Pressure vessels
A thermoplastic resin liner with a polyamide composition and reinforced outer shell addresses the limitations of direct blow molding by achieving high strength, rigidity, and heat resistance at the pinch-off portion, enhancing pressure vessel performance.
Patent Information
- Application Number
- JP2021016249
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-04
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-02-04
AI Technical Summary
Existing resin liners for pressure vessels produced through direct blow molding lack sufficient strength, rigidity, and heat resistance at the pinch-off portion, limiting their practical application.
A thermoplastic resin liner with a polyamide composition containing fibrous fillers, such as glass fibers with modified cross-sections, is used, and an outer shell reinforced with a cured product of a fiber composite material, ensuring a pinch-off portion with tensile strength of 100 MPa or more, flexural modulus of 6 GPa or more, and deflection temperature under load of 200°C or more.
The solution results in a pressure vessel with enhanced pressure resistance and cost competitiveness by improving the strength, rigidity, and heat resistance of the pinch-off portion.
Smart Images

Figure 0007581934000003 
Figure 0007581934000004 
Figure 0007581934000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure vessel having excellent pressure resistance, which is formed from a resin liner for a pressure vessel that can be directly blow molded and has excellent strength, rigidity and heat resistance, and an outer shell in which the outer surface of the resin liner is covered with a reinforcing layer made of a cured product of a reinforced fiber composite material. [Background technology]
[0002] Conventionally, it has been used for storing and transporting fuel tanks, natural gas, and hydrogen gas in automobiles. As a pressure vessel (Figure 1) for use in such a vessel, a thermoplastic resin vessel body (liner) is reinforced with an outer shell made of fiber-reinforced resin material, from the viewpoints of light weight and excellent durability (high toughness) under pressure. The main reinforcing fibers used for the outer shell are glass fiber and carbon fiber. Among these, carbon fiber, which has a high specific strength, is used officially as a transport tank or pressure accumulator for natural gas and hydrogen, because it is possible to design a pressure vessel with improved strength and rigidity while reducing its weight.
[0003] A commonly used pressure vessel is, for example, a resin liner (Fig. 2) with a cylindrical body and hemispherical dome parts at both ends of the body, and an outer shell formed on the outside of the liner body. The outer shell is made by winding a fiber-reinforced resin material, in which a long reinforced fiber bundle is impregnated with a matrix resin, around the outside of the liner body using the filament winding method (hereinafter sometimes abbreviated as FW method), and then heating and hardening the material to form a pressure vessel. In particular, pressure vessels intended to be filled with fuel for natural gas vehicles and fuel cell vehicles have been attracting attention in recent years, and as there is a possibility that large-scale market demand will emerge in the future, manufacturers are searching for ways to reduce the cost of pressure vessels.
[0004] Currently, pressure vessel liners are mainly made by injection molding (half-split) + welding processing (laser or heat) as shown in Figure 3. However, there are issues such as an increase in liner quality control items and increased costs due to low productivity, so direct blow molding and rotational molding, which do not require post-processing, have been considered as cost-reduction methods.
[0005] Recently, many manufacturers are considering using the direct blow molding method to create prototype liners. In the direct blow molding method, a portion of a cylindrical hot parison, generally made of thermosetting resin, is sandwiched between a pair of molds, forming a pinch-off portion (Fig. 4) that is striped and extends in the axial direction of the liner. In the pinch-off portion, a portion of the hot parison is constrained by the mold, resulting in a portion that is different in thickness from the other portions, and the pinch-off portion that extends in the axial direction becomes thinner, which can lead to a problem that the strength of the liner body is easily reduced. Therefore, each manufacturer is actively studying ways to solve the pinch-off problem that occurs during direct blow molding.
[0006] For example, a resin liner having a pinch-off shape with improved pressure resistance is known from Patent Document 1 (International Publication WO2018 / 207771). Patent Document 1 discloses a pressure vessel using a resin liner in which the valley shape of the pinch-off portion generated during direct blow molding is made gentler.
[0007] In addition, Patent Document 2 (International Publication WO2013 / 172226) is known as a blow molded product using a resin material with excellent pinch-off adhesion. Patent Document 2 describes a blow molded product using a resin composition in which an olefin resin is blended with an EVOH resin with excellent blow moldability. A blow molded article is disclosed.
[0008] Patent Document 3 (International Publication WO2006 / 112252) is known as a method for producing a pressure-resistant container liner using a liquid crystal polyamide resin with excellent pinch-off adhesion. Patent Document 3 discloses a pressure-resistant container liner that is made of a liquid crystal polyamide resin and is subjected to direct blow molding, in which the parison extrusion speed is set to 0.3 kg / min to 5 kg / min, the parison temperature is set to a temperature range of the melting point + 40°C, and the pinch-off portion has a tensile elongation of 1% or more.
[0009] A blow molded article that suppresses oxidative deterioration of a resin material is known from Patent Document 4 (JP Patent Publication 7-32460 A). Patent Document 4 discloses a blow molded article obtained by sandwiching a parison between dies, pinching off the parison, and then blowing the parison with an inert gas. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. WO2018 / 207771 [Patent Document 2] International Publication No. WO2013 / 172226 [Patent Document 3] International Publication No. WO2006 / 112252 [Patent Document 4] Japanese Patent Application Publication No. 7-32460 Summary of the Invention [Problem to be solved by the invention]
[0011] However, although the inventions described in the above Patent Documents 1 to 4 improve the pinch-off adhesion during direct blow molding, the strength, rigidity, and heat resistance of the pinch-off part are not at a level satisfactory for practical use, and there is no mention of a thermoplastic resin liner in which the pinch-off part of the molded product of the present invention has a tensile strength of 100 MPa or more, a flexural modulus of 6 GPa or more, and a deflection temperature under load of 200°C (load 0.45 MPa) or more.
[0012] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a thermoplastic resin liner which can be directly blow molded and which has excellent strength, rigidity and heat resistance. [Means for solving the problem]
[0013] In order to solve the above problems, the pressure vessel and the method for manufacturing the pressure vessel according to the present invention have any of the following configurations. That is, This pressure vessel comprises a cylindrical straight body portion and dome portions provided at both ends of the straight body portion and narrowing away from the straight body portion, the straight body portion and the dome portions being formed from a liner body made of thermoplastic resin and an outer shell in which the outer surface of the liner body is covered with a reinforcing layer made of a hardened fiber-reinforced composite material, the liner body being manufactured by direct blow molding, and the pinch-off portion formed in the dome portion has a tensile strength of 100 MPa or more, a flexural modulus of 6 GPa or more, and a deflection temperature under load (load 0.45 MPa) of 200°C or more.
[0014] The thermoplastic resin used in the liner body of the present invention is preferably a polyamide resin composition containing 15 to 200 parts by weight of a fibrous filler based on 100 parts by weight of polyamide resin.
[0015] In the present invention, the thickness of the pinch-off portion formed in the dome portion is preferably 1.15 to 1.30 times the thickness of the dome portion.
[0016] The fibrous filler contained in the polyamide resin composition of the present invention is preferably a modified cross section glass fiber having a modification ratio of 1.3 or more and 10 or less.
[0017] The polyamide resin contained in the polyamide resin composition of the present invention is preferably either nylon 11 or nylon 12.
[0018] The inner surface of the liner body of the present invention is measured at a wavelength of 1700 -1 ~1750cm -1It is preferable that the peak intensity ratio (peak intensity of direct blow molded product / peak intensity of resin material before direct blow molding) measured by FT-IR in the range is 0.005 or less. Effect of the Invention
[0022] According to the present invention, by using a direct blow molded thermoplastic resin liner with improved strength, rigidity and heat resistance at the pinch-off portion, it is possible to obtain a pressure vessel with significantly improved pressure resistance and cost competitiveness. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is a schematic diagram showing the component configuration of a pressure vessel. [Diagram 2] FIG. 2 is a schematic diagram showing the shape of a resin liner. [Diagram 3] FIG. 2 is a schematic diagram of an injection molded and welded resin liner. [Figure 4] This is a molded product showing the pinch-off shape of a resin liner processed by direct blow molding. [Diagram 5] FIG. 1 is a schematic diagram showing a direct blow molding device. [Figure 6] 1 is a graph showing the results of FT-IR analysis of the inner surface of a resin liner. [Figure 7] This is a molded product showing the degree of pinch-off dent. [Figure 8] FIG. 2 is a schematic diagram showing the shape of a resin liner directly blow molded in the examples. [Figure 9] FIG. 1 is a schematic diagram of an apparatus for performing a pressure test on a pressure vessel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of the present invention will be described in detail.
[0025] The pressure vessel of the present invention comprises a cylindrical straight body portion and dome portions provided at both ends of the straight body portion and narrowing in shape as they move away from the straight body portion, the straight body portion and the dome portion being formed by a liner body made of a thermoplastic resin and an outer shell in which the outer surface of the liner body is covered with a reinforcing layer made of a hardened fiber-reinforced composite material.
[0026] <Thermoplastic resin> The thermoplastic resin used in the liner body of the present invention is a polyamide resin composition containing a fibrous filler.
[0027] Examples of polyamide resins used in the polyamide resin composition include nylons synthesized using amino acids, lactams, or diamines and dicarboxylic acids as main raw materials.
[0028] Representative examples of such raw materials include amino acids such as 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, and para-aminomethylbenzoic acid, lactams such as ε-caprolactam and ω-laurolactam, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, 2-methylpentamethylenediamine, undecamethylenediamine, dodecamethylenediamine, 2,2,4- / 2,4,4-trimethylhexamethylenediamine, 5-methylnonamethylenediamine, metaxylylenediamine, paraxylylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, and 1-amino-3-amino Examples of the diamines include aliphatic, alicyclic, and aromatic diamines such as methyl-3,5,5-trimethylcyclohexane, bis(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, bis(aminopropyl)piperazine, and aminoethylpiperazine, and aliphatic, alicyclic, and aromatic dicarboxylic acids such as adipic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfoisophthalic acid, hexahydroterephthalic acid, and hexahydroisophthalic acid.
[0029] Preferred examples of polyamide resins that can be used include polycaproamide (nylon 6), polyhexamethylene adipamide (nylon 66), polytetramethylene adipamide (nylon 46), polypentamethylene adipamide (nylon 56), polyhexamethylene sebacamide (nylon 610), polyhexamethylene dodecamide (nylon 612), polyhexamethylene adipamide / polyhexamethylene terephthalamide copolymer (nylon 66 / 6T), polyhexamethylene adipamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6I), polyhexamethylene adipamide / polyhexamethylene terephthalamide / polyhexamethylene isophthalamide copolymer (nylon 66 / 6T / 6I), polyxylylene adipamide (nylon XD6), and mixtures or copolymers thereof. Particularly preferred are nylon 6, nylon 66, nylon 610, nylon 6 / 66 copolymer, nylon 6 / 12 copolymer, and the like.
[0030] Furthermore, as the polyamide resin used in the present invention, aliphatic polyamide (nylon 11, melting point 185°C) obtained by condensation polymerization of 11-aminoundecanoic acid obtained from castor oil, a vegetable oil, or aliphatic polyamide (nylon 12, melting point 175°C) obtained by condensation polymerization of lauryllactam, a monomer synthesized starting from the synthetic chemical butadiene, has the lowest melting point and water absorption rate, and can be more preferably used in terms of excellent blow molding processability and dimensional accuracy.
[0031] Examples of the fibrous filler contained in the polyamide resin composition of the present invention include glass fiber, milled glass fiber, carbon fiber, ceramic fiber, and mineral fiber. Among these, examples of the mineral fiber include potassium titanate whisker, zinc oxide whisker, calcium carbonate whisker, wollastonite whisker, asbestos fiber, and gypsum fiber. Examples of the ceramic fiber include alumina fiber and silicon carbide fiber. In the embodiment of the present invention, the preferred fibrous filler is generally called short fiber, which has a fiber length of 1 to 150 μm and a fiber diameter of 1 to 25 μm before blending. By using such a short fiber filler, the anisotropy of the filler is alleviated, and an isotropic warpage reduction effect can be imparted. The content of the fibrous filler is 15 to 200 parts by weight, more preferably 25 to 200 parts by weight, based on 100 parts by weight of the polyamide resin. If the fibrous filler content is less than 15 parts by weight, it is difficult to obtain the reinforcing effect of the filler, which is undesirable, whereas if it exceeds 200 parts by weight, the melt viscosity increases significantly, which is undesirable because direct blow molding processability is impaired.
[0032] Furthermore, by using an irregular cross-section glass fiber as the fibrous filler used in the present invention, it is possible to achieve both reduced warpage in the direction perpendicular to the flow direction of the molded product and high strength, which is preferable. Here, the cross-sectional shape of the irregular cross-section glass fiber is preferably flat, cocoon-shaped, oval, elliptical, semicircular or arc-shaped, rectangular, or a similar shape, and more preferably a flat cross-sectional shape. In the cross section perpendicular to the length direction of the glass fiber having a flat cross-sectional shape, the ratio (irregularity ratio) of the major axis (the longest linear distance of the cross section) to the minor axis (the longest linear distance perpendicular to the major axis) is preferably 1.3 to 10, more preferably 1.5 to 5. If the irregularity ratio of the fibrous filler is less than 1.3, the strength improvement effect is poor, and the upper limit of the irregularity ratio is 10 from the viewpoint of productivity.
[0033] The polyamide resin composition used in the present invention may contain the following compounds for the purpose of modifying the composition. The PPS resin composition may contain typical additives such as plasticizers, such as polyalkylene oxide oligomer compounds, thioether compounds, ester compounds, and organic phosphorus compounds; crystal nucleating agents, such as organic phosphorus compounds and polyether ether ketone; metal soaps, such as montanic acid waxes, lithium stearate, and aluminum stearate; release agents, such as ethylenediamine-stearic acid-sebacic acid polycondensates and silicone compounds; color inhibitors, such as hypophosphites; phenolic antioxidants, such as (3,9-bis[2-(3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy)-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane); phosphorus antioxidants, such as (bis(2,4-dicumylphenyl)pentaerythritol-diphosphite); water, lubricants, ultraviolet inhibitors, colorants, and foaming agents. Any of the above compounds is not preferred to be added in an amount exceeding 20% by weight of the total composition since this impairs the inherent properties of the PPS resin (A). The amount added should be no more than 10% by weight, and more preferably no more than 1% by weight.
[0034] Furthermore, in order to improve the adhesion between the fibrous filler and the polyamide resin and to suppress warpage deformation when the resin liner absorbs water, the fibrous filler can be surface-treated with an alkoxysilane compound having at least one functional group selected from epoxy groups, amino groups, isocyanate groups, hydroxyl groups, and mercapto groups. Specific examples of such compounds include epoxy group-containing alkoxysilane compounds such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercapto group-containing alkoxysilane compounds such as γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane; ureido group-containing alkoxysilane compounds such as γ-ureidopropyltriethoxysilane, γ-ureidopropyltrimethoxysilane, and γ-(2-ureidoethyl)aminopropyltrimethoxysilane; and γ-isocyanatopropyltriethoxysilane and γ-isocyanatopropyltrimethoxysilane. isocyanate group-containing alkoxysilane compounds such as γ-isocyanatopropyl methyl dimethoxysilane, γ-isocyanatopropyl methyl diethoxysilane, γ-isocyanatopropyl ethyl dimethoxysilane, γ-isocyanatopropyl ethyl diethoxysilane, and γ-isocyanatopropyl trichlorosilane; amino group-containing alkoxysilane compounds such as γ-(2-aminoethyl) aminopropyl methyl dimethoxysilane, γ-(2-aminoethyl) aminopropyl trimethoxysilane, and γ-aminopropyl trimethoxysilane; and hydroxyl group-containing alkoxysilane compounds such as γ-hydroxypropyl trimethoxysilane and γ-hydroxypropyl triethoxysilane.
[0035] <Method of producing polyamide resin composition> The polyamide resin composition used in the present invention is usually obtained by melt kneading. Representative examples of the melt kneader include a single-screw or twin-screw extruder, a Banbury mixer, a kneader, and a mixing roll, which are generally known melt kneaders, and kneaded at a processing temperature of the melting peak temperature of the polyamide resin +5 to 100 ° C. In this case, there is no particular restriction on the order of mixing the raw materials, and any method may be used, such as a method of blending all the raw materials and then melt kneading them by the above method, a method of blending some of the raw materials and then melt kneading them by the above method, and then blending and melt kneading the remaining raw materials, or a method of blending some of the raw materials and then using a side feeder to mix the remaining raw materials during melt kneading by a single-screw or twin-screw extruder. In addition, it is of course possible to add the small amount of additive components before molding after kneading and pelletizing the other components by the above method or the like.
[0036] <Reinforced fiber composite material> The reinforced fiber composite material of the reinforcing layer covering the outer surface of the liner body of the present invention is a cured product obtained by impregnating reinforcing fiber bundles with a thermosetting resin and then heating and curing the resin.
[0037] The thermosetting resin used in the present invention is not particularly limited as long as it is liquid, and examples thereof include epoxy resins, unsaturated polyester resins, phenolic resins, urea resins, melamine resins, etc. In particular, from the viewpoint of high adhesive strength, epoxy resins having precursors such as compounds of phenols, amines, carboxylic acids, and intramolecular unsaturated carbon are preferred.
[0038] Examples of glycidyl ether type epoxy resins that use phenols as precursors include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, epoxy resins with a biphenyl skeleton, phenol novolac type epoxy resins, cresol novolac type epoxy resins, resorcinol type epoxy resins, epoxy resins with a naphthalene skeleton, trisphenylmethane type epoxy resins, phenol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, diphenylfluorene type epoxy resins, and various isomers, alkyl, and halogen-substituted derivatives of each of these. Compounds in which epoxy resins made of phenols are modified with urethane or isocyanate are also included in this type.
[0039] Examples of glycidylamine type epoxy resins using amines as precursors include tetraglycidyldiaminodiphenylmethane, glycidyl compounds of xylylenediamine, triglycidylaminophenol, and positional isomers of glycidylaniline, and alkyl or halogen-substituted products.
[0040] Examples of epoxy resins that have a carboxylic acid as a precursor include glycidyl compounds of phthalic acid, and various isomers of glycidyl compounds of hexahydrophthalic acid and dimer acid.
[0041] Examples of epoxy resins having an intramolecularly unsaturated carbon as a precursor include alicyclic epoxy resins.
[0042] The curing agent used for heat curing the thermosetting resin of the present invention is not particularly limited as long as it cures the thermosetting resin. It may be a curing agent that undergoes an addition reaction such as amine or anhydride, or a curing catalyst that induces addition polymerization such as cationic polymerization or anionic polymerization, and two or more types of curing agents may be used in combination. As the curing agent, a compound having an amino group, an acid anhydride group, or an azide group is preferably suitable. For example, phenolic compounds such as dicyandiamide, alicyclic amines, aliphatic amines, aromatic amines, aminobenzoic acid esters, various acid anhydrides, phenol novolac resins, cresol novolac resins, imidazole derivatives, and t-butylcatechol, as well as Lewis acid complexes such as boron trifluoride complexes and boron trichloride complexes, may be mentioned.
[0043] The type of reinforcing fiber constituting the reinforcing fiber bundle used in the reinforced fiber composite material of the present invention is not particularly limited, and examples thereof include carbon fiber, metal fiber, organic fiber, and inorganic fiber. Two or more types of these may be used.
[0044] Examples of carbon fibers include polyacrylonitrile (PAN)-based carbon fibers made from PAN fibers, pitch-based carbon fibers made from petroleum tar or petroleum pitch, cellulose-based carbon fibers made from viscose rayon or cellulose acetate, vapor-grown carbon fibers made from hydrocarbons, graphitized fibers of these, etc. Among these carbon fibers, PAN-based carbon fibers are preferably used because of their excellent balance between strength and elastic modulus.
[0045] Examples of metal fibers include fibers made of metals such as iron, gold, silver, copper, aluminum, brass, and stainless steel.
[0046] Examples of organic fibers include fibers made of organic materials such as aramid, polybenzoxazole (PBO), polyphenylene sulfide, polyester, polyamide, and polyethylene. Examples of aramid fibers include para-aramid fibers, which are excellent in strength and elastic modulus, and meta-aramid fibers, which are excellent in flame retardancy and long-term heat resistance. Examples of para-aramid fibers include polyparaphenylene terephthalamide fibers and copolyparaphenylene-3,4'-oxydiphenylene terephthalamide fibers, and examples of meta-aramid fibers include polymetaphenylene isophthalamide fibers. As aramid fibers, para-aramid fibers, which have a higher elastic modulus than meta-aramid fibers, are preferably used.
[0047] Examples of inorganic fibers include fibers made of inorganic materials such as glass, basalt, silicon carbide, and silicon nitride. Examples of glass fibers include E-glass fiber (for electrical use), C-glass fiber (for corrosion resistance), S-glass fiber, and T-glass fiber (high strength and high elastic modulus). Basalt fiber is a fiber made from basalt, a mineral, and has very high heat resistance. Basalt generally contains 9 to 25% by weight of FeO or FeO2, which is an iron compound, and 1 to 6% by weight of TiO or TiO2, which is a titanium compound, but it is also possible to increase the amount of these components in a molten state and make the fiber.
[0048] The fiber-reinforced resin substrate in the first and second embodiments of the present invention is often expected to function as a reinforcing material, and therefore it is desirable for it to exhibit high mechanical properties. In order to exhibit high mechanical properties, it is preferable that the reinforcing fibers contain carbon fibers.
[0049] In the fiber-reinforced resin substrate in the first and second embodiments of the present invention, the reinforcing fibers are usually composed of one or more reinforcing fiber bundles each having a large number of single fibers bound together. The total number of filaments (single fibers) of the reinforcing fibers when one or more reinforcing fiber bundles are arranged is preferably 1,000 to 2,000,000.
[0050] From the viewpoint of productivity, the total number of filaments of the reinforcing fibers is more preferably 1,000 to 1,000,000, further preferably 1,000 to 600,000, and particularly preferably 1,000 to 300,000. The upper limit of the total number of filaments of the reinforcing fibers may be set in consideration of the balance between dispersibility and handleability, so long as the productivity, dispersibility, and handleability are maintained favorably.
[0051] The pinch-off portion formed in the dome portion of the liner body of the present invention will be described below.
[0052] During direct blow molding, a portion of a cylindrical hot parison made of thermoplastic resin is sandwiched between a pair of dies, forming a pinch-off portion (Fig. 4) in the dome portion that extends in the axial direction of the liner. At the pinch-off portion, a portion of the parison resin is constrained by the dies, creating a portion that is different in thickness from the other portions, and the pinch-off portion that extends in the axial direction becomes thinner, making it prone to a decrease in strength at the pinch-off portion. Therefore, the thickness of the pinch-off portion must be 1.15 times thicker than the dome portion, and there is a limit to the thickness of the hot parison that can be sandwiched between the dies, with the upper limit being 1.30 times.
[0053] If the pinch-off portion formed on the dome portion of the present invention is not firmly bonded, the pressure resistance of the pressure vessel will be significantly reduced, and therefore the pinch-off portion must have a tensile strength of 100 MPa, a flexural modulus of 6 GPa, and a deflection temperature under load (load 0.45 MPa) of 200° C. When 200 parts by weight of fibrous filler is contained per 100 parts by weight of polyamide resin, the upper limits of the tensile strength, flexural modulus, and deflection temperature under load of 300 MPa, 25 GPa, and 260° C., respectively, of the pinch-off portion.
[0054] <Pressure vessel manufacturing method> The method for manufacturing a pressure vessel of the present invention comprises a cylindrical straight body portion and dome portions provided at both ends of the straight body portion and narrowing away from the straight body portion, the straight body portion and the dome portions being formed of a liner body made of thermoplastic resin and an outer shell having an outer surface of the liner body covered with a reinforcing layer made of a hardened product of a reinforced fiber composite material, the liner body being formed by extruding a thermoplastic resin at an extrusion speed of 0.10 kg / sec to 0.50 kg / sec to form a hot parison, fixing the upper and lower ends of the hot parison with a mold, and molding by direct blow molding under molding conditions of a melting point of the thermoplastic resin +10°C or more, and wrapping a reinforced fiber composite material around the liner body and hardening it to form the outer shell.
[0055] <Method of manufacturing resin liners for pressure vessels> Of these, it is important to use the direct blow molding method (Fig. 5) as a manufacturing method for the liner body constituting the pressure vessel of the present invention. Direct blow molding is a hot parison method in which air is directly blown into the molten extruded hot parison before it cools, and is also called extrusion blow molding. Resin heated and melted by an extruder is extruded from a die head into a tube shape (hot parison), the molten parison is sandwiched between dies, air is blown into the inside, and after cooling, the dies are opened and the molded product is taken out. In the present invention, air is usually blown from the upper side of the die, but it may also be blown from the lower side or lateral side of the die. In the direct blow molding method, a dent called pinch-off (Fig. 4) occurs during the process of sandwiching the hot parison between the dies, so if pressure is applied from inside the molded product, cracks will develop starting from the pinch-off and the molded product will easily break. Therefore, in the present invention, in order to improve the dent at the pinch-off part, it is necessary to control the hot parison extrusion speed to a range of 0.10 kg / sec to 0.5 kg / sec. If the hot parison extrusion speed is below the lower limit of 0.10 kg / sec, the molten residence time in the extruder becomes long, which is undesirable because the resin is thermally deteriorated and its strength is reduced. If the hot parison extrusion speed exceeds the upper limit of 0.50 kg / sec, the hot parison discharge speed is too fast and the resin may be burned due to shear force, which is undesirable. In addition, in the present invention, in order to strengthen the adhesion of the pinch-off part, the hot parison formation temperature needs to be set to the melting point of the thermoplastic resin + 10°C or higher. However, if the hot parison formation temperature is set to be higher than the melting point + 100°C, the resin viscosity decreases due to the progress of thermal decomposition of the resin, and the hot parison draws down and becomes impossible to mold, which is undesirable. In addition, in the present invention, in order to improve the strength by improving the oxidative deterioration of the resin liner, it is preferable to use an inert gas (such as nitrogen, helium, or argon) with an oxygen concentration of 10% or less in the hot parison blowing process during direct blow molding. If air is used in the hot parison blowing process, the resin liner may be oxidatively deteriorated and become brittle, which is undesirable.
[0056] <Manufacturing method of outer shell> The present invention relates to a method for manufacturing a pressure vessel comprising a cylindrical body portion and dome portions provided at both ends of the body portion and tapering away from the body portion, the body portion and the dome portions being formed from a liner body made of thermoplastic resin and an outer shell having an outer surface covered with a reinforcing layer made of a cured fiber-reinforced composite material. The method for forming the outer shell having an outer surface covered with a reinforcing layer made of a cured fiber-reinforced composite material (called a filament winding method) is described below.
[0057] This manufacturing method includes the steps of (a) preparing a molded intermediate formed of a reinforcing layer composed of a plurality of reinforcing fiber composites by winding a reinforcing fiber composite impregnated with a liquid thermosetting resin composition around a liner, (b) holding the molded intermediate at room temperature and allowing the thermosetting resin composition impregnated in the reinforcing fiber composite to flow, and (c) heating the molded intermediate after step (b) to obtain a cured product of the reinforcing fiber composite impregnated with the thermosetting resin. In the present invention, room temperature refers to a temperature in the range of 5°C to 35°C.
[0058] In the step (a) of preparing a molded intermediate, a reinforced fiber composite is drawn out, impregnated with a thermosetting resin composition, and then wound around a liner. The liner can be freely selected depending on the application of the filament winding molded product. For example, in the manufacture of a hollow pipe member, a cylindrical liner that can be de-cored after the molded product is cured, or a liner of various shapes that can be de-cored by melting it by heating or the like can be used. In the manufacture of a pressure vessel, a metal or resin liner that ensures sealing properties for a predetermined content can be used. As a method of winding a reinforced fiber composite impregnated with a thermosetting resin composition around a liner, from the viewpoint of moldability and mechanical properties of the molded product, it is preferable to supply the reinforced fiber composite from a head that can be freely moved relative to the liner, and arrange the reinforced fiber composite so as to satisfy the required performance of the filament winding molded product.
[0059] In the step (b) of holding the intermediate molded article at room temperature, the intermediate molded article is held at room temperature, so that the thermosetting resin composition impregnated into the reinforced fiber composite is kept in a state of fluidity in at least a part of the step. In a state in which the thermosetting resin composition is capable of flowing, the air bubbles that have entered the reinforcing layer of the reinforced fiber composite obtained in the step (a) are exposed to the surface layer of the reinforcing layer of the reinforced fiber composite due to the buoyancy acting on the air bubbles and the tightening of the winding caused by the tension remaining in the fiber when the fiber is wound around the winding core. Therefore, by holding the intermediate molded article at room temperature, at least a part of the air bubbles in the reinforcing layer of the reinforced fiber composite can be removed, and the voids remaining in the filament winding molded article can be reduced. The intermediate molded article can be held while rotating the liner of the intermediate molded article as the center of rotation. This prevents the thermosetting resin composition having fluidity from dripping and falling off due to gravity. The falling off of the thermosetting resin composition increases the fiber volume content (Vf:%) of the filament winding molded product, which may deteriorate the product performance. In addition, the fallen thermosetting resin composition is often discarded, which reduces the product yield. By rotating the intermediate molded product while it is being held, the effects of the falling off of the thermosetting resin composition can be eliminated.
[0060] In the holding of the intermediate molded article, the holding temperature is room temperature, but preferably within the range of room temperature, and can be any temperature ±5°C determined according to the type of thermosetting resin composition and the conditions of use. When this range of any temperature ±5°C exceeds the range of room temperature, the excess is to be rounded down. Depending on the type and conditions of use of the thermosetting resin composition, if the temperature is high, the gelation of the thermosetting resin composition may proceed quickly, and sufficient resin flow time may not be ensured. In addition, if the temperature is low, the viscosity of the thermosetting resin composition may decrease, and it may take a long time to achieve the same degree of void reduction effect compared to when the temperature is high. Therefore, the holding temperature is not particularly limited as long as it is room temperature, but it is preferable that it is in a range determined according to the type of thermosetting resin composition used and the conditions of use.
[0061] In the step (c) of obtaining a cured product of the reinforced fiber composite material impregnated with the thermosetting resin, the molded intermediate body after being kept at room temperature is heated to thermally cure the thermosetting resin composition, but the method is not limited, and heating can be performed using any method such as a heater or an induction heating coil. During heating, the molded intermediate body can be rotated and held. By rotating and holding the molded intermediate body, it is possible to prevent the thermosetting resin composition from falling off.
[0062] The location of the step (a) of preparing a molded intermediate, the step (b) of holding the molded intermediate at room temperature, and the step (c) of obtaining a cured product of a reinforced fiber composite material impregnated with a thermosetting resin is not limited. That is, the molded intermediate may be moved between steps (a) and (b), or the steps may be performed continuously without moving. The molded intermediate may be moved between steps (b) and (c), or the steps may be performed continuously without moving. Furthermore, when the molded intermediate is moved between steps (b) and (c), the location of the movement may be the location where step (a) was performed.
[0063] The filament winding molded product obtained by the present invention can be widely used for aerospace applications, leisure applications, and general industrial applications, including pressure vessels, rolls, propeller shafts, flywheels, fishing rods, and golf club shafts. In particular, it can be suitably used for pressure vessels and the like that require strength. The pressure vessels produced by the present invention are not limited to hydrogen gas vehicles and natural gas vehicles, but are also suitably used for ships and aircraft, stationary types that are fixed to the ground and used, and air respirators used by hospitals and firefighters. The substances stored in the pressure vessels may be gases such as nitrogen, oxygen, argon, liquefied petroleum gas, and hydrogen, or liquefied versions of the above substances.
[0064] <Analysis method for oxidation deterioration of resin liners> The resin liner of the present invention has a peak intensity of 1700 cm in FT-IR measurement in order to improve the strength and toughness during pinch-off adhesion. -1 ~1750cm -1The peak intensity ratio due to material oxidation deterioration in the range (peak intensity of the direct blow molded product / peak intensity of the resin material before direct blow molding) must be 0.005 or less, and more preferably 0.002 or less. Specifically, the FT-IR measurement method of the present invention involves cutting out about 1 g of the surface of the molded product in three places, and measuring the surface area using an FT-IR device (TENSOR II manufactured by Bruker) using the ATR method (attenuated total reflection method: detector DLaTGS, incident angle 45°, Ge prism, resolution 4 cm). -1 ) was measured. The 1700 cm -1 ~1750cm -1 The degree of oxidative degradation was quantitatively evaluated based on the magnitude of the absorption peak intensity in the wavelength range of 1700 cm. -1 ~1750cm -1 It can be seen that there is a difference in the absorption peak intensity in the wavelength range, and that the absorption peak is hardly observed under blow molding conditions that suppress oxidative degradation.
[0065] <Tensile test at pinch-off part of resin liner> The pinch-off portion of the dome of the direct blow molded resin liner (thickness 3 mm) was cut into a strip of width 15 mm x length 125 mm, and a tensile test (n=5 for each) was performed in accordance with ASTM D3039 to measure the tensile strength.
[0066] <Bending test at pinch-off part of resin liner> The pinch-off portion of the dome of the direct blow molded resin liner (thickness 3 mm) was cut into a strip of width 15 mm x length 125 mm, and a bending test (n=3 for each) was performed in accordance with ASTM D790 to measure the bending modulus. <Measurement of deflection temperature under load at pinch-off part of resin liner> The pinch-off portion of the dome of the direct blow molded resin liner (thickness 3 mm) was cut into a strip of width 15 mm x length 125 mm, and the deflection temperature under load was measured in accordance with ASTM D648 (load 0.45 MPa, n=3 for each). EXAMPLES
[0067] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the descriptions of these examples. Physical properties in each example and comparative example were evaluated according to the following methods.
[0068] [Manufacturing method of resin liner] Using a Tahara accumulator-type extrusion blow molding device, the resin liner shape shown in FIG. 8 (wall thickness: 3 mm±0.5 mm, threaded portion: inner diameter φ13 mm, outer diameter φ24 mm) was obtained under the blow molding conditions of each Example and Comparative Example. <Extrusion blow molding equipment / equipment specifications> Extruder screw diameter: φ80mm Extruder screw arrangement: Deep groove full flight specification Accumulator pump capacity: 4000cc Extruder screw speed: 35 rpm Die shape: Die purge <Molding conditions> Hot parison length: 70mm Hot parison weight: 2000g Hot parison blowing gas: Air or inert gas (nitrogen gas used)
[0069] [Method for measuring hot parison extrusion speed] Under the blow molding conditions of each Example and Comparative Example, the time taken to complete extrusion of the hot parison to a length of 70 mm (parison weight 2000 g) was measured with a stopwatch (N=3), and the extrusion speed (kg / sec) was calculated.
[0070] [Method for measuring hot parison forming temperature] The surface temperature of the parison (length 70 mm) extruded under the blow molding conditions of each Example and Comparative Example was measured by infrared thermography (non-contact type) at two points, the parison extrusion side and the side opposite to the parison extrusion direction (hereinafter referred to as the anti-extrusion side).
[0071] [FT-IR measurement of resin liner (degree of oxidative deterioration of resin material)] Approximately 1 g of the inner surface of the resin liner obtained above was scraped off in three places, and the inner surface was measured by the ATR method using an FT-IR device (TENSOR II manufactured by Bruker). -1 ~1750cm -1 The degree of oxidative degradation was quantitatively evaluated based on the ratio of the absorption peak intensity in the wavelength range (peak intensity of the resin liner molded product / peak intensity of the resin raw material before blow molding). The smaller this value, the less oxidative degradation there was in the resin liner. <Measurement conditions> Light source: Globar (SiC) Detector: DLaTGS ·Resolution: 4cm -1 Number of times: 128 - Attachment: Thunderdome, single reflection ATR, incident angle 45°, Ge prism used
[0072] [Resin liner / pinch-off section tensile test (pinch-off adhesion)] The pinch-off portion of the dome part of the resin liner obtained above was cut into a strip shape of 15 mm wide x 125 mm long from two points on the parison extrusion direction side and the parison counter-extrusion direction side, and a tensile test (n=5 each) was carried out according to ASTM D3039 to measure the tensile strength. The larger this value, the better the pinch-off adhesion of the resin liner.
[0073] [Bending test of resin liner / pinch-off part (rigidity of pinch-off part)] The pinch-off part of the dome part of the direct blow molded resin liner (3mm thickness) was cut into a strip of width 15mm x length 125mm, and a bending test (n=3 for each) was carried out in accordance with ASTM D790 to measure the bending modulus. The larger this value, the better the rigidity of the pinch-off part of the resin liner.
[0074] [Measurement of deflection temperature under load of resin liner / pinch-off part (heat resistance of pinch-off part)] The pinch-off part of the dome part of the direct blow molded resin liner (3mm thickness) was cut into a strip of width 15mm x length 125mm, and the deflection temperature under load was measured (load 0.45MPa, n=3 for each) in accordance with ASTM D648. The higher this value, the less likely the pinch-off part of the resin liner is to be thermally deformed.
[0075] [Pressure vessel manufacturing method using filament winding method and pressure resistance test (pressure resistance)] The liner obtained above was placed in a filament winding molding machine, and a resin containing a liquid thermosetting resin composition (epoxy base:curing agent=100:32 mass ratio, uniformly mixed at room temperature of 25°C) was impregnated into a single bundle of carbon fiber "TORAYCA" (registered trademark) T700SC-24K manufactured by Toray Industries, Inc., and fed to the core. The fiber was wound over a 60 mm wide range at a winding angle of ±83° with respect to the axial direction of the core, and laminated to a thickness of 1 mm to prepare a molded intermediate. After winding the fiber, the intermediate was rotated at a speed of 7 rpm and held in a 20°C environment for 15 minutes. At the start of the holding, the viscosity of the resin was 1100 mPa·s.
[0076] After the above-mentioned holding, the intermediate molded article was heated at a temperature of 80°C for 2 hours and at a temperature of 110°C for 4 hours to harden the resin and obtain a pressure vessel for pressure resistance test. Next, the pressure vessel obtained above was placed in a pressure vessel water pressure burst test device shown in Figure 9, water was pumped and pressurized by a water pressure pump, and the burst pressure when the vessel burst was measured (N=3), and the pressure resistance performance was evaluated according to the following criteria. <Pressure resistance performance / criteria> ○: Burst pressure 100MPa or more △: Burst pressure 80MPa or less ×: Burst pressure 50MPa or less
[0077] [Raw materials] In the examples and comparative examples, the following raw materials were used.
[0078] <Reference Example 1> Thermoplastic resin used for direct blow molding Glass fiber reinforced nylon 6 resin-1: CM1046K4 (manufactured by Toray Industries, Inc., 20% glass fiber content, blow molding grade, glass fiber irregularity ratio 1.0, Amilan (registered trademark)) Glass fiber reinforced nylon 6 resin-2: Only the glass fiber containing CM1046K4 was changed to a modified cross-section glass fiber (CSG-3PA-830 manufactured by Nittobo Co., Ltd., modification ratio 4.0). Nylon 6 resin: CM1056 (Toray Industries, Inc., high viscosity, high impact blow molding grade, does not contain fibrous filler, Amilan (registered trademark))
[0079] Reference Example 2 Liquid thermosetting resin composition Epoxy base: Bisphenol A type liquid epoxy resin ("jER" (registered trademark) 828 (manufactured by Mitsubishi Chemical Corporation)) Hardener: mixture of poly(propylene glycol) diamine, isophorone diamine, cyclohexylamine, and polypropylene glycol ("ARADUR" (registered trademark) 3486 (manufactured by Huntsman Japan Co., Ltd.))
[0080] [Table 1]
[0081] [Table 2]
[0082] As described above, by comparing the Examples and Comparative Examples, it is apparent that the resin liner and pressure vessel of the present invention As shown in Figure 7, the pinch-off dent is improved and the pinch-off part is firmly bonded, forming a pinch-off part that exhibits high strength, high rigidity and high heat resistance, thereby achieving a dramatic improvement in pressure resistance. [Explanation of symbols]
[0083] 101 Pressure vessels 102 Reinforced fiber composites 103 Liner container 104 Base part 201 Cylindrical straight body 202 Hemispherical dome sections on both ends of the straight body 301 Injection molded liner (half part) 302 Injection molded liner (halved parts welded together) 401 Direct blow molded liner 402 Pinch-off occurred at the dent 501 Single Screw Extruder 502 Direct Blow Molding Mold 503 Hot Parison 701 Direct blow molded liner with large pinch-off dent 702 Direct blow molded liner with small pinch-off dents
Claims
1. A pressure vessel comprising a cylindrical straight body portion and dome portions provided at both ends of the straight body portion and tapering away from the straight body portion, the straight body portion and the dome portions being formed from a liner body made of thermoplastic resin and an outer shell in which the outer surface of the liner body is covered with a reinforcing layer made of a hardened fiber-reinforced composite material, the liner body being manufactured by direct blow molding, and the pinch-off portion formed in the dome portion has a tensile strength of 100 MPa or more, a flexural modulus of 6 GPa or more, and a deflection temperature under load (load 0.45 MPa) of 200°C or more.
2. 2. The pressure vessel according to claim 1, wherein the thermoplastic resin used for the liner body is a polyamide resin composition containing 15 to 200 parts by weight of a fibrous filler per 100 parts by weight of polyamide resin.
3. 3. The pressure vessel according to claim 1, wherein the thickness of the pinch-off portion formed in the dome portion is 1.15 to 1.30 times the thickness of the dome portion.
4. 3. The pressure vessel according to claim 2, wherein the fibrous filler contained in the polyamide resin composition is a modified cross-section glass fiber having a modification ratio of 1.3 or more and 10 or less.
5. 5. The pressure vessel according to claim 2, wherein the polyamide resin contained in the polyamide resin composition is either nylon 11 or nylon 12.
6. The inner surface of the liner body is measured at a wavelength of 1700 -1 ~1750cm -1 The pressure vessel according to any one of claims 1 to 5, characterized in that the peak intensity ratio (peak intensity of the direct blow molded product / peak intensity of the resin material before direct blow molding) measured by FT-IR in the range is 0.005 or less.
Citation Information
Patent Citations
Manufacture of blow-molded item
JP1995032460A
Production of nylon resin composition for blow molding
JP1996311332A
Manufacture of hollow molded body
JP1999010718A
Method of manufacturing for pressure-resistant container
JP2001150523A
Device and method for extrusion of molten resin, and device and method for molding of molten resin
JP2016203450A