Metal particle-containing composition, bonding paste, and bonded body
A metal particle composition with specific organic-coated particles and a dispersion medium addresses bonding strength issues in high-temperature environments, ensuring robust and printable bonding pastes.
Patent Information
- Application Number
- JP2020211948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-22
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-22
AI Technical Summary
Existing bonding materials, such as those using silver nanoparticles, suffer from poor bonding strength that decreases with cooling and heating cycles, and high concentrations lead to poor fluidity and blurred prints.
A metal particle-containing composition comprising metal particles with a specific diameter range coated with organic compounds having functional groups like hydroxyl, carboxy, or amino groups, along with a dispersion medium, to enhance bonding strength and printability.
The composition maintains high bonding strength through heating and cooling cycles and ensures excellent printability even at high metal particle concentrations, resulting in a strong and defect-free bonded body.
Smart Images

Figure 0007581841000001 
Figure 0007581841000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a metal particle-containing composition, a bonding paste, and a bonded body. [Background technology]
[0002] Conventionally, solder has been used as a bonding material for bonding metal members together, between a metal member and a semiconductor element, between a metal member and a light-emitting diode (LED) element, etc. In recent years, in the technical field of next-generation power electronics, devices such as SiC capable of operating at high temperatures are in demand. As a bonding material for manufacturing such devices, a substitute material for solder is required from the viewpoint of high-temperature operation reliability, and for example, as shown in Patent Documents 1 to 3, bonding materials such as bonding pastes using sinterable metal particles have been proposed.
[0003] Patent Document 1 discloses a bonding material containing metal submicron particles with an average primary particle size of 0.5 to 3.0 μm and metal nanoparticles with an average primary particle size of 1 to 200 nm that are coated with an organic compound having 6 to 8 carbon atoms. However, there is a problem in that the bonding strength at the bonded portion is poor, and the bonding strength decreases with thermal cycles.
[0004] Patent Document 2 discloses a bonding material containing silver nanoparticles having an average primary particle size of 1 to 200 nm and coated with an organic substance having 8 or less carbon atoms, and a flux component having at least two carboxyl groups. Patent Document 3 discloses a bonding material containing silver fine particles having an average primary particle size of 130 nm or less, and a cross-linked interparticle distance-maintaining agent that maintains the distance between the silver fine particles.
[0005] However, even with these bonding materials, there was a problem that the strength of the bonded parts was poor and the bonding strength decreased with thermal cycles, as with the technology disclosed in Patent Document 1. Furthermore, when a bonding paste containing a high concentration of silver nanoparticles was created to achieve a dense and strong bond, it also had the disadvantage of significantly poor fluidity. As a result, in the process of printing the bonding paste on the bonded parts, there was a problem that the printed parts were smudged and non-coated parts were formed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-80147 A [Patent Document 2] JP 2011-240406 A [Patent Document 3] JP 2018-109232 A Summary of the Invention [Problem to be solved by the invention]
[0007] Required properties of a bonding paste using metal particles include suitability for printing on the parts to be bonded, sufficient bonding strength, and minimal loss of bonding strength after reliability tests such as thermal cycles.
[0008] Therefore, the problem to be solved by the present invention is to provide a metal particle-containing composition that has high bonding strength at the bonded portion and suppresses the decrease in bonding strength due to thermal cycling. In addition to the above characteristics, the present invention is to provide a bonding paste that has excellent printability on the bonded body even if it contains a high concentration of metal particles. Furthermore, the present invention is to provide a bonded body that does not deteriorate due to thermal cycling. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention relates to a metal particle-containing composition comprising metal particles (A) having an average particle diameter of 180 nm to 1000 nm and a compound (B) having 20 to 80 carbon atoms and having two or more functional groups (b) which are any one selected from a hydroxyl group, a carboxy group, and an amino group.
[0010] The present invention also relates to the metal particle-containing composition, wherein the number of the functional groups is two or three.
[0011] The present invention also relates to the metal particle-containing composition, wherein the compound (B) has a branched and / or cyclic structure.
[0012] The present invention also relates to the metal particle-containing composition, wherein the compound (B) has an n-valent hydrocarbon group, where n is the number of the functional groups.
[0013] The present invention also relates to the metal particle-containing composition, wherein the n-valent hydrocarbon group has 30 to 60 carbon atoms.
[0014] The present invention also relates to the metal particle-containing composition, wherein the compound (B) comprises at least one member selected from the group consisting of dimer acid, trimer acid, dimer diol, trimer triol, dimer diamine and trimer triamine.
[0015] The present invention also relates to the metal particle-containing composition, which contains 0.1 to 3 parts by mass of the compound (B) relative to 100 parts by mass of the metal particles (A).
[0016] The present invention also relates to the metal particle-containing composition, which contains 0.3 to 2.5 parts by mass of the compound (B) relative to 100 parts by mass of the metal particles (A).
[0017] The present invention also relates to the metal particle-containing composition, wherein the metal particles (A) have an average particle size of 200 nm to 400 nm.
[0018] The present invention also relates to a bonding paste containing a dispersion medium (C) and the above metal particle-containing composition.
[0019] The present invention also relates to the bonding paste, wherein the mass of the metal particles (A) in the sum of the masses of the metal particles (A), the compound (B) and the dispersion medium (C) is 80 mass % to 95 mass %.
[0020] The present invention also relates to a bonded body in which a first bonded portion and a second bonded portion are bonded with the bonding paste. Effect of the Invention
[0021] According to the present invention, it is possible to provide a metal particle-containing composition that has high bonding strength at the bonded portion and does not decrease with thermal cycling. It is also possible to provide a bonding paste that has excellent printability in addition to the above effects. Furthermore, it is possible to provide a bonded body that does not deteriorate with thermal cycling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] In this specification, "metal particles (A) having an average particle size of 180 nm to 1000 nm" may be abbreviated as "metal particles (A)" and "compound (B) having 20 to 80 carbon atoms and having a plurality of identical functional groups in the molecule" may be abbreviated as "compound (B)".
[0023] The metal particle-containing composition of the present invention contains metal particles (A) and a compound (B). The bonding paste also contains a dispersion medium (C) in addition to the metal particles (A) and the compound (B). The metal particle-containing composition may be formed by volatilizing a part or all of the dispersion medium (C) from the bonding paste during the bonding process.
[0024] (Metal particles (A)) Examples of the metal in the metal particles (A) include gold, silver, copper, nickel, chromium, palladium, rhodium, ruthenium, indium, silicon, aluminum, tungsten, molybdenum, platinum, and alloys thereof. In addition, fine particles coated with a core and a material different from the core material, specifically, for example, silver-coated copper powder, in which the core is copper and the surface is coated with silver, can be mentioned. In addition, powders of metal oxides such as silver oxide, indium oxide, tin oxide, zinc oxide, ruthenium oxide, ITO (tin-doped indium oxide), AZO (aluminum-doped zinc oxide), and GZO (gallium-doped zinc oxide), as well as powders surface-coated with these metal oxides can be mentioned. The type of metal used may be one type, or two or more types may be used in combination.
[0025] The metal particles (A) are preferably selected from copper or silver, since a bonded body having particularly excellent strength can be obtained.Moreover, the metal particles (A) are more preferably silver, since it can be used at a wide range of firing temperatures and in various firing environments, such as under atmospheric pressure, in a nitrogen atmosphere, in a vacuum, or in a reducing atmosphere.
[0026] The metal particles (A) are within a specific average particle size range, and therefore have the ability to melt or bond together (hereinafter also referred to as sintering) at temperatures ranging from 200°C to 350°C at which the metal particle-containing composition or bonding paste is heated and sintered, making it possible for the particles to change into bulk metal. As a result, the objects to be bonded are bonded together. Hereinafter, the area formed by sintering the metal particles (A) between the objects to be bonded is referred to as the bonding layer.
[0027] In the present invention, it is important to use metal particles (A) having a specific average particle size. In this specification, the term "average particle size" means the 50% cumulative particle size distribution particle size (d50) on a volume basis determined by the measurement method described in the Examples. The d50 of the metal particles (A) is 180 to 1000 nm, preferably 200 to 400 nm, and more preferably 200 to 300 nm.
[0028] The metal particles (A) are preferably coated on the surface with an organic component (a). When the metal particles (A) are coated with the organic component (a), it is expected that the storage stability of the metal particle-containing composition and the bonding paste will increase. Examples of the organic component (a) include fatty acids, aliphatic amines, and aliphatic alcohols, and the organic component (a) is preferably a saturated or unsaturated fatty acid, more preferably a saturated or unsaturated fatty acid having 3 to 18 carbon atoms, and even more preferably a saturated or unsaturated fatty acid having 6 to 18 carbon atoms. The organic component (a) may contain one or more types.
[0029] The metal particles (A) may be used alone or in combination. If necessary, metal particles other than the metal particles (A) may be used in combination. When metal particles other than the metal particles (A) are used in combination, it is preferable to use metal particles having an average particle size of more than 1000 nm in combination.
[0030] <Compound (B)> Next, the compound (B) will be described. Generally, since metal particles are powder, when the compound (B) is not included, as the dispersion medium evaporates from the bonding paste, it becomes difficult to form an interface with the bonded part, but by coexisting the compound (B) of the present invention, even after a part or all of the dispersion medium (C) evaporates, the composition can behave as a liquid metal particle-containing composition, so that it is easy to form a good bonded interface that is integrated with the bonded part.
[0031] Compound (B) has two or more functional groups selected from hydroxyl groups, carboxy groups, and amino groups (hereinafter, these functional groups will be referred to as "functional groups (b)") in the molecule, and has a structure containing 20 to 80 carbon atoms.
[0032] The number of carbon atoms in compound (B) includes the number of carbon atoms in functional group (b). Therefore, when functional group (b) in compound (B) is a carboxy group, the number of carbon atoms in the carboxy group is considered to be the number of carbon atoms in compound (B).
[0033] In the compound (B), the skeleton (partial structure) excluding the functional group (b) is an organic residue, but is preferably a hydrocarbon group or a group in which multiple hydrocarbon groups are bonded with a linking group containing a hetero atom. Examples of such linking groups containing a hetero atom include -O- group (ether group), -C(=O)- group (carbonyl group), -C(=O)-O- group (also called ester group or oxycarbonyl group), and -C(=O)-NH- group (also called amide group or iminocarbonyl group). It is preferable that the compound (B) does not have any functional group other than the functional group (b).
[0034] The state of compound (B) is not particularly limited, but it is preferably liquid in the temperature range of 200° C. to 350° C., which is the temperature range in which the metal particle-containing composition of the present invention is fired. Compound (B) may be solid or liquid at room temperature (25° C.), but is more preferably liquid at room temperature in that it can be uniformly dispersed in the metal particle-containing composition and act effectively.
[0035] When the compound (B) has the property of being liquid in the above temperature range, it is expected that the wettability at the bonding interface with the bonded parts will increase, and the contact area will increase. As a result, it is possible to manufacture a bonded body having a strong bonding interface. In addition, even if voids are formed in the bonding layer during sintering, the fluidity of the metal particle-containing composition increases, so that the liquid compound (B) flows into defective parts such as voids, and it is possible to obtain a bonding layer and a bonded body with fewer defects.
[0036] The number of functional groups (b) in the compound (B) is preferably 2 or 3.
[0037] The compound (B) may have a linear structure or a branched and / or cyclic structure, but preferably has a branched and / or cyclic structure. When the compound (B) has a branched and / or cyclic structure, it is preferable that the compound (B) has a branched and / or cyclic structure, since the compound (B) has low crystallinity and is easily liquid with good fluidity.
[0038] When the number of functional groups (b) in compound (B) is n, compound (B) preferably has an n-valent hydrocarbon group. In compound (B), the skeleton excluding functional groups (b) is more preferably composed of only n-valent hydrocarbon groups, in that a strong bonded body can be obtained.
[0039] For the above reasons, it is preferable that the compound (B) does not evaporate immediately when sintering is started, but it does not necessarily have to remain in the formed bonding layer when sintering is completed. When the carbon number of the n-valent hydrocarbon group is 30 to 60, the amount of the compound (B) remaining in the bonding layer after sintering can be further reduced, which is preferable because it is easy to obtain a denser bonding layer. As a result, the initial bonding strength is excellent, and it can be expected that the decrease in the bonding strength due to the thermal cycle is further suppressed.
[0040] Specific examples of compound (B) having a linear structure include eicosane diacid, heneicosane diacid, docosane diacid, tetracosane diacid, triacontanedioic acid, dotriacontanedioic acid, tetracontanedioic acid, pentacontanedioic acid, hexacontanedioic acid, and batyl alcohol, but are not limited to these.
[0041] Examples of branched and / or cyclic structures include, but are not limited to, dimer acid, trimer acid, tetramer acid, dimer diol, trimer triol, tetramer tetraol, dimer diamine, trimer triamine, tetramer tetramine, phytantriol, and the like.
[0042] Among these specific examples, it is more preferable that the compound (B) is selected from the group consisting of dimer acid, trimer acid, dimer diol, trimer triol, dimer diamine, and trimer triamine, for the reasons described above.
[0043] Dimer acid, trimer acid, and tetramer acid can be produced by a polymerization reaction of unsaturated fatty acids. For example, they can be produced by a Diels-Alder reaction between oleic acid (carbon number 18) and linoleic acid (carbon number 18) or a radical reaction. The carbon numbers of dimer acid, trimer acid, and tetramer acid are preferably 36, 54, and 72, respectively. In addition, by appropriately changing the carbon number of the raw material unsaturated fatty acid, it is possible to produce a compound (B) having a carbon number other than the above. In this specification, the dimer, trimer, and tetramer of unsaturated fatty acid having 12 or more carbon atoms are referred to as dimer acid, trimer acid, and tetramer acid, respectively.
[0044] The dimer diol, trimer triol, and tetramer tetraol have a structure in which the carboxy group of the dimer acid is reduced to a hydroxyl group, respectively. The dimer diol, trimer triol, and tetramer tetraol preferably have 36, 54, and 72 carbon atoms, respectively.
[0045] The dimer diamine has a structure in which the carboxy group of the dimer acid is functionally converted to an amino group, the trimer triamine has a structure in which the carboxy group of the trimer acid is functionally converted to an amino group, and the tetramer tetramine has a structure in which the carboxy group of the tetramer acid is functionally converted to an amino group. The dimer diamine, trimer triamine, and tetramer tetramine preferably have 36, 54, and 72 carbon atoms, respectively.
[0046] Due to the manufacturing process, compound (B) may be a mixture of compounds having different degrees of polymerization. However, it may be used as a mixture of different polymerization products, or a specific single compound may be used.
[0047] In the metal particle-containing composition of the present invention, the compound (B) is preferably contained in an amount of 0.1 to 3 parts by mass, more preferably 0.3 to 2.5 parts by mass, per 100 parts by mass of the metal particles (A). Within this range, it is possible to obtain a bonded body that is particularly excellent in initial bonding strength and in which a decrease in bonding strength due to thermal cycles is suppressed.
[0048] The bonding paste of the present invention contains a dispersion medium (C), which serves to disperse the metal particles (A) and the compound (B).
[0049] The dispersion medium (C) may be any medium capable of uniformly dispersing the metal particles (A) and the compound (B). Specific examples include, but are not limited to, terpineol, dihydroterpineol, dihydroterpinyl acetate, Tersolve MTPH (manufactured by Nippon Terpene Co., Ltd.), Texanol (2,2,4-trimethylpentane-1,3-diol monoisobutyrate), carbitol, carbitol acetate, butyl carbitol, isophorone, γ-butyrolactone, dipropylene glycol monomethyl ether, dipropylene glycol methyl-n-propyl ether, 3-methoxy-3-methylbutyl acetate, ethylene glycol, hexanoic acid, propylene glycol diacetate, dipropylene glycol methyl ether acetate, 1,3-butylene glycol, and isoparaffin-based solvents contained in hydrocarbon-based solvents.
[0050] Among these dispersion media (C), terpineol, dihydroterpineol, tersolve MTPH, texanol, carbitol, carbitol acetate, butyl carbitol, isophorone, γ-butyl lactone, dipropylene glycol monomethyl ether, and isoparaffin-based solvents are more preferably used. These dispersion media (C) can be used alone or in combination.
[0051] When the joining paste is sintered, it is preferable that the boiling point of the dispersion medium (C) is lower than the boiling point of the compound (B), since the amount of the dispersion medium (C) coexisting with the metal particle-containing composition during sintering can be reduced and the content of the metal particles (A) can be increased.
[0052] The bonding paste of the present invention, which uses a combination of metal particles (A) and compound (B), has excellent fluidity even when the metal particles (A) are contained at a high concentration, i.e., when the content ratio of the dispersion medium (C) is low, and therefore has excellent printability on the bonded body, making it possible to obtain a stronger bonded body with fewer defects.
[0053] In the bonding paste, the mass ratio of the metal particles (A) to the sum of the masses of the metal particles (A), the compound (B), and the dispersion medium (C) is preferably 80% by mass to 95% by mass, more preferably 85% by mass to 94% by mass. By including the metal particles (A) in the above range, good printability of the bonding paste can be ensured, and the dispersion medium (C) can be prevented from remaining in the bonded body, and the generation of voids originating from the dispersion medium (C) can be prevented, resulting in good bonding strength.
[0054] The bonding paste of the present invention may contain additives, such as a sintering accelerator, a binder resin, or a resin-type dispersant.
[0055] Examples of the device for preparing the joining paste from the metal particles (A), the compound (B) and the dispersion medium (C) include a disperser, a three-roll mill, a bead mill, an ultrasonic disperser, and a planetary stirrer.
[0056] The bonding paste of the present invention can be used to bond a first portion to be bonded and a second portion to be bonded to obtain a bonded body.
[0057] The method of applying the bonding paste to the object to be bonded is not particularly limited as long as it can be applied uniformly to the member. For example, various printing methods such as screen printing, flexographic printing, offset printing, gravure printing, metal mask printing, gravure offset printing, and the like, and a discharge method using a dispenser, etc. are included. Since the bonding paste of the present invention has excellent fluidity even when it contains metal particles at a high concentration, it is particularly preferable to use it in combination with metal mask printing.
[0058] When placing the second part to be joined on the first part to be joined coated with the joining paste of the present invention, the second part to be joined can be placed under pressure. The pressure is appropriately set depending on the viscosity of the joining paste and the drying state of the paste, and is preferably 0.1 to 40 MPa, more preferably 0.3 to 30 MPa.
[0059] The sintering conditions for bonding the laminate in which the second bonded portion is placed on the first bonded portion may be appropriately changed, and may include, for example, conditions such as atmospheric pressure, nitrogen atmosphere, vacuum, or reducing atmosphere at 200 to 350°C. Examples of the sintering device include a hot air oven, an infrared oven, a reflow oven, a microwave oven, a hot plate, and an optical sintering device. These devices may be used alone or in combination as appropriate. Pressure may also be applied during sintering. The pressure is appropriately set depending on the viscosity of the bonding paste and the drying state of the paste, and is preferably 0.1 to 40 MPa, and more preferably 0.3 to 30 MPa.
[0060] Before the firing step, a preliminary drying step can be appropriately performed in order to remove organic components from the bonding coating film. For example, the pre-drying step can be performed under conditions in the range of 60 to 220°C using a device similar to the firing device.
[0061] A preferred method for joining two parts to be joined is to apply the joining paste of the present invention to a first part to be joined, place a second part to be joined on it, and heat it up to about 300° C. at a heating rate of about 2° C. / min to perform sintering. After the temperature rise is completed, it is preferable to maintain the temperature higher than the temperature at the end of the temperature rise for about 10 minutes to 2 hours.
[0062] The type of the parts to be joined is not particularly limited, and examples thereof include metal materials, semiconductor materials, plastic materials, ceramic materials, etc. Also included are electronic elements.
[0063] Examples of the metal include copper, gold, and aluminum. Examples of semiconductor materials include silicon, germanium, gallium arsenide, gallium phosphide, cadmium sulfide, silicon nitride, graphite, yttrium oxide, magnesium oxide, silicon carbide, and gallium nitride. Examples of the plastic material include polyimide, polyethylene, polypropylene, polyethylene terephthalate, polycarbonate, and polyethylene naphthalate. Examples of the ceramic material include glass and silicon.
[0064] Examples of electronic elements include semiconductor elements, LED elements, and power device elements.
[0065] The first and second joined parts may be of different types or may not be the same type. The surfaces of the joined parts may be subjected to a corona treatment, a plating treatment, or the like in order to increase the joining strength at the joined portion.
[0066] There is no limit to the thickness of the bonding layer formed when bonding parts to be bonded with the metal particle-containing composition or bonding paste of the present invention, but it is preferably 3 μm to 500 μm, more preferably 10 μm to 200 μm, and even more preferably 20 μm to 100 μm. EXAMPLES
[0067] The present invention will be described in detail below using examples and comparative examples, but the technical scope of the present invention is not limited thereto. In the examples, unless otherwise specified, "parts" means "parts by mass", "%" means "% by mass", and the numerical values in the tables mean "parts" unless otherwise specified.
[0068] (Production example 1) Metal particles A1 Under a nitrogen atmosphere, 200 parts of toluene and 22.3 parts of silver hexanoate were mixed while stirring at 25°C to obtain a 0.5M solution, and then 1.6 parts of diethylaminoethanol and 0.28 parts of oleic acid were added as a dispersant and dissolved. Then, 73.1 parts of a 20% aqueous solution of succinic acid dihydrazide (hereinafter referred to as SUDH) was added dropwise as a reducing agent, and the liquid color changed from light yellow to dark brown. The temperature was raised to 40°C to promote the reaction. After standing and separating, the aqueous phase was removed to remove excess reducing agent and impurities, and distilled water was added to the toluene layer several times, washing and separation were repeated, and then the process of adding toluene, centrifuging, and removing the supernatant was repeated twice. The precipitate was dried to obtain metal particles A1 in which silver particles were coated with hexanoic acid and oleic acid. The particle diameter of metal particles A1 was determined by the method described below, and d50 was 210 nm.
[0069] (Production example 2) Metal particles A2 Metal particles A2 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.8 parts and the amount of oleic acid was 0.31 parts. The d50 was 185 nm. (Production example 3) Metal particles A3 Metal particles A3 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.2 parts and the amount of oleic acid was 0.18 parts. The d50 was 290 nm. (Production example 4) Metal particles A4 Metal particles A4 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 1.0 part and the amount of oleic acid was 0.14 part. The d50 was 390 nm.
[0070] (Production example 5) Metal particles A5 Metal particles A5 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 0.6 parts and the amount of oleic acid was 0.070 parts. The d50 was 1100 nm. (Production example 6) Metal particles A6 Metal particles A6 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 2.3 parts and the amount of oleic acid was 2.8 parts. The d50 was 20 nm. (Production example 7) Metal particles A7 Metal particles A7 were obtained in the same manner as in Production Example 1, except that the amount of diethylaminoethanol was 2.1 parts and the amount of oleic acid was 0.71 parts. d50 was 85 nm. Of the metal particles produced by the above method, metal particles A1 to A4 correspond to metal particles (A), and metal particles A5 to A7 correspond to metal particles other than metal particles (A).
[0071] (Production Example 8) Trimertriol (Compound B4) Trimer triol was synthesized as follows, referring to the method described in JP-A-10-67835. Under a nitrogen atmosphere, 1000 g of an unsaturated fatty acid ester mixture containing 75% methyl oleate, 15% methyl linoleate, and 9% methyl stearate was reacted with 70 g of activated clay in an autoclave at 230° C. for 5 hours. The catalyst was filtered off from the reaction liquid, and 115 g of trimer acid trimethyl ester was obtained by distillation under reduced pressure. In a flask equipped with a dropping funnel, a condenser, a thermometer and a stirrer, 6.4 g of lithium aluminum hydride and 240 ml of diethyl ether were carefully mixed under a nitrogen atmosphere to prepare a dispersion of lithium aluminum hydride. Under a nitrogen atmosphere, while stirring the dispersion, a solution obtained by diluting 50 g of trimer acid trimethyl ester with 70 ml of diethyl ether was dropped over 120 minutes, and the reaction was carried out while maintaining the temperature at about 30°C or less. After dropping, the mixture was stirred for about 40 minutes, and then 13 g of ion-exchanged water was carefully dropped while cooling to inactivate the excess reducing agent. The reaction solution was carefully transferred to a flask containing 70 g of ice water, and 50 g of a 10% aqueous sulfuric acid solution was added. After leaving it to stand for a while, an appropriate amount of diethyl ether was added to the flask to extract the product. The ether layer was repeatedly washed with water until it became neutral, and the diethyl ether was distilled off to obtain 31 g of a trimer triol having 54 carbon atoms and consisting of three hydroxyl groups and a trivalent hydrocarbon group having a branched and cyclic structure. The obtained trimer triol was a viscous liquid at 25°C.
[0072] [Particle size measurement] Isopropyl alcohol was added to each metal particle (A) and dispersed in an ultrasonic disperser to obtain a 0.5% by mass dispersion. The particle size of the metal particles (A) in the dispersion was measured using Nanotrac UPA-EX150 (manufactured by Nikkiso Co., Ltd.) to determine the average particle size (d50).
[0073] [Compound (B)] The following materials were used as compounds (B) other than compound B4. However, compounds B8 and B9 are not compounds (B). The carbon number, material name, and properties at 25°C are written in parentheses. Compounds B1 to B3, B5, and B6 were manufactured by Croda Japan Co., Ltd., and B7 to B9 were reagents manufactured by Sigma-Aldrich. The boiling points of compounds B1 to B7 are all 350°C or higher.
[0074] Compound B1: Pripol 1009 (a hydrogenated dimer acid with 36 carbon atoms. It consists of two carboxyl groups and a divalent hydrocarbon group having a branched and cyclic structure. Liquid) Compound B2: Pripol 1040 (a trimer acid having 54 carbon atoms. It consists of three carboxyl groups and a trivalent hydrocarbon group having a branched and cyclic structure. Liquid) Compound B3: Pripol 2033 (a dimer diol having 36 carbon atoms. It consists of two hydroxyl groups and a divalent hydrocarbon group having a branched and cyclic structure. Liquid) Compound B5: Priamine 1071 [a mixture of a dimer triamine having 36 carbon atoms (liquid, consisting of two amino groups and a divalent hydrocarbon group having a branched and cyclic structure) and a trimer triamine having 54 carbon atoms (liquid, consisting of three amino groups and a trivalent hydrocarbon group having a branched and cyclic structure)] Compound B6: Priamine 1075 (a dimer diamine having 36 carbon atoms. It consists of two amino groups and a divalent hydrocarbon group having a branched and cyclic structure. Liquid) Compound B7: Docosanedioic acid (a straight-chain dibasic acid with 22 carbon atoms. Solid) Compound B8: Oleic acid (a monovalent straight-chain fatty acid with 18 carbon atoms. Liquid) Compound B9: Malonic acid (a divalent straight-chain fatty acid with three carbon atoms. Solid)
[0075] [Dispersion medium (C)] The following materials were used as the dispersion medium (C). The manufacturer's name, supplementary information, and boiling point are given in parentheses. Dispersion medium C1: Dihydroterpineol (manufactured by Nippon Terpene Chemical Co., Ltd., boiling point 207°C) Dispersion medium C2: Isobornylcyclohexanol (manufactured by Nippon Terpene Chemical Co., Ltd., boiling point 318°C) Dispersion medium C3: Isopar L (manufactured by Ando Parachemie Co., Ltd., isoparaffin with a boiling point of 185 to 198°C) Dispersion medium C4: Texanol (Tokyo Chemical Industry Co., Ltd., reagent, boiling point 244°C)
[0076] [Example 1] Metal particles A1 (92 parts), dihydroterpineol (8 parts), and compound B1 (1 part) were mixed using a planetary stirrer to prepare a bonding paste. Then, a bonded body was produced and evaluated by the method described below. The results are shown in Table 1.
[0077] [Examples 2 to 32], [Comparative Examples 1 to 8] A joining paste was obtained in the same manner as in Example 1, except that the types and amounts of materials were changed according to the composition shown in Table 1, and then evaluated. The results are shown in Table 1. In Table 1, unless otherwise specified, the numbers represent parts, and blank spaces represent no blending.
[0078] [Preparation of junction] Each joining paste was printed once on the plated surface of the joining part 1 described below under the printing conditions described below, and then the plated surface of the joining part 2 (chip) described below was placed facing the joining paste surface and heated under the sintering conditions described below to obtain each joining body. <Joined part 1> Gold-plated copper substrate: 20 x 20 x 3 mm <Joined part 2> Gold-plated SiC chip: 5×5×0.3mm <Printing conditions (metal mask printing)> Metal mask: 4mm square opening, 50μm thickness (manufactured by Celia Corporation) Metal squeegee: 40mm x 250mm, thickness 1mm (manufactured by Celia Corporation) <Sintering conditions> The unsintered bonded body was placed in a hot air oven, and the temperature was raised from 25°C to 300°C at 2°C / min. After reaching 300°C, it was held at 300°C for 2 hours. [Evaluation criteria (printability)] ○: Printing was possible on the bonded part 1. ×: Printing on the bonded portion 1 was not possible.
[0079] [Bonding strength (initial, after thermal cycle test) The bond strength (die shear strength) of the obtained bonded body was measured using the following measuring device and test conditions. Note that an asterisk (*) in Table 1 indicates that this evaluation was not performed because printing was not possible.
[0080] Measurement equipment: Universal bond tester (Daisi Japan Co., Ltd., 4000 series) <Test conditions> Measurement height: 100μm Measurement speed: 500μm / s Specifically, the bonded body was fixed at the site of the part to be bonded 1, and the bond was pushed from the interface between the part to be bonded 1 and the bonding layer toward the part to be bonded 2 at a height of 100 μm at a speed of 500 μm / s to determine the bonding strength at which the bond was destroyed. The bonding strength (initial strength) immediately after the bonded body was produced and the bonding strength after the cycle test described below were measured and evaluated based on the evaluation criteria below. The higher the adhesive strength value, the better, and a value of 15 MPa or more is within the practical range. The higher the evaluation criterion value, the better, and an evaluation criterion value of 2 or less indicates poor bonding.
[0081] [Evaluation Criteria] 5:30MPa or more 4: 20MPa or more and less than 30MPa 3: 15MPa or more and less than 20MPa 2: 5MPa or more and less than 15MPa 1: Less than 5MPa
[0082] <Cold-heat cycle test> The bonded body was stored for 500 cycles, with one cycle being a process of holding the bonded body at -40°C for 30 minutes, then holding it at 25°C for 15 minutes, and then holding it at 150°C for 30 minutes.The bonded body was then evaluated using the same procedures and criteria as the above-mentioned bond strength evaluation method.
[0083] When the bonding paste of the comparative example was used, the bonding strength was significantly low, and when the broken sample was observed after the die shear test, the breakage occurred at the interface between the gold-plated SiC chip and the bonding layer. On the other hand, when the bonding paste of the example was used, the bonding strength was very high. When the bonding paste of the example was used, it was confirmed that the printability was excellent and the bonding strength was very high even when the bonding paste contained a high concentration of metal particles, and the decrease in the bonding strength was suppressed even after the thermal cycle test.
[0084] [Table 1]
[0085]
Table 1
Claims
1. A metal particle-containing composition comprising metal particles (A) having an average particle size of 180 nm to 400 nm and a compound (B) having 20 to 80 carbon atoms and having two or more functional groups (b), each of which is any one selected from a hydroxyl group, a carboxy group, and an amino group.
2. 2. The metal particle-containing composition according to claim 1, wherein the number of the functional groups (b) is 2 or 3.
3. 3. The metal particle-containing composition according to claim 1, wherein the compound (B) has a branched and / or cyclic structure.
4. 4. The metal particle-containing composition according to claim 1, wherein the compound (B) has a hydrocarbon group having a valence of n, where n is the number of the functional groups (b).
5. 5. The metal particle-containing composition according to claim 4, wherein the n-valent hydrocarbon group has 30 to 60 carbon atoms.
6. The metal particle-containing composition according to any one of claims 1 to 5, characterized in that the compound (B) comprises at least one member selected from the group consisting of dimer acid, trimer acid, dimer diol, trimer triol, dimer diamine and trimer triamine.
7. 7. The metal particle-containing composition according to claim 1, comprising 0.1 to 3 parts by mass of the compound (B) relative to 100 parts by mass of the metal particles (A).
8. 8. The metal particle-containing composition according to claim 1, comprising 0.3 to 2.5 parts by mass of the compound (B) relative to 100 parts by mass of the metal particles (A).
9. 9. The metal particle-containing composition according to claim 1, wherein the metal particles (A) have an average particle size of 200 nm to 400 nm.
10. A bonding paste comprising a dispersion medium (C) and the metal particle-containing composition according to any one of claims 1 to 9.
11. The mass of the metal particles (A) relative to the sum of the masses of the metal particles (A), the compound (B), and the dispersion medium (C) is 80% by mass to 95% by mass. The bonding paste according to claim 10.
12. A method for manufacturing a joined body, comprising the steps of applying the joining paste according to claim 10 or 11 to a first joined part, placing a second joined part thereon, and joining the first joined part and the second joined part by sintering.
Citation Information
Patent Citations
Joining material and joining method using the same
JP2011080147A
Bonding material and bonding method using the same
JP2011240406A
Joining material and joint body
JP2016000861A
Joint material and joining method using same
JP2018109232A
Solder paste
JP2022060054A