Slide member and slide body
The incorporation of fired clay and solid lubricants in PTFE-based sliding members enhances low friction and wear resistance, addressing the need for improved performance under grease lubrication and in oil.
Patent Information
- Application Number
- JP2021064992
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-04-06
AI Technical Summary
Existing PTFE-based sliding members require higher low friction properties under grease lubrication and in oil.
A PTFE-based sliding member is developed by incorporating fired clay, magnesium phosphate, barium sulfate, and molybdenum disulfide as solid lubricants, with specific weight percentages, and optionally adding fillers like spherical carbon or glass fibers, to enhance wettability and reduce friction.
The solution results in a PTFE-based sliding member with improved low friction and wear resistance under grease lubrication and in oil, achieving reduced friction coefficients and enhanced wear resistance.
Smart Images

Figure 0007581113000002 
Figure 0007581113000003 
Figure 0007581113000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a slide member and a slide body. [Background technology]
[0002] Polytetrafluoroethylene resin (hereinafter abbreviated as "PTFE") has been widely used as a sliding member in the steering mechanism of vehicles such as automobiles because of its excellent self-lubricating property, low friction coefficient, and chemical resistance and heat resistance. Recently, a sliding member based on PTFE has become known (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-20568 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in recent years, there has been a demand for even lower friction in PTFE-based sliding members that are used under grease lubrication or in oil.
[0005] An object of the present invention is to provide a PTFE-based sliding member having higher low friction properties under grease lubrication and in oil, and a sliding body using the same. [Means for solving the problem]
[0006] The sliding member of the present invention is made of a polytetrafluoroethylene resin based on sintered clay. and solid lubricants is added the solid lubricant is magnesium phosphate, barium sulfate, and molybdenum disulfide, and the sliding member is added with 12 to 16% by weight of the magnesium phosphate, 13 to 19% by weight of the barium sulfate, 4 to 6% by weight of the molybdenum disulfide, and 1 to 4% by weight of the calcined clay. It is characterized by the above. Effect of the Invention
[0007] According to the present invention, it is possible to provide a PTFE-based sliding member having higher low friction properties under grease lubrication and in oil, and a sliding body using the same. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a diagram showing a slide body according to the first embodiment. [Diagram 2] FIG. 2 is a diagram showing the configuration of the sliding member. [Diagram 3] FIG. 3 is a graph showing the experimental results of the sliding member. [Figure 4] FIG. 4 is a graph showing the experimental results of the sliding member. [Diagram 5] FIG. 5 is a diagram showing the configuration of a sliding member according to the second embodiment. [Figure 6] FIG. 6 is a diagram showing the state of the friction test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an embodiment will be described with reference to the drawings. In the embodiment, an example in which a sliding body is used in a vehicle under grease lubrication will be described.
[0010] (First embodiment) For example, among the bearings used in the steering mechanism of vehicles such as automobiles, there are sliding bearings that have a low sliding speed and are used with grease lubrication. These bearings are used, for example, in the support yoke portion attached to the rack and pinion type power steering, where low friction is important.
[0011] Fig. 1 is a diagram showing a slide body 1 according to a first embodiment. As shown in Fig. 1, the slide body 1 has a substrate 2, a sintered layer 3, and a resin layer 4. The substrate 2 is a layer for imparting mechanical strength to the slide body 1. The substrate 2 may be called a backing metal or a backing metal layer. The substrate 2 may be, for example, a metal plate such as an Fe alloy, Cu, or Cu alloy.
[0012] The sintered layer 3 is a layer formed by scattering and sintering a copper alloy, such as copper-tin, copper-lead-tin, phosphor bronze, or a mixed powder of iron, copper, tin, etc., on the substrate 2. The sintered layer 3 is a porous layer. By providing the sintered layer 3 on the substrate 2, the adhesion between the resin layer 4 and the substrate 2 can be improved.
[0013] The resin layer 4 is a sliding member based on PTFE 5 (PTFE 5 is the main resin component) with calcined clay added to PTFE 5. The sliding member constituting the resin layer 4 will be described later with reference to Fig. 2. The sliding member is impregnated into the sintered layer 3, so that the substrate 2 and the sliding member are firmly adhered to each other.
[0014] In the sliding body 1, the sintered layer 3 is impregnated with a mixture of the raw materials constituting the sliding member, and then fired at 350 to 420° C. to form a resin layer 4 (slide member 41) on the substrate 2. The thickness of the resin layer 4 on the substrate 2 is 80 to 400 μm, and preferably 120 to 250 μm. It is preferable that the porous sintered layer is not exposed on the surface of the resin layer 4, but it may be exposed.
[0015] The sintered layer 3 is not essential, and for example, the substrate 2 may be roughened by shot blasting or the like, and the sliding member may be applied directly to the roughened surface. The application method may be spraying, tumbling, roll transfer, printing, or the like. The thickness of the applied surface is preferably 10 to 60 μm, more preferably 20 to 40 μm. A wire mesh may be used as the substrate 2 instead of a steel plate. In the case of a wire mesh, the method is basically the same as that of impregnating the porous sintered layer described above.
[0016] Next, the sliding member will be described. In the sliding member 41, calcined clay 6 is added to PTFE 5. In the first embodiment, calcined kaolin is used as an example of the calcined clay 6. Calcined kaolin is a natural clay mineral that is subjected to high-temperature treatment. By adding calcined clay 6 to PTFE 5, the oil wettability is improved due to the oil absorption effect of the calcined clay. When the oil wettability is improved, a lubricating oil film is easily generated under grease lubrication and in oil, and low friction is improved. Furthermore, wear resistance is improved by improving low friction. In the first embodiment, the addition rate of calcined clay 6 is preferably 1 vol% to 15 vol%.
[0017] The following experiment was carried out using a sliding member 41 in which calcined clay 6 was added to PTFE 5, and the oil contact angle and friction coefficient of the sliding member 41 were measured. Three types of sliding members 41 were used to carry out the experiment of measuring the oil contact angle and the friction coefficient: a sliding member (0) in which calcined clay 6 is not added to PTFE 5, a sliding member (5) in which calcined clay 6 is added to PTFE 5 at 5 vol%, and a sliding member (15) in which calcined clay 6 is added to PTFE 5 at 15 vol%.
[0018] The experimental environment was as follows. The experiment to measure the oil contact angle was performed at room temperature by dropping 0.2 μL of oil (Hycol, the main component of grease) onto the surface of the sliding member 41, and after 1 second, the oil contact angle was measured five times using a contact angle meter. The experiment to measure the friction coefficient was performed by pressing a Φ8 steel ball against the surface of the sliding member 41 and sliding it. The pressing load was 4.9 N, the sliding speed was 3.0 mm / s, and the sliding distance was 10 mm, and the experiment was performed at room temperature under grease lubrication. The results are shown in Figures 3 and 4. Note that the experimental results show that the smaller the oil contact angle, the better the wettability between the sliding member 41 and the oil.
[0019] 3, the horizontal axis indicates the amount of clay added to PTFE 5 in the slide member 41, and the vertical axis indicates the oil contact angle of oil dropped onto the slide member 41 with respect to the slide member 41. In FIG. 3, the plot of points where the amount of clay added is 0% indicates the oil contact angle with the slide member (0), the plot of points where the amount of clay added is 5% indicates the oil contact angle with the slide member (5), and the plot of points where the amount of clay added is 15% indicates the oil contact angle with the slide member (15).
[0020] As shown in Fig. 3, it can be seen that the oil contact angle for the sliding member (5) is smaller than the oil contact angle for the sliding member (0). In other words, the sliding member (5) has better wettability to oil than the sliding member (0). Similarly, it can be seen that the oil contact angle for the sliding member (15) is smaller than the oil contact angles for the sliding member (0) and the sliding member (5). In other words, the sliding member (15) has better wettability to oil than the sliding member (0) and the sliding member (5).
[0021] From the above experiments, the applicant of the present application discovered that the sliding member 41 in which the calcined clay 6 is added to the PTFE 5 in an amount of 5 to 15 vol % can have improved wettability with respect to oil.
[0022] Specifically, calcined clay is obtained by subjecting clay to high heat treatment, which activates and porous clay, increasing its oil absorption. For this reason, it is believed that adding it to PTFE5 improves its wettability with oil. When wettability with oil improves, it becomes easier for a lubricating oil film to form, and in addition to the inherent low friction of PTFE5, the effect of the oil lubrication further improves the low friction and wear resistance at the same time.
[0023] In addition, in Fig. 4, the horizontal axis represents the oil contact angles in the sliding member (0), the sliding member (5), and the sliding member (15), and the vertical axis represents the friction coefficient for each oil contact angle. Note that the oil contact angles (points plotted in Fig. 4) of the sliding member (0), the sliding member (5), and the sliding member (15) in Fig. 4 are the average values of the oil contact angles of the five experimental results plotted in Fig. 3. As shown in Fig. 4, the friction coefficient in the sliding member (0) is between 0.020 and 0.021. The friction coefficient in the sliding member (5) is between 0.019 and 0.020, which is close to 0.020. The friction coefficient in the sliding member (15) is between 0.019 and 0.020, which is close to 0.019.
[0024] In this way, the sliding member (5) has improved wettability and a smaller friction coefficient than the sliding member (0). Also, the sliding member (15) has improved wettability and a smaller friction coefficient than the sliding members (0) and (5). It is believed that better wettability allows oil to remain on the friction surface more easily, and the effect of reducing the frictional force of the oil is more pronounced.
[0025] In this way, the sliding member 41 of the first embodiment has a configuration in which the calcined clay 6 is added to the PTFE 5 base. Since the sliding member 41 of the first embodiment can improve wettability, in the presence of oil, the friction coefficient of the sliding member 41 can be made smaller than that in the case in which the calcined clay 6 is not added. Therefore, a PTFE-based sliding member 41 with higher low friction properties can be provided.
[0026] The friction coefficient can also be reduced in the slide body 1 in which the slide member 41 of the first embodiment is impregnated into the sintered layer 3 on the base material 2. As a result, a slide body 1 with even lower friction can be provided.
[0027] Furthermore, the slide member 41 and the slide body 1 of the first embodiment have improved wear resistance due to the addition of the calcined clay 6.
[0028] Second embodiment From here, the second embodiment of the present invention will be described. In the second embodiment, the same reference symbols as in the first embodiment are used for the same configurations as in the first embodiment, and the description will be simplified or omitted. The resin layer 4 in the second embodiment includes a sliding member 42. The sliding member 42 includes a solid lubricant 7 in addition to the PTFE 5 and the calcined clay 6. The PTFE 5 has the same configuration as in the first embodiment. The solid lubricant 7 is preferably magnesium phosphate, barium sulfate, molybdenum disulfide, or the like. The reason for adding the solid lubricant 7 in the second embodiment is to adjust the balance of low friction, wear resistance, and seizure resistance further from the first embodiment. In addition, the sliding body 1 of the second embodiment includes a sliding member 42.
[0029] Moreover, the solid lubricant 7 added to the sliding member 42 preferably contains magnesium phosphate at 12 to 16% by weight, barium sulfate at 13 to 19% by weight, and molybdenum disulfide at 4 to 6% by weight.
[0030] The calcined clay 6 added to the sliding member 42 is preferably contained at a ratio of 1 to 4% by weight.
[0031] Furthermore, 10 vol % or less of at least one filler selected from spherical carbon, glass spheres, carbon fiber, graphite fiber, glass fiber, resin powder, resin fiber, metal powder, and metal fiber may be added to the sliding member 42. By adding such a filler, the strength, wear resistance, etc. of the sliding material are improved depending on the type of filler.
[0032] The amount of PTFE 5 in slide member 42 is the amount remaining after subtracting the amount of solid lubricant 7 and filler (if a filler is included) from the amount of slide member 42, and is preferably 40 to 95% by weight, and more preferably 56 to 66% by weight.
[0033] The slide body 1 of the second embodiment is manufactured by forming a resin layer 4 on a substrate 2. The substrate 2 is made of the same material as in the first embodiment. The method of forming the resin layer 4 is also the same as in the first embodiment. The thickness and the degree of exposure of the resin layer 4 are also the same as in the first embodiment. As in the first embodiment, a steel plate may be roughened by shot blasting or the like, and the resin layer 4 may be applied directly to the roughened portion. The application method and the thickness of the applied surface are the same as in the first embodiment.
[0034] From here, Examples 1 to 5 of the second embodiment will be described. The raw materials contained in the sliding member 42 used in each example are as follows: PTFE (average particle size 350 to 550 μm), magnesium phosphate (particle size under 200 mesh), barium sulfate (average particle size 8 to 12 μm), molybdenum disulfide (average particle size 0.5 to 2.5 μm), and calcined clay (particle size under 325 mesh).
[0035] Example 1 After the surface of the substrate 2 was sanded, phosphorus bronze powder was scattered on a degreased backing steel plate, and then sintering was performed at 920 to 950°C to form a sintered layer 3 having a thickness of 0.1 to 0.2 mm (the same as in Examples 2 to 5). On the other hand, as the sliding member 42, a raw material mixture in which 15.6% by weight of magnesium phosphate, 13.0% by weight of barium sulfate, 6.0% by weight of molybdenum disulfide, and 3.1% by weight of calcined clay were added to PTFE 5 was impregnated and coated on the sintered layer 3 with a roll, and then the temperature was raised to 350 to 420°C to obtain a sample. The coating thickness of these samples (parts above the sintered layer 3) was 0.01 to 0.06 mm.
[0036] Example 2 As the sliding member 42, 12.5 wt% magnesium phosphate, 16.1 wt% barium sulfate, 4.1 wt% molybdenum disulfide, and 1.3 wt% calcined clay were added to PTFE 5, and the mixture was impregnated and coated on the sintered layer 3 with a roll, and then the temperature was raised to 350 to 420°C to obtain samples. The coating thickness of these samples (part above the sintered layer 3) was 0.01 to 0.06 mm.
[0037] Example 3 As the sliding member 42, 13.3 weight % magnesium phosphate, 16.9 weight % barium sulfate, 4.7 weight % molybdenum disulfide, and 2.1 weight % calcined clay were added to PTFE 5, and the mixture was impregnated and coated on the sintered layer 3 with a roll, and then the temperature was raised to 350 to 420°C to obtain samples. The coating thickness of these samples (part above the sintered layer 3) was 0.01 to 0.06 mm.
[0038] Example 4 As the sliding member 42, 14.0 wt% magnesium phosphate, 17.7 wt% barium sulfate, 5.4 wt% molybdenum disulfide, and 2.9 wt% calcined clay were added to PTFE 5, and the mixture was impregnated and coated on the sintered layer 3 with a roll, and then the temperature was raised to 350 to 420°C to obtain samples. The coating thickness of these samples (part above the sintered layer 3) was 0.01 to 0.06 mm.
[0039] Example 5 As the sliding member 42, 14.8 wt% magnesium phosphate, 18.5 wt% barium sulfate, 6.0 wt% molybdenum disulfide, and 3.6 wt% calcined clay were added to PTFE 5, and the mixture was impregnated and coated on the sintered layer 3 with a roll, and then the temperature was raised to 350 to 420°C to obtain samples. The coating thickness of these samples (part above the sintered layer 3) was 0.01 to 0.06 mm.
[0040] The sliding members 42 produced in Examples 1 to 5 were subjected to the following wear test. (1) Amount of wear during wear test and (2) Coefficient of friction during wear test FIG. 6 is a diagram showing the state of the friction test. FIG. 6(a) is a diagram showing the state of the test from the axial direction of the shaft J. FIG. 6(b) is a side view of the AA cross section of FIG. 6(a). FIG. 6(c) is a diagram showing the shape of the sample, and FIG. 6(d) is a BB cross section of FIG. 6(C). As shown in FIG. 6, a sample S (radius: R13 mm, height: 9.5 mm, length in the arc direction: 30 mm, length in the axial direction: 32 mm) having a sliding body 1 in the shape of an arc plate was attached to a base D, and a load was applied to the base D to press the sample against the peripheral portion of a shaft J having a shaft diameter of Φ26 mm, and a sliding test was performed in which the sample reciprocated in the axial direction (left and right direction in FIG. 6(b)). The test was performed under the following conditions: reciprocating stroke: 20 mm, sliding speed: 55 mm / s, evaluation time: 3 hours, load: 3500 N, load type: static load, oil temperature: room temperature, oil supply method: grease application, oil type: Kyodo Yushi Moly White LSG, shaft material: S45C, shaft hardness: HRC24~30, shaft roughness: Ra0.05~0.1. The results are summarized in Table 1.
[0041] [Table 1]
[0042] That is, in Example 1, the wear amount was 5 μm and the friction coefficient was 0.09, in Example 2, the wear amount was 9 μm and the friction coefficient was 0.07, in Example 3, the wear amount was 7 μm and the friction coefficient was 0.07, in Example 4, the wear amount was 9 μm and the friction coefficient was 0.06, and in Example 5, the wear amount was 8 μm and the friction coefficient was 0.06.
[0043] Thus, the sliding member 42 of the second embodiment has a configuration in which the calcined clay 6 and the solid lubricant 7 are added to the PTFE 5 base. Since the calcined clay 6 is added to the sliding member 42 of the second embodiment, the wettability under grease lubrication can be improved and the friction coefficient of the sliding member 42 can be reduced. Therefore, a PTFE-based sliding member 42 with higher low friction properties can be provided.
[0044] In the second embodiment, 12 to 16 wt % magnesium phosphate, 13 to 19 wt % barium sulfate, 4 to 6 wt % di-fed molybdenum, and 1 to 4 wt % calcined clay are added to the PTFE 5 as the solid lubricant 7. This improves the oil wettability and reduces the friction coefficient of the sliding member 42 under grease lubrication and in oil. This makes it possible to provide a PTFE-based sliding member 42 with even lower friction properties.
[0045] Also, in the slide body 1 in which the sintered layer 3 on the base material 2 is impregnated with the slide member 42 of the second embodiment, the friction coefficient under grease lubrication and in oil can be reduced. Therefore, a slide body 1 with even lower friction can be provided.
[0046] Furthermore, the slide member 42 and the slide body 1 of the second embodiment have improved wear resistance due to the addition of the calcined clay 6.
[0047] Although the embodiment of the present invention has been described above, the embodiment and the modified examples are merely examples and are not intended to limit the scope of the invention. The novel embodiment and the modified examples can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. The embodiment and the modified examples, and the modified examples are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0048] 1. Slider 2 Base material 3 Sintered layer 4 Resin layer 5. PTFE 6 Calcined Clay 7 Solid Lubricants 41 Sliding member 42 Sliding member D. Pedestal S Sample J Bearing
Claims
1. It is made of polytetrafluoroethylene resin with calcined clay and solid lubricants added. The solid lubricant is magnesium phosphate, barium sulfate, or molybdenum disulfide, The magnesium phosphate is added in an amount of 12 to 16% by weight, the barium sulfate is added in an amount of 13 to 19% by weight, the molybdenum disulfide is added in an amount of 4 to 6% by weight, and the calcined clay is added in an amount of 1 to 4% by weight. Sliding member.
2. 2. The sliding member according to claim 1, further comprising a filler added to the polytetrafluoroethylene resin, the filler being at least one selected from spherical carbon, glass spheres, carbon fibers, graphite fibers, glass fibers, resin powder, resin fibers, metal powder, and metal fibers, the filler comprising 10% by weight or less in total.
3. A sliding body comprising the sliding member according to claim 1 or 2 provided on a substrate.
Citation Information
Patent Citations
Sliding material
JP1989261514A
Sliding material
JP2002020568A
Resin composition for sliding member and sliding member
WO2005007741A1