Rare earth sintered magnet and its manufacturing method

The method addresses the challenge of achieving high coercive force and low impurity/carbon concentration in rare earth sintered magnets by using hydrogen-containing powder pulverization and controlled heat treatment, resulting in magnets with improved magnetic properties for applications like electric vehicles.

JP7582058B2Active Publication Date: 2024-11-13SHIN ETSU CHEMICAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021080141
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-19
Filing Date
2021-05-11
Publication Date
2024-11-13
Estimated Expiration
2041-05-11

AI Technical Summary

Technical Problem

Existing methods for producing rare earth sintered magnets face challenges in achieving high coercive force (HcJ) while maintaining low impurity and carbon concentrations, particularly due to increased impurity levels and carbon concentration gradients, which affect magnetic properties and industrial productivity.

Method used

A manufacturing method involving hydrogen-containing powder pulverization, followed by vacuum sintering with controlled heat treatment conditions, including atmospheric and vacuum steps, to minimize carbon concentration differences and impurities, and a grain boundary diffusion process to enhance coercive force.

Benefits of technology

The method produces rare earth sintered magnets with low impurity and narrow carbon concentration distributions, resulting in improved magnetic properties and enhanced coercive force suitable for applications requiring high heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582058000001
    Figure 0007582058000001
  • Figure 0007582058000002
    Figure 0007582058000002
  • Figure 0007582058000003
    Figure 0007582058000003
Patent Text Reader

Abstract

To provide a rare earth sintered magnet which is low in impurity density and has less carbon density difference in the magnet, and a manufacturing method for the same.SOLUTION: A manufacturing method for a rare earth sintered magnet has: a melting step for obtaining material alloy; a pulverization step for preparing alloy fine powders; a molding step for obtaining a mold of the alloy fine powders; and a sintering step for sintering the mold. The pulverization step includes a coarse pulverization step and a fine pulverization step that include hydrogen storage processing, and includes a lubricant addition step before or after the coarse pulverization step. The sintering step includes an atmosphere heat treatment step and a vacuum heat treatment step. At the atmosphere heat treatment step, temperature is raised to decomposition temperature of lubricant or higher and to sintering temperature or lower to be held for a prescribed time, and temperature raising and the prescribed temperature holding are performed in 10 kPa to 100 kPa inert gas atmosphere.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rare earth sintered magnet having a low impurity concentration and a narrow carbon concentration distribution within the magnet, and a method for producing the same. [Background technology]

[0002] Rare earth sintered magnets are essential functional materials for energy saving and high performance, and their range of applications and production volume are expanding year by year. Among rare earth sintered magnets, Nd-based sintered magnets (hereinafter referred to as "Nd magnets") in particular have high residual magnetic flux density (hereinafter referred to as "B r "), and are used, for example, in drive motors for hybrid and electric vehicles, motors for electric power steering, motors for air conditioner compressors, voice coil motors (VCM) for hard disk drives, etc. r However, in order to further miniaturize the motor, Nd magnets have a higher B r What is required is...

[0003] On the other hand, at high temperatures, the coercive force (H cJ This causes irreversible thermal demagnetization. For this reason, rare earth sintered magnets used in automobiles, particularly in electric vehicle motors, have a high H cJ It is required that the applicant have:

[0004] Conventionally, Nd magnet H cJ In order to increase the B content, it is common to add heavy rare earth elements such as Dy and Tb. r This is not necessarily a preferable method because it leads to a decrease in the yield of the alloy and because these heavy rare earth elements are scarce and expensive resources.

[0005] In addition, the H of Nd magnets cJAnother method for increasing H is known to be grain refinement. This method mainly involves reducing the particle size of the powder during pulverization before compaction, thereby reducing the size of the grains after sintering. Within a certain particle size range, the H increases linearly with the refinement. cJ However, when the powder is refined beyond a certain level, the impurity concentration (mainly oxygen and nitrogen) of the powder increases due to a decrease in the grinding ability during fine grinding and an increase in the reactivity of the powder. cJ decreases or H cJ Even if an increase in H is observed, it is possible to cJ In order to improve these problems, a method of changing the grinding gas during fine grinding to a noble gas such as He or Ar (Patent Document 1) and a method of using hydrogen-containing powder during fine grinding (Patent Documents 2 and 3) have been proposed.

[0006] Other Nd magnets H cJ One known method for increasing the magnet strength is the grain boundary diffusion method, which selectively accumulates heavy rare earth elements (Dy, Tb, etc.) in the grain boundary phase of a Nd magnet (Patent Documents 4 and 5). In this method, compounds of heavy rare earth elements such as Dy and Tb are attached to the magnet surface by a method such as coating, and then a heat treatment is performed at high temperature to form a structure with high concentrations of Dy and Tb only in the areas very close to the grain boundaries of the main phase particles in the Nd magnet, thereby increasing the magnet strength. r High H cJ It is possible to obtain an increase effect. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 2014 / 142137 [Patent Document 2] International Publication No. 2013 / 100008 [Patent Document 3] International Publication No. 2014 / 123079 [Patent Document 4] International Publication No. 2006 / 044348 [Patent Document 5] International Publication No. 2013 / 100010 Summary of the Invention [Problem to be solved by the invention]

[0008] However, the method proposed in Patent Document 1 above of changing the grinding gas to a noble gas such as He or Ar during fine grinding is difficult to implement on an industrial scale, considering the price difference with nitrogen gas. In addition, the grain boundary diffusion method described in Patent Documents 4 and 5 is very useful for increasing the coercive force, but the B r In order to improve the magnetization, if the amount of added elements or R in the magnet is reduced, or if the amount of impurity elements (carbon, oxygen, nitrogen) is increased by increasing the amount of lubricant to improve the orientation, H cJ The effect of increasing the H concentration by the grain boundary diffusion method is significantly reduced. cJ Since there is a limit to the amount of increase, for applications that require high heat resistance, such as electric vehicles, the H of the magnet material itself before the grain boundary diffusion method is used. cJ It is necessary to increase the coercive force.

[0009] In the methods described in Patent Documents 2 and 3, hydrogen-containing powder is pulverized in an oxygen-free atmosphere to suppress oxidation, and the added lubricant is decomposed by the desorbed hydrogen during sintering to reduce the carbon concentration. This method is effective in reducing the impurity concentration in the magnet, especially the carbon concentration, but on the other hand, the organic lubricant evaporates during sintering, generating hydrocarbon gas in the heat treatment furnace, which causes a gas attack that increases the carbon concentration from the magnet surface to a depth of up to several mm compared to the inside of the magnet. Generally, carbon is an impurity element that adversely affects magnetic properties, especially coercivity, so when the above method is used, it is necessary to grind the surface area extensively, which has a significant adverse effect on industrial productivity.

[0010] The present invention has been made in consideration of the above circumstances, and has an object to provide a rare earth sintered magnet having a low impurity concentration and small carbon concentration difference within the magnet, and a method for producing the same. [Means for solving the problem]

[0011] In order to achieve the above-mentioned object, the inventors have conducted extensive research focusing on the sintering heat treatment conditions. As a result, they have discovered that in a method using hydrogen-containing powder during fine pulverization, by holding the material in an inert gas atmosphere under an appropriate pressure range and within an appropriate temperature range below the sintering temperature for a certain period of time before performing vacuum sintering at the sintering temperature, the difference in carbon concentration between the surface and center of the magnet can be suppressed, and that a sintered magnet having a difference between the carbon concentration at the surface and the carbon concentration at the center of the magnet with 0.005 to 0.03 mass %, for example, can be obtained. This discovery has led to the completion of the present invention.

[0012] Therefore, the present invention provides the following method for producing a rare earth sintered magnet and the following rare earth sintered magnet. 1. A method for producing a raw alloy having a predetermined composition by melting the raw material, a crushing process for crushing the raw alloy to prepare an alloy fine powder, a compacting process for compacting the alloy fine powder under application of a magnetic field to obtain a compact, and a sintering process for heat treating the compact to obtain a sintered body, comprising the steps of R (R is one or more elements selected from rare earth elements, and Nd is a must), T (T is one or more elements selected from iron group elements, and Fe is a must), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M 2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta, The pulverization step includes a coarse pulverization step and a fine pulverization step, The coarse grinding step further includes a grinding step by hydrogen absorption, Without dehydrogenation treatment, The hydrogen-containing coarse powder is then used in the milling step, The pulverization step includes a lubricant addition step of adding a lubricant before or after the coarse pulverization step, The sintering step includes an atmospheric heat treatment step of heating the molded body to a predetermined temperature that is equal to or higher than the decomposition temperature of the lubricant and equal to or lower than the sintering temperature of the sintered body, and maintaining the predetermined temperature for a predetermined time, and performing this heating and maintaining the predetermined temperature in an inert gas atmosphere of 10 kPa to 100 kPa to heat the molded body, and a vacuum heat treatment step of switching to a vacuum atmosphere after the atmospheric heat treatment step and heating the molded body to the sintering temperature of the sintered body. 2. The method for producing a rare earth sintered magnet according to claim 1, wherein the lubricant is at least one selected from the group consisting of stearic acid, zinc stearate, decanoic acid and lauric acid. 3. The method for producing a rare earth sintered magnet according to claim 1 or 2, wherein the inert gas forming the inert gas atmosphere in the atmospheric heat treatment step is He gas, Ar gas or N2 gas. 4. The method for producing a rare earth sintered magnet according to any one of claims 1 to 3, wherein the predetermined temperature which is equal to or higher than the decomposition temperature of the lubricant and equal to or lower than the sintering temperature of the sintered body is 400°C to 800°C. 5. The method for producing a rare earth sintered magnet according to any one of claims 1 to 4, wherein the predetermined temperature is maintained for a time period of 0.5 to 10 hours in the atmospheric heat treatment step. 6. In the hydrogen absorption pulverization step, the hydrogen pressure is 100 kPa or more, and in the fine pulverization step, the coarsely pulverized raw alloy is pulverized in a non-oxidizing gas atmosphere having a moisture content of 100 ppm or less to a volume-based median diameter D 50 6. The method for producing a rare earth sintered magnet according to claim 1, wherein the mixture is finely pulverized to a size of 0.2 μm to 10 μm. 7. The method for producing a rare earth sintered magnet according to any one of claims 1 to 6, wherein in the atmospheric heat treatment step, while maintaining the inert gas atmosphere pressure at 10 kPa to 100 kPa, evacuation at a rate of 0.1 to 1000 kPa / min and subsequent introduction of the inert gas at a rate of 1 to 100 kPa / min are carried out multiple times. 8. In the atmospheric heat treatment step, the inert gas atmosphere pressure is set within the pressure range of 10 kPa to 100 kPa at a predetermined pressure P k 0.5P k Super ~1.5P k The manufacturing methods of rare earth sintered magnets vary in less than 7 ranges. 9. The carbon content is 0.05 mass% or less, and the surface carbon concentration C of the sintered magnet is s and central carbon concentration C c The difference ΔC between these values ​​is 0.005% by mass to 0.03% by mass. 10. Carbon concentration at the center of sintered magnets, C c 10. The rare earth sintered magnet according to claim 9, wherein the content is 0.057 mass % or less. 11. R (R is one or more elements selected from rare earth elements, and Nd is a must), T (T is one or more elements selected from iron group elements, and Fe is a must), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M 2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta.) and further comprising an oxygen content of 0.1 mass% or less and a nitrogen content of 0.05 mass% or less. is less than or equal to 9 or 10 Rare earth sintered magnet. 12. R content is 12.0 atomic % to 16.0 atomic % (R is one or more elements selected from rare earth elements, and Nd is essential), M 1 The content is 0.1 atomic % to 2.0 atomic % (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi. 2 The content is 0.1 atomic % to 0.5 atomic % (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf and Ta. 13. A rare earth sintered magnet according to any one of 9 to 12, having an average crystal grain size of 4 μm or less. 14. Regarding the degree of orientation in sintered magnets, r [%] and the average crystal grain size is D [μm], the following relationship (1) 0.26×D+97≦O r ≦0.26×D+99 (1) A rare earth sintered magnet that satisfies any of the above criteria 9 to 13. 15. Within 500 μm from the surface of the sintered magnet, at least a portion of the surface vicinity of a main phase particle has a region having a higher concentration of R' (R' is one or more elements selected from rare earth elements and constitutes at least a portion of the above-mentioned R) than the center portion of the main phase particle. 11 or 12 Rare earth sintered magnet. Effect of the Invention

[0013] According to the present invention, it is possible to produce a rare earth sintered magnet having a low impurity concentration and a narrow carbon concentration distribution, and to provide a rare earth sintered magnet with excellent magnetic properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The method for producing a rare earth sintered magnet of the present invention includes a melting step of melting a raw material to obtain a raw material alloy having a predetermined composition, a crushing step of crushing the raw material alloy to prepare an alloy fine powder, a molding step of compacting the alloy fine powder under an applied magnetic field to obtain a green body, and a sintering step of heat-treating the green body to obtain a sintered body.

[0015] First, in the melting step, the metal or alloy that is the raw material for each element is weighed out to obtain a desired composition. After weighing out the raw materials to obtain the desired composition, the raw materials are melted, for example, by high-frequency melting, and cooled to produce a raw alloy. The raw alloy is generally cast by a melting casting method in which the alloy is poured into a flat mold or a book mold, or a strip casting method. In addition, the main phase R2Fe 14The present invention can also be applied to the so-called two-alloy method, in which an alloy close to the B compound composition and an R-rich alloy that becomes a liquid phase auxiliary at the sintering temperature are separately prepared, and then weighed and mixed after coarse grinding. However, since the α-Fe phase is easily crystallized in the alloy close to the main phase composition depending on the cooling rate and alloy composition during casting, it is preferable to perform a homogenization treatment for 1 hour or more at 700 to 1200 ° C in a vacuum or Ar atmosphere as necessary for the purpose of homogenizing the structure and eliminating the α-Fe phase. Note that when an alloy close to the main phase composition is prepared by the strip casting method, homogenization can be omitted. In addition to the above casting method, the so-called liquid quenching method can also be applied to the R-rich alloy that becomes a liquid phase auxiliary.

[0016] The rare earth sintered magnet produced by the present invention is composed of R (R is one or more elements selected from rare earth elements, and Nd is essential), T (T is one or more elements selected from iron group elements, and Fe is essential), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M 2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta.) The metals or alloys used as the raw materials are selected according to the composition of the magnet. Details of the composition of the magnet to be manufactured will be described later.

[0017] The above-mentioned pulverization step is a multi-stage process including at least a coarse pulverization step and a fine pulverization step. In the coarse pulverization step, for example, a jaw crusher, a Braun mill, a pin mill, or hydrogen pulverization can be used as an appropriate method. In the present invention, from the viewpoint of reducing the amount of O, N, and C and obtaining excellent magnetic properties, at least one step of the coarse pulverization step is a hydrogen pulverization step in which the alloy is occluded by exposing the alloy ingot to a hydrogen atmosphere of a certain pressure or more. The hydrogen pressure at this time is not particularly limited, but from the viewpoint of reducing the adverse effect on productivity due to the time required for hydrogen occlusion, it is preferable that it is 100 kPa or more. After carrying out the hydrogen occlusion pulverization step, the alloy ingot with an increased temperature is cooled and transported to the next step. At this time, it is preferable to cool it to around room temperature from the viewpoint of preventing oxidation. By such a hydrogen pulverization step, it is possible to obtain a coarse powder that is usually pulverized to 0.05 mm to 3 mm, particularly 0.05 mm to 1.5 mm.

[0018] In the fine pulverization step, the coarse powder obtained in the coarse pulverization step can be pulverized using a jet mill with a non-oxidizing gas stream such as N2, He, or Ar. In the present invention, in the fine pulverization step, the coarse powder is preferably pulverized to a volume-based median diameter D 50 The magnet is then finely pulverized to 0.2 μm to 10 μm, more preferably 0.5 μm to 5 μm, by a jet mill. Since the O and N in the rare earth sintered magnet are mainly mixed in during the fine pulverization process, it is necessary to control the jet mill atmosphere in order to adjust the O and N contents in the rare earth sintered magnet. For example, the O content in the rare earth sintered magnet is adjusted by controlling the O amount and dew point in the jet mill atmosphere, and it is preferable that the moisture content in the atmosphere during pulverization is 100 ppm or less, and the oxygen concentration is 1 ppm or less. Note that the above volume-based median diameter D 50 is the particle size when the cumulative volume frequency is 50%.

[0019] The N content in the rare earth sintered magnet can be adjusted, for example, by (A) pulverizing the magnet in a jet mill using a He or Ar gas stream, (B) pulverizing the magnet by introducing hydrogen into a jet mill using a N2 gas stream, or (C) pulverizing the magnet using a hydrogen-containing coarse powder using a jet mill using a N2 gas stream. In this case, in the case of (B) or (C), by introducing hydrogen gas or using a hydrogen-containing coarse powder, hydrogen is preferentially adsorbed onto the active surface generated by pulverization, inhibiting the adsorption of nitrogen, thereby making it possible to reduce the amount of N in the rare earth sintered magnet.

[0020] Here, the pulverization step includes a lubricant addition step in which a lubricant is appropriately added before or after the coarse pulverization step in order to improve the orientation of the powder in the next step of compacting in a magnetic field. Examples of the lubricant include saturated fatty acids such as stearic acid (decomposition temperature 376°C), decanoic acid (decomposition temperature 270°C), and lauric acid (decomposition temperature 225°C), and saturated fatty acid salts such as zinc stearate (decomposition temperature 376°C). In the lubricant addition step, while increasing the amount of lubricant added is usually effective in improving the orientation, the C derived from the lubricant forms many R-CON phases in the rare earth sintered magnet, which increases the H cJ A dilemma occurs in that the orientation of the magnet is significantly decreased. In this case, in the present invention, fine powder obtained by pulverizing coarse powder containing hydrogen is used, so that the amount of lubricant can be increased for the fine powder when improving the orientation. That is, in the rare earth sintered magnet made from such fine powder, when hydrogen contained inside is released during heat treatment, the lubricant chemically adsorbed on the surface of the fine powder by the hydrogen is decomposed by a carbonyl reduction reaction or the like, and further decomposed and dissociated into a highly volatile lower alcohol by a cracking reaction with hydrogen gas, which is considered to reduce the C content remaining in the rare earth sintered magnet. The amount of the lubricant added is appropriately set according to the type of lubricant, and is not particularly limited, but is preferably 0.01 to 0.5 parts by mass, particularly 0.05 to 0.3 parts by mass, per 100 parts by mass of the coarsely pulverized powder or the raw alloy.

[0021] In the compacting step, for example, a magnetic field of 400 to 1600 kA / m is applied to the alloy powder to orient it in the direction of the easy magnetization axis, and the powder is compacted in a compression molding machine. 3 That is, from the viewpoint of securing the strength of the molded body and obtaining good handling properties, the molded body density is preferably 2.8 g / cm. 3 It is preferable that the B is more than 100%. In addition, a binder such as PVA or fatty acid can be added to increase the strength of the molded body after molding. On the other hand, it is possible to obtain a suitable B by suppressing the disturbance of the particle orientation when pressed while obtaining sufficient molded body strength. r From the viewpoint of obtaining a compact density of 4.2 g / cm 3 The following is preferable: In order to suppress oxidation of the alloy fine powder, molding is preferably carried out in an inert gas atmosphere such as nitrogen gas or Ar gas.

[0022] The sintering step is a step of sintering the compact obtained in the compacting step in an inert gas atmosphere such as Ar gas or in a high vacuum, and in the present invention, the sintering step includes an atmospheric heat treatment step in which heat treatment is performed in an inert gas atmosphere and a vacuum heat treatment step in which heat treatment is performed in a vacuum atmosphere. In the present invention, in order to suppress the temperature drop of the compact caused by the release of hydrogen gas in the compact (endothermic reaction) and the occurrence of cracks caused by the temperature difference, the compact is held at a predetermined temperature for a predetermined time in an inert gas atmosphere in the atmospheric heat treatment step, and then sintered in the vacuum heat treatment step. Here, in order to sufficiently decompose the lubricant by hydrogen gas, it is necessary to set the holding temperature in the atmospheric heat treatment step to be equal to or higher than the lubricant decomposition temperature and equal to or lower than the sintering temperature, and the holding temperature may be appropriately set according to the type of lubricant. For example, when the above-mentioned stearic acid (decomposition temperature 376°C), decanoic acid (decomposition temperature 270°C), lauric acid (decomposition temperature 225°C), zinc stearate (decomposition temperature 376°C), etc. are used as lubricants, it is preferable to set the temperature to 400°C to 800°C. Similarly, the holding time is preferably set to, for example, 0.5 to 10 hours. Furthermore, in order to suppress the carbon concentration distribution within the magnet due to gas attack from hydrocarbon gas resulting from decomposition of the lubricant, the holding at the specified temperature for the specified time in this atmospheric heat treatment step is carried out in an inert gas atmosphere of 10 kPa to 100 kPa. By satisfying such holding conditions, it is possible to alleviate the effects of gas attack near the surface while promoting the decomposition of the lubricant in the magnet.

[0023] In the above atmospheric heat treatment step, the inert gas atmosphere pressure may be maintained within the above range of 10 kPa to 100 kPa, and evacuation at a rate of 0.1 to 1000 kPa / min and introduction of the inert gas at a rate of 0.1 to 100 kPa / min may be performed multiple times, thereby reducing the hydrocarbon gas concentration in the system and more effectively mitigating the effects of gas attack on the magnet. Furthermore, in this case, although not particularly limited, the inert gas atmosphere pressure may be set within the above pressure range of 10 kPa to 100 kPa at a predetermined pressure P set within the range. k 0.5P k Super ~1.5P kIt is preferable to repeat the above evacuation / inert gas introduction so that the change in the magnet surface density is within a range of less than 100 nm. By satisfying such holding conditions, the decomposition of the lubricant in the magnet can be promoted while more effectively and reliably mitigating the effects of gas attack near the surface.

[0024] In the above atmospheric heat treatment step, the inert gas forming the inert gas atmosphere is not particularly limited, but preferably used are He gas, Ar gas, N2 gas, etc.

[0025] Next, the vacuum heat treatment step involves heat treatment in a high vacuum at the sintering temperature of the molded body, and is not particularly limited, but it is preferable to carry out the heat treatment by holding the molded body at a temperature in the range of 950°C to 1200°C for 0.5 to 10 hours.

[0026] In the present invention, after the atmospheric heat treatment step and the vacuum heat treatment step in the sintering step are sequentially performed, the obtained sintered body is then subjected to H cJ In order to increase the temperature of the sintered body, a heat treatment may be performed at a temperature lower than the sintering temperature. The heat treatment after sintering may be a two-stage heat treatment consisting of a high-temperature heat treatment and a low-temperature heat treatment, or only a low-temperature heat treatment may be performed. In the high-temperature heat treatment, the sintered body is preferably heat-treated at a temperature of 600 to 950°C, and in the low-temperature heat treatment, the sintered body is preferably heat-treated at a temperature of 400 to 600°C.

[0027] The obtained rare earth sintered magnet was ground into a predetermined shape and then 1 The oxide of R 2 Fluoride, R 3 Acid fluoride, R 4 hydroxide, R 5 Carbonate of R 6 Basic carbonate of R 7 One or more metals or alloys selected from (R 1 ~R 7The rare earth sintered magnet may be subjected to a so-called grain boundary diffusion treatment, in which a diffusion source (one or more selected from rare earth elements) is present on the surface of the rare earth sintered magnet and heat-treated. The diffusion source may be fixed to the magnet surface by a dip coating method in which the sintered magnet is immersed in a slurry containing a powdered diffusion source, the slurry is applied, and then dried, a screen printing method, or a dry film formation method such as sputtering or PLD. The temperature of the grain boundary diffusion heat treatment is lower than the sintering temperature, and is preferably 700°C or higher. The time is not particularly limited from the viewpoint of obtaining a good sintered magnet structure and magnetic properties, but is preferably 5 minutes to 80 hours, and more preferably 10 minutes to 50 hours. The above R contained in the powder is removed by this grain boundary diffusion treatment. 1 ~R 7 is diffused into the magnet, cJ For the sake of convenience, the rare earth element introduced by grain boundary diffusion is referred to as R 1 ~R 7 However, after grain boundary diffusion, both are included in the above-mentioned R component of the rare earth sintered magnet of the present invention. 1 ~R 7 As the diffusion source containing H, it is preferable to use a metal, compound, or intermetallic compound containing HR (HR is one or more elements selected from Dy, Tb, and Ho), which can more effectively diffuse H. cJ It is possible to increase the number of

[0028] The magnet to which the above grain boundary diffusion treatment has been applied exhibits a characteristic concentration distribution of the R element. That is, within at least 500 μm of the magnet surface to which the above diffusion source has been applied, at least a portion of the surface vicinity of the main phase particle has a higher R' concentration (R' is one or more elements selected from rare earth elements, and R introduced by the above grain boundary diffusion treatment) than the center of the main phase particle. 1 ~R 7 A structure is formed in which there are areas with high concentrations of elements such as Cr.

[0029] The rare earth sintered magnet produced by the method for producing a rare earth sintered magnet of the present invention has a narrow carbon concentration distribution. For example, the carbon concentration C s and the carbon concentration in the center, C c It is possible to obtain a rare earth sintered magnet with a difference ΔC between the Br and H cJ The reason for this is believed to be as follows. In general, rare earth sintered magnets have some of the rare earth elements on the surface of the magnet evaporated during sintering, reducing the amount of rare earth elements on the surface, making the surface composition Fe-rich, R2Fe 17 The R2Fe phase is formed, which reduces Br and HcJ. By increasing the amount of boron (B) added, 17 However, in this case, the center becomes rich in B, so the R1Fe4B4 phase precipitates and Br decreases. Here, carbon (C) generally acts together with B to form the main phase R2Fe 14 It is known that X phase (X is B or C) is formed. Therefore, C s C c By increasing the concentration by 0.005 mass% or more, the precipitation of the R1Fe4B4 phase in the center of the magnet is suppressed, while a sufficient amount of R2Fe 14 Since the X phase can be formed, high Br and H cJ In addition, when the carbon concentration difference ΔC exceeds 0.03 mass%, the R2Fe alloy, in which carbon is the main phase at the surface, can be obtained. 14 In addition to the X phase, RCO compounds are formed, which reduces the amount of rare earth in the grain boundary phase. cJ will decrease significantly.

[0030] The rare earth sintered magnet produced by the method for producing a rare earth sintered magnet of the present invention is, as described above, composed of R (R is one or more elements selected from rare earth elements, and Nd is essential), T (T is one or more elements selected from iron group elements, and Fe is essential), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta.) and usually further contains O, N, C, and unavoidable impurities.

[0031] As mentioned above, R is one or more elements selected from rare earth elements, and Nd is essential. The content of R is not particularly limited, but from the viewpoint of suppressing crystallization of α-Fe in the melted alloy and promoting normal densification during sintering, it is preferably 12.0 atomic % or more of the entire rare earth magnet, more preferably 13.0 atomic % or more. Also, from the viewpoint of obtaining a high Br, it is preferably 16.0 atomic % or less, more preferably 15.5 atomic % or less.

[0032] The proportion of Nd in R is not particularly limited, but is preferably 60 atomic % or more, and more preferably 75 atomic % or more of all R elements. In addition, R elements other than Nd are not particularly limited, but may preferably contain Pr, Dy, Tb, Ho, Er, Sm, Ce, Y, etc.

[0033] The above T is at least one element selected from the iron group elements, i.e., Fe, Co, and Ni, with Fe being essential. The content of T is determined by the above R, B, M 1 , M 2 The remainder is made up of elements other than O, C, and N, and is preferably 70 atomic % or more and 85 atomic % or less of the entire rare earth magnet. The Fe content is preferably 70 atomic % or more and 82 atomic % or less of the entire rare earth magnet, and more preferably 75 atomic % or more and 80 atomic % or less.

[0034] The content of B is preferably 5.0 atomic % or more, more preferably 5.5 atomic % or more, from the viewpoint of forming a sufficient main phase and securing a sufficient Br. In addition, in consideration of the influence of Br due to precipitation of Nd1Fe4B4 phase when the content of B is too high, the content of B is preferably 8.0 atomic % or less, more preferably 7.0 atomic % or less.

[0035] The above M 1As described above, is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi. M 1 The content of H is determined from the viewpoint of obtaining the optimum temperature range in the heat treatment to ensure good productivity, and cJ From the viewpoint of suppressing the decrease in Br, the content is preferably 0.1 atomic % or more, more preferably 0.3 atomic % or more, and further preferably 0.5 atomic % or more. From the viewpoint of obtaining a high Br, the content is preferably 2.0 atomic % or less, and more preferably 1.5 atomic % or less.

[0036] The above M 2 As described above, is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta. 2 The inclusion of M has the effect of suppressing abnormal grain growth during the sintering process and preventing a decrease in Br. 2 The content of is not particularly limited, but is preferably 0.5 atomic % or less, more preferably 0.3 atomic % or less, and further preferably 0.2 atomic % or less. 2 If the content exceeds 0.5 atomic percent, M 2 M formed by the elements 2 -B phase is R2T 14 Decrease the B phase ratio to B r In addition, although not particularly limited, from the viewpoint of effectively suppressing abnormal grain growth of crystal grains, M 2 It is preferable that the content of is 0.1 atomic % or more.

[0037] The content of O is preferably 0.1 mass % or less, and more preferably 0.08 mass % or less. When the content of O is within this range, the magnetic properties, particularly the H cJ The N content is preferably 0.05% by mass or less, and more preferably 0.03% by mass or less. When the N content is within this range, H cJ Furthermore, the C content is preferably 0.07 mass% or less, and more preferably 0.05 mass% or less. When the C content is within this range, the HcJ The decrease in the amount of

[0038] In the rare earth sintered magnet of the present invention, the average crystal grain size is preferably 4 μm or less, and more preferably 3.5 μm or less. cJ can be obtained. The average crystal grain size can be measured, for example, by the following procedure. First, the cross section of the sintered magnet is polished to a mirror finish, and then the cross section is immersed in an etching solution such as Villela's solution (for example, a mixed solution of glycerin:nitric acid:hydrochloric acid=3:1:2) to selectively etch the grain boundary phase, and observed with a laser microscope. Next, based on the obtained observation image, the cross-sectional area of ​​each particle is measured by image analysis, and the diameter as an equivalent circle is calculated. Then, the average diameter is obtained based on the data of the area fraction occupied by each particle size. The average diameter may be, for example, the average of a total of about 2,000 particles in 20 different images. It can be easily measured by observing the magnet surface or cross section with, for example, a laser microscope.

[0039] Furthermore, the degree of orientation in the sintered magnet was r When the average crystal grain size is D [μm], it is preferable that the following relational expression (1) is satisfied. 0.26×D+97≦O r ≦0.26×D+99 (1)

[0040] Orientation degree O r By satisfying the relationship between the average crystal grain size D [μm] and the above formula (1), a high B r and high H cJThe reason for this is not entirely clear, but it can be speculated as follows. Generally, the crystal grain size is refined by refining the powder size before compacting and sintering, but as the powder size becomes finer, the surface area ratio of the powder increases, which increases the frictional resistance between the powder particles, making it difficult for the powder to be oriented during magnetic field compaction. Experiments by the inventors have shown that this change is worsened by 0.26% for a fine powder size of 4 μm or less and a crystal grain size refinement of 1 μm. Also, when the degree of orientation of the powder is low, a high B r However, if the degree of orientation is too high, the H cJ It is known that the B r and high H cJ It has been found that the degree of orientation can be stably obtained when the degree of orientation is within the range of the above relational expression (1).

[0041] Here, the above orientation degree O r [%] is not particularly limited, but it is important to bring out the potential of the material and achieve a good B r From the viewpoint of obtaining the above, the degree of orientation is preferably 96% or more, and more preferably 97% or more, and it is preferable that the relationship of the above relational formula (1) is achieved within a range that satisfies the requirement of this preferred degree of orientation and the above average crystal grain size of 4 μm or less. r [%] can be measured by a known method such as electron backscatter diffraction (EBSD). EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0043] [Examples 1 to 16, Comparative Examples 1 to 20] Nd metal, Pr metal, ferroboron alloy, electrolytic Co, Al metal, Cu metal, Ga metal, Si metal, zirconium metal and electrolytic iron (all metals are 99% or more pure) were weighed and mixed in a predetermined ratio, melted and cast by strip casting to obtain flake-shaped raw alloy with a thickness of 0.2 to 0.4 mm. The obtained flake-shaped raw alloy was hydrogen embrittled in a pressurized hydrogen atmosphere (hydrogen pressure: 150 kPa, moisture content: 2.2 ppm) to obtain coarsely pulverized powder. Next, 0.2 parts by mass of stearic acid (decomposition temperature: 376°C) was added and mixed with 100 parts by mass of the obtained coarsely pulverized powder, and then dry-pulverized in a nitrogen stream (moisture content: 10 ppm) using an airflow pulverizer (jet mill device) to obtain a pulverized particle size (D 50 The resulting alloy powder had a particle size of 2.9 μm. 50 ) is the volume-based median diameter obtained by the laser diffraction method using the airflow dispersion method. This finely pulverized powder was filled into the mold of a molding machine in a N2 gas atmosphere, and while being oriented in a magnetic field of 15 kOe (1.19 MA / m), it was pressed and molded in a direction perpendicular to the magnetic field. The density of the molded body at this time was 3.0 to 4.0 g / cm. 3 It was.

[0044] The obtained compact was subjected to atmospheric heat treatment in an Ar gas atmosphere under the conditions shown in Table 1, and then sintered in a vacuum at 1040 to 1080°C (a temperature at which densification by sintering is sufficient for each sample) for 5 hours to obtain a Nd magnet material. The density of the obtained Nd magnet material was 7.5 g / cm. 3 The results were as above. Furthermore, metal composition analysis was performed on the central portion of the obtained Nd magnet material using high-frequency inductively coupled plasma optical emission spectroscopy (ICP-OES). The results showed that the contents of Nd were 24.1 mass% Nd, 6.5 mass% Pr, 66.3 mass% Fe, 0.5 mass% Co, 0.2 mass% Cu, 0.2 mass% Zr, 0.1 mass% Al, 1 mass% B, 0.1 mass% Si, and 0.8 mass% Ga (the rest were impurity elements) in all of Examples 1 to 16 and Comparative Examples 1 to 20. Furthermore, the degree of orientation O rThe average grain size D [μm] was measured by EBSD and a laser microscope, and the results were 98.6% and 3.6 μm for Examples 1 to 16 and Comparative Examples 1 to 20, respectively, satisfying the following formula (1). 0.26×D+97≦O r ≦0.26×D+99 (1)

[0045] [Table 1]

[0046] The surface of the obtained Nd magnet material was polished by 0.1 mm, and then samples were made by machining the end and center of the Nd magnet material into rectangular parallelepiped shapes of 6 mm x 6 mm x 3 mm, respectively, and analysis of oxygen, carbon, and nitrogen was performed by infrared absorption gas analysis. The analysis results of carbon concentration are shown in Tables 2 to 4. The analysis results of oxygen concentration and nitrogen concentration were almost the same within the analytical error in Examples 1 to 16 and Comparative Examples 1 to 14, and the values ​​were 0.08 mass% for oxygen concentration and 0.02 mass% for nitrogen concentration. In addition, the analysis was performed while avoiding the crack generation part for Comparative Examples 1 to 10, but since large cracks occurred in Comparative Examples 15 to 20, it was not possible to analyze the center and end of the Nd magnet material.

[0047] [Table 2]

[0048] [Table 3]

[0049] [Table 4]

[0050] When comparing Examples 1 to 16 and Comparative Examples 1 to 14, it can be seen that in cases where the conditions of the present invention are met (Examples 1 to 16), the carbon concentration in the magnet center is low at 0.06 mass% or less, and the carbon concentration difference ΔC between the magnet end and the magnet surface is suppressed to a low level of 0.03 mass% or less. On the other hand, when the holding temperature is lower than the specification of the present invention (the decomposition temperature of stearic acid is 376°C), the lubricant is not fully decomposed, so the overall carbon concentration, including the magnet center, does not decrease sufficiently. Also, when the holding pressure is higher than the specification of the present invention, ΔC increases to 0.04 mass% or more. This is thought to be because the decomposition of the lubricant progresses further in the magnet center, while the amount of generated hydrocarbon gas also increases, increasing the effect of gas attack on the surface. On the other hand, when the holding pressure is lower than the specification of the present invention, cracks occur in the magnet, as shown in Comparative Examples 15 to 20 in Table 1. Furthermore, when the holding temperature is 400°C to 800°C, there is a tendency for ΔC to be lower and for the carbon concentration in the center to decrease further.

[0051] [Examples 17 to 32, Comparative Examples 21 to 40] Magnets were produced in the same manner as in Example 1. At that time, the amount of lubricant (stearic acid) added was 0.1 parts by mass per 100 parts by mass of the coarsely pulverized powder. The heat treatment conditions at that time are shown in Table 5. For the obtained magnets, the magnet ends and the magnet center were analyzed for carbon concentration, oxygen concentration, and nitrogen concentration in the same manner as in Example 1. The carbon concentration analysis results are shown in Tables 6 to 8. The oxygen concentration and nitrogen concentration analysis results were almost the same within the analytical error in Examples 17 to 32 and Comparative Examples 21 to 40, with the values ​​being 0.09 mass% for oxygen concentration and 0.02 mass% for nitrogen concentration. In addition, for Comparative Examples 21 to 30, the analysis was performed while avoiding the crack generation area, but for Comparative Examples 35 to 40, large cracks occurred, so the analysis of the Nd magnet material center and ends could not be performed. Furthermore, the central portion of the obtained Nd magnet material was subjected to metal composition analysis using ICP-OES, and the results showed that the composition was 24.1 mass% Nd, 6.5 mass% Pr, 66.3 mass% Fe, 0.5 mass% Co, 0.2 mass% Cu, 0.2 mass% Zr, 0.1 mass% Al, 1 mass% B, 0.1 mass% Si, and 0.8 mass% Ga (the rest were impurity elements) for all of Examples 17 to 32 and Comparative Examples 21 to 40. Furthermore, the orientation degree was measured using EBSD, and the average crystal grain size was measured using a laser microscope, and the results were 98.1% and 3.6 μm, respectively, for all of Examples 17 to 32 and Comparative Examples 21 to 40, satisfying the above formula (1).

[0052] [Table 5]

[0053] [Table 6]

[0054] [Table 7]

[0055] [Table 8]

[0056] When comparing Examples 17 to 32 and Comparative Examples 21 to 34, it can be seen that in cases where the conditions of the present invention are met (Examples 17 to 32), the carbon concentration in the magnet center is low at 0.04 mass% or less, and the carbon concentration difference ΔC between the magnet end and the magnet surface is suppressed to a low level of 0.02 mass% or less. On the other hand, when the holding temperature is lower than the specification of the present invention (the decomposition temperature of stearic acid is 376°C), the lubricant is not fully decomposed, so the overall carbon concentration, including the magnet center, does not decrease sufficiently. Also, when the holding pressure is higher than the specification of the present invention, ΔC increases to 0.03 mass% or more. This is thought to be because the decomposition of the lubricant progresses further in the magnet center, while the amount of generated hydrocarbon gas also increases, increasing the effect of gas attack on the surface. On the other hand, when the holding pressure is lower than the specification of the present invention, cracks occur in the magnet, as shown in Comparative Examples 35 to 40 in Table 5. Furthermore, when the holding temperature is 600°C to 800°C, there is a tendency for ΔC to be lower and for the carbon concentration in the center to decrease further.

[0057] [Examples 33 to 38] A magnet was produced in the same manner as in Example 17. The holding time during the atmospheric heat treatment was changed. The heat treatment conditions are shown in Table 9. The obtained magnet was analyzed for carbon concentration, oxygen concentration, and nitrogen concentration at the magnet end and center in the same manner as in Example 1. The carbon concentration analysis results are shown in Table 10. The oxygen concentration and nitrogen concentration analysis results were almost the same within the analytical error in Examples 33 to 38, with the oxygen concentration being 0.09 mass% and the nitrogen concentration being 0.02 mass%. In addition, the metal composition analysis of the center of the obtained Nd magnet material using ICP-OES showed that all of Examples 33 to 38 had Nd 24.1 mass%, Pr 6.5 mass%, Fe 66.3 mass%, Co 0.5 mass%, Cu 0.2 mass%, Zr 0.2 mass%, Al 0.1 mass%, B 1 mass%, Si 0.1 mass%, and Ga 0.8 mass% (the rest were impurity elements). Furthermore, the degree of orientation was measured by EBSD and the average crystal grain size was measured by a laser microscope, and both were 98.1% and 3.6 μm, respectively, which satisfied the above formula (1).

[0058] [Table 9]

[0059] [Table 10]

[0060] A comparative study of Examples 33 to 38 reveals that by setting the holding time within the range of 0.5 to 10 hours, the carbon concentration in the center and edges of the magnet can be reduced even further than under other conditions, while maintaining the same ΔC. This is believed to be because setting the holding time within the above range ensures that there is enough time for the lubricant to decompose, and the holding process is completed before the effects of gas attack become significant.

[0061] [Examples 39 to 51] Magnets were produced using the same procedure as in Example 17. However, in the atmospheric heat treatment step in the sintering process, evacuation and inert gas introduction were alternately repeated under the conditions in Table 11 (hereinafter, this process will be referred to as atmospheric gas exchange treatment). For the obtained magnets, the magnet ends and center were analyzed for carbon concentration, oxygen concentration, and nitrogen concentration in the same manner as in Example 1. The analysis results of carbon concentration are shown in Table 12. The analysis results of oxygen concentration and nitrogen concentration were almost the same within the analytical error in Examples 39 to 51, with the values ​​being 0.09 mass% for oxygen concentration and 0.02 mass% for nitrogen concentration. In addition, the central portion of the obtained Nd magnet material was subjected to metal composition analysis using ICP-OES, and the results showed that the composition of each of Examples 39 to 51 was 24.1 mass% Nd, 6.5 mass% Pr, 66.3 mass% Fe, 0.5 mass% Co, 0.2 mass% Cu, 0.2 mass% Zr, 0.1 mass% Al, 1 mass% B, 0.1 mass% Si, and 0.8 mass% Ga (the rest were impurity elements). Furthermore, the degree of orientation was measured using EBSD and the average crystal grain size was measured using a laser microscope, and the results were 98.1% and 3.6 μm, respectively, satisfying the above formula (1).

[0062] [Table 11]

[0063] [Table 12]

[0064] The following findings were obtained by comparing Examples 39 to 51 and Example 21. When the evacuation speed is 0.1 to 1000 kPa / min and the inert gas introduction speed is 1 to 100 kPa / min (Examples 40 to 44, Examples 47 to 50), it can be seen that the carbon concentration on the magnet surface is further reduced, thereby reducing ΔC. This is believed to be because, during the atmospheric heat treatment process, the hydrocarbon gas in the inert gas atmosphere caused by the decomposition of the lubricant is removed by repeating the evacuation / inert gas introduction process, thereby suppressing gas attack on the magnet surface. On the other hand, when the evacuation speed of the evacuation process is very slow (Example 39) or the introduction speed of the inert gas is very slow (Example 46), the generated hydrocarbon gas cannot be completely removed, and therefore the results are thought to be equivalent to those when the atmospheric gas exchange process is not performed (Example 21). Furthermore, when the evacuation speed of the vacuum evacuation process is very fast (Example 45) or when the inert gas introduction speed is very fast (Example 51), in addition to the hydrocarbon gas in the system, hydrogen gas that promotes the decomposition of the lubricant in the magnet is excessively removed, which is thought to reduce ΔC but slightly increase the carbon concentration in the center and ends of the magnet.

[0065] [Examples 52 to 56] A magnet was produced in the same manner as in Example 17. However, in the atmospheric heat treatment step, an atmospheric gas exchange process was performed under the conditions in Table 13. The obtained magnet was analyzed for carbon concentration, oxygen concentration, and nitrogen concentration at the magnet end and center in the same manner as in Example 1. The carbon concentration analysis results are shown in Table 14. The oxygen concentration and nitrogen concentration analysis results were almost the same within the analytical error in Examples 52 to 56, with the oxygen concentration being 0.09 mass% and the nitrogen concentration being 0.02 mass%. In addition, a metal composition analysis was performed on the center of the obtained Nd magnet material using ICP-OES, and the results were Nd 24.1 mass%, Pr 6.5 mass%, Fe 66.3 mass%, Co 0.5 mass%, Cu 0.2 mass%, Zr 0.2 mass%, Al 0.1 mass%, B 1 mass%, Si 0.1 mass%, and Ga 0.8 mass% in all of Examples 52 to 56 (the rest were impurity elements). Furthermore, the degree of orientation was measured by EBSD and the average crystal grain size was measured by a laser microscope, and both were 98.1% and 3.6 μm, respectively, which satisfied the above formula (1).

[0066] [Table 13]

[0067] [Table 14]

[0068] The following findings were obtained by comparing Examples 52 to 56. k (60 kPa in Examples 52 to 56) k Super ~1.5P k When controlled within a range satisfying the condition below (Examples 52, 53, and 55), the carbon concentration and ΔC at the center and ends of the magnet were reduced compared to outside that range. Outside this range, as in Examples 45 and 51, in addition to the hydrocarbon gas in the system, hydrogen gas that promotes the decomposition of the lubricant in the magnet is excessively removed, which is thought to reduce ΔC but slightly increase the carbon concentration at the center and ends of the magnet.

[0069] As described above, the rare earth sintered magnets produced by the methods of the present invention obtained in Examples 1 to 56 have sufficiently low oxygen, nitrogen, and carbon concentrations, and the difference in carbon concentration between the magnet surface and center is small, making them suitable for use in electric vehicles and other applications that require high coercive force.

Claims

1. The method includes a melting step of melting a raw material to obtain a raw material alloy having a predetermined composition, a crushing step of crushing the raw material alloy to prepare an alloy fine powder, a molding step of compressing the alloy fine powder under application of a magnetic field to obtain a molded body, and a sintering step of heat-treating the molded body to obtain a sintered body, and R (R is one or more elements selected from rare earth elements, and Nd is an essential element), T (T is one or more elements selected from iron group elements, and Fe is an essential element), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M 2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta, The pulverization step includes a coarse pulverization step and a fine pulverization step, The coarse pulverization step further includes a pulverization step by hydrogen absorption, and the hydrogen-containing coarse powder is used in the subsequent fine pulverization step without performing a dehydrogenation treatment; The pulverization step includes a lubricant addition step of adding a lubricant before or after the coarse pulverization step, The sintering step includes an atmospheric heat treatment step of heating the molded body to a predetermined temperature that is equal to or higher than the decomposition temperature of the lubricant and equal to or lower than the sintering temperature of the sintered body, and maintaining the predetermined temperature for a predetermined time, and performing this heating and maintaining the predetermined temperature in an inert gas atmosphere of 10 kPa to 100 kPa to heat the molded body, and a vacuum heat treatment step of switching to a vacuum atmosphere after the atmospheric heat treatment step to heat the molded body to the sintering temperature of the sintered body.

2. 2. The method for producing a rare earth sintered magnet according to claim 1, wherein the lubricant is at least one selected from the group consisting of stearic acid, zinc stearate, decanoic acid, and lauric acid.

3. The inert gas forming the inert gas atmosphere in the atmospheric heat treatment step is He gas, Ar gas, or N 2 3. The method for producing a rare earth sintered magnet according to claim 1, wherein the gas is a gas.

4. The method for producing a rare earth sintered magnet according to any one of claims 1 to 3, wherein the predetermined temperature which is equal to or higher than the decomposition temperature of the lubricant and equal to or lower than the sintering temperature of the sintered body is 400°C to 800°C.

5. The method for producing a rare earth sintered magnet according to any one of claims 1 to 4, wherein the holding time at the predetermined temperature in the atmospheric heat treatment step is 0.5 hours to 10 hours.

6. In the hydrogen absorption pulverization step, the hydrogen pressure is 100 kPa or more, and in the fine pulverization step, the coarsely pulverized raw alloy is pulverized in a non-oxidizing gas atmosphere having a moisture content of 100 ppm or less to a volume-based median diameter D 50 The method for producing a rare earth sintered magnet according to any one of claims 1 to 5, wherein the mixture is pulverized to a size of 0.2 µm to 10 µm by a pressure of 0.5 to 1000.

7. 7. The method for producing a rare earth sintered magnet according to claim 1, wherein the atmospheric heat treatment step includes a step of repeatedly performing evacuation at a rate of 0.1 to 1000 kPa / min and subsequent introduction of an inert gas at a rate of 1 to 100 kPa / min while maintaining the inert gas atmosphere pressure at 10 kPa to 100 kPa.

8. In the atmospheric heat treatment step, the inert gas atmosphere pressure is set within the pressure range of 10 kPa to 100 kPa at a predetermined pressure P k 0.5P k Super ~ 1.5P k The method for producing a rare earth sintered magnet according to claim 7, wherein the temperature varies within a range of less than 100° C.

9. The carbon content is 0.05 mass% or less, and the surface carbon concentration C of the sintered magnet is s and central carbon concentration C c The rare earth sintered magnet is characterized in that the difference ΔC between the above is 0.005% by mass and 0.03% by mass.

10. Carbon concentration at the center of sintered magnet C c The rare earth sintered magnet according to claim 9, wherein the content of Mn is 0.057 mass % or less.

11. R (R is one or more elements selected from rare earth elements, and Nd is essential), T (T is one or more elements selected from iron group elements, and Fe is essential), B, M 1 (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; and M 2 (M 2 is one or more elements selected from Ti, V, Zr, Nb, Hf, and Ta, and further has an oxygen content of 0.1 mass% or less and a nitrogen content of 0.05 mass% or less.

12. R content is 12.0 atomic % to 16.0 atomic % (R is one or more elements selected from rare earth elements, and Nd is essential), M 1 The content is 0.1 atomic % to 2.0 atomic % (M 1 is one or more elements selected from Al, Si, Cr, Mn, Cu, Zn, Ga, Ge, Mo, Sn, W, Pb, and Bi; M 2 The content is 0.1 atomic % to 0.5 atomic % (M 2 The rare earth sintered magnet according to any one of claims 9 to 11, wherein:

13. The rare earth sintered magnet according to any one of claims 9 to 12, wherein the average crystal grain size is 4 µm or less.

14. Regarding the degree of orientation in the sintered magnet, r [%] and the average crystal grain size is D [μm], the following relational expression (1) is satisfied. 0.26×D+97≦O r ≦0.26×D+99 ・・・(1) The rare earth sintered magnet according to any one of claims 9 to 13, which satisfies the above.

15. 13. The rare earth sintered magnet according to claim 11, wherein within at least 500 μm from the surface of the sintered magnet, at least a portion of the surface of a main phase particle has a region having a higher concentration of R' (R' is one or more elements selected from rare earth elements and constitutes at least a portion of the R) than the central portion of the main phase particle.

Citation Information

Patent Citations

  • Method for improving performance of sintered neodymium-iron-boron magnet

    CN110767401A

  • Method for manufacturing sintered magnet of rare earth element

    JP2003183764A

  • Method for removing lubricant

    JP2007327102A

  • R-iron-boron based sintered magnet and method for manufacturing the same

    JP2017147426A

  • R-t-b based permanent magnet