Superconducting layer connection structure, superconducting wire, superconducting coil, superconducting device, and superconducting layer connection method
The superconducting layer connection structure with a rare earth oxide and metal composition addresses the challenge of balancing electrical resistance and mechanical strength, improving the performance of superconducting connections in NMR and MRI devices.
Patent Information
- Application Number
- JP2021149038
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Existing superconducting layer connection structures struggle to achieve a balance between low electrical resistance and high mechanical strength, which is crucial for applications in devices like NMR and MRI equipment.
A superconducting layer connection structure is developed using a connection layer composed of a rare earth element, barium, copper, and oxygen, with a specific area ratio and particle configuration, including a first substance of rare earth oxide superconductor and a second substance of metal, to ensure strong and low-resistance connections.
The proposed structure achieves low electrical resistance and high mechanical strength, enhancing the critical current capacity and durability of superconducting connections, particularly in nuclear magnetic resonance and magnetic resonance imaging equipment.
Smart Images

Figure 0007581165000002 
Figure 0007581165000003 
Figure 0007581165000004
Abstract
Description
[Technical field]
[0001] FIELD OF THE PRESENT EMBODIMENTS The present invention relates to a connection structure of superconducting layers, a superconducting wire, a superconducting coil, a superconducting device, and a method of connecting superconducting layers. [Background technology]
[0002] For example, nuclear magnetic resonance (NMR) and magnetic resonance imaging (MRI) devices use superconducting coils to generate strong magnetic fields. Superconducting coils are formed by winding superconducting wire around a bobbin.
[0003] In order to make a superconducting wire longer, for example, a plurality of superconducting wires are connected. For example, the ends of two superconducting wires are connected using a connection structure. The connection structure for connecting the superconducting wires is required to have low electrical resistance and high mechanical strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6675590 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a connection structure for superconducting layers that can achieve low electrical resistance and high mechanical strength. [Means for solving the problem]
[0006] The superconducting layer connection structure of the embodiment includes a first superconducting layer, a second superconducting layer, and a first substance provided between the first superconducting layer and the second superconducting layer, the first substance including rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). and a connection layer including a first region where the second material and the first superconducting layer contact each other at a first interface between the first superconducting layer and the connection layer, the first area ratio per unit area of the first region where the second material and the first superconducting layer contact each other is 1% or more and 50% or less, and a second area ratio per unit area of the second region where the second material and the second superconducting layer contact each other at a second interface between the second superconducting layer and the connection layer is 1% or more and 50% or less. the second material includes a plurality of particles, and in a cross section perpendicular to the first interface, at least some of the particles are in contact with the first superconducting layer and have a flat shape, and in the cross section, at least another part of the particles are in contact with the second superconducting layer and have a flat shape. . [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a schematic cross-sectional view of a connection structure of superconducting layers according to the first embodiment. [Diagram 2] 3A to 3C are diagrams showing preparation of a first superconducting layer and a second superconducting layer in the method for connecting superconducting layers according to the first embodiment. [Diagram 3] 4A to 4C are diagrams illustrating removal of a first protective layer and a second protective layer in the method for connecting superconducting layers according to the first embodiment. [Figure 4] 4A to 4C are diagrams illustrating application of a slurry onto a first superconducting layer and a second superconducting layer in the method for connecting superconducting layers according to the first embodiment. [Diagram 5] 3 is a diagram showing a state in which a first superconducting layer and a second superconducting layer are opposed to each other in the method for connecting superconducting layers according to the first embodiment. FIG. [Figure 6] 3 is a diagram showing a state in which a first superconducting layer and a second superconducting layer are superimposed in the method for connecting superconducting layers according to the first embodiment. FIG. [Figure 7] 4 is a diagram showing a state in which a first superconducting layer and a second superconducting layer are pressurized in the method for connecting superconducting layers according to the first embodiment. FIG. [Figure 8] FIG. 4 is a schematic cross-sectional view of a connection structure of superconducting layers in a comparative example. [Figure 9]FIG. 6 is a schematic cross-sectional view of a connection structure of superconducting layers according to a second embodiment. [Figure 10] FIG. 11 is a schematic cross-sectional view of a connection structure of superconducting layers according to a third embodiment. [Figure 11] FIG. 11 is a schematic cross-sectional view of a superconducting wire according to a fourth embodiment. [Figure 12] FIG. 13 is a schematic cross-sectional view of a first modified example of the superconducting wire according to the fourth embodiment. [Figure 13] FIG. 13 is a schematic cross-sectional view of a second modified example of the superconducting wire according to the fourth embodiment. [Figure 14] FIG. 13 is a schematic cross-sectional view of a superconducting wire according to a sixth embodiment. [Figure 15] FIG. 13 is a schematic cross-sectional view of a first modified example of the superconducting wire according to the sixth embodiment. [Figure 16] FIG. 13 is a schematic cross-sectional view of a second modified example of the superconducting wire of the sixth embodiment. [Figure 17] FIG. 13 is a schematic cross-sectional view of a third modified example of the superconducting wire of the sixth embodiment. [Figure 18] FIG. 13 is a schematic perspective view of a superconducting coil according to a seventh embodiment. [Figure 19] FIG. 13 is a schematic cross-sectional view of a superconducting coil according to a seventh embodiment. [Figure 20] FIG. 13 is a block diagram of a superconducting device according to an eighth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals will be used to designate the same or similar components, and the description of components that have already been described may be omitted as appropriate.
[0009] In this specification, the "particle size" of a particle, etc., is the long diameter of the particle, unless otherwise specified. The long diameter of a particle is the maximum length among the lengths between any two points on the periphery of the particle. The short diameter of a particle is the length between two points that pass through the midpoint of the two points that are the basis of the long diameter of the particle and intersect with the periphery of the particle, which is perpendicular to the long diameter direction of the particle. The aspect ratio of a particle is the ratio of the long diameter to the short diameter (long diameter / short diameter). The long diameter and short diameter of a particle can be determined, for example, by image analysis of a scanning electron microscope image (SEM image). The above definition of "particle size" is an example, and the definition of "particle size" is not limited to this.
[0010] In this specification, the detection of elements contained in particles and the measurement of the atomic concentration of elements can be performed, for example, by energy dispersive X-ray spectroscopy (EDX) or wavelength dispersive X-ray analysis (WDX). Furthermore, the identification of substances contained in particles can be performed, for example, by powder X-ray diffraction.
[0011] (First embodiment) The connection structure of the superconducting layer of the first embodiment includes a first superconducting layer, a second superconducting layer, and a connection layer provided between the first superconducting layer and the second superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). At a first interface between the first superconducting layer and the connecting layer, a first area ratio per unit area of a first region where the second material and the first superconducting layer contact is 1% or more and 50% or less, and at a second interface between the second superconducting layer and the connecting layer, a second area ratio per unit area of a second region where the second material and the second superconducting layer contact is 1% or more and 50% or less.
[0012] 1 is a schematic cross-sectional view of a connection structure of superconducting layers according to a first embodiment. The connection structure 100 of the first embodiment is a structure that physically and electrically connects two superconducting layers. The connection structure 100 is used, for example, to connect two superconducting wires and extend the length of the superconducting wires.
[0013] The connection structure 100 includes a first superconducting member 10, a second superconducting member 20, and a connection layer 30. The connection structure 100 is a structure in which the first superconducting member 10 and the second superconducting member 20 are connected by the connection layer 30. The connection layer 30 is provided between the first superconducting member 10 and the second superconducting member 20.
[0014] The first superconducting member 10 comprises a first substrate 12, a first intermediate layer 14, and a first superconducting layer 16. The second superconducting member 20 comprises a second substrate 22, a second intermediate layer 24, and a second superconducting layer 26.
[0015] The first substrate 12 is, for example, a metal. The first substrate 12 is, for example, a nickel alloy or a copper alloy. The first substrate 12 is, for example, a nickel-tungsten alloy.
[0016] The first superconducting layer 16 is, for example, an oxide superconducting layer. The first superconducting layer 16 includes, for example, a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first superconducting layer 16 includes, for example, at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0017] The first superconducting layer 16 is, for example, (RE)Ba2Cu3O δ (RE is a rare earth element, 6≦δ≦7) The first superconducting layer 16 has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3Oδ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7). The first superconducting layer 16 is, for example, a rare earth oxide superconductor.
[0018] The first superconducting layer 16 includes, for example, a single crystal having a perovskite structure.
[0019] The first superconducting layer 16 is formed on the first intermediate layer 14, for example, by using a metal organic deposition method (MOD method), a pulsed laser deposition method (PLD method), or a metal organic chemical vapor deposition method (MOCVD method).
[0020] The first intermediate layer 14 is provided between the first substrate 12 and the first superconducting layer 16. The first intermediate layer 14 is in contact with, for example, the first superconducting layer 16. The first intermediate layer 14 has a function of improving the crystal orientation of the first superconducting layer 16 formed on the first intermediate layer 14.
[0021] The first intermediate layer 14 includes, for example, a rare earth oxide. The first intermediate layer 14 has, for example, a laminated structure of a plurality of films. The first intermediate layer 14 has, for example, a structure in which yttrium oxide (Y2O3), yttria-stabilized zirconia (YSZ), and cerium oxide (CeO2) are laminated from the first substrate 12 side.
[0022] The second substrate 22 is, for example, a metal. The second substrate 22 is, for example, a nickel alloy or a copper alloy. The second substrate 22 is, for example, a nickel-tungsten alloy.
[0023] The second superconducting layer 26 is, for example, an oxide superconducting layer. The second superconducting layer 26 includes, for example, a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first superconducting layer 16 includes, for example, at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0024] The second superconducting layer 26 is, for example, (RE)Ba2Cu3O δ (RE is a rare earth element, 6≦δ≦7) The first superconducting layer 16 has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3O δ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7). The first superconducting layer 16 is, for example, a rare earth oxide superconductor.
[0025] The second superconducting layer 26 includes, for example, a single crystal having a perovskite structure.
[0026] The second superconducting layer 26 is formed on the second intermediate layer 24 by, for example, the MOD method, the PLD method, or the MOCVD method.
[0027] The second intermediate layer 24 is provided between the second substrate 22 and the second superconducting layer 26. The second intermediate layer 24 is in contact with, for example, the second superconducting layer 26. The second intermediate layer 24 has a function of improving the crystal orientation of the second superconducting layer 26 formed on the second intermediate layer 24.
[0028] The second intermediate layer 24 includes, for example, a rare earth oxide. The second intermediate layer 24 has, for example, a laminated structure of a plurality of films. The second intermediate layer 24 has, for example, a structure in which yttrium oxide (Y2O3), yttria-stabilized zirconia (YSZ), and cerium oxide (CeO2) are laminated from the second substrate 22 side.
[0029] The connection layer 30 is provided between the first superconducting layer 16 and the second superconducting layer 26. The connection layer 30 contacts the first superconducting layer 16. The connection layer 30 contacts the second superconducting layer 26.
[0030] The interface between the first superconducting layer 16 and the connecting layer 30 is a first interface (P1 in FIG. 1), and the interface between the second superconducting layer 26 and the connecting layer 30 is a second interface (P2 in FIG. 1).
[0031] The connecting layer 30 is used to physically and electrically connect the first superconducting layer 16 and the second superconducting layer 26 .
[0032] The connecting layer 30 includes a first material 30a and a second material 30b.
[0033] The first material 30a contacts the first superconducting layer 16. The first material 30a contacts the second superconducting layer .
[0034] The first material 30a is an oxide superconductor. The first material 30a includes rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O). The first material 30a includes at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0035] The first material 30a is, for example, (RE)Ba2Cu3O δ(RE is a rare earth element, 6≦δ≦7) The first material 30a has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3O δ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7).
[0036] The first substance 30a includes, for example, crystals having a perovskite structure.
[0037] The first substance 30a is, for example, in the form of a plate.
[0038] The second material 30b contacts the first superconducting layer 16. The second material 30b contacts the second superconducting layer .
[0039] The second material 30b is a conductor, for example, a metal.
[0040] The second material 30b includes at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The second material 30b is, for example, silver (Ag).
[0041] The second substance 30b contains, for example, oxygen (O). The atomic concentration of oxygen (O) contained in the second substance 30b is, for example, not less than 0.01% and not more than 35%.
[0042] At a first interface P1 between the first superconducting layer 16 and the connection layer 30, the area ratio per unit area of a first region where the second material 30b and the first superconducting layer 16 contact is 1% or more and 50% or less. Also, at a second interface P2 between the second superconducting layer 26 and the connection layer 30, the area ratio per unit area of a second region where the second material 30b and the second superconducting layer 26 contact is 1% or more and 50% or less. The unit area is, for example, 1 mm 2 It is.
[0043] The area ratio of the first region is obtained, for example, by obtaining a ratio of the length where the second material 30b contacts the first superconducting layer 16 to the length of the first interface P1 in cross sections of multiple connection layers 30 parallel to the direction from the first superconducting layer 16 to the second superconducting layer 26, and calculating an average value of the obtained multiple length ratios. The area ratio of the second region is obtained, for example, by obtaining a ratio of the length where the second material 30b contacts the second superconducting layer 26 to the length of the second interface P2 in cross sections of multiple connection layers 30 parallel to the direction from the first superconducting layer 16 to the second superconducting layer 26, and calculating an average value of the obtained multiple length ratios.
[0044] The second substance 30b includes a plurality of particles, for example, as shown in Fig. 1. The median value of the major axis of the plurality of particles is, for example, not less than 100 nm and not more than 10 µm.
[0045] For example, among the plurality of particles, the aspect ratio of a particle in contact with the first interface P1 is 5 or more and 100 or less. Also, among the plurality of particles, the aspect ratio of a particle in contact with the second interface P2 is 5 or more and 100 or less.
[0046] 1, the major axis direction of the particles is aligned in a direction parallel to the first interface P1 or the second interface P2. In particular, the major axis direction of the particles in contact with the first superconducting layer 16 or the second superconducting layer 26 is aligned in a direction parallel to the first interface P1 or the second interface P2.
[0047] The major axis direction of the particle is, for example, in the range of 0 to 30 degrees with respect to the first interface P1, and the major axis direction of the particle is, for example, in the range of 0 to 30 degrees with respect to the second interface P2.
[0048] Next, an example of a method for connecting superconducting layers according to the first embodiment will be described. The method for connecting superconducting layers according to the first embodiment is a method for forming a connection structure 100. Figures 2, 3, 4, 5, 6, and 7 are diagrams showing the method for connecting superconducting layers according to the first embodiment.
[0049] A method for connecting superconducting layers in a first embodiment includes preparing a first superconducting layer and a second superconducting layer, sandwiching a substance containing a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O) and silver oxide between the first superconducting layer and the second superconducting layer, and performing a heat treatment while applying pressure to the first superconducting layer and the second superconducting layer.
[0050] First, a first superconducting layer 16 and a second superconducting layer 26 are prepared. A first superconducting member 10 and a second superconducting member 20 are prepared (FIG. 2).
[0051] The first superconducting member 10 includes a first substrate 12, a first intermediate layer 14, a first superconducting layer 16, and a first protective layer 18. The first protective layer 18 is provided on the first superconducting layer 16. The first protective layer 18 has a function of protecting the first superconducting layer 16.
[0052] The first protective layer 18 is, for example, a metal. The first protective layer 18 includes, for example, silver (Ag) or copper (Cu).
[0053] The second superconducting member 20 includes a second substrate 22, a second intermediate layer 24, a second superconducting layer 26, and a second protective layer 28. The second protective layer 28 is provided on the second superconducting layer 26. The second protective layer 28 has a function of protecting the second superconducting layer 26.
[0054] The second protective layer 28 is, for example, a metal. The second protective layer 28 includes, for example, silver (Ag) or copper (Cu).
[0055] Next, the first protective layer 18 on the first superconducting layer 16 is removed. Next, the second protective layer 28 on the second superconducting layer 26 is removed (FIG. 3). The first protective layer 18 and the second protective layer 28 are removed by using, for example, a wet etching method.
[0056] Next, a slurry 29 is prepared. The slurry 29 contains silver oxide particles 29a. Next, a slurry 29 is applied onto the first superconducting layer 16 and the second superconducting layer 26 (FIG. 4).
[0057] Next, the first material 30a is prepared. The first material 30a is in the form of a plate.
[0058] The first material 30a includes rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O). The first material 30a is a rare earth oxide. The first material 30a is, for example, GdBa2Cu3O δ It is a sintered body with (6≦δ≦7).
[0059] The first material 30a is, for example, a composite of a rare earth oxide superconductor produced by the MOD method and a sintered body of a rare earth oxide superconductor sintered from an oxide raw material. δ A composite can be produced by applying a MOD solution to a sintered body with (6≦δ≦7) and subjecting it to heat treatment. The heat treatment temperature is, for example, 700°C or higher and 850°C or lower. The heat treatment is performed, for example, at atmospheric pressure. The heat treatment is performed, for example, in an air atmosphere, an Ar atmosphere, a nitrogen atmosphere, an oxygen atmosphere, a mixed atmosphere of Ar and oxygen, or a mixed atmosphere of nitrogen and oxygen. By using the composite, the electrical connectivity between the connection layer 30 and the first and second superconducting layers 16 and 26 can be improved, and the electrical resistance can be reduced.
[0060] Next, for example, the second superconducting layer 26 is inverted to face the first superconducting layer 16 and the second superconducting layer 26 with the first material 30a and the slurry 29 sandwiched therebetween (FIG. 5). Then, the first superconducting layer 16 and the second superconducting layer 26 are superimposed with the first material 30a sandwiched therebetween (FIG. 6).
[0061] Next, the overlapping first superconducting layer 16 and second superconducting layer 26 are pressurized in the direction from the second superconducting layer 26 to the first superconducting layer 16 (FIG. 7). For example, pressure is applied by placing a weight on the overlapping portion. For example, pressure is applied using a press. For example, pressure can be applied by creating a jig for pressurization and clamping the two together. When a jig is used, the jig may be removed after connection, or may remain attached. Removing the jig makes it easier to wind the coil, so it is preferable to remove it.
[0062] Next, a heat treatment is performed while the first superconducting layer 16 and the second superconducting layer 26 are under pressure.
[0063] The temperature of the heat treatment is, for example, 300° C. or more and 850° C. or less. For example, it is preferable that the temperature is 400° C. or more and 800° C. or less. The heat treatment is performed, for example, at atmospheric pressure. The first heat treatment is performed, for example, in an air atmosphere, an Ar atmosphere, a nitrogen atmosphere, an oxygen atmosphere, a mixed atmosphere of Ar and oxygen, or a mixed atmosphere of nitrogen and oxygen.
[0064] Through the heat treatment, the silver oxide particles 29a are sintered while being reduced, so that large-sized silver particles are formed at the interface between the first superconducting layer 16 and the connecting layer 30 and at the interface between the second superconducting layer 26 and the connecting layer 30.
[0065] Next, a second heat treatment may be performed at a second temperature. The second heat treatment is performed in an atmosphere containing oxygen. The second heat treatment is performed in an atmosphere having the same oxygen partial pressure as the first heat treatment or a higher oxygen partial pressure than the first heat treatment. The second heat treatment is an oxygen anneal.
[0066] The second temperature is, for example, lower than the first temperature. The second temperature is, for example, 400° C. or higher and 600° C. or lower. The second heat treatment may be performed by cooling the first heat treatment to a temperature lower than the second temperature and then reheating to the second temperature. The second heat treatment may also be performed by continuously lowering the temperature to the second temperature after the first heat treatment.
[0067] The second heat treatment is performed, for example, under atmospheric pressure, and the oxygen partial pressure of the atmosphere for the second heat treatment is, for example, 30% or more.
[0068] By the above method, the first superconducting layer 16 and the second superconducting layer 26 are connected together. By the above method, the connection structure 100 of the first embodiment shown in FIG.
[0069] Next, the operation and effects of the superconducting layer connection structure and the superconducting layer connection method of the first embodiment will be described.
[0070] For example, nuclear magnetic resonance (NMR) and magnetic resonance imaging (MRI) devices use superconducting coils to generate strong magnetic fields. Superconducting coils are formed by winding superconducting wire around a bobbin.
[0071] In order to make a superconducting wire longer, for example, a plurality of superconducting wires are connected. For example, the ends of two superconducting wires are connected using a connection structure. The connection structure for connecting the superconducting wires is required to have low electrical resistance and high mechanical strength.
[0072] The connection structure 100 of the superconducting layers of the first embodiment uses a connection layer 30 including a first material 30a and a second material 30b. The first material 30a is a rare earth oxide superconductor. The second material 30b is a metal. By using the connection layer 30 including a rare earth oxide superconductor and a metal, a connection structure 100 having low electrical resistance and high mechanical strength can be realized.
[0073] Moreover, in the method for connecting superconducting layers in the first embodiment, the connection layer 30 is formed using silver oxide. By forming the connection layer 30 using silver oxide, it is possible to realize the connection structure 100 having low electrical resistance and high mechanical strength. This will be described in detail below.
[0074] 8 is a schematic cross-sectional view of a connection structure of superconducting layers of a comparative example. A connection structure 900 of superconducting layers of the comparative example differs from the connection structure 100 of the first embodiment in that the connection layer 30 does not include the second material 30b.
[0075] For example, when stress is applied to the connection structure 900, the connection layer 30 and the first superconducting layer 16 may be separated at a first interface (P1 in FIG. 8) between the connection layer 30 and the first superconducting layer 16. Also, when stress is applied to the connection structure 900, the connection layer 30 and the second superconducting layer 26 may be separated at a second interface (P2 in FIG. 8) between the connection layer 30 and the second superconducting layer 26.
[0076] In the connection structure 100 of superconducting layers of the first embodiment, the second material 30b contained in the connection layer 30 contacts the first superconducting layer 16, thereby increasing the connection strength between the connection layer 30 and the first superconducting layer 16 at the first interface P1. Also, in the connection structure 100 of superconducting layers of the first embodiment, the second material 30b contained in the connection layer 30 contacts the second superconducting layer 26, thereby increasing the connection strength between the connection layer 30 and the second superconducting layer 26 at the second interface P2. Therefore, a connection structure 100 with high mechanical strength can be realized.
[0077] The first material 30a included in the connection layer 30 contacts the first superconducting layer 16, thereby ensuring a path for the superconductor to continue at the first interface P1. The first material 30a included in the connection layer 30 contacts the second superconducting layer 26, thereby ensuring a path for the superconductor to continue at the second interface P2. This reduces the contact resistance at the first interface P1 and the second interface P2, thereby realizing a connection structure 100 with low electrical resistance. This increases the critical current that can flow through the connection structure 100.
[0078] At the first interface P1 between the first superconducting layer 16 and the connection layer 30, the first area ratio per unit area of the first region where the second material 30b and the first superconducting layer 16 contact is 1% or more and 50% or less. If the first area ratio is less than 1%, the connection strength between the connection layer 30 and the first superconducting layer 16 at the first interface P1 is insufficient. If the first area ratio exceeds 50%, the electrical resistance of the connection structure 100 becomes too high.
[0079] From the viewpoint of increasing the connection strength between the connection layer 30 and the first superconducting layer 16 at the first interface P1, the first area ratio is preferably 5% or more, and more preferably 8% or more. Also, from the viewpoint of decreasing the electrical resistance of the connection structure 100, the first area ratio is preferably 30% or less, and more preferably 15% or less.
[0080] At the second interface P2 between the second superconducting layer 26 and the connection layer 30, the second area ratio per unit area of the second region where the second material 30b and the second superconducting layer 26 contact is 1% or more and 50% or less. If the second area ratio is less than 1%, the connection strength between the connection layer 30 and the second superconducting layer 26 at the second interface P2 is insufficient. If the second area ratio exceeds 50%, the electrical resistance of the connection structure 100 becomes too high.
[0081] From the viewpoint of increasing the connection strength between the connection layer 30 and the second superconducting layer 26 at the second interface P2, the second area ratio is preferably 5% or more, and more preferably 8% or more. Also, from the viewpoint of decreasing the electrical resistance of the connection structure 100, the second area ratio is preferably 30% or less, and more preferably 15% or less.
[0082] The second substance 30b includes a plurality of particles, and the median value of the major axis of the plurality of particles is preferably 100 nm or more and 10 μm or less. When the median value of the major axis is 100 nm or more, the connection strength at the first interface P1 or the second interface P2 is high. Furthermore, when the median value of the major axis is 10 μm or less, the electrical resistance of the connection structure 100 is low.
[0083] The second substance 30b includes a plurality of particles, and among the plurality of particles, the aspect ratio of the particles in contact with the first interface P1 is preferably 5 or more, and more preferably 10 or more. Similarly, among the plurality of particles, the aspect ratio of the particles in contact with the second interface P2 is preferably 5 or more, and more preferably 10 or more. When the aspect ratio of the particles exceeds the above-mentioned lower limit, it becomes easy to simultaneously improve the connection strength of the first interface P1 and the second interface P2 of the connection structure 100 and reduce the electrical resistance of the connection structure 100.
[0084] The major axis direction of the particles of the second material 30b is preferably aligned in a direction parallel to the first interface P1 or the second interface P2. In particular, the major axis direction of the particles in contact with the first superconducting layer 16 or the second superconducting layer 26 is preferably aligned in a direction parallel to the first interface P1 or the second interface P2.
[0085] The major axis direction of the particles of the second substance 30b is preferably in the range of 0 to 30 degrees with respect to the first interface P1. Also, the major axis direction of the particles is preferably in the range of 0 to 30 degrees with respect to the second interface P2, for example.
[0086] By aligning the long diameter direction of the particles of the second substance 30b in a direction parallel to the first interface P1 or the second interface P2, it becomes easier to simultaneously improve the connection strength of the first interface P1 and the second interface P2 of the connection structure 100 and reduce the electrical resistance of the connection structure 100.
[0087] The second material 30b preferably contains oxygen (O). When the second material 30b contains oxygen, the mechanical strength of the second material 30b is improved. Therefore, the mechanical strength of the connection structure 100 is improved.
[0088] Moreover, the second material 30b bonds to the first superconducting layer 16, the second superconducting layer 26, and the first material 30a. Since the first superconducting layer 16, the second superconducting layer 26, and the first material 30a are all oxides, the second material 30b containing oxygen makes it easier to bond to the first superconducting layer 16, the second superconducting layer 26, and the first material 30a, improving the bonding strength.
[0089] Moreover, the first superconducting layer 16, the second superconducting layer 26, and the first material 30a are, for example, rare earth oxide superconductors. The superconducting properties of rare earth oxide superconductors are significantly reduced by oxygen defects. When the second material 30b contains oxygen, oxygen desorption from the first superconducting layer 16, the second superconducting layer 26, and the first material 30a is suppressed. Therefore, the high superconducting properties of the first superconducting layer 16, the second superconducting layer 26, and the first material 30a can be maintained.
[0090] From the viewpoints of improving the mechanical strength of the second material 30b, improving the bonding strength of the second material 30b, and maintaining high superconducting properties of the first superconducting layer 16, the second superconducting layer 26, and the first material 30a, the atomic concentration of oxygen (O) contained in the second material 30b is preferably 0.01% or more, more preferably 0.05% or more, and even more preferably 0.1% or more. On the other hand, from the viewpoint of reducing the electrical resistance of the second material 30b, the atomic concentration of oxygen (O) contained in the second material 30b is preferably 35% or less, more preferably 15% or less, and even more preferably 5% or less.
[0091] The method for connecting superconducting layers in the first embodiment involves sandwiching silver oxide particles 29a between the first superconducting layer 16 and the first material 30a, and between the second superconducting layer 26 and the first material 30a, and then applying heat treatment to form the connection layer 30. The heat treatment sinters the silver oxide particles 29a while reducing them, and large grain sizes are formed at the interface between the first superconducting layer 16 and the connection layer 30, and at the interface between the second superconducting layer 26 and the connection layer 30. The large grain sizes are the second material 30b.
[0092] By using silver oxide particles 29a, the particles are sintered at a lower temperature than when silver particles are used, for example. Therefore, particles with a large diameter can be formed at a low temperature. Therefore, the first superconducting layer 16, the second superconducting layer 26, and the first material 30a, which are made of oxide superconductors, can be prevented from being exposed to high temperatures. Therefore, deterioration of the superconducting properties of the first superconducting layer 16, the second superconducting layer 26, and the first material 30a can be prevented, and a connection structure 100 having low electrical resistance and high mechanical strength can be realized.
[0093] As described above, according to the superconducting layer connection structure and the superconducting layer connection method of the first embodiment, low electrical resistance and high mechanical strength can be achieved.
[0094] Second Embodiment The connection structure of the superconducting layers of the second embodiment differs from the connection structure of the superconducting layers of the first embodiment in that the first substance contains a plurality of particles. In the following, some of the contents that overlap with the first embodiment may be omitted.
[0095] 9 is a schematic cross-sectional view of a connection structure of superconducting layers according to the second embodiment. The connection structure 200 of the second embodiment is a structure that physically and electrically connects two superconducting layers. The connection structure 200 is used, for example, to connect two superconducting wires and elongate the superconducting wires.
[0096] The connection structure 200 includes a first superconducting member 10, a second superconducting member 20, and a connection layer 30. The connection structure 200 is a structure in which the first superconducting member 10 and the second superconducting member 20 are connected by the connection layer 30. The connection layer 30 is provided between the first superconducting member 10 and the second superconducting member 20.
[0097] The connecting layer 30 includes a first material 30a and a second material 30b.
[0098] The first material 30a includes a plurality of particles. The first material 30a is, for example, in a state in which the plurality of particles are sintered. Voids exist between the particles.
[0099] Each of the plurality of particles is an oxide superconductor. Each of the plurality of particles includes a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first material 30a includes at least one rare earth element (RE) selected from the group consisting of, for example, yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0100] Each of the plurality of particles is, for example, (RE)Ba2Cu3O δ(RE is a rare earth element, 6≦δ≦7) The first material 30a has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3O δ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7).
[0101] Each of the plurality of particles includes, for example, a crystal having a perovskite structure.
[0102] The second material 30b contacts the first superconducting layer 16. The second material 30b contacts the second superconducting layer .
[0103] The second material 30b is a conductor, for example, a metal.
[0104] The second material 30b includes at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The second material 30b is, for example, silver (Ag).
[0105] The second substance 30b contains, for example, oxygen (O). The atomic concentration of oxygen (O) contained in the second substance 30b is, for example, not less than 0.01% and not more than 35%.
[0106] At a first interface P1 between the first superconducting layer 16 and the connecting layer 30, the area ratio per unit area of a first region where the second material 30b and the first superconducting layer 16 contact is 1% or more and 50% or less. Also, at a second interface P2 between the second superconducting layer 26 and the connecting layer 30, the area ratio per unit area of a second region where the second material 30b and the second superconducting layer 26 contact is 1% or more and 50% or less.
[0107] The second substance 30b includes, for example, a plurality of particles. The median value of the major axis of the plurality of particles is, for example, 100 nm or more and 10 μm or less.
[0108] For example, among the plurality of particles, the aspect ratio of a particle in contact with the first interface P1 is 5 or more and 100 or less. Also, among the plurality of particles, the aspect ratio of a particle in contact with the second interface P2 is 5 or more and 100 or less.
[0109] Next, an example of a method for connecting superconducting layers according to the second embodiment will be described. The method for connecting superconducting layers according to the second embodiment is a method for forming a connection structure 200.
[0110] The steps from preparing the first superconducting layer 16 and the second superconducting layer 26 to using and removing the first protective layer 18 and the second protective layer 28 are the same as the method of connecting superconducting layers in the first embodiment.
[0111] Next, a slurry is prepared, the slurry including the first crystal particles, the first particles, the second particles, the third particles, and silver oxide particles.
[0112] The first crystalline particles will eventually become part of the first material 30a, and the silver oxide particles will eventually become part of the second material 30b.
[0113] The first crystal particles include a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first crystal particles are rare earth oxides. The first crystal particles are, for example, single crystals or polycrystals having a perovskite structure. The first crystal particles are, for example, (RE)Ba2Cu3O δ It has a chemical composition expressed as (RE is rare earth element, 6≦δ≦7).
[0114] The first crystal particles have, for example, a plate-like or flat shape. The median particle size of the first crystal particles is, for example, 100 nm or more and 10 μm or less.
[0115] The first crystal particles are formed, for example, by pulverizing a rare earth oxide superconductor, which is formed, for example, by sintering a powder raw material.
[0116] The first crystal particles are, for example, a composite of a powder obtained by crushing a sintered body of a rare earth oxide superconductor and a rare earth oxide superconductor produced by the MOD method. For example, GdBa2Cu3O δ A composite can be produced by applying an MOD solution to sintered powder (6≦δ≦7) and heat treating it. The heat treatment temperature is, for example, 700°C or higher and 850°C or lower. The heat treatment is performed, for example, at atmospheric pressure. The heat treatment is performed, for example, in an air atmosphere, an Ar atmosphere, a nitrogen atmosphere, an oxygen atmosphere, a mixed atmosphere of Ar and oxygen, or a mixed atmosphere of nitrogen and oxygen. By using the composite, the electrical connectivity between the connection layer 30 and the first and second superconducting layers 16 and 26 can be improved, and the electrical resistance can be reduced.
[0117] The first particles include rare earth elements (RE) and oxygen (O). The first particles have a chemical composition expressed as, for example, RE2O3 (RE is a rare earth element).
[0118] The second particles include barium (Ba), carbon (C), and oxygen (O). The second particles have a chemical composition expressed as, for example, BaCO3.
[0119] The third particles include copper (Cu) and oxygen (O). The third particles have a chemical composition expressed as, for example, CuO.
[0120] The slurry 29 includes, for example, a sintering aid and a thickening agent. The sintering aid is, for example, sodium alginate.
[0121] Next, the slurry is applied onto the second superconducting layer 26 .
[0122] Next, for example, the second superconducting layer 26 is turned over and the first superconducting layer 16 and the second superconducting layer 26 are placed opposite each other with the slurry sandwiched therebetween. Then, the first superconducting layer 16 and the second superconducting layer 26 are superposed on each other.
[0123] Next, the overlapping first superconducting layer 16 and second superconducting layer 26 are pressed in a direction from the second superconducting layer 26 toward the first superconducting layer 16 .
[0124] Next, a first heat treatment is performed at a first temperature while the first superconducting layer 16 and the second superconducting layer 26 are under pressure.
[0125] The first temperature is, for example, 500° C. or more and 850° C. or less. For example, it is preferably 600° C. or more and 800° C. or less. The first heat treatment is performed, for example, at atmospheric pressure. The first heat treatment is performed, for example, in an air atmosphere, an Ar atmosphere, a nitrogen atmosphere, an oxygen atmosphere, a mixed atmosphere of Ar and oxygen, or a mixed atmosphere of nitrogen and oxygen.
[0126] The first heat treatment causes the first particles, the second particles, and the third particles to react to form second crystal particles that are superconductors. The first particles, the second particles, and the third particles are the raw materials for the second crystal particles that are superconductors. The second crystal particles eventually become part of the first material 30a.
[0127] The second crystal particles 32 contain a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The second crystal particles 32 are rare earth oxides. The second crystal particles 32 are, for example, single crystals or polycrystals having a perovskite structure. The second crystal particles 32 are, for example, (RE)Ba2Cu3O δ It has a chemical composition expressed as (RE is rare earth element, 6≦δ≦7).
[0128] The second crystal particles 32 are, for example, spherical or amorphous. The median diameter of the second crystal particles 32 is smaller than the median diameter of the first crystal particles 31. The median diameter of the second crystal particles 32 is, for example, not less than 10 nm and less than 1 μm.
[0129] For example, the first particles, the second particles, and the third particles that did not contribute to the formation of the second crystal particles remain in the connection layer 30.
[0130] The first heat treatment sinters the first crystal particles and the second crystal particles.
[0131] The first heat treatment causes the silver oxide particles to be sintered while being reduced, so that large-sized silver particles are formed at the interface between the first superconducting layer 16 and the connecting layer 30 and at the interface between the second superconducting layer 26 and the connecting layer 30.
[0132] Next, a second heat treatment is performed at a second temperature. The second heat treatment is performed in an atmosphere containing oxygen. The second heat treatment is performed in an atmosphere having the same oxygen partial pressure as the first heat treatment or a higher oxygen partial pressure than the first heat treatment. The second heat treatment is an oxygen anneal.
[0133] The second temperature is, for example, lower than the first temperature. The second temperature is, for example, 400° C. or higher and 600° C. or lower. The second heat treatment may be performed by cooling the first heat treatment to a temperature lower than the second temperature and then reheating to the second temperature. The second heat treatment may also be performed by continuously lowering the temperature to the second temperature after the first heat treatment.
[0134] The second heat treatment is performed, for example, under atmospheric pressure, and the oxygen partial pressure of the atmosphere for the second heat treatment is, for example, 30% or more.
[0135] The connection layer 30 is formed by the first heat treatment and the second heat treatment.
[0136] By the above method, the first superconducting layer 16 and the second superconducting layer 26 are connected together. By the above method, the connection structure 200 of the second embodiment is formed.
[0137] As described above, according to the superconducting layer connection structure and the superconducting layer connection method of the second embodiment, low electrical resistance and high mechanical strength can be achieved.
[0138] (Third embodiment) The superconducting layer connection structure of the third embodiment includes a first superconducting layer, a second superconducting layer, and a connection layer provided between the first superconducting layer and the second superconducting layer, the connection layer including a first material including rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O), and a second material including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn), the second material being in contact with the first superconducting layer and the second superconducting layer, and the second material being continuous between the first superconducting layer and the second superconducting layer. The superconducting layer connection structure of the third embodiment is different from the superconducting layer connection structure of the first embodiment in that the second material is continuous between the first superconducting layer and the second superconducting layer. Hereinafter, some of the contents that overlap with the first embodiment will be omitted.
[0139] 10 is a schematic cross-sectional view of a connection structure of superconducting layers according to the third embodiment. The connection structure 300 of the third embodiment is a structure that physically and electrically connects two superconducting layers. The connection structure 300 is used, for example, to connect two superconducting wires and elongate the superconducting wires.
[0140] The connection structure 300 includes a first superconducting member 10, a second superconducting member 20, and a connection layer 30. The connection structure 300 is a structure in which the first superconducting member 10 and the second superconducting member 20 are connected by the connection layer 30. The connection layer 30 is provided between the first superconducting member 10 and the second superconducting member 20.
[0141] The connecting layer 30 includes a first material 30a and a second material 30b.
[0142] The first substance 30a includes a plurality of particles. The first substance 30a is, for example, in a state in which the plurality of particles are sintered.
[0143] Each of the plurality of particles is an oxide superconductor. Each of the plurality of particles includes a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first material 30a includes at least one rare earth element (RE) selected from the group consisting of, for example, yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0144] Each of the plurality of particles is, for example, (RE)Ba2Cu3O δ (RE is a rare earth element, 6≦δ≦7) The first material 30a has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3O δ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7).
[0145] Each of the plurality of particles includes, for example, a crystal having a perovskite structure.
[0146] The second material 30b contacts the first superconducting layer 16. The second material 30b contacts the second superconducting layer 26. The second material 30b is continuous between the first superconducting layer 16 and the second superconducting layer 26.
[0147] The second material 30b is a conductor, for example, a metal.
[0148] The second material 30b includes at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The second material 30b is, for example, silver (Ag).
[0149] The second substance 30b contains, for example, oxygen (O). The atomic concentration of oxygen (O) contained in the second substance 30b is, for example, not less than 0.01% and not more than 35%.
[0150] In a cross section parallel to the direction from the first superconducting layer 16 to the second superconducting layer 26, the area ratio of the second material 30b to a unit area is, for example, not less than 5% and not more than 50%.
[0151] At a first interface P1 between the first superconducting layer 16 and the connection layer 30, the area ratio per unit area of the first region where the second material 30b and the first superconducting layer 16 contact is, for example, 1% or more and 50% or less. Also, at a second interface P2 between the second superconducting layer 26 and the connection layer 30, the area ratio per unit area of the second region where the second material 30b and the second superconducting layer 26 contact is, for example, 1% or more and 50% or less.
[0152] The superconducting layer connection structure 300 of the third embodiment can be formed, for example, by adjusting the size of the first crystal particles, the shape of the first crystal particles, the quantitative ratio of the first crystal particles to silver oxide particles, etc. in the superconducting layer connection method of the second embodiment.
[0153] For example, in the method for connecting superconducting layers according to the second embodiment, it is possible to form connection structure 300 by making the size of the first crystal grains relatively large and increasing the amount of silver oxide grains relatively.
[0154] In the connection structure 300, the second material 30b is continuous between the first superconducting layer 16 and the second superconducting layer 26, thereby achieving even higher mechanical strength compared to the connection structure 100 of the first embodiment.
[0155] In a cross section parallel to the direction from the first superconducting layer 16 to the second superconducting layer 26, the area ratio of the second material 30b per unit area is preferably 5% or more, and more preferably 10% or more. When the area ratio exceeds the lower limit, the mechanical strength of the connection structure 300 is further increased.
[0156] In a cross section parallel to the direction from the first superconducting layer 16 to the second superconducting layer 26, the area ratio of the second material 30b per unit area is preferably 50% or less, more preferably 40% or less, and even more preferably 30% or less. When the area ratio is below the upper limit, the electrical resistance of the connection structure 300 is further reduced.
[0157] As described above, according to the superconducting layer connection structure and the superconducting layer connection method of the third embodiment, low electrical resistance and high mechanical strength can be achieved.
[0158] (Fourth embodiment) The superconducting wire of the fourth embodiment comprises a first superconducting wire including a first superconducting layer, a second superconducting wire including a second superconducting layer, a third superconducting layer having a first surface and a second surface opposite to the first surface, and connecting layers provided between the first superconducting layer and the third superconducting layer and between the second superconducting layer and the third superconducting layer, the connecting layers including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The first superconducting layer and the second superconducting layer are located on the side of the first surface of the third superconducting layer, and at a first interface between the first superconducting layer and the connecting layer, a first area ratio per unit area of the first region where the second material and the first superconducting layer contact is 1% or more and 50% or less, at a second interface between the second superconducting layer and the connecting layer, a second area ratio per unit area of the second region where the second material and the second superconducting layer contact is 1% or more and 50% or less, and at a third interface between the third superconducting layer and the connecting layer, a third area ratio per unit area of the second region where the second material and the third superconducting layer contact is 1% or more and 50% or less. The superconducting wire of the fourth embodiment uses the superconducting layer connection structure of the first embodiment as a structure for connecting the first superconducting wire and the second superconducting wire. Hereinafter, some of the contents that overlap with the first embodiment will be omitted.
[0159] 11 is a schematic cross-sectional view of a superconducting wire according to a fourth embodiment. Superconducting wire 400 according to the fourth embodiment includes first superconducting wire 401, second superconducting wire 402, and connecting member 403. Superconducting wire 400 according to the fourth embodiment is elongated by connecting first superconducting wire 401 and second superconducting wire 402 using connecting member 403.
[0160] The first superconducting wire 401 includes a first substrate 12, a first intermediate layer 14, a first superconducting layer 16, and a first protective layer 18. The second superconducting wire 402 includes a second substrate 22, a second intermediate layer 24, a second superconducting layer 26, and a second protective layer 28. The connecting member 403 includes a third substrate 42, a third intermediate layer 44, and a third superconducting layer 46.
[0161] The first substrate 12 is, for example, a metal. The first substrate 12 is, for example, a nickel alloy or a copper alloy. The first substrate 12 is, for example, a nickel-tungsten alloy.
[0162] The first superconducting layer 16 is, for example, an oxide superconducting layer. The first superconducting layer 16 includes, for example, a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The first superconducting layer 16 includes, for example, at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0163] The first superconducting layer 16 includes, for example, a single crystal having a perovskite structure.
[0164] The first superconducting layer 16 is formed on the first intermediate layer 14 by using, for example, the MOD method, the PLD method, or the MOCVD method.
[0165] The first intermediate layer 14 is provided between the first substrate 12 and the first superconducting layer 16. The first intermediate layer 14 is in contact with, for example, the first superconducting layer 16. The first intermediate layer 14 has a function of improving the crystal orientation of the first superconducting layer 16 formed on the first intermediate layer 14.
[0166] The first intermediate layer 14 includes, for example, a rare earth oxide. The first intermediate layer 14 has, for example, a laminated structure of a plurality of films. The first intermediate layer 14 has, for example, a structure in which yttrium oxide (Y2O3), yttria-stabilized zirconia (YSZ), and cerium oxide (CeO2) are laminated from the first substrate 12 side.
[0167] The first protective layer 18 is provided on the first superconducting layer 16. The first protective layer 18 is in contact with, for example, the first superconducting layer 16. The first protective layer 18 has a function of protecting the first superconducting layer 16.
[0168] The first protective layer 18 is, for example, a metal. The first protective layer 18 includes, for example, silver (Ag) or copper (Cu).
[0169] The second substrate 22 is, for example, a metal. The second substrate 22 is, for example, a nickel alloy or a copper alloy. The second substrate 22 is, for example, a nickel-tungsten alloy.
[0170] The second superconducting layer 26 is, for example, an oxide superconducting layer. The second superconducting layer 26 includes, for example, a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The second superconducting layer 26 includes, for example, at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0171] The second superconducting layer 26 includes, for example, a single crystal having a perovskite structure.
[0172] The second superconducting layer 26 is formed on the second intermediate layer 24 by, for example, a metal organic deposition method (MOD method), a PLD method, or an MOCVD method.
[0173] The second intermediate layer 24 is provided between the second substrate 22 and the second superconducting layer 26. The second intermediate layer 24 is in contact with, for example, the second superconducting layer 26. The second intermediate layer 24 has a function of improving the crystal orientation of the second superconducting layer 26 formed on the second intermediate layer 24.
[0174] The second intermediate layer 24 includes, for example, a rare earth oxide. The second intermediate layer 24 has, for example, a laminated structure of a plurality of films. The second intermediate layer 24 has, for example, a structure in which yttrium oxide (Y2O3), yttria-stabilized zirconia (YSZ), and cerium oxide (CeO2) are laminated from the second substrate 22 side.
[0175] The second protective layer 28 is provided on the second superconducting layer 26. The second protective layer 28 is in contact with, for example, the second superconducting layer 26. The second protective layer 28 has a function of protecting the second superconducting layer 26.
[0176] The second protective layer 28 is, for example, a metal. The second protective layer 28 includes, for example, silver (Ag) or copper (Cu).
[0177] The third substrate 42 is, for example, a metal. The third substrate 42 is, for example, a nickel alloy or a copper alloy. The third substrate 42 is, for example, a nickel-tungsten alloy.
[0178] The third superconducting layer 46 has a first surface and a second surface. The first superconducting layer 16 and the second superconducting layer 26 are located on the first surface side of the third superconducting layer 46. In FIG. 11 , the first surface is the lower surface of the third superconducting layer 46, and the second surface is the upper surface of the third superconducting layer 46. The first superconducting layer 16 and the second superconducting layer 26 are located on the lower surface side of the third superconducting layer 46.
[0179] The third superconducting layer 46 is, for example, an oxide superconducting layer. The third superconducting layer 46 includes, for example, a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O). The third superconducting layer 46 includes, for example, at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0180] The third superconducting layer 46 includes, for example, a single crystal having a perovskite structure.
[0181] The third superconducting layer 46 is formed on the third intermediate layer 44 by using, for example, the MOD method, the PLD method, or the MOCVD method.
[0182] The third intermediate layer 44 is provided between the third substrate 42 and the third superconducting layer 46. The third intermediate layer 44 is in contact with, for example, the third superconducting layer 46. The third intermediate layer 44 has a function of improving the crystal orientation of the third superconducting layer 46 formed on the third intermediate layer 44.
[0183] The third intermediate layer 44 includes, for example, a rare earth oxide. The third intermediate layer 44 has, for example, a laminated structure of a plurality of films. The third intermediate layer 44 has, for example, a structure in which yttrium oxide (Y2O3), yttria-stabilized zirconia (YSZ), and cerium oxide (CeO2) are laminated from the third substrate 42 side.
[0184] For example, no protective layer is provided in contact with the third superconducting layer 46. For example, no metal protective layer is provided in contact with the third superconducting layer 46. For example, no protective layer containing silver (Ag) or copper (Cu) is provided in contact with the third superconducting layer 46.
[0185] The connection layer 30 is provided between the first superconducting layer 16 and the third superconducting layer 46. The connection layer 30 contacts the first superconducting layer 16. The connection layer 30 contacts the third superconducting layer 46.
[0186] The connection layer 30 is provided between the second superconducting layer 26 and the third superconducting layer 46. The connection layer 30 contacts the second superconducting layer 26. The connection layer 30 contacts the third superconducting layer 46.
[0187] The interface between the first superconducting layer 16 and the connecting layer 30 is a first interface (P1 in FIG. 11). The interface between the second superconducting layer 26 and the connecting layer 30 is a second interface (P2 in FIG. 11). The interface between the third superconducting layer 46 and the connecting layer 30 is a third interface (P3 in FIG. 11).
[0188] The connecting layer 30 between the first superconducting layer 16 and the third superconducting layer 46 and the connecting layer 30 between the second superconducting layer 26 and the third superconducting layer 46 are continuous.
[0189] The connection layer 30 is not present, for example, between the first superconducting layer 16 and the second superconducting layer 26. Between the first superconducting layer 16 and the second superconducting layer 26, for example, there is an air gap.
[0190] The connection layer 30 of the fourth embodiment has a similar configuration to the connection layer 30 of the first embodiment shown in FIG.
[0191] The connecting layer 30 includes a first material 30a and a second material 30b.
[0192] The first material 30a contacts the first superconducting layer 16. The first material 30a contacts the second superconducting layer 26. The first material 30a contacts the third superconducting layer 46.
[0193] The first material 30a is an oxide superconductor. The first material 30a includes rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O). The first material 30a includes at least one rare earth element (RE) selected from the group consisting of yttrium (Y), lanthanum (La), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0194] The first material 30a is, for example, (RE)Ba2Cu3O δ (RE is a rare earth element, 6≦δ≦7) The first material 30a has a chemical composition expressed as, for example, GdBa2Cu3O δ (6≦δ≦7), YBa2Cu3O δ (6≦δ≦7), or EuBa2Cu3O δ It has a chemical composition expressed as (6≦δ≦7).
[0195] The first substance 30a includes, for example, crystals having a perovskite structure.
[0196] The first substance 30a is, for example, in the form of a plate.
[0197] The second material 30b contacts the first superconducting layer 16. The second material 30b contacts the second superconducting layer 26. The second material 30b contacts the third superconducting layer 46.
[0198] The second material 30b is a conductor, for example, a metal.
[0199] The second material 30b includes at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The second material 30b is, for example, silver (Ag).
[0200] The second substance 30b contains, for example, oxygen (O). The atomic concentration of oxygen (O) contained in the second substance 30b is, for example, not less than 0.01% and not more than 35%.
[0201] At a first interface P1 between the first superconducting layer 16 and the connection layer 30, the area ratio per unit area of a first region where the second material 30b and the first superconducting layer 16 contact is 1% or more and 50% or less. At a second interface P2 between the second superconducting layer 26 and the connection layer 30, the area ratio per unit area of a second region where the second material 30b and the second superconducting layer 26 contact is 1% or more and 50% or less. At a third interface P3 between the third superconducting layer 46 and the connection layer 30, the area ratio per unit area of a third region where the second material 30b and the third superconducting layer 46 contact is 1% or more and 50% or less.
[0202] The second substance 30b includes, for example, a plurality of particles. The median value of the major axis of the plurality of particles is, for example, 100 nm or more and 10 μm or less.
[0203] For example, among the plurality of particles, the aspect ratio of a particle in contact with the first interface P1 is 5 or more and 100 or less. Also, among the plurality of particles, the aspect ratio of a particle in contact with the second interface P2 is 5 or more and 100 or less.
[0204] In superconducting wire 400 of the fourth embodiment, for example, a current flows from first superconducting wire 401 through connection layer 30, connection member 403, and connection layer 30 to second superconducting wire 402.
[0205] Since first superconducting wire 401 and connecting member 403 are connected using connecting layer 30, the connection structure connecting first superconducting wire 401 and connecting member 403 has low electrical resistance and high mechanical strength. Also, since second superconducting wire 402 and connecting member 403 are connected using connecting layer 30, the connection structure connecting second superconducting wire 402 and connecting member 403 has low electrical resistance and high mechanical strength.
[0206] Therefore, the connection structure that connects first superconducting wire 401 and second superconducting wire 402 has low electrical resistance and high mechanical strength. Therefore, superconducting wire 400 has low electrical resistance and high mechanical strength.
[0207] It is also possible to connect three or more superconducting wires to form a longer superconducting wire.
[0208] In the superconducting wire of the fourth embodiment, the case where the connection structure of the superconducting layers of the first embodiment is used has been described as an example, but the connection structure of the second embodiment can be used instead of the connection structure of the superconducting layers of the first embodiment. That is, the connection layer described in the second embodiment can be used as the connection layer 30.
[0209] (First Modification) 12 is a schematic cross-sectional view of a first modified example of the superconducting wire of the fourth embodiment. Superconducting wire 410 of the modified example of the fourth embodiment differs from superconducting wire 400 of the fourth embodiment in that it includes a reinforcing material 60.
[0210] Reinforcing material 60 is provided between first superconducting wire 401 and second superconducting wire 402. Reinforcing material 60 is provided between first superconducting layer 16 and second superconducting layer 26, for example.
[0211] Reinforcing material 60 is in contact with, for example, first superconducting wire 401 and second superconducting wire 402. Reinforcing material 60 is in contact with connecting layer 30, for example.
[0212] By providing reinforcing material 60, the mechanical strength of superconducting wire 410 is improved.
[0213] The reinforcing material 60 is, for example, a metal or a resin. The reinforcing material 60 is, for example, a solder. The reinforcing material 60 is, for example, a solder containing silver (Ag) and indium (In).
[0214] (Second Modification) 13 is a schematic cross-sectional view of a modified example of the superconducting wire of the fourth embodiment. Superconducting wire 420 of the modified example of the fourth embodiment differs from superconducting wire 400 of the fourth embodiment in that second substance 30b is disposed at both ends of connection layer 30.
[0215] The second substance 30b disposed at the end of the connection layer 30 is provided, for example, continuously between the first superconducting layer 16 and the superconducting layer 46 of the connection member 403. Also, the second substance 30b is provided continuously between the second superconducting layer 26 and the superconducting layer 46 of the connection member 403.
[0216] By disposing the second material 30b at the end of the connection layer 30, it is possible to disperse the stress applied to the opposing first superconducting layer 16 and second superconducting layer 26 when pressure is applied from above and below. This makes it possible to suppress cracks occurring in the first superconducting layer 16 and the second superconducting layer 26, and to realize a superconducting wire with high mechanical strength. It is also effective in obtaining a high critical current.
[0217] As described above, according to the fourth embodiment, a superconducting wire that is long and has low electrical resistance and high mechanical strength can be realized by connecting two superconducting wires.
[0218] Fifth embodiment The superconducting wire of the fifth embodiment includes a first superconducting wire including a first superconducting layer, a second superconducting wire including a second superconducting layer, a third superconducting layer having a first surface and a second surface opposite to the first surface, and connection layers provided between the first superconducting layer and the third superconducting layer and between the second superconducting layer and the third superconducting layer, the connection layers including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn). The first and second superconducting layers are located on the side of the first surface of the third superconducting layer, a portion of the second material contacts the first and third superconducting layers, a portion of the second material is continuous between the first and third superconducting layers, another portion of the second material contacts the second and third superconducting layers, and another portion of the second material is continuous between the second and third superconducting layers. The superconducting wire of the fifth embodiment differs from the superconducting wire of the fourth embodiment in that the superconducting wire of the fifth embodiment includes a connection layer similar to that of the third embodiment. Hereinafter, some of the contents that overlap with the fourth embodiment will be omitted.
[0219] The superconducting wire of the fifth embodiment has a structure similar to that of the superconducting wire 400 of the fourth embodiment shown in Fig. 11. The connection layer 30 of the fifth embodiment has a configuration similar to that of the connection layer 30 of the third embodiment shown in Fig. 10.
[0220] A portion of the second material 30b contacts the first superconducting layer 16 and the third superconducting layer 46, and a portion of the second material 30b is continuous between the first superconducting layer 16 and the third superconducting layer 46. A portion of the second material 30b is present in the connection layer 30 between the first superconducting layer 16 and the third superconducting layer 46.
[0221] Another portion of the second material 30b contacts the second superconducting layer 26 and the third superconducting layer 46, and another portion of the second material 30b is continuous between the second superconducting layer 26 and the third superconducting layer 46. A portion of the second material 30b is present in the connection layer 30 between the second superconducting layer 26 and the third superconducting layer 46.
[0222] As described above, according to the fifth embodiment, a superconducting wire that is long and has low electrical resistance and high mechanical strength can be realized by connecting two superconducting wires.
[0223] Sixth embodiment The superconducting wire of the sixth embodiment differs from the superconducting wire of the fourth or fifth embodiment in that the connection layer includes a first portion and a second portion that are spaced apart from each other. Hereinafter, some of the contents that overlap with the fourth or fifth embodiment will not be described.
[0224] 14 is a schematic cross-sectional view of a superconducting wire according to the sixth embodiment. A superconducting wire 600 according to the sixth embodiment includes a first superconducting wire 401, a second superconducting wire 402, and a connecting member 403. The superconducting wire 600 according to the sixth embodiment is elongated by connecting the first superconducting wire 401 and the second superconducting wire 402 using the connecting member 403.
[0225] The first superconducting wire 401 includes a first substrate 12, a first intermediate layer 14, a first superconducting layer 16, and a first protective layer 18. The second superconducting wire 402 includes a second substrate 22, a second intermediate layer 24, a second superconducting layer 26, and a second protective layer 28. The connecting member 403 includes a third substrate 42, a third intermediate layer 44, and a third superconducting layer 46.
[0226] The connection layer 30 includes a first portion 30x and a second portion 30y. The first portion 30x and the second portion 30y are spaced apart from each other.
[0227] The first portion 30x is provided between the first superconducting layer 16 and the third superconducting layer 46. The first portion 30x contacts the first superconducting layer 16. The first portion 30x contacts the third superconducting layer 46.
[0228] The second portion 30y is provided between the second superconducting layer 26 and the third superconducting layer 46. The second portion 30y contacts the second superconducting layer 26. The second portion 30y contacts the third superconducting layer 46.
[0229] The connection layer 30 of the sixth embodiment has a configuration similar to that of the connection layer 30 of the first embodiment shown in Fig. 1, the connection layer 30 of the second embodiment shown in Fig. 9, or the connection layer 30 of the third embodiment shown in Fig. 10. The first portion 30x and the second portion 30y have a configuration similar to that of the connection layer 30 of the first embodiment shown in Fig. 1, the connection layer 30 of the second embodiment shown in Fig. 9, or the connection layer 30 of the third embodiment shown in Fig. 10.
[0230] In the superconducting wire 600 of the sixth embodiment, for example, a current flows from the first superconducting wire 401 through the first portion 30x of the connection layer 30, the connection member 403, and the second portion 30y of the connection layer 30 to the second superconducting wire 402.
[0231] (First Modification) 15 is a schematic cross-sectional view of a first modified example of the superconducting wire of the sixth embodiment. A superconducting wire 610 of the first modified example of the sixth embodiment differs from superconducting wire 600 of the sixth embodiment in that a part of a surface of first superconducting layer 16 facing third superconducting layer 46 is exposed, and a part of a surface of second superconducting layer 26 facing third superconducting layer 46 is exposed.
[0232] There is a region where the connection layer 30 is not present on the upper surface of the first superconducting layer 16 near the end on the second superconducting layer 26 side. Also, there is a region where the connection layer 30 is not present on the upper surface of the second superconducting layer 26 near the end on the first superconducting layer 16 side.
[0233] (Second Modification) 16 is a schematic cross-sectional view of a second modified example of the superconducting wire of the sixth embodiment. A superconducting wire 620 of the second modified example of the sixth embodiment differs from superconducting wire 610 of the first modified example in that a reinforcing material 60 is provided.
[0234] The reinforcing material 60 is provided between the first superconducting wire 401 and the second superconducting wire 402. The reinforcing material 60 is provided, for example, between the first superconducting layer 16 and the second superconducting layer 26. The reinforcing material 60 is provided, for example, between the first superconducting layer 16 and the third superconducting layer 46. The reinforcing material 60 is provided, for example, between the second superconducting layer 26 and the third superconducting layer 46. The reinforcing material 60 is provided, for example, between the first portion 30x and the second portion 30y.
[0235] By providing reinforcing material 60, the mechanical strength of superconducting wire 620 is improved.
[0236] The reinforcing material 60 is, for example, a metal or a resin. The reinforcing material 60 is, for example, a solder. The reinforcing material 60 is, for example, a solder containing silver (Ag) and indium (In).
[0237] (Third Modification) 17 is a schematic cross-sectional view of a modified example of the superconducting wire of the sixth embodiment. The superconducting wire 630 of the modified example of the sixth embodiment differs from the superconducting wire 600 of the sixth embodiment in that the second substance 30b is disposed at both ends of the first portion 30x of the connection layer 30 and at both ends of the second portion 30y of the connection layer 30.
[0238] The second material 30b disposed at both ends of the first portion 30x of the connecting layer 30 is provided continuously between the first superconducting layer 16 and the superconducting layer 46 of the connecting member 403, for example. The second material 30b disposed at both ends of the second portion 30y of the connecting layer 30 is provided continuously between the second superconducting layer 26 and the superconducting layer 46 of the connecting member 403, for example.
[0239] By disposing the second material 30b on both ends of the first portion 30x of the connection layer 30 and on both ends of the second portion 30y of the connection layer 30, it is possible to disperse stress applied to the opposing first and second superconducting layers 16 and 26 and the superconducting layer 46 of the connection member when pressure is applied from above and below. This makes it possible to suppress cracks occurring in the first and second superconducting layers 16 and 26 and the superconducting layer 46 of the connection member, thereby realizing a superconducting wire with high mechanical strength. It is also effective in obtaining a high critical current.
[0240] As described above, according to the sixth embodiment, a superconducting wire that is long and has low electrical resistance and high mechanical strength can be realized by connecting two superconducting wires.
[0241] Seventh embodiment The superconducting coil of the seventh embodiment includes the superconducting wire of any one of the fourth to sixth embodiments. In the following, some of the contents that overlap with the fourth to sixth embodiments may be omitted.
[0242] Fig. 18 is a schematic perspective view of a superconducting coil according to the seventh embodiment. Fig. 19 is a schematic cross-sectional view of the superconducting coil according to the seventh embodiment.
[0243] The superconducting coil 700 of the seventh embodiment is used as a coil for generating a magnetic field in superconducting equipment such as NMR, MRI, heavy particle beam therapy equipment, or superconducting magnetic levitation railway vehicles.
[0244] Superconducting coil 700 includes a winding form 110, a first insulating plate 111a, a second insulating plate 111b, and a winding portion 112. Winding portion 112 includes superconducting wire 120 and an inter-wire layer .
[0245] FIG. 19 shows a state in which the first insulating plate 111a and the second insulating plate 111b are removed.
[0246] The reel 110 is made of, for example, fiber-reinforced plastic. The superconducting wire 120 is, for example, in a tape shape. The superconducting wire 120 is wound around the reel 110 in a concentric, so-called pancake shape, with the winding center C as the center, as shown in FIG.
[0247] Inter-wire layer 130 has a function of fixing superconducting wire 120. Inter-wire layer 130 has a function of preventing superconducting wire 120 from being damaged by vibration during use of a superconducting device or by friction between the superconducting wires.
[0248] The first insulating plate 111a and the second insulating plate 111b are formed of, for example, fiber-reinforced plastic. The first insulating plate 111a and the second insulating plate 111b have a function of insulating the winding portion 112 from the outside. The winding portion 112 is located between the first insulating plate 111a and the second insulating plate 111b.
[0249] The superconducting wire 120 may be any of the superconducting wires according to the fourth to sixth embodiments.
[0250] As described above, according to the seventh embodiment, by using a superconducting wire having low electrical resistance and high mechanical strength, a superconducting coil with improved characteristics can be realized.
[0251] Eighth embodiment The superconducting device of the eighth embodiment is a superconducting device including the superconducting coil of the seventh embodiment. Hereinafter, some of the description overlapping with the seventh embodiment will be omitted.
[0252] 20 is a block diagram of a superconducting device according to an eighth embodiment. The superconducting device according to the eighth embodiment is a heavy particle beam therapy device 800. The heavy particle beam therapy device 800 is an example of a superconducting device.
[0253] The heavy ion beam therapy device 800 includes an injection system 50 , a synchrotron accelerator 52 , a beam transport system 54 , an irradiation system 56 , and a control system 58 .
[0254] The injection system 50 has a function of generating carbon ions to be used in therapy, and performing pre-acceleration for injection into the synchrotron accelerator 52. The injection system 50 has, for example, an ion generation source and a linear accelerator.
[0255] The synchrotron accelerator 52 has a function of accelerating the carbon ion beam injected from the injection system 50 to an energy level suitable for treatment. The synchrotron accelerator 52 uses the superconducting coil 700 of the seventh embodiment.
[0256] The beam transport system 54 has a function of transporting the carbon ion beam injected from the synchrotron accelerator 52 to the irradiation system 56. The beam transport system 54 has, for example, a bending electromagnet.
[0257] The irradiation system 56 has a function of irradiating a patient, who is an irradiation target, with the carbon ion beam injected from the beam transport system 54. The irradiation system 56 has, for example, a rotating gantry that enables the carbon ion beam to be irradiated from any direction. The superconducting coil 700 of the seventh embodiment is used in the rotating gantry.
[0258] The control system 58 controls the injection system 50, the synchrotron accelerator 52, the beam transport system 54, and the irradiation system 56. The control system 58 is, for example, a computer.
[0259] In the heavy ion beam therapy device 800 of the eighth embodiment, the superconducting coil 700 of the seventh embodiment is used in the synchrotron accelerator 52 and the rotating gantry. Therefore, the heavy ion beam therapy device 800 with excellent characteristics is realized.
[0260] In the eighth embodiment, a heavy ion beam therapy device 800 has been described as an example of a superconducting device, but the superconducting device may also be a nuclear magnetic resonance device (NMR), a magnetic resonance imaging device (MRI), or a superconducting magnetic levitation railway vehicle. EXAMPLES
[0261] Examples 1 to 13 and Comparative Examples 1 to 3 will be described. The first area ratio, the second area ratio, the third area ratio, and the fourth area ratio of Examples 1 to 13 and Comparative Examples 1 to 3 are shown in Table 1. Furthermore, the evaluation results of Examples 1 to 13 and Comparative Examples 1 to 3 are shown in Tables 1 to 7.
[0262] [Table 1]
[0263] Example 1 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. The length of each wire was 10 cm. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layers (first and second superconducting layers).
[0264] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 930°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0265] Silver oxide powder was dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layers (first and second superconducting layers) of the 10 cm superconducting wire. The superconducting wires were then stacked with the portions coated with the slurry facing each other, with a thin plate-shaped superconductor sandwiched between them, and sandwiched between plates from above and below, as shown in Fig. 8. The wires were then screwed together so that a load was applied to the joints while sandwiched between the plates, and placed in a furnace as is.
[0266] The first heat treatment was carried out by heating to 500° C. in an air atmosphere, and a connection structure for the superconducting wires was formed.
[0267] Terminals were attached to both ends of the superconducting wire after connection, and the temperature dependence of the electrical resistance was measured, confirming a clear drop in electrical resistance at around 93 K. The electrical resistance value of this connection structure after the clear drop in electrical resistance was set as a reference value of 1.0, and the relative electrical resistance values are shown in the following examples and comparative examples.
[0268] The connection structure of Example 1 maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength sufficient to withstand thermal contraction from room temperature to 80 K. A tensile load was applied to both ends of the connection structure of Example 1, and the load at which the connection peeled off was set as a reference value of 1.0, and relative strength is shown in the following Examples and Comparative Examples.
[0269] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance having a composition of (6≦δ≦7) and silver (second substance) were identified. At a first interface between the first superconducting layer and the connection layer, the first area ratio per unit area of the first region where the second substance and the first superconducting layer contact was 10%, and at a second interface between the second superconducting layer and the connection layer, the second area ratio per unit area of the second region where the second substance and the second superconducting layer contact was 15%.
[0270] Example 2 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0271] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0272] Gd2O3 powder, BaCO3 powder, and CuO powder were mixed in a mortar. The mixed powder and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The parts of the superconducting wire to which the slurry was applied were then placed face to face, with a thin plate-shaped superconductor sandwiched between them, and the wires were sandwiched between plates from above and below, resulting in the structure shown in Figure 8. The wires were then screwed in place so that a load was applied to the connection parts while they were sandwiched between the plates, and the wires were then placed in a furnace as is.
[0273] The first heat treatment was performed by heating to 800°C in an air atmosphere, followed by cooling to near room temperature, introducing oxygen gas into the furnace, and heating to 500°C in an oxygen atmosphere to perform the second heat treatment, thereby forming a connection structure for the superconducting wire.
[0274] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.3. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.4.
[0275] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (second substance) were identified. The area ratio of the first substance was 12% and the area ratio of the second substance was 13%.
[0276] The joints contained Gd2O3, BaCO3, CuO, and compounds of Gd, Cu, and O.
[0277] Example 3 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0278] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ An oxide superconductor with a composition of (6≦δ≦7) was produced. The surface of the obtained oxide superconductor was polished to process it into a thin plate. The MOD solution was applied to the thin plate, which was then dried in an oven and then heat-treated at 800℃.
[0279] Silver oxide powder was dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The wires were then stacked with the parts coated with the slurry facing each other, with a thin plate-shaped superconductor sandwiched between them, and sandwiched between plates from above and below, as shown in Fig. 8. The wires were then screwed together so that a load was applied to the joints while they were sandwiched between the plates, and placed in a furnace as is.
[0280] The first heat treatment was performed by heating to 800°C in a mixed atmosphere of Ar and oxygen, and then cooled to near room temperature.Oxygen gas was introduced into the furnace, and the second heat treatment was performed by heating to 500°C in an oxygen atmosphere to form a connection structure for the superconducting wire.
[0281] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.01. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.2.
[0282] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (a second substance) were identified. The area ratio of the first substance was 20% and the area ratio of the second substance was 18%.
[0283] Example 4 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0284] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ An oxide superconductor with a composition of (6≦δ≦7) was produced. The oxide superconductor thus produced was pulverized to obtain a powdered superconductor.
[0285] Gd2O3 powder, BaCO3 powder, and CuO powder were mixed in a mortar. The mixed powder, powdered superconductor, and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The superconducting wires were then stacked with the slurry-coated parts facing each other to form the structure shown in Figure 9, and sandwiched between plates from above and below. While sandwiched between the plates, the wires were screwed in place so that weight was applied to the joints, and the wires were then placed in a furnace as is.
[0286] The first heat treatment was performed by heating to 800°C in an air atmosphere, followed by cooling to near room temperature, introducing oxygen gas into the furnace, and heating to 500°C in an oxygen atmosphere to perform the second heat treatment, thereby forming a connection structure for the superconducting wire.
[0287] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.6. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.2.
[0288] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (second substance) were identified. The area percentage of the first substance was 10% and the area percentage of the second substance was 12%.
[0289] The joints contained Gd2O3, BaCO3, CuO, and compounds of Gd, Cu, and O.
[0290] Example 5 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δTwo oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0291] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ An oxide superconductor with a composition of (6≦δ≦7) was produced. The oxide superconductor obtained was pulverized to obtain a powdered superconductor. The powdered superconductor was coated with an MOD solution, dried in an oven, and then heat-treated at 800°C.
[0292] Powdered superconductor and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The superconducting wires were then stacked so that the parts where the slurry was applied faced each other, as shown in Figure 9, and sandwiched between plates from above and below. The wires were then screwed together so that a load was applied to the joints while they were sandwiched between the plates, and placed in a furnace as is.
[0293] The first heat treatment was performed by heating to 800°C in a mixed atmosphere of Ar and oxygen, and then cooled to near room temperature.Oxygen gas was introduced into the furnace, and the second heat treatment was performed by heating to 500°C in an oxygen atmosphere to form a connection structure for the superconducting wire.
[0294] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.03. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.1.
[0295] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (second substance) were identified. The area ratio of the first substance was 15% and the area ratio of the second substance was 17%.
[0296] Example 6 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Three oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. One of the wires was 3 cm long, and the remaining two were 10 cm long. The 3 cm wire was wet etched between both ends, and the two 10 cm wires were wet etched 1 cm from their ends using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0297] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 930°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0298] Gd2O3 powder, BaCO3 powder, and CuO powder were mixed in a mortar. The mixed powder and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layers (first and third superconducting layers) of the 10 cm superconducting wire and the exposed oxide superconducting layers (second superconducting layers) of the 3 cm superconducting wire. The superconducting wires were then stacked with the slurry-coated parts facing each other, sandwiching a thin plate-shaped superconductor between them, and sandwiched between plates from above and below, as shown in FIG. 11. The wires were screwed together so that a load was applied to the joints while sandwiched between the plates, and then placed in a furnace.
[0299] The first heat treatment was performed by heating to 800°C in a mixed atmosphere of Ar and oxygen, and then cooled to near room temperature.Oxygen gas was introduced into the furnace, and the second heat treatment was performed by heating to 500°C in an oxygen atmosphere to form a connection structure for the superconducting wire.
[0300] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.4. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.0.
[0301] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (a second substance) were identified. The area percentage of the first substance was 15%, the area percentage of the second substance was 20%, and the area percentage of the third substance was 13%.
[0302] Example 7 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Three oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. One of the wires was 3 cm long, and the remaining two were 10 cm long. The 3 cm wire was wet etched between both ends, and the two 10 cm wires were wet etched 1 cm from their ends using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0303] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 930°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δAn oxide superconductor with a composition of (6≦δ≦7) was produced. The oxide superconductor obtained was pulverized to obtain a powdered superconductor. The powdered superconductor was coated with an MOD solution, dried in an oven, and then heat-treated at 800°C.
[0304] Silver oxide powder was dispersed in acetone to prepare a slurry, which was then applied to both ends of the exposed oxide superconducting layer (second superconducting layer) of the 3 cm superconducting wire, and then heat-treated at 500°C in air.
[0305] Powdered superconductor and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layers (first and third superconducting layers) of the 10 cm superconducting wire and the exposed oxide superconducting layer (second superconducting layer) of the 3 cm superconducting wire, and then the superconducting wires were stacked with the slurry-coated parts facing each other to form the structure shown in Figure , and sandwiched between plates from above and below. While sandwiched between plates, they were screwed so that weight would be applied to the joints, and then placed in a furnace as is.
[0306] The first heat treatment was performed by heating to 800°C in a mixed atmosphere of Ar and oxygen, and then cooled to near room temperature.Oxygen gas was introduced into the furnace, and the second heat treatment was performed by heating to 500°C in an oxygen atmosphere to form a connection structure for the superconducting wire.
[0307] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.05. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.2.
[0308] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δA first substance with a composition of (6≦δ≦7) and silver (second substance) were identified. The area percentage of the first substance was 25%, the area percentage of the second substance was 30%, and the area percentage of the third substance was 22%.
[0309] Example 8 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Three oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. One of the wires was 3 cm long, and the remaining two were 10 cm long. Both ends of the 3 cm wire and 1 cm from the ends of the two 10 cm wires were wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0310] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 930°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ An oxide superconductor with a composition of (6≦δ≦7) was produced. The oxide superconductor obtained was pulverized to obtain a powdered superconductor. The powdered superconductor was coated with an MOD solution, dried in an oven, and then heat-treated at 800°C.
[0311] Powdered superconductor and silver oxide powder were dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layers (first and fourth superconducting layers) of the 10 cm superconducting wire and the exposed oxide superconducting layers (second and third superconducting layers) of the 3 cm superconducting wire, and then the superconducting wires were stacked with the slurry-coated portions facing each other to form the structure shown in Fig. 13, and sandwiched between plates from above and below. The wires were screwed together so that a load was applied to the joints while sandwiched between the plates, and then placed in a furnace as is.
[0312] The first heat treatment was performed by heating to 800°C in a mixed atmosphere of Ar and oxygen, and then cooled to near room temperature.Oxygen gas was introduced into the furnace, and the second heat treatment was performed by heating to 500°C in an oxygen atmosphere to form a connection structure for the superconducting wire.
[0313] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, a clear superconducting transition was confirmed at around 93 K, with a relative electrical resistance value of 0.04. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80 K, and had a connection strength that could withstand thermal contraction from room temperature to 80 K. The relative connection strength was 1.0.
[0314] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (second substance) were identified. The first area percentage was 17%, the second area percentage was 22%, the third area percentage was 24%, and the fourth area percentage was 18%.
[0315] Example 9 After forming the connection structure, a connection structure was formed in the same manner as in Example 6, except that the gaps were filled with indium silver solder to obtain the structure shown in FIG. 12, and measurements and observations were then performed.
[0316] Example 10 Except for increasing the ratio of silver oxide powder to the powdered superconductor when preparing the slurry, a connection structure was formed and measured and observed in the same manner as in Example 5. The connection layer had a structure as shown in Figure 10, and the second substance was present continuously between the first superconducting layer and the second superconducting layer.
[0317] Example 11 A connection structure was formed, measured, and observed in the same manner as in Example 2, except that Gd (gadolinium) was changed to Eu (erbium).
[0318] Example 12 A connection structure was formed, measured, and observed in the same manner as in Example 2, except that Gd (gadolinium) was changed to Y (yttrium).
[0319] (Example 13) A connection structure was formed, measured, and observed in the same manner as in Example 1, except that the silver oxide powder was changed to indium powder and the first heat treatment was performed at 300° C. in an Ar atmosphere.
[0320] Comparative Example 1 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. The length of each wire was 10 cm. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layers (first and second superconducting layers).
[0321] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 930°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0322] The exposed superconducting layers were placed facing each other, a thin plate-shaped superconductor was placed between them, and they were then sandwiched between plates from above and below, resulting in the structure shown in Figure 8. With the plates still sandwiched in place, screws were used to apply weight to the joints, and the assembly was then placed in a furnace as is.
[0323] The first heat treatment was carried out by heating to 800° C. in an air atmosphere, and a connection structure for the superconducting wires was formed.
[0324] The sample of Comparative Example 1 peeled off immediately after being removed from the furnace, and no connection structure was formed.
[0325] Comparative Example 2 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0326] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0327] A small amount of ethyl acetate was added to silver oxide powder to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The wires were then stacked with the parts coated with the slurry facing each other, with a thin plate-shaped superconductor sandwiched between them, and sandwiched between plates from above and below, as shown in Fig. 8. The wires were then screwed together so that a load was applied to the joints while they were sandwiched between the plates, and the wires were then placed in a furnace.
[0328] The first heat treatment was carried out by heating to 500° C. in an air atmosphere, and a connection structure for the superconducting wires was formed.
[0329] When terminals were attached to both ends of the connected superconducting wire and the temperature dependence of electrical resistance was measured, no clear superconducting transition was confirmed and a high resistance value was shown. Furthermore, this connection structure maintained the same connectivity as at room temperature even when the temperature was lowered to 80K, and had a connection strength that could withstand thermal contraction from room temperature to 80K. The relative connection strength was 2.0.
[0330] The cross section of the joint was observed by SEM and SEM-EDX, and it was found that δ A first substance with a composition of (6≦δ≦7) and silver (a second substance) were identified. The area ratio of the first substance was 55% and the area ratio of the second substance was 60%.
[0331] Comparative Example 3 An intermediate layer and GdBa2Cu3O on a Hastelloy substrate 7-δ Two oxide superconducting wires were prepared, each of which had a layer (oxide superconducting layer) formed on it and was covered with a protective layer of silver and copper. Each was 10 cm long. A portion of 1 cm from the end of each superconducting wire was wet etched using a mixed solution of nitric acid, ammonia, and hydrogen peroxide to expose the oxide superconducting layer.
[0332] Gd2O3, BaCO3, and CuO powders were prepared, appropriately weighed, thoroughly mixed, and the mixed powder was heat-treated at 900°C to obtain a calcined body. The calcined body was pulverized, and the obtained powder was compression-molded to produce a green compact. The obtained green compact was sintered at 950°C and then heat-treated at 500°C in an oxygen atmosphere to obtain GdBa2Cu3O δ We fabricated an oxide superconductor with a composition of (6≦δ≦7). The surface of the obtained oxide superconductor was polished and processed into a thin plate.
[0333] Silver powder was dispersed in acetone to prepare a slurry. The obtained slurry was applied to the exposed oxide superconducting layer of the 10 cm superconducting wire. The wires were then stacked with the parts coated with the slurry facing each other, with a thin plate-shaped superconductor sandwiched between them, and sandwiched between plates from above and below, as shown in Figure 1. The wires were then screwed together so that a load was applied to the joints while they were sandwiched between the plates, and placed in a furnace as is.
[0334] The first heat treatment was carried out by heating to 500° C. in an air atmosphere, and a connection structure for the superconducting wires was formed.
[0335] The sample of Comparative Example 1 peeled off immediately after being removed from the furnace, and no connection structure was formed.
[0336] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0337] 16 First superconducting layer 26 Second superconducting layer 30 Connection Layer 30a First Substance 30b Second substance 46 Third Superconducting Layer 100 Connection structure of the first embodiment 200 Connection structure of the second embodiment 300 Connection structure of the third embodiment 400 Superconducting wire of the fourth embodiment 401 The first superconducting wire 402 Second Superconducting Wire 600 Superconducting wire of the sixth embodiment 700 Superconducting Coil 800 Heavy ion beam therapy device P1 First interface P2 Second interface P3 Third Interface
Claims
1. A first superconducting layer; A second superconducting layer; and a connection layer provided between the first superconducting layer and the second superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn); a first area ratio of a first region where the second material and the first superconducting layer are in contact with each other per unit area at a first interface between the first superconducting layer and the connection layer is 1% or more and 50% or less; a second area ratio of a second region where the second material and the second superconducting layer are in contact with each other per unit area at a second interface between the second superconducting layer and the connection layer is 1% or more and 50% or less; the second material includes a plurality of particles, and in a cross section perpendicular to the first interface, at least some of the particles are in contact with the first superconducting layer and have a flat shape; A connection structure of superconducting layers, wherein at least another part of the plurality of particles in the cross section is in contact with the second superconducting layer and has a flat shape.
2. In the cross section, the major axis direction of at least a portion of the plurality of particles is in a range of 0 degrees or more and 30 degrees or less with respect to the first interface, 2. The superconducting layer connection structure according to claim 1, wherein in the cross section, the major axis direction of at least another part of the plurality of particles is in the range of 0 degree to 30 degree with respect to the second interface.
3. A first superconducting layer; A second superconducting layer; and a connection layer provided between the first superconducting layer and the second superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn); a first area ratio of a first region where the second material and the first superconducting layer are in contact with each other per unit area at a first interface between the first superconducting layer and the connection layer is 1% or more and 50% or less; a second area ratio of a second region where the second material and the second superconducting layer are in contact with each other per unit area at a second interface between the second superconducting layer and the connection layer is 1% or more and 50% or less; A connection structure of a superconducting layer, wherein the second material includes a plurality of particles, and in a cross section perpendicular to the first interface, at least some of the particles among the plurality of particles that contact the first superconducting layer have an aspect ratio of 5 or more, and in the cross section, at least some of the particles among the plurality of particles that contact the second superconducting layer have an aspect ratio of 5 or more.
4. 4. The connection structure of superconducting layers according to claim 1, wherein the first substance is in contact with the first superconducting layer and the second superconducting layer.
5. A connection structure of a superconducting layer described in any one of claims 1 to 4, wherein the median long diameter of the multiple particles is 100 nm or more and 10 μm or less.
6. 6. The superconducting layer connection structure according to claim 1, wherein the second substance contains oxygen (O).
7. A first superconducting layer; A second superconducting layer; and a connection layer provided between the first superconducting layer and the second superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn); a portion of the second material contacts the first superconducting layer and the second superconducting layer; the portion is continuous between the first superconducting layer and the second superconducting layer; A connection structure of a superconducting layer, wherein the portion is provided between a first portion of the first material and a second portion of the first material different from the first portion.
8. 8. The connection structure of superconducting layers according to claim 7, wherein said first substance is in contact with said first superconducting layer and said second superconducting layer.
9. 9. A superconducting layer connection structure according to claim 7 or claim 8, wherein in a cross section parallel to a direction from the first superconducting layer to the second superconducting layer, the area ratio per unit area of the second material is 5% or more and 50% or less.
10. a first area ratio of a first region where the second material and the first superconducting layer are in contact with each other per unit area at a first interface between the first superconducting layer and the connection layer is 1% or more and 50% or less; 10. A superconducting layer connection structure according to claim 7, wherein at a second interface between the second superconducting layer and the connection layer, a second area ratio per unit area of a second region where the second material and the second superconducting layer are in contact is 1% or more and 50% or less.
11. a first superconducting wire including a first superconducting layer; a second superconducting wire including a second superconducting layer; a third superconducting layer having a first surface and a second surface opposite to the first surface; a connection layer provided between the first superconducting layer and the third superconducting layer and between the second superconducting layer and the third superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn); the first superconducting layer and the second superconducting layer are located on a side of the third superconducting layer facing the first surface; a first area ratio of a first region where the second material and the first superconducting layer are in contact with each other per unit area at a first interface between the first superconducting layer and the connection layer is 1% or more and 50% or less; a second area ratio of a second region where the second material and the second superconducting layer are in contact with each other per unit area at a second interface between the second superconducting layer and the connection layer is 1% or more and 50% or less; a third area ratio of a third region where the second material and the third superconducting layer are in contact with each other per unit area at a third interface between the third superconducting layer and the connection layer is 1% or more and 50% or less; The second substance includes a plurality of particles, and the median major axis of the plurality of particles is 100 nm or more and 10 μm or less.
12. 12. The superconducting wire according to claim 11, wherein the first material is in contact with the first superconducting layer, the second superconducting layer, and the third superconducting layer.
13. In a cross section perpendicular to the first interface, at least a portion of the plurality of particles contacts the first superconducting layer and has a flat shape; In a cross section perpendicular to the second interface, at least another part of the plurality of particles is in contact with the second superconducting layer and has a flat shape; 13. The superconducting wire according to claim 11 or 12, wherein in a cross section perpendicular to the third interface, at least another portion of the plurality of particles is in contact with the third superconducting layer and is a flat particle.
14. In a cross section perpendicular to the first interface, the major axis direction of at least a portion of the plurality of particles is in a range of 0 degrees or more and 30 degrees or less with respect to the first interface, In a cross section perpendicular to the second interface, a major axis direction of at least another part of the plurality of particles is in a range of 0 degree or more and 30 degree or less with respect to the second interface, 14. The superconducting wire according to claim 13, wherein in a cross section perpendicular to the third interface, the major axis direction of at least another portion of the plurality of particles is in the range of 0 degree to 30 degree with respect to the third interface.
15. a first superconducting wire including a first superconducting layer; a second superconducting wire including a second superconducting layer; a third superconducting layer having a first surface and a second surface opposite to the first surface; a connection layer provided between the first superconducting layer and the third superconducting layer and between the second superconducting layer and the third superconducting layer, the connection layer including a first substance including a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O), and a second substance including at least one metal element selected from the group consisting of silver (Ag), aluminum (Al), indium (In), copper (Cu), tin (Sn), and zinc (Zn); the first superconducting layer and the second superconducting layer are located on a side of the third superconducting layer facing the first surface; a portion of the second material contacts the first superconducting layer and the third superconducting layer; the portion of the second material is continuous between the first superconducting layer and the third superconducting layer; Another portion of the second material is in contact with the second superconducting layer and the third superconducting layer; the other portion of the second material is continuous between the second superconducting layer and the third superconducting layer; the portion of the second material is provided between the first superconducting layer and the third superconducting layer, between a first portion of the first material and a second portion of the first material different from the first portion; A superconducting wire, wherein the other portion of the second material is provided between the second superconducting layer and the third superconducting layer, between a third portion of the first material and a fourth portion of the first material different from the third portion.
16. 16. The superconducting wire according to claim 15, wherein the first material is in contact with the first superconducting layer, the second superconducting layer, and the third superconducting layer.
17. A superconducting coil comprising the superconducting wire according to any one of claims 11 to 16.
18. A superconducting device comprising the superconducting coil according to claim 17.
19. providing a first superconducting layer and a second superconducting layer; applying a slurry containing silver oxide particles onto the first superconducting layer and the second superconducting layer; a plate-shaped substance containing a rare earth element (RE), barium (Ba), copper (Cu), and oxygen (O) is sandwiched between the slurry on the first superconducting layer and the slurry on the second superconducting layer; A method for connecting superconducting layers, comprising the steps of: subjecting the first superconducting layer and the second superconducting layer to a heat treatment while applying pressure to each other.
20. A method for producing a superconducting layer comprising the steps of: preparing a first superconducting layer and a second superconducting layer; A slurry containing particles containing rare earth elements (RE), barium (Ba), copper (Cu), and oxygen (O) and particles of silver oxide is sandwiched between the first superconducting layer and the second superconducting layer; A method for connecting superconducting layers, comprising the steps of: subjecting the first superconducting layer and the second superconducting layer to a heat treatment while applying pressure to each other.
21. The heat treatment includes a first heat treatment at a first temperature; A method for connecting superconducting layers according to claim 19 or 20, further comprising: a second heat treatment at a second temperature in an atmosphere having the same oxygen partial pressure as that of the first heat treatment or a higher oxygen partial pressure than that of the first heat treatment.
22. 22. The method for connecting superconducting layers according to claim 21, wherein the first temperature is 800° C. or less.
23. 23. The method for connecting superconducting layers according to claim 21 or 22, wherein the second temperature is lower than the first temperature.
Citation Information
Patent Citations
Joining of superconductor
JP1990302380A
Connection structure of superconducting wire rod and method for connecting superconducting wire rod
JP2017117523A
Superconducting bulk conjugate and manufacturing method of superconducting bulk conjugate
JP2018035015A
Superconducting wire manufacturing method and superconducting wire joining member
JP6675590B2
Method for producing superconducting wire material and superconducting joining member
US20180025812A1