Slurry, method for producing slurry, method for producing spherical particles, and spherical particles

A slurry with negatively charged dispersants and particles addresses rapid precipitation issues, enabling stable, high-concentration dispersion and production of spherical particles with controlled composition using FD-POEM.

JP7580715B2Active Publication Date: 2024-11-12TOHOKU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020180009
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-27
Publication Date
2024-11-12
Estimated Expiration
2040-10-27

AI Technical Summary

Technical Problem

Conventional slurries disperse particles in pure water, leading to rapid precipitation within tens of minutes and limiting the concentration of dispersed particles.

Method used

A slurry containing a negatively charged dispersant and negatively charged particles, stabilized by repulsive forces, allowing for long-term dispersion and higher concentrations, produced using a freeze-drying pulsed pressure applied orifice method (FD-POEM).

Benefits of technology

The slurry stabilizes particle dispersion for extended periods and enables higher concentrations, producing spherical particles with reduced voids and controlled composition through varying particle ratios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580715000002
    Figure 0007580715000002
  • Figure 0007580715000003
    Figure 0007580715000003
  • Figure 0007580715000004
    Figure 0007580715000004
Patent Text Reader

Abstract

To provide slurry capable of stably dispersing particles for a relatively long time and dispersing the particles even at a higher concentration, a method for producing slurry, and a method for producing spherical particles utilizing the slurry.SOLUTION: A liquid is added with: a dispersant negatively charged in the liquid; and one or plural kinds of particles negatively charged in the liquid. The dispersant may be made of nanobubbles for example.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a slurry, a method for producing a slurry, a method for producing spherical particles, and spherical particles. [Background technology]

[0002] Conventionally, slurries in which particles are dispersed in liquid have been used in various fields such as inks, paints, foods, cosmetics, etc. Moreover, slurries are generally prepared by dispersing particles in pure water (see, for example, Patent Documents 1 and 2).

[0003] The slurry is also used as a raw material for producing monodisperse particles by using the so-called pulsated orifice ejection method (POEM) (see, for example, Patent Documents 3 to 5). This POEM method can produce particles with a uniform particle size of several tens to several hundreds of μm. The inventors of the present invention have also developed a freeze-dry pulsated orifice ejection method (FD-POEM) that is an extension of this POEM method (see, for example, Non-Patent Document 1). This FD-POEM method is a method in which slurry droplets containing metal particles or ceramic particles are dropped from a liquid vibrator, the droplets are frozen in liquid nitrogen, and the droplets are freeze-dried to obtain monodisperse particles. This FD-POEM method can obtain spherical particles by utilizing the surface tension of the liquid. In addition, by preparing a slurry in which the mixture ratio of multiple types of particles in the slurry is changed, the composition of the spherical particles to be produced can be freely controlled. The produced spherical particles can be used as raw materials for additive manufacturing. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-110201 A [Patent Document 2] JP 2020-50534 A [Patent Document 3] JP 2002-155305 A [Patent Document 4] JP 2004-182477 A [Patent Document 5] JP 2006-126776 A [Non-patent literature]

[0005] [Non-Patent Document 1] Naoyuki Nomura, Weiwei Zhou, Zhenxing Zhou, Kyosuke Yoshimi, "Attempt at Laser 3D Additive Manufacturing of Ultra-High Temperature Resistant MoSiBTiC Alloy", Ceramics, 2020, 55, No.2, pp.90-92 Summary of the Invention [Problem to be solved by the invention]

[0006] The slurries described in Patent Documents 1 and 2 have a problem in that particles dispersed in pure water settle in a short time, for example, within several tens of minutes, and therefore have a problem in that the particle concentration cannot be increased.

[0007] The present invention has been made with a focus on such problems, and has an object to provide a slurry that can stably disperse particles for a relatively long period of time and can disperse particles even at higher concentrations, a method for producing the slurry, a method for producing spherical particles using the slurry, and spherical particles. [Means for solving the problem]

[0008] In order to achieve the above object, a slurry according to the present invention is characterized in that it contains a negatively charged dispersant and one or more types of negatively charged particles in a liquid.

[0009] The method for producing a slurry according to the present invention is characterized in that a dispersant that is negatively charged in the liquid and one or more types of particles that are negatively charged in the liquid are added to a liquid.

[0010] The slurry according to the present invention can be suitably manufactured by the manufacturing method of the slurry according to the present invention. The slurry according to the present invention contains a dispersant and particles, both of which are negatively charged, in the liquid, so that the dispersant and each particle, and each particle repel each other in the liquid. Therefore, each particle is less likely to gather, and each particle is less likely to float and settle. As a result, the slurry according to the present invention can stably disperse particles for a long time compared to a slurry in which at least one of the dispersant and each particle is not negatively charged. In addition, the particles can be dispersed even at a higher concentration.

[0011] In the slurry and the method for producing the slurry according to the present invention, each particle may be any particle that is negatively charged in the liquid. Each particle may be, for example, a metal particle or a non-metal particle. Also, each particle may have, for example, a particle made of Mo, a particle made of Si, a particle made of TiC, and a particle made of MoB. It is preferable that the slurry and the method for producing the slurry according to the present invention do not contain a dispersant or particles that are positively charged in the liquid of the slurry.

[0012] In the slurry and the method for producing the slurry according to the present invention, the dispersant may be any material that is negatively charged in the liquid. The dispersant may be, for example, oxidized carbon nanotubes (CNTs) or nanobubbles consisting of minute bubbles with a size of 1 μm or less.

[0013] The method for producing spherical particles according to the present invention is characterized in that droplets of the slurry according to the present invention are dropped, the droplets are frozen, and then freeze-dried to obtain spherical particles.

[0014] According to the method for producing spherical particles of the present invention, it is possible to obtain spherical particles having each component of the particles contained in the slurry. In addition, the ratio of voids contained in the obtained spherical particles can be reduced to 10% or less. In addition, the composition of the obtained spherical particles can be controlled by changing the mixing ratio of multiple types of particles in the slurry. For example, when each particle is composed of particles made of Mo, particles made of Si, particles made of TiC, and particles made of MoB, it is possible to produce spherical particles of Mo-Si-B-TiC alloy (nominal composition is Mo-5Si-10B-10TiC (mol.%)).

[0015] The method for producing spherical particles according to the present invention preferably uses a freeze-drying pulsed pressure-added orifice method (FD-POEM method) to obtain the spherical particles from the slurry, and for example, it is preferable to drip the liquid droplets using a liquid vibrator and freeze the droplets in liquid nitrogen. The slurry according to the present invention is not limited to being used as a raw material for spherical particles, and can also be used for inks, paints, foods, cosmetics, etc. by adjusting the composition.

[0016] The spherical particles according to the present invention are characterized in that they are made of a Mo-Si-B-TiC alloy and contain voids at a rate of 10% or less.

[0017] The spherical particles according to the present invention can be suitably produced by the method for producing a slurry according to the present invention. The spherical particles according to the present invention may contain voids in a ratio of 8% or less, 4% or more, or 5% or more. Effect of the Invention

[0018] According to the present invention, it is possible to provide a slurry that can stably disperse particles for a relatively long period of time and can disperse particles even at higher concentrations, a method for producing the slurry, a method for producing spherical particles using the slurry, and spherical particles. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is an explanatory diagram showing a slurry manufacturing method according to an embodiment of the present invention, in which (a) is an oblique view showing the state in which particles to be dispersed are placed in a container, (b) is an oblique view showing the state in which a liquid and a dispersant are placed in the container and stirred, and (c) is an explanatory diagram showing the state of the dispersant and each particle in the liquid. [Diagram 2] 1 is a graph showing the change over time in zeta potential of nanobubbles, which are a dispersant, in water in the manufacturing method of a slurry according to an embodiment of the present invention. [Diagram 3] 1A and 1B are electron microscope photographs of spherical particles produced by a method for producing a slurry according to an embodiment of the present invention, using pure water containing no dispersant and slurries with concentrations of (a) 5 vol% and (b) 8 vol%. [Figure 4] 1A to 1C are electron microscope photographs of spherical particles produced by a method for producing a slurry according to an embodiment of the present invention, using water containing nanobubbles and slurries with concentrations of (a) 5 vol%, (b) 15 vol%, and (c) 20 vol%. [Diagram 5] 4(c) is a graph showing the particle size distribution of the spherical particles of FIG. 4(c), (a) the spherical particles of FIG. 3(a), (b) the spherical particles of FIG. 4(b), and (c) the spherical particles of FIG. 4(c). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described with reference to the drawings and examples. 1 to 5 show a slurry, a method for producing the slurry, a method for producing spherical particles, and spherical particles according to an embodiment of the present invention. In the method for producing a slurry according to an embodiment of the present invention, a dispersant that is negatively charged in a liquid and one or more types of particles that are negatively charged in the liquid are added to a liquid and stirred.

[0021] In a specific example shown in FIG. 1, first, particles 11a, 11b, and 11c to be dispersed are placed in a container 1 (see FIG. 1(a)). Here, three types of particles 11a, 11b, and 11c are placed, but the type of particles may be one type, two types, or four or more types. Next, a liquid and a dispersant are placed in the container 1 and stirred (see FIG. 1(b)). Here, nanobubbles are used as the dispersant, and water 12 containing nanobubbles is placed in the container 1. The dispersant is not limited to nanobubbles, and any dispersant that is negatively charged in the liquid, such as oxidized carbon nanotubes (CNT), may be used. In addition, any method may be used for stirring, and for example, stirring may be performed using a stirring blade 2 or ultrasonic vibration.

[0022] In this manner, the method for producing a slurry according to an embodiment of the present invention can produce a slurry according to an embodiment of the present invention, which contains a negatively charged dispersant and one or more types of negatively charged particles in a liquid.

[0023] Since the slurries according to the embodiments of the present invention contain negatively charged dispersants and particles in the liquid, as shown in FIG. 1(c), the nanobubbles 12a of the dispersant and the particles 11a, 11b, and 11c, and the particles 11a, 11b, and 11c themselves repel each other in the liquid (see the double-headed arrows in FIG. 1(c)). Therefore, the particles 11a, 11b, and 11c are less likely to gather together, and the particles 11a, 11b, and 11c are less likely to float and settle. As a result, the slurries according to the embodiments of the present invention can stably disperse particles for a long time compared to those in which at least one of the dispersants and the particles is not negatively charged. In addition, the particles can be dispersed even at a higher concentration.

[0024] In the slurry and the method for producing the slurry according to the embodiment of the present invention, the particles may be any particles that are negatively charged in the liquid. The particles may be, for example, metal particles or non-metal particles.

[0025] The method for producing spherical particles according to the embodiment of the present invention is a slurry freeze-drying pulsed pressure-added orifice method (FD-POEM method) according to the embodiment of the present invention, which can obtain spherical particles using the slurry according to the embodiment of the present invention. That is, droplets of the slurry according to the embodiment of the present invention are dropped using a liquid vibrating device, and the droplets are frozen in liquid nitrogen, and then freeze-dried to obtain spherical particles.

[0026] According to the method for producing spherical particles of the embodiment of the present invention, it is possible to obtain spherical particles having each component of the particles contained in the slurry. In addition, the ratio of voids contained in the obtained spherical particles can be reduced to 10% or less. In addition, the composition of the obtained spherical particles can be controlled by changing the mixing ratio of multiple types of particles in the slurry. For example, when each particle is composed of a particle made of Mo, a particle made of Si, a particle made of TiC, and a particle made of MoB, it is possible to produce the spherical particles of the embodiment of the present invention composed of a Mo-Si-B-TiC alloy. EXAMPLES

[0027] A slurry was produced by the method for producing a slurry according to the embodiment of the present invention, and spherical particles were produced by using the slurry by the method for producing spherical particles according to the embodiment of the present invention. First, four types of particles, namely, particles made of Mo, particles made of Si, particles made of TiC, and particles made of MoB, and water containing nanobubbles were prepared as particles to be dispersed in the slurry. Here, the liquid of the slurry was water, and the dispersant was nanobubbles. In addition, the water containing nanobubbles was commercially available. As shown in FIG. 2, nanobubbles have the characteristic of being negatively charged in liquid and being able to maintain that state for a relatively long period of time. In addition, all four types of particles are negatively charged in liquid.

[0028] The four types of particles were added to water containing nanobubbles at concentrations of 5 vol%, 8 vol%, 10 vol%, 15 vol%, 20 vol%, and 30 vol%, and stirred to produce six types of slurries. For comparison, the four types of particles were added to pure water not containing nanobubbles at the same concentrations, and stirred to produce six types of slurries. The results of observing the state of each slurry 10 minutes after stirring are shown in Table 1. In Table 1, an x ​​mark indicates a state in which the particles have settled, and an o mark indicates a state in which no particle precipitation is observed.

[0029] [Table 1]

[0030] As shown in Table 1, when pure water was used, particle precipitation was observed in slurries with a concentration of 10 vol% or more 10 minutes after stirring. In addition, in the slurry with a concentration of 8 vol%, particle precipitation was not observed 10 minutes after stirring, but was observed within 30 minutes. In contrast, when water containing nanobubbles was used, particle precipitation was observed in the slurry with a concentration of 30 vol% 10 minutes after stirring, but was not observed in slurries with a lower concentration. In addition, in the slurry with a concentration of 20 vol%, particle precipitation was not observed 10 minutes after stirring, but was observed within 30 minutes. In addition, in the slurry with a concentration of 15 vol%, particle precipitation was not observed 30 minutes after stirring, but was observed within 60 minutes.

[0031] Among the produced slurries, those in which the particles had not settled even after 10 minutes of stirring were used to produce spherical particles by the method for producing spherical particles according to the embodiment of the present invention. First, the produced slurry was supplied to an orifice (liquid reservoir) of a liquid vibration device, and the slurry was vibrated at 10 Hz using a diaphragm (thin plate), and droplets were ejected from a nozzle with a diameter of 600 μm provided in the orifice. The ejected droplets were dropped into liquid nitrogen and frozen, and then the frozen particles were taken out and dried by a freeze dryer to produce spherical particles. The produced spherical particles were MoSiBTiC alloy.

[0032] Spherical particles produced using pure water and slurries with concentrations of 5 vol% and 8 vol%, and using water containing nanobubbles and slurries with concentrations of 5 vol%, 15 vol%, and 20 vol% are shown in Figures 3 and 4. Furthermore, the particle size distributions of spherical particles produced using pure water and slurries with concentrations of 5 vol%, and using water containing nanobubbles and slurries with concentrations of 15 vol% and 20 vol% are shown in Figure 5.

[0033] As shown in Figures 3 and 4, it was confirmed that the gaps became smaller and the density became higher as the concentration of the slurry increased. It was also confirmed that the shape became more spherical as the concentration of the slurry increased. It was also confirmed that the particle size became smaller as the concentration of the slurry increased, as shown in Figure 5.

[0034] Next, the ratio of voids (void fraction) was measured for spherical particles manufactured using a slurry with a concentration of 5 vol% using pure water, and slurries with concentrations of 10 vol%, 15 vol%, and 20 vol% using water containing nanobubbles. The void fraction was measured by X-ray CT measurement using a submicron focus X-ray inspection device ("TUX-3200N" manufactured by Mars Token X-ray Inspection Co., Ltd.), and the void fraction was calculated using 3D image analysis software ("ExFact VR 2.1" manufactured by Japan Visual Science Co., Ltd.).

[0035] As a result, the void ratio of the spherical particles produced using pure water and a slurry with a concentration of 5 vol% was 12.5%, whereas the void ratios of the spherical particles produced using water containing nanobubbles and slurries with concentrations of 10 vol%, 15 vol%, and 20 vol% were 7.4%, 5.3%, and 6.2%, respectively. This confirmed that the void ratio of the spherical particles produced using water containing nanobubbles and a high-concentration slurry was reduced compared to those produced using pure water. [Explanation of symbols]

[0036] 1 container 2 Stirring blade 11a, 11b, 11c particles 12 Water containing nanobubbles 12a Nanobubbles

Claims

1. A liquid containing a negatively charged dispersant and one or more types of negatively charged particles, The particles include particles made of Mo, particles made of Si, particles made of TiC, and particles made of MoB. A slurry comprising:

2. 2. The slurry according to claim 1, wherein the dispersant comprises nanobubbles.

3. The method comprises adding to a liquid a dispersant that is negatively charged in the liquid and one or more types of particles that are negatively charged in the liquid, The particles include particles made of Mo, particles made of Si, particles made of TiC, and particles made of MoB. A method for producing a slurry comprising the steps of:

4. 4. The method for producing a slurry according to claim 3, wherein the dispersant is made of nanobubbles.

5. A method for producing spherical particles, comprising dropping droplets of a slurry containing a negatively charged dispersant and one or more types of negatively charged particles into a liquid, freezing the droplets, and then freeze-drying the droplets to obtain spherical particles.

6. A method for producing spherical particles, comprising dripping droplets of the slurry according to claim 1 or 2, freezing the droplets, and then freeze-drying the droplets to obtain spherical particles.

7. 7. The method for producing spherical particles according to claim 5, wherein the droplets are dropped using a liquid vibrator and the droplets are frozen in liquid nitrogen.

8. The method for producing spherical particles according to any one of claims 5 to 7, characterized in that the spherical particles are obtained from the slurry using a freeze-drying pulse pressure orifice method.

9. 9. The method for producing spherical particles according to claim 5, wherein the spherical particles contain voids at a rate of 10% or less.

10. The method for producing spherical particles according to any one of claims 5 to 9, characterized in that the spherical particles are made of a Mo-Si-B-TiC alloy.

11. The spherical particles are made of a Mo-Si-B-TiC alloy and contain voids at a ratio of 10% or less.

Citation Information

Patent Citations

  • Equipment and method for manufacturing monodispersed particle, and monodispersed particle manufactured by the manufacturing method

    JP2002155305A

  • Method of manufacturing ceramic spherical monodisperse particle, ceramic spherical monodisperse particle manufactured by the method and apparatus for manufacturing the same

    JP2004182477A

  • Photonic crystal and its manufacturing method, structure for manufacturing photonic crystal, and its manufacturing method

    JP2006126776A

  • Supply method and supply device of polishing slurry, and polishing apparatus

    JP2013110201A

  • Method for producing alloy particle dispersion, alloy particle dispersion, and method for producing coated base material

    JP2020002445A