Blazed diffraction grating and method for manufacturing the same
The innovative manufacturing method for blazed diffraction gratings with a sawtooth shape and specific coating film configuration addresses the challenge of achieving high precision and efficiency in the vacuum and deep ultraviolet regions by forming an acute apex angle, resulting in improved diffraction efficiency.
Patent Information
- Application Number
- JP2020131790
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-03
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-08-03
Smart Images

Figure 0007581692000001 
Figure 0007581692000002 
Figure 0007581692000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a blazed diffraction grating, which is a wavelength separating / selecting element used in a spectrometer, a demultiplexer, etc., and to a method for manufacturing a blazed diffraction grating. [Background technology]
[0002] There are various types of diffraction gratings, but a diffraction grating in which the cross-sectional shape of the grooves is sawtooth is called a blazed diffraction grating. Since it exhibits high diffraction efficiency for light of specific wavelengths in the ultraviolet to visible light region, it is often used in visible and ultraviolet spectroscopes (see Patent Document 1).
[0003] Known methods for manufacturing blazed diffraction gratings include the ion beam etching method, in which an ion beam is irradiated at a specified angle onto a pattern mask formed by the holographic exposure method using the interference of two laser beams to cut the substrate, and the mechanical cutting method, in which grooves are machined one by one using a ruling engine. Holographic exposure has very little stray light due to periodic errors, so holographic exposure is often used to manufacture diffraction gratings that require low stray light.
[0004] Fig. 1 is a diagram illustrating a method for manufacturing a blazed diffraction grating by ion beam etching. In the ion beam etching method, first, a photoresist is applied to the surface of a flat substrate 1 made of quartz, glass, or the like to form a photoresist layer 2 (Fig. 1(a)). Then, this photoresist layer 2 is exposed and developed to form interference fringes due to two-beam interference, forming a parallel-line resist pattern 3 as shown in Fig. 1(b) (holographic exposure). Next, using this resist pattern 3 as a mask, etching is performed with an ion beam from obliquely above so that the desired blaze angle θB is formed on the substrate 1, forming grating grooves 4 with a sawtooth cross section on the substrate 1 (Figs. 1(c)-(e)). Thereafter, as shown in Fig. 1(f), a metal film 5 made of aluminum, gold, or the like is coated on the surface of the grating grooves 4 to complete the blazed diffraction grating.
[0005] Typically, in the above-mentioned etching process, ion beam etching is performed using an etching gas whose etching rate for the substrate 1 is faster than whose etching rate for the resist pattern 3, i.e., whose selectivity (=etching rate for the substrate material (e.g., glass) / etching rate for photoresist) is greater than 1.
[0006] A master blazed diffraction grating is manufactured through these steps. A release agent layer is formed on the grating surface of this master diffraction grating, and a metal thin film is formed on top of that. A glass substrate is then attached onto this metal thin film via an adhesive, and after the adhesive has hardened, the glass substrate is peeled off from the master diffraction grating. As a result, the metal thin film with the grating grooves formed therein is transferred upside down to the glass substrate, and a replica diffraction grating is obtained. This replica diffraction grating is used as a matrix to manufacture a blazed diffraction grating as a product (see Patent Document 1). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2009-92687 A Summary of the Invention [Problem to be solved by the invention]
[0008] Spectrophotometers using such blazed diffraction gratings have traditionally been developed primarily for the absorption measurement of liquid samples, but in recent years, there has been a rapid increase in applications for measuring the reflection and absorption of solids such as semiconductors, thin films, glass materials, and absorbents. These applications require highly accurate, high-energy (vacuum ultraviolet region) spectrometers, and these performances depend heavily on the performance of the diffraction grating, so there was a demand for blazed diffraction gratings that could obtain high diffraction efficiency in the vacuum ultraviolet and deep ultraviolet regions.
[0009] Thus, in order to obtain high diffraction efficiency in the vacuum ultraviolet region (120 to 200 nm) and deep ultraviolet region (200 to 300 nm), it is necessary to shorten the grating spacing and form a diffraction grating pattern with a shallow blaze angle θB (for example, a height of 100 nm or less) on the substrate. Furthermore, in order to produce peak wavelengths in increments of several tens of nm (for example, 120 nm, 160 nm), it is necessary to control the height of the diffraction grating pattern with an accuracy of around several nm. However, in the conventional manufacturing method described in Patent Document 1, an ideal sinusoidal resist pattern is formed on a substrate by holographic exposure, and then an ion beam is irradiated from above at a target angle to form a diffraction grating pattern. This requires precise understanding and control of the incidence angle α and spread angle of the ion beam, and it is difficult to achieve such precision due to the performance of the etching equipment. Furthermore, in order to manufacture a blazed diffraction grating with a small blaze angle θB, it is necessary to increase the incident angle α of the ion beam. In this case, however, the step surface 12 between one blaze surface 11 and the adjacent blaze surface 11 is deeply etched, resulting in a rounded apex angle β, making it difficult to obtain high diffraction efficiency.
[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a blazed diffraction grating that has a diffraction grating pattern in which the blaze height is formed with higher accuracy than existing ones, and that can obtain high diffraction efficiency in the vacuum ultraviolet and deep ultraviolet regions. [Means for solving the problem]
[0011] A blazed diffraction grating of a first aspect of the present invention comprises a substrate having a sawtooth cross-sectional shape and in which blaze surfaces and step surfaces are repeatedly arranged alternately in one direction, a reflective film formed to cover the surfaces of the blaze surface and the step surface, and a coating film formed to cover the surface of the reflective film, and is configured so that the sum of the film thicknesses of the reflective film and the coating film is maximum at the tops of the blaze surface and the step surface and minimum at the bottoms.
[0012] A method for manufacturing a blazed diffraction grating according to a second aspect of the present invention includes the steps of: preparing a substrate having a sawtooth cross-sectional shape in which blaze surfaces and step surfaces are repeatedly arranged alternately in one direction; forming a reflective film to cover the surfaces of the blaze surface and the step surface; and forming a coating film to cover the surface of the reflective film, wherein the steps of forming these films form the coating film so that the film thickness of the coating film is maximum at the tops of the blaze surface and the step surface and minimum at the bottoms. Effect of the Invention
[0013] According to the present invention, it is possible to realize a blazed diffraction grating that has a diffraction grating pattern in which the blaze height is formed with higher accuracy than existing ones and that can obtain high diffraction efficiency in the vacuum ultraviolet and deep ultraviolet regions. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a diagram illustrating a conventional method for manufacturing a blazed diffraction grating. [Diagram 2] FIG. 2 is a diagram illustrating the configuration of a blazed diffraction grating according to a first embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing a schematic configuration of a vacuum chamber used for manufacturing the blazed diffraction grating according to the first embodiment of the present invention. [Figure 4] FIG. 4 is a diagram showing the results of measuring the cross-sectional shape of the blazed diffraction grating according to the first embodiment of the present invention. [Diagram 5] FIG. 5 is a diagram showing the results of measuring the cross-sectional shape of a blazed diffraction grating according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, a blazed diffraction grating and a method for manufacturing a blazed diffraction grating according to the present invention will be described in detail based on preferred embodiments (examples) shown in the accompanying drawings.
[0016] (First embodiment) Fig. 2 is a diagram illustrating the configuration of a blazed diffraction grating 20 according to a first embodiment of the present invention, in which Fig. 2(a) is a plan view of the blazed surface viewed in the vertical direction, and Fig. 2(b) is an enlarged cross-sectional view taken along line AA in Fig. 2(a). As shown in Fig. 2, the blazed diffraction grating 20 of this embodiment includes a substrate 22, a reflective film 24, and a coating film 26.
[0017] The base material 22 is a replica diffraction grating formed by a conventional ion beam etching method or the like, and a basic diffraction grating 22a formed of resin on a rectangular plate-shaped glass base material is formed. The basic diffraction grating 22a is configured by repeatedly forming basic blaze surfaces 22b and basic step surfaces 22c alternately in one direction so that the cross-sectional shape is sawtooth-shaped, and in this embodiment, a basic diffraction grating with 1600 grooves, blaze height (h1): 40 nm, and blaze wavelength: 120 nm is used.
[0018] The reflective film 24 is a thin metal film formed to cover the basic diffraction grating 22a, and in this embodiment is an aluminum (Al) film having a thickness of 80 nm. The reflective film 24 is formed on the basic blaze surface 22b and the basic step surface 22c by using a method such as vacuum deposition or sputtering (details will be described later).
[0019] The coating film 26 is a thin film formed to cover the reflective film 24 by using a vacuum deposition method, a sputtering method, or the like, and in this embodiment, it is a magnesium fluoride (MgF2) film that prevents the surface of the reflective film 24 from being oxidized. By forming the coating film 26, a diffraction grating 26a consisting of a blaze surface 26b and a step surface 26c is formed on the coating film 26. Note that the thickness of the coating film 26 in this embodiment is not uniform, but changes monotonically in one direction on the basic blaze surface 22b, and the thickness (t2 in FIG. 2(b)) at the top (convex part of the unevenness) of the basic diffraction grating 22a is thicker than the thickness (t1 in FIG. 2(b)) at the bottom (concave part of the unevenness) of the basic diffraction grating 22a. As a result, the grooves of the coating film 26 formed on the coating film 26 are deeper than the grooves of the basic diffraction grating 22a. In other words, the blazed diffraction grating 20 of this embodiment is configured so that the sum of the film thicknesses of the reflective film 24 and the coating film 26 is maximum at the tops of the blazed surfaces 26b and the step surfaces 26c and minimum at the bottoms. The thickness of the coating film 26 is as follows: t2 and the film thickness at the bottom is t1 When the above formula (1) is satisfied, it is preferable that the following conditional expression (1) is satisfied. In this embodiment, the blaze height (h2) is 60 nm. t2-t1 ≦80 nm (1)
[0020] In this way, when the reflective film 24 and the coating film 26 are formed on the basic diffraction grating 22a of the substrate 22, the inclination of the blaze surface 26b and the step surface 26c becomes steeper than the inclination of the basic blaze surface 22b and the basic step surface 22c. The angle β2 (vertex angle) is smaller (i.e., acute) than the angle β1 between the base blaze surface 22b and the base step surface 22c. Therefore, the blaze angle θB2 of the blazed diffraction grating 20 is larger than the blaze angle θB1 of the base diffraction grating 22a, and as a result, the blaze wavelength becomes 180 nm (i.e., shifted to the longer wavelength side). In addition, the diffraction efficiency is increased because the apex angle of the blaze is acute (details will be described later). In this specification, the relative diffraction efficiency refers to a value that indicates the efficiency of the blazed diffraction grating 20 alone excluding the reflectance of the coating material (i.e., the coating film 26), and is a value indicated by "absolute diffraction efficiency / reflectance of the coating material."
[0021] (Method of manufacturing blazed diffraction grating 20) Next, a method for manufacturing the blazed diffraction grating 20 of this embodiment will be described in detail.
[0022] (1) Preparation of substrate 22 In manufacturing the blazed diffraction grating 20, first, a substrate 22 (basic replica diffraction grating) is prepared, which is formed by a conventional ion beam etching method or the like.
[0023] (2) Attachment of the base material 22 The substrate 22 is then mounted in a vacuum chamber 100 . Fig. 3 is a diagram showing a schematic configuration of a vacuum chamber 100 used for manufacturing the blazed diffraction grating 20 of this embodiment. As shown in Fig. 3, the vacuum chamber 100 is composed of a chamber body 101 and a vacuum pump 102, and the chamber body 101 is provided with a dome body 110, an aluminum boat 120, a magnesium fluoride boat 130, a shutter 140 for the aluminum boat 120, and a shutter 150 for the magnesium fluoride boat 130. The dome body 110 is a dome-shaped body with a radius of 300 mm that rotates horizontally, and the upper end (connection part) of the dome body 110 is disposed approximately 500 mm above the deposition sources (shutters 140, 150). The surface of the dome body 110 serves as a mounting surface on which the substrate 22 is placed, and the substrate 22 is attached at a position approximately 45 mm below the upper end (connection part) of the dome body 110 with the blaze direction facing the inside of the dome body 110.
[0024] (3) Preparation of the Vacuum Chamber 100 Next, materials are placed into the aluminum boat 120 and the magnesium fluoride boat 130, respectively, and the vacuum pump 102 is started to evacuate the inside of the chamber body 101.
[0025] (4) Formation of Reflective Film 24 Next, after it is confirmed that the inside of the chamber body 101 has reached a film-forming vacuum degree, aluminum and magnesium fluoride are melted in with the shutters 140 and 150 closed. Then, after it is confirmed again that the inside of the chamber body 101 has reached a film-forming vacuum degree, the dome body 110 is rotated at 20 rpm to start vaporizing aluminum, and after confirming a predetermined deposition rate (for example, a predetermined value of 10 nm / sec or more), the shutter 140 is opened. Then, when the desired film thickness (for example, about 80 nm) is confirmed with the film thickness meter, the shutter 140 is closed. Note that the reflective film 24 does not necessarily have to have a uniform film thickness, but it is preferable that the film thickness be approximately uniform.
[0026] (5) Formation of Coating Film 26 Next, evaporation of magnesium fluoride is started, and after a predetermined deposition rate (eg, a predetermined value of 2 nm / sec or more) is confirmed, the shutter 150 is opened. Then, when the desired film thickness (for example, 20 nm) is confirmed with the film thickness meter, the shutter 150 is closed.
[0027] (6) Removal of the finished product The chamber body 101 is opened to the atmosphere, and the finished product on which the coating film 26 is formed is taken out of the chamber body 101, thereby obtaining the blazed diffraction grating 20 of this embodiment.
[0028] 4A shows the results of measuring the cross-sectional shape of the substrate 22 before the formation of the reflective film 24 and the coating film 26 (i.e., the cross-sectional shapes of the basic blaze surface 22b and the basic step surface 22c), and FIG. 4B shows the results of measuring the cross-sectional shape of the blazed diffraction grating 20 after the formation of the reflective film 24 and the coating film 26 (i.e., the cross-sectional shapes of the blaze surface 26b and the step surface 26c). In FIGS. 4A and 4B, the solid lines show the measurement results when a sample of the blazed diffraction grating 20 of this embodiment is measured from left to right, and the dashed lines show the measurement results when a sample of the blazed diffraction grating 20 of this embodiment is measured from right to left. 4(a) and (b), the blazed diffraction grating 20 of this embodiment has a blaze height 20 nm higher and an acute apex angle, resulting in a higher diffraction efficiency (maximum relative diffraction efficiency: 55%) than a diffraction grating with the same blaze height.
[0029] Although the present embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications are possible within the scope of the technical concept of the present invention.
[0030] For example, in this embodiment, a blazed diffraction grating 20 with a blaze height (h2): 60 nm and a blaze wavelength: 180 nm was obtained using a substrate 22 with a blaze height (h1): 40 nm and a blaze wavelength: 120 nm, but by changing the deposition conditions of the coating film 26, diffraction gratings 26a with various blaze heights (h2) can be formed, and blazed diffraction gratings 20 with different blaze wavelengths (for example, 120 to 300 nm) can be manufactured. Therefore, it is possible to obtain blazed diffraction gratings 20 with different blaze wavelengths without producing (preparing) a master diffraction grating according to the blaze height (h2) as in the conventional method.
[0031] Furthermore, although the thickness of the reflective film 24 in this embodiment is 80 nm, the present invention is not limited to this configuration, and the thickness can be set within the range of 40 to 80 nm.
[0032] (Second Example) FIG. 5 is a diagram illustrating the cross-sectional shape of the blazed diffraction grating 20 manufactured by changing the deposition conditions of the coating film 26. FIG. 5(a) shows the result of measuring the cross-sectional shape of the substrate 22 before deposition of the reflective film 24 and the coating film 26 of the second embodiment (i.e., the cross-sectional shapes of the basic blaze surface 22b and the basic step surface 22c), and FIG. 5(b) shows the result of measuring the cross-sectional shape of the blazed diffraction grating 20 after deposition of the reflective film 24 and the coating film 26 of the second embodiment (i.e., the cross-sectional shapes of the blazed surface 26b and the step surface 26c). In FIG. 5(a) and FIG. 5(b), the solid lines show the measurement results when a sample of the blazed diffraction grating 20 of this embodiment is measured from left to right, and the dashed lines show the measurement results when a sample of the blazed diffraction grating 20 of this embodiment is measured from right to left.
[0033] The blazed diffraction grating 20 of this embodiment differs from the blazed diffraction grating 20 of the first embodiment in that it uses a substrate 22 with 1200 grooves, a blaze height (h1): 45 nm, and a blaze wavelength: 140 nm, and has a blaze height (h2): 90 nm and a blaze wavelength: 220 nm. The manufacturing method of the blazed diffraction grating 20 of this embodiment is the same as that of the first embodiment. 5(a) and (b), the blazed diffraction grating 20 of this embodiment has a blaze height 40 nm higher and an acute apex angle, and a higher diffraction efficiency (maximum relative diffraction efficiency: 70%) was obtained than a diffraction grating with the same blaze height.
[0034] [Aspects] It will be appreciated by those skilled in the art that the exemplary embodiments described above are examples of the following aspects.
[0035] (Item 1) A blazed diffraction grating (20) according to one embodiment comprises: a substrate (22) having a sawtooth cross-sectional shape, in which blazed surfaces (22b) and stepped surfaces (22c) are alternately and repeatedly arranged in one direction; a reflective film (24) formed so as to cover the surfaces of the blaze surface (22b) and the step surface (22c); a coating film (26) formed so as to cover the surface of the reflective film (24); Equipped with The sum of the film thicknesses of the reflective film (24) and the coating film (26) is configured to be maximum at the tops of the blazed surface (22b) and the step surface (22c) and minimum at the bottoms.
[0036] According to the blazed diffraction grating described in paragraph 1, since the apex angle of the blaze is acute, higher diffraction efficiency can be obtained compared to conventional blazed diffraction gratings. In addition, since a new blazed surface and step surface different from the blazed surface (22b) and step surface (22c) are formed by the coating film (26), a blazed diffraction grating with an arbitrary blazed wavelength can be obtained.
[0037] (2) The blazed diffraction grating (20) according to (1), The coating film (26) has a thickness at the top of t2 and the film thickness at the bottom is t1 is configured to satisfy the following conditional expression (1). t2-t1 ≦80 nm (1)
[0038] According to the blazed diffraction grating described in item 2, by appropriately selecting t1 and t2 that satisfy conditional formula (1), high diffraction efficiency can be obtained at specific wavelengths in the vacuum ultraviolet and deep ultraviolet regions.
[0039] (Item 3) The blazed diffraction grating (20) according to item 1 or 2, The coating film (26) is configured so that the film thickness on the blazed surface (22b) monotonically increases from the bottom to the top.
[0040] According to the blazed diffraction grating described in paragraph 3, the loss of light is reduced, and therefore the diffraction efficiency can be further improved.
[0041] (Item 4) A blazed diffraction grating (20) according to any one of items 1 to 3, The coating film (26) is a vapor-deposited film of a fluoride.
[0042] The blazed diffraction grating described in item 4 can be manufactured easily and inexpensively.
[0043] (Item 5) In the blazed diffraction grating (20) according to item 4, The fluoride is magnesium fluoride.
[0044] The blazed diffraction grating described in item 5 can be manufactured easily and inexpensively.
[0045] (Item 6) A blazed diffraction grating (20) according to any one of items 1 to 5, The reflective film has a substantially constant thickness.
[0046] The blazed diffraction grating described in item 6 has a constant diffraction efficiency.
[0047] (Item 7) In the blazed diffraction grating (20) according to item 6, The reflective film has a thickness of 40 to 80 nm.
[0048] The blazed diffraction grating described in item 7 has a constant diffraction efficiency.
[0049] (Item 8) A blazed diffraction grating (20) according to any one of items 1 to 7, The reflective film is a vapor-deposited aluminum film.
[0050] The blazed diffraction grating described in item 8 can be manufactured easily and inexpensively.
[0051] (Item 9) A blazed diffraction grating (20) according to any one of items 1 to 8, The blaze wavelength is 120 to 300 nm.
[0052] According to the blazed diffraction grating described in item 9, high diffraction efficiency can be obtained in the vacuum ultraviolet and deep ultraviolet regions.
[0053] (Item 10) A method for manufacturing a blazed diffraction grating (20) according to one embodiment includes the steps of: A step of preparing a substrate (22) having a sawtooth cross-sectional shape and in which blazed surfaces (22b) and stepped surfaces (22c) are alternately and repeatedly arranged in one direction; forming a reflective film (24) so as to cover the surfaces of the blaze surface (22b) and the step surface (22c); forming a coating film (26) so as to cover a surface of the reflective film (24); Including, In the step of forming the coating film (26), the coating film (26) is formed so that the thickness of the coating film (26) is maximum at the tops of the blaze surface (22b) and the step surface (22c) and is minimum at the bottoms.
[0054] According to the method for manufacturing a blazed diffraction grating described in item 10, since the apex angle of the blaze is acute, a blazed diffraction grating with higher diffraction efficiency than a conventional blazed diffraction grating can be obtained. In addition, since a new blazed surface and step surface different from the blazed surface (22b) and step surface (22c) are formed by the coating film (26), a blazed diffraction grating with an arbitrary blaze wavelength can be obtained.
[0055] (Item 11) A method for manufacturing a blazed diffraction grating (20) according to item 10, The coating film (26) has a thickness at the top of t2 and the film thickness at the bottom is t1 is configured to satisfy the following conditional expression (1). t2-t1 ≦80 nm (1)
[0056] According to the method for producing a blazed diffraction grating described in item 11, a blazed diffraction grating having high diffraction efficiency in the vacuum ultraviolet and deep ultraviolet regions can be obtained.
[0057] (Item 12) A method for manufacturing a blazed diffraction grating (20) according to item 10 or 11, In the step of forming the coating film (26), the coating film (26) is formed so that the film thickness of the coating film (26) on the blazed surface (22b) monotonically increases from the bottom to the top.
[0058] According to the method for producing a blazed diffraction grating described in item 12, a blazed diffraction grating with reduced light loss and high diffraction efficiency can be obtained.
[0059] (Item 13) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 12, The coating film (26) is a vapor-deposited film of a fluoride.
[0060] According to the method for producing a blazed diffraction grating described in item 13, a blazed diffraction grating can be obtained easily and inexpensively.
[0061] (Item 14) A method for manufacturing a blazed diffraction grating (20) according to item 13, comprising: The fluoride is magnesium fluoride.
[0062] According to the method for producing a blazed diffraction grating described in item 14, a blazed diffraction grating can be obtained easily and inexpensively.
[0063] (Item 15) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 14, comprising: In the step of forming the coating film, the coating film is formed at a rate of 2 nm / sec or more.
[0064] According to the method for producing a blazed diffraction grating described in item 15, a coating film with a stable thickness can be formed, and a blazed diffraction grating with constant diffraction efficiency can be obtained.
[0065] (Item 16) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 15, In the step of forming the reflective film (24), the reflective film (24) is formed so that the film thickness is approximately constant.
[0066] According to the method for producing a blazed diffraction grating described in item 16, a blazed diffraction grating with constant diffraction efficiency can be obtained.
[0067] (Item 17) A method for manufacturing a blazed diffraction grating (20) according to item 16, comprising: The reflective film has a thickness of 40 to 80 nm.
[0068] According to the method for producing a blazed diffraction grating described in item 17, a blazed diffraction grating with constant diffraction efficiency can be obtained.
[0069] (Item 18) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 17, comprising: The reflective film is an evaporated aluminum film.
[0070] According to the method for producing a blazed diffraction grating described in item 18, a blazed diffraction grating can be obtained easily and inexpensively.
[0071] (Item 19) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 18, comprising: In the step of forming the reflective film, the reflective film is formed at a rate of 10 nm / sec or more.
[0072] According to the method for producing a blazed diffraction grating described in item 19, a reflective film with a stable film thickness can be formed, and a blazed diffraction grating with constant diffraction efficiency can be obtained.
[0073] (Item 20) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 19, comprising: The blaze wavelength is 120 to 300 nm.
[0074] According to the method for producing a blazed diffraction grating described in item 20, a blazed diffraction grating having high diffraction efficiency in the vacuum ultraviolet and deep ultraviolet regions can be obtained.
[0075] (Item 21) A method for manufacturing a blazed diffraction grating (20) according to any one of items 10 to 20, comprising: After preparing the base material, the method further includes attaching the substrate to a surface of the dome body; In the step of forming the reflective film and the step of forming the coat film, the reflective film and the coat film are formed in a state in which the dome body is rotated around the central axis at a predetermined number of rotations.
[0076] According to the method for producing a blazed diffraction grating described in item 21, a coating film with a stable thickness can be formed by utilizing centrifugal force, and a blazed diffraction grating with constant diffraction efficiency can be obtained. [Explanation of symbols]
[0077] 1: Substrate 2: Photoresist layer 3: Resist pattern 4: Lattice groove 5: Metal film 11: Blazed surface 12: Step surface 20: Blazed diffraction grating 22: Base material 22a: Basic diffraction grating 22b: Basic blaze surface 22c: Foundation step surface 24: Reflective film 26: Coating film 26a: Diffraction grating 26b: Blazed surface 26c: Step surface 100: Vacuum chamber 101: Chamber body 102: Vacuum pump 110: Dome body 120: Aluminum boat 130: Magnesium fluoride boat 140: Shutter 150: Shutter
Claims
1. A substrate having a sawtooth cross-sectional shape, in which blazed surfaces and stepped surfaces are repeatedly arranged alternately in one direction; a reflective film formed so as to cover the surfaces of the blaze surface and the step surface; a coating film formed so as to cover a surface of the reflective film; Equipped with A blazed diffraction grating, wherein by changing the thickness of the coating film, a total thickness of the reflective film and the coating film between the tops of the blazed surfaces and the step surfaces of the substrate and the coating film is maximized, and a total thickness of the film between the bottoms of the blazed surfaces and the step surfaces of the substrate and the coating film is minimized.
2. 2. The blazed diffraction grating according to claim 1, wherein the following conditional expression (1) is satisfied, where t2 is a thickness of the coating film between the top portions and t1 is a thickness of the coating film between the bottom portions: t2-t1 ≦ 80nm...(1)
3. 3. The blazed diffraction grating according to claim 1, wherein the thickness of the coating film on the blazed surface monotonically increases from the bottom to the top.
4. The blazed diffraction grating according to claim 1 , wherein the coating film is a vapor-deposited film of a fluoride.
5. The blazed diffraction grating of claim 4 , wherein the fluoride is magnesium fluoride.
6. The blazed diffraction grating according to claim 1 , wherein the reflective film has a substantially constant thickness.
7. 7. The blazed diffraction grating according to claim 6, wherein the reflective film has a thickness of 40 to 80 nm.
8. The blazed diffraction grating according to claim 1 , wherein the reflective film is an evaporated aluminum film.
9. The blazed diffraction grating according to any one of claims 1 to 8, wherein the blaze wavelength is 120 to 300 nm.
10. A step of preparing a substrate having a sawtooth cross-sectional shape, in which blazed surfaces and stepped surfaces are repeatedly arranged alternately in one direction; forming a reflective film so as to cover the surfaces of the blazed surface and the step surface; forming a coating film so as to cover a surface of the reflective film; Including, A method for manufacturing a blazed diffraction grating, wherein the step of forming the coating film includes changing a thickness of the coating film to form the coating film so that a sum of film thicknesses of the reflective film and the coating film between the tops of the blazed surface and the step surface of the substrate and the coating film is maximized, and a sum of film thicknesses between the bottoms of the blazed surface and the step surface of the substrate and the coating film is minimized.
11. 11. The method for manufacturing a blazed diffraction grating according to claim 10, wherein the following conditional formula (1) is satisfied, when a thickness of the coating film between the top portions is t2 and a thickness of the coating film between the bottom portions is t1: t2-t1 ≦ 80nm...(1)
12. 12. The method for manufacturing a blazed diffraction grating according to claim 10, wherein the step of forming the coating film forms the coating film such that a film thickness of the coating film on the blazed surface monotonically increases from the bottom to the top.
13. The method for manufacturing a blazed diffraction grating according to claim 10 , wherein the coating film is a vapor-deposited film of a fluoride.
14. The method for producing a blazed diffraction grating according to claim 13, wherein the fluoride is magnesium fluoride.
15. The method for manufacturing a blazed diffraction grating according to claim 10 , wherein the step of forming the coating film comprises depositing the coating film at a rate of 2 nm / sec or more.
16. 16. The method for manufacturing a blazed diffraction grating according to claim 10, wherein the step of forming the reflective film comprises forming the reflective film so that the film thickness is substantially constant.
17. The method for manufacturing a blazed diffraction grating according to claim 16, wherein the reflective film has a thickness of 40 to 80 nm.
18. The method for manufacturing a blazed diffraction grating according to claim 10 , wherein the reflective film is an evaporated aluminum film.
19. The method for manufacturing a blazed diffraction grating according to claim 10 , wherein the step of forming the reflective film comprises depositing the reflective film at a rate of 10 nm / sec or more.
20. The method for producing a blazed diffraction grating according to any one of claims 10 to 19, wherein the blaze wavelength is 120 to 300 nm.
21. After providing the substrate, the method further includes attaching the substrate to a surface of the dome body; 21. The method for manufacturing a blazed diffraction grating according to claim 10, wherein the step of forming the reflective film and the step of forming the coating film form the reflective film and the coating film while rotating the dome body at a predetermined number of rotations around a central axis.
Citation Information
Patent Citations
Protective film of replica diffraction grating
JP1999160513A
Formed structure
JP2004358924A
Excimer laser device with improved endurance
JP2006295129A
Replica diffraction grating
JP2009092687A
Echelle diffraction grating, excimer laser, echelle diffraction grating manufacturing method and argon fluoride excimer laser