Powder composition for forming thick film conductor, paste for forming thick film conductor, and thick film conductor
A conductive powder and lead-free glass powder composition with specific ratios of SiO2, Bi2O3, and CuO addresses adhesion and plating challenges, ensuring strong adhesion and effective plating in thick film conductors.
Patent Information
- Application Number
- JP2020193286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-20
AI Technical Summary
Existing thick film conductor compositions face challenges in achieving both adhesion to ceramic substrates and plating, particularly when using lead-free glass powders, as high content of glass powder hinders effective plating adherence.
A powder composition comprising a conductive powder and a lead-free glass powder, with specific ratios of SiO2, Bi2O3, and CuO, along with optional CuO, to ensure adhesion and plating adherence, utilizing the anchor effect of a fine step-like pattern on the conductor surface.
The composition achieves both strong adhesion to ceramic substrates and effective plating, even with reduced lead-free glass powder content, enhancing the adhesive strength and plating properties of thick film conductors.
Smart Images

Figure 0007581791000003 
Figure 0007581791000004 
Figure 0007581791000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder composition for forming a thick film conductor, a paste for forming a thick film conductor, and a thick film conductor, and more particularly to a powder composition for forming a thick film conductor and a paste for forming a thick film conductor used for forming a thick film conductor on a ceramic substrate or the like when producing a chip resistor, a resistor network, a hybrid IC, or the like, and in particular to a powder composition for forming a lead-free thick film conductor, a paste for forming a thick film conductor, and a thick film conductor. [Background technology]
[0002] When forming a thick-film conductor using the thick-film technology, generally, a conductive powder with high conductivity is dispersed in an organic vehicle together with an oxide powder such as a glass powder to obtain a paste for forming a thick-film conductor. This paste is then applied in a predetermined shape onto a ceramic substrate such as an alumina substrate by screen printing or the like, and fired at 500°C to 900°C to form the thick-film conductor.
[0003] As the conductive powder, powders of Au, Ag, Pd, Pt, etc., which have high electrical conductivity and can be sintered in an air atmosphere and have a number average particle size of 10 μm or less, are used. Of these, inexpensive Ag powder and Pd powder are mainly used.
[0004] As the glass powder, a lead borosilicate glass powder or a lead aluminoborosilicate glass powder, which has an easy softening point and high chemical durability, is used. However, in recent years, there has been an increasing demand for lead-free conductor pastes from the viewpoint of preventing environmental pollution, and therefore, there is a demand for alternative glass powders. Patent Document 1 discloses a lead-free thick-film conductor forming composition.
[0005] By the way, the thick film conductor formed by using such a composition for forming a thick film conductor is applied as an electrode of electronic components such as chip resistors, resistor networks, and hybrid ICs used in the electronics industry. For example, as shown in the schematic cross-sectional view of FIG. 1, a chip resistor 100 includes an alumina substrate 10, an internal electrode 20 consisting of an upper electrode 21, a side electrode 22, and a back electrode 23 formed by a thick film conductor, a resistive film 30 consisting of a ruthenium oxide-based thick film resistor, and a protective film 40 made of insulating glass covering the resistive film 30. The positional relationship between these is such that a pair of upper electrodes 21 are arranged facing each other in a non-contact state with a gap therebetween, and the resistive film 30 is arranged so as to bridge the gap formed by the upper electrodes 21. In addition, on the exposed electrode surface of the internal electrode 20, an intermediate electrode 50 made of Ni plating or the like and an external electrode 60 made of Sn-Pb solder plating or lead-free solder plating of a Sn-based alloy as an alternative thereto are further formed by electrolytic plating. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-043622 A Summary of the Invention [Problem to be solved by the invention]
[0007] The composition for forming a thick-film conductor contains glass powder in order to ensure adhesion between the thick-film conductor and a ceramic substrate such as an alumina substrate, etc. However, if the glass powder content is high, there is a problem that plating is difficult to adhere to the thick-film conductor.
[0008] Therefore, an object of the present invention is to provide a powder composition for forming a thick film conductor, a paste for forming a thick film conductor, and a thick film conductor which are substantially free of lead and can achieve both good adhesion to a ceramic substrate and good plating even with a small content of lead-free glass powder. [Means for solving the problem]
[0009] In order to solve the above problems, the powder composition for forming a thick-film conductor according to the present invention contains a conductive powder and a lead-free glass powder, and the lead-free glass powder contains, calculated as oxides, 15 mass % to 60 mass % of SiO2, 25 mass % to 70 mass % of Bi2O3, and 5 mass % to 20 mass % of CuO.
[0010] The powder composition for forming a thick-film conductor according to the present invention may further contain CuO powder.
[0011] The powder composition for forming a thick film conductor according to the present invention may have an amount of copper, calculated as CuO, of 1 part by mass or less per 100 parts by mass of the conductive powder.
[0012] The conductive powder may be at least one selected from gold powder, silver powder, palladium powder, and platinum powder.
[0013] The lead-free glass powder may be contained in an amount of 1 part by mass to 3 parts by mass with respect to 100 parts by mass of the conductive powder.
[0014] In order to solve the above problems, the paste for forming a thick film conductor of the present invention contains a mixture of the powder composition for forming a thick film conductor of the present invention, a solvent, and a resin.
[0015] In order to solve the above problems, the thick-film conductor of the present invention includes a conductive powder and lead-free glass, and the lead-free glass contains, calculated as oxides, 15 mass % to 60 mass % of SiO2, 25 mass % to 70 mass % of Bi2O3, and 5 mass % to 20 mass % of CuO.
[0016] The thick film conductor according to the present invention may further contain CuO. Effect of the Invention
[0017] The present invention can provide a powder composition for forming a thick film conductor, a paste for forming a thick film conductor, and a thick film conductor which are substantially free of lead and can achieve both good adhesion to a ceramic substrate and good plating even with a small content of lead-free glass powder. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a schematic cross-sectional view of a chip resistor. [Diagram 2] FIG. 2 is a SEM image of the thick-film conductor according to Example 1. [Diagram 3] FIG. 13 is a diagram showing an SEM image of the thick-film conductor according to Comparative Example 1. [Figure 4] FIG. 13 is a diagram showing an SEM image of a thick-film conductor according to Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Specific embodiments of the present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and can be modified as appropriate without departing from the gist of the present invention.
[0020] The composition for forming a thick-film conductor of the present invention contains a conductive powder and a lead-free glass powder. The lead-free glass powder contains, calculated as oxides, 15% by mass to 60% by mass of SiO2, 25% by mass to 70% by mass of Bi2O3, and 5% by mass to 20% by mass of CuO. As described below, with such a composition for forming a thick-film conductor, even if the content of the lead-free glass powder is small, 1 part by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the conductive powder, a thick-film conductor with excellent plating can be obtained while ensuring adhesion to a ceramic substrate.
[0021] The present inventors have conducted extensive research into lead-free glass powders in order to improve the adhesion of thick-film conductors to ceramic substrates, and as a result have found lead-free glass powders that can be used in compositions for forming thick-film conductors. What is even more surprising is that the addition of the glass powder results in the formation of a fine stepped stripe pattern on the surface of the thick-film conductor. Since the fine stepped pattern is precipitated on the surface of the thick-film conductor, it is expected that the adhesion between the surface of the thick-film conductor and Ni plating film or the like will be improved by the anchor effect. That is, the adhesion between the thick-film conductor and the plating film will be improved by the anchor effect.
[0022] The present invention has been completed based on these findings. The present invention will be described in detail below in the order of (1) a powder composition for forming a thick film conductor and (2) a paste for forming a thick film conductor. In addition, (3) a method for producing a thick film conductor using the paste for forming a thick film of the present invention and (4) a thick film conductor will also be described in detail.
[0023] [(1) Powder composition for forming thick-film conductor] In the present invention, a lead-free powder composition for forming a thick-film conductor can be obtained, and such a composition can be composed of at least a conductive powder and a lead-free glass powder. Here, lead-free means that it is acceptable to include a case where no lead is contained and a case where lead is contained in an unavoidable impurity of 100 mass ppm or less due to lead being mixed in raw material powders such as lead-containing conductive powders and glass powders or in the manufacturing process.
[0024] (Conductive powder) The conductive powder used in the present invention may be any powder used in the formation of a normal thick-film conductor, such as powder of a noble metal such as Au, Ag, Pd, or Pt. These noble metal powders may be used alone or in combination of two or more. Among these, it is preferable to use Ag powder, Pd powder, or a mixture of these powders, in view of their low melting point and cost.
[0025] The conductive powder may be granular, flake-like, or the like, and the shape to be used is appropriately selected according to the application. The number average particle size of the granular conductive powder is preferably 10 μm or less, and considering that the coating property of the paste for forming a thick film conductor according to the present invention is deteriorated, the number average particle size is more preferably 0.1 μm or more and 5.0 μm or less. If the number average particle size exceeds 10 μm, the firing may be delayed during the temperature rise process, which is not preferable. For example, when using a mixed powder of Ag powder and Pd powder, considering that the coating property of the paste for forming a thick film conductor according to the present invention is deteriorated and the uniform dispersion of the Ag powder and the Pd powder is considered, it is preferable that the number average particle size of the granular Ag powder is 0.1 μm or more and 3.0 μm or less, and the number average particle size of the granular Pd powder is 0.01 μm or more and 0.3 μm or less. Here, the number average particle size is the number average particle size obtained from a scanning electron microscope (SEM) image of the powder. In addition, all or part of the granular silver powder may be a flake silver powder having a flake surface diameter of 0.1 μm to 10 μm. The flake surface diameter is the number average diameter determined from a scanning electron microscope (SEM) image of the powder.
[0026] (Lead-free glass powder containing copper) In the present invention, Bi2O3-SiO2-based glass powder is used as the copper-containing lead-free glass powder. In addition, B2O3, alkaline earth elements, and ZnO may be contained to ensure the fluidity of the glass. Considering the temperature at which the thick-film conductor is formed by removing organic components such as resin from the paste for forming the thick-film conductor and forming the thick-film conductor, the glass transition point of these lead-free glass powders is preferably 400°C or higher and 550°C or lower. The lead-free glass used may be crystallized glass or amorphous glass that does not crystallize. The lead-free glass powder is a glass powder that does not contain lead, or a glass powder that contains 100 mass ppm or less of lead as an unavoidable impurity. Here, the glass transition point is measured as the temperature indicating the bending point of the thermal expansion curve by measuring a rod-shaped sample obtained by remelting the lead-free glass powder in the air using thermomechanical analysis (TMA).
[0027] The glass composition in the lead-free glass powder can be a composition that can realize the above-mentioned glass transition point and softening point. In the lead-free glass powder, the content of SiO2 in terms of oxide is 15 mass% or more and 60 mass% or less. If the content of SiO2 is less than 15 mass%, the chemical resistance of the glass may decrease, and the weather resistance, water resistance, and chemical resistance of the glass in the thick-film conductor may decrease, and as a result, problems such as plating defects may occur when Ni plating is performed on the thick-film conductor. On the other hand, if the content of SiO2 is more than 60 mass%, the softening temperature of the glass becomes too high, and the adhesion between the thick-film conductor and the ceramic substrate may be impaired.
[0028] By including bismuth in the lead-free glass powder, the adhesive strength between the internal electrode formed of the thick-film conductor and the ceramic substrate such as an alumina substrate can be improved. For example, the bismuth content in the lead-free glass powder, calculated as Bi2O3, can be set to 25% by mass or more and 70% by mass or less to improve the adhesive strength.
[0029] Furthermore, the lead-free glass powder contains CuO, which provides an effect of improving the adhesive strength with the ceramic substrate. The copper content in the lead-free glass is 5% by mass to 20% by mass as CuO. If the CuO content is less than 5% by mass, the adhesive strength with the ceramic substrate cannot be expected to be improved. On the other hand, if the CuO content exceeds 20% by mass, the adhesive strength with the ceramic substrate cannot be expected to be improved. As the copper-containing lead-free glass powder, one type of lead-free glass powder may be used, or a mixture of multiple lead-free glass powders may be used. When a mixture of multiple lead-free glass powders is used, at least one of these lead-free glass powders must contain copper. For example, the lead-free glass powder contains cupric oxide (CuO) as a copper component, which provides an effect of improving the adhesive strength of the thick-film conductor.
[0030] The amount of total copper contained in the lead-free glass powder, converted into CuO, is desirably 0.05 parts by mass or more and 0.2 parts by mass or less per 100 parts by mass of the conductive powder. If the amount of total copper contained in the lead-free glass powder, converted into CuO, is less than 0.05 parts by mass per 100 parts by mass of the conductive powder, there is a risk that the improvement of the adhesive strength and plating adhesion of the thick film conductor cannot be expected. Also, even if the amount of total copper contained in the lead-free glass powder, converted into CuO, is more than 0.2 parts by mass per 100 parts by mass of the conductive powder, there are cases in which the improvement of the adhesive strength with the ceramic substrate cannot be expected.
[0031] The content of the lead-free glass powder in the powder composition for forming a thick-film conductor is preferably 1 part by mass or more and 3 parts by mass or less with respect to 100 parts by mass of the conductive powder. In consideration of the adhesive strength with the ceramic substrate, plating property, solder wettability, etc., the content is more preferably 1 part by mass or more and 2 parts by mass or less, and even more preferably 1 part by mass or more and 1.5 parts by mass or less. If the content of the lead-free glass powder is less than 1 part by mass, the adhesive strength with the ceramic substrate may be reduced. Also, if the content is more than 3 parts by mass, a phenomenon in which glass floats on the surface of the thick-film conductor may occur, which may reduce the plating property of the thick-film conductor, the solder wettability, etc.
[0032] Furthermore, even if the content of the lead-free glass powder in the powder composition for forming a thick film conductor is 3 parts by mass or less, more preferably (2 parts by mass or less), and even more preferably (1.5 parts by mass or less) per 100 parts by mass of the conductive powder, the thick film conductor can achieve a practical adhesive strength due to the composition of the lead-free glass powder used in the present invention.
[0033] The shape of the lead-free glass powder can be various, such as spherical or needle-like, and is not particularly limited. However, the D of the volume cumulative particle size distribution measured by a particle size distribution analyzer using laser diffraction of the lead-free glass powder is 50 The diameter (median diameter) is preferably 10 μm or less. Considering the coatability of the paste for forming a thick film conductor according to the present invention and the uniform dispersion of the conductive powder and the lead-free glass powder, D50 The diameter is more preferably 0.5 μm or more and 3 μm or less. 50 If the diameter is larger than 10 μm, it is undesirable because it inhibits uniform dispersion of the conductive powder and the lead-free glass powder, causing uneven distribution of the lead-free glass powder and decreasing the adhesive strength between the thick-film conductor and the substrate.
[0034] (Oxide powder) In addition to the lead-free glass powder described above, the powder composition for forming a thick-film conductor may contain oxide powders other than these within a range that does not impair the effects of the present invention. For example, at least one oxide powder such as CuO, Bi2O3, SiO2, ZnO, TiO2, ZrO2, and MnO2 may be added to improve the adhesive strength, acid resistance, solder wettability, etc. of the thick-film conductor. However, from the viewpoint of suppressing an increase in resistance value, the content of oxide powders other than the lead-free glass powder is preferably limited to a range of about 0 to 10 parts by mass in total relative to 100 parts by mass of the conductive powder.
[0035] (CuO powder) Among these oxide powders, the use of CuO in combination is expected to further improve the adhesive strength. However, if the total amount of copper, calculated as CuO, exceeds 1 part by mass per 100 parts by mass of conductive powder, it may affect the electrical properties of the resistive film formed on the surface of the thick-film conductor. Furthermore, the resistive film used together with the thick-film conductor is used by applying and firing a thick-film resistor paste, and the resistive film formed may contain CuO as an additive to adjust the electrical properties. There is a concern that the CuO contained in the thick-film conductor will diffuse into the resistive film when the thick-film resistor paste is fired, changing the electrical properties of the resistive film, so it is not preferable to contain more than 1.5 parts by mass of copper as mentioned above.
[0036] In addition, the powder composition for forming a thick-film conductor of the present invention is preferably a mixture of conductive powder, lead-free glass powder, and CuO powder. By using these mixtures, it is possible to obtain a paste for forming a thick-film conductor or a thick-film conductor with more uniform contents. As a mixing method, known techniques such as a ball mill and a bead mill can be used, and these techniques can be used to obtain a sufficiently uniform mixture.
[0037] [(2) Paste for forming thick film conductors] An example of the paste for forming a thick film conductor of the present invention is a paste containing a mixture of the above-mentioned powder composition for forming a thick film conductor of the present invention, a solvent, and a resin.
[0038] As the solvent, terpineol, butyl carbitol, etc., which are generally used in pastes for forming thick-film conductors, can be used, and as the resin, ethyl cellulose, methacrylate, etc., which are generally used in pastes, can be used. The resin and the solvent are mixed in advance to form an organic vehicle, which can be used to manufacture a paste for forming thick-film conductors. For example, from the viewpoint of cost and ease of handling, a solution of ethyl cellulose in terpineol can be used as the organic vehicle. In the organic vehicle, the ratio of the resin and the solvent is appropriately selected depending on the printability and application method of the final paste composition for forming thick-film conductors.
[0039] The content of the organic vehicle in the paste for forming a thick film conductor can be 15 parts by mass or more and 250 parts by mass or less with respect to 100 parts by mass of the conductive powder. If the content of the organic vehicle is less than 15 parts by mass, the viscosity may be too high and the application of the paste for forming a thick film conductor may be substantially impossible, and if the content exceeds 250 parts by mass, problems may occur such as the occurrence of component bias due to the settling of particles in the paste for forming a thick film conductor, and the denseness of the film of the thick film conductor after firing. Considering the printability and ease of application, the settling of particles as the paste for forming a thick film conductor, and the denseness of the film of the thick film conductor, the content is preferably 20 parts by mass or more and 100 parts by mass or less.
[0040] The paste for forming a thick film conductor of the present invention can be produced by kneading the powder composition for forming a thick film conductor with an organic vehicle. The kneading method is not particularly limited, but can be kneaded using known techniques such as a wet kneading mill, a roll mill, and a tapered roll mill. The viscosity of the resulting conductor paste is appropriately selected depending on the thickness of the intended thick film conductor and the type of ceramic substrate.
[0041] Another example of the paste for forming a thick film conductor of the present invention other than those described above is a paste for forming a thick film conductor comprising conductive particles, lead-free glass particles, and optionally copper oxide particles, a solvent, and a resin, in which the content of the lead-free glass particles is 1.5 parts by mass or more and 3 parts by mass or less per 100 parts by mass of the conductive particles, and the content of the copper oxide particles is 0.5 parts by mass or more and 1 part by mass or less per 100 parts by mass of the conductive particles.
[0042] The contents of the conductive particles, the lead-free glass particles, and the copper oxide particles, which are optionally contained, are the same as those of the conductive powder, the lead-free glass powder, and the copper oxide powder described in the section on the powder composition for forming a thick film conductor above, and therefore the description thereof will be omitted here. Also, the solvent and the resin are the same as those described in the example of the paste for forming a thick film conductor above, and therefore the description thereof will be omitted.
[0043] The paste for forming a thick-film conductor of the present invention can be produced, for example, by adding conductive particles, lead-free glass particles, and optionally copper oxide particles to an organic vehicle to form a mixture, and kneading the mixture. The kneading method is not particularly limited, and kneading can be performed using known techniques such as a wet kneading mill, a roll mill, and a tapered roll mill. The viscosity of the resulting conductor paste is appropriately selected depending on the thickness of the desired thick-film conductor and the type of ceramic substrate.
[0044] In addition to the lead-free glass powder and copper oxide powder, the paste for forming a thick film conductor described above can contain oxide powders other than these to the extent that the effect of the present invention is not impaired. For example, at least one oxide powder such as Bi2O3, SiO2, ZnO, TiO2, ZrO2, and MnO2 can be added to improve the adhesive strength, acid resistance, solder wettability, etc. of the thick film conductor. However, from the viewpoint of suppressing an increase in resistance value, the content of oxide powders other than the lead-free glass powder and the copper oxide powder is preferably limited to a range of about 0 to 10 parts by mass in total relative to 100 parts by mass of the conductive powder.
[0045] [(3) Manufacturing method of thick-film conductors] A method for manufacturing a thick film conductor can include, for example, a coating step of coating a paste for forming a thick film conductor of the present invention onto a ceramic substrate, a drying step of drying the substrate onto which the paste has been coated, and then a firing step of firing at a temperature of 500°C or higher and lower than 900°C.
[0046] (Coating process) The coating process is not particularly limited, and any known technique such as screen printing, letterpress printing, gravure printing, or other printing methods, or a dispenser drawing method can be used, but from the viewpoint of mass production with an appropriate film thickness, it is preferable to apply the coating by screen printing. As the ceramic substrate, a 96% alumina substrate, forsterite, or the like is used depending on the application of the electronic component, and the paste for forming a thick film conductor of the present invention can be applied to any substrate.
[0047] (drying process) After the paste for forming a thick film conductor is applied to the ceramic substrate, it is preferable to dry the applied film together with the ceramic substrate at a temperature condition of 80°C or more and 200°C or less for 2 minutes or more and 15 minutes or less. In this way, by providing a drying step between the application step and the firing step, it is possible to prevent the volatilization and combustion of the solvent, etc., due to the volatile components such as the solvent remaining even during firing, and therefore, when a firing furnace is used in the firing step, it is possible to obtain an effect of preventing contamination of the firing furnace. In this step, the drying method is not particularly limited, and known means such as an oven or a belt-type drying furnace can be used, but from the viewpoint of mass production, it is preferable to dry using a belt-type drying furnace. In addition, if the drying temperature is less than 80°C, the time required for drying is long, which may deteriorate productivity, and therefore this is not preferable. In addition, if the drying temperature exceeds 200°C, the resin may be oxidized, and the film after drying may become brittle, which is not preferable.
[0048] (Firing process) In the firing process after the drying process, the dried film is heated together with the ceramic substrate to fire the film. As a firing method, it is preferable to use a belt furnace. In this case, the peak temperature in firing is 500°C or more and less than 900°C, preferably 700°C or more and less than 900°C. If the peak temperature is less than 500°C, the lead-free glass powder is not melted sufficiently, which may cause a problem of impairing adhesion with the ceramic substrate. On the other hand, if the peak temperature is 900°C or more, the film may be oversintered, and in particular, when a paste for forming a thick film conductor mainly composed of Ag, which has a low melting point, is used, the conductive particles and glass particles may be separated, and the thick film conductor may be formed in an island shape, which may cause a problem that a uniform electrode film cannot be formed.
[0049] It is necessary to hold the above peak temperature for 5 minutes or more and 20 minutes or less, preferably 7 minutes or more and 13 minutes or less. If the peak temperature is held for more than 20 minutes, the thick film conductor film may be oversintered, and if the holding time is less than 5 minutes, the sintering may be insufficient. In addition, the total time of the firing process, which includes heating to the peak temperature, holding the peak temperature, and cooling from the peak temperature, must be 20 minutes or more and 90 minutes or less, preferably 30 minutes or more and 60 minutes or less. If the total time is less than 20 minutes, the heating rate and cooling rate may become too large, and the thick film conductor may crack due to a sudden temperature change. In addition, if the total time exceeds 90 minutes, there is a risk of a problem of reduced productivity.
[0050] In order to perform firing at the peak temperature and firing time described above, it is preferable that the heating rate to the peak temperature is 20°C / min or more and 150°C / min or less, and the cooling rate from the peak temperature is 20°C / min or more and 200°C / min or less. If the heating rate is less than 20°C / min or the cooling rate is less than 20°C / min, productivity may deteriorate, which is not preferable. Also, if the heating rate exceeds 150°C / min or the cooling rate exceeds 200°C / min, it is not preferable because the thick-film conductor may crack due to a sudden temperature change.
[0051] The atmosphere during firing is not particularly limited, but firing in an air atmosphere is preferred from the viewpoint of softening the lead-free glass.
[0052] [(4) Thick film conductor] The thick-film conductor of the present invention obtained from the paste for forming a thick-film conductor of the present invention by the above-mentioned manufacturing method contains a conductive component, a glass component obtained by melting a lead-free glass powder, and CuO as appropriate. CuO means a state in which it is dissolved in the glass.
[0053] Furthermore, since the thick-film conductor contains CuO, the glass is less likely to protrude from the surface, and fine stepped stripes are formed on the surface.
[0054] The preferred thickness of the thick-film conductor is 5.0 μm to 10.0 μm, inclusive, because this thickness range satisfies the adhesiveness of the thick-film conductor to the ceramic substrate and prevents glass from coming off the surface of the thick-film conductor.
[0055] Therefore, the thick-film conductor of the present invention manufactured using the thick-film conductor forming paste of the present invention has excellent properties, such as good adhesive strength with a ceramic substrate and good plating adhesion. Good plating adhesion can be evaluated as the thickness of Ni electroplating. It has been confirmed that when Ni electroplating is performed at the same current density, a thick-film conductor with glass relief even locally on the surface has a thinner plating thickness than a thick-film conductor in which CuO is added to suppress glass relief on the surface. EXAMPLES
[0056] The present invention will be further described below with reference to examples, but the scope of the present invention is not limited to these examples.
[0057] In Examples 1 and 2 and Comparative Examples 1 to 3, a powder composition for forming a thick-film conductor and a paste for forming a thick-film conductor were prepared using the conductive powder and copper oxide powder shown below and any of the spherical lead-free glass powders 1 to 3 shown in Table 1, and a thick-film conductor was further manufactured. For the obtained thick-film conductor, the fired film thickness was measured, the surface condition was observed, the resistance value was measured, and the adhesive strength with the substrate was evaluated. Furthermore, the thick-film conductor was subjected to Ni electroplating to measure the plating film thickness. The total of alkali metal oxides in Table 1 is mainly the total of metal oxides of Li, K, and Na.
[0058] [Table 1]
[0059] (Conductive powder) Granular silver powder A and flake-shaped silver powder B were used as conductive powders. Silver powder A has a number average particle size of 0.2 μm, and silver powder B has a number average particle size of 6.0 μm. Granular palladium powder has a number average particle size of 0.2 μm. The conductive powder was composed of 48.6 mass% silver powder A, 48.6 mass% silver powder B, and 1.8 mass% palladium powder.
[0060] (copper oxide powder) As the copper oxide powder, CuO (number average particle size: 0.3 μm) was used.
[0061] [Preparation of Powder Composition for Forming Thick Film Conductor] The conductive powder, lead-free glass powder and copper oxide powder were mixed to have the composition shown in Table 2, and the mixture was stirred in a ball mill to prepare a powder composition for forming a thick-film conductor.
[0062] [Preparation of paste for forming thick film conductor] A paste for forming a thick-film conductor was prepared by mixing 73.5% by mass of the powder composition for forming a thick-film conductor prepared above with 26.5% by mass of an organic vehicle, and then kneading the mixture with a three-roll mill. The organic vehicle was prepared by mixing 7% by mass of ethyl cellulose with 93% by mass of a terpineol solution as a solvent, and heating the mixture to dissolve the ethyl cellulose.
[0063] [Manufacturing of thick film conductors] The thick-film conductor forming paste prepared above was screen-printed on a 96% alumina substrate (25.4 mm x 25.4 mm x 1 mm) using a screen printer (application process), and then dried at 150°C for 5 minutes using a belt-type drying furnace (drying process). The dried film and alumina substrate were fired in the belt furnace for a total of 30 minutes at a peak temperature of 850°C for 9 minutes (firing process), forming a thick-film conductor of a specified pattern.
[0064] [Evaluation of physical properties of thick-film conductors] The thick-film conductor manufactured above was subjected to the following methods: measurement of fired film thickness, plating film thickness, observation of surface condition, measurement of resistance value, and evaluation of adhesive strength with the alumina substrate. The evaluation results are shown in Table 2.
[0065] (Measurement of fired film thickness) The thickness of the thick-film conductor after firing was measured using a contact type surface roughness meter.
[0066] (Plating thickness) The thickness of the Ni electroplated surface from the alumina substrate of the sample in which Ni electroplating was performed on the fired thick-film conductor by the method described below was measured using a contact-type surface roughness meter, and the plating thickness was calculated by subtracting the thickness of the thick-film conductor from the obtained result.
[0067] (Observation of surface condition) The surface condition of the thick-film conductor was observed using a scanning electron microscope (SEM) to confirm the presence or absence of stepped stripes and glass protrusion. Fig. 2 shows an SEM image of the thick-film conductor of Example 1, Fig. 3 shows an SEM image of the thick-film conductor of Comparative Example 1, and Fig. 4 shows an SEM image of the thick-film conductor of Comparative Example 2.
[0068] (Resistance measurement) The resistance value of a sample of a thick-film conductor formed in a pattern with a width of 0.5 mm and a length of 50 mm on an alumina substrate was measured with a digital multimeter.
[0069] (Evaluation of adhesive strength) A thick-film conductor was formed on an alumina substrate in a 2.0 mm × 2.0 mm pad pattern. The Ni plating solution was adjusted to 280 g / L of nickel sulfate, 60 g / L of nickel chloride, and 40 g / L of boric acid, and the current density was set at 5 × 10 -3 A / mm 2 (5×10 -9 A / m 2) and Ni electroplating was performed for 2 minutes to prepare a sample. A 0.65 mm diameter Sn-plated copper wire was soldered to the plated sample using lead-free solder with a composition of 96.5 mass% Sn-3 mass% Ag-0.5 mass% Cu to prepare a test piece. The initial strength of the adhesive strength was evaluated by pulling the Sn-plated copper wire of the test piece in a direction perpendicular to the plane of the alumina substrate using a tensile tester, peeling the thick conductor film from the alumina substrate, measuring the tensile force at the time of peeling, and calculating the maximum, minimum, and average values. In addition, the thermally deteriorated adhesive strength was evaluated by applying a heat load of 150°C for 24 hours to the same test piece as above, deteriorating it, and then performing a tensile test in the same manner, and calculating the maximum, minimum, and average values. 15 test pieces were evaluated for both the initial adhesive strength and the thermally deteriorated adhesive strength.
[0070] [Table 2]
[0071] (Thick film conductor thickness and resistance) The thickness of the thick-film conductor was within the range of 5.0 μm to 10.0 μm in all of Examples 1 and 2 and Comparative Examples 1 to 3, and no abnormality was observed in the thickness.Also, no abnormality was observed in the resistance value.
[0072] (Evaluation of adhesive strength) From the results of Examples 1 and 2 and Comparative Examples 1 and 2, no particular abnormality was observed in the adhesive strength in either the initial evaluation or the evaluation after thermal degradation. Moreover, from the results of Comparative Example 3, it was confirmed that the adhesive strength was not practical in either the initial evaluation or the evaluation after thermal degradation.
[0073] Moreover, the results of Example 1 and Comparative Examples 1 and 2 show that the adhesive strength is high when the glass component contains 12 mass% CuO. Moreover, the results of Example 2 and Comparative Example 3 show that Example 2 can secure a practical adhesive strength (average value) of 40 N or more even if the thick-film conductor composition does not contain CuO powder.
[0074] (Observation of surface condition) In Example 1, the glass component contained 12 mass% CuO, which resulted in a large amount of stepped striped patterns, and the surface condition was such that the anchor effect could be expected to improve plating adhesion (Fig. 2). In Comparative Example 1, no striped patterns were observed (Fig. 3). In Comparative Example 2, the glass component contained 23 mass% CuO, which resulted in some stepped striped patterns, but the surface condition was not such that the anchor effect could be expected (Fig. 4).
[0075] In addition, when comparing the thickness of the Ni electroplating film in Examples 1 and 2 with that in Comparative Examples 1 to 3, it is found that the Ni electroplating film becomes thicker by including CuO in the glass component. From this result, it is clear that the plating adhesion of the thick film conductor obtained from the powder composition for forming a thick film conductor containing CuO in the glass component is excellent.
[0076] [summary] As is apparent from Examples 1 and 2 and Comparative Examples 1 to 3, it is clear that the powder composition for forming a thick film conductor and the method for producing a paste for forming a thick film conductor of the present invention can provide a thick film conductor that is easy to plate and maintains high adhesive strength.
[0077] Although the preferred embodiment of the present invention has been described in detail above, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally fall within the technical scope of the present invention. [Explanation of symbols]
[0078] 10 Alumina substrate 20 Internal electrode 21 Top electrode 22 Side electrode 23 Back electrode 30 Resistive film 40 Protective film 50 Intermediate electrode 60 External electrode 100 Chip Resistors
Claims
1. A conductive powder; and a lead-free glass powder, The lead-free glass powder has a content of SiO 2 15% by mass to 60% by mass of Bi 2 O 3 and 5% to 20% by mass of CuO; A powder composition for forming a thick-film conductor, the powder composition having a total copper content, calculated as CuO, of 1 part by mass or less per 100 parts by mass of the conductive powder.
2. The powder composition for forming a thick film conductor according to claim 1 , further comprising a CuO powder.
3. The powder composition for forming a thick-film conductor according to claim 1, wherein the lead-free glass powder is a powder that does not contain SrO.
4. 4. The powder composition for forming a thick-film conductor according to claim 1, wherein the conductive powder is at least one selected from the group consisting of gold powder, silver powder, palladium powder and platinum powder.
5. 5. The powder composition for forming a thick-film conductor according to claim 1, wherein the lead-free glass powder is contained in an amount of 1 to 3 parts by mass per 100 parts by mass of the conductive powder.
6. A paste for forming a thick-film conductor, comprising a mixture of the powder composition for forming a thick-film conductor according to any one of claims 1 to 5, a solvent, and a resin.
7. A conductive powder; and lead-free glass, The lead-free glass has a content of SiO 2 15% by mass to 60% by mass of Bi 2 O 3 and 5% to 20% by mass of CuO; A thick-film conductor having a total copper amount, calculated as CuO, of 1 part by mass or less per 100 parts by mass of the conductive powder.
8. The thick film conductor of claim 7 further comprising CuO.
Citation Information
Patent Citations
Leadless glass powder for silver paste of anode of solar cell and preparation method of leadless glass powder
CN102503150A
Lead-free soldering-resistant electric conduction silver paste for electro-thermal film quartz glass tube electric heating piece and preparation method
CN103165220A
Glass composition containing neither cadmium nor lead and thick film paste composition
JP1996067533A
Composition for forming thick film conductor, thick film conductor formed by using the same, and chip resistor using thick film conductor
JP2012043622A
Conductive composition, method for manufacturing conductor, and method for forming wiring of electronic component
JP2018190491A