Portland cement concrete, lightweight concrete oyster attachment base and its manufacturing method

A lightweight concrete adhesion base with reduced alkalinity and enhanced calcium content, using biocalcium powder and dark pigments, addresses the issue of high alkalinity in marine substrates, promoting oyster larval attachment and growth while ensuring concrete durability and cost-effectiveness.

JP7580683B2Active Publication Date: 2024-11-12HARBIN ENG UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022533423
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-12-01
Publication Date
2024-11-12
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

Current concrete substrates used in marine environments have high alkalinity, leading to increased seawater pH, inhibiting oyster larval attachment and growth, and traditional methods of oyster cultivation are inefficient and environmentally harmful, lacking effective ecological restoration solutions.

Method used

A lightweight concrete oyster adhesion base is developed using reduced cement amounts, biocalcium powder, carbonate salts, and dark pigments, combined with CO2 curing to lower alkalinity and enhance calcium carbonate content, promoting oyster larval attachment and growth while maintaining concrete durability.

Benefits of technology

The solution effectively reduces alkalinity, enhances oyster larval attachment and growth, and improves concrete durability, reducing labor and transportation costs while minimizing environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580683000006
    Figure 0007580683000006
  • Figure 0007580683000007
    Figure 0007580683000007
  • Figure 0007580683000008
    Figure 0007580683000008
Patent Text Reader

Abstract

This technology relates to an oyster attachment base, particularly to a Portland cement concrete or lightweight concrete oyster attachment base and its manufacturing method. By mixing an attractant into the marine sessile organism attachment base for attracting, it improves the ability to attract, transform, and promote the long-term growth of sessile organisms, and has little effect on other performance properties of the concrete, so it can be used in the construction of marine ecological projects and corrosion prevention of marine concrete projects.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority to Chinese Patent Application No. 201911210488.X, filed on December 2, 2019, entitled "Portland cement concrete oyster adhesion base and manufacturing method thereof," and claims the benefit of priority to Chinese Patent Application No. 201911210477.1, filed on December 2, 2019, entitled "Lightweight concrete oyster adhesion base and manufacturing method thereof," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a technology for oyster attachment base, in particular to a Portland cement concrete, lightweight concrete oyster attachment base and a manufacturing method thereof, and belongs to the interdisciplinary field of marine sessile organisms and concrete. [Background technology]

[0003] With the improvement of people's living standards, the demand for oysters as a health food is increasing. Traditional small-scale aquaculture and farming methods cannot meet the growing demand for oysters. At the same time, with the increase in the amount of oyster reef restoration and the construction of marine ecological projects such as oyster reefs, the demand for oyster attachment substrates is increasing. Common farming methods include crack-building farming, ground seeding farming, bridge stone and standing stone farming, and hanging farming, but there is a problem that it takes a long time for oysters to reach a sufficient attachment rate on the attachment substrate. In addition, with the increase in the amount of oyster farming, the oyster attachment substrate of shellfish such as the shell of the mussel cannot fully meet the needs of oyster larvae, and the price of shellfish attachment substrates is rising. In addition, in patent application CN106719186 recently filed by Ocean University of China, a new oyster attachment base was produced by mixing 15%-20% shell powder and 5%-15% shell waste into the cement paste mass, the shell waste roughens the surface of the attachment base and increases the amount of oysters that attach, the shell waste is easier to collect seedlings from than the shells of the sea mussel, and has a superior larval attachment effect. However, since the water reducer is not taken into consideration in controlling the amount of water used and curing, the permeability of the concrete is determined by the water-cement ratio and curing. As a result, a large amount of alkali contained in the adhesion base is released, increasing the alkalinity of the seawater that comes into contact with it, and inhibiting the attachment of oyster larvae. In particular, when larvae are raised in aquaculture ponds, if the water area is small, the pH value of the water area will rise and the oyster larvae may die. At the same time, if a large amount of shell powder is mixed in, the color of the cement adhesion base will change from dark gray to a light color, which is unfavorable for oyster attachment.

[0004] Concrete has the advantages of being easy to process, easy for larvae to attach, easy to remove, abundant materials, and low cost, but research on the attachment base of cement-based materials is immature, and the problem of high pH causes high mortality of larvae, so concrete can only be used after immersion in seawater for more than one year. In addition, attracting marine organisms with ions is mainly used for laboratory experiments, and since it is expensive and difficult to control, the development and application of technology to attract marine organisms with ions is always limited. Therefore, it is inevitable to invent concrete with low alkalinity and high attraction efficiency as a substrate to attract oysters to attach.

[0005] At the same time, in recent decades, the rapid development of the economy in China's coastal areas, but no attention has been paid to environmental protection, which has caused large-scale destruction of the ecosystem in China's coastal areas, which has serious impacts on the ecosystem and economy of China's coastal areas. At present, with the implementation of a series of relevant national policies, China's marine project construction is also entering a peak period, and at the same time, the large-scale construction of marine projects and breakwaters to ensure the stabilization of the surrounding sea areas will further damage the already fragile marine ecosystem. If proper protection measures for the ecological environment are not taken, it will damage the ecosystem of China's coastal areas more seriously. At the same time, most of the infrastructure in China's coastal areas cannot be dismantled and the ecosystem of the sea area needs to be restored, so people gradually realize that the application of ecological technology to many infrastructures can effectively improve or restore the ecosystem of the marine area. Therefore, building concrete projects with high ecological effect or ecologicalizing existing concrete projects is very important and urgent for the improvement of the ecological environment of China's coastal areas. However, up to now, the ecological technology of projects in tidal areas such as breakwaters is still a blank in China.

[0006] Oysters, as "ecological engineers", are mainly concentrated in the tidal range and within 30 meters of water depth, and at the same time, they prefer to attach to the same kind of shells to form thick oyster reefs, so they can attach densely to the breakwater and realize the ecologicalization of the breakwater. In addition, the current oyster reefs are seriously damaged, and most of them need to be reattached on a large scale to realize the restoration of the ecosystem. Both the construction of marine ecological projects and the restoration of oyster reefs can achieve their ecological functions through mass propagation of oysters. Therefore, concrete oyster attachment bases are in great demand. Current research on oyster attachment in China and abroad is as follows:

[0007] 1. The effect of ions on the attachment and metamorphosis of marine sessile larvae

[0008] Research on the attachment and metamorphosis of marine sessile organism larvae in China and abroad has mainly focused on the effects of ion concentration in the solution. The ions and substances that have been studied in depth are K + , NH3, Ca 2+ , Cu 2+ The first three ions or substances can promote the attachment or transformation of oysters at appropriate concentrations, but Cu 2+ The promoting effect of K is unclear and even increases larval mortality at high concentrations. + induces larval metamorphosis by affecting the behavior of cell membranes, and NH3 enters the cells and causes an increase in intracellular pH, which depolarizes the neurons of the behavioral pathway and induces sessile metamorphosis. Many studies on the attachment and metamorphosis of sessile organisms to the surfaces of materials such as polyethylene boards, shells, and tiles are carried out in solution, but when applied to real marine concrete projects, such methods are not easily achievable or are too costly.

[0009] Currently, the widespread application of concrete in marine projects, especially in recent oyster reef restoration projects, makes concrete the most commonly used substrate material for marine sessile organisms. However, concrete materials are significantly different from traditional shells, limestone, rubber tires, and plastic boards. Concrete has high alkalinity, high calcium ions, and is also rich in other ions such as potassium ions and sodium ions, which greatly affect the attachment and growth of oysters. Currently, oyster reef restoration projects use newly constructed concrete members and discarded concrete as restoration substrates, but the effect is not ideal.

[0010] II. Effects of different types of cement concrete on marine plants and sessile organisms

[0011] At present, almost all marine concrete projects use Portland cement concrete with high alkalinity (pore solution pH value is usually 12.0-13.0), while the pH value of seawater is usually 7.9-8.4. Due to the existence of an alkali concentration gradient, concrete in contact with seawater will continuously release alkali, thereby raising the pH of the seawater in this sea area and destroying the local ecosystem. It has a great inhibitory effect on the attachment and growth of sessile organisms, especially alkali-sensitive organisms, on its surface, which has a great impact. At present, as can be seen from research conducted by China and other countries, there are great differences in the bioadhesion effect of different types of concrete artificial reefs, and Portland cement concrete artificial reefs made of sulfoaluminate cement and fly ash have excellent bioadhesion effect, and their alkalinity is lower than that of ordinary Portland cement concrete. [1]Similarly, mixing 40% to 60% fly ash and slag powder into cement concrete has a good eco-effect. In addition, the types and amount of organisms attached to concrete made of granular cementitious materials are greater than those of concrete made of granular cementitious materials, and the higher the content of granular cementitious materials, the greater the impact on the ecosystem. Low-alkalinity cement concrete, such as aluminate cement, especially slag Portland cement, which contains 50% slag powder, is used in the construction of ecological concrete projects in the United States, so it has an eco-effect of attracting marine plants and animals [2, 3]. By mixing concrete with low-alkalinity cement, the amount of alkali-sensitive organisms (mainly marine plants) can be effectively increased, but the increase in the amount and density of attachment to oysters is limited.

[0012] 3. The effect of calcium substances on the adhesion of marine sessile organisms

[0013] As can be seen from Chugai's research, the chemical element composition of the attachment substrate has a great influence on the attachment, metamorphosis, and subsequent growth of oyster larvae. The most commonly used calcium-containing substrates (limestone and concrete) can effectively attract oyster larvae to attach, and the attraction effect is comparable to that of shells. It indicates that calcium plays an important role in the attachment, metamorphosis, and growth of oyster larvae.

[0014] Recently, in addition to the traditional substrate, people have been studying the attachment of oyster larvae by increasing the calcium content in concrete and adding calcium substances to cement-based materials. In the current study, 80 mesh cow bone powder, calcium carbonate powder, and gypsum powder (dosages of 62.5% and 375% of the cement weight) are mixed into mortar respectively to conduct oyster attachment experiments, and it was found that under the same conditions, the order of calcium endowment form in the ability to attract oyster larvae is cow bone powder > calcium carbonate = calcium sulfate, and the dosage of calcium carbonate powder is 5%-60% of the mortar weight (41.7%-500.0% of the cement weight), and it is most effective when the dosage is 20% (166.7% of the cement weight). Adding cow bone powder, calcium carbonate powder, and gypsum powder can increase the amount of oyster attachment, but if the dosage is too high (the weight of calcium powder exceeds 41.7% of the cement weight and even reaches 500.0%), it will have a negative effect on the mechanical properties and durability of concrete, making it unsuitable for concrete projects in marine environments. Furthermore, although powdered bone has a strong attraction effect on oyster adhesion, if it exceeds 10% of the cement, mold will grow in the concrete. Therefore, currently, powdered bone and calcium substances such as calcium carbonate are mixed into concrete, but they are completely unusable in the harsh marine environment because they do not take into consideration the effect of the marine environment on the durability of concrete structures.

[0015] In Chinese patent application CN104529286, starting from the viewpoint of waste utilization, 5mm-8mm oyster shells of 10%-20% of the cement weight are mixed into the artificial fish reef, which results in concrete that does not affect the adhesion of organisms and does not pollute the environment. In CN104938384, 150-200 mesh biocalcium carbonate powder (fish bone, coral, egg shell, shell = 1:1:1:1) and shell waste of 10%-20% of the cement weight are simultaneously mixed into the artificial fish reef, which shows that with the increase in the content of biocalcium carbonate powder, the amount of organisms attracted gradually increases, and when the content of biocalcium carbonate is the highest (20% of the cement weight), the amount of organisms (marine plants, marine organisms) attracted by biocalcium carbonate is the highest. Similarly, in order to reduce the alkalinity of the concrete artificial fish reef surface, it is easier for microorganisms and algae to attach, the amount and population of organisms increases, and the effect of attracting fish is better. The deposit of the cement mortar coating layer of biocalcium carbonate is harmless to the environment and living organisms. Biocalcium carbonate powder, oyster shell waste, etc. are mixed into concrete for the production of artificial fish reefs and bioattachment experiments, and the biocalcium carbonate powder promotes the effect of collecting organisms, mainly marine plants and microorganisms.

[0016] Anyway, calcium content is essential for the attachment of oyster larvae, and some current experimental results also prove that mixing an appropriate amount of calcium carbonate material into cement-based materials can promote the attachment and growth of oyster larvae. However, cement concrete contains a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5. At room temperature, the pH value of saturated calcium hydroxide solution is about 12. Therefore, the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5 × 10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting shellfish to attach is thought to be 10 to 25 mmol / L. Even when oyster larvae are placed in a saturated calcium carbonate solution, the Ca concentration suitable for oyster attachment is not sufficient. 2+Sufficient Ca to provide a concentration 2+ Furthermore, while Ca(OH)2 in cement concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate material is added to concrete to promote the attachment of oyster larvae, Ca 2+ may decide not to play a dominant role.

[0017] Also, if the amount of shell powder is too high, the weight ratio of shell powder to cement exceeds 10% and even reaches 500%, which greatly affects the durability of concrete. Although mixing an appropriate amount of calcium carbonate material can not reduce or improve the anti-penetration property of concrete, an excessive dosage is very disadvantageous to the concrete's resistance to sulfuric acid corrosion and sulfate corrosion from seawater.

[0018] Therefore, there are still many problems in the mixing of calcium substances such as biocalcium carbonate, cow bone powder, calcium carbonate powder, etc. into concrete to attract the attachment of marine sessile organism larvae, particularly problems in concrete performance due to excessive calcium dosage and problems such as mold growth due to cow bone powder.

[0019] 4. The effect of color on the adhesion of marine sessile organisms

[0020] The color of the substrate has a certain effect on the attachment, metamorphosis, and growth of marine sessile larvae. It has been reported overseas that dark-colored substrates can promote the growth of oysters in low-temperature waters. As can be seen from Chinese research, oyster larvae have a certain preference for color. The preference of Hong Kong oyster larvae for the color of plastic attachment substrates is black > white > red. Pacific oyster larvae tend to attach to black and gray plastic plates, and it is thought that black and gray may be protective colors for oyster larvae to avoid predators. Barnacles like to attach to red substrates. Pearl oysters also prefer dark (black, red), non-reflective substrates and show phototactic behavior. Alteromonas calwellii recently attracts oyster larvae by producing compounds involved in melanin synthesis.

[0021] At present, research on the effect of substrate color on the attachment of marine sessile larvae is limited to organic polymer plates, such as plastic plates, polyethylene plates, asbestos plates, etc. As one of the most potential alternative substrates, concrete is especially used in current oyster reef restoration, artificial biological projects, and corrosion protection of marine reinforced concrete, and the effect of its color on the attachment amount of sessile larvae has yet to be investigated.

[0022] 5. Effect of roughness on the attachment of marine sessile larvae

[0023] In general, the surface roughness of the attachment substrate has a certain effect on the attachment of oyster and barnacle larvae. As can be seen from Chugai's research, more oyster and barnacle larvae attach to rough surfaces than to smooth surfaces, other conditions being equal. Rough surfaces provide better tactile stimulation for oyster and barnacle larvae to crawl and attach, extend the residence time of oyster larvae on the substrate, and the presence of cracks and holes can protect the larvae and prevent them from being attacked by predators. In addition, the surface area is larger than that of smooth surfaces, and there is a potential richer and more diverse microbial environment. As can be seen from new research, more marine organisms attach to textured concrete surfaces than smooth surfaces, which can promote the attachment and metamorphosis of larvae. However, some studies show that roughness does not have a significant effect on the attachment and metamorphosis of larvae.

[0024] Anyway, the above studies have been carried out on the effects of different substrates, colors and roughness on the adhesion of marine sessile organisms, but recently, the effect of mixing calcium materials into concrete on the adhesion of marine sessile organisms has been studied. However, due to the knowledge of related fields such as marine biology, marine microorganisms, marine chemistry, marine concrete project materials and structures, etc., the interdisciplinary fields are greatly different, so when carrying out interdisciplinary research, there are many problems, such as the water-cement ratio of the above cement-based materials being unclear, the mechanism of calcium carbonate materials inducing the adhesion of oysters being unclear, the durability of concrete being significantly insufficient due to too much calcium powder added to cement, and mold growth on the mixed cow bone powder, and experts in marine concrete project materials and structures lack the necessary expertise for the adhesion of marine sessile organisms, so interdisciplinary experts need to work together to solve many problems. Summary of the Invention

[0025] The object of the present invention is to provide a concrete adhesion base with excellent durability that attracts sessile organisms to adhere quickly and densely to the concrete surface, thereby solving the problems that the current concrete oyster adhesion base has, in that the amount of cement used is large and the amount of water used is not controlled or cured, resulting in improved permeability of the concrete, the adhesion base containing a large amount of alkali, and the alkali released continuously and rapidly increases the alkalinity of the seawater in contact with it, inhibiting the adhesion of marine sessile organism larvae, and at the same time, the color of the cement adhesion base changes from dark gray to a light color due to the mixing of a large amount of shell powder, which is unfavorable for the adhesion of oyster larvae.

[0026] The method of achieving the present invention is as follows. The present invention reduces the amount of cement used in the adhesion base, selects an appropriate cement type, and mixes in an appropriate mineral admixture to obtain a cement with low alkalinity. In addition, the addition of dark color pigments, biocalcium powder, carbonate (hydrogen) salt, etc., and the use of CO2 curing further reduces the alkalinity of the concrete, improves the calcium carbonate content of the concrete surface, and synergistically promotes the early attachment, metamorphosis, and later growth of oyster larvae. At the same time, the structure of the adhesion base is designed. In addition, the adhesion base is directly attached to the larvae in the culture pond, and does not need to be used after being immersed in seawater for a long time, and the service life of the adhesion base can be more than 50 years if there is no severe collision or destruction.

[0027] The present invention further has the following structural features.

[0028] The components of the material 1 are Portland cement, mineral admixture, coarse aggregate, sand, water, dark color pigment, bio-calcium powder, carbonate (hydrogen) salt, and superplasticizer, and the weight percentages thereof are 9.0% to 17.0%, 4.0% to 11.5%, 38.4% to 47.8%, 24.9% to 37.3%, 6.2% to 9.0%, 0.3 to 2.0%, 0.3 to 2.0%, 0.3 to 1.5%, and 0.02% to 0.1%, respectively.

[0029] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red;

[0030] Preferably, the method for modifying the dark pigments involves modifying these pigments according to their impact on concrete performance, and using one of transparent resins, organosilicon, dimethylsiloxane, and superhydrophobic materials for the modification treatment.

[0031] Preferably, the bio-calcium powder is cow bone powder and bio-calcium carbonate powder, and the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and has a fineness of 100 mesh to 1000 mesh.

[0032] Preferably, the method for modifying the bio-calcium powder is to treat 100 mesh to 500 mesh oyster shell powder, eggshell powder, coral powder, and fish bone powder with one or two of ethanoic acid, acetic acid, silicic acid, and sulfurous acid, and treat 100 mesh to 500 mesh cow bone powder with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

[0033] Preferably, the modified carbonate (hydrogen) salt is one or more of sodium carbonate, potassium carbonate, calcium bicarbonate, sodium bicarbonate, potassium bicarbonate, using diatomaceous earth as a carrier to achieve sustained release of the corresponding ions after complexing with those inorganic salts, reducing or eliminating the adverse effects on concrete performance.

[0034] Preferably, the Portland cement is ordinary Portland cement having a strength rating >32.5, and the mineral admixture comprises a combination of one or more of silica fume, slag, and fly ash.

[0035] Preferably, the sand is one or more of river sand, machine-made sand (the parent material is one of basalt or granite), or desalinated sea sand, and has good grading.

[0036] A method for producing a Portland cement concrete oyster-attached base, comprising: Step S1 of designing different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacturing molding forms with different roughness; Step S2 of accurately measuring Portland cement, mineral admixtures, coarse aggregates, sand, water, dark pigments, bio-calcium powder, modified bicarbonates, and superplasticizers; First, put the coarse aggregate and sand into the concrete mixer and mix for 0.5 to 1 minute, then add Portland cement, mineral admixture, dark pigment, bio-calcium powder, and modified carbonate (hydrogen) salt and mix for another 1 to 2 minutes, then add water and superplasticizer and mix for 2 to 6 minutes, mix evenly, and then pour and vibrate in step S3; The method includes step S4 of immediately placing the molded concrete specimen in a curing box with high concentration CO2 for curing for 0.5 to 5 hours to reduce the alkalinity of the cement specimen, and then curing for 28 days as standard or according to actual conditions.

[0037] This makes it possible to produce a Portland cement concrete oyster attachment base with excellent attracting effect.

[0038] The materials of component 2 are dark pigment, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer, and the weight percentages of the dark pigment, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer are 0.3-2.0%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively.

[0039] The components of the material 3 are cow bone powder, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer, and the weight percentages of the cow bone powder, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer are 0.3-2.0%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively.

[0040] The components of the material 4 are a dark pigment, a carbonate or bicarbonate, a Portland cement, a mineral admixture, crushed stone, sand, water, and a superplasticizer, and the weight percentages of the dark pigment, the carbonate or bicarbonate, the Portland cement, the mineral admixture, the crushed stone, the sand, the water, and the superplasticizer are 0.3-2.0%, 0.3-1.5%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively.

[0041] The object of the present invention is to solve the problems that currently occur due to the lack of consideration given to control of water usage and curing (the permeability of concrete is determined by the water-cement ratio and curing), resulting in the release of a large amount of alkali contained in the adhesion base, which increases the alkalinity of seawater that comes into contact with it and inhibits the attachment of marine sessile organism larvae, and at the same time, due to the mixing of a large amount of shell powder, the color of the cement adhesion base changes from dark gray to a light color, which is unfavorable for oyster attachment. In order to solve these problems, the present invention aims to provide a lightweight concrete adhesion base that is highly durable and attracts sessile organisms to attach quickly and densely to the concrete surface.

[0042] The realization method of the present invention is as follows. The present invention reduces the amount of segments used in the adhesion base, selects the appropriate cement type, adds appropriate mineral admixtures, obtains low-alkalinity cement, and at the same time controls the water-cement ratio of the concrete of the adhesion base, controls its release rate, and mixes in adhesion color, dark color substances, calcium carbonate and trace elements according to the preferences of oysters, thereby promoting the early attachment, metamorphosis and later growth of oysters, and designs the structure of the adhesion base. In addition, the adhesion base is directly attached to the larvae in the culture pond, and does not need to be used after being immersed in seawater for a long time. If there is no severe collision or destruction, the service life of the adhesion base can be more than 50 years.

[0043] In addition, the use of lightweight aggregate concrete can reduce the weight of the concrete attachment base, thereby reducing transportation and labor costs during the manufacturing, transportation, and curing of test specimens. In addition, in actual marine aquaculture, it can reduce the labor costs of fishermen who move the attachment base to harvest oysters, reduce costs such as transporting and fixing the concrete project, and further reduce the risk of it accidentally falling to the ground and being damaged during use.

[0044] The present invention further has the following structural features.

[0045] The components of the material 1 are cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, calcium carbonate powder, trace elements, and superplasticizer, and the weight percentages thereof are 22.0% to 35.0%, 25.0% to 38.0%, 16.0% to 30.0%, 8.5% to 16.5%, 0.6% to 3.0%, 0.6% to 3.0%, 0.2% to 1.8%, and 0.03% to 0.18%, respectively.

[0046] Preferably, the deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

[0047] Preferably, the dark pigments are modified according to their impact on concrete performance, and the modification treatment is carried out with one of transparent resins, organosilicon, dimethylsiloxane, and superhydrophobic materials.

[0048] Preferably, the trace elements are zinc, iron, potassium and phosphorus, which are modified with natural minerals, industrial products or chemical reagents, including one or more of zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate, potassium phosphate, ammonium phosphate and iron phosphate, to achieve sustained release of the corresponding ions and reduce or eliminate the adverse effects on the performance of concrete. However, in the case of eutrophication areas, do not select materials containing nitrogen or phosphorus elements.

[0049] Preferably, the calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, and processed precipitated calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultra-fine precipitated calcium carbonate, and has a fineness of greater than 200 mesh.

[0050] Preferably, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt, lightweight ceramsite having a maximum particle size of less than 20mm.

[0051] Preferably, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, and has a particle size of 0.2 mm to 5 mm.

[0052] Preferably, the cementitious material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, where the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag and alkali-activated slag + fly ash.

[0053] A method for manufacturing a lightweight concrete oyster-attached base, comprising: Step S1: accurately weighing cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, calcium carbonate powder, trace elements, and superplasticizer; The method includes step S2 of firstly putting the lightweight coarse aggregate and the lightweight fine aggregate into the concrete mixer and stirring for 0.5-1 minute, then adding the cementitious material, the dark color pigment, the calcium carbonate powder and the trace elements and continuing to stir for 0.5-1 minute, then adding the water and the superplasticizer and stirring for 2-6 minutes, and then stirring evenly, and then pouring and vibrating, and then curing for 28 days according to the standard curing or curing according to the actual situation.

[0054] This makes it possible to produce a lightweight concrete oyster attachment base with excellent attracting effect.

[0055] The components of the material 2 are dark pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, and the weight percentages of the dark pigment, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively.

[0056] The components of the material 3 are calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, and the weight percentages of the calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively.

[0057] The components of the material 4 are dark color pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer, and the weight percentages of the dark color pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer are 0.6-3.0%, 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively.

[0058] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0059] The present invention uses dilute acid modification and composite crushing technology to fully exert the attracting ability of cow bone powder, greatly reduce the dosage of cow bone powder, and perform anticorrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage and at the same time has a high oyster larvae attachment ability and solves the problem of mold growth on concrete. Similarly, by controlling the fineness of calcium carbonate powder, the water-cement ratio at the dosage level, and mixing dark color pigments, the strength and permeability of concrete are hardly affected. For concrete mixed with these attractants, the amount of oyster larvae attached to the concrete mixed with the attractants is significantly increased compared to concrete without the attractants.

[0060] By using lightweight aggregate concrete, the present invention can reduce the weight of the concrete attachment base, and reduce transportation costs and labor costs in the processes of manufacturing, transporting, and curing the test specimens.In addition, in actual sea farming, it can reduce the labor costs of fishermen who move the attachment base to harvest oysters, and reduce costs such as transportation and fixing when applied to marine concrete projects.Furthermore, it can reduce the risk of accidentally falling to the ground and being damaged during use. [Brief description of the drawings]

[0061] [Figure 1] Mold grows on the surface of concrete that has a different mix ratio, that is, 10% cow bone powder mixed in. [Diagram 2] The powder size is 200 mesh, and the mixing ratio is different when 10% modified cow bone powder is mixed. [Diagram 3] FIG. 1 is a schematic diagram of a 210-day actual marine adhesion experiment. [Figure 4] FIG. 1 is a schematic diagram of a 300-day actual marine adhesion experiment. [Diagram 5] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 6] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 7] FIG. 1 is a schematic diagram of a concrete oyster attachment base. [Figure 8]FIG. 1 is a schematic diagram of a 300-day actual marine adhesion experiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0062] The invention will now be further described with reference to the drawings and specific embodiments.

[0063] These examples are only used to explain the present invention, and do not limit the scope of the present invention. The implementation method of Examples 1 to 20 is the same, and the shape of the concrete oyster adhesion base is designed, specifically referring to Figures 5 to 7, and their concrete mix ratio is as follows:

[0064] In Example 1, the weight percentages of ordinary Portland cement, crushed stone, sand, water and polycarboxylate water-reducing agent powder are 17.1%, 46.67%, 29.0%, 7.2% and 0.03%, respectively.

[0065] Here, the coarse aggregate refers to crushed stone, the maximum particle size of which is less than 20mm, which can be one of crushed stones of basalt, granite and diabase, and has good grading, and the particle size of sand is 0.16mm-5.0mm, where the sand is one or more of river sand, machine-made sand (base material is basalt or granite), and sea sand, and the water must meet the quality standard for water for concrete (JGJ63-2006), with Cl- content <1000mg / L, PH value >4.5, and has little effect on the initial setting time difference and final setting time, strength, and permeability of cement. Also, the above materials selected in Examples 1-21 are the same.

[0066] In Example 2, the mix ratio of the reference concrete was 10.26%, 0.86%, 5.98%, 46.67%, 29.0%, 7.2%, and 0.03% by weight of ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, and polycarboxylate water-reducing agent powder, respectively. [Table 1]

[0067] As can be seen from the above examples, when blast furnace slag powder and silica fume are mixed into concrete, it can not only fill the gaps between particles such as cement, but also cause a pozzolanic reaction, which then improves the interface microstructure of the transition area, not only ensures the basic strength of the concrete, but also reduces the alkalinity and permeability of the concrete itself. It plays an important role in reducing the alkalinity difference caused by the contact between the concrete and seawater in contact with it, and at the same time, the low permeability suppresses the release rate of alkali, and finally, it makes it easier for oyster larvae to attach to the concrete surface.

[0068] The weight percentages of Example 3, unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0069] The weight percentages of Example 4, unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0070] The weight percentages of Example 5, unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0071] The weight percentages of Example 6, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0072] The weight percentages of Example 7, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0073] The weight percentages of Example 8, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0074] The modification method of the modified dark pigment is as follows: Use 196 transparent resin, mix 3% hardener and 1.5% accelerator, mix with pigment, and the volume ratio of pigment to resin is 1:0.2, cure at room temperature for 4 hours, cure at 60℃ for 4 hours, then crush by beating, and grind by vibration mill until the powder size exceeds 400 mesh. [Table 2]

[0075] Black pigments have a significant effect on the permeability of concrete, and as the dosage increases, the amount of oyster larvae attached decreases. On the one hand, the permeability of concrete improves, so the leaching of alkali in concrete increases, and on the other hand, iron oxide is converted into iron ions, and the concentration of iron ions increases, which may inhibit the attachment of oyster larvae. To address this problem, the pigment is covered with resin and then crushed into powder, which can greatly improve the permeability prevention of concrete, and especially when the dosage is 1.37%, its electric flux increases by only 3.2%. At the same time, with the increase in dark pigment, the amount of oyster attachment also increases, and when the dosage is 1.37%, it appears as a decrease in the attachment rate of oyster larvae, unlike before the modification.

[0076] In Example 9, the weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0077] The weight percentages of Example 10, unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0078] In Example 11, the weight percentages of unmodified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder were 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0079] In Example 12, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.51%, 10.26%, 0.79%, 5.54%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0080] In Example 13, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.75%, 5.23%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0081] In Example 14, the weight percentages of modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 1.37%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0082] The method for modifying the bone powder is as follows: 100 mesh bone powder is added to a 2% phosphoric acid solution, the weight ratio of the two is 1:3, the temperature is 20-30°C, the mixer is stirred at 200-500 revolutions / min for 30 minutes, the centrifuge is centrifuged at 3000-5000 revolutions / min for 3 minutes, the supernatant is discarded, and the centrifuged solid is washed with water 2-3 times, the washing water is not acidic, the centrifuged solid is vacuum dried at 40°C, and the dried bone powder and the 1:4 slag powder are ground in a vibration mill until the fineness exceeds 200 mesh, and then prepared for use. [Table 3] Note: The modified cow bone powder is ground to a powder size of 200 to 300 mesh.

[0083] In response to the problem that cow bone powder is difficult to crush and generally difficult to continue crushing to about 100 mesh, here, 80 mesh cow bone powder is first chemically modified with 2% concentration dilute phosphoric acid, and then dried cow bone powder and 1:4 slag powder are crushed in a vibrating mill until the fineness exceeds 200 mesh. In this way, the contact between the modified cow bone powder and the alkaline substance in the concrete is improved, and at the same time, the microstructure inside the concrete is denser and there is no mold phenomenon that occurred before. After modification, in the case of low dosage, the penetration prevention of the concrete is also improved. Even when the dosage reaches 1.37%, the electric flux increases to only 4.2%, and the attachment change rate of oyster larvae increases from 205% to 400%.

[0084] The weight percentages of Example 15, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 0.51%, 10.26%, 0.68%, 4.79%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0085] The weight percentages of Example 16, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 0.86%, 10.26%, 0.64%, 4.48%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively.

[0086] The weight percentages of Example 17, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), modified cow bone powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water and polycarboxylate water reducer powder are 0.86%, 1.37%, 10.26%, 0.58%, 4.03%, 46.67%, 29.0%, 7.2%, and 0.03%, respectively. [Table 4]

[0087] Compared with the control group, when the dosage of modified dark pigment is 0.86%, the dosage of modified cow bone powder is 0.51%, 0.86% and 1.37%, respectively, and the attachment amount of oyster larvae is increased by 167%, 300% and 500%, respectively. In addition, when the modified cow bone powder is mixed independently and at the same time the dosage of modified dark pigment at 0.86% is mixed, the conversion rate of oyster larvae is increased by 10% in each case. This shows that the two attractants have a synergistic effect.

[0088] The weight percentages of Example 18, modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, sodium carbonate and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.71%, 4.79%, 46.67%, 29.0%, 7.2%, 0.3%, and 0.03%, respectively.

[0089] In Example 19, the weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, sodium carbonate and polycarboxylate water reducer powder are 0.86%, 10.26%, 0.65%, 4.58%, 46.67%, 29.0%, 7.2%, 0.8%, and 0.03%, respectively.

[0090] The method for modifying sodium carbonate is as follows: select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 100g sodium carbonate to 100g water at room temperature, stir until completely dissolved, and prepare for use; then add 150g of the above diatomaceous earth into the solution, stir in a mixer with a rotation speed of 200-500 revolutions per minute for 30 minutes, and then dry in a drying oven with a drying temperature of 100°C to obtain the product. [Table 5]

[0091] In this embodiment, the dark pigment and sodium carbonate are mixed together to provide a dark concrete surface, meet the phototaxis requirements of oyster eyespot larvae, and provide calcium carbonate necessary for the attachment and metamorphosis of oyster larvae. Mixing them together can improve the attachment rate of oyster larvae. When the ratio of dark pigment is 0.86% and the ratio of sodium carbonate is 0.8%, the attachment rate is improved by 116%, which proves that carbonate (hydrogen) salt can promote the attraction of oyster larvae to attach.

[0092] In Example 20, the weight percentages of modified dark pigment (mass ratio of iron black:aniline black mixture = 1:1), bio-calcium powder, ordinary Portland cement, silica fume, blast furnace slag powder, crushed stone, sand, water, sodium carbonate and polycarboxylate water reducer powder are 0.86%, 0.86%, 10.26%, 0.54%, 3.78%, 46.67%, 29.0%, 7.2%, 0.8%, and 0.03%, respectively.

[0093] In this embodiment, a combination of dark pigment, bio-calcium powder, and sodium carbonate is mixed in, ensuring that the basic performance of the concrete is not significantly affected. Therefore, it not only provides a dark concrete surface and meets the phototaxis requirements of oyster eyespot larvae, but also provides the nutrients necessary for the attachment of oyster larvae and the synthesis of calcium carbonate in the case of metamorphosis, and further improves the attachment rate of oyster larvae.

[0094] The specific operation steps of the methods of carrying out Examples 1 to 20 are as follows:

[0095] According to the above-mentioned method for producing the Portland cement concrete adhesion base, three cylindrical specimens with a diameter of 100×50 mm and five rectangular specimens with a diameter of 200×200×30 mm are produced, which are respectively used to test the concrete's resistance to chloride ion penetration for 28 days and the adhesion and transformation of oyster larvae in the laboratory after standard curing for 28 days. The specific operation steps are as follows:

[0096] (1) Formation of specimen

[0097] 1. Calculate and accurately weigh out the ordinary Portland cement, mineral admixture, crushed stone, sand, water, dark color pigment, bio-calcium powder, carbonate (hydrogen) salt and polycarboxylate water reducer powder according to the above mass.

[0098] 2. Sandpaper with different surface roughness (including 20 mesh, 60 mesh, and 200 mesh) was attached to the inside of the mold of the rectangular concrete specimen in preparation for use.

[0099] 3. First, put the crushed stone and sand into a concrete mixer and mix for 0.5 to 1 minute. Next, add regular Portland cement, mineral admixtures, bio-calcium powder, carbonate (hydrogen) salt, and dark pigment and mix for another 0.5 to 1 minute. After that, add water and superplasticizer and mix for 2 to 6 minutes. After mixing evenly, pour, vibrate, and cut out into molds, and three cylindrical specimens with Φ100×50mm and five rectangular specimens with 200×200×30mm can be produced.

[0100] 4. The molded concrete specimens were immediately placed in a CO2 curing box under 10 atmospheres of pressure and cured for 2 hours to reduce the alkalinity of the cement specimens. They were then cured for 28 days as per the standard procedure, and permeability evaluations were performed for each stage. After 28 days, oyster larvae attachment and metamorphosis tests were performed in the laboratory.

[0101] (II) The specific steps of the rapid chloride ion permeability test are as follows: According to the standard "Standard Test Method for Electrical Indication of Concrete's Ability to Resist Chloride Ion Penetration" (ASTM1202-2017), when curing for 28 days, take out three cylindrical specimens of Φ100×50mm from the curing chamber, and clean the water and impurities on their surfaces. After the surfaces are dried, apply a thin layer of epoxy to the surface of the cylindrical specimen. Then, place the specimen in a vacuum saturator for 20-24 hours. Then, take out the specimen, clean its surface, and place it in an organic glass mold. At the same time, detect the sealing between the specimen and the mold, and then put a 3% sodium chloride solution (electrode is connected to the negative pole of the power supply) and a 0.3 mol / L sodium hydroxide solution (electrode is connected to the positive pole of the power supply) into the mold on both sides. Then start the experimental equipment, and after 6 hours, record the test data, and repeat the above operations for the last two specimens. Finally, calculate the strength according to the norm.

[0102] (3) The specific steps of the laboratory oyster larvae attachment and metamorphosis test are as follows:

[0103] After 28 days of standard curing, the rectangular specimens of 200×200×30 mm are taken out of the curing room, and the water and impurities on their surfaces are washed off, and then they are placed in a test pond. A test pond (2.8m×1.7m×1m) is created in the laboratory, and the amount of oyster larvae is 0.85ind / ml3. The seawater in the pond is sand-filtered seawater from the Yellow Sea, and the salinity is about 32%~34%. After the seawater level is higher than the concrete specimen, oxygen pipes are evenly arranged in the test pond to prepare for throwing the oyster larvae. After slowly stirring the oyster larvae in the bucket, a beaker is used to accurately measure the mass of the seawater containing the oyster larvae, and then the mass is evenly thrown into the test pond.

[0104] After the oyster attachment attraction test began, the seawater in the test pond was replaced every day, with the amount of water replaced being 1 / 3 of the total capacity of the test pond. A screen (200 mesh or more) was used to block the drainage outlet to prevent unattached oyster larvae from being washed away with the water. The larvae on the screen were then thrown back into the test pond. Chlorella was fed at regular intervals and in quantitative amounts using a Pasteur pipette at 9:00 and 19:00 every day, and the attachment situation of the oysters was observed.

[0105] After the test has been continued for a specified age, the water in the test pond is drained, the specimens are taken out, and the number and survival rate of oysters on the surface of the specimens are counted, recorded and analyzed. For the statistics, the smooth bottom surface is used when pouring and molding the concrete.

[0106] Compared with Reference 1 (New concrete artificial reef and its manufacturing method CN104529286 A), the differences are as follows:

[0107] The object of the present invention is different from that of Reference 1, in which oyster shell powder is mixed into concrete, but the purpose is waste utilization, restoration and improvement of artificial fish reefs. The object of the present invention is to attract oyster larvae to attach.

[0108] Compared with Reference 2 (Biomimetic concrete artificial reef and its manufacturing method 2015 CN104938384 A), the differences are as follows:

[0109] (1) The objective of the present invention is different from that of Reference 2. In Reference 2, oyster shells or oyster shell powder are mixed into concrete, but the objective is to improve the aquatic environment by attracting fish, microorganisms, and algae through biomimetic surface and increasing the number of microorganisms, and oysters are not mentioned. The objective of the present invention is to attract oyster larvae to attach.

[0110] (2) According to Reference 2, biocalcium carbonate powder (150-200 mesh) less than 10% of the dosage of the segment is ineffective for attraction and attachment. However, in the course of research, it is found that the optimal dosage of bovine bone powder and biocalcium carbonate powder (fineness of 100-1000 mesh) is less than 10% of the cementitious material by using modified bovine bone powder and biocalcium carbonate powder.

[0111] (3) The modification of beef bone powder and biocalcium carbonate powder is specifically performed by treating eggshell powder, coral powder, oyster shell powder, and fish bone powder of 100 mesh to 500 mesh with one or two of tannic acid, acetic acid, silicic acid, and sulfurous acid, and treating beef bone powder of 100 mesh to 500 mesh with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

[0112] (4) In the references, it is difficult to embed oyster shells on the concrete surface, and not all project surfaces use this method, which is not feasible. The present invention adds shell powder into the concrete to attract organisms to attach, and the dosage of shell powder accounts for 10% of the cementitious material mass, which is easy to implement and can greatly improve the amount of oyster attachment.

[0113] (5) In recent years, serious corrosion of artificial reefs has been observed in marine environments. The serious corrosion is mainly caused by the combined action of biological sulfuric acid secreted by anaerobic microorganisms such as Thiobacillus subtilis and acidic substances secreted by other bacteria. However, calcium carbonate has very poor resistance to acid corrosion. If the content of calcium carbonate with large fineness is too high, it can cause serious acid corrosion.

[0114] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:

[0115] (1) In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete independently. The fineness of all calcium materials in the present invention is greater than 100 mesh, which is greater than the fineness of the materials in Reference 3. Similarly, cow bone powder is mixed, but one or more biocalcium carbonate powders such as oyster shell powder, egg shell powder, fish bone powder, and coral powder are mixed in combination. The purpose is to fully exert its attraction ability while taking into account the grading of concrete particles.

[0116] (2) At room temperature, when the cow bone powder is crushed by a vibrating mill and the fineness exceeds 80 mesh, the cow bone powder contains a large amount of collagen, so it becomes lumpy and cannot be crushed further. In the present invention, by using the dilute acid modification technology and crushing with other substances, cow bone powder with small particle size and modified bio-calcium powder with fineness > 200 mesh can be obtained. The obtained bio-calcium powder retains the original substance of bio-calcium, improves the release rate of the substance for attracting oyster larvae to attach, and reduces the dosage of bio-calcium powder, thereby reducing the impact on cement concrete performance.

[0117] (3) Bone powder contains a large amount of collagen and other organic substances. Mixing a large amount of these substances will reduce the strength and permeability of concrete. Especially when the dosage exceeds 5%, the strength of concrete will rapidly decrease, the permeability will be significantly reduced, and mold will grow on the concrete surface under standard curing conditions. Figure 1 shows the mold growing on the concrete surface. Figure 2 shows the surface of the modified concrete. As can be seen from Figure 1, the mold on the concrete surface is white and cotton-like, covering almost the entire concrete surface, while when the cow bone powder, age and curing conditions are the same, there is no mold on the concrete surface in Figure 2.

[0118] The present invention utilizes the dilute acid modification and composite crushing technology to fully exert the attracting ability of cow bone powder, greatly reducing the dosage of cow bone powder, and carrying out anti-corrosion treatment and modification to produce a composite attractant mainly made of cow bone powder, which has a low dosage, a high oyster larvae attachment ability, and solves the problem of mold growth on concrete. The amount of oyster larvae attached to concrete containing the attractant is significantly higher than that of concrete without the attractant.

[0119] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that adding an appropriate amount of calcium carbonate material to cement-based materials can promote the attachment and growth of oyster larvae. However, cement concrete contains a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5, and at room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment.2+ Furthermore, while Ca(OH)2 in cement concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate material is added to concrete to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.

[0120] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:

[0121] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the concrete is diluted and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the concrete increases, and the amount of HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the concrete will increase rapidly, the alkali and carbonate in the concrete will be rapidly leached, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, so the adhesion will decrease,

[0122] 2) With the same amount of substitute aggregate, the permeability of concrete decreased with increasing dosage, and the calcium ions and OH - The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.

[0123] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.

[0124] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:

[0125] In Reference 4, concrete is used to attract marine organisms, which mainly starts from the size and diversity of the attached organisms, the main attached organisms being various algae. In the present invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look similar, they are actually quite different. Figures 3 and 4 respectively show a comparison of the biofouling situation after about 210 days of actual sea attachment experiment in Reference 4 and the biofouling situation after 300 days of actual sea attachment experiment in the present invention.

[0126] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to achieve low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristic of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the alkali resistance of marine plants and sessile organisms such as oysters and barnacles is different, and the environment required in the attachment stage and later stage is different, for example, the attachment, transformation and later growth of barnacles and oysters require a large amount of calcium ions.

[0127] Thus, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, marine plants and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain, according to Reference 1, the technical features in the present invention in which the reduction in alkalinity of concrete and the balance of calcium ion concentration are closely related to the attachment of marine sessile organisms.

[0128] The unique features and beneficial effects of the present invention are as follows:

[0129] Deep color pigment

[0130] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) are modified and then mixed into concrete to change the color of the concrete, making the concrete darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.

[0131] Marine biology researchers have studied the attachment of marine sessile organisms using different colored substrates to breed and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, dark colored concrete is used to attract oyster larvae to attach. The present invention adds dark color pigments to darken the color of the concrete surface and promote the attachment of oyster larvae. Since other materials are mixed into the concrete, it affects the concrete performance. The present invention considers that concrete with different cements has different surface colors. Therefore, the dosage of the dark color material is determined based on the cement type and dosage. The dark color pigment also affects the concrete performance. Most importantly, the dark color pigment is mixed in while simultaneously reducing the alkali and Ca in the concrete. 2+ If the permeability of concrete is not controlled, the released alkali will affect the attachment, metamorphosis and growth of sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the permeability prevention of concrete is designed and controlled, and the main measures are the selection of the type of dark color pigment, the control of the dosage and modification. With the increase in the dosage of dark color material, the amount of larvae attachment will increase, and when the dosage is 0.5%-6% of the cementitious material, the amount of larvae attachment is the highest, and then increases slightly or remains unchanged.

[0132] Carbonate (hydrogen) salt

[0133] According to the inventor's research, the main mechanism by which calcium carbonate materials are mixed into cement-based materials to attract oysters is CO3 2- Ca 2+ Since calcium carbonate plays a major role in the attachment and metamorphosis of oyster larvae, the present invention innovatively provides a method of attracting oyster larvae to attach to the concrete surface by using non-calcium carbonate carbonates and hydrogen carbonates. Therefore, by mixing and modifying carbonates (hydrogen) salts (sodium carbonate, potassium carbonate, calcium hydrogen carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate), the strength and permeation prevention properties of the concrete are basically unchanged, and the attachment attraction rate of oyster larvae is greatly improved. Specifically, the method is as follows.

[0134] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms in order to clarify the attachment mechanism of oysters and the purpose of their reproduction and proliferation, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. It can be seen that the interdisciplinary fusion of the attachment of marine sessile organisms and concrete materials science can add corresponding substances into concrete to attract oyster larvae to attach to the concrete surface. Since soluble salts have a great impact on concrete performance such as early workability, adhesion time, and later strength and anti-permeability, the present invention uses diatomaceous earth as a carrier to fix these salts inside diatomaceous earth, reducing the impact of soluble salts on concrete performance, while utilizing the effect of diatomaceous earth in improving concrete performance, and realizes that even if these attractants are added, the excellent mechanical properties and anti-permeability of concrete can be maintained. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is kept at a very low level, especially after immersion in seawater for a certain period of time. When the mass of sodium carbonate mixed independently is 0.8%, the growth of the induction efficiency is the highest, reaching 66%. Therefore, similarly, this part of knowledge is related to the interdisciplinary fusion of marine sessile organisms, chemistry, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain technical characteristics closely related to concrete with excellent ability to attract oyster larvae to attach in the present invention, due to the conventional background, by mixing carbonate (hydrogen) salt into concrete, changing the content of carbonate (hydrogen) salt on the concrete surface, and controlling the permeability of concrete.

[0135] Permeability of concrete

[0136] The strength and permeability of concrete are the two most important performances of concrete. Adding different attractants into standard concrete will affect the performance of concrete, so when mixing different substances to promote the attachment, metamorphosis and subsequent growth of oyster larvae, first, it is necessary to control it as a whole so as not to have a significant effect on the strength and permeability of concrete; second, raw materials are selected according to the suitability of various raw materials; if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related studies consider the effect of calcium content on the attachment of oyster larvae, but do not consider the performance of the concrete itself, and do not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of concrete will change the permeability of alkali and ions inside the concrete, and the lower the permeability of concrete, the higher the permeability of alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkali and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may be more serious, especially when the cement content is high. Therefore, it is necessary to ensure that the change in the permeability of the concrete by mixing the attractant into the concrete is within a controllable range, for example, the change does not exceed 10%, so that their attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect of oyster larvae cannot be evaluated.

[0137] It is necessary to grasp the optimum environment required for marine sessile organisms to attach, transform and grow later, and to design concrete starting from the seepage prevention of concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the seepage prevention of concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether one skilled in the art of concrete engineering or marine biology, according to the prior background, in the present invention, the overall control of the seepage prevention of concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0138] Increased roughness

[0139] Rough surfaces provide better tactile stimulation for oyster larvae to crawl and attach, increasing the attachment force and extending the residence time of oyster larvae on the substrate; at the same time, the presence of cracks and holes can protect the larvae and reduce the possibility of being attacked by predators, and the attachment rate of oyster larvae is improved on rough attachment substrates because the surface area available for attachment is larger than that on smooth attachment substrates.

[0140] Thus, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the ability to effectively attract oysters to attach and the high durability of concrete in the present invention, which are the color change by mixing dark color pigments into concrete, the modification of cow bone powder, the crushing technology, and the control of hydrogen carbonate and concrete permeability, according to References 1 to 3. Also, according to Reference 4, the reduction in concrete alkalinity and the balance of calcium ion concentration in the present invention cannot obtain the technical features closely related to the attachment of marine sessile organisms.

[0141] The implementation methods of Examples A1 to A14 are the same, and concrete oyster adhesion bases with different shapes are designed and manufactured, specifically see Figures 5 to 7. Their concrete mix ratios are as follows:

[0142] In Example A1, the mix ratio of ordinary Portland cement concrete is 29.37%, 33.53%, 24.48%, 12.59%, and 0.03% by weight of ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water, and polycarboxylate water-reducing agent powder, respectively.

[0143] Wherein, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite with a maximum particle size of less than 20mm. The lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, with a particle size of 0.2mm-5mm and high grade. The water needs to meet the quality standard for water for concrete (JGJ63-2006), with Cl- content <1000mg / L and PH value >4.5, and has little effect on the initial setting time difference and final setting time, strength and permeability of cement. In addition, the above materials selected in Examples A1-15 are the same.

[0144] Regarding the mix ratio of Example A2, the standard concrete, the weight percentages of ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water-reducing agent powder were 17.62%, 1.47%, 10.28%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0145] The weight percentages of Example A3, unmodified dark pigment, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0146] The weight percentages of Example A4, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0147] The weight percentages of Example A5, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0148] The weight percentages of Example A6, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.17%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0149] The modified dark pigment is 196 transparent resin, mixed with 3% hardener and 1.5% accelerator, and the volume ratio of pigment to resin is 1:0.2. It is cured at room temperature for 4 hours, then cured at 60℃ for 4 hours, and then crushed by beating and ground by vibration mill until the powder size exceeds 400 mesh.

[0150] In Example A7, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 0.87%, 17.62%, 1.36%, 9.52%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0151] In Example A8, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 17.62%, 1.29%, 8.99%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0152] In Example A9, the weight percentages of calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 17.62%, 1.17%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0153] The weight percentages of Example A10, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 0.87%, 17.62%, 1.18%, 8.23%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0154] The weight percentages of Example A11, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 1.47%, 17.62%, 1.10%, 7.71%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0155] The weight percentages of Example A12, modified dark pigment (mass ratio of iron black:aniline black mixture=1:1), calcium carbonate powder, ordinary Portland cement, silica fume, blast furnace slag powder, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 1.47%, 2.35%, 17.62%, 0.99%, 6.94%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0156] The weight percentages of Example A13, calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 0.5%, 1.47%, 17.62%, 0.93%, 6.50%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0157] The weight percentages of Example A14, calcium carbonate powder, zinc sulfate, modified dark pigment (iron black:aniline black mixture in a mass ratio of 1:1), ordinary Portland cement, blast furnace slag powder, silica fume, lightweight coarse aggregate, lightweight fine aggregate, water and polycarboxylate water reducer powder are 2.35%, 1.2%, 1.47%, 17.62%, 0.84%, 5.89%, 33.53%, 24.48%, 12.59%, and 0.03%, respectively.

[0158] The preparation method of modified zinc sulfate is as follows: Select diatomaceous earth with SiO2 content >90% and fineness of 600 mesh, add 150g water in a mixer at 60°C, then add 100g zinc sulfate, stir until completely dissolved, and prepare for use; then heat 150g of the above diatomaceous earth to 60°C, add it into the solution, stir for 10 minutes in a mixer with a rotation speed of 200-500 revolutions / min, and then dry in a drying oven with a drying temperature of 100°C to obtain modified zinc sulfate.

[0159] The specific operation steps of the method of carrying out Examples A1 to A14 are as follows:

[0160] According to the above-mentioned lightweight concrete oyster attachment base manufacturing method, three Φ100×50mm cylindrical specimens and ten 200×200×30mm rectangular specimens are manufactured, which are respectively used to test the concrete's 28-day chloride ion penetration resistance and the oyster larvae attachment and transformation situation in the laboratory after 28 days of standard curing. The specific operation steps are as follows:

[0161] (1) Formation of specimen

[0162] 1. Calculate and accurately weigh out ordinary Portland cement, lightweight coarse aggregate, lightweight fine aggregate, water, dark color pigment, calcium carbonate powder, trace elements and polycarboxylate water reducer powder according to the above mass.

[0163] 2. First, put the lightweight coarse aggregate and lightweight fine aggregate into a concrete mixer and mix for 0.5 to 1 minute. Then add Portland cement, calcium carbonate powder, trace elements, and dark pigment and continue to mix for 0.5 to 1 minute. Next, add water and superplasticizer and mix for 2 to 6 minutes. After uniform mixing, pour, vibrate, and cut into molds to produce three cylindrical specimens with a diameter of 100 x 50 mm and five rectangular specimens with a diameter of 200 x 200 x 30 mm. Finally, put them into a standard curing chamber to cure for 28 days, and perform the corresponding permeability evaluation for each age. After 28 days, conduct the adhesion and metamorphosis test of oyster larvae in the laboratory.

[0164] (II) The specific steps of the rapid chloride ion permeability test are as follows:

[0165] According to the standard "Standard Test Method for Electrical Indication of Concrete's Ability to Resist Chloride Ion Penetration" (ASTM1202-2017), when curing for 28 days, take out three cylindrical specimens of Φ100×50mm from the curing chamber, and clean the water and impurities on their surfaces. After the surfaces are dried, apply a thin layer of epoxy to the surface of the cylindrical specimen. Then, place the specimen in a vacuum saturator for 20-24 hours. Then, take out the specimen, clean its surface, and place it in an organic glass mold. At the same time, detect the sealing between the specimen and the mold, and then put a 3% sodium chloride solution (electrode is connected to the negative pole of the power supply) and a 0.3 mol / L sodium hydroxide solution (electrode is connected to the positive pole of the power supply) into the mold on both sides. Then start the experimental equipment, and after 6 hours, record the test data, and repeat the above operations for the last two specimens. Finally, calculate the strength according to the norm.

[0166] (3) The specific steps of the laboratory oyster larvae attachment and metamorphosis test are as follows:

[0167] After 28 days of standard curing, the rectangular specimens of 200×200×30 mm are taken out of the curing room, and the water and impurities on their surfaces are washed off, and then they are placed in a test pond. A test pond is created in the laboratory, and the amount of oyster larvae is 0.85 ind / ml3. The seawater in the pond is sand-filtered seawater from the Yellow Sea, and the salinity is about 32% to 34%. After the seawater level is higher than the concrete specimens, oxygen pipes are evenly arranged in the test pond to prepare for throwing the oyster larvae. After slowly stirring the oyster larvae in the bucket, a beaker is used to accurately measure the mass of the seawater containing the oyster larvae, and then the mass is evenly thrown into the test pond. After the oyster attachment attraction test began, the seawater in the test pond was replaced every day, with the amount of water replaced being 1 / 3 of the total capacity of the test pond. A screen (200 mesh or more) was used to block the drainage outlet to prevent unattached oyster larvae from being washed away with the water. The larvae on the screen were then thrown back into the test pond. Chlorella was fed at regular intervals and in quantitative amounts using a Pasteur pipette at 9:00 and 19:00 every day, and the attachment situation of the oysters was observed.

[0168] After the test was continued for 30 days, the water in the test pond was drained, the test specimens were taken out, and the number and survival rate of oysters on the surface of the test specimens were counted, recorded and analyzed. For the statistics, the smooth bottom surface was used when pouring and molding the concrete.

[0169] Compared to Reference 3 (Fan Ruiliang: The effects of substrate type on oyster attachment, growth, population establishment and reef development [D]), the differences are as follows:

[0170] In Reference 3, 80 mesh cow bone powder, calcium powder, and gypsum powder are taken and mixed into concrete separately. The fineness of the calcium materials mixed in the present invention is all above 200 mesh, which is larger than the fineness of the materials in Reference 3. The purpose is to fully exert the attraction ability of the concrete particles while taking into account their grading.

[0171] In the examples, concrete is prepared using 600 mesh calcium carbonate powder, which has a high fineness and has almost no effect on the concrete performance after being mixed into the concrete. The calcium carbonate powder can be well dispersed inside the concrete, thereby increasing the adhesion rate of the attracted oyster larvae.

[0172] As can be seen from the references and the materials examined, calcium content is essential for the attachment of oyster larvae, and some current test results also prove that adding an appropriate amount of calcium carbonate material to cement-based materials can promote the attachment and growth of oyster larvae. However, cement concrete contains a large amount of calcium ions, and the pH value of the pore solution is generally above 12.5, and at room temperature, the pH value of saturated calcium hydroxide solution is about 12, so the calcium ion concentration in the concrete pore solution is about 5 mmol / L, and the solubility of calcium carbonate is very low, at 25°C, it is 9.5×10 -5 mol / L(9.5×10 -2 Currently, the optimal range of calcium ion concentration for attracting oysters to attach is thought to be 10-25 mmol / L, and even when oyster larvae are placed in a saturated calcium carbonate solution, there is not enough Ca to provide the ion concentration suitable for oyster attachment. 2+ Furthermore, while Ca(OH)2 in cement concrete can be released quickly, it takes time for calcium carbonate to dissolve. Therefore, when calcium carbonate material is added to concrete to promote the attachment of oyster larvae, Ca 2+ It can be determined that HCO3 does not play a dominant role. - In the case of transformation, Ca 2+ Together with the calcium carbonate, a secondary shell of calcium carbonate is formed. After calcium carbonate is mixed in, it reacts with CO2 and water to generate Ca(HCO3)2, which is involved in adhesion and is the basic mechanism that promotes the adhesion of oyster larvae.

[0173] There is an optimal amount of calcium carbonate for cement-based materials, which can be explained by the following three aspects:

[0174] 1) With the same amount of substitute cement, as the dosage of calcium carbonate increases, the alkali in the concrete is diluted and the total alkalinity decreases. However, as the dosage of calcium carbonate increases, the probability of dissolving calcium carbonate in the concrete increases, and the amount of HCO3 in the solution increases. - The content is improved, which promotes the adhesion and transformation of oysters. However, if the dosage is too large, the permeability of the concrete will increase rapidly, the alkali and carbonate in the concrete will be rapidly leached, the adverse effect of the alkali will become obvious, and the critical effect or adverse effect of the carbonate will begin to appear, so the adhesion will decrease,

[0175] 2) With the same amount of substitute aggregate, the permeability of concrete decreased with increasing dosage, and the calcium ions and OH - The leaching of calcium ions decreased, but the permeability of carbonate ions gradually improved and reached a certain value, and the attachment of oysters reached its maximum value. As the dosage continued to increase, the calcium ions decreased significantly, and carbonates may also decrease. The calcium ion concentration limited the attachment of oyster larvae, which was manifested as a decrease in the attachment amount.

[0176] 3) With the same amount of alternative mineral admixture, the permeability improved with increasing dosage, and the increase in calcium carbonate reduced the amount of HCO3 required for oyster attachment. - As the concentration reaches the appropriate range, which is manifested as improved oyster larval attachment, and the mineral admixture dosage continues to increase, the mineral admixture dosage decreases, and the amount of leached alkali and carbonate increases, but the alkali and HCO3 - Too many ions inhibit the attachment of oyster larvae.

[0177] Compared to Reference 4 (Li Zhenzhen, Gong Pihai, Guan Changtao, et al. Bioadhesion effect of concrete artificial reefs with different cement types [J]. Progress in Fisheries Science, 2017, 38(5):57-63.), the differences are as follows:

[0178] In Reference 4, composite Portland cement, slag Portland cement, pozzolanic Portland cement, fly ash Portland cement and alumina cement are used, and in the present invention, ordinary Portland cement is mixed with mineral admixtures to realize low alkalinity segments, where silica fume is one of the mineral admixtures, which has high activity and appropriate dosage has obvious effect on improving the durability of reinforced concrete in marine environment, and low alkalinity cement with excellent strength and durability can be obtained through optimization design and testing. At the same time, due to the high penetration prevention characteristics of silica fume concrete, even if the alkalinity inside the concrete is high, a large number of oyster larvae can attach, transform and grow. In addition, the low alkalinity sulfoaluminate cement is mixed to adjust the alkalinity of cement concrete and provide a suitable pH value for the attachment of oyster larvae. In addition, marine plants and sessile organisms such as oysters and barnacles have different alkali tolerances, and the environments required during the attachment and later stages are different. For example, the attachment, metamorphosis and later growth of barnacles and oysters require large amounts of calcium ions.

[0179] In Reference 4, concrete is used to attract marine organisms, which mainly starts from the size and diversity of the attached organisms, the main attached organisms being various algae. In the present invention, the research objective is to attract oysters to attach, but the alkali resistance of oysters and barnacles is higher than that of algae, and the attachment and transformation of oysters requires a large amount of calcium ions, so although the two types of concrete look similar, they are actually quite different. Figures 3 and 8 respectively show a comparison of the biofouling situation after about 210 days of actual sea attachment experiments in Reference 4 and the biofouling situation after 300 days of actual sea attachment experiments in the present invention.

[0180] The unique features and beneficial effects of the present invention are as follows:

[0181] Deep color pigment

[0182] Taking advantage of the phototaxis of oyster eyespot larvae, dark color pigments (one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red) are modified and then mixed into concrete to change the color of the concrete, making the concrete darker and making the oyster larvae think that it is a dark environment, attracting the oyster larvae to reach the dark concrete surface by themselves, increasing the probability of contact between the oyster larvae and the concrete surface, and increasing the probability of attracting the oyster larvae to attach. Specifically, it is as follows.

[0183] Marine biology researchers have studied the attachment of marine sessile organisms using different colored substrates to breed and grow or eliminate undesirable populations, which belongs to the field of marine biology. It is completely different from marine concrete engineering and concrete materials science, which are two major fields entirely. Through the interdisciplinary fusion of marine sessile organisms and concrete materials science, dark colored concrete is used to attract oyster larvae to attach. The present invention adds dark color pigments to darken the color of the concrete surface and promote the attachment of oyster larvae. Since other materials are mixed into the concrete, it affects the concrete performance. The present invention considers that concrete with different cements has different surface colors. Therefore, the dosage of the dark color material is determined based on the cement type and dosage. The dark color pigment also affects the concrete performance. Most importantly, the dark color pigment is mixed in while simultaneously reducing the alkali and Ca in the concrete. 2+ If the permeability of concrete is not controlled, the released alkali will affect the attachment, metamorphosis and growth of sessile organism larvae, and if the dosage exceeds a certain value, the amount of larvae attachment will decrease. In the present invention, the permeability prevention of concrete is designed and controlled, and the main measures are the selection of the type of dark color pigment, the control of the dosage and modification. With the increase in the dosage of dark color material, the amount of larvae attachment will increase, and when the dosage is 0.5%-6% of the cementitious material, the amount of larvae attachment is the highest, and then increases slightly or remains unchanged.

[0184] trace elements

[0185] The oyster body contains a large amount of zinc, much higher than the seawater in which it lives, and at the same time, the oyster body contains a lot of Fe, P, and K elements. At the same time, adequate Zn in the solution 2+ and K + The concentration can promote the early attachment and metamorphosis of oyster larvae. Therefore, zinc sulfate, potassium sulfate, potassium nitrate, iron sulfate, zinc phosphate, ammonium nitrate, potassium phosphate, ammonium phosphate, iron phosphate, and calcium phosphate are used as trace elements and mixed into concrete, and the modification of these substances basically does not change the strength and penetration prevention properties of the concrete, but greatly improves the attachment attraction rate of oyster larvae. The details are as follows:

[0186] Marine biology researchers have studied the effects of different ions on the attachment and metamorphosis of marine sessile organisms, which belongs to the field of marine biology, in order to clarify the attachment mechanism of oysters and the purpose of their reproduction and proliferation. It is completely different from marine concrete engineering and concrete materials science, which are completely two major fields. It can be seen that the interdisciplinary fusion of marine sessile organisms and concrete materials science can add corresponding substances into concrete to attract oyster larvae to attach to the concrete surface. Since soluble salts have a great impact on concrete performance such as early workability, hardening time, and later strength and anti-permeability, the present invention uses diatomaceous earth as a carrier to fix these inorganic salts inside diatomaceous earth, reducing the impact of soluble salts on concrete performance, while utilizing the effect of diatomaceous earth in improving concrete performance, and realizes that even if these attractants are added, the excellent mechanical properties and anti-permeability of concrete can be maintained. In addition, since diatomaceous earth has a sustained release effect as a carrier, the release of soluble salts is relatively slow, and the release rate is kept at a very low level, especially after immersion in seawater for a certain period of time. Therefore, similarly, this part of knowledge relates to the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether a person skilled in the field of concrete engineering or a person skilled in the field of marine biology, due to the conventional background, cannot obtain technical characteristics closely related to concrete with excellent ability to attract oyster larvae to attach in the present invention by mixing trace elements into concrete, changing the ion content of trace elements on the concrete surface, and controlling the permeability of the concrete.

[0187] Permeability of concrete

[0188] The strength and permeability of concrete are the two most important performances of concrete. Adding different attractants into standard concrete will affect the performance of concrete, so when mixing different substances to promote the attachment, metamorphosis and subsequent growth of oyster larvae, first, it is necessary to control it as a whole so as not to have a significant effect on the strength and permeability of concrete; second, raw materials are selected according to the suitability of various raw materials; if the performance of the raw materials cannot meet the actual requirements, the desired function can be achieved by modifying them before adding the raw materials. However, in fact, the above-mentioned related studies consider the effect of calcium content on the attachment of oyster larvae, but do not consider the performance of the concrete itself, and do not consider the water-cement ratio, calcium content and curing, etc., and the change in the permeability of concrete will change the permeability of alkali and ions inside the concrete, and the lower the permeability of concrete, the higher the permeability of alkali and ions inside it will be, which may increase exponentially. Therefore, these released alkali and ions have a great impact on the larvae, changing from promoting attachment to inhibiting attachment, and this situation may be more serious, especially when the cement content is high. Therefore, it is necessary to ensure that the change in the permeability of the concrete by mixing the attractant into the concrete is within a controllable range, for example, the change does not exceed 10%, so that their attractant effects can be compared, otherwise the influence of mixing the attractant independently or mixing the attractants in combination on the attractant effect of oyster larvae cannot be evaluated.

[0189] It is necessary to grasp the optimum environment required for marine sessile organisms to attach, transform and grow later, and to design concrete starting from the seepage prevention of concrete, and not to ignore the fact that only considering the dosage of various raw materials will bring about changes in the seepage prevention of concrete. Therefore, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, chemistry and marine concrete engineering, and whether one skilled in the art of concrete engineering or marine biology, according to the prior background, in the present invention, the overall control of the seepage prevention of concrete cannot obtain the technical characteristics that are closely related to the ability of the attractant to effectively attract oysters to attach.

[0190] By using lightweight aggregate concrete, the present invention can reduce the weight of the concrete attachment base, and reduce transportation costs and labor costs in the processes of manufacturing, transporting, and curing the test specimens.In addition, in actual sea farming, it can reduce the labor costs of fishermen who move the attachment base to harvest oysters, and reduce costs such as transportation and fixing when applied to marine concrete projects.Furthermore, it can reduce the risk of accidentally falling to the ground and being damaged during use.

[0191] Thus, similarly, this part of knowledge concerns the interdisciplinary fusion of marine sessile organisms, marine plants, and marine concrete engineering, and neither a person skilled in the field of concrete engineering nor a person skilled in the field of marine biology can obtain the technical features closely related to the ability to effectively attract oysters to attach and the high durability of concrete, as shown in Reference 3, by mixing dark color pigments into concrete and controlling the permeability of concrete by mixing calcium carbonate powder and trace elements in the present invention. Also, as shown in Reference 4, the reduction in alkalinity of concrete and the balance of calcium ion concentration in the present invention cannot obtain the technical features closely related to the attachment of marine sessile organisms.

[0192] Although embodiments of the present invention will be shown and described, it will be understood that those skilled in the art can make various changes, modifications, substitutions and variations to these embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the claims and their equivalents.

Claims

1. A Portland cement concrete oyster adhesion base, comprising Portland cement, mineral admixture, coarse aggregate, sand, water, dark pigment, bio-calcium powder, carbonate or bicarbonate, and superplasticizer, the weight percentages of Portland cement, mineral admixture, coarse aggregate, sand, water, dark pigment, bio-calcium powder, carbonate or bicarbonate, and superplasticizer being 9.0% to 17.0%, 4.0% to 11.5%, 38.4% to 47.8%, 24.9% to 37.3%, 6.2% to 9.0%, 0.3% to 2.0%, 0.3% to 2.0%, 0.3% to 1.5%, and 0.02% to 0.1%, respectively; The mineral admixture comprises a combination of one or more of silica fume, slag, and fly ash; The deep color pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red; The bio-calcium powder includes cow bone powder and bio-calcium carbonate powder, and the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder, and the fineness of the bio-calcium powder is 100 mesh to 1000 mesh.

2. The Portland cement concrete oyster-attached base according to claim 1, characterized in that the bio-calcium powder is prepared by treating 100 mesh to 500 mesh oyster shell powder, eggshell powder, coral powder, and fish bone powder with one or two of ethanoic acid, acetic acid, silicic acid, and sulfurous acid, and treating 100 mesh to 500 mesh cow bone powder with one or two of diluted phosphoric acid, sulfuric acid, hydrochloric acid, and nitric acid.

3. The Portland cement concrete oyster adhesion base according to claim 1, characterized in that the carbonate or bicarbonate is one or more of sodium carbonate, potassium carbonate, calcium bicarbonate, sodium bicarbonate, and potassium bicarbonate, and the carbonate or bicarbonate is modified and used as a carrier to achieve sustained release of corresponding ions after being combined with one or more of sodium carbonate, potassium carbonate, calcium bicarbonate, sodium bicarbonate, and potassium bicarbonate, thereby reducing or eliminating the adverse effects on concrete performance.

4. A method for producing a Portland cement concrete oyster-attached base, comprising: Step S1: Design different roughness according to the preferred characteristics of oyster larvae to attach to rough surfaces, and then manufacture molding forms with different roughness; Portland cement, mineral admixture, coarse aggregate, sand, water, dark pigment, bio-calcium powder, modified carbonate or bicarbonate, and superplasticizer are precisely weighed, and the weight percentages of Portland cement, mineral admixture, coarse aggregate, sand, water, dark pigment, bio-calcium powder, carbonate or bicarbonate, and superplasticizer are 9.0% to 17.0%, 4.0% to 11.5%, 38.4% to 47.8%, 24.9% to 37.3%, 6.2% to 9.0%, 0.3% to 2.0%, 0.3% to 2.0%, 0.3% to 1.5%, and 0.02% to 0.1%, respectively, and the mineral admixture comprises one or more combinations of silica fume, slag, and fly ash; Step S2: the dark pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red; the bio-calcium powder includes cow bone powder and bio-calcium carbonate powder; the bio-calcium carbonate powder includes one or more combinations of oyster shell powder, fish bone powder, eggshell powder, and coral powder; the fineness of the bio-calcium powder is 100 mesh to 1000 mesh; the modified carbonate or bicarbonate is compounded with one or more of sodium carbonate, potassium carbonate, calcium bicarbonate, sodium bicarbonate, and potassium bicarbonate using diatomaceous earth as a carrier; First, put the coarse aggregate and sand into the concrete mixer and mix for 0.5-1 minute, then add Portland cement, mineral admixture, dark pigment, bio-calcium powder, and modified carbonate or bicarbonate and mix for another 1-2 minutes, then add water and superplasticizer and mix for 2-6 minutes, and then mix evenly, then pour and vibrate in step S3; Step S4: immediately place the concrete specimen into a high-concentration CO2 curing box and cure for 0.5 to 5 hours to reduce the alkalinity of the cement specimen; and then cure for 28 days according to standard curing or curing according to actual conditions. This method is characterized in that it is possible to produce a Portland cement concrete oyster attachment base with excellent attracting effect.

5. A Portland cement concrete oyster adhesion base comprising a dark pigment, Portland cement, a mineral admixture, crushed stone, sand, water, and a superplasticizer, the weight percentages of the dark pigment, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer being 0.3-2.0%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively, the mineral admixture including one or more combinations of silica fume, slag, and fly ash, and the dark pigment being one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

6. A Portland cement concrete oyster attachment base comprising: powdered cow bone, Portland cement, a mineral admixture, crushed stone, sand, water, and a superplasticizer; the weight percentages of the powdered cow bone, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer are 0.3-2.0%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively; and the mineral admixture includes one or more combinations of silica fume, slag, and fly ash.

7. A Portland cement concrete oyster adhesion base comprising a dark pigment, a carbonate or bicarbonate, Portland cement, a mineral admixture, crushed stone, sand, water, and a superplasticizer, the weight percentages of the dark pigment, carbonate or bicarbonate, Portland cement, mineral admixture, crushed stone, sand, water, and superplasticizer being 0.3-2.0%, 0.3-1.5%, 9.0%-17.0%, 4.0%-11.5%, 38.4%-47.8%, 24.9%-37.3%, 6.2%-9.0%, and 0.02%-0.1%, respectively, the mineral admixture including one or more combinations of silica fume, slag, and fly ash, and the dark pigment being one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

8. The composition is composed of a cementitious material, a lightweight coarse aggregate, a lightweight fine aggregate, water, a dark pigment, a calcium carbonate powder, a trace element and a superplasticizer, and the weight percentages of the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water, the dark pigment, the calcium carbonate powder, the trace element and the superplasticizer are respectively 22.0% to 35.0%, 25.0% to 38.0%, 16.0% to 30.0%, 8.5% to 16.5%, 0.6% to 3.0%, 0.6% to 3.0%, 0.2% to 1.8% and 0.03% to 0.03%. 18%, the lightweight coarse aggregate is one or two of crushed lightweight porous basalt and lightweight ceramsite, the maximum particle size of which is less than 20 mm, the lightweight fine aggregate is one or two of crushed zeolite and lightweight ceramic sand, the particle size of which is 0.2 mm to 5 mm, the trace elements are zinc, iron, potassium or phosphorus, and the following are examples of the trace elements: zinc sulfate, calcium phosphate, zinc phosphate, potassium sulfate, potassium nitrate, iron sulfate, ammonium nitrate , potassium phosphate, ammonium phosphate, and iron phosphate, the dark pigment being one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red, the cementitious material being one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, the Portland cement mixed with mineral admixtures comprising a combination of one or more of silica fume, slag powder, and fly ash, the sulfoaluminate cement comprising one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material comprising one of alkali-activated slag and alkali-activated slag + fly ash.

9. The calcium carbonate powder is one or more of calcite, chalk, limestone, marble, aragonite, travertine powder, light calcium carbonate, activated calcium carbonate, calcium carbonate whiskers, and ultrafine light calcium carbonate, and its fineness is more than 200 mesh. The lightweight concrete oyster adhesion base according to claim 8.

10. The oyster adhesion base is composed of a dark pigment, a cementitious material, a lightweight coarse aggregate, a lightweight fine aggregate, water and a superplasticizer, the weight percentages of the dark pigment, the cementitious material, the lightweight coarse aggregate, the lightweight fine aggregate, the water and the superplasticizer being 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively, the lightweight coarse aggregate being one or two of crushed lightweight porous basalt and lightweight ceramsite having a maximum particle size of less than 20 mm, the lightweight fine aggregate being one or two of crushed zeolite and lightweight ceramic sand having a particle size of 0.2 mm-5 mm, the cementitious material being one or two of crushed lightweight porous basalt and lightweight ceramsite having a maximum particle size of less than 20 mm, the lightweight fine aggregate being one or two of crushed zeolite and lightweight ceramic sand having a particle size of 0.2 mm-5 mm, The material is one of Portland cement mixed with mineral admixtures, sulfoaluminate cement, and alkali-activated cementitious material, wherein the Portland cement mixed with mineral admixtures includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag, and alkali-activated slag + fly ash, the lightweight concrete oyster attachment base.

11. The oyster attachment base is composed of calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and a superplasticizer, the weight percentages of the calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer being 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively, the lightweight coarse aggregate being one or two of crushed lightweight porous basalt and lightweight ceramsite having a maximum particle size of less than 20 mm, the lightweight fine aggregate being one or two of crushed zeolite and lightweight ceramic sand having a particle size of 0.2 mm-5 mm, The cementitious material is one of Portland cement mixed with mineral admixture, sulfoaluminate cement, and alkali-activated cementitious material, wherein the Portland cement mixed with mineral admixture includes one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement includes one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, and the alkali-activated cementitious material includes one of alkali-activated slag, and alkali-activated slag + fly ash.

12. The oyster attachment base is composed of a dark pigment, calcium carbonate powder, a cementitious material, a lightweight coarse aggregate, a lightweight fine aggregate, water and a superplasticizer, the weight percentages of the dark pigment, calcium carbonate powder, cementitious material, lightweight coarse aggregate, lightweight fine aggregate, water and superplasticizer being 0.6-3.0%, 0.6-3.0%, 22.0%-35.0%, 25.0%-38.0%, 16.0%-30.0%, 8.5%-16.5% and 0.03%-0.18%, respectively, the lightweight coarse aggregate being one or two of crushed lightweight porous basalt and lightweight ceramsite having a maximum particle size of less than 20 mm, the lightweight fine aggregate being one or two of crushed zeolite and lightweight ceramic sand having a particle size of 0.2 mm-5 mm, the cementitious material being porous aggregate mixed with a mineral admixture. A lightweight concrete oyster-attached base, characterized in that the base is one of Rutland cement, sulfoaluminate cement, and alkali-activated cementitious material, in which the Portland cement mixed with mineral admixtures comprises one or more combinations of silica fume, slag powder, and fly ash, the sulfoaluminate cement comprises one or two of fast-setting sulfoaluminate cement, high-strength sulfoaluminate cement, and expanded sulfoaluminate cement, the alkali-activated cementitious material comprises one of alkali-activated slag, and alkali-activated slag + fly ash, and the dark pigment is one or two of iron black, aniline black, carbon black, antimony sulfide, red iron oxide, and organic pigment red.

Citation Information

Patent Citations

  • Novel concrete artificial fish reef and preparation method thereof

    CN104529286A

  • Bionic concrete artificial fish reef and preparation method thereof

    CN104938384A

  • Mortar for inducing sessile organisms on underwater oceanographic engineering surface and preparation method

    CN111499290A

  • Precast concrete block for artificial fish reef, production of precast concrete block for artificial fish reef, and use of precast concrete block for artificial fish reef