Metal base boards, electronic component mounting boards
A substrate with a semi-softening circuit layer and optimized insulating layer thickness-to-elastic modulus ratio addresses thermal stress issues, enhancing solder layer reliability by preventing cracks during thermal cycles.
Patent Information
- Application Number
- JP2020062822
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-31
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing metal-based substrates face limitations in reducing thermal stress on solder layers due to the flexibility of insulating layers, which compromises the ability to suppress thermal expansion of circuit layers, leading to potential solder cracks during cooling and heating cycles.
The substrate design includes a circuit layer with a semi-softening temperature of 100°C to 150°C and an insulating layer with a specific thickness-to-elastic modulus relationship (10
The design effectively suppresses thermal stress on solder layers, preventing cracks even under thermal cycling, ensuring reliable bonding of electronic components.
Smart Images

Figure 0007581644000002 
Figure 0007581644000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal base substrate and an electronic component mounting board using the same. [Background technology]
[0002] A substrate for mounting electronic components such as semiconductor elements is preferably a metal base substrate capable of efficiently dissipating heat generated by the operation of the electronic components to the outside. A known metal base substrate is a metal base substrate in which a metal substrate is used as a base substrate, an insulating layer, and a circuit layer are laminated in this order. The electronic components are bonded to the circuit layer via a solder layer. In a metal base substrate configured in this way, heat generated by the electronic components is transferred to the metal substrate via the insulating layer, and dissipated from the metal substrate to the outside.
[0003] The insulating layer of the metal base substrate is generally formed from an insulating resin composition containing a resin with excellent insulating properties and ceramic particles (thermally conductive filler, inorganic filler) with excellent thermal conductivity. Polyimide resin, polyamide-imide resin, and silicone resin are used as the resin for the insulating layer. Conventionally, in such metal base substrates, the thermal stress applied to the solder layer has been reduced by lowering the elastic modulus of the resin constituting the insulating layer (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5650084 [Patent Document 2] Patent No. 5665449 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the inventions disclosed in Patent Documents 1 and 2, although the thermal stress caused by the expansion of the metal substrate can be alleviated by reducing the elastic modulus of the resin constituting the insulating layer, there is a limit to how much the thermal stress applied to the solder layer can be reduced because the circuit layer also thermally expands. Furthermore, the lower the elastic modulus of the resin constituting the insulating layer, the more flexible the insulating layer becomes, making it difficult to suppress the thermal expansion of the circuit layer.
[0006] The present invention has been made in consideration of the above circumstances, and aims to provide a metal base substrate that is less susceptible to solder cracks even when subjected to a thermal cycle while electronic components are bonded via a solder layer, and an electronic component mounting board using the same. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have discovered the following: By limiting the range of the half-softening temperature of the circuit layer and defining the relationship between the thickness of the insulating layer and the elastic modulus of the resin that constitutes the insulating layer, it is possible to suppress the thermal stress applied to the solder layer.
[0008] Based on this knowledge, the present invention proposes the following means. The metal base substrate of the present invention is a metal base substrate comprising a metal substrate, an insulating layer laminated on one side of the metal substrate, and a circuit layer laminated on the side of the insulating layer opposite the metal substrate, wherein the circuit layer is made of a metal having a half-softening temperature of 100°C or more and 150°C or less, the insulating layer contains a resin, and the relationship between the thickness t (μm) of the insulating layer and the elastic modulus E (GPa) of the insulating layer at 100°C satisfies the following formula (1). 10 <t / E···(1)
[0009] In the present invention, the insulating layer may be made of the resin having a filler dispersed therein.
[0010] In the present invention, an adhesive layer may be provided between the insulating layer and the circuit layer or between the insulating layer and the metal substrate, and the adhesive layer may have a filler dispersed therein and may contain a smaller volume fraction of the filler than the insulating layer.
[0011] The electronic component mounting board of the present invention is characterized by comprising a metal base substrate as described above, and an electronic component bonded to the circuit layer of the metal base substrate via a solder layer. [Brief description of the drawings]
[0012] [Figure 1] 1 is a cross-sectional view showing an electronic component mounting board including a metal base substrate according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto, and may be modified as appropriate within the scope of the effects of the present invention.
[0014] FIG. 1 is a cross-sectional view showing an electronic component mounting board including a metal base substrate according to one embodiment of the present invention. The electronic component mounting board 10 has a metal base substrate 20 and an electronic component 11 bonded to the metal base substrate 20 via a solder layer 12. The electronic component 11 is not particularly limited, and examples thereof include a semiconductor element, a resistor, a capacitor, and a crystal oscillator. Examples of the semiconductor element include a metal-oxide-semiconductor field effect transistor (MOSFET), an insulated gate bipolar transistor (IGBT), a large scale integration (LSI), a light emitting diode (LED), an LED chip, and an LED-CSP (LED-Chip Size Package).
[0015] The solder layer 12 can be made of various solders such as Sn-Ag-Cu solder, without any particular limitation.
[0016] The metal base substrate 20 has a metal substrate 21, an insulating layer 22 laminated on one side of the metal substrate 21, and a circuit layer 23 laminated on the side of the insulating layer 22 opposite the metal substrate 21 side.
[0017] The metal substrate 21 is a member that becomes the base of the metal base substrate 20. As the metal substrate 21, for example, a copper plate, an aluminum plate, or a laminate of these may be used.
[0018] The insulating layer 22 is formed from an insulating and thermally conductive resin composition containing an insulating resin (resin) 22a and ceramic particles (filler) 22b. By forming the insulating layer 22 from a highly insulating insulating resin 22a in which highly thermally conductive and insulating ceramic particles 22b are dispersed, it is possible to further reduce the thermal resistance of the entire metal base substrate 20 from the circuit layer 23 to the metal substrate 21 while maintaining the insulation. This allows the heat generated in the electronic component 11 to be easily dissipated from the metal substrate 21 side.
[0019] The insulating resin 31 is preferably a polyimide resin, a polyamide-imide resin, or a mixture thereof. Polyimide resin and polyamide-imide resin have imide bonds, and therefore have excellent heat resistance and mechanical properties.
[0020] As the ceramic particles 22b, which is an example of the filler, silica (silicon dioxide) particles, alumina (aluminum oxide) particles, boron nitride (BN) particles, titanium oxide particles, alumina-doped silica particles, alumina hydrate particles, aluminum nitride particles, etc. can be used. The ceramic particles 22b may be used alone or in combination of two or more types. Among these ceramic particles, alumina particles are preferred because of their high thermal conductivity. The form of the ceramic particles 22b is not particularly limited, but is preferably an agglomerated particle of fine ceramic particles or a single crystal ceramic particle.
[0021] The agglomerated particles of fine ceramic particles may be agglomerates in which the primary particles are relatively weakly connected, or may be aggregates in which the primary particles are relatively strongly connected. The aggregated particles may further aggregate to form particle aggregates. The primary particles of the ceramic particles 22b form aggregated particles and are dispersed in the insulating resin (resin) 22a of the insulating layer 22, whereby a network is formed by mutual contact between the ceramic particles 22b, and heat is easily conducted between the primary particles of the ceramic particles 22b, thereby improving the thermal conductivity of the insulating layer 22.
[0022] Commercially available agglomerated particles of fine ceramic particles include silica particles such as AE50, AE130, AE200, AE300, AE380, AE90E (all manufactured by Nippon Aerosil Co., Ltd.), T400 (manufactured by Wacker), and SFP-20M (manufactured by Denka Co., Ltd.); alumina particles such as Alu65 (manufactured by Nippon Aerosil Co., Ltd.) and AA-04 (manufactured by Sumitomo Chemical Co., Ltd.); boron nitride particles such as AP-170S (manufactured by Maruka); titanium oxide particles such as AEROXIDE(R)TiO2 P90 (manufactured by Nippon Aerosil Co., Ltd.); alumina-doped silica particles such as MOX170 (manufactured by Nippon Aerosil Co., Ltd.); and alumina hydrate particles manufactured by Sasol.
[0023] The single crystal ceramic particles are preferably α-alumina single crystal particles having an α-alumina (αAl2O3) crystal structure. Examples of commercially available α-alumina single crystal particles include AA-03, AA-04, AA-05, AA-07, and AA-1.5 of the Advanced Alumina (AA) series sold by Sumitomo Chemical Co., Ltd.
[0024] The content of the ceramic particles 22b in the insulating layer 22 may be, for example, within a range of 60 volume % or more and 80 volume % or less. If the content of the ceramic particles 22b is too small, the thermal conductivity of the insulating layer 22 is not sufficiently improved, and the thermal resistance of the entire metal base substrate 20 may become high. On the other hand, if the content of the ceramic particles 22b is too large, the content of the insulating resin 22a is relatively reduced, and the elastic modulus of the insulating layer 22 becomes too high, making it difficult for the insulating layer 22 to relieve the stress applied to the solder layer 12 due to thermal cycles.
[0025] The thickness of the insulating layer 22 is not particularly limited, but is preferably within the range of 1 μm to 200 μm, and more preferably within the range of 3 μm to 100 μm, for example.
[0026] The insulating layer 22 of the metal base substrate 20 of this embodiment is formed so that the relationship between the thickness t (μm) of the insulating layer 22 and the elastic modulus E (GPa) of the insulating layer 22 at 100° C. satisfies the following formula (1). 10 <t / E···(1) If the elastic modulus of insulating layer 22 is reduced so that the relationship between thickness t of insulating layer 22 and elastic modulus E of insulating layer 22 satisfies the above-mentioned formula (1), the stress due to thermal expansion of metal substrate 21 can be sufficiently alleviated.
[0027] The circuit layer 23 may be a metal foil having a semi-softening temperature of 100° C. or more and 150° C. or less, and may be, for example, aluminum, copper, or an alloy of these metals. Of these metals, copper is preferable. An example of copper is 4N copper (99.99% purity). Such 4N copper preferably contains a small amount of additive element to set the semi-softening temperature to 100° C. or more and 150° C. or less. Examples of additive elements include yttrium, scandium, samarium, lanthanum, cerium, boron, titanium, vanadium, chromium, manganese, iron, zirconium, hafnium, neodymium, tantalum, calcium, and manganese.
[0028] The thickness of the circuit layer 23 is in the range of 10 μm to 2000 μm, preferably in the range of 20 μm to 200 μm. If the thickness of the circuit layer 23 is too thin, the allowable current may be small and the thermal resistance may be high. On the other hand, if the thickness of the circuit layer 23 is too thick, it may be difficult to form a circuit pattern by etching.
[0029] The circuit layer 23 of this embodiment uses a metal foil having a half-softening temperature of 100° C. or more and 150° C. or less, such as a 4N copper foil. The semi-softening temperature referred to here is the annealing temperature corresponding to an intermediate proof strength between the proof strength before annealing when a sample is annealed and the proof strength measured by a tensile test, and the proof strength when completely softened (a state in which the proof strength does not change even if the annealing temperature is further increased after 30 minutes of annealing is considered to be completely softened). Note that the proof strength before annealing is the proof strength after cold rolling.
[0030] In addition to the above-mentioned configuration, an adhesive layer 25 may be provided between the insulating layer 22 and the circuit layer 23, or between the insulating layer 22 and the metal substrate 21, or both. In this embodiment, an example in which the adhesive layer 25 is provided between the insulating layer 22 and the circuit layer 23 is shown. The adhesive layer 25 is preferably made of a resin. Examples of the resin include silicone resin, epoxy resin, polyamide-imide resin, and polyimide resin. The silicone resin includes modified silicone resins into which various organic groups have been introduced. Examples of the modified silicone resin include polyimide-modified silicone resin, polyester-modified silicone resin, urethane-modified silicone resin, acrylic-modified silicone resin, olefin-modified silicone resin, ether-modified silicone resin, alcohol-modified silicone resin, fluorine-modified silicone resin, amino-modified silicone resin, mercapto-modified silicone resin, and carboxy-modified silicone resin. Examples of the epoxy resin include bisphenol A-type epoxy resin, bisphenol F-type epoxy resin, novolac-type epoxy resin, aliphatic-type epoxy resin, and glycidylamine-type epoxy resin. These resins may be used alone or in combination of two or more.
[0031] In order to improve thermal conductivity, the adhesive layer 25 may have a thermally conductive filler dispersed therein. As the thermally conductive filler, ceramic particles can be used. Examples of the ceramic particles include silica particles, alumina particles, boron nitride particles, titanium oxide particles, alumina-doped silica particles, alumina hydrate particles, and phosphoric acid-coated aluminum nitride particles.
[0032] The volume percentage of the filler contained in the adhesion layer 25 is preferably smaller than that of the filler contained in the insulating layer 22. When ceramic particles are used as the filler, the content of the filler in the adhesion layer 22 may be within a range of 20 volume % or more and 60 volume % or less.
[0033] According to the metal base substrate 20 of this embodiment configured as described above, and electronic component mounting substrate 10 using the same, by using a circuit layer 23 having a semi-softening temperature of 100°C or more and 150°C or less, and by configuring insulating layer 22 so that the relationship between the thickness t (μm) and the elastic modulus E (GPa) of insulating layer 22 at 100°C satisfies the above-mentioned formula (1), it is possible to prevent excessive stress from being applied to solder layer 12 even when a thermal cycle is applied when electronic component 11 is joined via solder layer 12, and it is possible to realize a metal base substrate 20 that is less susceptible to solder cracks, and an electronic component mounting substrate 10 using the same.
[0034] Although one embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. This embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention. EXAMPLES
[0035] The effect of the present invention was verified. (Creating copper foil to be used as circuit layers) Yttrium (Y) was added to oxygen-free copper with a purity of 99.996% by mass or more to the concentration shown in Table 1, and the copper was melted by vacuum melting (0.1 Pa). The resulting ingot was then hot-rolled to a thickness of 10 mm, after which it was faced and repeatedly annealed and cold-rolled to the specified thickness.
[0036] (Preparation of coating solution for forming insulating layer) Alumina (Al2O3) particles (AA-07: manufactured by Sumitomo Chemical Co., Ltd.) were prepared as ceramic particles. 1.0 g of the prepared alumina particles was added to 10 g of NMP (N-methyl-2-pyrrolidone) and ultrasonicated for 30 minutes to prepare a ceramic particle dispersion. Next, a polyimide solution (commercial product) of a solvent-soluble polyimide having an elastic modulus of 100 MPa at 100°C and a ceramic particle dispersion were mixed so that the content of ceramic particles relative to the total amount of resin components and ceramic particles was 60% by volume. The mixture was then diluted with a solvent so that the concentration of polyimide in the mixture was 5% by mass. The mixture was then dispersed by repeating a high-pressure injection process at a pressure of 50 MPa 10 times using a wet atomizer (Starburst: manufactured by Sugino Machine Co., Ltd.) to prepare a ceramic particle-dispersed polyimide solution (coating liquid for forming an insulating layer).
[0037] (Formation of insulating layer) The insulating layer-forming coating layer was formed by applying the above-mentioned insulating layer-forming coating solution to the surface of a 50 mm x 50 mm copper substrate with a thickness of 2.0 mm by a bar coating method so that the value obtained by dividing the thickness (μm) of the insulating layer generated by heating by the elastic modulus (GPa) of the insulating layer at 100 ° C. was the value shown in Table 1. Next, the copper substrate on which the insulating layer-forming coating layer was formed was placed on a hot plate, heated from room temperature to 60 ° C. at 3 ° C. / min, heated at 60 ° C. for 100 minutes, further heated to 120 ° C. at 1 ° C. / min, and heated at 120 ° C. for 100 minutes to dry the insulating layer-forming coating layer. Thereafter, the copper substrate was heated at 250 ° C. for 1 minute and at 400 ° C. for 1 minute to form an insulating layer on one side of the copper substrate.
[0038] The elastic modulus of the insulating layer was measured according to the following procedure. The insulating layer was applied to a 0.1 mm copper plate and dried, after which the copper plate was removed by etching to isolate the insulating film. The elastic modulus of the obtained insulating film was measured at 100°C by the tensile method using a dynamic viscoelasticity measuring device (Solid Viscoelasticity Analyzer RSA-G2: manufactured by TA Instruments Japan, Inc.). The measurement conditions were a frequency of 1 Hz and a heating rate of 1°C / min.
[0039] (Pasting of circuit layers) A 40 mm x 40 mm copper foil (wiring layer) having the thickness shown in Table 1 was laminated on the insulating layer, and then heated in a vacuum at 215°C for 120 minutes while applying a pressure of 5 MPa using a carbon jig to bond the insulating layer and the copper foil. In this manner, a metal base substrate was produced in which a copper substrate, an insulating layer, and copper foil were laminated in this order.
[0040] Table 1 shows the verification results of invention examples 1 to 36 and comparative examples 1 to 3. Note that in Table 1, the "reliability" is determined by the reliability test shown below, and is marked with an ◯ when the reliability is 80% or higher, and an × when the reliability is less than 80%. (Reliability test) An insulating layer was formed on a metal substrate, copper foil was formed on the insulating layer as a wiring layer, and Sn-Ag-Cu solder was applied to form a solder layer of 2.5 cm length x 2.5 cm width x 100 μm thickness. A 2.5 cm square Si chip was mounted on the solder layer to prepare a test specimen. The test specimen was subjected to 3000 cycles of cold and hot cycles of -40°C x 30 minutes to 150°C x 30 minutes per cycle. The test specimen after the cold and hot cycles was embedded in resin, and the observation surface formed by polishing the cross section near the center of the chip was observed, and the length (mm) of the cracks generated in the solder layer was measured. The value calculated from the length of one side of the solder layer and the measured crack length using the following formula indicating reliability was taken as the joint reliability. A joint reliability of 90% or more was rated as ◯, and the rest was rated as ×. Reliability (%) = {(length of one side of solder layer (25 mm) - 2 x crack length) / length of one side of bonding layer (25 mm)} x 100
[0041] [Table 1]
[0042] According to the results shown in Table 1, the metal base substrates of Examples 1 to 36 of the present invention, which have an insulating layer having a semi-softening temperature of 100°C or more and 150°C or less, and in which the relationship between the insulating layer thickness t (μm) and the insulating layer elastic modulus E (GPa) at 100°C satisfies the following formula (1), were confirmed to be metal base substrates that meet the necessary reliability requirements and are less susceptible to solder cracks in the solder layer even when subjected to thermal cycles. On the other hand, the metal base substrates of Comparative Examples 1 to 3 do not meet the necessary reliability requirements, and there is a concern that solder cracks may occur in the solder layer when subjected to thermal cycles. Thus, the effects of the metal base substrate of the present invention were confirmed. [Explanation of symbols]
[0043] 10 Electronic component mounting board 11 Electronic Components 12 Solder layer 20 Metal base board 21 Metal Substrate 22 Insulating layer 22a Insulating resin (resin) 22b Ceramic particles (filler) 23 circuit layers.
Claims
1. A metal base substrate comprising a metal substrate, an insulating layer laminated on one surface of the metal substrate, and a circuit layer laminated on a surface of the insulating layer opposite to the metal substrate, The circuit layer is made of a metal having a half-softening temperature of 100° C. or more and 150° C. or less, The metal base substrate is characterized in that the insulating layer contains a resin, and the relationship between the thickness t (μm) of the insulating layer and the elastic modulus E (GPa) of the insulating layer at 100° C. satisfies the following formula (1). 10<t / E...(1)
2. 2. The metal base board according to claim 1, wherein the insulating layer is made of the resin having a filler dispersed therein.
3. an adhesion layer having a filler dispersed therein is provided between the insulating layer and the circuit layer or between the insulating layer and the metal substrate; 3. The metal base substrate according to claim 2, wherein the adhesive layer contains a smaller volumetric percentage of filler than the insulating layer.
4. 4. An electronic component mounting board comprising: the metal base substrate according to claim 1; and an electronic component bonded to the circuit layer of the metal base substrate via a solder layer.
Citation Information
Patent Citations
Thin film el element
JP1981050084A
Curved fluorescent lamp and its manufacture
JP1981065449A
Metal base circuit board
JP1999008450A
Metal base substrate
JP2020013874A
Metal base substrate
WO2019151122A1