Optical film and method for producing optical film
The optical film with a sputtered metal or alloy layer on a resin film, featuring a specific island-like structure and high surface resistivity, addresses breakage and adhesion issues, achieving superior radio wave and visible light performance.
Patent Information
- Application Number
- JP2020015014
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-01-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-01-31
AI Technical Summary
Existing optical films with indium island structures are prone to breakage during manufacturing processes due to low melting points, and films with low surface energy layers suffer from poor adhesion and durability issues, hindering effective radio wave transmission and visible light reflectivity.
An optical film comprising a resin film with a sputtered metal or alloy layer having an island-like structure, characterized by a maximum height roughness of 8.5 nm or more, an average island diameter of 20 nm or less, and a surface resistivity of 250Ω/□ or more, formed using a honeycomb-shaped filter during sputtering to enhance radio wave transmittance and visible light reflectivity.
The solution provides an optical film with excellent radio wave transmittance and visible light reflectivity, maintaining a durable and discontinuous island-like structure that enhances both radio wave transparency and mirror-like appearance.
Smart Images

Figure 0007580736000002 
Figure 0007580736000003 
Figure 0007580736000004
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film and a method for producing the optical film. [Background technology]
[0002] In order to improve the safety of motorcycles, automobiles, and other transport vehicles, the installation of automotive radars that use electromagnetic waves such as millimeter waves is progressing. Automotive radars are installed on the front, rear, or left and right (lateral) sides of the vehicle body, and can recognize the appropriate distance between vehicles and obstacles (e.g. people, objects) in the dark.
[0003] The mounting location of this automotive radar is set in the center of the vehicle body for reasons such as improving accuracy, because if it is too low, it will be obstructed by the road, and if it is too high, it will miss the target point. Therefore, when mounting the automotive radar at the front of the vehicle body, the automotive radar is installed on the back side of or in the vicinity of the emblem provided at the front of the vehicle body.
[0004] However, emblems and the grille (front grille) nearby are usually plated with decorative metal plating (especially chrome plating) that has a metallic luster, and such metal plating blocks electromagnetic waves and does not allow them to pass through, which can cause problems in the transmission and reception of electromagnetic waves by automotive radar.
[0005] Therefore, in order to place an automobile radar behind an emblem, it has been proposed to manufacture an exterior part such as an emblem that has a decorative metallic luster and does not have an absorption region in the electromagnetic wave frequency band due to the island-like structure of indium by evaporating indium onto a resin film and attaching the film to the surface of the emblem by an insert molding method (see Patent Document 1). In the case of a normal metal coating (e.g., aluminum, tin, chromium, etc.) used for an emblem, etc., the wettability (affinity) to the resin film is too high, and the island-like structure immediately changes to a continuous coating on the resin film, so that no gaps through which electromagnetic waves can pass are formed. In contrast, indium has low wettability to the resin film, so it is easy to create fine island-like structures of indium on the resin film by vacuum deposition, and the appearance has a uniform metallic luster similar to that of normal metal plating.
[0006] In addition, a radio wave-transmitting transparent laminate is known in which a discontinuous island-shaped metal layer is formed on a transparent plastic film via a layer of polytetrafluoroethylene (hereinafter, PTFE) or the like having a surface energy of 40 dyn / cm or less (see Patent Document 2). When a layer with a surface energy of 40 dyn / cm or less is provided, the cohesive force of the metal increases when the metal layer is formed by a method such as sputtering, and as a result, the metal layer is more likely to be formed in an island shape. When the metal layer is discontinuous, the surface resistance increases, improving radio wave transmittance. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2002-135030 A [Patent Document 2] Patent No. 5527480 Summary of the Invention [Problem to be solved by the invention]
[0008] When a coating having an indium island structure is formed as in Patent Document 1, the melting point of indium is as low as 156°C, so the island structure may easily break. For example, when a protective layer for protecting the coating is formed by injection molding (insert molding), a viscous molten resin at 200°C or higher is poured into a mold in which a resin film having the coating is inserted. Therefore, the indium island structure is easily broken by contact with the molten resin. Therefore, when insert molding is performed using a resin film having such an indium coating, a pretreatment is required to harden and protect the indium island structure with a low-temperature curing resin, which causes a problem of complicating the manufacturing process.
[0009] Furthermore, in the case of Patent Document 2, the adhesion between the layer having a surface energy of 40 dyn / cm or less and the metal layer is low, and the durability is insufficient for practical use.
[0010] An object of the present invention is to provide an optical film having excellent radio wave transmittance, visible light reflectance, etc., and a method for producing the same. [Means for solving the problem]
[0011] The means for solving the above problems are as follows. <1> An optical film comprising a resin film and a sputtered film containing a metal or an alloy formed on one surface of the resin film, wherein the sputtered film has an island structure, the maximum height roughness (Rz) of the sputtered film is 8.5 nm or more, and the average diameter of the islands in the island structure is 20 nm or less.
[0012] <2> The thickness of the sputtered film is 10 nm or more. <1> The optical film according to claim 1.
[0013] <3> The surface resistivity of the sputtered film is 250 Ω / □ or more, and the visible light reflectance of the sputtered film is 40% or more. <1> or <2> The optical film according to claim 1.
[0014] <4> The metal or alloy is silver or a silver alloy. <1> ~ <3> 13. An optical film according to any one of the above.
[0015] <5> A method for manufacturing an optical film in which a sputtered film is formed on a resin film by a sputtering method, comprising: disposing a honeycomb-shaped filter having a plurality of openings between the resin film and a target containing a metal or alloy; and depositing sputtered particles passing through the openings on the resin film, thereby forming the sputtered film having an island structure, a maximum height roughness (Rz) of 8.5 nm or more, and an average diameter of the islands in the island structure of 20 nm or less. Effect of the Invention
[0016] According to the present invention, it is possible to provide an optical film having excellent radio wave transmittance, visible light reflectance, etc., and a method for producing the same. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic configuration of an optical film 1 according to an embodiment. [Diagram 2] An explanatory diagram showing a schematic diagram of a method for forming a sputtered film on a resin film using a batch-type magnetron sputtering device. [Diagram 3] AFM image of the sputtered film surface in Example 3 [Figure 4] AFM image of the sputtered film surface of Comparative Example 7 [Diagram 5] Graph showing the relationship between the thickness of a sputtered film and its surface resistivity [Figure 6] Graph showing the relationship between sputtered film thickness and visible light reflectance [Figure 7] Graph showing the relationship between sputtered film thickness and maximum height roughness (Rz) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] [Optical Film] An optical film according to one embodiment of the present invention will be described with reference to the drawings. Fig. 1 is a cross-sectional view that shows a schematic configuration of an optical film 1 according to one embodiment. As shown in Fig. 1, the optical film 1 includes a resin film 2 and a sputtered film 3.
[0019] (Resin film) The resin film 2 is a film-like member that has optical transparency to visible light and the like and supports the sputtered film 3. The resin film 2 preferably has appropriate flexibility. The resin film 2 is made of, for example, a polyester resin such as polyethylene terephthalate (PET) or polybutylene terephthalate (PBT), a polycarbonate resin (PC), an acrylic resin such as polymethyl methacrylate (PMMA), triacetyl cellulose (TAC), or a cycloolefin resin (COP). Of these, the resin constituting the resin film 2 is preferably a polyester resin, and particularly preferably polyethylene terephthalate.
[0020] The resin film 2 may have a single layer structure or a multilayer structure (laminate structure) as long as the object of the present invention is not impaired. For example, the resin film 2 may be a laminate including a core layer made of the above-mentioned resin and a hard coat layer (e.g., ultraviolet-curable acrylic resin, etc.) laminated on one or both sides of the core layer.
[0021] The thickness of the resin film 2 is not particularly limited as long as it does not impair the object of the present invention, and is, for example, 2 μm to 188 μm.
[0022] The resin film 2 may be subjected to surface treatment such as corona discharge treatment, glow discharge treatment, flame treatment, ultraviolet irradiation treatment, electron beam irradiation treatment, and ozone treatment, as long as it does not impair the object of the present invention.
[0023] (Sputtered film) The sputtered film 3 is a discontinuous film containing a metal or an alloy formed on one side of the resin film 2 by sputtering using a honeycomb filter described later. The sputtered film 3 has an island structure. In this specification, the term "island structure" refers to a structure in which a plurality of aggregates (corresponding to islands) made of metal or alloy particles are independently arranged in a planar shape. The sputtered film 3 having the island structure is a discontinuous film as described above, and has a lower surface resistance value than a continuous film. The sputtered film 3 contains a metal or an alloy as a main component. The sputtered film 3 contains a metal or an alloy in an amount of 90 atomic % or more, preferably 95 atomic % or more, and more preferably 99 atomic % or more. Examples of the metal or alloy contained in the sputtered film 3 include silver (Ag), palladium (Pd), gold (Au), platinum (Pt), nickel (Ni), aluminum (Al), and alloys thereof. As the metal or alloy, silver or a silver alloy is preferable. In this embodiment, the sputtered film 3 is formed directly on the resin film 2, but in other embodiments, it may be formed on the resin film 2 via another layer as long as this does not impair the objective of the present invention.
[0024] The thickness of the sputtered film 3 is not particularly limited as long as it does not impair the object of the present invention, but for example, the lower limit of the thickness of the sputtered film 3 is preferably 10 nm or more, and more preferably 11 nm or more. The upper limit of the thickness of the sputtered film 3 is preferably 20 nm or less. When the thickness of the sputtered film 3 is within this range, it is easy to adjust the maximum height roughness (Rz) of the sputtered film 3 to a predetermined value, and it is easy to obtain a sputtered film 3 with a discontinuous island structure. The thickness of the sputtered film 3 can be measured using a fluorescent X-ray analyzer, as described later.
[0025] The thickness of the sputtered film 3 can be adjusted by appropriately setting, for example, the pressure in the chamber, the discharge current, the discharge time, and the like during film formation by sputtering.
[0026] The sputtered film 3 is a discontinuous film containing a metal or an alloy and has an island structure. Since the sputtered film 3 has an island structure, it has a high surface resistivity and excellent radio wave transmittance.
[0027] The lower limit of the maximum height roughness (Rz) of the sputtered film 3 is 8.5 nm or more, and preferably 9.0 nm or more. The upper limit of the maximum height roughness (Rz) is not particularly limited as long as it does not impair the object of the present invention, but is preferably 40 nm or less, and more preferably 35 nm or less. When the maximum height roughness (Rz) of the sputtered film 3 is in this range, a discontinuous island structure is easily ensured.
[0028] The maximum height roughness (Rz) of the sputtered film 3 can be adjusted by appropriately setting the size of the openings of the honeycomb filter used when forming the sputtered film 3. Similarly to the thickness of the sputtered film 3 described above, the maximum height roughness (Rz) of the sputtered film 3 can also be adjusted by appropriately setting the pressure in the chamber, the discharge current, the discharge time, etc. when forming the film by sputtering. The method for measuring the maximum height roughness (Rz) of the sputtered film 3 will be described later.
[0029] The surface resistivity of the sputtered film 3 is 250 Ω / □ or more, and preferably 1.0×10 9 The surface resistivity of the sputtered film 3 is equal to or greater than Ω / □.
[0030] The visible light reflectance (lower limit) of the sputtered film 3 is 40% or more. The upper limit of the visible light reflectance of the sputtered film 3 is not particularly limited as long as it does not impair the object of the present invention, but for example, when the optical film 1 is used as a half mirror, the visible light reflectance is preferably 60% or less, more preferably 55% or less, and even more preferably 50% or less.
[0031] The average island diameter (upper limit) in the island-like structure of the sputtered film 3 is 20 nm or less, preferably 17 nm or less. The average island diameter (lower limit) is preferably 7 nm or more, more preferably 8 nm or more. When the average island diameter is within this range, the surface resistivity is high and the radio wave transmittance is excellent. The method for measuring the average island diameter will be described later.
[0032] Here, a method for forming the sputtered film 3 will be described with reference to Fig. 2. Fig. 2 is an explanatory diagram that shows a schematic diagram of a method for forming the sputtered film 3 on the resin film 2 using a batch-type magnetron sputtering device (hereinafter referred to as "sputtering device") 10. Before forming the sputtered film 3, the resin film 2 may be placed in a chamber 11 of the sputtering device 10 and subjected to a heat treatment (e.g., heating at 75°C for 8 hours) to remove gas components contained in the resin film 2.
[0033] 2, in a chamber 11, a resin film 2 is placed on a stage 12. A target material 13 is disposed to face the resin film 2 on the stage 12 with a predetermined distance TS therebetween. The distance TS is the distance between the target material 13 and the resin film 2. A magnetron 14 is disposed on the rear side of the target material 13.
[0034] As shown in FIG. 2, a filter 15 is disposed between the target material 13 and the resin film 2. The filter 15 is honeycomb-shaped including a plurality of openings 15a, and is made of, for example, a metal material such as aluminum, a plastic material, or the like. The openings 15a in this embodiment are regular hexagonal in plan view, and have holes penetrating the filter 15 in the thickness direction on the inside. In this specification, the length of the openings 15a is equal to the thickness D of the filter 15. The filter 15 is made up of a collection of a plurality of openings 15a having the same opening diameter d and the same length. In other embodiments, the openings may be rectangular, triangular, or the like in plan view.
[0035] The filter 15 is disposed so as to face the resin film 2 on the stage 12 while maintaining a predetermined gap FS. The gap FS is the distance between the filter 15 and the resin film 2. The filter 15 is disposed so that the penetration direction of the holes of the openings 15a coincides with the direction in which the target material 13 and the resin film 2 are arranged (the vertical direction in FIG. 2).
[0036] In order to form a sputtered film 3 on the resin film 2 thus placed in the chamber 11, a voltage is applied between the stage 12 and the target material 14. The voltage is applied so that the stage 12 (resin film 2) side serves as the anode and the target material 13 side serves as the cathode.
[0037] 2 shows a schematic diagram of sputtered particles 16 generated from target material 13. Of the sputtered particles 16 generated from target material 13, those having relatively high energy that have passed through openings 15a of filter 15 are deposited on resin film 2. Then, for a predetermined period of time, sputtered particles 16 are deposited in islands in the thickness direction on resin film 2, thereby forming sputtered film 3 having a discontinuous island structure. Note that sputtered particles 16 having relatively low energy are blocked by filter 15.
[0038] The island structure of the sputtered film 3 is adjusted by appropriately setting the size (opening diameter d, length D), interval FS, film formation temperature, etc. of the openings 15a of the filter 15. If the length D of the openings 15a of the filter 15 is too long, the film formation speed will be slow, which is undesirable. If the length D of the openings 15a of the filter 15 is too short, sputtered particles 16 with relatively low energy will pass through the openings 15a, which is undesirable.
[0039] The temperature inside the chamber 11 during the formation of the sputtered film 3 is preferably about room temperature (23° C.) (e.g., −20° C. to 120° C.). When the temperature inside the chamber 11 is within this range, the metal or alloy particles on the resin film 2 do not gather too much together in the surface direction of the resin film 2, making it easy to form a suitably discontinuous island structure, and the sputtered film 3 can be formed without the resin film 2 being deformed.
[0040] By the above-mentioned method, the desired sputtered film 3 can be formed on the resin film 2. The resin film 2 having the sputtered film 3 formed thereon in this manner is used as the optical film 1.
[0041] In addition, in the optical film 1, a layer other than the sputtered film 3 may be formed on the resin film 2 as long as the object of the present invention is not impaired. For example, a protective film may be formed on the surface of the sputtered film 3, a SiO2 film or the like may be formed in order to improve the adhesion between the resin film 2 and the sputtered film 3, or an optical film such as an ITO film may be formed in order to adjust the optical properties (e.g., refractive index) of the optical film 1. Furthermore, the sputtered film 3 may be formed on both sides of the resin film 2 as necessary.
[0042] (Application) The optical film 1 can be used as a radio wave transmitting half mirror or the like for use in automobile glass (windshield, etc.) or building window glass, for example. EXAMPLES
[0043] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples in any way.
[0044] In the following Examples and Comparative Examples, a batch-type magnetron sputtering device was used for the sputtering deposition. The flow rate of the gas supplied to each chamber of the sputtering device was appropriately adjusted using a predetermined mass flow controller.
[0045] Example 1 As the resin film, PET with HC (total thickness: 135 μm) was prepared, in which hard coat layers (ultraviolet-curable acrylic resin, thickness: 5 μm) were formed on both sides of a core layer (thickness: 125 μm) made of PET. In addition, an aluminum honeycomb filter including a plurality of openings (regular hexagonal opening diameter (maximum diameter): 3.2 mm, thickness: 13 mm) was prepared as the filter 1. With the filter 1 disposed between the resin film and the target, a sputtered film (silver alloy layer) was formed by sputtering on one side of the resin film under the film formation conditions shown below, to obtain the optical film of Example 1.
[0046] <Film formation conditions: sputtered film> Target: Silver containing 1 atomic % palladium, deposition pressure: 0.4 Pa, DC power: 0.25 W / cm 2 , Target-resin film distance: 100 mm, Filter-resin film distance: 50 mm, Film formation temperature: Room temperature (23°C), Substrate transport speed: 0.08 m / min
[0047] Example 2 An optical film of Example 2 was produced in the same manner as in Example 1, except that the substrate conveying speed was changed to 0.06 m / min.
[0048] Example 3 The optical film of Example 3 was produced in the same manner as in Example 1, except that the substrate conveying speed was changed to 0.15 m / min, the target-resin film distance was changed to 75 mm, and the filter-resin film distance was changed to 25 mm.
[0049] [Comparative Examples 1 to 3] Optical films of Comparative Examples 1 to 3 were produced in the same manner as in Example 1, except that the substrate conveying speed was changed to 0.39 m / min, 0.044 m / min, and 0.034 m / min, respectively.
[0050] [Comparative Examples 4 to 7] The optical films of Comparative Examples 4 to 7 were produced in the same manner as in Example 1, except that no filter was placed between the resin film and the target and the substrate conveying speed was changed to 9.16 m / min, 5.50 m / min, 3.05 m / min, and 1.83 m / min, respectively.
[0051] Comparative Example 8 Except for using Filter 2 instead of Filter 1 and changing the substrate conveying speed to 0.39 m / min, an optical film of Comparative Example 8 was produced in the same manner as in Example 1. Filter 2 was an aluminum honeycomb filter including a plurality of openings (regular hexagonal opening diameter (maximum diameter): 9.5 mm, thickness: 15 mm).
[0052] 〔evaluation〕 (Thickness of sputtered film) The thickness (average value for a diameter of 30 mm) of the sputtered film in Example 1 was measured using a fluorescent X-ray analyzer (product name "ZSX-100e", manufactured by Rigaku Corporation). The results are shown in Table 1.
[0053] (Maximum height roughness Rz) Using an atomic force microscope (AFM) (product name "FTM-9600", manufactured by Shimadzu Corporation), a surface image (AFM image) of the sputtered film of Example 1, etc. was obtained, and the maximum height roughness Rz (nm) was obtained from the AFM image. Here, referring to FIG. 3, a method for measuring the maximum height roughness Rz of the sputtered film of Example 2 will be specifically described. FIG. 3 is an AFM image of the surface of the sputtered film of Example 2. The display size (observation field) of the AFM image is 2.00 μm × 2.00 μm. The maximum height roughness Rz (nm) was obtained along a line segment AB (figure) extending in one direction shown in such an AFM image. Next, the maximum height roughness Rz (nm) was obtained along a line segment CD (a line segment perpendicular to the line segment AB) shown in the same image of FIG. 3. Each line segment AB and CD has the same length and is 0.5 μm. The average value of these two maximum height roughnesses Rz (nm) was taken as the maximum height roughness Rz (nm) of the sputtered film surface in Example 2. It is shown in Table 1.
[0054] 4 is an AFM image of the surface of the sputtered film of Comparative Example 7. Similarly, in the case of Comparative Example 7, the maximum height roughness Rz (nm) of the surface of the sputtered film of Comparative Example 7 was determined from two line segments AB and CD that are perpendicular to each other and shown in the image.
[0055] (Average diameter of island structures) For the silver alloy layer of Example 1, etc., the average diameter of the islands in the island structure was measured by the method described below. A sample cut into 1 cm square from the optical film of Example 1, etc. was observed with an atomic force microscope to obtain an AFM image, and 10 islands in the island structure of the sputtered film were randomly selected from the AFM image, and the major and minor diameters of each island were measured and the average diameter was calculated. The major diameter is the diameter of the circumscribing circle of the island, and the minor diameter is the diameter of the inscribing circle of the island. The results are shown in Table 1.
[0056] (Surface resistivity) A sample (size: 5 cm square) was cut out from the optical film of Example 1, etc., and the surface resistance value (Ω / □) was measured using the sample in accordance with JIS K 6911. The measurement device used was a Hiresta-UP MCP-HT450 (manufactured by Mitsubishi Chemical Corporation). The probe (electrode) of the measurement device was pressed against the surface of the sputtered film of the sample, and the current value (temperature condition: 20°C) flowing through the surface was measured, and the surface resistance value (Ω / □) was calculated from the current value. The results are shown in Table 1.
[0057] (Visible light reflectance) A sample (size: 5 cm square) was cut out from the optical film of Example 1, and the visible light reflectance (%) of the sputtered film was measured using the sample. The visible light reflectance was evaluated in accordance with JIS R 3106. A spectrophotometer (U4100, manufactured by Hitachi High-Tech Corporation) was used as the evaluation equipment. The results are shown in Table 1.
[0058] [Table 1]
[0059] In the optical films of Examples 1 to 3, the sputtered film made of a silver alloy film has a discontinuous island structure (see, for example, FIG. 3). As shown in Table 1, it was confirmed that these optical films have high surface resistivity and excellent radio wave transmittance. It was also confirmed that the optical films of Examples 1 to 3 have high visible light reflectance and a mirror-like appearance. In this way, the optical films of Examples 1 to 3 have both radio wave transmittance (high surface resistivity) and high visible light reflectance.
[0060] In Examples 1 to 3, the average diameter of the islands in the island-like structure was 20 nm or less, and all of the islands were small. This is presumably because the use of a honeycomb filter removes low-energy sputtered particles, while only high-energy sputtered particles with uniform directionality reach the resin film (base film), and the high-energy sputtered particles that reach the resin film can move an extremely small, fixed distance on the resin film surface, forming an island-like structure in which the sputtered particles are aggregated into small particles on the resin film surface.
[0061] In Comparative Example 1, the thickness of the sputtered film was too thin, and the visible light reflectance was low. Although the surface resistivity of Comparative Example 1 was high, this was due to the resin film (insulation) rather than the sputtered film.
[0062] In Comparative Examples 2 and 3, similar to Example 1, the sputtered films were formed using filter 1, but the sputtered films did not have an island structure and had a small maximum height roughness (Rz). In addition, the sputtered films in Comparative Examples 2 and 3 were too thick. It was confirmed that Comparative Examples 2 and 3 had low surface resistivity (i.e., high conductivity) and were difficult to transmit radio waves.
[0063] In Comparative Examples 4 to 7, a sputtered film was formed without using filter 1. It was confirmed that the sputtered film did not have an island structure and had too low a surface resistivity, making it difficult for radio waves to pass through.
[0064] Comparative Example 8 is a case where a sputtered film was formed using a filter 2 with large openings. In such Comparative Example 8, a continuous sputtered film was formed instead of an island structure, and radio wave transmittance was not obtained.
[0065] The results of Examples 1 to 3 and Comparative Examples 1 to 7 are summarized in the graphs of Figs. 5 to 7 according to the presence or absence of filter 1. Fig. 5 is a graph showing the relationship between the thickness and surface resistivity of the sputtered film, Fig. 6 is a graph showing the relationship between the thickness and visible light reflectance of the sputtered film, and Fig. 7 is a graph showing the relationship between the thickness and maximum height roughness (Rz) of the sputtered film. The horizontal axis of each graph of Figs. 5 to 7 represents the thickness (nm) of the sputtered film. The vertical axis of the graph of Fig. 5 represents the surface resistivity (Ω / □) of the sputtered film, the vertical axis of the graph of Fig. 6 represents the visible light reflectance (%) of the sputtered film, and the vertical axis of the graph of Fig. 7 represents the maximum height roughness Rz (nm) of the sputtered film. In the graphs of each figure, Examples 1 to 3 are shown as "Experimental 1 to 3", and Comparative Examples 1 to 7 are shown as "Comparative 1 to 7". [Explanation of symbols]
[0066] 1...optical film, 2...resin film, 3...sputtered film, 10...sputtering device, 11...chamber, 12...stage, 13...target material, 14...magnetron, 15...filter
Claims
1. A resin film; a sputtered film containing a metal or an alloy, the sputtered film being formed directly on one surface of the resin film, The sputtered film has an island structure, The maximum height roughness (Rz) of the sputtered film is 8.5 nm or more; The thickness of the sputtered film is 10 nm or more, the average diameter of the islands in the island structure is 20 nm or less; the metal or alloy is silver or a silver alloy; The surface resistivity of the sputtered film is 1.0×10 9 Ω / □ or more.
2. An optical film as described in claim 1, wherein the thickness of the sputtered film is 20 nm or less, and the visible light reflectance of the sputtered film is 40% or more.
3. A method for producing an optical film, comprising forming a sputtered film on a resin film by a sputtering method, a honeycomb filter including a plurality of openings is disposed between the resin film and a target including a metal or an alloy, and facing the resin film with a predetermined distance therebetween; and sputtered particles passing through the openings are deposited on the resin film to form the sputtered film having an island structure, a maximum height roughness (Rz) of 8.5 nm or more, and an average diameter of the islands in the island structure of 20 nm or less; The method for manufacturing an optical film, wherein the filter is disposed so that a penetration direction of the holes of the opening coincides with a direction in which the target and the resin film are aligned.
4. The method for producing an optical film according to claim 3 , wherein the metal or alloy is silver or a silver alloy.
5. The method for producing an optical film according to claim 3 or 4, wherein the sputtered film has a thickness of 10 nm or more.
Citation Information
Patent Citations
Feed hopper for molding sand
JP1980027480A
Radio wave transmitting exterior component and its manufacturing method
JP2002135030A
Accessory, its manufacturing method, and timepiece
JP2008020264A
Layered body
JP2019188797A
Electromagnetic wave transmissible metallic sheen article
JP2019188809A