system (or illuminator) IL configured to condition a radiation beam B (e.g. EUV radiation); - a support structure (e.g. mask table) MT configured to support a patterning device (e.g. mask or reticle) MA and connected to a first positioner PM configured to accurately position the patterning device; and - a substrate table (e.g. a wafer table) WT configured to hold a substrate (e.g. a resist-coated wafer) W and connected to a second positioner PW configured to accurately position the substrate; and - a projection system (e.g. a reflective projection system) PS configured to project a pattern imparted to a radiation beam B by a patterning device MA onto a target portion C (e.g. comprising one or more dies) of the substrate W.
[0015]
[0019] The illumination system IL may include various types of optical components, such as refractive, reflective, magnetic, electromagnetic, electrostatic or other types of optical components, or any combination thereof, for directing, shaping or controlling radiation.
[0016]
[0020] The support structure MT holds the patterning device MA in a manner that depends on the orientation of the patterning device, the design of the lithographic apparatus, and other conditions, such as whether or not the patterning device is held in a vacuum environment. The support structure MT may use mechanical, vacuum, electrostatic or other clamping techniques to hold the patterning device MA. The support structure MT may be for example a frame or a table, which may be fixed or movable as required. The support structure MT may ensure that the patterning device MA is at a desired position, for example with respect to the projection system PS.
[0017]
[0021] The term "patterning device", as used herein, should be interpreted broadly as referring to any device that can be used to impart a radiation beam B with a pattern in its cross-section to create a pattern in a target portion C of a substrate W. The pattern imparted to the radiation beam B may correspond to a particular functional layer in a device being created in the target portion C, such as an integrated circuit.
[0018]
[0022] The patterning device MA may be transmissive or reflective. Examples of patterning devices include masks, programmable mirror arrays, and programmable liquid crystal display (LCD) panels. Masks are well known in lithography, and include mask types such as binary, alternating phase-shift, and attenuated phase-shift, as well as various hybrid mask types. An example of a programmable mirror array employs a matrix arrangement of small mirrors, each of which can be individually tilted so as to reflect an incoming radiation beam in different directions. The tilted mirrors impart a pattern to the radiation beam which is reflected by the mirror matrix.
[0019]
[0023] Like the illumination system IL, the projection system PS may include various types of optical components, such as refractive, reflective, magnetic, electromagnetic, electrostatic, etc. optical components, or any combination thereof, as appropriate to the exposure radiation used, or other factors such as the use of a vacuum. It may be desirable to use a vacuum for EUV radiation, as other gases may be too absorbing of the radiation. Therefore, a vacuum environment may be provided throughout the beam path using a vacuum wall and vacuum pumps.
[0020]
[0024] As here depicted, lithographic apparatus 100 is of a reflective type (e.g., uses a reflective mask).
[0021]
[0025] Lithographic apparatus 100 may be of a type having two (dual stage) or more substrate tables WT (and / or two or more support structures MT). In such a "multi-stage" lithographic apparatus, the additional substrate tables WT (and / or the additional support structures MT) may be used in parallel, or preparatory steps may be performed on one or more substrate tables WT (and / or one or more support structures MT) while another one or more substrate tables WT (and / or one or more other support structures MT) are being used for exposure.
[0022]
[0026] Referring to FIG. 1, the illumination system IL receives a beam of extreme ultraviolet radiation from a source collector module SO. Methods for generating EUV light include, but are not necessarily limited to, converting a material having at least one element, such as xenon, lithium, or tin, and having one or more emission lines in the EUV range, into a plasma state. In one such method, often referred to as laser-produced plasma ("LPP"), a fuel, such as a droplet, stream, or cluster of a material having a desired line-emitting element, can be irradiated with a laser beam to generate the desired plasma. The source collector module SO can be part of an EUV radiation system that includes a laser (not shown in FIG. 1) for providing a laser beam to excite the fuel. The resulting plasma emits output radiation, such as EUV radiation, which is collected using a radiation collector located in the source collector module. For example, when a CO2 laser is used to provide the laser beam for fuel excitation, the laser and the source collector module SO can be separate components.
[0023]
[0027] In such a case, the laser is not considered to form part of lithographic apparatus 100, and the radiation beam B is delivered from the laser to the source collector module SO using a beam delivery system including, for example, suitable directing mirrors and / or beam expanders. In other cases the source may be an integral part of the source collector module SO, for example when the source is a discharge produced plasma EUV generator, often referred to as a DPP source.
[0024]
[0028] The illumination system IL may comprise an adjuster for adjusting the angular intensity distribution of the radiation beam. Typically, at least the outer and / or inner radial extent (commonly referred to as σ-outer and σ-inner, respectively) of the intensity distribution in a pupil plane of the illumination system IL may be adjusted. The illumination system IL may also include various other components, such as faceted field and pupil mirror devices. The illumination system IL may condition the radiation beam B to have a desired uniformity and intensity distribution across its cross-section.
[0025]
[0029] The radiation beam B is incident on a patterning device (e.g. mask) MA, held on a support structure (e.g. mask table) MT, and is patterned by the patterning device MA. After reflection from the patterning device (e.g. mask) MA, the radiation beam B passes through a projection system PS, which focuses the radiation beam B onto a target portion C of a substrate W. With the aid of a second positioner PW and a position sensor PS2 (e.g. an interferometer arrangement, a linear encoder or a capacitive sensor), the substrate table WT can be accurately moved, for example to position a different target portion C in the path of the radiation beam B. Similarly, the patterning device (e.g. mask) MA can be accurately positioned with respect to the path of the radiation beam B using a first positioner PM and another position sensor PS1. The patterning device (e.g. mask) MA and substrate W can be aligned using mask alignment marks M1, M2 and substrate alignment marks P1, P2.
[0026]
[0030] The controller 500 controls the overall operation of the lithographic apparatus 100, and in particular performs the operational processes described in detail below. The controller 500 may be implemented as a suitably programmed general-purpose computer including a central processing unit, volatile and non-volatile storage means, one or more input and output devices such as a keyboard and a screen, one or more network connections and one or more interfaces connected to various parts of the lithographic apparatus 100. It will be appreciated that a one-to-one relationship between the control of the computer and the control of the lithographic apparatus 100 is not necessary. In some embodiments of the invention, one computer may control multiple lithographic apparatuses 100. In some embodiments of the invention, multiple networked computers may be used to control one lithographic apparatus 100. The controller 500 may be configured to control one or more associated process devices and substrate handling devices in a lithocell or cluster of which the lithographic apparatus 100 forms a part. The controller 500 may be configured to be subordinate to a supervisory control system of the lithocell or cluster and / or to an overall control system of the fab.
[0027]
[0031] 2 shows lithographic apparatus 100 in more detail, including a source collector module SO, an illumination system IL, and a projection system PS. An EUV radiation emitting plasma 210 may be formed by a plasma source. The EUV radiation may be generated by a gas or vapor, for example Xe gas, Li vapor, or Sn vapor, in which the radiation emitting plasma 210 is generated to emit radiation in the EUV range of the electromagnetic spectrum. In an embodiment, a plasma of tin (Sn) is provided that is excited to generate EUV radiation.
[0028]
[0032] Radiation emitted by the radiation-emitting plasma 210 travels from the source chamber 211 to the collector chamber 212 .
[0029]
[0033] The collector chamber 212 may include a radiation collector CO. Radiation passing through the radiation collector CO may be focused at a virtual source point IF. The virtual source point IF is commonly referred to as an intermediate focus, and the source collector module SO is configured such that the virtual source point IF is located at or near an opening 221 in the enclosure structure 220. The virtual source point IF is an image of the radiation emitting plasma 210.
[0030]
[0034] The radiation then passes through an illumination system IL, which may include a faceted field mirror device 22 and a faceted pupil mirror device 24 arranged to provide a desired angular distribution of the unpatterned beam 21 at the patterning device MA, as well as a desired uniformity of the radiation intensity at the patterning device MA. Upon reflection of the unpatterned beam 21 off the patterning device MA, which is held by a support structure MT, a patterned beam 26 is formed, which is imaged by the projection system PS via reflective elements 28, 30 onto a substrate W held by a substrate table WT.
[0031]
[0035] In general, more elements than shown may be present in the illumination system IL and projection system PS. Further, there may be more mirrors than shown, for example, 1 to 6 more reflective elements may be present in the projection system PS than shown in FIG.
[0032]
[0036] Alternatively, the source collector module SO may be part of an LPP radiation system.
[0033]
[0037] As shown in Figure 1, in an embodiment, a lithographic apparatus 100 comprises an illumination system IL and a projection system PS. The illumination system IL is configured to emit a radiation beam B. The projection system PS is separated from a substrate table WT by an intervening space. The projection system PS is configured to project a pattern imposed in the radiation beam B onto a substrate W. The pattern is for EUV radiation in the radiation beam B.
[0034]
[0038] The intervening space between the projection system PS and the substrate table WT may be at least partially evacuated, the intervening space may be defined by a solid surface at the position of the projection system PS, through which the used radiation is directed towards the substrate table WT.
[0035]
[0039] In one embodiment, the lithographic apparatus 100 comprises a dynamic gas lock. The dynamic gas lock comprises a membrane assembly 80. In one embodiment, the dynamic gas lock comprises a hollow portion covered by the membrane assembly 80 positioned in an intervening space. The hollow portion is located around the radiation path. In one embodiment, the lithographic apparatus 100 comprises a gas blower configured to blow a gas flow inside the hollow portion. After passing through the membrane assembly, the radiation is incident on the substrate W.
[0036]
[0040] In one embodiment, the lithographic apparatus 100 comprises a membrane assembly 80. As mentioned above, in one embodiment, the membrane assembly 80 is for a dynamic gas lock. In this case, the membrane assembly 80 acts as a filter for filtering DUV radiation. Additionally or alternatively, in one embodiment, the membrane assembly 80 is a pellicle for a patterning device MA for EUV lithography. The membrane assembly 80 of the present invention may be used for a dynamic gas lock, or for a pellicle, or for another purpose such as a spectral purity filter. In one embodiment, the membrane assembly 80 comprises a membrane 40, which may also be referred to as a membrane stack. In one embodiment, the membrane is configured to transmit at least 80% of the incident EUV radiation.
[0037]
[0041] Conceptually, an EUV film stack consists of one or more material layers. These layers are deposited in a specific order to meet functional requirements resulting in an optimal film stack in terms of performance (over lifetime), reliability, and cost. Layers with specific functional requirements can be selected, for example, from a core material layer (i.e., the core layer of the film or film stack), a layer for thermal emission enhancement, an oxidation barrier layer, a corrosion barrier layer, and / or a processing etch stop layer. It is also possible for a single material layer to meet multiple functional requirements (e.g., corrosion barrier and emission enhancement in the case of a Ru layer).
[0038]
[0042] In an embodiment, membrane assembly 80 is configured to enclose the patterning device MA and protect it from airborne particles and other forms of contamination, which can lead to manufacturing defects on the substrate W. For example, in an embodiment, the pellicle is configured to reduce the likelihood of particles migrating into the stepping field of the patterning device MA of lithographic apparatus 100.
[0039]
[0043] If the patterning device MA is left unprotected, contamination may result in the need to clean or discard the patterning device MA. Cleaning the patterning device MA interrupts valuable production time, discarding the patterning device MA is costly, and replacing the patterning device MA also interrupts valuable production time.
[0040]
[0044] Figure 3 shows, in cross-section, a schematic representation of a portion of a membrane assembly 80 according to an embodiment of the present invention. The membrane assembly 80 is for EUV lithography. The membrane assembly 80 comprises a membrane 40. The membrane 40 is emissive to EUV radiation. Of course, the membrane 40 may not have 100% emissivity to EUV radiation. However, the membrane may have, for example, an emissivity of at least 50%. As shown in Figure 3, in an embodiment the membrane 40 is substantially planar. In an embodiment, the plane of the membrane 40 is substantially parallel to the plane of the patterning device MA.
[0041]
[0045] The membrane assembly 80 has a shape, such as a square, a circle, or a rectangle. The shape of the membrane assembly 80 is not particularly limited. The size of the membrane assembly 80 is not particularly limited. For example, in one embodiment, the diameter of the membrane assembly 80 is in the range of about 100 mm to about 500 mm, for example, about 200 mm.
[0042]
[0046] As shown in Fig. 3, in one embodiment, the membrane assembly 80 comprises a boundary 81. The boundary 81 is configured to hold the membrane 40. The boundary 81 provides mechanical stability to the membrane 40. The boundary 81 is configured to reduce the likelihood of the membrane 40 being deformed from its planar shape. In one embodiment, the membrane 40 is pre-tensioned during manufacture. The boundary 81 is configured to maintain tension in the membrane 40 so that the membrane 40 does not assume an undulating shape during use of the lithographic apparatus 100. In one embodiment, the boundary 81 extends along a periphery of the membrane 40. The outer periphery of the membrane 40 is positioned above the boundary 81 (according to the view of Fig. 3).
[0043]
[0047] The thickness of the border 81 is not particularly limited. For example, in one embodiment, the thickness of the border 81 is at least 300 μm, optionally at least 400 μm. In one embodiment, the thickness of the border 81 is at most 1,000 μm, optionally at most 800 μm. In one embodiment, the width of the border 81 is at least 1 mm, optionally at least 2 mm, optionally at least 4 mm. In one embodiment, the width of the border 81 is at most 10 mm, optionally at most 5 mm, optionally at most 4 mm.
[0044]
[0048] 3, in one embodiment, membrane assembly 80 includes frame assembly 50. Frame assembly 50 is connected to interface 81. In one embodiment, frame assembly 50 is initially manufactured as a separate component from interface 81 and then connected to interface 81. For example, the combination of membrane 40 and interface 81 may be manufactured together, while frame assembly 50 may be manufactured separately. In a subsequent manufacturing step, frame assembly 50 may be attached or secured to interface 81.
[0045]
[0049] In one embodiment, the width of frame assembly 50 is at least 2 mm, optionally at least 5 mm, optionally at least 8 mm. In one embodiment, the width of frame assembly 50 is at most 20 mm, optionally at most 10 mm, optionally at most 8 mm.
[0046]
[0050] In one embodiment, frame assembly 50 comprises frame 51. Frame 51 is the portion of frame assembly 50 that is connected to interface 81. In one embodiment, frame 51 is made of the same material as interface 81. For example, in one embodiment, interface 81 and frame 51 are both made of a material that includes silicon. In one embodiment, interface 81 is made of silicon. In one embodiment, frame 51 is made of silicon. In one embodiment, the thermal expansion of interface 81 is substantially matched to the thermal expansion of frame 51. In one embodiment, frame 51 is attached to interface 81 by an adhesive. In one embodiment, the thermal expansion of the adhesive is substantially matched to the thermal expansion of frame 51 and / or interface 81.
[0047]
[0051] 3, a frame assembly 50 is configured to attach to a patterning device MA. The frame assembly 50 is for maintaining the position of the membrane 40 relative to the patterning device MA. Although this embodiment is described with reference to a patterning device MA, the invention is equally applicable to a membrane assembly 80 that connects to a component different from the patterning device MA.
[0048]
[0052] In one embodiment, the frame assembly 50 is connected to the boundary 81 in a direction perpendicular to the plane of the membrane 40. This is shown in FIG. 3. In FIG. 3, the plane of the membrane 40 extends from left to right, from in to out of the plane of the paper. The direction perpendicular to the plane of the membrane 40 corresponds to the vertical (i.e., up and down) direction in FIG. 3. The frame assembly 50 is connected directly below the boundary 81. In FIG. 3, the boundary 81 and the frame assembly 50 are aligned vertically. In one embodiment, the interface between the boundary 81 and the frame assembly 50 lies in a plane that is substantially parallel to the plane of the membrane 40.
[0049]
[0053] In one embodiment, the membrane assembly 80 is configured to be detachable from the patterning device MA. This allows intermediate inspection of the patterning device MA to be performed. In one embodiment, the frame assembly 50 is configured to be repeatedly attached and detached from the patterning device MA.
[0050]
[0054] In use, frame assembly 50 is between boundary 81 and the patterning device MA. This arrangement differs from an arrangement in which the frame assembly is positioned radially outward of the boundary. It is anticipated that one embodiment of the present invention will achieve a reduction in the space around membrane 40 that is required to hold membrane 40 in the proper position relative to the patterning device MA.
[0051]
[0055] The membrane assembly according to the comparative example has a frame assembly radially outward of the boundary that requires radial access to attach / detach the frame assembly to / from the patterning device. A space of about 16 mm may be required to accommodate the boundary, the frame assembly, and space to access the frame assembly.
[0052]
[0056] In contrast, in one embodiment, frame assembly 50 is positioned directly below boundary 81, thereby reducing the radial space required to accommodate boundary 81 and frame assembly 50. For example, in one embodiment, the radial space required to accommodate boundary 81, frame assembly 50, and space to access frame assembly 50 is approximately 12 mm.
[0053]
[0057] It is anticipated that one embodiment of the present invention will reduce the space required for attachment features in the region of the patterning device MA. Attachment features are features used to attach the membrane assembly 80 to the patterning device MA. In one embodiment, attachment features are provided between the boundary 81 and the patterning device MA. This is shown in Figure 3 and described in more detail below.
[0054]
[0058] In one embodiment, frame assembly 50 includes at least one hole 52. In one embodiment, hole 52 is a cavity or chamber in frame 51 of frame assembly 50. Hole 52 is configured to receive a stud 60. Stud 60 protrudes from patterning device MA.
[0055]
[0059] 3 shows studs 60 secured to the patterning device MA. In one embodiment, the studs 60 are affixed to the patterning device MA using an adhesive. Alternatively, the studs 60 could be integrally formed with the patterning device MA. As a further alternative, the studs 60 could be initially manufactured as a separate component from the patterning device MA and then secured to the patterning device MA using means other than an adhesive, such as screws.
[0056]
[0060] The studs 60 and holes 52 are attachment features. In one embodiment, the studs 60 and holes 52 are provided between the boundary 81 and the patterning device MA. This differs from previously known arrangements in which the attachment features are positioned radially outward of the boundary 81.
[0057]
[0061] As shown in Figure 3, in one embodiment, hole 52 at least partially overlaps boundary 81 when viewed in a direction perpendicular to the plane of membrane 40. This is shown in Figure 3, where hole 52 partially overlaps boundary 81 when viewed vertically. Looking at Figure 3, a vertical line can be drawn that extends through both boundary 81 and hole 52.
[0058]
[0062] In one embodiment, the frame assembly 50 includes a locking mechanism 55. The locking mechanism 55 is configured to lock the frame assembly 50 to the studs 60. In one embodiment, the locking mechanism 55 includes a resilient member 53. In one embodiment, the locking mechanism 55 includes a resilient member 53 for each hole 52. In one embodiment, the frame assembly 50 includes a plurality of holes 52, e.g., two, three, four, or more holes 52. A resilient member 53 is provided corresponding to each hole 52.
[0059]
[0063] As shown in Figure 3, in one embodiment, the resilient member 53 comprises a spring. For example, the spring may be a coil spring or a leaf spring. In an alternative embodiment, the resilient member 53 comprises an elastic member such as rubber. In an alternative embodiment, the resilient member 53 comprises a flexure. The flexure may be machined using, for example, an electro-discharge machining process.
[0060]
[0064] Figures 4 to 6 show diagrammatically the stages of use of the locking mechanism 55. Figures 4 to 6 are shown in plan view. Figure 4 shows an initial state in which the frame assembly 50 is positioned on the stud 60 to receive the stud 60 in the hole 52. As shown in Figure 4, the resilient member 53 extends into the hole 52. The stud 60 can therefore contact the resilient member 53 when received in the hole 52. The resilient member 53 is configured to be compressible when the stud 60 received in the hole 52 presses the resilient member 53 in a direction in the plane of the membrane 40. For example, in Figure 4, the stud 60 can press the resilient member 53 to the right of the figure.
[0061]
[0065] As shown in Figures 3-6, in one embodiment, the locking mechanism 55 includes a locking member 54 for each hole 52. The locking members 54 are configured to be movable to a locked position in which the locking members 54 extend into the holes 52. In the locked position, the compressed resilient members 53 exert a force against the stud 60 received in the holes 52, toward the locking members 54. This is shown in the sequence of Figures 4-6.
[0062]
[0066] As shown in the transition from Figure 4 to Figure 5, the stud 60 and the frame assembly 50 move relative to one another such that the stud 60 presses against the resilient member 53. As shown in Figure 5, the stud 60 compresses the resilient member 53.
[0063]
[0067] As shown in the transition from Figure 5 to Figure 6, the locking member 54 moves to a locked position in which the locking member 54 extends into the aperture 52. For example, as shown in Figures 4-6, in one embodiment, the frame assembly 50 includes at least one locking aperture 56. The locking member 54 passes through the locking aperture 56.
[0064]
[0068] Figure 6 shows the locking member 54 in the locked position. The resilient member 53 exerts a force against the stud 60 in the direction of the locking member 54. In the situation shown in Figure 5, an external force must be applied to the frame assembly 50 and / or the stud 60 in order for the stud 60 to compress the resilient member 53. Once the locking member 54 is in the locked position (e.g., as shown in Figure 6), no external force is required because the locking member 54 holds the stud 60 and the frame assembly 50 in the proper position relative to each other.
[0065]
[0069] As mentioned above, the studs 60 are positioned below the boundary 81, rather than radially outside of it. This may require an increase in the distance (also known as the standoff) between the patterning device MA and the membrane 40. The distance between the surface of the patterning device MA and the membrane 40 corresponds substantially to the combined height of the frame assembly 50 and boundary 81. In one embodiment, the combined height of the frame assembly 50 and boundary 81 is at least 1 mm, at least 2 mm, optionally at least 5 mm. In one embodiment, the combined height of the frame assembly 50 and boundary 81 is at most 20 mm, optionally at most 10 mm, optionally at most 5 mm.
[0066]
[0070] In one embodiment, the resilient member 53 includes a spring made of a material such as stainless steel. In one embodiment, the resilient member 53 is connected to a contact pad 57 made of a different material than the resilient member 53. For example, the contact pad 57 can be made of the same material as the stud 60 and / or the locking member 54. In one embodiment, the contact pad 57 includes titanium. In one embodiment, the locking member 54 includes titanium. In one embodiment, the stud 60 includes titanium. Titanium is known to provide a ductile contact. However, in alternative embodiments, other materials can be used for the contact pad 57, the stud 60, and the locking member 54.
[0067]
[0071] As shown in Figures 4-6, in one embodiment, the cross-sectional area of the hole 52 in plan view is larger than the cross-sectional area of the stud 60. The hole 52 is oversized relative to the stud 60. In one embodiment, a resilient member 53 is provided for an end stop (not shown). The resilient member 53 protrudes into the hole 52 when viewed in plan view (as shown in Figure 4). Thus, the resilient member 53 effectively reduces the cross-sectional area of the hole 52 in plan view. The remaining cross-sectional dimension of the hole 52 is larger than the dimension of the stud 60. Thus, when the frame assembly 50 is moved vertically on the stud 60, the stud 60 can be received within the hole 52. The frame assembly 50 is pushed laterally against the resilient member 53, causing the resilient member 53 to deflect inward. A locking member 54 is positioned to prevent the frame assembly 50 from bending backwards. In one embodiment, the locking member 54 is a pin. The locking member 54 can be inserted from the side or from the top. After inserting the locking member 54, the frame assembly 50 is locked to the patterning device MA.
[0068]
[0072] In one embodiment, the frame assembly 50 includes four holes 52 evenly distributed around the circumference of the frame assembly 50. In one embodiment, the frame assembly 50 has a shape similar to the boundary 81 and follows the circumference of the membrane 40. FIG. 3 shows the elastic members 53 radially inward of the holes 52. However, this is not necessarily the case. The elastic members 53 may be radially outward of the holes 52, or may not be radially inward or outward relative to the holes 52. The holes 52 are positioned between the elastic members 53 and the locking members 54.
[0069]
[0073] In one embodiment, a resilient member 53 is radially inward of the holes 52 on one side of the membrane assembly 80, while another resilient member 53 is radially outward of another hole 52 on the opposite side of the membrane assembly 80. This allows the studs 60 on either side of the patterning device MA to compress both resilient members 52 with a single movement of the membrane assembly 80 relative to the patterning device MA. In one embodiment, the membrane assembly 80 is configured such that all of the studs 60 received in corresponding holes 52 compress the corresponding resilient members 52 with a single movement of the membrane assembly 80 relative to the patterning device MA.
[0070]
[0074] 4-6, in one embodiment, the locking member 54 is provided as a loose part. In an alternative embodiment, the locking member 54 can be integral with the remainder of the frame assembly 50, provided that the locking member 54 can be slid into the locked position.
[0071]
[0075] In one embodiment, the diameter (in plan view) of stud 60 is at least 1 mm, optionally at least 2 mm, optionally at least 3 mm. In one embodiment, the diameter of stud 60 is at most 10 mm, optionally at most 5 mm, optionally at most 3 mm.
[0072]
[0076] As noted above, in one embodiment, elastic member 53 extends into hole 52 when uncompressed. In one embodiment, the distance that elastic member 53 extends into hole 52 is at least 0.1 mm, optionally at least 0.2 mm, and optionally at least 0.5 mm. In one embodiment, the distance that elastic member 53 extends into hole 52 is at most 2 mm, optionally at most 1 mm, and optionally at most 0.5 mm.
[0073]
[0077] As mentioned above, the diameter of hole 52 is larger than the diameter of stud 60. In one embodiment, the diameter of hole 52 is at least 0.2 mm, optionally at least 0.5 mm, optionally at least 1 mm larger than the diameter of stud 60. In one embodiment, the diameter of hole 52 is at most 5 mm, optionally at most 2 mm, optionally at most 1 mm larger than the diameter of stud 60. In one embodiment, the length of locking member 54 is at least 1 mm, optionally at least 2 mm, optionally at least 4 mm.
[0074]
[0078] In one embodiment, the length of locking member 54 is at most 10 mm, optionally at most 5 mm, optionally at most 4 mm. In one embodiment, the width of locking member 54 is at least 0.2 mm, optionally at least 0.5 mm, optionally at least 1 mm. In one embodiment, the width of locking member 54 is at most 5 mm, optionally at most 2 mm, optionally at most 1 mm.
[0075]
[0079] It is anticipated that one embodiment of the present invention will achieve a reduction in the tooling steps required for attaching / detaching the membrane assembly 80 to / from the patterning device MA.
[0076]
[0080] Figure 7 shows a schematic cross-sectional view of a membrane 40 according to one embodiment of the present invention. As shown in Figure 7, the membrane 40 comprises a stack. The stack comprises a number of layers.
[0077]
[0081] In one embodiment, the stack includes at least one silicon layer 41. The silicon layer 41 includes a form of silicon. In one embodiment, the stack includes at least one silicon compound layer 43. The silicon compound layer 43 is made of a compound of silicon and another element selected from the group consisting of boron, phosphorus, bromine, and sulfur. However, other elements can be used. Specifically, in one embodiment, the element that combines with silicon to form the silicon compound layer 43 is any element that can be used as a dopant material for doping the silicon layer 41. This embodiment is described using boron as the element that combines with silicon for convenience only. This embodiment is not limited to the element being boron.
[0078]
[0082] In one embodiment, silicon compound layer 43 comprises silicon boride, which has the chemical formula SiB x where x can be 3, 4, 6, 14, 15, 40, etc. Silicon boride has metallic properties. Specifically, silicon compound layer 43 has metallic properties that increase the emissivity of film 40 to EUV radiation. It is estimated that a film made of only silicon layer 41 would have a low emissivity, perhaps around 3%. If a metal or compound with metallic properties is added to film 40, the emissivity increases dramatically.
[0079]
[0083] Metals have been found to limit the practical thickness of the film due to EUV absorption. By providing a silicon film layer 43, it is expected that one embodiment of the present invention will achieve an increase in the possible thickness of the film 40 that has sufficient emissivity for use in lithographic apparatus 100.
[0080]
[0084] 7, in one embodiment, silicon compound layer 43 is formed as an intermediate layer between silicon layer 41 and non-metallic layer 42 that includes an element that combines with silicon to form silicon compound layer 43. For example, in one embodiment, non-metallic layer 42 includes boron. In one embodiment, the boron is provided in the form of boron carbide. However, alternative forms of boron may be used.
[0081]
[0085] In one embodiment, silicon layer 41 is initially provided adjacent to non-metal layer 42. Boron in non-metal layer 42 locally dopes silicon in silicon layer 41. The boron dopes the silicon to an extent that silicon boride is produced forming silicon compound layer 43. The boron dopes the silicon such that there are more boron atoms than silicon atoms in the doped silicon, i.e., forming silicon boride.
[0082]
[0086] In one embodiment, the silicon layer 41 and the non-metallic layer 42 are provided as multiple layers. Locally, the membrane 40 can be strengthened with boron silicide (by lamination effect and by radiation hardening of boron in silicon) to enable the membrane 40 to withstand high temperatures.
[0083]
[0087] As shown in FIG. 7, in one embodiment the stack includes a plurality of silicon layers 41, a plurality of non-metal layers 42, and a silicon compound layer 43 between each pair of silicon layers 41 and non-metal layers 42.
[0084]
[0088] 7, in one embodiment, the stack includes layers in the following order: non-metal layer 42, silicon compound layer 43, silicon layer 41, silicon compound layer 43, non-metal layer 42, silicon compound layer 43, silicon layer 41, silicon compound layer 43, non-metal layer 42, silicon compound layer 43, silicon layer 41, silicon compound layer 43, and non-metal layer 42. This is a multi-layer stack. In one embodiment, the stack includes a non-metal layer 42, then a repeating set of four layers including silicon compound layer 43, silicon layer 41, silicon compound layer 43, and non-metal layer 42.
[0085]
[0089] In one embodiment, the thickness of each non-metallic layer 42 is at least 0.5 nm, optionally at least 1 nm, optionally at least 2 nm. In one embodiment, the thickness of each non-metallic layer 42 is at most 10 nm, optionally at most 5 nm, optionally at most 2 nm.
[0086]
[0090] In one embodiment, the thickness of each silicon compound layer 43 is at least 0.5 nm, optionally at least 1 nm, optionally at least 2 nm. In one embodiment, the thickness of each silicon compound layer 43 is at most 10 nm, optionally at most 5 nm, optionally at most 2 nm.
[0087]
[0091] In one embodiment, the thickness of each silicon layer 41 is at least 2 nm, optionally at least 5 nm, optionally at least 8 nm. In one embodiment, the thickness of each silicon layer 51 is at most 20 nm, optionally at most 10 nm, optionally at most 8 nm.
[0088]
[0092] The embodiment shown in FIG. 7, which includes an 8 nm thick silicon layer 41, a 2 nm thick non-metallic layer 42, and a 2 nm thick silicon compound layer 43, is expected to achieve approximately 90% emissivity to EUV radiation.
[0089]
[0093] FIG. 8 shows an alternative embodiment in which the stack includes layers in the following order: non-metal layer 42, silicon compound layer 43, silicon layer 41, silicon compound layer 43, and non-metal layer 42.
[0090]
[0094] As shown in Figure 8, in one embodiment, the film 40 includes only one silicon layer 41. In such an embodiment, the silicon layer 41 may have a thickness of at least 10 nm, optionally at least 20 nm, optionally at least 38 nm. In one embodiment, the single silicon layer 41 has a thickness of at most 100 nm, optionally at most 50 nm, optionally at most 38 nm. The embodiment shown in Figure 8, having a 38 nm thick silicon layer 41, a 4 nm thick non-metallic layer 42, and a 2 nm thick silicon compound layer 43, is expected to achieve about 90% emissivity for EUV radiation.
[0091]
[0095] In one embodiment, the total thickness of the silicon compound layers in the stack is up to about 20 nm. If the total thickness is not too large, the metals and compounds with metallic properties improve the emissivity of the film 40. If the layers of metals or compounds with metallic properties are too thick, the emissivity may decrease.
[0092]
[0096] FIG. 9 shows a schematic representation of an alternative embodiment of the membrane 40. As shown in FIG. 9, in one embodiment, the stack comprises at least one silicon layer 41, at least one capping layer 46, and at least one anti-migration layer 47. In one embodiment, the capping layer 46 comprises ruthenium. The capping layer 46 is disposed on an outer surface of the membrane 40. The anti-migration layer 47 comprises at least one of molybdenum and titanium. An anti-migration layer 47 is adjacent to each capping layer 46.
[0093]
[0097] The ruthenium-containing capping layer 46 increases the emissivity of the film 40. The capping layer 46 reduces the likelihood of oxidation of the film 40. The capping layer 46 is configured to protect the film 40 from hydrogen gas.
[0094]
[0098] During use of the lithographic apparatus 100, the film 40 may heat up as it absorbs radiation. As the capping layer 46 heats up, the material of the capping layer 46 (e.g., ruthenium) may migrate. Migration is the transport of material caused by the gradual movement of ions within the capping layer 46. When material begins to migrate, it may form islands within the capping layer 46. When material begins to migrate, the capping layer 46 becomes less effective at reducing oxidation, protecting against hydrogen gas, and increasing emissivity. Thus, during use of the lithographic apparatus 100, the film 40 may begin to oxidize and its emissivity may decrease.
[0095]
[0099] By providing the anti-migration layer 47, migration of the capping layer 46 is reduced. Molybdenum and titanium are metals with relatively high melting points and good emissivity to UV radiation. Titanium and molybdenum do not migrate as much as ruthenium when heated. Titanium and molybdenum have good metal-to-metal contact to ruthenium. By providing the anti-migration layer 47 adjacent to the capping layer 46, migration of the capping layer 46 is reduced. As a result, the good properties of the capping layer 46 are maintained even at high temperatures, even if the capping layer 46 heats up during use of the lithographic apparatus 100.
[0096]
[0100] 9, in one embodiment, the stack includes layers in the following order: a capping layer 46 comprising ruthenium on an outer surface of membrane 40, an anti-migration layer 47 comprising at least one of molybdenum and titanium, a silicon layer 41, an anti-migration layer 47 comprising at least one of molybdenum and titanium, and a capping layer 46 comprising ruthenium on the other outer surface of membrane 40. In one embodiment, a capping layer 46 comprising ruthenium is provided on both outer surfaces of membrane 40.
[0097]
[0101] FIG. 10 shows an alternative embodiment of a membrane that combines the idea of using a silicon compound layer 43 with the use of an anti-migration layer 47 .
[0098]
[0102] 10, in one embodiment, the stack includes layers in the following order: a capping layer 46 comprising ruthenium on the outer surface of membrane 40, an anti-migration layer 47 comprising at least one of molybdenum and titanium, a silicon layer 41, a silicon compound layer 43, and a non-metal layer 42.
[0099]
[0103] During fabrication of membrane assembly 80, the boron carbide layer can chemically protect silicon layer 41 from etching processes. In one embodiment, membrane 40 includes a periodic structure. In one embodiment, the period is not set equal to 6.6 nm or 6.7 nm. If the period is at or close to 6.7 nm, the membrane can act as a mirror for EUV radiation.
[0100]
[0104] Silicon may crystallize in a diamond cubic crystal structure. In one embodiment, boundary 81 comprises a cubic crystal of silicon. In one embodiment, boundary 81 comprises <100> It has a crystallographic direction.
[0101]
[0105] In one embodiment, the silicon layer 41 is made of polycrystalline or nanocrystalline silicon. Polycrystalline or nanocrystalline silicon has brittle properties. Therefore, a membrane 40 with a silicon layer 41 made of polycrystalline or nanocrystalline silicon may break into many particles if the membrane assembly 80 is broken. One embodiment of the present invention is expected to achieve improved mechanical properties of the membrane assembly 80.
[0102]
[0106] Polycrystalline silicon and nanocrystalline silicon each have high transparency to EUV radiation. Polycrystalline silicon and nanocrystalline silicon each have good mechanical strength.
[0103]
[0107] However, it is not essential that the silicon layer 41 film be formed from polycrystalline or nanocrystalline silicon, for example in alternative embodiments, the silicon layer 41 is formed from a multi-lattice membrane or silicon nitride.
[0104]
[0108] In another alternative embodiment, the silicon layer 41 is formed from monocrystalline silicon. In such an embodiment, the monocrystalline silicon film can be formed by silicon on insulator (SOI) techniques. The starting material for this product is a so-called SOI substrate. The SOI substrate is a substrate that includes a silicon carrier substrate with a thin monocrystalline silicon layer on top of a buried insulating SiO2 layer. In one embodiment, the thickness of the monocrystalline silicon layer can range from about 5 nm to about 5 μm. In one embodiment, the silicon layer 41 is present on the SOI substrate before the SOI substrate is used in the manufacturing method.
[0105]
[0109] In one embodiment, silicon layer 41 includes silicon in one of the allotropic forms, such as amorphous silicon, monocrystalline silicon, polycrystalline silicon, or nanocrystalline silicon. Nanocrystalline silicon refers to a polycrystalline silicon matrix with a certain amorphous silicon content. In one embodiment, polycrystalline or nanocrystalline silicon is formed by crystallizing amorphous silicon in silicon layer 41. For example, in one embodiment, silicon layer 41 is added to the stack as an amorphous silicon layer. Above a certain temperature, the amorphous silicon layer crystallizes into a polycrystalline layer or a nanocrystalline silicon layer. For example, silicon layer 41 as an amorphous silicon layer changes into silicon layer 41 as a polycrystalline layer or a nanocrystalline silicon layer.
[0106]
[0110] In one embodiment, the amorphous silicon layer is doped in situ during growth. In one embodiment, the amorphous silicon layer is doped after growth. By adding p-type or n-type dopants, the silicon conductivity is increased, which has a positive effect on the thermo-mechanical behavior due to the power of the EUV radiation source.
[0107]
[0111] In one embodiment, film 40 is thin enough that it has a high enough transmission to EUV radiation, for example greater than 50%. In one embodiment, film 40 has a thickness of at most about 200 nm, optionally at most about 150 nm. A 150 nm Si film transmits about 77% of the incident EUV radiation. In one embodiment, film 40 has a thickness of at most about 100 nm. A 100 nm Si film transmits about 84% of the incident EUV radiation. A 60 nm Si film transmits about 90% of the incident EUV radiation.
[0108]
[0112] In one embodiment, membrane 40 is thick enough to be mechanically stable when membrane assembly 80 is secured to a patterning device MA of lithographic apparatus 100 and during use of lithographic apparatus 100. In one embodiment, membrane 40 has a thickness of at least about 10 nm, optionally at least about 20 nm, optionally at least about 35 nm. In one embodiment, membrane 40 has a thickness of about 55 nm.
[0109]
[0113] 11 to 13 show, in cross-sectional view, schematic representations of different embodiments of a membrane 40 according to the invention. When designing the membrane 40, there is a trade-off between the thickness of the membrane 40, its stability, and its robustness.
[0110]
[0114] As shown in FIG. 11, in one embodiment, the membrane 40 comprises a silicon layer 41 sandwiched between two capping layers 46. In one embodiment, the silicon layer 41 comprises polysilicon. In one embodiment, the two capping layers 46 are made of the same (capping) material. However, this is not necessarily the case. In alternative embodiments, the material used for one of the capping layers 46 is different from the material used for the other of the capping layers 46.
[0111]
[0115] In one embodiment, capping layer 46 is on the outer surface of membrane 40. Thus, in one embodiment, the stack includes layers in the following order: capping layer 46 on the outer surface of membrane 40, silicon layer 41, and capping layer 36 comprising a silicide of a transition metal.
[0112]
[0116] In one embodiment, the capping layer 46 comprises a silicide of a transition metal, such as, but not limited to, Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, or W.
[0113]
[0117] Transition metal silicides transmit a very high percentage of EUV radiation. It is desirable for the transmission of film 40 to EUV radiation to be as high as possible. In one embodiment, the materials of the stack are selected to have an extinction coefficient k of less than 0.0175 for EUV radiation having a wavelength of 13.5 nm.
[0114]
[0118] The extinction coefficient k is related to EUV transmission. When EUV radiation passes through a medium, some of the EUV radiation is attenuated. This is conveniently called the complex refractive index
number
[0115]
[0119] Here, the real part of the complex refractive index, n, is the refractive index and indicates the phase velocity. The extinction coefficient, k, is the imaginary part of the complex refractive index. The extinction coefficient, k, indicates the amount of attenuation when an electromagnetic wave propagates through a material.
[0116]
[0120] In the above description, the value of the extinction coefficient k is given for radiation with a wavelength of 13.5 nm. Using this value and a given material thickness, it is possible to calculate the EUV transmission / absorption of a layer within film 40. For a layer of material with a particular value of extinction coefficient k=0.0175, a 4 nm thick layer will absorb 6% of the EUV radiation (i.e., a 6% EUV transmission loss).
[0117]
[0121] It is not necessary for capping layer 46 to comprise a transition metal silicide. In alternative embodiments, one or both of capping layers 46 comprises a transition metal boride, a transition metal carbide, a transition metal nitride, a transition metal oxide, or a pure form of the transition metal.
[0118]
[0122] Table 1 lists, for selected suitable capping layer materials, values of melting point, coefficient of thermal expansion (CTE), film resistivity, EUV radiation transmission, capping layer thickness d (in nm) corresponding to 6% EUV transmission loss, real part n of the complex refractive index for radiation having a wavelength of 13.5 nm, and extinction coefficient k for radiation having a wavelength of 13.5 nm, in order of decreasing EUV transmission value.
[0119]
[0123] Examples of suitable capping layer materials are (in decreasing order of EUV transmission value from 99.8% to 94.6%): Si, Y, YSi2, LaSi2, ZrSi2, SiB4, B, Zr, YB6, NbSi3, MoSi2, YC2, SiC, ZrB2, La, CeSi2, B4C, Nb, CeB6, LaB6, NbB2, ZrC, Ce, Mo, CeC2, YN, LaC2, MoB, LaN, C, Mo2C, NbC, TiSi2, Ru2Si3, Si3N6, BN, ZrN , VSi2, CeN, RuB2, NbN, SiO2, Y2O3, MoN, TiB2, La2O3, Nb2O5, WSi2, Ti, ZrO2, B2O3, MoO3, TiC, RuC, SiCr, Ru, WB2, VB2, TaSi2 , CeO2, TiN, RuN, RuO2, TiO3, VC, V, TaB2, VN, WC, CrB, TiW, CrN, W, HfO2, Cr3C2, WN, TaC, Ta2O5, TaN, Cr, Al2O3, Ta, and Pt.
[0120]
[0124] Suitable capping layer materials that may provide an optimal combination of melting point, resistivity, EUV transmission, refractive index n, and extinction coefficient k are, for example, CeB6, LaB6, NbSi3, Zr, YSi2, CeSi2, Y, CeC2, LaC2, LaSi2, ZrB2, Nb, LaN, YC2, ZrSi2, SiB4, B, YB6, MoSi2, YC2, SiC, La, B4C, Ce, CeN, Ru2Si3, YN, ZrC, NbB2, NbC, Mo2C, MoB, and Mo. [Table 1]
[0121]
[0125] Transition metal silicides transmit a higher percentage of EUV radiation than transition metal borides, transition metal carbides, transition metal nitrides, transition metal oxides, or the transition metals in pure form.
[0122]
[0126] In terms of EUV transmission properties, possible materials for film 40 are ranked as follows, from most to least transparent to EUV radiation: transition metal silicides, transition metal borides, pure transition metals, transition metal carbides, transition metal nitrides, and transition metal oxides. Depending on the transition metal, pure transition metals may be superior to transition metal borides. Depending on the transition metal, transition metal carbides may be superior to pure transition metals. An example of a transition metal carbide is molybdenum carbide.
[0123]
[0127] Moreover, transition metal suicides have particularly desirable EUV reflective properties. It is desirable for the EUV reflectance (i.e., the percentage of EUV radiation that is reflected by the surface of film 40) to be as low as possible. Transition metal suicides reflect EUV radiation at a lower rate than transition metal oxides, transition metal borides, transition metal carbides, transition metal nitrides, or pure forms of the transition metals.
[0124]
[0128] In one embodiment, the materials of the stack of films 40 are selected such that the index of refraction of the stack for EUV radiation having a wavelength of 13.5 nm is greater than 0.95. An index of refraction close to 1 limits EUV reflection at the interfaces of film 40.
[0125]
[0129] In terms of EUV reflective properties, possible materials for film 40 are ranked as follows, from least to most reflective of EUV radiation: transition metal silicides, transition metal oxides, pure transition metals, transition metal borides, transition metal carbides, and transition metal nitrides. However, there is no significant difference in EUV radiation properties between transition metal oxides, pure transition metals, transition metal borides, and transition metal carbides.
[0126]
[0130] It is desirable for the film 40 to have a low resistance, and in particular for the capping layer 46 to have a low resistance, since conductive coatings can increase the resistance of the film 40. Transition metal silicides have a lower resistance than transition metal carbides, transition metal nitrides, or transition metal oxides.
[0127]
[0131] In one embodiment, the material of the capping layer 46 is such that the resistance of the capping layer 46 is 10 -3 It is selected to be less than Ωm.
[0128]
[0132] In terms of resistivity, possible materials for film 40 are ranked as follows, from lowest to highest resistivity: pure transition metals, transition metal borides, transition metal silicides, transition metal carbides, transition metal nitrides, transition metal oxides.
[0129]
[0133] During use, membrane 40 may reach operating temperatures of up to about 600° C. It is therefore desirable for the materials used in the stack of membrane 40 to have high melting points. In one embodiment, the materials in the stack are selected to have a melting point greater than 1200° C.
[0130]
[0134] In terms of melting point, possible materials for film 40 are ranked from highest melting point to lowest: transition metal carbides, transition metal borides, transition metal nitrides, pure transition metals, transition metal oxides, and transition metal silicides. Depending on the transition metal, transition metal borides may have a higher melting point than transition metal carbides. Depending on the transition metal, transition metal oxides may have a higher melting point than pure transition metals.
[0131]
[0135] In one embodiment, the materials of the layers other than the silicon layer 41 are selected to have a thermal expansion coefficient close to that of the silicon layer 41. The thermal expansion coefficient of the silicon layer 41 is approximately 2.6×10 -6 The thermal expansion coefficient may be in the range of m / mK. Matching the thermal expansion coefficient to that of the silicon layer 41 in the core of the membrane 40 reduces the likelihood of thermo-mechanical failure of the membrane 40. In one embodiment, the materials of the stack have a thermal expansion coefficient of about 2×10 -6 m / mK to about 6×10 -6 The temperature is selected to be in the range of m / mK.
[0132]
[0136] The ranking of possible materials for membrane 40 in terms of their coefficient of thermal expansion depends heavily on the particular compound.
[0133]
[0137] As shown in FIG. 12, in one embodiment, a transition metal layer 48 is provided between the silicon layer 41 and one of the capping layers 46. The transition metal layer 48 includes a transition metal. For example, the transition metal may be Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, or W. In one embodiment, the transition metal of the transition metal layer 48 is provided in a pure form (i.e., not a suicide, boride, carbide, nitride, or oxide of the transition metal). Thus, in one embodiment, the stack of the film 40 includes, in order, the capping layer 46, the transition metal layer 48, the silicon layer, and the capping layer 46.
[0134]
[0138] In one embodiment, capping layer 46 includes a boride, carbide (e.g., molybdenum carbide), nitride, or oxide of a transition metal. The transition metal of transition metal layer 48 can be the same as the transition metal capping layer 46. In an alternative embodiment, the transition metal of transition metal layer 48 is different from the transition metal used in capping layer 46.
[0135]
[0139] 13, in one embodiment, a transition metal layer 48 is provided on either side of the silicon layer 41. A transition metal layer 48 is provided between each of the silicon layer 41 and the capping layer 46. Thus, in one embodiment, the stack of film 40 includes, in order, capping layer 46, transition metal layer 48, silicon layer, transition metal layer 48, and capping layer 46.
[0136]
[0140] When selecting which material to use for film 40, there are tradeoffs between the properties identified above, namely EUV transmission, EUV reflectance, melting point, coefficient of thermal expansion, and resistivity.
[0137]
[0141] A ranking of possible stacks for film 40 based on capping layer 46 using the criteria identified above can be summarized in Table 2. 1 indicates the best ranking, 2 indicates the next best ranking, etc. If different stacks are given the same ranking (e.g., there are three different stacks given a ranking of 2), then they are considered to be equally good. In this table, M represents transition metal and pSi(core) represents polysilicon as silicon layer 41 in the core of film 40. The symbol " / " indicates where one layer ends and another begins.
[0138]
[0142] In one embodiment, the boride is non-conducting (e.g., B). In one embodiment, the carbide is non-conducting (e.g., B4C or SiC). In one embodiment, the nitride is non-conducting (e.g., SiN). Any of the capping layer materials listed above may be suitable in the combinations shown in Table 2. Examples of such film stacks that are thermally, mechanically, and chemically resistant (e.g., to EUV radiation and H2 exposure) at temperatures up to 450°C are, for example, ZrO2 / SiN / pSi / SiN / Mo / Ru, and B / (SiN) / pSi / (SiN) / Mo / B. For example, in the B / SiN / pSi / SiN / Zr / B stack, the cap layer combination Zr and B allowed for 87-88% EUV transmission while reducing the film's sensitivity to EUV reflection (EUVR) to less than 0.04%. In the film stack B / pSi / B / Zr / B stack, B is a capping layer but also acts as a diffusion barrier layer, and Zr is an emissive layer. [Table 2]
[0139]
[0143] In one embodiment, the film 40 stack includes a diffusion barrier layer. The thickness of the diffusion barrier layer is preferably less than 1 nm to minimize EUV losses. The diffusion barrier layer is between the transition metal layer 48 and the silicon layer 41 or silicon compound layer 43. The diffusion barrier layer is configured to reduce intermixing and / or reaction between the transition metal of the transition metal layer 48 and the silicon layer 41 or silicon compound layer 43. For example, in one embodiment, the diffusion barrier layer is configured to reduce or prevent silicidation between the transition metal and the underlying silicon core material. Intermixing or reaction between the transition metal and silicon may undesirably change the properties of the film 40. For example, the emissivity of the film 40 may be undesirably decreased and / or the physical stress of the film 40 may change.
[0140]
[0144] In one embodiment, the diffusion barrier layer comprises a material selected from the group consisting of B, B4C, C, Cr, Mg, Mo, Re, Ta, Ti, V, W, and nitrides of any of B, B4C, C, Cr, Mg, Mo, Re, Ta, Ti, V, and W.
[0141] In an embodiment, the membrane assembly 80 is applied as a pellicle or as part of a dynamic gas lock. Alternatively, the membrane assembly 80 can be applied in other filtration areas, such as illumination, or for beam splitters. In an embodiment, the dynamic gas lock is configured to block debris in the lithographic apparatus 100. In an embodiment, the dynamic gas lock is positioned between the projection system PS and the substrate W. The dynamic gas lock reduces the likelihood that particles from or near the substrate W reach optical components in or around the projection system PS. Similarly, the dynamic gas lock can protect the illumination system IL. In an alternative embodiment, the dynamic gas lock is positioned at a virtual source point IF. For example, the dynamic gas lock can be positioned between the source collector module SO and the illumination system IL.
[0142]
[0145] Although particular reference is made herein to the use of lithographic apparatus in the manufacture of ICs, it should be understood that the lithographic apparatus described herein has other applications, such as the manufacture of integrated optical systems, guidance and detection patterns for magnetic domain memories, flat panel displays, LCDs, thin film magnetic heads, etc. The substrates described herein may be processed, before or after exposure, for example in a track (a tool that typically applies a layer of resist to a substrate and develops the exposed resist), a metrology tool, and / or an inspection tool. Where appropriate, the disclosure herein may be applied to these and other substrate processing tools. Furthermore, a substrate may be processed multiple times, for example to produce a multi-layer IC, and thus the term substrate as used herein may also refer to a substrate that already includes multiple processed layers.
[0143]
[0146] While specific embodiments of the invention have been described above, it will be appreciated that the invention may be practiced otherwise than as described. For example, various photoresist layers may be replaced with non-photoresist layers which perform the same functions.
[0144]
[0147] The above description is illustrative and not limiting. Thus, it will be apparent to one skilled in the art that modifications can be made to the invention as described without departing from the scope of the claims set out below.
Claims
1. 1. A film for EUV lithography, the film having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W, the film comprising a stack formed by a plurality of layers, the layer materials of the stack being selected such that the refractive index of the stack for EUV radiation having a wavelength of 13.5 nm is greater than 0.
95.
2. A film for EUV lithography, the film having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W, the film comprising a stack formed by a plurality of layers, the layer materials of the stack having a resistance of 10 -3 Films for EUV lithography selected to be less than Ω·m.
3. 1. A film for EUV lithography, the film having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W, the film comprising a stack formed by a plurality of layers, the layer materials of the stack being selected such that they have a melting point higher than 1200° C.
4. A film for EUV lithography, the film having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W, the film comprising a stack formed by a plurality of layers, the layer materials of the stack having a thermal expansion coefficient of about 2×10 -6 m / mK to about 6 x 10 -6 Films for EUV lithography selected to be in the range of m / mK.
5. 1. A film for EUV lithography, the film having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W, the film comprising a stack formed by a plurality of layers, the stack comprising layers in the following order: a capping layer comprising ruthenium at an outer surface of the film, and an anti-migration layer comprising titanium.
6. The materials include YSi2, LaSi2, ZrSi2, SiB4, YB6, NbSi3, MoSi2, YC2, ZrB2, CeSi2, CeB6, LaB6, NbB2, ZrC , CeC2, YN, LaC2, MoB, LaN, Mo2C, NbC, TiSi2, Ru2Si3, ZrN, VSi2, CeN, RuB2, NbN, Y2O3, MoN, TiB 2, La2O3, Nb2O5, WSi2, ZrO2, MoO3, TiC, RuC, SiCr, WB2, VB2, TaSi2, CeO2, TiN, RuN, RuO2, TiO3, VC, TaB2, VN, WC, CrB, CrN, HfO2, Cr3C2, WN, TaC, Ta2O5, TaN.
7. The membrane of any one of claims 1 to 4, wherein the layer of material is a capping layer provided on an outer surface of the membrane.
8. The membrane according to any one of claims 1 to 5, wherein the stack comprises at least one silicon compound layer.
9. The membrane of any one of claims 1 to 5, wherein the stack comprises a silicon layer having silicon in one of the following allotropic forms: amorphous silicon, monocrystalline silicon, polycrystalline silicon, or nanocrystalline silicon.
10. The film of any one of claims 1 to 5, wherein the stack comprises a capping layer comprising Ru and a Mo transition metal layer.
11. 6. The film of any one of claims 1 to 5, wherein the layer comprises a material selected from the group consisting of transition metal silicides, transition metal borides, transition metal carbides, transition metal nitrides, and transition metal oxides, and / or wherein at least one transition metal layer is between the capping layer and the silicon layer, the transition metal layer comprising a transition metal selected from the group consisting of Zr, Y, Mo, Cr, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W.
12. A film for EUV lithography having a thickness of 200 nm or less and comprising at least one layer of a material selected from M-silicide, M-boride, M-boride / M, M-carbide, M-carbide / M, M-nitride, M-nitride / M, M-oxide, M-oxide / M, where M is a transition metal selected from the group consisting of Y, Mo, Hf, Ir, Mn, Nb, Os, Pd, Pt, Re, Rh, Ru, Ta, Ti, V, and W; and a boundary that holds the membrane.
13. The membrane assembly of claim 12 , comprising a frame connected to the boundary.
14. The membrane assembly of claim 13 , wherein the frame is made of the same material as the boundary.
15. 15. The membrane assembly of claim 13 or 14, wherein the thermal expansion of the boundary substantially matches the thermal expansion of the frame.
16. The membrane assembly according to any one of claims 13 to 15, wherein the frame and / or the border are made of silicon.
17. A patterning device assembly for EUV lithography comprising the membrane of any of claims 1-11 or the membrane assembly of claims 12-16.
18. A dynamic gas lock assembly for EUV lithography comprising a membrane according to any of claims 1-11 or a membrane assembly according to claims 12-16.
Citation Information
Patent Citations
Filter window, lithographic projection apparatus, methods of manufacturing filter window and device, and device manufactured thereby
JP2008124495A
Pellicle and method of producing pellicle
JP2009271262A
pellicle
JP2016080967A
Mechanical fixture of pellicle to lithographic photomask
US20120140199A1
Pellicle, reticle assembly and lithographic apparatus
WO2013152921A1